Catalyst for regenerating working solution for hydrogen peroxide synthesis

A palladium catalyst with a spinel-structured carrier and cerium support improves hydrogen peroxide production efficiency by enhancing palladium dispersion and durability, addressing catalyst inactivation issues.

JP7591144B2Active Publication Date: 2024-11-27HEESUNG CATALYSTS CORP
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
JP2023528754
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2020-11-16
Filing Date
2021-11-10
Publication Date
2024-11-27
Estimated Expiration
2041-11-10

AI Technical Summary

Technical Problem

Palladium-based catalysts used in hydrogen peroxide production suffer from decreased regeneration efficiency due to catalyst inactivation and co-catalyst desorption during the hydrogenation and oxidation steps, leading to reduced production efficiency and durability.

Method used

A palladium catalyst with a spinel-structured carrier and auxiliary metals like cerium is used, with palladium positioned in a ring shape inside the carrier to enhance dispersion and durability, preventing loss during reactions.

Benefits of technology

The catalyst exhibits high reaction selectivity, improved activity, and increased durability by maintaining active metal concentration and preventing physical abrasion, enhancing the regeneration efficiency of hydrogen peroxide production.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007591144000005
    Figure 0007591144000005
  • Figure 0007591144000006
    Figure 0007591144000006
  • Figure 0007591144000007
    Figure 0007591144000007
Patent Text Reader

Abstract

The present invention relates to a catalyst for a working solution for synthesizing hydrogen peroxide, a method for producing the same, and a method for regenerating the working solution, and more particularly to a palladium catalyst using a spinel support, which is used in the process of regenerating a working solution for hydrogen peroxide production, a method for producing the same, and a technology for regenerating a working solution using the same. The catalyst of the present invention exhibits high efficiency and high physical / chemical durability in the regeneration reaction or hydrogenation reaction.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a catalyst for a working solution for synthesizing hydrogen peroxide, a method for producing the same, and a method for regenerating the working solution, and more particularly to a palladium catalyst using a spinel carrier, which is used in a process for regenerating a working solution for producing hydrogen peroxide, a method for producing the same, and a technology for regenerating a working solution using the same. The catalyst of the present invention exhibits high efficiency and high physical / chemical durability in a regeneration reaction or a hydrogenation reaction. [Background technology]

[0002] Hydrogen peroxide is a compound used in various fields such as semiconductors, pharmaceuticals, and chemical synthesis. Hydrogen peroxide can be produced by a direct synthesis method using hydrogen and oxygen, or by the anthraquinone method using successive hydrogenation and oxidation steps from anthraquinone compounds. The technology for producing hydrogen peroxide using the anthraquinone method is described as follows.

[0003] [ka]

[0004] Hydrogen peroxide is produced by repeatedly hydrogenating and oxidizing a working solution (WS) in which alkylanthraquinone (usually called 2-ethylanthraquinone, EAQ) is dissolved in a suitable organic solvent. When these hydrogenating and oxidizing processes are repeated, by-products such as tetrahydroanthraquinone (THAQ) accumulate in the working solution, and the catalyst is deactivated due to the deposition of coke in the catalyst, reducing the efficiency of hydrogen peroxide production and regeneration. Summary of the Invention [Problem to be solved by the invention]

[0005] In particular, palladium catalysts used in the process of regenerating the by-product tetrahydroanthraquinone (THAQ) into anthraquinone are prepared by adding a co-catalyst such as magnesium to control the acid site of the support, but as the catalytic reaction is repeated, the co-catalyst fixed to the support gradually detaches from the catalyst, causing the regeneration reaction activity to gradually decrease, and therefore, the adhesion of the metal supported on the support is important for the durability of the catalyst. Therefore, the technical problem to be solved by the present invention is to provide a palladium catalyst having acid resistance and durability that can be used in the regeneration reaction of hydrogen peroxide working solution or the hydrogen peroxide production process, and a method for preparing the same. [Means for solving the problem]

[0006] In order to solve the above problems, the present inventors have used a carrier with controlled catalytic acid sites and pore structure, and have positioned a palladium active layer in a ring shape inside the carrier to increase the density of the active metal inside the carrier, and have improved the dispersion of palladium particles by introducing an auxiliary metal, thereby improving the reaction activity. In addition, the catalyst of the present invention has an active metal located inside the carrier, which suppresses the loss of the active metal due to wear during the reaction, thereby improving the durability of the catalyst.

