Artificial graphite and its manufacturing method, and secondary battery and power consumption device containing the artificial graphite

Artificial graphite with controlled density and particle size, produced through a specialized process, addresses the volumetric expansion issue in secondary batteries, enhancing energy density and safety by improving particle bonding and electrolyte infiltration.

JP7591139B2Active Publication Date: 2024-11-27CONTEMPORARY AMPEREX TECHNOLOGY (HONG KONG) LIMITED
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
JP2023522555
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2021-12-24
Publication Date
2024-11-27
Estimated Expiration
2041-12-24

AI Technical Summary

Technical Problem

Secondary batteries experience volumetric expansion during the cycling process due to the change in volume of the negative electrode active material, leading to increased internal stress, reduced energy density, and compromised safety and service life.

Method used

The use of artificial graphite with specific properties, including a powder compaction density and volume distribution particle size ratio of A≧0.5, combined with a manufacturing process involving crushing, granulation, graphitization, and mechanofusion, to produce rounded particles that enhance bonding force and reduce electrode expansion.

Benefits of technology

The artificial graphite significantly reduces volumetric expansion, maintains high energy density, improves safety performance, and extends the cycle life of secondary batteries by enhancing particle bonding and electrolyte infiltration.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007591139000004
    Figure 0007591139000004
  • Figure 0007591139000005
    Figure 0007591139000005
  • Figure 0007591139000006
    Figure 0007591139000006
Patent Text Reader

Abstract

The present application provides artificial graphite and a method for producing the same, as well as a secondary battery and a power consuming device including the artificial graphite. The artificial graphite contains secondary particles and satisfies A≧0.5, where A is the powder compaction density of the artificial graphite at a pressure of 2t and its volume distribution particle size D v This is a ratio of 1. The secondary battery according to the present application can have low cycle volume expansion while maintaining high energy density.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present application relates to the field of secondary battery technology, and in particular to artificial graphite and its manufacturing method, as well as secondary batteries and power consuming devices containing the artificial graphite. [Background technology]

[0002] Secondary batteries are widely used due to their excellent characteristics such as high energy density, non-pollution, and long service life.

[0003] However, in secondary batteries, the volume of the negative electrode active material changes during the continuous charging and discharging of lithium, for example, volume expansion occurs during the cycle process, which increases the internal stress of the battery and thereby affects the service life and safety performance of the battery. Recently, with the rapid popularization of new energy vehicles, the market has increasingly higher requirements for the service life and safety performance of power-type secondary batteries. Therefore, in order to increase the market competitiveness of new energy vehicles, it is necessary to provide a new technology that can reduce the volume expansion of secondary batteries. Summary of the Invention [Problem to be solved by the invention]

[0004] The present application has been made in view of the above problems, and aims to provide an artificial graphite having both low expansion and high gram capacity, a method for producing the same, and a negative electrode plate produced using the artificial graphite as a negative electrode active material. Further, the present application aims to provide a secondary battery having low volume expansion during cycle processes and high energy density, and a power consuming device including the secondary battery. [Means for solving the problem]

[0005] In order to achieve the above object, a first aspect of the present application provides an artificial graphite, the artificial graphite containing secondary particles and satisfying A≧0.5, wherein A is the powder compaction density (unit: g / cm) of the artificial graphite at a pressure of 2t. 3 ) and its volume distribution particle size Dv This is a ratio to 1 (unit: μm).

[0006] In some embodiments, the synthetic graphite satisfies 0.50≦A≦1.40, optionally 0.70≦A≦1.30, and further optionally 0.70≦A≦1.00.

[0007] In some embodiments, the synthetic graphite may be secondary particles.

[0008] In some embodiments, the synthetic graphite has a powder compaction density of 1.60 g / cm at 2 t pressure. 3 -1.95g / cm 3 and optionally 1.70 g / cm 3 -1.90g / cm 3 may be also possible.

[0009] In some embodiments, the volume distribution particle size D of the artificial graphite v 1 may be 1.5 μm-3.5 μm, alternatively 1.8 μm-3.2 μm, and further alternatively 2.0 μm-3.2 μm.

[0010] In some embodiments, the volume distribution particle size D of the artificial graphite v 50 may be 10.0 μm-20.0 μm, and alternatively may be 12.0 μm-18.0 μm.

[0011] In some embodiments, the gram capacity of the synthetic graphite is 350 mAh / g or greater, optionally 352 mAh / g or greater.

[0012] A second aspect of the present invention provides a method for producing artificial graphite, the method comprising the steps of: Step S1: crushing, classifying, and shaping the raw material to obtain a precursor; Step S2, in which the precursor obtained in step S1 is granulated to obtain an intermediate 1; Step S3: performing a graphitization treatment on the intermediate 1 obtained in step S2 at a temperature of 2700° C. to 3200° C. to obtain an intermediate 2; Step S4 of mechanically treating the intermediate 2 obtained in step S3 by mechanofusion to obtain artificial graphite; Wherein, the artificial graphite contains secondary particles and satisfies A≧0.5, where A is the powder compaction density of the artificial graphite at 2t pressure and the volume distribution particle size D of the artificial graphite. v It is a ratio to 1.

[0013] In some embodiments, during the mechanical processing of step S4, the rotation speed of the Mechanofusion may be 600 rpm-1400 rpm, and optionally 800 rpm-1200 rpm.

[0014] In some embodiments, the processing time of the machine processing in step S4 may be 5 min-30 min, and optionally 5 min-25 min.

[0015] In some embodiments, an adhesive may be added in the granulation process of step S2, and the amount of the added adhesive may be 5%-15% of the weight of the precursor for granulation in step S2, and optionally the adhesive may include one or more of coal tar, asphalt, epoxy resin, and phenolic resin.

[0016] In some embodiments, the feedstock in step S1 may include one or more of petroleum green coke, calcined petroleum coke, needle green coke, calcined needle coke, asphalt coke, and metallurgical coke. Optionally, the feedstock may include one or more of petroleum green coke, needle green coke, and calcined needle coke.

[0017] A third aspect of the present application provides a secondary battery, the secondary battery including a negative electrode plate, the negative electrode plate including a negative electrode active material, the negative electrode active material including artificial graphite according to the first aspect of the present application, or including artificial graphite produced by the method according to the second aspect of the present application.

[0018] A fourth aspect of the present application provides a power consuming device including the secondary battery of the third aspect of the present application. Effect of the Invention

[0019] In the secondary battery according to the present application, the negative electrode active material includes artificial graphite, the artificial graphite includes secondary particles, and satisfies A≧0.5, where A is the powder compaction density of the artificial graphite at a pressure of 2t and the volume distribution particle size D of the artificial graphite. v 1. The artificial graphite particles according to the present application are rounded, and the bonding strength between the particles can be significantly improved. In the cycle process of the secondary battery, the high bonding strength between the artificial graphite particles, which are the negative electrode active material, can effectively maintain the contact between the particles and reduce the increase in the thickness of the electrode plate, thereby significantly reducing the expansion of the electrode plate, and further significantly reducing the volume expansion in the cycle process of the secondary battery containing this artificial graphite. The volume expansion in the cycle process of the secondary battery is low, which is advantageous for maintaining a high volume energy density. The low volume expansion can further reduce the internal stress of the battery core of the secondary battery, reduce the deformation of the battery core due to the action of the internal stress, and effectively improve the safety performance of the secondary battery. Therefore, the artificial graphite according to the present application can improve the safety performance and energy density of the secondary battery. In addition, the secondary battery with low volume expansion can maintain an internal structure suitable for the infiltration of the electrolyte in the cycle process, and can fully infiltrate the electrolyte into the battery core, increase the transmission channel of lithium ions, and thereby improve the cycle performance of the secondary battery. At the same time, the low expansion of the plate is also advantageous in avoiding the risk of short circuiting the battery core, and further improves the safety performance of the secondary battery. The power consumption device of the present application includes the secondary battery of the present application, and therefore has at least the same advantages as the secondary battery.

