Polyarylene sulfide resin composition

The polyarylene sulfide resin composition uses inorganic nanotubes and fillers to enhance crystallization and reduce burrs, addressing slow crystallization and burr formation issues while ensuring insulation and moldability.

JP7591396B2Active Publication Date: 2024-11-28POLYPLASTICS CO LTD
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
JP2020210089
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2020-12-18
Publication Date
2024-11-28
Estimated Expiration
2040-12-18

Smart Images

  • Figure 0007591396000001
    Figure 0007591396000001
Patent Text Reader

Abstract

To provide a polyarylene sulfide resin composition with less occurrence of burrs.SOLUTION: The polyarylene sulfide resin composition contains 0.01 pt.mass or more and less than 10 pts.mass of inorganic nanotubes (limited to ones containing no carbon atoms) based on 100 pts.mass of a polyarylene sulfide resin having a melt viscosity of 5-500 Pa s as measured at a temperature of 310°C and a shear rate of 1,200 sec-1. The inorganic nanotubes are preferably one kind selected from the group consisting of aluminosilicate nanotubes, boron nitride nanotubes, titanium oxide nanotubes, metal sulfide nanotubes, and metal halide nanotubes.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a polyarylene sulfide resin composition. [Background technology]

[0002] Polyarylene sulfide resins (hereinafter sometimes referred to as "PAS resins"), such as polyphenylene sulfide resins (hereinafter sometimes referred to as "PPS resins"), have high heat resistance, mechanical properties, chemical resistance, dimensional stability, and flame retardancy, and are therefore widely used as materials for electrical and electronic equipment parts, automotive equipment parts, chemical equipment parts, etc. However, PAS resins have problems such as long molding cycle times due to their slow crystallization rate, and frequent generation of burrs during molding.

[0003] As a method for reducing the occurrence of burrs, the addition of various alkoxysilane compounds is known (see Patent Documents 1 and 2). teeth PAS resin With It is known to have high reactivity, improved mechanical properties, and the effect of suppressing burr generation, etc. However, there is a limit to the effect of suppressing burr generation, and it does not fully satisfy market demand, and it does not have the effect of accelerating the crystallization speed.

[0004] In order to solve the above problems, a resin composition has been proposed in which a specific PAS resin is blended with specific carbon nanotubes and, if necessary, specific amounts of an inorganic filler (see Patent Document 3).In addition, a resin composition has been proposed that contains two types of PPS resins with different melt viscosities and kaolin, attapulgite, or a mixture thereof, each having a specific average particle size (see Patent Document 4). [Prior art documents] [Patent documents]

[0005] [Patent Document 1] Special Publication No. 6-21169 [Patent Document 2] Japanese Unexamined Patent Publication No. 1-146955 [Patent Document 3] JP 2006-143827 A [Patent Document 4] Japanese Patent Application Publication No. 09-157525 Summary of the Invention [Problem to be solved by the invention]

[0006] In order to sufficiently suppress the occurrence of burrs, the resin composition described in Patent Document 3 needs to add a relatively large amount of carbon nanotubes. In that case, the resin composition will have electrical conductivity due to the electrical conductivity of the carbon nanotubes. Such a resin composition cannot be used for molded products that require insulation. In addition, Patent Document 4 describes that kaolin, attapulgite, or a mixture thereof having a predetermined average particle size "is thought to have the effect of imparting thixotropy to the material (the effect of increasing the shear rate dependency of the melt viscosity), and the occurrence of burrs is thought to be significantly reduced by suddenly increasing the melt viscosity of the material during the pressure holding process (the process in which the shear rate decreases) in injection molding." In other words, since inorganic fillers such as kaolin are used for the purpose of suddenly increasing the melt viscosity of the material in injection molding, it is thought that a certain amount or more is necessary, and it is actually described that 10 to 150 parts by weight are preferable for 100 parts by weight of the PPS resin composition. Although the occurrence of burrs can be suppressed by adding inorganic fillers such as kaolin, there is a concern that other problems such as reduced moldability and strength may occur due to the large amount added.

[0007] The present invention has been made in consideration of the above-mentioned problems in the conventional art, and an object of the present invention is to provide a polyarylene sulfide resin composition which produces little burrs. [Means for solving the problem]

[0008] One aspect of the present invention that solves the above problems is as follows. (1) Temperature 310℃ and shear rate 1200sec -1A polyarylene sulfide resin composition comprising 100 parts by mass of a polyarylene sulfide resin having a melt viscosity of 5 to 500 Pa·s as measured by a method according to claim 1, and 0.01 part by mass or more and less than 10 parts by mass of inorganic nanotubes (limited to those containing no carbon atoms).

