Resin composition, pellets, and molded body
A resin composition combining polyphenylene ether resin with polypropylene homopolymer, polyolefin copolymer, and hollow inorganic filler, along with a hydrogenated block copolymer, addresses the trade-off between impact and heat resistance, resulting in low specific gravity molded articles with enhanced mechanical properties.
Patent Information
- Application Number
- JP2023090808
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2022-10-04
- Filing Date
- 2023-06-01
- Publication Date
- 2024-11-27
- Estimated Expiration
- 2043-06-01
AI Technical Summary
The use of hollow inorganic fillers in polyphenylene ether resin compositions to reduce weight results in decreased impact resistance, and adding impact modifiers to improve impact resistance often compromises heat resistance.
A resin composition is formulated by blending polyphenylene ether resin with specific polypropylene homopolymer, polyolefin copolymer, hollow inorganic filler, and a hydrogenated block copolymer to maintain heat resistance while enhancing impact resistance.
The composition achieves a low specific gravity with excellent impact resistance and maintains heat resistance, producing molded articles with improved mechanical properties.
Smart Images

Figure 0007591093000001 
Figure 0007591093000002 
Figure 0007591093000003
Abstract
Description
[Technical field]
[0001] The present invention relates to a resin composition, a pellet, and a molded article, and in particular to a resin composition containing a polyphenylene ether resin as a main component. [Background technology]
[0002] Resin compositions containing polyphenylene ether resin as a base resin (hereinafter sometimes referred to as "polyphenylene ether resin compositions") have features such as heat resistance, electrical properties, dimensional stability, impact resistance, and low specific gravity. For this reason, polyphenylene ether resin compositions are widely used for applications such as various electric and electronic parts, office equipment parts, automobile parts, building materials, and various other exterior materials and industrial products. In addition, reinforcing fillers are sometimes blended to reinforce polyphenylene ether resin compositions.
[0003] On the other hand, from the viewpoint of weight reduction, hollow inorganic fillers are sometimes blended into thermoplastic resins as reinforcing fillers. For example, Patent Document 1 discloses a resin composition comprising at least one thermoplastic resin (A) at 20% by mass or more and 99% by mass or less, hollow microspheres (B) at 1% by mass or more and 80% by mass or less, and organic fibers (C) at 1% by mass or more and 100% by mass or less relative to 100% by mass of the total amount of the thermoplastic resin (A) and the hollow microspheres (B), wherein the organic fibers (C) have a melting point and a decomposition onset temperature higher than the melting point of the thermoplastic resin (A). [Prior art documents] [Patent documents]
[0004] [Patent Document 1] JP 2016-108372 A Summary of the Invention [Problem to be solved by the invention]
[0005] As described above, the use of hollow inorganic fillers as reinforcing fillers can reduce the weight of resin compositions or molded articles obtained from the resin compositions. However, the impact resistance of the molded articles tends to decrease. In addition, when an impact modifier is added to improve the impact resistance, the heat resistance tends to decrease. The present invention has an object to solve the above problems, and to provide a resin composition having a low specific gravity containing a polyphenylene ether resin and a hollow inorganic filler, which is capable of providing a molded article having excellent impact resistance while maintaining the heat resistance of the polyphenylene ether resin, as well as pellets and a molded article. [Means for solving the problem]
[0006] In view of the above problems, the present inventors have conducted research and found that the above problems can be solved by blending a predetermined polyolefin and a predetermined block copolymer together with a hollow filler into a polyphenylene ether resin. Specifically, the above problems were solved by the following means. <1> (a) a polyphenylene ether resin; (b) a polypropylene homopolymer; (c) a polyolefin copolymer having a melt flow rate (MFR) of 0.3 to 25 g / 10 min at a load of 2.16 kg and a temperature of 230°C, as measured in accordance with JIS-K7210; (d) a hollow inorganic filler; (e) Block copolymers and Including, The (e) block copolymer is a hydrogenated product containing a vinyl aromatic compound block (e1) and an isoprene polymer block (e2), The resin composition contains the hollow inorganic filler (d) in an amount of 6 to 30 parts by mass based on 100 parts by mass of the resin composition. <2> The (d) hollow inorganic filler is contained in an amount of 6 to 20 parts by mass based on 100 parts by mass of the resin composition. <1> The resin composition according to claim 1. <3> The (d) hollow inorganic filler has a compressive fracture strength of 105 to 130 MPa. <1> or <2> The resin composition according to claim 1. <4> The (a) polyphenylene ether resin is contained in an amount of 40 to 65 mass%, and the (b) polypropylene homopolymer and the (c) polyolefin copolymer are contained in an amount of 35 to 60 mass% in total, relative to 100 mass% in total of the (a) polyphenylene ether resin, the (b) polypropylene homopolymer, and the (c) polyolefin copolymer. <1> ~ <3> The resin composition according to claim 1. <5> Further, (f) a polystyrene resin having a weight average molecular weight (Mw) of 3,000 to 20,000 is contained. <1> ~ <4> 10. The resin composition according to claim 9 . <6> The content of vinyl aromatic compound units in the (e) block copolymer is 50% by mass or more and less than 80% by mass. <1> ~ <5> 10. The resin composition according to claim 9 . <7> The (d) hollow inorganic filler has a compressive fracture strength of 105 to 130 MPa; The (a) polyphenylene ether resin is contained in an amount of 40 to 65 mass%, and the (b) polypropylene homopolymer and the (c) polyolefin copolymer are contained in an amount of 35 to 60 mass% in total, relative to 100 mass% in total of the (a) polyphenylene ether resin, the (b) polypropylene homopolymer, and the (c) polyolefin copolymer; Further, (f) a polystyrene resin having a weight average molecular weight (Mw) of 3,000 to 20,000, The content of vinyl aromatic compound units in the (e) block copolymer is 50% by mass or more and less than 80% by mass. <1> ~ <6> 10. The resin composition according to claim 9 . <8> <1> ~ <7> 2. A pellet of the resin composition according to claim 1. <9> <1> ~ <7> 2. A molded article molded from the resin composition according to claim 1. <10> <8> A molded body formed from the pellets according to claim 1. Effect of the Invention
[0007] It is now possible to provide a resin composition having a low specific gravity, which contains a polyphenylene ether resin and a hollow inorganic filler, and which is capable of providing a molded article having excellent impact resistance while maintaining the heat resistance of the polyphenylene ether resin, as well as pellets and molded articles. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0008] Hereinafter, an embodiment of the present invention (hereinafter, simply referred to as "the present embodiment") will be described in detail. Note that the present embodiment is an example for explaining the present invention, and the present invention is not limited to the present embodiment. In this specification, the use of "to" means that the numerical values before and after it are included as the lower limit and upper limit. In this specification, various physical properties and characteristic values are those at 23° C. unless otherwise specified. If the measurement methods, etc. described in the standards shown in this specification vary from year to year, they will be based on the standards as of January 1, 2022, unless otherwise stated.