[0020] In the method for producing artificial graphite according to the present application, after the graphitization step, the graphitized particles are mechanically treated using mechanofusion to remove the edge angles of the aggregated particles, and the surfaces of the finally obtained artificial graphite particles can be made more rounded. When this artificial graphite is used as the negative electrode plate active material of a secondary battery, the bonding strength between the particles can be significantly improved, and the plate expansion can be significantly reduced, thereby obtaining a secondary battery with low volume expansion during the cycle process, and a power consumption device including this secondary battery. [Brief description of the drawings]

[0021] In order to more clearly explain the technical solutions of the embodiments of the present application, the following briefly introduces the drawings that need to be used in the embodiments of the present application. It is obvious that the drawings described below are only some embodiments of the present application, and those skilled in the art can also obtain other drawings based on the drawings without exerting creative efforts. [Figure 1] FIG. 1 is a schematic diagram of a secondary battery according to an embodiment of the present application. [Diagram 2] FIG. 1 is a schematic diagram of a battery module according to an embodiment of the present application. [Diagram 3] FIG. 1 is a schematic diagram of a battery pack according to an embodiment of the present application. [Figure 4] FIG. 4 is an exploded view of FIG. [Diagram 5] 1 is a schematic diagram of a power consuming device according to an embodiment of the present application; [Figure 6a-6c] 1A to 1C are SEM (scanning electron microscope) images of artificial graphite according to Examples 1, 2, and 3 of the present application, respectively. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0022] Hereinafter, with appropriate reference to the drawings, embodiments specifically disclosing the artificial graphite and its manufacturing method, secondary battery, and power consumption device of the present application will be described in detail. However, unnecessary detailed description may be omitted. For example, detailed description of well-known matters and duplicated description of actually the same structure may be omitted. This is to avoid the following description becoming unnecessarily long and to allow those skilled in the art to easily understand. Note that the drawings and the following description are provided to allow those skilled in the art to fully understand the present application, and are not intended to limit the subject matter described in the claims.

[0023] The "ranges" disclosed in this application are defined in the form of lower and upper limits, and a given range is defined by selecting one lower limit and one upper limit, and the selected lower and upper limits define the boundaries of the particular range. Such defined ranges may be inclusive or exclusive of the extreme values, and may be arbitrarily combined, i.e., any lower limit may be combined with any upper limit to form a range. For example, if ranges of 60-120 and 80-110 are listed for a particular parameter, it is understood that ranges of 60-110 and 80-120 are also envisaged. It is understood that if 1 and 2 are listed as minimum range values, and 3, 4 and 5 are listed as maximum range values, then the ranges 1-3, 1-4, 1-5, 2-3, 2-4 and 2-5 are all envisaged. In this application, unless otherwise specified, the numerical range "ab" represents a shorthand representation of any combination of real numbers from a to b, where a and b are both real numbers. For example, a numerical range of "0-5" indicates that all real numbers between "0-5" have already been listed in this specification, and "0-5" is merely a shorthand for combinations of these numbers. Also, expressing a parameter as an integer ≧2 is equivalent to disclosing that the parameter is, for example, the integers 2, 3, 4, 5, 6, 7, 8, 9, 10, 11, 12, etc.

[0024] Unless otherwise stated, all the embodiments and optional embodiments of the present application can be combined with each other to form a new technical solution.

[0025] Unless otherwise stated, all technical features and optional technical features of this application can be combined with each other to form a new technical solution.

[0026] Unless otherwise stated, all steps in this application may be performed in sequence or randomly, and preferably in sequence. For example, the method includes steps (a) and (b) to mean that the method may include steps (a) and (b) performed in sequence, or steps (b) and (a) performed in sequence. For example, the method mentioned above may further include step (c) to mean that step (c) may be added to the method in any order, for example, the method may include steps (a), (b) and (c), may include steps (a), (c) and (b), may include steps (c), (a) and (b), etc.

[0027] Unless otherwise specified, the terms "comprise" and "comprises" referred to in this application may be open ended or closed ended. For example, the terms "comprise" and "comprises" may further include or include other ingredients not listed, or may include or include only the ingredients listed.

[0028] Unless otherwise stated, in this application, the term "or" is inclusive. For example, the phrase "A or B" means "A, B, or both A and B." More specifically, "A or B" is satisfied if A is true (or exists) and B is false (or does not exist), if A is false (or does not exist) but B is true (or exists), or if both A and B are true (or exist).

[0029] In the description of this specification, it should be explained that unless otherwise specified, "more than" and "less than" are inclusive, and "multiple" in "one or more" means two or more.

[0030] Electric energy, as an economical, practical, clean, easy-to-control and convert energy form, is increasingly being applied to various power consumption devices. Secondary batteries have advantages such as high energy density, excellent portability, no memory effect, and environmental friendliness, making them a preferred power source for power consumption devices. However, secondary batteries undergo volume expansion due to the expansion of their negative electrode plates during cycling, which causes an increase in the internal stress of the battery, thus causing the risk of failure of the secondary battery, limiting the improvement of the energy density of the secondary battery, and further affecting the service life and safety performance of the battery. Therefore, how to reduce the volume expansion of the secondary battery during the cycling process has become a focus in the secondary battery technology field.

[0031] As a result of intensive research, the inventors have found that artificial graphite containing secondary particles has a powder compaction density (unit: g / cm) of artificial graphite at a pressure of 2 tonnes. 3 ) and the volume distribution particle size D of this artificial graphite v 1 (unit: μm) satisfies A≧0.5, the bonding strength between the artificial graphite particles, which are the negative electrode plate active material, can be significantly improved, and the volume expansion during the cycle process of a secondary battery containing this artificial graphite can be significantly reduced, which is advantageous for the secondary battery to maintain a high energy density, and further, the service life and safety performance of the secondary battery, as well as the battery module, battery pack and power consuming device including this secondary battery can be improved.

[0032] (Artificial graphite) The first aspect of the present application provides an artificial graphite, which contains secondary particles and satisfies A≧0.5, where A is the powder compaction density of the artificial graphite at 2t pressure and the volume distribution particle size D of the artificial graphite. v It is a ratio to 1.