[0009] (2) The polyarylene sulfide resin composition according to (1) above, wherein the inorganic nanotubes are one selected from the group consisting of aluminosilicate nanotubes, boron nitride nanotubes, titanium oxide nanotubes, metal sulfide nanotubes, and metal halide nanotubes.

[0010] (3) The polyarylene sulfide resin composition according to (2) above, wherein the aluminosilicate nanotubes are halloysite nanotubes or metahalloysite nanotubes.

[0011] (4) The polyarylene sulfide resin composition according to any one of (1) to (3), further comprising 5 to 250 parts by mass of a non-conductive inorganic filler (excluding the inorganic nanotubes) per 100 parts by mass of the polyarylene sulfide resin.

[0012] (5) The polyarylene sulfide resin composition according to (4) above, wherein the non-conductive inorganic filler is one or more selected from the group consisting of glass fibers, glass beads, glass flakes, calcium carbonate and talc. Effect of the Invention

[0013] According to the present invention, it is possible to provide a polyarylene sulfide resin composition which produces little burrs. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0014] The polyarylene sulfide resin composition of the present embodiment was subjected to a shear rate of 1200 sec at a temperature of 310°C. -1The composition contains 0.01 part by mass or more and less than 10 parts by mass of inorganic nanotubes (limited to those containing no carbon atoms) per 100 parts by mass of polyarylene sulfide resin having a melt viscosity of 5 to 500 Pa·s as measured by the method described above.

[0015] The PAS resin composition of this embodiment contains inorganic nanotubes, thereby suppressing the generation of burrs. It is presumed that the mechanism by which the addition of inorganic nanotubes suppresses burrs is due to an improvement in the crystallization speed (improved solidification speed due to the nucleating agent effect). In addition, the improvement in the crystallization speed can shorten the molding cycle. Furthermore, since inorganic nanotubes are generally insulating, the insulating properties of the PAS resin composition are not reduced by using insulating inorganic nanotubes. In this respect, it differs from those that use carbon nanotubes. Each component of the PAS resin composition of the present embodiment will be described below.

[0016] [Polyarylene sulfide resin] PAS resin is characterized by its excellent mechanical properties, electrical properties, heat resistance and other physical and chemical properties, as well as its good processability. PAS resin is a polymeric compound mainly composed of a repeating unit -(Ar-S)- (where Ar is an arylene group), and in this embodiment, a PAS resin with a generally known molecular structure can be used.

[0017] Examples of the arylene group include p-phenylene, m-phenylene, o-phenylene, substituted phenylene, p,p'-diphenylenesulfone, p,p'-biphenylene, p,p'-diphenyleneether, p,p'-diphenylenecarbonyl, naphthalene, etc. The PAS resin may be a homopolymer consisting of the above repeating units, or a copolymer containing the following different repeating units may be preferred from the standpoint of processability, etc.

[0018] As the homopolymer, a polyphenylene sulfide resin using p-phenylene group as an arylene group and having p-phenylene sulfide group as a repeating unit is preferably used. As the copolymer, a combination of two or more different arylene sulfide groups consisting of the above-mentioned arylene groups can be used, and a combination containing p-phenylene sulfide group and m-phenylene sulfide group is particularly preferably used. Among them, a combination containing 70 mol % or more, preferably 80 mol % or more of p-phenylene sulfide group is suitable from the viewpoint of physical properties such as heat resistance, moldability, and mechanical properties. Among these PAS resins, a high molecular weight polymer having a substantially linear structure obtained by condensation polymerization from a monomer mainly composed of a bifunctional halogenated aromatic compound is particularly preferably used. The PAS resin used in this embodiment may be a mixture of PAS resins having two or more different molecular weights.

[0019] In addition to the linear PAS resin, examples of the polymer include a polymer in which a partially branched structure or crosslinked structure is formed by using a small amount of a monomer such as a polyhaloaromatic compound having three or more halogen substituents during condensation polymerization, and a polymer in which the melt viscosity is increased by oxidative crosslinking or thermal crosslinking by heating a low molecular weight linear polymer at high temperature in the presence of oxygen or the like, thereby improving moldability.

[0020] The melt viscosity of the PAS resin used as the base resin in this embodiment (310°C, shear rate 1200 sec -1 From the viewpoint of the balance between mechanical properties and fluidity, the melt viscosity of the PAS resin is preferably 5 to 500 Pa·s, including the case of the above-mentioned mixed system. The melt viscosity of the PAS resin is preferably 7 to 300 Pa·s, more preferably 10 to 250 Pa·s, and particularly preferably 13 to 200 Pa·s.

