Laminated foam sheets and skin materials

The integration of a thermoplastic colored resin layer between the foam and surface layer in laminated foam sheets allows for enriched color and design on uneven patterns, addressing productivity issues in conventional methods.

JP7591110B2Active Publication Date: 2024-11-27INOAC CORP
View PDF 9 Cites 0 Cited by

Patent Information

Application Number
JP2023171250
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2023-10-02
Publication Date
2024-11-27
Estimated Expiration
2039-04-24

AI Technical Summary

Technical Problem

Conventional laminated foam sheets have limited decorative color options due to the need for precise alignment of colored skin materials with uneven patterns, which affects productivity.

Method used

A laminated foam sheet design where a thermoplastic colored resin layer is integrated between the foam and a surface layer with permeation parts, allowing the resin to penetrate and expose various colors on the uneven pattern during thermal compression.

Benefits of technology

Enriches the color and design of the uneven pattern without deviation, enabling a variety of colors and maintaining a predetermined design.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007591110000001
    Figure 0007591110000001
  • Figure 0007591110000002
    Figure 0007591110000002
  • Figure 0007591110000003
    Figure 0007591110000003
Patent Text Reader

Abstract

To provide a laminated foam sheet in which an uneven pattern formed by thermal compression molding can have a variety of colors, and a method for producing the same.SOLUTION: A skin material 14 in which a thermoplastic colored resin layer 20 is formed on a surface sheet body 16 having a permeation part 18 that communicates between front and back sides so as to match at least a formation position of the permeation part 18, is laminated so that the colored resin layer 20 is located on a foam 12 side. Then, A formation position of the permeation part 18 in the skin material 14 is thermally compressed to form a recessed part 11a having an uneven pattern, and the colored resin layer 20 melted during the thermal compression is allowed to permeate into the permeation part 18 of the surface sheet body 16 and exposed on a surface of the recessed part 11a.SELECTED DRAWING: Figure 4
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a laminated foam sheet obtained by laminating a skin material onto a foam and forming an uneven pattern on the surface thereof, and to a method for producing the same. [Background technology]

[0002] Surface materials are provided on the surfaces of automobile and motorcycle seats, vehicle interior materials such as door trims and instrument panels, and furniture such as chairs and sofas for the purpose of decorating and protecting the target components, and a laminated foam sheet having an uneven surface pattern is known as such a surface material. Such a laminated foam sheet is produced by laminating a flexible skin material onto a soft polyurethane foam, and then thermally compressing the surface with a heating and compressing device having an uneven surface pattern formed thereon (Patent Document 1). [Prior art documents] [Patent documents]

[0003] [Patent Document 1] JP 2014-184580 A Summary of the Invention [Problem to be solved by the invention]

[0004] Incidentally, conventional laminated foam sheets can realize three-dimensional designs utilizing the shadows and the like generated by the uneven pattern on the surface. However, conventional laminated foam sheets have monotonous colors depending on the material used for the skin material, and the decorativeness of the uneven pattern is limited. Here, although it is possible to enrich the color of the uneven pattern of the laminated foam sheet by using a skin material with an appropriate color pattern and performing heat compression, it is necessary to process the color pattern imparted to the skin material and the uneven pattern formed by heat compression in a precise alignment, and the requirement of precise processing causes a problem of difficulty in productivity.

[0005] That is, an object of the present invention is to provide a laminated foam sheet capable of enriching the color of the surface of the uneven pattern, and a method for producing the same. [Means for solving the problem]

[0006] In order to overcome the above problems and achieve the intended object, the first invention provides: A laminated foam sheet in which a skin material is laminated on one side of a foam and an uneven pattern is formed on the skin material side by thermal compression molding, the skin material comprises a surface layer having a permeation portion that connects at least the concave portions of the uneven pattern to the front and back, and a thermoplastic colored resin layer located at the formation position of the permeation portion in the surface layer and between the foam body, The colored resin layer melted during thermal compression molding permeates the permeation portion of the surface layer and is exposed on the surface of the recess. In this way, the colored resin layer melted during the thermal compression molding penetrates into the penetration part of the surface layer and is exposed on the surface of the recessed parts, so that the uneven pattern can be made to have a variety of colors, making it possible to enrich the design. Also, since the colored resin layer penetrates into the penetration part of the surface layer and colors the surface of the recessed parts, the three-dimensional uneven pattern and the color pattern do not shift, and a desired design can be realized.