[0033] The inventors have determined the powder compaction density of artificial graphite at a pressure of 2t and the volume distribution particle size D of this artificial graphite. v It has been found that when the ratio A to 1 is A≧0.5, the binding force between the artificial graphite particles of the negative electrode plate can be significantly improved, and the cycle expansion of the negative electrode plate can be significantly reduced, thereby significantly reducing the volume expansion of the secondary battery containing this artificial graphite during the cycle process. The volume increase during the cycle process of the secondary battery is small, which is advantageous for maintaining a high energy density. In particular, a secondary battery with low cycle expansion can maintain an internal structure suitable for electrolyte infiltration during the cycle process, and can fully infiltrate the electrolyte into the battery core, thereby improving the cycle life of the secondary battery. At the same time, the secondary battery has low cycle expansion, and can further reduce the internal stress of the battery core, reduce the deformation of the battery core due to the action of internal stress, and effectively improve the safety performance of the secondary battery. Therefore, the safety performance and service life of the battery module, battery pack and power consumption device using this secondary battery can also be improved.

[0034] In some embodiments, the synthetic graphite may satisfy 0.50≦A≦1.40, such as 0.60≦A≦1.40, 0.70≦A≦1.30, 0.80≦A≦1.20, 0.50≦A≦1.30, 0.60≦A≦1.30, 0.70≦A≦1.00, etc.

[0035] In some embodiments, the synthetic graphite may be secondary particles.

[0036] In some embodiments, the powder compaction density of the synthetic graphite at 2t pressure is 1.60 g / cm 3 -1.95g / cm 3 and optionally 1.70 g / cm 3 -1.95g / cm 3 , 1.75g / cm 3 -1.90g / cm 3 , e.g. 1.70g / cm 3 , 1.80g / cm 3 , 1.90g / cm3 , 1.95g / cm 3 , 1.70g / cm 3 -1.90g / cm 3 , 1.75g / cm 3 -1.95g / cm 3 , 1.80g / cm 3 -1.95g / cm 3 , 1.80g / cm 3 -1.90g / cm 3 By setting the powder compaction density of the artificial graphite in an appropriate range, the compaction density of the negative electrode plate can be improved, and thus the energy density of the secondary battery can be further improved.

[0037] In some embodiments, the volume distribution particle size D of the artificial graphite v 1 may be 1.5 μm-3.5 μm, alternatively 1.8 μm-3.2 μm, and further alternatively 2.0 μm-3.2 μm, for example 1.6 μm-3.4 μm, 1.7 μm-3.3 μm, 1.9 μm-3.1 μm, 2.0 μm-3.0 μm, 2.3 μm-2.8 μm, 2.5 μm-3.5 μm, etc. Suitable D of artificial graphite v 1 is suitable for making the surface more rounded, which is advantageous for significantly improving the binding force between particles when used as a negative electrode active material, and further, can effectively maintain the contact between particles, reduce the increase in plate thickness, and reduce the cycle expansion of the plate, which is not only advantageous for reducing the volume expansion of the secondary battery during cycle expansion, but also advantageous for improving the energy density of the secondary battery.

[0038] In some embodiments, the volume distribution particle size D of the artificial graphite v 50 may be 10.0 μm-20.0 μm, or alternatively 12.0 μm-18.0 μm, for example 10.0 μm-18.0 μm, 14.0 μm-16.0 μm, 14.0 μm-18.0 μm, etc. Suitable D of artificial graphite v 50 is suitable for having high active ion and electron transport properties, and can reduce the side reaction of the electrolyte at the negative electrode. vThe artificial graphite having an average particle diameter of 100 to 150 mm is also advantageous in improving its own powder compaction density. By using this artificial graphite, the compaction density of the electrode plate can be increased, thereby improving the energy density of the secondary battery.

[0039] In some embodiments, the gram capacity of the artificial graphite is 350 mAh / g or more, and optionally 352 mAh / g or more. The higher the gram capacity of the artificial graphite, the higher the energy density of a secondary battery containing it. The artificial graphite of the present application has a high gram capacity while having low cycle expansion, and by using both in combination, the secondary battery of the present application has both low cycle expansion and high energy density characteristics.

[0040] (Manufacturing method of artificial graphite) In a second aspect, the present application provides a method for producing artificial graphite, which can produce any one of the above artificial graphites.

[0041] In an embodiment of the present application, a method for producing artificial graphite is provided, which comprises the steps of: Step S1: crushing, classifying, and shaping the raw material to obtain a precursor; Step S2, in which the precursor obtained in step S1 is granulated to obtain an intermediate 1; Step S3: performing a graphitization treatment on the intermediate 1 obtained in step S2 at a temperature of 2700° C. to 3200° C. to obtain an intermediate 2; Step S4 of mechanically treating the intermediate 2 obtained in step S3 by mechanofusion to obtain artificial graphite; Wherein, the artificial graphite contains secondary particles and satisfies A≧0.5, where A is the powder compaction density of the artificial graphite at 2t pressure and the volume distribution particle size D of the artificial graphite. v It is a ratio to 1.

[0042] In some implementations, during mechanical processing, the rotation speed of the mechanofusion may be 600 rpm-1400 rpm, and optionally 800 rpm-1200 rpm, such as 600 rpm-1300 rpm, 600 rpm-1200 rpm, 700 rpm-1400 rpm, 800 rpm-1400 rpm, 800 rpm-1300 rpm, 900 rpm-1200 rpm, etc. When mechanical processing is performed on the intermediate 2 obtained in step S3, the appropriate rotation speed of the mechanofusion is determined based on the required volume distribution particle size D v It is possible to ensure that artificial graphite satisfying the above requirement of 1 (which may be 1.5 μm-3.5 μm, optionally 1.8 μm-3.2 μm, and further optionally 2.0 μm-3.2 μm) is obtained, thereby obtaining artificial graphite having the required rounded surface.

[0043] In some implementations, the processing time of the mechanical processing may be 5 min (min)-30 min, alternatively 5 min-25 min, such as 10 min-30 min, 5 min-27 min, 5 min-26 min, 10 min-20 min, 5 min-15 min, etc. In the mechanical processing, the appropriate mechanical processing time is determined based on the required volume distribution particle size D v It is possible to ensure that artificial graphite satisfying the above requirement of 1 (which may be 1.5 μm-3.5 μm, optionally 1.8 μm-3.2 μm, and further optionally 2.0 μm-3.2 μm) is obtained, thereby obtaining artificial graphite having the required rounded surface.

[0044] In some implementations, the feedstock may include one or more of petroleum green coke, calcined petroleum coke, needle green coke, calcined needle coke, asphalt coke, and metallurgical coke. Optionally, the feedstock may include one or more of petroleum green coke, needle green coke, and calcined needle coke.

[0045] In some embodiments, in step S1, the raw material may be crushed by using equipment and methods known in the art, such as a jet mill, a mechanical mill, or a roll mill. In the crushing process, a large amount of undersized particles are often generated, and oversized particles may exist in some cases. Therefore, after crushing, a classification process can be performed according to needs to remove undersized particles and oversized particles in the crushed powder. After the classification process, a particle product with a good particle size distribution can be obtained, and D can be selected to facilitate the subsequent shaping and / or granulation process. v 50 may be 8.0-13.5 μm. The classification process may be carried out using equipment and methods known in the art, such as a classification sieve, a gravity classifier, a centrifugal classifier, and the like.

[0046] In some embodiments, in step S1, equipment (e.g., a shaping machine or other shaping equipment) and methods known in the art may be adopted to perform a shaping process on the particle product obtained after the classification process, for example, to grind the edge angles of the particle product obtained by the classification process, thus facilitating subsequent operations and making the product obtained after the shaping process highly stable.