[0021] The PAS resin composition of the present embodiment may contain other resin components in addition to the PAS resin as a resin component, within a range that does not impair the effect. The other resin components are not particularly limited, and examples thereof include polyethylene resin, polypropylene resin, polyamide resin, polyacetal resin, modified polyphenylene ether resin, polyethylene terephthalate resin, polybutylene terephthalate resin, polyethylene naphthalate resin, polyimide resin, polyamideimide resin, polyetherimide resin, polysulfone resin, polyethersulfone resin, polyetherketone resin, polyetheretherketone resin, liquid crystal resin, fluorine resin, cyclic olefin resin (cyclic olefin polymer, cyclic olefin copolymer, etc.), thermoplastic elastomer, silicone polymer, various biodegradable resins, etc. Two or more types of resin components may be used in combination. Among them, polyamide resin, modified polyphenylene ether resin, liquid crystal resin, etc. are preferably used from the viewpoints of mechanical properties, electrical properties, physical and chemical properties, processability, etc.

[0022] [Inorganic nanotubes] In this embodiment, inorganic nanotubes are used for the purpose of suppressing the occurrence of burrs. As described above, the suppression of burr occurrence by inorganic nanotubes is believed to be due to the improvement of the solidification speed due to the nucleating agent effect. Therefore, even if a relatively small amount is added, the occurrence of burrs can be suppressed. Note that in this embodiment, inorganic nanotubes are limited to those that do not contain carbon atoms. Therefore, inorganic nanotubes do not include carbon nanotubes. Note that inorganic nanotubes are tubular inorganic substances with diameters on the order of nanometers.

[0023] Examples of inorganic nanotubes used in this embodiment include aluminosilicate nanotubes, boron nitride nanotubes, titanium oxide nanotubes, metal sulfide nanotubes, and metal halide nanotubes. As the aluminosilicate nanotubes, halloysite nanotubes or metahalloysite nanotubes are preferred. Among these, halloysite nanotubes are preferred from the viewpoints of low cost and easy availability. Examples of metal sulfide nanotubes include molybdenum, tungsten, or copper sulfide nanotubes, etc. Examples of metal halide nanotubes include nickel chloride, cadmium chloride, or cadmium iodide nanotubes, etc.

[0024] In this embodiment, the average length of the inorganic nanotubes is preferably 100 nm to 20 μm, more preferably 500 nm to 15 μm, even more preferably 1 to 10 μm, and particularly preferably 1 to 5 μm. The average outer diameter of the inorganic nanotubes is preferably 5 to 100 nm, more preferably 10 to 80 nm, and even more preferably 30 to 70 μm. The aspect ratio of the inorganic nanotubes is preferably 1 to 4000, and more preferably 5 to 2000. Here, the aspect ratio of an inorganic nanotube is a value obtained by dividing the length of the inorganic nanotube by the diameter of the inorganic nanotube, and the manufacturer's value (a value published by the manufacturer in a catalog or the like) can be used.

[0025] In the PAS resin composition of the present embodiment, the inorganic nanotubes are contained in an amount of 0.01 parts by mass or more and less than 10 parts by mass per 100 parts by mass of the PAS resin. If the amount is less than 0.01 parts by mass, the effect of suppressing burr generation becomes insufficient, and if the amount is 10 parts by mass or more, mechanical properties such as Charpy impact strength tend to deteriorate. The content of the inorganic nanotubes is preferably 0.5 to 9.9 parts by mass, more preferably 1.0 to 9.5 parts by mass.

[0026] Among the inorganic nanotubes according to this embodiment, examples of the halloysite nanotubes on the market include "Halloysite G (685445)" manufactured by Applied Minerals.

[0027] [Non-conductive inorganic filler] In this embodiment, it is preferable to include a non-conductive inorganic filler in the PAS resin composition from the viewpoint of improving mechanical properties while ensuring insulation. Examples of the non-conductive inorganic filler include fibrous inorganic fillers, plate-like inorganic fillers, and granular inorganic fillers, and one of these may be used alone or two or more may be used in combination. In this specification, when the term "inorganic filler" is used, it means a non-conductive inorganic filler unless it is clearly stated that it is a conductive filler.

[0028] Examples of the fibrous inorganic filler include mineral fibers such as glass fibers, whiskers, wollastonite, zinc oxide fibers, titanium oxide fibers, silica fibers, silica-alumina fibers, boron nitride fibers, silicon nitride fibers, boron fibers, and potassium titanate fibers, and metal fibrous materials such as titanium fibers, and these can be used alone or in combination of two or more. Among these, glass fibers are preferred.