[0007] The second invention is The surface layer is a fibrous sheet body in which the penetration portion is formed between the fibers, and the colored resin layer melted during thermal compression molding penetrates between the fibers of the sheet body and is exposed on the surface. In this way, the color of the uneven pattern of the laminated foam sheet whose surface is decorated with a fiber sheet body can be made diverse.

[0008] The third invention is The surface layer is a sheet body having holes formed therethrough as the infiltration portions in accordance with the positions at which the recesses of the uneven pattern are formed, and the colored resin material melted during thermal compression molding infiltrates into the holes of the sheet body and is exposed on the surface. In this way, even if the surface layer is made of a material that the molten colored resin layer cannot penetrate, the colored resin layer that penetrates into the holes in the surface layer and is exposed on the surface of the recesses can add variety to the colors of the uneven pattern, thereby enriching the design.

[0009] The fourth invention is A method for producing a laminated foam sheet, comprising laminating a skin material on one side of a foam and forming a concave-convex pattern on the skin material side by thermal compression molding, comprising the steps of: The skin material is formed by forming a thermoplastic colored resin layer on a surface layer having a permeation portion that connects the front and back of the skin material so that the colored resin layer is located on the foam side. The position where the penetration portion in the skin material is to be formed is thermally compressed to form recesses of the uneven pattern, and the colored resin layer melted during the thermal compression is allowed to penetrate into the penetration portion of the skin material and be exposed on the surface of the recesses. In this way, the colored resin layer melted during the thermal compression molding penetrates the penetration part of the surface layer and is exposed on the surface of the recesses, so that the uneven pattern can be rich in color and design. Also, because the colored resin layer penetrates the penetration part of the surface layer and colors the surface of the recesses, the three-dimensional uneven pattern and the color pattern do not shift, and a desired design can be realized.

[0010] The fifth invention is The surface layer is a fibrous sheet body in which the penetration portion is formed between the fibers, and the colored resin layer melts during thermal compression and penetrates between the fibers of the sheet body, causing it to be exposed on the surface. In this way, the uneven pattern of the laminated foam sheet having a fibrous sheet body as a surface layer can be made colorful.

[0011] The sixth invention is The surface layer is a sheet body having holes formed therethrough as the penetration portion, and the colored resin layer melted during thermal compression is allowed to penetrate into the holes of the skin material and be exposed on the surface. In this way, even if the surface layer is made of a material that the molten colored resin layer cannot penetrate, the colored resin layer that penetrates into the holes in the surface layer and is exposed on the surface of the recesses can enrich the design by giving the uneven pattern a variety of colors.

[0012] The seventh invention is The method comprises applying molten colored resin to a mold in a predetermined thickness, placing a sheet body that forms the surface layer on top of the molten colored resin, and cooling and hardening the colored resin to form the skin material. In this way, by overlapping a sheet body forming a surface layer on the molten colored resin, the surface layer and the colored resin layer can be reliably integrated, so that the molten colored resin layer can be reliably penetrated into the penetration portion of the surface layer during thermal compression molding and exposed on the surface of the recess.

[0013] The eighth invention is The gist of the invention is that a transparent hot melt film is laminated between a sheet body forming the surface layer and a colored resin sheet of a predetermined thickness, and the skin material is formed by melting the hot melt film. In this way, the surface layer and the colored resin layer can be reliably integrated by the hot melt film, so that the colored resin layer melted during the thermal compression molding can be reliably permeated into the permeation portion of the surface layer and exposed on the surface of the recessed portion. In addition, by using a transparent hot melt film, the surface of the recessed portion can be colored in a color corresponding to the color of the colored resin layer. Effect of the Invention