[0047] In some embodiments, step S1 may further include removing fines after shaping. Fines may be removed using equipment and methods known in the art, such as a classifier, a gravity classifier, a centrifugal classifier, etc.

[0048] In some embodiments, in step S2, the precursor obtained in step S1 is granulated to aggregate the independently dispersed primary particles to form secondary particles. In the granulation process, an adhesive may be used, and optionally the amount of the adhesive may be 2%-15%, such as 2%-12%, 4%-12%, 5%-15%, 6%-10%, etc., of the weight of the precursor for granulation in step S2, and optionally the adhesive may include one or more of coal tar, asphalt, epoxy resin, and phenolic resin.

[0049] In step S2, granulation may be performed using equipment known in the art, such as a granulator. The granulator usually includes a stirring reaction vessel and a module for controlling the temperature of the reaction vessel. In addition, the D of the product (i.e., intermediate 1) obtained by granulation can be controlled by adjusting process conditions such as the stirring rotation speed, the temperature increase rate, the granulation temperature, and the temperature decrease rate during granulation. v 50 can be controlled to 14.5-24.0 μm. Optionally, in the present application, the stirring rotation speed during granulation is 800 r / min-1500 r / min, the temperature rise rate is 8-15° C. / min, the granulation temperature is 400° C.-650° C., and the granulation time is 6-10 hours.

[0050] In some embodiments, in step S3, the intermediate 1 obtained in step S2 is graphitized to obtain an intermediate 2. In some embodiments, the temperature at which the graphitization is performed in step S3 may be 2700° C.-3200° C., for example, 2700° C.-3100° C., 3000° C.-3200° C., 2800° C.-3100° C., etc.

[0051] In some embodiments, during the mechanical treatment in step S4, the rotation speed of the Mechanofusion may be 600 rpm-1400 rpm, and optionally 800 rpm-1200 rpm, such as 600 rpm, 700 rpm, 800 rpm, 900 rpm, 1100 rpm, 1400 rpm, 600 rpm-1200 rpm, 700 rpm-1200 rpm, 900 rpm-1100 rpm, etc. The processing time of the mechanical treatment may be 5 min-30 min, and optionally 5 min-25 min, such as 5 min, 10 min, 15 min, 20 min, 25 min, 30 min, 5 min-25 min, 5 min-20 min, 5 min-15 min, 10 min-20 min, etc. The appropriate range of mechanofusion rotation speed and appropriate range of mechanical processing time can remove the edge angles of the aggregated particles and make the final artificial graphite particles more rounded, which not only contributes to improving the bonding force between particles, but also improves the volume distribution particle size D of the obtained artificial graphite. v1 in the range of 1.5μm-3.5μm, and the powder compaction density at 2t pressure is 1.60g / cm 3 -1.95g / cm 3 and artificial graphite that satisfies A ≥ 0.5 (A is the powder compaction density of artificial graphite at 2t pressure (unit: g / cm 3 ) and the volume distribution particle size of artificial graphite D v 1 (unit: μm)), and can significantly reduce the cycle expansion of the negative electrode plate containing this artificial graphite and the volume expansion during the cycle process of the secondary battery containing this artificial graphite, thereby contributing to obtaining a secondary battery that combines high volumetric energy density and low volumetric cycle expansion. If the rotation speed and mechanical treatment time of the mechanofusion are above the above ranges, the rotation speed is too high and the time is too long, resulting in an increase in defects on the material surface, and the capacity is rapidly attenuated during the cycle process of the secondary battery containing this artificial graphite. If the rotation speed and mechanical treatment time of the mechanofusion are below the above ranges, the rotation speed is too low and the time is too short, resulting in insufficient removal of particle edge angles, and the bonding force between particles cannot be improved, and the effect of reducing expansion is not clear.

[0052] Artificial graphite D v 1, D v 50 can be measured using a laser particle size analyzer (e.g., Malvern Master Size 3000) with reference to standard GB / T 19077.1-2016.

[0053] Here, D v 1, D v The physical definition of 50 is as follows:

[0054] D v 1: Particle diameters that account for 1% of the total volume are smaller than this value.

[0055] D v 50: The particle diameter occupying 50% of the total volume may be larger than this value, and the particle diameter occupying 50% of the total volume may be smaller than this value. D v 50 represents the median particle size of the powder.

[0056] The powder compaction density of the artificial graphite can be tested by adopting methods known in the art, for example, referring to the standard GB / T 24533-2009, and can be tested by an electronic pressure tester (such as UTM7305). A certain amount of powder can be placed in a compaction mold, different pressures can be set, and the thickness of the powder at different pressures can be read out from the machine, and the compaction density at different pressures can be calculated.

[0057] (Secondary battery) The present application provides a secondary battery, which includes any one of the artificial graphites according to the first aspect of the present invention, or includes any one of the artificial graphites produced by the method according to the second aspect of the present invention.

[0058] Generally, a secondary battery includes a positive electrode plate, a negative electrode plate, an electrolyte, and a separator. During charging and discharging of the battery, active ions shuttle between the positive electrode plate and the negative electrode plate to store and release ions. The electrolyte serves to conduct ions between the positive electrode plate and the negative electrode plate. The separator is installed between the positive electrode plate and the negative electrode plate, and serves mainly to prevent short circuit between the positive and negative electrodes, while allowing ions to pass through.

[0059] [Negative electrode plate] The negative electrode plate includes a negative electrode current collector and a negative electrode film disposed on at least one surface of the negative electrode current collector. For example, the negative electrode current collector has two surfaces facing each other in the thickness direction of the negative electrode current collector, and the negative electrode film layer is disposed on either one or both of the two facing surfaces of the negative electrode current collector.

[0060] The negative electrode current collector may be made of a material having good electrical conductivity and mechanical strength, and may serve as a conductor and a current collector. In some embodiments, the negative electrode current collector may be made of copper foil.

[0061] The negative electrode film includes a negative electrode active material, the negative electrode active material includes any one of the artificial graphites according to the first aspect of the present application, and the volume expansion of the negative electrode plate including the artificial graphite of the present application during cycling can be significantly reduced. The low volume expansion is not only beneficial for the secondary battery to maintain a high volumetric energy density, but also contributes to reducing the internal stress of the battery core of the secondary battery and reducing the deformation of the battery core caused by the internal stress, and can effectively improve the safety performance of the secondary battery.

[0062] In some embodiments, the step of manufacturing a negative electrode plate by employing any one or more of the artificial graphites of the present application may include dispersing a negative electrode active material including any one or more of the artificial graphites of the present application, an adhesive, and an optional thickener and conductive agent in a solvent (the solvent may be deionized water) to form a uniform negative electrode slurry; and coating the negative electrode slurry on a negative electrode current collector, and obtaining a negative electrode plate after processes such as drying and cooling.

[0063] In some embodiments, the negative plate further optionally includes other negative active materials that can be used in secondary battery negative electrodes, which can be one or more of other graphite materials (e.g., other synthetic graphite, natural graphite), mesocarbon microbeads (abbreviated as MCMB), hard carbon, soft carbon, silicon-based materials, and tin-based materials.