[0007] Therefore, the above problems can be solved by an acid-resistant and heat-resistant palladium catalyst using a support with a spinel structure. Also, the above problems can be solved by a palladium catalyst using an auxiliary metal supported on a support with a spinel structure to improve palladium dispersion. Also, the durability / activity stability can be improved by a palladium catalyst with a ring structure inside the support.

[0008] The present invention provides a catalyst for regenerating a working solution for synthesizing hydrogen peroxide or for synthesizing hydrogen peroxide, in the form of a support having a spinel structure and palladium and an auxiliary metal supported thereon. The spinel structure is, but is not limited to, an aluminum-based spinel structure, and is preferably MgAl 2 O 4 , ZnAl 2 O 4 , CaAl 2 O4 , FeAl 2 O 4 , (Mg,Zn)Al 2 O 4 , (Mg,Fe)Al 2 O 4 The spinel structure may be an alumina-spinel composite oxide further containing alumina. In the catalyst of the present invention, the auxiliary metal may be selected from the group consisting of cerium, calcium, barium, strontium, zirconium, titanium, radium, silicon and aluminum. The catalyst support of the present invention may further contain at least one halogen component selected from the group consisting of chlorine, phosphorus and fluorine. In the present invention, palladium is present in the inside of the support in a ring shape separated from the surface of the support, and specifically, palladium may be present in the inside of the support at a distance of 5 to 10 μm from the surface of the support. Palladium, which is an active component in the catalyst of the present invention, is present in the support at a concentration of 0.005 to 0.16 wt % / m 2 and the auxiliary metal may be present in the support at an activity density of 0.0001 to 0.002 wt% / m 2 Alternatively, the halogen component may be present uniformly in the carrier at a density of 0.004 to 0.04 wt% / m 2 The carrier in the catalyst of the present invention can be uniformly present with a pore size of 7 to 14 nm and a density of 0.2 to 0.5 m. 3 / g pore volume and 70-200 m 2 The material may have a specific surface area of ​​100 / g. Effect of the Invention

[0009] The catalyst according to the present invention has a high reaction selectivity by suppressing the acid sites that induce side reactions inside the carrier, and has a cyclic structure in which the active metal is concentrated inside the carrier, and the introduction of the auxiliary metal induces high dispersion of palladium. The catalyst according to the present invention uses a magnesium aluminate spinel structure in which magnesium is located inside the carrier skeleton and can prevent magnesium from being removed when the catalyst is reused, and the auxiliary metal is used to position palladium on it to increase the degree of dispersion and increase the number of palladium active sites, thereby maximizing reaction activity. In addition, the palladium active metal can be preserved from the physical wear of the catalyst that occurs during the reaction, ensuring high durability. [Brief description of the drawings]

[0010] [Figure 1] 1 is a schematic structure of a catalyst according to the present invention. [Diagram 2] 1 shows XRD patterns of catalyst supports used in Examples 1 to 3 of the present invention. [Diagram 3] 1 is a SEM and EPMA image of a catalyst according to Example 1 of the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0011] The present invention will be described in detail below. The catalyst having durability / acid resistance disclosed by the present invention was developed as a catalyst for regenerating a working solution, but it can also be applied to a hydrogenation catalyst for producing hydrogen peroxide. In the present invention, the catalyst for regenerating a working solution is mainly described, but the application field is not limited to the regeneration reaction. In the present invention, the catalytic active component is supported on a carrier, and the carrier is also called a support.

[0012] The present invention relates to a palladium catalyst using a carrier with controlled acid sites as a spinel structure. The spinel structure used in the present invention generally has a structure in which X and Y metals are XY 2 O 4In the present invention, the spinel structure that can be particularly applied to the catalyst for producing hydrogen peroxide or for regenerating a working solution is an aluminum-based spinel structure MgAl 2 O 4 , ZnAl 2 O 4 , CaAl 2 O 4 , FeAl 2 O 4 , (Mg,Zn)Al 2 O 4 , (Mg,Fe)Al 2 O 4 The preferred form is Al, which can simultaneously utilize the large surface area of ​​alumina and the basicity of the spinel structure. 2 O 3 -XY 2 O 4 A composite oxide form can be used.

[0013] In the palladium catalyst according to the present invention, an auxiliary metal can be applied to the spinel-structured carrier to increase the dispersion of palladium. It is believed that the auxiliary metal can increase the number of active sites of palladium and maximize the reaction activity by increasing the degree of dispersion by positioning the catalytically active component thereon. A preferred example of the auxiliary metal is cerium, which induces high dispersion of palladium. In addition, calcium, barium, strontium, zirconium, titanium, radium, silicon, or aluminum can be used as the auxiliary metal.