[0009] The resin composition of the present embodiment comprises (a) a polyphenylene ether resin, (b) a polypropylene homopolymer, (c) a polyolefin copolymer having a melt flow rate (MFR) of 0.3 to 25 g / 10 min at a load of 2.16 kg and a temperature of 230° C., as measured in accordance with JIS-K7210 (sometimes referred to as “(c) polyolefin copolymer” in this specification), (d) a hollow inorganic filler, and (e) a block copolymer, wherein the (e) block copolymer is a hydrogenated product containing a vinyl aromatic compound block (e1) and an isoprene polymer block (e2), and is characterized in that the (d) hollow inorganic filler is contained in a proportion of 6 to 30 parts by mass relative to 100 parts by mass of the resin composition. By adopting such a configuration, it is possible to provide a resin composition which contains a polyphenylene ether resin and a hollow inorganic filler and has a low specific gravity, and which is capable of providing a molded article having excellent impact resistance while maintaining the heat resistance of the polyphenylene ether resin.
[0010] By blending (d) hollow inorganic filler with (a) polyphenylene ether resin, the specific gravity of the resin composition can be reduced. In addition, (b) polypropylene homopolymer also has a lower specific gravity than (a) polyphenylene ether resin, so the specific gravity of the resin composition is reduced by adding (b) polypropylene homopolymer. However, when hollow inorganic filler (d) is blended, impact resistance tends to deteriorate. In addition, polypropylene homopolymer (b) also tends to deteriorate impact resistance. However, in this embodiment, it is presumed that blending polyolefin copolymer (c) can suppress the deterioration of impact resistance caused by blending polypropylene homopolymer (b). This is presumed to be because polypropylene homopolymer (b) and polyolefin copolymer (c) are partially mixed and the other portions are dispersed, forming a dispersion structure that can absorb larger impact energy. The resin composition of the present embodiment also contains a hydrogenated block copolymer (e) containing a vinyl aromatic compound block (e1) and an isoprene polymer block (e2). The component (e) is itself an elastomer and is not only easily absorbs impact energy, but also has a structure similar to that of the vinyl aromatic compound block (e1) (a) polyphenylene ether resin and the isoprene polymer block (e2) (b) polypropylene homopolymer, and the respective components have similar structures. It was hypothesized that (a) it also acts as a compatibilizer due to its high affinity with the resin, and that by finely dispersing the polyphenylene ether resin, it was possible to improve impact resistance and maintain heat resistance.
[0011] <(a) Polyphenylene ether resin> The resin composition of the present embodiment contains (a) a polyphenylene ether resin. The polyphenylene ether resin (a) used in the resin composition of this embodiment may be a known polyphenylene ether resin, and may be, for example, a polymer having a structural unit represented by the following formula in the main chain. The polyphenylene ether resin (a) may be either a homopolymer or a copolymer.
[0012] [ka] (Wherein, two R a each independently represents a hydrogen atom, a halogen atom, a primary or secondary alkyl group, an aryl group, an aminoalkyl group, a halogenated alkyl group, a hydrocarbyloxy group, or a halogenated hydrocarbyloxy group; b each independently represents a hydrogen atom, a halogen atom, a primary or secondary alkyl group, an aryl group, a halogenated alkyl group, a hydrocarbyloxy group, or a halogenated hydrocarbyloxy group. a cannot both become hydrogen atoms.)
[0013] R a and R b are each independently preferably a hydrogen atom, a primary or secondary alkyl group, or an aryl group. Suitable examples of the primary alkyl group include a methyl group, an ethyl group, an n-propyl group, an n-butyl group, an n-amyl group, an isoamyl group, a 2-methylbutyl group, a 2,3-dimethylbutyl group, a 2-, 3-, or 4-methylpentyl group, or a heptyl group. Suitable examples of the secondary alkyl group include an isopropyl group, a sec-butyl group, or a 1-ethylpropyl group. In particular, R a R is preferably a primary or secondary alkyl group having 1 to 4 carbon atoms or a phenyl group. b is preferably a hydrogen atom.
[0014] Suitable examples of the (a) polyphenylene ether resin homopolymer include 2,6-dialkylphenylene ether polymers such as poly(2,6-dimethyl-1,4-phenylene ether), poly(2,6-diethyl-1,4-phenylene ether), poly(2,6-dipropyl-1,4-phenylene ether), poly(2-ethyl-6-methyl-1,4-phenylene ether), and poly(2-methyl-6-propyl-1,4-phenylene ether). Examples of the copolymer include 2,6-dialkylphenol / 2,3,6-trialkylphenol copolymers such as 2,6-dimethylphenol / 2,3,6-trimethylphenol copolymer, 2,6-dimethylphenol / 2,3,6-triethylphenol copolymer, 2,6-diethylphenol / 2,3,6-trimethylphenol copolymer, and 2,6-dipropylphenol / 2,3,6-trimethylphenol copolymer; graft copolymers obtained by graft polymerizing styrene onto poly(2,6-dimethyl-1,4-phenylene ether); and graft copolymers obtained by graft polymerizing styrene onto a 2,6-dimethylphenol / 2,3,6-trimethylphenol copolymer.
[0015] In the present embodiment, the polyphenylene ether resin (a) is preferably poly(2,6-dimethyl-1,4-phenylene ether) or a random copolymer of 2,6-dimethylphenol and 2,3,6-trimethylphenol. Also, a polyphenylene ether resin having a specified number of terminal groups and copper content as described in JP-A-2005-344065 can be suitably used.
[0016] The (a) polyphenylene ether resin preferably has an intrinsic viscosity of 0.2 to 0.8 dL / g, more preferably 0.3 to 0.6 dL / g, at 30°C, measured in chloroform. By making the intrinsic viscosity 0.2 dL / g or more, the mechanical strength of the resin composition tends to be improved, while by making it 0.8 dL / g or less, the fluidity tends to be improved and molding processing tends to be easier. In addition, two or more (a) polyphenylene ether resins having different intrinsic viscosities may be used in combination to achieve this intrinsic viscosity range.
[0017] The method for producing the polyphenylene ether resin (a) used in this embodiment is not particularly limited, and may be, for example, a method of oxidatively polymerizing a monomer such as 2,6-dimethylphenol in the presence of an amine copper catalyst according to a known method, in which the intrinsic viscosity can be controlled within a desired range by selecting reaction conditions. The intrinsic viscosity can be controlled by selecting conditions such as polymerization temperature, polymerization time, and catalyst amount.