[0064] In some embodiments, the adhesive may be selected from one or more of polyacrylic acid (PAA), sodium polyacrylate (PAAS), polyacrylamide (PAM), polyethylene alcohol (PVA), styrene butadiene rubber (SBR), sodium alginate (SA), polymethacrylic acid (PMAA), and carboxymethyl chitosan (CMCS).

[0065] In some examples, the viscosity increasing agent may be sodium carboxymethylcellulose (CMC-Na).

[0066] In some embodiments, the conductive agent used in the negative plate may be selected from one or more of graphite, superconducting carbon, acetylene black, carbon black, ketjen black, carbon dots, carbon nanotubes, graphene, and carbon nanofibers.

[0067] [Positive electrode plate] The positive electrode plate includes a positive electrode current collector and a positive electrode film that is disposed on at least one surface of the positive electrode current collector and includes a positive electrode active material. For example, the positive electrode current collector has two surfaces that face each other in the thickness direction of the positive electrode current collector, and the positive electrode film layer is disposed on either one or both of the two facing surfaces of the positive electrode current collector.

[0068] The positive electrode current collector may be made of a material having good electrical conductivity and mechanical strength, and in some embodiments, may be made of aluminum foil.

[0069] The present application is not limited to a specific type of positive electrode active material, and any material that can be used for the positive electrode of a secondary battery known in the art may be adopted, and those skilled in the art can select it according to actual needs.

[0070] In some embodiments, the secondary battery may be a lithium-ion secondary battery. The positive electrode active material may be selected from lithium transition metal oxides and their modifying materials, and the modifying materials may perform doping modification and / or coating modification on the lithium transition metal oxides. For example, the lithium transition metal oxide may be selected from one or more of lithium cobalt oxide, lithium nickel oxide, lithium manganese oxide, lithium nickel manganese oxide, lithium nickel cobalt manganese oxide, lithium nickel cobalt aluminum oxide, and lithium-containing phosphates with an olivine structure.

[0071] For example, the positive electrode active material of a secondary battery is LiCoO2, LiNiO2, LiMnO2, LiMn2O4, LiNi 1 / 3 Co 1 / 3 Mn 1 / 3 O2(NCM333), LiNi0.5 Co 0.2 Mn 0.3 O2(NCM523), LiNi 0.6 Co 0.2 Mn 0.2 O2(NCM622), LiNi 0.8 Co 0.1 Mn 0.1 O2(NCM811), LiNi 0.85 Co 0.15 Al 0.05 It may be selected from one or more of O2, LiFePO4 (LFP) and LiMnPO4.

[0072] In some embodiments, the positive electrode membrane may further include an adhesive. There is no limitation on the type of adhesive, and those skilled in the art may select it according to actual needs. For example, the adhesive used in the positive electrode membrane may include one or more of polyvinylidene fluoride (PVDF) and polytetrafluoroethylene (PTFE).

[0073] In some embodiments, the positive electrode film further includes a conductive agent. The type of the conductive agent is not limited, and a person skilled in the art can select it according to actual needs. For example, the conductive agent used in the positive electrode film may include one or more of graphite, superconducting carbon, acetylene black, carbon black, ketjen black, carbon dots, carbon nanotubes, graphene, and carbon nanofibers.

[0074] [Electrolyte] The electrolyte serves to conduct ions between the positive and negative electrodes. The present application is not specifically limited to the type of electrolyte, and may be selected according to need. For example, the electrolyte may be liquid, gel, or all solid.

[0075] In some embodiments, the electrolyte is an electrolytic solution that includes an electrolyte salt and a solvent.

[0076] In some embodiments, the electrolyte salt may be selected from one or more of LiPF6 (lithium hexafluorophosphate), LiBF4 (lithium tetrafluoroborate), LiClO4 (lithium perchlorate), LiAsF6 (lithium hexafluoroarsenate), LiFSI (lithium bis(fluorosulfonyl)imide), LiTFSI (lithium bis(trifluoromethanesulfonate), LiTFS (lithium trifluoromethanesulfonate), LiDFOB (lithium difluoro(oxalato)borate), LiBOB (lithium bis(oxalato)borate), LiPO2F2 (lithium difluorophosphate), LiDFOP (lithium difluorobis(oxalato)phosphate), and LiTFOP (lithium tetrafluoro(oxalato)phosphate).

[0077] In some examples, the solvent may be selected from one or more of ethylene carbonate (EC), propylene carbonate (PC), ethyl methyl carbonate (EMC), diethyl carbonate (DEC), dimethyl carbonate (DMC), dipropyl carbonate (DPC), methyl propyl carbonate (MPC), ethyl propyl carbonate (EPC), butylene carbonate (BC), fluoroethylene carbonate (FEC), methyl formate (MF), methyl acetate (MA), ethyl acetate (EA), propyl acetate (PA), methyl propionate (MP), ethyl propionate (EP), propyl propionate (PP), methyl butyrate (MB), ethyl butyrate (EB), 1,4-butyrolactone (GBL), sulfolane (SF), dimethyl sulfone (MSM), ethyl methyl sulfone (EMS), and diethyl sulfone (ESE).

[0078] In some embodiments, the electrolyte solution further optionally includes additives, for example, the additives may include anode film-forming additives, cathode film-forming additives, and additives that can improve some performance of the battery, such as additives that improve the overcharge performance of the battery, additives that improve the high temperature performance of the battery, and additives that improve the low temperature performance of the battery.

[0079] [Separator] A separator is further included in secondary batteries using an electrolyte and in some secondary batteries using a solid electrolyte. The separator is disposed between the positive electrode plate and the negative electrode plate and plays a role of isolation. The present application is not particularly limited to the type of separator, and any known porous structure separator having good chemical stability and mechanical stability can be selected and used. In some embodiments, the material of the separator may be selected from one or more of glass fiber, nonwoven fabric, polyethylene, polypropylene, and polyvinylidene fluoride. The separator may be a single layer film or a multi-layer composite film. When the separator is a multi-layer composite film, the materials of each layer may be the same or different.

[0080] [Exterior body] In some embodiments, the secondary battery may include an exterior body for packaging the positive electrode plate, the negative electrode plate, and the electrolyte. For example, the positive electrode plate, the negative electrode plate, and the separator may be stacked or wound to form a stacked structure battery core or a wound structure battery core, and the battery core is packaged in the exterior body, and an electrolyte may be adopted as the electrolyte, and the electrolyte is impregnated into the battery core. The number of battery cores in the secondary battery may be one or several, and can be adjusted according to demand.

[0081] In some embodiments, the exterior body of the secondary battery may be a soft bag, for example, a pouch-type soft bag. The material of the soft bag may be plastic, for example, may include one or more of polypropylene (PP), polybutylene terephthalate (PBT), polybutylene succinate (PBS), etc. The exterior body of the secondary battery may be a hard case, for example, an aluminum case, etc.

[0082] In some embodiments, the positive plate, the negative plate, and the separator may be fabricated into an electrode assembly by a winding process or a stacking process.

[0083] The present application is not particularly limited to the shape of the secondary battery, which may be cylindrical, rectangular or any other shape. Figure 1 shows a secondary battery 5 with a rectangular structure as an example.

[0084] The secondary battery according to the present invention may be assembled into a battery module. The number of secondary batteries included in the battery module may be multiple, and the specific number may be adjusted according to the application and capacity of the battery module.