[0014] According to the laminated foam sheet and the manufacturing method thereof of the present invention, it is possible to enrich the color of the surface of the uneven pattern. [Brief description of the drawings]

[0015] [Figure 1]FIG. 1(a) is a schematic diagram showing a laminated foam sheet using a fiber surface sheet as a skin material, FIG. 1(b) is a schematic diagram showing the state before thermal compression in which a skin material using a fiber surface sheet and a foam are laminated, and FIG. 1(c) is a schematic diagram showing the state in which a molten colored resin layer has penetrated into the penetration portion of the surface layer during thermal compression molding. [Diagram 2] FIG. 1(a) is a schematic diagram showing a laminated foam sheet using a sheet of synthetic leather or the like as a skin material, FIG. 1(b) is a schematic diagram showing the state before thermal compression in which a skin material using a surface sheet of synthetic leather or the like and a foam are laminated, and FIG. 1(c) is a schematic diagram showing the state in which a molten colored resin layer has penetrated into the penetration portion of the surface layer during thermal compression molding. [Diagram 3] FIG. 1 is a schematic diagram showing a laminate of a skin material and a foam before thermal compression, in which (a) shows a laminate of the skin material and the foam using a fiber surface sheet, (b) shows a state in which the skin material in which the perforated surface sheet is laminated to a colored resin layer is laminated to the foam, and (c) shows a state in which the skin material in which the surface sheet and the colored resin layer are perforated is laminated to the foam. [Figure 4] FIG. 1 is a schematic diagram showing a manufacturing process for a laminated foam sheet, in which (a) shows a laminate of a skin material and a foam using a fiber surface sheet placed on the base of a heating and compression device, and (b) shows the laminate of (a) being thermally compressed. [Diagram 5] FIG. 1 is a schematic diagram showing the manufacturing process of a laminated foam sheet, in which (a) shows a laminate of a perforated skin material and a foam on a surface sheet body, the laminate being placed on the base of a heating and compressing device, and (b) shows the laminate of (a) being thermally compressed. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0016] Next, the laminated foam sheet and the manufacturing method thereof according to the present invention will be described below with reference to the accompanying drawings. In this embodiment, a laminated foam sheet suitable for use as a cover for a seat of a vehicle such as an automobile and a manufacturing method thereof will be described as an example.

[0017] As shown in Figs. 1 and 2, the laminated foam sheet 10 has a skin material 14 laminated on one side of a foam 12, and the foam 12 is crushed on the skin material 14 side by thermal compression molding to form an uneven pattern. The skin material 14 of the laminated foam sheet 10 has a surface layer 16 exposed on the surface of the sheet 10 and a thermoplastic colored resin layer 20 provided so as to be positioned at the formation position of the recesses 11a forming the uneven pattern in the surface layer 16 and between the foam 12, in a laminated form, and is configured so that the colored resin layer 20 melted during thermal compression molding penetrates the penetration portion 18 of the skin material 14 and is exposed on the surface of the recesses 11a. The uneven pattern of the laminated foam sheet 10 is formed by crushing the foam 12 by thermal compression molding, and can be formed in any shape depending on the design, such as a regular pattern such as a lattice pattern, or a pattern like an animal or plant. The height of the convex portions 11b (depth of the concave portions 11a) of the uneven pattern is not particularly limited, but is preferably about 3 to 30 mm. The height of the convex portions 11b (depth of the concave portions 11a) of the uneven pattern does not need to be constant, and the height of the convex portions 11b (depth of the concave portions 11a) may be varied depending on the design, etc. In FIG. 1 and other figures, the height of the convex portions 11b (depth of the concave portions 11a) is constant for the sake of convenience of explanation.

[0018] As the foam 12 of the laminated foam sheet 10, various types of conventionally known foams 12 such as soft polyurethane foam, polyethylene foam, EVA foam, etc. can be used. The foam 12 may be composed of one type of foam 12, or may be composed by laminating a plurality of foams 12. As the foam 12, it is preferable to use a soft polyurethane foam, which has excellent cushioning properties and durability and can easily form an uneven pattern by thermal compression molding. Such a soft polyurethane foam is formed by a known method in which polyurethane raw materials including polyol, blowing agent, catalyst, foam stabilizer, polyisocyanate, and appropriate additives (flame retardant, ester additive, etc.) are mixed in a mixer and reacted to foam.