[0018] The content of the polyphenylene ether resin (a) in the resin composition of this embodiment is preferably 20.0 parts by mass or more, more preferably 25.0 parts by mass or more, even more preferably 28.0 parts by mass or more, even more preferably 30.0 parts by mass or more, and even more preferably 33.0 parts by mass or more, in 100 parts by mass of the resin composition. By making it equal to or more than the lower limit, the heat resistance (particularly, the deflection temperature under load) of the obtained molded body tends to be further improved. In addition, the upper limit of the content of the polyphenylene ether resin (a) is preferably 45.0 parts by mass or less, more preferably 40.0 parts by mass or less, and even more preferably 38.0 parts by mass or less, in 100 parts by mass of the resin composition. By making it equal to or less than the upper limit, the effect of improving the flowability of the resin composition, improving the impact resistance, and reducing the specific gravity of the obtained molded body tends to be further improved. The resin composition of the present embodiment may contain only one type of (a) polyphenylene ether resin, or may contain two or more types. When two or more types are contained, the total amount is preferably in the above range.
[0019] <(b) Polypropylene homopolymer> The resin composition of the present embodiment contains (b) a polypropylene homopolymer. The (b) polypropylene homopolymer used in this embodiment is a polymer containing polypropylene as a main component. That is, the polypropylene homopolymer (b) in this embodiment may contain other monomer units without departing from the spirit of the present invention. However, the polypropylene homopolymer (b) in this embodiment preferably contains 95% by mass or more (preferably 97% by mass or more, more preferably 99% by mass or more) of propylene units.
[0020] (b) The polypropylene homopolymer may contain a crystal nucleating agent. As the crystal nucleating agent, known crystal nucleating agents can be used, and examples thereof include metal salts of carboxylic acids, dibenzylidene sorbitol derivatives, and alkali metal salts of phosphoric esters. Specific examples of the crystal nucleating agent include sodium benzoate, aluminum adipate, aluminum pt-butylbenzoate, 1,3,2,4-dibenzylidene sorbitol, 1, 3,2,4-bis(p-methyl-benzylidene)sorbitol, 1,3,2,4-bis( p-ethylbenzylidene)sorbitol, 1,3,2,4-bis(3,4-dimethylbenzylidene)sorbitol, sodium bis(4-t-butylphenyl)phosphate, sodium bis(4-t-methylphenyl)phosphate, potassium bis(4,6-di-t-butylphenyl)phosphate, sodium 2,2'-methylene-bis(4,6-di-t-butylphenyl)phosphate, and sodium 2,2'-ethylidene-bis(4,6-di-t-butylphenyl)phosphate.
[0021] (b) The polypropylene homopolymer has a melt flow rate (MFR) measured according to JIS-K7210 under a load of 2.16 kg and at a temperature of 230° C. of preferably 0.1 g / 10 min or more, more preferably 0.5 g / 10 min or more, even more preferably 1.0 g / 10 min or more, even more preferably 1.5 g / 10 min or more, and even more preferably 2.0 g / 10 min or more. By making it equal to or greater than the lower limit, the fluidity of the resin composition tends to be improved. The MFR is also preferably equal to or less than 10.0 g / 10 min, more preferably equal to or less than 8.0 g / 10 min, even more preferably equal to or less than 5.0 g / 10 min, even more preferably equal to or less than 4.0 g / 10 min, and even more preferably equal to or less than 3.0 g / 10 min. By making it equal to or less than the upper limit, the nominal tensile strain and impact resistance of the molded article tend to be improved. When the resin composition of the present embodiment contains two or more kinds of (b) polypropylene homopolymers, it is preferable that the MFR of the mixture of (b) polypropylene homopolymers is in the above range.
[0022] The content of the polypropylene homopolymer (b) in the resin composition of this embodiment is preferably 20.0 parts by mass or more, more preferably 23.0 parts by mass or more, and even more preferably 25.0 parts by mass or more in 100 parts by mass of the resin composition. By setting it to the lower limit or more, the effect of improving the flowability of the resin composition and reducing the specific gravity of the obtained molded body tends to be improved. In addition, the upper limit of the content of the polypropylene homopolymer (b) is preferably 38.0 parts by mass or less, more preferably 35.0 parts by mass or less, and even more preferably 32.0 parts by mass or less in 100 parts by mass of the resin composition. By setting it to the upper limit or less, the decrease in impact resistance and heat resistance of the molded body tends to be suppressed. The resin composition of the present embodiment may contain only one type of (b) polypropylene homopolymer, or may contain two or more types. When two or more types are contained, the total amount is preferably in the above range.
[0023] <(c) Polyolefin copolymer> The resin composition of the present embodiment contains (c) a polyolefin copolymer having a melt flow rate (MFR) of 0.3 to 25 g / 10 min at a temperature of 230° C. under a load of 2.16 kg, measured in accordance with JIS-K7210. The MFR is preferably 0.5 g / 10 min or more, more preferably 1.0 g / 10 min or more, even more preferably 3.0 g / 10 min or more, even more preferably 5.0 g / 10 min or more, and even more preferably 5.5 g / 10 min or more. By making it equal to or greater than the lower limit, the flowability of the resin composition tends to be improved. The MFR is also preferably 20.0 g / 10 min or less, more preferably 15.0 g / 10 min or less, even more preferably 10.0 g / 10 min or less, even more preferably 8.0 g / 10 min or less, and even more preferably 7.5 g / 10 min or less. By making it equal to or less than the upper limit, the impact resistance of the molded article tends to be improved. When the resin composition of the present embodiment contains two or more kinds of (c) polyolefin copolymers, it is preferable that the MFR of the mixture of (c) polyolefin copolymers is in the above range.
[0024] The polyolefin copolymer (c) used in this embodiment is a copolymer of two or more kinds of olefins. The olefin is preferably an olefin having 2 to 5 carbon atoms, and more preferably ethylene, propylene, or butene. In the present embodiment, it is preferable that the copolymer is a copolymer of at least two of ethylene, propylene, and butene, and specifically, it is preferable that the copolymer is an ethylene-propylene-butene copolymer, an ethylene-propylene copolymer, an ethylene-butene copolymer, or a propylene-butene copolymer. In particular, it is preferable that the copolymer is an ethylene-propylene-butene copolymer, an ethylene-propylene copolymer, or an ethylene-butene copolymer, and it is more preferable that the copolymer is an ethylene-propylene-butene copolymer. In addition, the copolymer of two or more olefins in this embodiment may contain other monomer units within the scope of the present invention. However, the copolymer of two or more olefins in this embodiment is preferably 95% by mass or more (preferably 97% by mass or more, more preferably 99% by mass or more) of the copolymer is an olefin unit. The same applies to a copolymer of at least two of ethylene, propylene, and butene.