[0085] Fig. 2 shows an example of a battery module 4. Referring to Fig. 2, in the battery module 4, the multiple secondary batteries 5 may be arranged in sequence along the longitudinal direction of the battery module 4. Of course, they may be arranged in any other manner. Furthermore, the multiple secondary batteries 5 may be fixed by fasteners.

[0086] Optionally, the battery module 4 may further include a housing having an accommodating space, and the multiple secondary batteries 5 are accommodated in the accommodating space.

[0087] In the present invention, the battery modules assembled with the secondary batteries may be assembled into a battery pack, and the number of battery modules included in the battery pack may be adjusted according to the application and capacity of the battery pack.

[0088] 3 and 4 show an example of a battery pack 1. Referring to FIG. 3 and FIG. 4, the battery pack 1 may include a battery box and a plurality of battery modules 4 installed in the battery box. The battery box may include an upper housing 2 and a lower housing 3, and the upper housing 2 is covered by the lower housing 3 to form a sealed space for accommodating the battery modules 4. The plurality of battery modules 4 may be arranged in the battery box in any manner.

[0089] (power consumption equipment) The present application further provides a power consuming device, which includes a secondary battery according to the present application, and the secondary battery provides a power source for the power consuming device. The power consuming device may be, but is not limited to, a mobile device (e.g., a mobile phone, a laptop, etc.), an electric vehicle (e.g., a pure electric vehicle, a hybrid electric vehicle, a plug-in hybrid electric vehicle, an electric bicycle, an electric scooter, an electric golf cart, an electric truck, etc.), an electric train, a ship and a satellite, an energy storage system, etc.

[0090] The power consumption device can select a secondary battery, a battery module or a battery pack according to its usage demand.

[0091] 5 shows an example power consuming device, such as a pure electric vehicle, a hybrid electric vehicle, or a plug-in hybrid electric vehicle, etc. A battery pack or a battery module may be employed to meet the demand for high power and high energy density of the secondary battery of the power consuming device.

[0092] As another example, the power consuming device may be a mobile phone, a tablet computer, a notebook computer, etc. These power consuming devices are generally required to be thin, and may employ a secondary battery as a power source. EXAMPLES

[0093] The following describes examples of the present application. The examples described below are illustrative and are used only to interpret the present application, and should not be understood as limiting the present application. In the examples, specific techniques or conditions are not specified, but are carried out according to techniques or conditions described in the literature in the field or product instructions. Reagents or equipment used that do not specify the manufacturer are all common products that can be purchased commercially.

[0094] [Performance test] (1) Gram capacity test of artificial graphite The prepared artificial graphite, conductive agent Super P, thickener (CMC-Na), adhesive (SBR) are mixed with deionized water as solvent in a mass ratio of 94.5:1.5:1.5:2.5 to prepare a slurry, which is then coated on a copper foil current collector and dried in an oven for use. A lithium metal sheet is used as the counter electrode, a polyethylene (PE) film is used as the separator, and ethylene carbonate (EC), ethyl methyl carbonate (EMC), and diethyl carbonate (DEC) are mixed in a volume ratio of 1:1:1. LiPF6 is then uniformly dissolved in the above solution to obtain an electrolyte, of which the concentration of LiPF6 is 1mol / L. The above parts are assembled into a CR2430 type coin battery in a glove box protected by argon gas.

[0095] The resulting coin battery was left to stand for 12 hours, then discharged at a constant current of 0.05 C to 0.005 V, left to stand for 10 minutes, then discharged at a constant current of 50 μA to 0.005 V, left to stand for 10 minutes, then discharged at a constant current of 10 μA to 0.005 V, and then charged at a constant current of 0.1 C to 2 V, and the charge capacity was recorded. The ratio of the charge capacity to the mass of the artificial graphite is the gram capacity of the artificial graphite produced.

[0096] (2) Cyclic expansion rate test of negative electrode plate The thickness of the negative electrode plate after cold pressing was marked as H0. A secondary battery was fabricated by the cold pressed negative electrode plate, the positive electrode plate, the separator, and the electrolyte. At 25°C, the secondary battery was cycled at 1C / 1C with 100% DOD (100% depth of discharge, i.e., fully charged and then fully discharged) by a Neware charger. The discharge capacity of the first cycle (i.e., the initial capacity) was marked as 100%, and the cycle was stopped when the cycle capacity retention rate was 80% of the initial capacity. Then, the secondary battery was charged to 100% SOC (State of Charge), the secondary battery was disassembled, and the thickness of the corresponding negative electrode plate was tested and marked as H1. The cycle expansion rate of the negative electrode plate was (H1 / H0-1)×100%.

[0097] (3) Cycle capacity retention rate A charge / discharge test was performed on the lithium-ion battery at 25°C. One charge / discharge cycle process is as follows: constant current charging at 1C to 4.3V, followed by constant voltage charging at 0.05C at 4.3V, leaving it for 5 minutes, followed by constant current discharging at 1C to 2.8V, and recording the battery capacity at this time as C1. The above is one charge / discharge cycle of the battery. 1200 cycles were performed according to the above process, and the battery capacity C1200 at this time was recorded. Cycle capacity retention rate = C1200 / C1 x 100%.

[0098] (4) Negative electrode plate cohesion test Double-sided tape was attached to both sides of a 2 cm wide stainless steel plate, and the electrode plate that needed to be tested was attached evenly to the double-sided tape, with the same length and width. The copper foil tape was attached evenly to the surface of the electrode plate (ensuring that the surface after attachment was smooth and wrinkle-free), and a small amount of the copper foil tape was left to attach to the paper sheet (so that the copper foil tape and the paper sheet were in a straight line). The parameters of the tensile machine were set, and the electrode plate was placed vertically in the center of the card slot of the tensile machine, and then placed vertically up and down. Clicked start test on the computer, and the cohesive strength data was obtained.

[0099] Example 1 Manufacturing artificial graphite S1: The needle raw coke raw material is sent to the jaw crusher by the vibrating feeder for coarse crushing, and then the accepted material is sent to the mechanical mill for fine crushing, classification and shaping, and then D v 50 to obtain a precursor having a diameter of 11 μm.

[0100] S2: The precursor obtained in step S1 is added to the reaction vessel, and asphalt (D v The mixture was granulated by adding the powder (50 is 5μm-8μm), the stirring speed was set to 1200 r / min, the temperature was raised to 560℃ at a rate of 10℃ / min at room temperature, and the mixture was kept at this temperature for 8 hours. v The mixture is granulated until the particle size reaches 18 μm to obtain intermediate 1.

[0101] S3: The intermediate 1 obtained in step S2 is added to a graphitization furnace, heated to 3000°C, graphitized, and sieved through a 200 mesh screen to obtain intermediate 2.

[0102] S4: The intermediate 2 obtained in step S3 is placed in a mechanofusion and mechanically treated, during which the rotation speed of the mechanofusion is 900 rpm, the mechanical treatment time is 15 min, and D v 50 is 14 μm, D v 1 is 2μm, and the powder compaction density at 2t pressure is 1.8g / cm 3 The artificial graphite was obtained with a gram capacity of 357mAh / g, and the specific performance index parameters are shown in Table 1 below. The SEM image of the artificial graphite produced in this Example 1 is shown in Figure 6a.