[0014] Palladium, which is a catalytically active component in the palladium catalyst according to the present invention, is formed in a ring structure inside the carrier. The ring structure is a structure formed by concentrating catalytically active components in the interior spaced apart from the outer periphery of a catalyst having a normal circular structure, and no active components are present in the outer periphery or in the center of the catalyst. The presence or absence of ring formation and the thickness of the ring vary depending on the type and concentration of reagents used in the synthesis process, and the ring structure can preserve the active metal from the physical wear of the catalyst that occurs during the reaction, thereby maintaining high durability.

[0015] The present invention relates to a palladium catalyst and a method for producing the same, which is obtained by supporting cerium on a magnesium aluminate support having a spinel structure, which is prepared by heat-treating a mixture of magnesium and alumina, calcining the support to fix the cerium, impregnating the support with palladium, and reducing the support. When the catalyst is used in the regeneration process of a working solution, an efficient regeneration conversion rate is confirmed.

[0016] Example 1 Carrier preparation step: Magnesium nitrate (Mg(NO 3 ) 2 6H 2 O, Aldrich Co., Ltd.), aluminum nitrate (Al(NO 3 ) 3 9H 2 O, Aldrich Co., Ltd.) and aqueous ammonia (28 wt% NH 4 The carrier was manufactured using OH (Daejeong Chemical Co., Ltd.). First, magnesium nitrate was dissolved in distilled water, and then aluminum nitrate was dissolved in the distilled water at a molar ratio of Mg / Al of 0.5 to prepare an aqueous solution. Ammonia water was added to this aqueous solution to adjust the pH to 10.5 and stirred at room temperature for 12 hours, and then beads of about 100 microns in size were manufactured from which moisture had been removed using a spray dryer. The beads were then thoroughly dried at 105°C for 12 hours using a dryer. An oxide carrier (magnesium aluminate) with spinel crystallinity was obtained by heat treatment at 900°C for 10 hours.

[0017] Catalyst preparation step: Cerium, used as the auxiliary metal, was prepared by the synthesis of cerium nitrate (Ce(NO)) as a precursor. 3) 3 6H 2 O) was used as the active metal, and palladium was used as the precursor, palladium chloride (H 2 PdCl 4 ) was used. First, the magnesium aluminate support was mixed with ionized water in which cerium was dissolved, equivalent to 0.25% of the total weight of the catalyst. The composition with cerium supported was then heat-treated at 550°C for 2 hours in an air atmosphere to fix the metal. Then, a palladium precursor equivalent to 1.0% of the total weight of the catalyst and hydrogen peroxide (H 2 O 2 ) and 0.2% equivalent of HCl were added, and the mixture was heated to 80° C. with stirring and maintained at that temperature for 1 hour.

[0018] Catalyst reduction step: A reducing agent was added to the cerium-palladium supported composite. Sodium formate (NaCOOH) was used as the reducing agent. The temperature was raised to 60°C so that Na could be ionized during reduction to generate sufficient hydrogen, and the temperature was maintained for 1 hour to complete the catalyst shown in Figure 1.

[0019] Catalyst properties: Cerium was uniformly distributed inside the support. Palladium showed a ring structure that was mainly distributed at a distance of 15 μm from the outer periphery of the support. The active density of palladium in the catalyst was 0.1559 wt% / m 2 The activity density referred to in the present invention means the amount of active metal per surface area of ​​the support where the active metal is located, and a high value of this value means a large number of metal active sites capable of causing a reaction within a certain volume of support, which is understood as a value proportional to the catalytic activity.

[0020] Example 2 A catalyst was produced in the same manner as in Example 1, except that the heat treatment temperature in the carrier production step was 700°C.

[0021] Catalyst properties: The support crystal phase was a mixture of alumina and magnesium aluminate phases, and the active metal had a ring-shaped structure similar to Example 1. Palladium showed a ring structure that was mainly distributed at a distance of 16 μm from the outer periphery of the support, and the active density of palladium in the prepared catalyst was 0.0679 wt% / m 2 It was calculated that:

[0022] Example 3 A catalyst was produced in the same manner as in Example 1, except that the heat treatment temperature in the carrier production step was 500°C.