[0025] The content of the polyolefin copolymer (c) in the resin composition of this embodiment is preferably 1.0 part by mass or more, more preferably 2.0 parts by mass or more, even more preferably 3.0 parts by mass or more, even more preferably 4.0 parts by mass or more, and even more preferably 5.0 parts by mass or more, in 100 parts by mass of the resin composition. By making it equal to or more than the lower limit, the impact resistance and nominal tensile strain of the molded body tend to be further improved. In addition, the upper limit of the content of the polyolefin copolymer (c) is preferably 20.0 parts by mass or less, more preferably 15.0 parts by mass or less, even more preferably 12.0 parts by mass or less, even more preferably 10.0 parts by mass or less, and may be 5.9 parts by mass or less, in 100 parts by mass of the resin composition. By making it equal to or less than the upper limit, the heat resistance of the molded body tends to be further improved. The resin composition of the present embodiment may contain only one type of (c) polyolefin copolymer, or may contain two or more types. When two or more types are contained, the total amount is preferably in the above range.
[0026] <Blending ratio of components (a) to (c)> The blend ratio of (a) the polyphenylene ether resin, (b) the polypropylene homopolymer, and (c) the polyolefin copolymer in the resin composition of this embodiment will be described. The composition of the present embodiment preferably contains 40 to 65 mass% of the (a) polyphenylene ether resin and 35 to 60 mass% of the (b) polypropylene homopolymer and the (c) polyolefin copolymer in total, relative to 100 mass% of the (a) to (c) components in total. More preferably, the content of the polyphenylene ether resin (a) relative to 100% by mass of the total of the components (a) to (c) is preferably 45% by mass or more, more preferably 48% by mass or more, even more preferably 50% by mass or more, and may be 51% by mass or more. By making it equal to or more than the lower limit, the heat resistance of the obtained molded article tends to be further improved. In addition, the content of the polyphenylene ether resin (a) relative to 100% by mass of the total of the components (a) to (c) is preferably 60% by mass or less, more preferably 57% by mass or less, even more preferably 55% by mass or less, and even more preferably 53% by mass or less. By making it equal to or less than the upper limit, the flowability of the resin composition and the effect of reducing the specific gravity of the obtained molded article tend to be further improved.
[0027] More preferably, the total content of (b) polypropylene homopolymer and (c) polyolefin copolymer relative to 100% by mass of the total of the (a) to (c) components is 40% by mass or more, more preferably 43% by mass or more, even more preferably 45% by mass or more, and even more preferably 47% by mass or more. By making it equal to or more than the lower limit, the effect of improving the flowability of the resin composition and reducing the specific gravity of the molded body tends to be further improved. In addition, the total content of (b) polypropylene homopolymer and (c) polyolefin copolymer relative to 100% by mass of the total of the (a) to (c) components is preferably 55% by mass or less, more preferably 52% by mass or less, even more preferably 50% by mass or less, and even more preferably 49% by mass or less. By making it equal to or less than the upper limit, the heat resistance of the obtained molded body tends to be further improved.
[0028] The mass ratio (b) / (c) of the (b) polypropylene homopolymer and (c) polyolefin copolymer is preferably 1.5 or more, more preferably 2.0 or more, even more preferably 2.5 or more, even more preferably 3.0 or more, and even more preferably 3.5 or more. The (b) / (c) ratio is preferably 14.0 or less, more preferably 10.0 or less, even more preferably 7.0 or less, and even more preferably 6.0 or less.
[0029] <(d) Hollow inorganic filler> The resin composition of the present embodiment contains (d) hollow inorganic filler in a ratio of 6 to 30 parts by mass in 100 parts by mass of the resin composition. That is, the content of (d) hollow inorganic filler in 100% by mass of the resin composition is 6 to 30% by mass. (d) By including the hollow inorganic filler, a resin composition having a low specific gravity can be obtained. (d) Examples of hollow inorganic fillers include silica balloons, alumina balloons, hollow glass particles, and hollow ceramic particles, with hollow glass particles and hollow ceramic particles being preferred.
[0030] (d) The apparent density of the hollow inorganic filler is 0.40 g / cm 3 It is preferable that the content is 0.42 g / cm or more. 3 More preferably, it is 0.44 g / cm or more. 3 More preferably, it is 0.45 g / cm or more. 3 More preferably, it is 0.46 g / cm or more. 3 It is more preferable that the density is 0.47 g / cm or more depending on the application. 3 By making the density equal to or greater than the lower limit, the shell thickness of the hollow particles becomes thick, and crushing during kneading with the resin tends to be suppressed. In addition, the apparent density of the (d) hollow inorganic filler is 0.65 g / cm 3 It is preferable that the value is 0.6 / cm or less. 3 It is more preferable that the thickness is 0.56 / cm or less, depending on the application, etc. 3 Below, 0.55 / cm3 By making the content equal to or less than the upper limit, there is a tendency that the specific gravity of the molded article can be reduced more effectively. (d) The apparent density of the hollow inorganic filler can be calculated by measuring the mass with an electronic balance and then measuring the volume with a gas pycnometer using helium gas as the gas medium.
[0031] The (d) hollow inorganic filler preferably has a compressive fracture strength of 105 MPa or more, more preferably 108 MPa or more, and even more preferably 110 MPa or more. By making it equal to or greater than the lower limit, crushing during kneading with the resin tends to be suppressed, and the specific gravity of the molded product tends to be effectively reduced. The (d) hollow inorganic filler also preferably has a compressive fracture strength of 130 MPa or less. If it is equal to or greater than the upper limit, the shell thickness of the hollow particles becomes thick, and the effect of adding the filler to reduce the specific gravity tends to be poor. The compressive fracture strength of the hollow inorganic filler (d) is the hydrostatic pressure at which 10% by volume of the hollow inorganic filler is fractured, and is measured in a dispersion in glycerol using ASTM D3102-72 "Hydrostatic Disintegration Strength of Hollow Glass Microspheres."
[0032] The average particle size of the hollow inorganic filler (d) is the value of D50, and is preferably 5 μm or more, more preferably 10 μm or more, and even more preferably 15 μm or more, and is preferably 50 μm or less, more preferably 40 μm or less, and even more preferably 30 μm or less.