[0103] Negative electrode plate manufacturing The artificial graphite, conductive agent (Super P), adhesive (SBR), and thickener (CMC-Na) are mixed in a mass ratio of 96.2:0.8:1.8:1.2 with an appropriate amount of deionized water and thoroughly stirred to form a homogeneous negative electrode slurry. The negative electrode slurry is coated on the surface of a negative electrode current collector copper foil, and the negative electrode plate is obtained after drying and cold pressing. The compaction density of the negative electrode plate is 1.65 g / cm. 3 and the surface density is 11.4 mg / cm 2 The results of the cohesive force test of this negative electrode plate, the cycle expansion rate test, and the cycle capacity retention rate test of the secondary battery are shown in Table 2 below.

[0104] Positive electrode plate manufacturing Cathode active material LiNi 0.5 Co 0.2 Mn 0.3 O2 (NCM523), conductive agent (Super P), and adhesive PVDF are mixed in a weight ratio of 96.2:2.7:1.1 with an appropriate amount of NMP and thoroughly stirred to form a homogeneous positive electrode slurry. The positive electrode slurry is coated on the surface of a positive electrode current collector aluminum foil, and then dried and cold pressed to obtain a positive electrode plate. The compaction density of the positive electrode plate is 3.45 g / cm. 3 and the surface density is 18.8 mg / cm 2It is.

[0105] Electrolyte production Ethylene carbonate (EC), ethyl methyl carbonate (EMC) and diethyl carbonate (DEC) are mixed in a volume ratio of 1:1:1, and LiPF6 is uniformly dissolved in the above solution to obtain an electrolyte, in which the concentration of LiPF6 is 1 mol / L.

[0106] Separator Polyethylene (PE) film is used.

[0107] Secondary battery manufacturing The positive electrode plate, separator, and negative electrode plate are stacked in order and wound to obtain a battery core, which is then inserted into an exterior body, the above electrolyte is added, and the secondary battery is obtained after going through processes such as packaging, standing, chemical formation, and aging. The exterior body is a hard case with a length*width*height=148mm*28.5mm*97.5mm.

[0108] Example 2-14 The manufacturing method of Examples 2 to 6 is similar to that of Example 1, with the difference being that the raw materials used in the manufacture of the artificial graphite are adjusted. The process parameters of each Example and the test results of the physical parameters of the manufactured artificial graphite are shown in Table 1 below. The cohesion test results of the negative electrode plate containing this artificial graphite, the cycle expansion rate results, and the cycle capacity retention rate results of the secondary battery containing this negative electrode plate are shown in Table 2 below.

[0109] Specifically, the raw material for the artificial graphite in Example 2 is calcined petroleum coke, the raw material for the artificial graphite in Example 3 is petroleum green coke (without adhesive), the raw material for the artificial graphite in Example 4 is calcined needle coke, the raw material for the artificial graphite in Example 5 is asphalt coke, and the raw material for the artificial graphite in Example 6 is metallurgical coke. Figures 6b and 6c are SEM images of the artificial graphite produced in Examples 2 and 3, respectively.

[0110] The manufacturing method of Examples 7 to 9 is similar to that of Example 1, with the difference being that the amount of adhesive used in the granulation process in producing the artificial graphite is adjusted. The process parameters of each Example and the test results of the physical parameters of the produced artificial graphite are shown in Table 1 below. The cohesion test results, cycle expansion rate results, and cycle capacity retention rate results of the negative electrode plate containing this artificial graphite are shown in Table 2 below.

[0111] Specifically, the amount of adhesive asphalt used in Example 7 was 15% of the weight of the precursor to be granulated in step S2, the amount of adhesive asphalt used in Example 8 was 8% of the weight of the precursor to be granulated in step S2, and the amount of adhesive asphalt used in Example 9 was 5% of the weight of the precursor to be granulated in step S2.

[0112] Examples 10-11 are similar to the manufacturing method of Example 1, with the difference being that the graphitization temperature for producing the artificial graphite is adjusted. The process parameters of each Example and the test results of the physical parameters of the produced artificial graphite are shown in Table 1 below. The cohesion test results, cycle expansion rate results, and cycle capacity retention rate results of the negative electrode plate containing this artificial graphite are shown in Table 2 below.

[0113] The manufacturing method of Examples 12-14 is similar to that of Example 1, with the difference being that the degree of mechanical fusion treatment in the production of artificial graphite is adjusted. The process parameters of each Example and the test results of the physical parameters of the produced artificial graphite are shown in Table 1 below. The cohesion test results, cycle expansion rate results, and cycle capacity retention rate results of the negative electrode plate containing this artificial graphite are shown in Table 2 below.

[0114] Comparative Example 1-12 Comparative Examples 1-6 are similar to the manufacturing methods of Examples 1-6, respectively, but differ in that there is no mechanical fusion step after graphitization in step S3. The process parameters of each comparative example and the test results of the physical parameters of the manufactured artificial graphite are shown in Table 1 below, and the cohesion test results, cycle expansion rate results, and cycle capacity retention rate results of the negative electrode plate containing this artificial graphite are shown in Table 2 below.

[0115] The manufacturing method of Comparative Examples 7-10 is similar to that of Example 1, with the difference being that the degree of mechanical fusion treatment in step S4 is adjusted. The process parameters of each Comparative Example and the test results of the physical parameters of the manufactured artificial graphite are shown in Table 1 below, and the cohesion test results, cycle expansion rate results, and cycle capacity retention rate results of the negative electrode plate containing this artificial graphite are shown in Table 2 below.

[0116] The manufacturing method of Comparative Examples 11-12 is similar to that of Example 1, and the difference is that the mechanical treatment method in step S4 is adjusted. Specifically, in Comparative Example 11, a high-speed airflow impact granulator (temperature: 600°C, treatment time: 8 hours) is used to mechanically crush and spheronize the intermediate 2 obtained in step S3, and the intermediate 2 is sieved to obtain D v In Comparative Example 12, the intermediate 2 obtained in step S3 is mechanically crushed and spheronized using an air flow scroll crusher (power is 0.7 MPa), and then sieved to obtain spherical artificial graphite particles having a diameter of 10 μm to 15 μm. v The result is spherical artificial graphite particles having a particle diameter of 10 μm-15 μm. The process parameters of each comparative example and the test results of the physical parameters of the produced artificial graphite are shown in Table 1 below, and the cohesive strength test results of the negative electrode plate containing this artificial graphite, the cycle expansion rate results, and the cycle capacity retention rate results of the secondary battery containing this negative electrode plate are shown in Table 2 below.

[0117] Table 1: Test results of process and physical parameters for Examples 1-14 and Comparative Examples 1-12 [Table 1] TIFF0007591139000002.tif186168

[0118] Table 2: Performance test results of Examples 1-14 and Comparative Examples 1-12 [Table 2]

[0119] Comparing Examples 1-14 and Comparative Examples 1-12 shown in Table 1 and Table 2 above, when intermediate body 2 is subjected to an appropriate mechanical fusion treatment after graphitization treatment, the artificial graphite obtained by the production has A of 0.5 or more (for example, 0.50≦A≦1.40, optionally 0.70≦A≦1.30, and further optionally 0.70≦A≦1.00, where A is the powder compaction density of the artificial graphite at 2t pressure and its volume distribution particle size D v 1), the cohesion of the negative electrode plate containing this artificial graphite can be significantly improved, the cycle expansion rate of the electrode plate can be significantly reduced, and the artificial graphite can maintain a high gram capacity, which has an obvious effect on reducing the volume expansion of the secondary battery containing this artificial graphite in the cycle process and improving the energy density and cycle capacity retention rate of the secondary battery, etc., and can effectively improve the service life and safety performance of the secondary battery.