[0023] Catalyst properties: The support crystal phase was an alumina phase, and the active metal showed a ring-shaped structure similar to that of Example 1. Palladium showed a ring structure distributed at a thickness of 14 μm mainly away from the outer periphery of the support, and the active density of palladium in the prepared catalyst was 0.0646 wt% / m 2 It was calculated that:

[0024] Comparative Example 1 A pure alumina carrier was used instead of a spinel structure carrier. Thus, magnesium was supported on the alumina carrier by impregnation. First, magnesium nitrate equivalent to 4.5% and cerium nitrate equivalent to 0.25% of the total weight of the catalyst were mixed with ionized water. The prepared magnesium-cerium composite solution was impregnated into the alumina carrier by dry wetting. The composition supporting magnesium-cerium was heat-treated at 550°C for 2 hours in an air atmosphere to fix the metal. Then, 100g of the alumina composition supporting magnesium-cerium was added to 200ml of water, and palladium precursor equivalent to 1.0%, hydrogen peroxide equivalent to 1.0%, and HCl equivalent to 0.2% of the total weight of the catalyst were added, and the temperature was raised to 80°C while stirring, and the temperature was maintained for 30 minutes.

[0025] The catalytic reduction process was carried out by adding a reducing agent to the magnesium-cerium-palladium supported composite. Sodium formate (NaCOOH) was used as the reducing agent. During the reduction, the temperature was raised to 60°C so that Na could be ionized to generate sufficient hydrogen, and the temperature was maintained for 1 hour.

[0026] Catalyst properties: Magnesium and cerium are uniformly distributed inside the support. Palladium mainly shows a ring structure with a thickness of 16 μm, which is separated from the outer periphery of the support. The palladium activity density in the prepared catalyst is 0.0491 wt% / m 2 It was calculated that:

[0027] Comparative Example 2 A catalyst was produced in the same manner as in Comparative Example 1, except that hydrogen peroxide was not used when supporting palladium.

[0028] Catalyst properties: Magnesium, cerium and palladium are uniformly distributed inside the carrier. The palladium activity density in the produced catalyst is 0.005wt% / m 2 It was calculated that:

[0029] Comparative Example 3 A catalyst was produced in the same manner as in Comparative Example 2, except that cerium was not supported. Catalyst properties: Magnesium and palladium are both uniformly distributed inside the support. The palladium activity density in the produced catalyst was 0.0051 wt% / m 2 It was calculated that:

[0030] Experimental example: Carrier characteristics The crystal phases and pore structures of the supports produced in Examples 1 to 3 and Comparative Examples 1 to 3 are shown in Table 1 and FIG.

[0031] [Table 1]

[0032] As can be seen from Table 1 and FIG. 2, the spinel structure of Examples 1 to 3 is determined by the calcination temperature of the support, and as the temperature increases, the specific surface area and pore volume decrease, but the pore size gradually increases. In FIG. 2, the diffraction peak of Example 3 has the crystallinity of alumina alone and does not form a spinel structure, and in the case of the 700°C heat-treated support of Example 2, alumina and spinel crystal phases are mixed. When the heat treatment temperature is increased to 900°C or higher as in Example 1, a pure spinel crystal phase is finally formed, and the pore size of the support is significantly increased as shown in Table 1. In view of this, it is possible to predict smooth diffusion and movement of reactants and products within the catalyst when this is used in an actual catalytic reaction.

[0033] Example 2: Physicochemical properties of palladium inside the support Table 2 shows the results of measuring the dispersion degree, particle size, and intra-particle palladium distribution of the catalysts of Examples 1 to 3 and Comparative Examples 1 to 3 using a chemisorption analyzer and an electron probe micro analyzer (EPMA).

[0034] [Table 2]

[0035] According to the analysis results in Table 2, it was confirmed that the palladium dispersion of Comparative Example 3 not carrying cerium was significantly lower than that of Examples 1-3 and Comparative Examples 1-2, and that the other examples, except for Comparative Example 3, generally showed high palladium dispersion and low palladium particle size. Based on the above results, it was confirmed that cerium is located on the surface of the carrier and plays a role in dispersing palladium metal into small particles evenly. The distribution of palladium in the catalyst particles was adjusted by hydrogen peroxide and hydrochloric acid, and palladium particles could be positioned in a ring shape on the surface of the catalyst using this. The palladium metal distribution in Examples 1-3 and Comparative Example 1 was produced at intervals of 5-8 μm from the outer periphery of the catalyst. It was confirmed that the thickness of the ring was distributed between 10-20 μm. Scanning electron microscope (SEM) and EPMA images of Example 1 are shown in FIG. 3.