[0033] The content of the hollow inorganic filler (d) in the resin composition of this embodiment is 6 parts by mass or more, preferably 8 parts by mass or more, and may be 12 parts by mass or more in 100 parts by mass of the resin composition. By making it equal to or more than the lower limit, the specific gravity of the molded body tends to be effectively reduced. In addition, the upper limit of the content of the hollow inorganic filler (d) is 30 parts by mass or less in 100 parts by mass of the resin composition, and may be 28 parts by mass or less, 25 parts by mass or less, 20 parts by mass or less, 18 parts by mass or less, or 16 parts by mass or less depending on the application. By making it equal to or less than the upper limit, the decrease in impact resistance and mechanical strength of the molded body tends to be suppressed. The resin composition of the present embodiment may contain only one type of hollow inorganic filler (d), or may contain two or more types. When two or more types are contained, the total amount is preferably in the above range.
[0034] <(e) Block copolymer> The resin composition of this embodiment contains a block copolymer (e), which is a hydrogenated product containing a vinyl aromatic compound block (e1) and an isoprene polymer block (e2). The inclusion of the block copolymer (e) enhances the impact resistance of the resulting molded article and also functions as a compatibilizer. That is, the vinyl aromatic compound block (e1) enhances the compatibility with (a) polyphenylene ether resin, and the isoprene polymer block (e2) enhances the compatibility with (b) polypropylene homopolymer and (c) polyolefin copolymer. It is presumed that by using a hydrogenated product, the isoprene polymer block has an alternating copolymer structure of ethylene and propylene, which has good affinity with polypropylene homopolymer and leads to various good physical properties.
[0035] The vinyl aromatic compound constituting the vinyl aromatic compound block (e1) may be a vinyl allyl compound, preferably at least one selected from the group consisting of styrene, α-methylstyrene, styrene substituted with an alkoxy group, 2-vinylpyridine, 4-vinylpyridine, vinylnaphthalene, and vinylnaphthalene substituted with an alkyl group, more preferably styrene and α-methylstyrene, and even more preferably styrene. The vinyl aromatic compound may be one type or two or more types.
[0036] The content of the vinyl aromatic compound unit in the block copolymer (e) used in this embodiment is preferably 50% by mass or more, more preferably 55% by mass or more, even more preferably 60% by mass or more, and even more preferably 63% by mass or more. By making it equal to or more than the lower limit, the impact resistance of the obtained molded article can be effectively improved without decreasing the heat resistance. In addition, the content of the vinyl aromatic compound unit in the block copolymer (e) is preferably less than 80% by mass, more preferably 75% by mass or less, and even more preferably 70% by mass or less. By making it equal to or less than the upper limit, the impact resistance and nominal tensile strain of the obtained molded article tend to be improved.
[0037] The content of isoprene units in the block copolymer (e) used in this embodiment is preferably 20% by mass or more, more preferably 25% by mass or more, and even more preferably 30% by mass or more. By making it equal to or more than the lower limit, the impact resistance and nominal tensile strain of the obtained molded article tend to be further improved. In addition, the content of isoprene units in the block copolymer (e) is preferably 50% by mass or less, more preferably 47% by mass or less, even more preferably 40% by mass or less, and may be 35% by mass or less. By making it equal to or less than the upper limit, the impact resistance of the obtained molded article can be effectively improved without decreasing the heat resistance. This effect tends to be further improved.
[0038] In the block copolymer (e) used in the present embodiment, the total of the vinyl aromatic compound units and the isoprene units preferably accounts for 90 mass% or more of the block copolymer (e), and may be 95 mass% or more, or may be 99 mass% or more.
[0039] The block copolymer (e) used in this embodiment is preferably SEPS, which is represented by the following structural formula, where l, m, and n are each a number greater than 0. [ka]
[0040] The block copolymer (e) used in the present embodiment is a hydrogenated product, and may be a partially hydrogenated product or a fully hydrogenated product, with the fully hydrogenated product being preferred.
[0041] The content of the block copolymer (e) in the resin composition of this embodiment is preferably 5 parts by mass or more, more preferably 7 parts by mass or more, even more preferably 10 parts by mass or more, and even more preferably 13 parts by mass or more, relative to 100 parts by mass of the resin component. By making it equal to or more than the lower limit, the impact resistance of the molded article tends to be improved. In addition, the upper limit of the content of the block copolymer (e) is preferably 25 parts by mass or less, more preferably 20 parts by mass or less, even more preferably 17 parts by mass or less, and even more preferably 16 parts by mass or less, relative to 100 parts by mass of the resin composition. By making it equal to or less than the upper limit, the decrease in heat resistance tends to be suppressed. The resin composition of the present embodiment may contain only one type of (e) block copolymer, or may contain two or more types. When two or more types are contained, the total amount is preferably in the above range.
[0042] In this embodiment, the (e) block copolymer preferably flows when measured at a load of 2.16 kg and a temperature of 230° C. according to JISK7210. Specifically, the melt flow rate (MFR) measured at a load of 2.16 kg and a temperature of 230° C. according to JISK7210 is preferably 0.1 g / 10 min or more, more preferably 0.15 g / 10 min or more, and even more preferably 0.3 g / 10 min or more. By making it equal to or greater than the lower limit, the fluidity of the resin composition tends to be improved and the moldability tends to be further improved. In addition, the MFR is preferably 7.0 g / 10 min or less, more preferably 5.0 g / 10 min or less, even more preferably 3.0 g / 10 min or less, even more preferably 2.0 g / 10 min or less, and may be 1.0 g / 10 min or less. By making it equal to or less than the upper limit, the impact resistance tends to be further improved. The difference between the MFR of the block copolymer (e) and the MFR of the polypropylene homopolymer (b) (MFR(b)-MFR(e)) is preferably 1.0 g / 10 min or more and 3.0 g / 10 min or less. The difference between the MFR of the block copolymer (e) and the MFR of the polyolefin copolymer (c) (MFR(c)-MFR(e)) is preferably 0.1 g / 10 min or more and is preferably 10.0 g / 10 min or less. By setting the content within such a range, the effects of the present invention tend to be more effectively exhibited.
[0043] <(f) Low molecular weight polystyrene resin> In addition to the above components, the resin composition of the present embodiment preferably contains (f) a polystyrene resin having a weight average molecular weight (Mw) of 3,000 to 20,000 (hereinafter, simply referred to as "(f) low molecular weight polystyrene resin"). By containing (f) low molecular weight polystyrene resin, the impact resistance and bending strength of the obtained molded article tend to be improved. The weight average molecular weight of the (f) low molecular weight polystyrene resin is 3,000 or more, preferably 5,000 or more, more preferably 7,000 or more, and even more preferably 8,000 or more. Below the lower limit, mechanical properties such as tensile and bending properties of the entire resin composition tend to decrease. In addition, the weight average molecular weight of the (f) low molecular weight polystyrene resin is 20,000 or less, preferably 18,000 or less, more preferably 15,000 or less, and even more preferably 12,000 or less. By making it below the upper limit, the fluidity of the polyphenylene ether resin is increased, the dispersibility of the polyphenylene ether domain is improved, and the impact resistance of the obtained molded article tends to be improved. (f) The weight average molecular weight of the low molecular weight polystyrene resin is the polystyrene equivalent molecular weight obtained by gel permeation chromatography (GPC) measurement.