[0120] In Comparative Examples 1-6, there is no mechanical fusion treatment step after the graphitization treatment step, and the negative electrode plate produced thereby has a high cycle expansion rate and low cohesion, which is disadvantageous for reducing the volume expansion during the cycle process of a secondary battery containing this negative electrode plate and is disadvantageous for improving the energy density of the secondary battery.

[0121] In Comparative Examples 7-8, the mechanical fusion treatment time is too long or too short in the mechanical treatment process. In Comparative Example 7, the treatment time is too long, which reduces the cycle capacity retention rate of the secondary battery. In Comparative Example 8, the mechanical fusion treatment time is too short, and the performance of the negative electrode plate and secondary battery obtained thereby corresponds to the performance of the negative electrode plate or secondary battery obtained without mechanical treatment in Comparative Examples 1-6. In Comparative Examples 9-10, the rotation speed of mechanofusion is too low or too high in the mechanical treatment process. In Comparative Example 9, the rotation speed is too low, which fails to achieve the purpose of mechanical treatment. The performance of the negative electrode plate and secondary battery obtained thereby corresponds to the performance of the negative electrode plate or secondary battery obtained without mechanical treatment in Comparative Examples 1-6. In Comparative Example 10, the cycle expansion rate of the negative electrode plate can be reduced to a certain extent by combining a rotation speed that is too high and a mechanical treatment time that is too short, but a rotation speed that is too high is disadvantageous to improving the cycle capacity retention rate of the secondary battery.

[0122] In Comparative Examples 11-12, a high-speed air impact granulator and an air scroll pulverizer were used to mechanically crush and spheronize the intermediate 2 obtained in step S3, and both produced spheronized artificial graphite. However, it was found that the use of the above two types of mechanical processing equipment was disadvantageous in improving the cohesive force of the negative electrode plate, and the effect of reducing the cycle expansion rate of the negative electrode plate was unclear. It was also found that it was difficult to grasp the degree of mechanical processing by the air scroll pulverizer, and the stability was low.

[0123] It should be noted that the present application is not limited to the above-mentioned embodiment. The above-mentioned embodiment is an example, and any embodiment having substantially the same configuration as the technical idea and the same effect within the scope of the technical solution of the present application is included in the technical scope of the present application. In addition, various modifications that a person skilled in the art can make to the embodiment and other methods constructed by combining some of the components in the embodiment are also included in the scope of the present application, within the scope of the purpose of the present application. [Explanation of symbols]

[0124] Here, the explanation of the symbols is as follows. 1. Battery pack, 2. Upper housing, 3. Lower housing, 4. Battery module; 5. Secondary battery.

Claims

1. Artificial graphite, Contains secondary particles, and The artificial graphite has a volume distribution particle size D v 1 of 2.0 μm to 3.5 μm, and a powder compaction density of the artificial graphite at a pressure of 2 t of 1.60 g / cm 3 to 1.95 g / cm 3 .

2. The artificial graphite according to claim 1, wherein the artificial graphite satisfies 0.50≦A≦0.98, and A is the ratio of the powder compaction density (unit: g / cm 3 ) of the artificial graphite at a pressure of 2 t to the volume distribution particle size D v 1 (unit: μm) of the artificial graphite.

3. The artificial graphite according to claim 1 or 2, wherein the artificial graphite is a secondary particle.

4. 4. The artificial graphite according to claim 1, wherein the powder compaction density of the artificial graphite at 2 t pressure is 1.70 g / cm 3 to 1.90 g / cm 3 .

5. The volume distribution particle size D of the artificial graphite v The artificial graphite according to any one of claims 1 to 4, wherein 1 is 2.0 μm to 3.2 μm.

6. The volume distribution particle size D of the artificial graphite v 6. The artificial graphite according to any one of claims 1 to 5, wherein 50 is 10.0 μm to 20.0 μm.

7. The artificial graphite described in claim 6, wherein the volume distribution particle size Dv50 of the artificial graphite is 12.0 μm-18.0 μm.

8. 8. The artificial graphite according to claim 1, wherein the gram capacity of the artificial graphite is 350 mAh / g or more.

9. The artificial graphite of claim 8, wherein the gram capacity of the artificial graphite is 352 mAh / g or greater.

10. A method for producing artificial graphite, comprising the steps of: Step S1: crushing, classifying, and shaping the raw material to obtain a precursor; Step S2, in which the precursor obtained in step S1 is granulated to obtain an intermediate 1; Step S3: performing a graphitization treatment on the intermediate 1 obtained in step S2 at a temperature of 2700° C. to 3200° C. to obtain an intermediate 2; Step S4 of mechanically treating the intermediate 2 obtained in step S3 by mechanofusion to obtain artificial graphite; The method for producing artificial graphite, wherein the artificial graphite contains secondary particles, and the volume distribution particle size D v 1 of the artificial graphite is 2.0 μm-3.5 μm, and the powder compaction density of the artificial graphite at a pressure of 2 t is 1.60 g / cm 3 -1.95 g / cm 3 .

11. The manufacturing method according to claim 10, wherein the rotation speed of the Mechanofusion during mechanical processing is 600 rpm-1400 rpm.

12. The manufacturing method described in claim 11, wherein during mechanical processing, the rotation speed of the mechanofusion is 800 rpm-1200 rpm.

13. The method according to any one of claims 10 to 12, wherein the processing time of the mechanical treatment is 5 min to 30 min.

14. The manufacturing method described in claim 13, wherein the processing time of the mechanical treatment is 5 min to 25 min.

15. The manufacturing method according to any one of claims 10 to 14, wherein an adhesive is added in the granulation process, and the amount of the added adhesive used is 5%-15% of the weight of the precursor for granulation in step S2.

16. The manufacturing method described in claim 15, wherein the adhesive includes one or more of coal tar, asphalt, epoxy resin, and phenolic resin.

17. 17. The process of any one of claims 10 to 16, wherein the feedstock comprises one or more of petroleum green coke, calcined petroleum coke, needle green coke, calcined needle coke, asphalt coke, and metallurgical coke.

18. The method of claim 17, wherein the raw materials include one or more of petroleum green coke, needle green coke, and calcined needle coke.

19. A secondary battery comprising a negative electrode plate, the negative electrode plate comprising a negative electrode active material, the negative electrode active material comprising the artificial graphite according to claim 1 .

20. 20. A power consuming device comprising the secondary battery of claim 19.

Citation Information

Patent Citations

  • Negative electrode active material for secondary battery, secondary battery containing the same and its manufacturing method

    JP2009266800A

  • Negative electrode material for lithium ion secondary battery, negative electrode mixture for lithium ion secondary battery, negative electrode lithium ion secondary battery, and lithium ion secondary battery

    JP2012227151A

  • Novel graphite material

    JP2016026137A