[0019] The thickness of the foam 12 is not particularly limited, but is preferably about 5 to 30 mm. In particular, by making the foam 12 10 mm or more thick, the three-dimensional effect of the uneven pattern formed by thermal compression molding can be enhanced, and the laminated foam sheet 10 can be made to have excellent design. For example, a soft polyurethane foam as the foam 12 can be formed by cutting a soft slab foam 12 obtained by foaming a polyurethane raw material at room temperature and atmospheric pressure to a predetermined thickness. By cutting such a soft slab foam 12 to a predetermined thickness, the foam 12 can be obtained efficiently.

[0020] The skin material 14 comprises a surface sheet body (surface layer) 16 having permeation portions 18 at least in the recesses 11a of the uneven pattern, and a thermoplastic colored resin layer 20 provided so as to be positioned at the formation positions of the recesses 11a of the uneven pattern in the surface sheet body 16 and between the foam 12. For this surface sheet body 16, a fiber sheet body mainly made of fibers such as flexible and stretchable knitted fabric, woven fabric, or nonwoven fabric, or a sheet body such as synthetic leather or natural leather can be suitably used.

[0021] Specifically, the fiber surface sheet body 16 is preferably a knitted fabric such as tricot, jersey, double raschel, woven fabric or nonwoven fabric made of fibers containing elastic fibers having elasticity, a nonwoven fabric raw material with many embossed parts formed thereon that is stretched to give elasticity, or a needle punched nonwoven fabric with excellent elasticity obtained by spirally crimping fibers. In addition, the fiber used for the fiber sheet body may be natural fibers such as cotton, hemp, or wool, or synthetic fibers such as rayon, acetate, polyamide, polyacrylonitrile, polyethylene terephthalate, or vinylon. Such a fiber sheet body may be preferably one having air permeability in which a permeation part 18 that connects the front and back is formed by the gap between the fibers, and the colored resin layer 20 melted during the thermal compression molding may be permeated into the permeation part 18 between the fibers to be exposed on the surface. When a fibrous sheet body that does not have sufficient permeation parts 18 between the fibers is used, holes are formed as the permeation parts 18 in the fibrous sheet body by hole punching or the like as described below, so that the colored resin layer 20 melted during thermal compression molding can permeate into the permeation parts 18 between the fibers and be exposed on the surface. The symbol TE in Figs. 1 and 4 indicates a colored part formed by the permeation of the molten colored resin layer 20 into the permeation parts 18 between the fibers.

[0022] The surface sheet body 16 of synthetic leather can be formed by a conventionally known method of impregnating and coating a base material made of knitted fabric, woven fabric, nonwoven fabric, etc. with a synthetic resin such as polyvinyl chloride or thermosetting polyurethane. Such a sheet body of synthetic leather or natural leather is configured so that holes are formed as the permeation parts 18 by a perforation process or the like as described below, and the molten colored resin layer 20 is permeated into the holes as the permeation parts 18 during thermal compression molding and exposed on the surface. The symbol TE in Figs. 2 and 5 indicates a colored part formed by the permeation of the molten colored resin layer 20 into the holes as the permeation parts 18.