[0044] The (f) low-molecular-weight polystyrene resin used in this embodiment may be a styrene homopolymer (polystyrene) or a copolymer of styrene and another monomer. In this embodiment, the (f) low-molecular-weight polystyrene resin preferably contains styrene units in all of its constituent units at 50% by mass or more, more preferably at 70% by mass or more, and even more preferably at 90% by mass or more, and may contain 95% by mass or more. When the (f) low-molecular-weight polystyrene resin used in this embodiment is a copolymer of styrene and another monomer, examples of the copolymer include styrene-acrylic resin, acrylonitrile butadiene styrene resin, styrene-acrylonitrile resin, styrene-butadiene resin, and styrene-ethylene butadiene styrene resin.
[0045] When the resin composition of the present embodiment contains the low molecular weight polystyrene resin (f), the content is preferably 0.5 parts by mass or more, more preferably 1.0 parts by mass or more, and even more preferably 2.0 parts by mass or more, relative to 100 parts by mass of the resin components (the total of the components (a) to (c) and (e)) contained in the resin composition. By making the content equal to or more than the lower limit, the dispersibility of the polyphenylene ether domain is improved, and the impact resistance of the obtained molded body tends to be improved. In addition, the upper limit of the content of the low molecular weight polystyrene resin (f) is preferably 10.0 parts by mass or less, more preferably 7.0 parts by mass or less, even more preferably 6.0 parts by mass or less, even more preferably 5.0 parts by mass or less, even more preferably 4.5 parts by mass or less, and even more preferably 4.0 parts by mass or less, relative to 100 parts by mass of the resin composition. By making the content equal to or less than the upper limit, the deterioration of heat resistance and mechanical properties such as tensile properties and bending properties tends to be more effectively suppressed. The resin composition of the present embodiment may contain only one type of (f) low-molecular-weight polystyrene resin, or may contain two or more types. When two or more types are contained, the total amount is preferably in the above range.
[0046] <Other ingredients> The resin composition of the present embodiment may contain other components in addition to those described above. Specific examples of the resin include thermoplastic resins such as polyamide resin, polyester resin, polyphenylene sulfide resin, liquid crystal polyester resin, polycarbonate resin, polyacetal resin, polyacrylonitrile resin, acrylic resin, and polyethylene resin, and thermosetting resins such as epoxy resin, melamine resin, and silicone resin. These thermoplastic resins and thermosetting resins can also be used in combination of two or more kinds. The resin composition of the present embodiment may also contain resin additives. Specifically, the resin composition may contain stabilizers, colorants, internal lubricants (fatty acid metal salts, polyethylene wax, etc.), heat stabilizers (zinc oxide, etc.), release agents (silicone oils, fatty acids, fatty acid esters, etc.), weather resistance improvers, nucleating agents, impact resistance improvers, plasticizers, flow improvers, etc. When these components are contained, the total content of the resin composition is preferably within the range of 0.01 to 5 mass %.
[0047] The resin composition of the present embodiment is prepared so that the total amount of (a) polyphenylene ether resin, (b) polypropylene homopolymer, (c) polyolefin copolymer, (d) hollow inorganic filler, and (e) block copolymer, as well as other components blended as necessary, is 100 mass %. Furthermore, in the resin composition of the present embodiment, the total of (a) the polyphenylene ether resin, (b) the polypropylene homopolymer, (c) the polyolefin copolymer, (d) the hollow inorganic filler, and (e) the block copolymer preferably accounts for 92 mass% or more of the resin composition, more preferably 94 mass% or more, and even more preferably 96 mass% or more. In addition, in the resin composition of this embodiment, the total of (a) polyphenylene ether resin, (b) polypropylene homopolymer, (c) polyolefin copolymer, (d) hollow inorganic filler, and (e) block copolymer, as well as (f) low molecular weight polystyrene resin, stabilizer, and pigment which are blended as necessary, preferably accounts for 95 mass% or more of the resin composition, more preferably 97 mass% or more, and even more preferably 99 mass% or more.
[0048] <<Stabilizer>> The resin composition of the present embodiment may contain a stabilizer such as a heat stabilizer or an antioxidant. Examples of the stabilizer include inorganic heat stabilizers such as phenol-based stabilizers, amine-based stabilizers, phosphorus-based stabilizers, thioether-based stabilizers, and zinc oxide. Among them, in this embodiment, phenol-based stabilizers and zinc oxide are preferred. For the stabilizer, the descriptions in paragraph 0036 of International Publication No. 2019 / 026689 and paragraphs 0044 to 0046 of JP-A-2022-001624 can be referred to, and the contents thereof are incorporated herein.
[0049] As the phenol-based stabilizer, a hindered phenol-based stabilizer is preferably used. Specific examples of hindered phenol stabilizers include pentaerythritol tetrakis[3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate], octadecyl-3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate, thiodiethylene bis[3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate], N,N'-hexane-1,6-diylbis[3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionamide], 2,4-dimethyl-6-(1-methylpentadecyl)phenol, diethyl[[3,5-bis(1,1-dimethylethyl)-4-hydroxyphenyl]methyl]phosphate, 3,3',3'',5,5',5''-hexa-tert-butyl-a,a',a''-(mesityle) 4,6-bis(octylthiomethyl)-o-cresol, ethylene bis(oxyethylene) bis[3-(5-tert-butyl-4-hydroxy-m-tolyl)propionate], hexamethylene bis[3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate], 1,3,5-tris(3,5-di-tert-butyl -4-hydroxybenzyl)-1,3,5-triazine-2,4,6(1H,3H,5H)-trione, 2,6-di-tert-butyl-4-(4,6-bis(octylthio)-1,3,5-triazin-2-ylamino)phenol, 2-[1-(2-hydroxy-3,5-di-tert-pentylphenyl)ethyl]-4,6-di-tert-pentylphenyl acrylate, and the like.
[0050] Among them, pentaerythritol tetrakis[3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate] and octadecyl-3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate are preferred. Specific examples of such hindered phenol stabilizers include "Irganox (registered trademark, the same applies below) 1010" and "Irganox 1076" manufactured by BASF, and "Adeka STAB AO-50" and "Adeka STAB AO-60" manufactured by ADEKA.