[0036] Experimental Example 3: Catalyst regeneration efficiency A regeneration evaluation reaction was carried out to measure the regeneration efficiency of the catalysts in the Examples and Comparative Examples. The reactor was evaluated using a stirring reaction system made of SUS material. A magnetic bar was placed in the circular stirring reactor, and 10g of catalyst was added to 50g of by-product working solution generated during the hydrogenation reaction to measure the regeneration efficiency. The catalytic activity was expressed as a conversion rate and was calculated using the following formula: Conversion rate (%) = [(THAQ area value of working solution - THAQ area value of reactant) / (THAQ area value of working solution)] * 100

[0037] The activity analysis was performed using a liquid chromatography (LC) analyzer, and the palladium content was measured using an inductively coupled plasma spectrometry (ICP) analyzer, and the results are shown in Table 3. Table 3 shows the results of evaluating the THAQ->EAQ conversion rate using the catalysts prepared in the examples and comparative examples.

[0038] [Table 3]

[0039] The catalytic activity was evaluated to be better in Examples 1 to 3 and Comparative Example 1, in which palladium was supported in a ring shape, than in Comparative Examples 2 and 3, in which palladium was uniformly supported on the catalyst support. From the results, it was found that the concentration of metal active sites on the surface of the catalyst increases the frequency of contact with the reactants, and thus a faster catalytic reaction occurs. Among the ring-shaped catalysts, Example 1 in particular showed the highest activity, and it was found that the larger the pore size of the support, the easier the diffusion and movement of reactants and products within the catalyst, and the faster the reaction rate. Next, in order to show the catalyst durability, the activity evaluation results after 50 catalytic reactions and catalyst regeneration (heat treatment at 550°C for 6 hours) were performed showed that although the values ​​were lower than the initial activity, they were still the same as the initial activity procedure. There was almost no loss of magnesium content in Example 1, whereas there was some loss in the remaining Examples and Comparative Examples. It was also found that there was a correlation between the amount of magnesium loss and the activity results.

[0040] Finally, after applying physical impacts using a ball mill for 24 hours, only catalysts of a certain size were selected from which fine powders were removed and evaluated for reaction. When applying continuous impacts to the outside of the catalyst using a ball mill, the catalyst loses surface particles due to the external physical impacts, which is the same tendency in commercial processes. As a result of the evaluation of the catalyst milled for 24 hours, it was confirmed that the catalyst with palladium present in a ring shape maintained similar performance to the initial performance. This means that since there is no palladium on the outermost periphery of the ring-shaped catalyst, even if surface particles are lost, the loss of palladium active material is minimized. In the case of a homogeneous catalyst where the palladium active layer has no gap with the surface, the loss of catalyst surface particles means the loss of palladium active material. The results were confirmed from the analysis of the palladium content loss rate in the catalyst.

Claims

1. A catalyst for regenerating a working solution for synthesizing hydrogen peroxide, comprising palladium and cerium as an auxiliary metal supported on a carrier, wherein palladium is present in the form of a spherical shell apart from the surface of the carrier within the carrier, and the carrier has a spinel structure. A catalyst characterized by:

2. The spinel structure is an aluminum-based spinel structure, and is MgAl 2 O 4 , Z nAl 2 O 4 , CaAl 2 O 4 , FeAl 2 O 4 , (Mg,Zn)Al 2 O 4 , (Mg,Fe)Al 2 O 4 Selected from The catalyst according to claim 1.

3. The spinel structure is an alumina-spinel composite oxide further containing alumina. The catalyst according to claim 1.

4. The carrier further contains chlorine as a halogen component. The catalyst according to claim 1.

5. Inside the carrier, palladium is present at a distance of 5 to 10 μm from the surface of the carrier. The catalyst according to claim 1.

6. The palladium is present in the carrier at a concentration of 0.005 to 0.16 wt % / m 2 exists with an activity density of The catalyst according to claim 1.

7. The auxiliary metal is added to the support in an amount of 0.0001 to 0.002 wt % / m 2 exists uniformly at a density of The catalyst according to claim 1.

8. The halogen component is contained in the carrier at 0.004 to 0.04 wt % / m 2 exists uniformly at a density of The catalyst according to claim 4.

9. The support has a pore size of 7 to 14 nm and a 3 / g pore volume and 70-200 m 2 / g specific surface area The catalyst according to claim 1.

Citation Information

Patent Citations

  • JP1964-004474B

  • JP1974041040A

  • Noble metal support, and method of producing acrylic acid ester and / or methacrylic acid ester

    JP2008161869A

  • Manufacturing method of regeneration catalyst for working solution used for hydrogen peroxide production

    JP2009034663A