[0023] The colored resin layer 20 is formed of a thermoplastic synthetic resin, and is formed into an appropriate color by kneading a colorant or pigment of an appropriate color with the synthetic resin using a mixer. The synthetic resin forming the colored resin layer 20 is not particularly limited, and polyethylene, polyvinyl chloride, polyethylene terephthalate, or other conventionally known thermoplastic synthetic resins can be used. The colored resin layer 20 may be formed of a solid layer of synthetic resin, or may be formed of a foamed synthetic resin. The thickness of the colored resin layer 20 is not particularly limited, but can be determined according to the thickness of the surface sheet body 16 so that the colored resin layer 20 melted during thermal compression molding can penetrate the penetration portion 18 of the surface sheet body 16 and be exposed on the surface of the recess 11a. Specifically, the colored resin layer 20 is preferably formed to be 1 / 4 to 2 times the thickness of the surface sheet body 16, and more preferably 1 / 2 to 1.5 times the thickness of the colored resin layer 20. By forming the colored resin layer 20 in such a range, the molten colored resin layer 20 can be reliably permeated into the surface of the top sheet body 16, and a predetermined color can be imparted to the uneven pattern. A synthetic resin having a lower melting point than the synthetic fibers, synthetic leather, etc., that form the top sheet body 16 is used for this colored resin layer 20. By forming the colored resin layer 20 from a material having a lower melting point than the top sheet body 16, the colored resin layer 20 can be melted without melting the top sheet body 16 during thermal compression molding, and the colored resin layer 20 can be permeated into the permeated portion 18 of the top sheet body 16.

[0024] Depending on the application of the laminated foam sheet 10, the skin material 14 may have a backing layer (not shown) laminated on the side of the colored resin layer 20 opposite the surface sheet body 16. Such a backing layer may be made of a woven fabric, nonwoven fabric, or synthetic resin sheet with low elasticity. By providing the backing layer, the skin material 14 can be given a so-called firm texture.

[0025] 1 to 5, the laminated foam sheet 10 having a concave-convex pattern on its surface may have a backing fabric 22 laminated on the back surface of the foam 12, which is the side opposite to the skin material 14. For such a backing fabric 22, it is preferable to use a woven or nonwoven fabric with low elasticity, and more preferably a fabric with a basis weight of 30 g / m 2 Among the above nylon or polyester nonwoven fabrics, woven fabrics, and knitted fabrics, queen knitted fabrics are preferred. The presence of a backing fabric with little stretch gives the laminated foam sheet 10 a firm feel, and weakens the force that causes the unevenly shaped soft polyurethane foam to return to a smooth shape.

[0026] Next, a method for producing the laminated foam sheet 10 according to this embodiment will be described.

[0027] The method for manufacturing the laminated foam sheet 10 of this embodiment includes a skin material formation step of forming a skin material 14, a laminate formation step of forming a laminate 24 by laminating the skin material 14 on the foam 12, and a concave-convex pattern formation step of forming a concave-convex pattern on the skin material 14 side of the laminate 24.

[0028] The skin forming process is a process for forming a skin 14 by laminating a thermoplastic colored resin layer 20 at least in accordance with the formation position of the permeation portion 18 on a surface sheet body 16 having a permeation portion 18 that connects the front and back. As a first example of the skin forming process, a synthetic resin colored in a predetermined color is melted and applied to a mold to a predetermined thickness by an application device such as a coater, and the surface sheet body 16 is placed on the molten synthetic resin, and the synthetic resin is cooled and hardened, and then removed from the mold, thereby forming a skin 14 in which the surface sheet body 16 and the colored resin layer 20 are laminated. That is, by placing the surface sheet body 16 on the molten synthetic resin and cooling and hardening it, the synthetic resin itself can function as an adhesive to be integrated. Note that the skin 14 can be easily removed from the mold by applying the molten synthetic resin on a release material placed on the mold. Furthermore, the skin material 14 provided with a lining layer can be formed by applying molten synthetic resin to the woven fabric, nonwoven fabric, or synthetic resin sheet that will form the lining layer while it is placed in a mold, and then placing the surface sheet body 16 on top in the same manner as described above and allowing the synthetic resin to cool and harden.