[0051] The content of the stabilizer in the resin composition of this embodiment is, in 100 parts by mass of the resin composition, preferably 0.001 parts by mass or more, more preferably 0.005 parts by mass or more, even more preferably 0.01 parts by mass or more, and even more preferably 0.08 parts by mass or more, and is preferably 3 parts by mass or less, more preferably 2 parts by mass or less, and even more preferably 1 part by mass or less. By setting the content of the stabilizer in the above range, the effect of adding the stabilizer is more effectively exhibited. The resin composition of the present embodiment may contain only one type of stabilizer, or may contain two or more types. When two or more types are contained, the total amount is preferably in the above range.
[0052] <<Coloring agent>> The resin composition of the present embodiment may contain a colorant. By containing a colorant, the obtained molded article can be given a color, and the design property tends to be improved. The colorant may be either a pigment or a dye, but is preferably a pigment. Examples of pigments include inorganic pigments (black pigments such as carbon black, red pigments such as iron oxide red, orange pigments such as molybdate orange, white pigments such as titanium oxide), organic pigments (yellow pigments, orange pigments, red pigments, blue pigments, green pigments, etc.), and inorganic pigments are preferred, and carbon black is preferred for black pigments, and zinc sulfide is preferred for white pigments. Among white pigments, titanium oxide has high hardness and causes the crushing of the hollow inorganic filler (d), so it is preferable that it is substantially free of titanium oxide. Substantially free of titanium oxide means that the content of titanium oxide is, for example, less than 0.01 parts by mass in 100 parts by mass of the resin composition, preferably less than 0.005 parts by mass, more preferably less than 0.001 parts by mass, and even more preferably less than 0.0001 parts by mass. When a colorant is blended into the resin composition of the present embodiment, the colorant may be blended in the form of a master batch. When the resin composition in this embodiment contains a colorant, the content thereof is preferably 0.01 parts by mass or more, more preferably 0.1 parts by mass or more, even more preferably 0.3 parts by mass or more, and even more preferably 0.5 parts by mass or more, in 100 parts by mass of the resin composition, and may be 0.9 parts by mass or more when white streaks tend to appear in the molded product. The content of the colorant is preferably 10.0 parts by mass or less, more preferably 5.0 parts by mass or less, and even more preferably 3.0 parts by mass or less, in 100 parts by mass of the resin composition. The resin composition of the present embodiment may contain only one type of colorant, or may contain two or more types. When two or more types are contained, the total amount is preferably in the above range.
[0053] <Method of producing resin composition> As a method for producing the resin composition of the present embodiment, any method may be adopted. For example, the components (a) polyphenylene ether resin, (b) polypropylene homopolymer, (c) polyolefin copolymer, (d) hollow inorganic filler, and (e) block copolymer are mixed using a mixing means such as a V-type blender to prepare a lump-sum blend, which is then melt-kneaded in a vented extruder to form pellets. Alternatively, a two-stage kneading method may be used in which some components are thoroughly mixed in advance, and then melt-kneaded in a vented extruder to produce pellets, which are then mixed with other components, and melt-kneaded in a vented extruder. (d) The hollow inorganic filler may be side-fed.
[0054] <Characteristics of resin composition> The resin composition of the present embodiment can particularly satisfy the following properties. The resin composition of the present embodiment preferably has a small specific gravity. Specifically, the specific gravity of the resin composition of the present embodiment is 0.93 g / cm 3 It is preferable that the density is 0.92 g / cm or less. 3 More preferably, it is 0.91 g / cm or less. 3 More preferably, it is 0.90 g / cm or less. 3 More preferably, it is 0.89 g / cm or less. 3 It is even more preferable that the lower limit is 0.80 g / cm or less. 3 The above is practical, and 0.85g / cm 3 But it fully meets the performance requirements. The resin composition of the present embodiment preferably has excellent impact resistance. Specifically, the resin composition of the present embodiment is molded into an ISO test piece, and the notched Charpy impact strength in accordance with ISO-179-1 and ISO179-2 is 4.9 kJ / m 2 It is preferable that the concentration is 5.0 kJ / m or more. 2 More preferably, it is 5.3 kJ / m or more. 2 More preferably, it is 5.6 kJ / m or more. 2 More preferably, it is 5.8 kJ / m or more. 2It is more preferable that the upper limit is 12.0 kJ / m or more. There is no particular upper limit, but it is preferably 12.0 kJ / m 2 The following is practical. The resin composition of the present embodiment is preferably excellent in heat resistance. Specifically, the resin composition of the present embodiment is molded into an ISO test piece, and the deflection temperature under load of 1.80 MPa measured in accordance with ISO-75-2 is preferably 61° C. or higher, more preferably 70° C. or higher, even more preferably 75° C. or higher, even more preferably 78° C. or higher, and even more preferably 80° C. or higher. The upper limit is not particularly specified, but a practical value is 110° C. or lower. The Charpy impact strength and the deflection temperature under load are measured according to the description in the examples given later.
[0055] <Molding of resin composition> The resin composition of the present embodiment is used in the form of pellets, and the molded article of the present embodiment is formed from the resin composition or pellets of the present embodiment. In the present embodiment, the manufacturing method of the molded body is not particularly limited, and any molding method generally used for resin compositions can be used. Examples of such molding methods include injection molding, ultra-high speed injection molding, injection compression molding, two-color molding, gas-assisted hollow molding, molding using a heat-insulating mold, molding using a rapid heating mold, foam molding (including supercritical fluid), insert molding, IMC (in-mold coating molding) molding, extrusion molding, sheet molding, thermoforming, rotational molding, lamination molding, press molding, and blow molding. A molding method using a hot runner system can also be used.
[0056] <Applications of resin compositions, pellets, and molded articles> The resin composition, pellets, and molded article of this embodiment can be widely used in applications in which polyphenylene ether resins, in particular blends of polyphenylene ether resins and styrene-based resins, are generally used. For example, it is suitable for automobile exterior and exterior panel parts, automobile interior parts, and automobile underhood parts, such as bumpers, fenders, door panels, moldings, emblems, engine hoods, wheel covers, roofs, spoilers, engine covers, and other exterior and exterior panel parts, underhood parts, and interior parts such as instrument panels and console box trims. They can also be used as cabinets and chassis for various computers and their peripheral devices, other office automation equipment, televisions, videos, various disk players, refrigerators, air conditioners, liquid crystal projectors, and the like. Furthermore, the material can be used for fuel cases for solid methanol batteries, secondary battery containers, fuel cell water pipes, water-cooling tanks, boiler exterior cases, ink-peripheral parts and components and chassis for inkjet printers, as well as molded products such as water piping and joints. In this embodiment, it is particularly preferably used as a wearable terminal housing. EXAMPLES
[0057] The present invention will be described in more detail below with reference to examples. The materials, amounts, ratios, processing contents, processing procedures, etc. shown in the following examples can be appropriately changed without departing from the spirit of the present invention. Therefore, the scope of the present invention is not limited to the specific examples shown below. If the measuring instruments used in the examples are difficult to obtain due to discontinuation or the like, measurements can be made using other instruments with equivalent performance.