[0029] In addition, as a second example of the skin material forming process, a transparent hot melt film is placed on one side of a colored sheet formed of a synthetic resin colored in a predetermined color to a predetermined thickness, and a surface sheet body 16 is placed on the hot melt film, and the hot melt film is melted in this state to bond the colored sheet and the surface sheet body 16, thereby forming a skin material 14 in which the surface sheet body 16 and the colored resin layer 20 are laminated. This hot melt film can be melted by high-frequency heating, ultrasonic sealing, heat pressing, etc. In addition, the hot melt film can be various conventionally known films such as polyacrylic, polyolefin, polyester, etc., and can be appropriately selected according to the material of the surface sheet body 16 and the colored sheet to be bonded. In addition, it is preferable to adopt a hot melt film having a lower melting point than the colored sheet. In this way, by adopting a hot melt film having a lower melting point than the colored sheet, it is possible to prevent the colored sheet from melting in the process of melting the hot melt film. The skin material 14 provided with a backing layer can be formed by placing a hot melt film on a backing layer such as a woven fabric, nonwoven fabric, or synthetic resin sheet, placing a colored sheet on the hot melt film, and then placing a transparent hot melt film and the surface sheet body 16 on the colored sheet in the same manner as above, and melting each hot melt film. The hot melt film between the backing layer and the colored resin layer 20 does not have to be transparent.

[0030] In the skin forming process, a hole punching process is performed to form holes as permeation parts 18 that connect the front and back of the surface sheet body 16 according to the material of the surface sheet body 16 used and the position and shape according to the design of the color to be applied to the surface of the surface sheet body 16. This hole punching process can be performed either before or after the surface sheet body 16 and the colored resin layer 20 are integrated together. That is, the surface sheet body 16 that has been previously punched with a hole punching device can be placed so as to be overlaid on the molten synthetic resin or colored sheet as described above, or the permeation parts 18 can be formed in the surface sheet body 16 of the skin material 14 by punching the surface sheet body 16 and the colored resin layer 20 laminated together with a hole punching device. In this way, by overlapping the surface sheet body 16, which has been previously perforated, on the molten synthetic resin or colored sheet as described above, a skin material 14 in which the permeation portion 18 is formed only in the surface sheet body 16 can be formed as shown in FIG. 3(b), and by perforating the surface sheet body 16 and the colored resin layer 20 laminated together, a skin material 14 in which the permeation portion 18 is formed in each of the surface sheet body 16 and the colored layer can be formed as shown in FIG. 3(c). The holes as the permeation portion 18 formed in the surface sheet body 16 can be formed in an appropriate position and shape depending on the design of the laminated foam sheet 10 to be finally obtained. In addition, when a fiber sheet body in which gaps that connect the front and back are formed between the fibers is used as the surface sheet body 16, the perforation process can be omitted and the gaps between the fibers can be used as the permeation portion 18 (FIG. 3(a)). When perforation processing is performed on a surface sheet body 16 in which gaps are formed between the fibers that connect the front and back, the difference in shape and size of the permeation portions 18 formed by the gaps (permeation portions 18) formed between the fibers and the holes (permeation portions 18) formed by the perforation processing can enrich the variety of colors exposed on the surface.

[0031] In the laminate formation process, as shown in Fig. 3, the skin material 14 is laminated on the foam 12 with the surface sheet 16 facing outward to form a laminate 24. In this laminate formation process, the skin material 14 may be integrated with one side of the foam 12 by a known integration method such as frame lamination, lamination using an adhesive, etc. Here, in a configuration in which a lining layer is not provided, or a configuration in which a lining layer is provided but the surface sheet 16 and the colored resin layer 20 are integrated and then holes are opened to form the infiltration portion 18, the skin material 14 and the foam 12 can be integrated by the molten colored resin layer 20 during thermal compression molding, and integration by frame lamination or the like can be omitted.

[0032] Here, the frame lamination is a method in which the surface of the foam 12 is melted by irradiation of a flame burner or the like, and the skin material 14 is laminated and welded to the melted surface. The temperature of the flame burner or the like is generally about 600 to 1300°C. The lamination using an adhesive is a method in which an adhesive is applied to at least one of the adhesive surfaces of the foam 12 and the skin material 14, and the foam 12 and the skin material 14 are laminated and bonded so that the adhesive-applied surface is sandwiched between them. As the adhesive, a hot melt adhesive or the like is used. In addition, when the backing fabric 22 is used, the other surface of the foam 12 is melted by a flame burner or the like, and the backing fabric 22 is welded to the melted surface, or the backing fabric is bonded to the other surface of the foam 12 with an adhesive.

[0033] In the uneven pattern forming process, the surface of the skin material 14 of the laminate 24, in which the skin material 14 and the foam 12 are laminated, is thermally compressed by a heating and compressing device 26 having a surface formed with an uneven pattern, thereby crushing the foam 12 and forming the uneven pattern. Examples of thermal compression using the heating and compressing device 26 having a surface formed with an uneven pattern include a heat press method using a compression molding die having a surface formed with an uneven pattern and a roll heat compression method using an embossing roll.

[0034] The heat pressing method will be described. In the heat pressing method, as shown in FIG. 4 or FIG. 5, the laminate 24 is placed between a compression mold 30 formed into a desired uneven shape and a base 28 with the skin material 14 facing the compression mold 30. Then, the convex portion 30a of the compression mold 30 heated to a temperature at which the colored resin layer 20 of the skin material 14 melts by a heating means such as an electric heating wire (not shown) is pressed against the position where the permeation portion 18 is formed in the skin material 14 (surface sheet body 16) to perform heat compression, whereby the foam 12 is crushed and a concave portion 11a is formed on the surface of the laminate 24 to form an uneven pattern. In this way, the colored resin layer 20 is melted by pressing the convex portion 30a of the heated compression mold 30 against the base 28 to perform heat compression, and the molten colored resin layer 20 is permeated into the permeation portion 18 of the surface sheet body 16. Thereafter, the compression mold 30 is separated from the laminate 24 to harden the molten colored resin layer 20, thereby producing a laminated foam sheet 10 in which the recesses 11a formed on the surface of the laminate 24 are exposed on the surface and the recesses 11a of the uneven pattern are colored with the color of the colored resin layer 20. Here, the heating temperature of the compression mold 30 is not particularly limited, but is preferably 170 to 210°C. The thermal compression may be performed for a time that allows the colored resin layer 20 to melt and permeate into the permeation portion 18 of the surface sheet member 16, and is preferably 60 to 400 seconds.

[0035] On the other hand, in the roll heat compression method, the skin material 14 is heated at a temperature at which the colored resin layer 20 melts, and the laminate 24 is continuously fed to an embossing roll (not shown) having a convex portion on its surface to heat-compress the skin material 14, whereby the foam 12 is crushed to form an uneven pattern on the surface of the laminate 24. In this way, the colored resin layer 20 is melted by pressing the convex portion of the heated embossing roll against the laminate 24 and heat-compressing the laminate 24, and the molten colored resin layer 20 is permeated into the permeation portion 18 of the surface layer. Thereafter, the colored resin layer 20 of the laminate 24 sent out from the embossing roll is hardened, and is exposed on the surface of the concave portion 11a formed on the surface of the laminate 24, so that the laminated foam sheet 10 in which the concave portion 11a of the concave portion pattern is colored with the color of the colored resin layer 20 can be manufactured. Here, the heating temperature of the embossing roll is not particularly limited, but is preferably 180 to 220°C. The feed speed (feed rate) of the laminate 24 to the embossing roll may be any speed at which the colored resin layer 20 can melt and permeate into the permeation portion 18 while being pressed against the convex portions of the embossing roll for thermal compression, and is preferably about 1 to 10 m / min. In either case of the thermal press method or the roll thermal compression method, the molten colored resin layer 20 may be hardened by natural cooling, or the molten colored resin layer 20 may be hardened by cooling with a cooling means (not shown) such as a blower.