[0058] 1. Raw materials The following raw materials were used: [Table 1] [Table 2]
[0059] The above MFR means the melt flow rate measured in accordance with JIS-K7210 under a load of 2.16 kg and at a temperature of 230°C. The above-mentioned SEBS is a hydrogenated block copolymer composed of styrene and butadiene.
[0060] 2. Examples 1 to 14, Comparative Examples 1 to 5 Each component was mixed at the ratios (by parts by mass) shown in Tables 3 to 6 below, and melt kneading was performed at a cylinder temperature of 280°C and a screw rotation speed of 200 rpm using a twin-screw extruder (manufactured by Shibaura Machine Co., Ltd.: TEM26SX) to obtain a resin composition (pellets). Using the obtained resin composition (pellets), the following evaluations were carried out. The results are shown in Tables 3 to 6.
[0061] <Ash content> 2 g of the pellets obtained by the above manufacturing method were incinerated in accordance with JIS7250, Method A, and the ash content was measured. The unit of the ash content was expressed as mass%.
[0062] <Manufacture of ISO test piece> After drying the pellets obtained by the above manufacturing method at 100°C for 2 hours, an ISO-15103-compliant 4-mm-thick ISO3167:93 Type A test piece (hereinafter referred to as the "ISO test piece") was injection molded at a cylinder temperature of 270°C and a mold temperature of 70°C using an injection molding machine (manufactured by Shibaura Machine Co., Ltd., "EC75SX").
[0063] <Specific gravity> Using the test piece obtained by cutting the above-obtained ISO test piece, the specific gravity (g / cm 3 ) was measured according to Method A in accordance with JISK7112.
[0064] <Notched Charpy impact strength> The above-obtained ISO test piece was machined in accordance with ISO-179-1 and ISO179-2, the gripping parts at both ends were cut off, and a notch (cutout) was made in the center to form a notched Charpy impact test piece. For the obtained notched Charpy impact test piece, as an impact resistance evaluation, in accordance with ISO-179-1 and ISO179-2, the notched Charpy impact strength at 23°C (unit: kJ / m 2) was measured.
[0065] <Deflection temperature under load (DTUL)> In accordance with ISO-75-2, the deflection temperature under load (unit: °C) was measured at 1.80 MPa using a rectangular test piece of 80 mm x 10 mm x 4 mmt that was prepared by machining the parallel part of the ISO test piece obtained above.
[0066] <Tensile strength and nominal tensile strain> According to ISO-527, the tensile strength (unit: MPa) and nominal tensile strain (unit: %) were measured using the ISO test pieces obtained above.
[0067] <Flexural strength and flexural modulus> The parallel portion of the ISO test piece obtained above was machined to produce a rectangular test piece of 80 mm x 10 mm x 4 mmt, and the bending strength (unit: MPa) and bending modulus (unit: MPa) were measured in accordance with ISO-178 under an environment of temperature 23°C and humidity 50%.
[0068] [Table 3]
[0069] [Table 4]
[0070] [Table 5]
[0071] [Table 6]
[0072] As is clear from the above results, the resin composition of the present invention is a resin composition containing a polyphenylene ether resin and a hollow inorganic filler, and has a low specific gravity, and can provide a molded product having excellent impact resistance while maintaining heat resistance. Furthermore, the resin composition also has excellent tensile properties and bending properties.
Claims
1. (a) a polyphenylene ether resin; (b) a polypropylene homopolymer; and (c) a polyolefin copolymer having a melt flow rate (MFR) of 0.3 to 25 g / 10 min at a load of 2.16 kg and a temperature of 230° C., as measured in accordance with JIS-K7210; (d) a hollow inorganic filler; (e) a block copolymer; Including, The (c) polyolefin copolymer is a copolymer of two or more olefins, The (e) block copolymer is a hydrogenated product of a block copolymer containing a vinyl aromatic compound block (e1) and an isoprene polymer block (e2), The resin composition contains the hollow inorganic filler (d) in an amount of 6 to 30 parts by mass per 100 parts by mass of the resin composition.
2. The resin composition according to claim 1, comprising the hollow inorganic filler (d) in an amount of 6 to 20 parts by mass per 100 parts by mass of the resin composition.
3. The resin composition according to claim 1 or 2, wherein the hollow inorganic filler (d) has a compressive fracture strength of 105 to 130 MPa.
4. 3. The resin composition according to claim 1 or 2, comprising 40 to 65 mass% of the polyphenylene ether resin (a) and 35 to 60 mass% of the polypropylene homopolymer (b) and the polyolefin copolymer (c) relative to a total of 100 mass% of the polyphenylene ether resin (a), the polypropylene homopolymer (b), and the polyolefin copolymer (c).
5. The resin composition according to claim 1 or 2, further comprising (f) a polystyrene resin having a weight average molecular weight (Mw) of 3,000 to 20,000.
6. The resin composition according to claim 1 or 2, wherein the content of the vinyl aromatic compound unit in the block copolymer (e) is 50% by mass or more and less than 80% by mass.
7. (d) the hollow inorganic filler has a compressive fracture strength of 105 to 130 MPa; The composition contains 40 to 65 mass% of the polyphenylene ether resin (a) and 35 to 60 mass% of the polypropylene homopolymer (b) and the polyolefin copolymer (c) in total, relative to 100 mass% of the polyphenylene ether resin (a), the polypropylene homopolymer (b), and the polyolefin copolymer (c), Further, (f) a polystyrene resin having a weight average molecular weight (Mw) of 3,000 to 20,000, The resin composition according to claim 1 or 2, wherein the content of the vinyl aromatic compound unit in the block copolymer (e) is 50% by mass or more and less than 80% by mass.
8. A pellet of the resin composition according to claim 1 or 2.
9. A molded article molded from the resin composition according to claim 1 or 2.
10. A compact formed from the pellets according to claim 8.
Citation Information
Patent Citations
Resin composition
JP1988118344A
Thermoplastic resin composition having improved light discoloration
JP2004204013A
Thermoplastic resin composition and molded automobile exterior panel
JP2004285089A
Flexible poly(arylene ether) compositions and articles thereof
JP2008524381A
Resin composition, molded article, and method of manufacturing molded article
JP2016108372A