[0036] In this way, in the laminated foam sheet 10 according to the present invention, the colored resin layer 20 melted during thermal compression molding permeates the permeation portion 18 of the surface sheet body 16 and is exposed on the surface of the recesses 11a, so that the color of the uneven pattern can be varied to produce a laminated foam sheet 10 with a high design quality. In addition, since the colored resin layer 20 permeates the permeation portion 18 of the surface sheet body 16 and colors the surface of the recesses 11a of the uneven pattern, the three-dimensional uneven pattern and the color pattern do not shift, and a desired design can be realized. In this case, by using a fiber sheet body as the surface sheet body 16 as shown in FIG. 1 or FIG. 4, the color of the uneven pattern of the laminated foam sheet 10 whose surface is decorated with a fiber sheet body can be varied. 2 or 5, even if the surface sheet body 16 is made of a material that the molten colored resin layer 20 cannot penetrate, such as synthetic leather, the colored resin layer 20 penetrates into the holes formed in the surface sheet body 16 and is exposed on the surface of the recesses 11a, making it possible to provide a laminated foam sheet 10 with a highly designed texture by providing a variety of colors for the uneven pattern. Also, as shown in FIG. 2 or 5, the molten colored resin layer 20 does not penetrate into holes provided in positions that are not thermally compressed, making it possible to provide a greater variety of colors for the laminated foam sheet 10. The same applies when a fiber sheet body is used as the surface sheet body 16.

[0037] In addition, by applying a molten colored resin to a mold with a predetermined thickness, placing the surface sheet body 16 on the molten colored resin, and cooling and hardening the colored resin to form the skin material 14, the surface sheet body 16 and the colored resin layer 20 can be reliably integrated in a state that matches the formation position of the permeation portion 18 of the surface sheet body 16, so that the colored resin layer 20 melted during thermal compression molding can be reliably permeated into the permeation portion 18 of the surface sheet body 16 and exposed on the surface of the recess 11a. Similarly, when the surface sheet body 16 and the colored resin layer 20 are reliably integrated by a hot melt film, the surface sheet body 16 and the colored resin layer 20 can be reliably integrated in a state that matches the formation position of the permeation portion 18 of the surface sheet body 16, so that the colored resin layer 20 melted during thermal compression molding can be reliably permeated into the permeation portion 18 of the surface sheet body 16 and exposed on the surface of the recess 11a. In addition, by using a transparent hot melt film, the surface of the recess 11a can be colored in a color corresponding to the color of the colored resin layer 20. [Explanation of symbols]

[0038] 10 laminated foam sheet, 12 foam, 14 skin material, 16 surface sheet body (surface layer) 18 Permeation portion (gaps between fibers, holes), 20 Colored resin layer

Claims

1. A laminated foam sheet in which a skin material is laminated on one side of a foam and an uneven pattern is formed on the skin material side by thermal compression molding, The skin material has a surface layer having a permeation portion that penetrates at least the recesses of the uneven pattern from the front to the back, a thermoplastic colored resin layer located at a position where the infiltrated portion is formed in the surface layer and between the foam body, The penetration portion forms a space communicating with the front and back of the surface layer, A laminated foam sheet, characterized in that the resin of the colored resin layer melted during thermal compression molding permeates into the spaces and is exposed on the surfaces of the recesses.

2. A laminated foam sheet in which a skin material is laminated on one side of a foam and an uneven pattern is formed on the skin material side by thermal compression molding, The skin material includes a surface layer of a fiber sheet body that forms spaces between the fibers, a thermoplastic colored resin layer on the foam side of the surface layer, A laminated foam sheet, characterized in that the resin of the colored resin layer melted during thermal compression molding permeates into the spaces between the fibers and is exposed on the surfaces of the recesses of the uneven pattern.

3. A skin material laminated to a foam body, comprising: A surface layer; A thermoplastic colored resin layer is laminated on the back surface of the surface layer, The surface layer is (1) Having a through-hole that penetrates from the front to the back and through which the resin of the colored resin layer can penetrate, or (2) The sheet is made of a fiber through which the resin of the colored resin layer can permeate. Skin material.

4. The skin material according to claim 3; a foam laminated on the colored resin layer of the skin material; A laminated foam sheet comprising:

Citation Information

Patent Citations

  • Decorative textured sheet production method

    JP1978114861A

  • Interior material

    JP1985094940U

  • Change-color synthetic resin laminated sheet

    JP1988135236A

  • Bag foundation cloth, its manufacture and bag using the cloth

    JP2000079010A

  • Method for manufacturing pattern sheet

    JP2002316365A