[0029] Examples of commercially available glass fibers include chopped glass fiber (ECS03T-790DE, average fiber diameter: 6 μm) manufactured by Nippon Electric Glass Co., Ltd., and Owens Corning Japan N Examples of such glass fibers include chopped glass fiber (CS03DE 416A, average fiber diameter: 6 μm) manufactured by the same company, chopped glass fiber (ECS03T-747H, average fiber diameter: 10.5 μm) manufactured by Nippon Electric Glass Co., Ltd., chopped glass fiber (ECS03T-747, average fiber diameter: 13 μm) manufactured by Nippon Electric Glass Co., Ltd., irregular cross section chopped strand CSG 3PA-830 (long diameter 28 μm, short diameter 7 μm) manufactured by Nitto Boseki Co., Ltd., and irregular cross section chopped strand CSG 3PL-962 (long diameter 20 μm, short diameter 10 μm) manufactured by Nitto Boseki Co., Ltd.

[0030] The fibrous inorganic filler may be surface-treated with various surface treatment agents such as commonly known epoxy compounds, isocyanate compounds, silane compounds, titanate compounds, fatty acids, etc. The surface treatment can improve adhesion to the PAS resin. The surface treatment agent may be applied to the fibrous inorganic filler in advance before the material is prepared to perform surface treatment or convergence treatment, or may be added simultaneously when the material is prepared.

[0031] The fiber diameter of the fibrous inorganic filler is not particularly limited, but may be, for example, 5 μm or more and 30 μm or less in the initial shape (shape before melt kneading). Here, the fiber diameter of the fibrous inorganic filler refers to the major axis of the fiber cross section of the fibrous inorganic filler.

[0032] Examples of the powdered and granular inorganic filler include talc (granular), silica, quartz powder, glass beads, glass powder, silicates such as calcium silicate, aluminum silicate, and diatomaceous earth, metal oxides that do not have electrical conductivity such as iron oxide, zinc oxide, and alumina (granular), metal carbonates such as calcium carbonate and magnesium carbonate, metal sulfates such as calcium sulfate and barium sulfate, and other nitrides such as silicon carbide, silicon nitride, boron nitride, and aluminum nitride, poorly soluble ion crystal particles such as calcium fluoride and barium fluoride; and fillers using semiconductor materials (element semiconductors such as Si, Ge, Se, and Te; compound semiconductors such as oxide semiconductors, etc.), and these can be used alone or in combination. Among these, glass beads and calcium carbonate are preferred. Examples of commercially available calcium carbonate products include Whiten P-30 (average particle size (50% d): 5 μm) manufactured by Toyo Fine Chemical Co., Ltd. Examples of commercially available glass beads include EGB731A (average particle size (50% d): 20 μm) manufactured by Potters Barotini Co., Ltd. and EMB-10 (average particle size (50% d): 5 μm) manufactured by Potters Barotini Co., Ltd. The powdered inorganic filler may also be surface-treated like the fibrous inorganic filler.

[0033] Examples of the plate-like inorganic filler include glass flakes, talc (plate-like), mica, kaolin, clay, alumina (plate-like), etc., and these can be used alone or in combination of two or more. Among these, glass flakes and talc are preferred. Examples of glass flakes on the market include REFG-108 (average particle size (50% d): 623 μm) manufactured by Nippon Sheet Glass Co., Ltd., Fine Flake (average particle size (50% d): 169 μm) manufactured by Nippon Sheet Glass Co., Ltd., REFG-301 (average particle size (50% d): 155 μm) manufactured by Nippon Sheet Glass Co., Ltd., and REFG-401 (average particle size (50% d): 310 μm) manufactured by Nippon Sheet Glass Co., Ltd. Examples of talc products on the market include Crown Talc PP manufactured by Matsumura Sangyo Co., Ltd. and Talcan Powder PKNN manufactured by Hayashi Kasei Co., Ltd. The plate-like inorganic filler may also be surface-treated in the same manner as the fibrous inorganic filler.

[0034] In the present embodiment, among the above inorganic fillers, one or more selected from the group consisting of glass fiber, glass beads, glass flakes, calcium carbonate, and talc are preferred. In addition, from the viewpoint of improving mechanical properties, the inorganic filler (However, this does not include inorganic nanotubes.) is for 100 parts by mass of PAS resin It is preferable that the content is 5 to 250 parts by mass, Contains 15 to 200 parts by weight twist Preferably, the content is 25 to 150 parts by mass. Furthermore Preferably, the content is 30 to 110 parts by mass. especially preferable.

[0035] As described above, the PAS resin composition of the present embodiment preferably contains a non-conductive inorganic filler, but may contain a conductive inorganic filler as long as the effect of the present embodiment is not hindered. When the PAS resin composition of the present embodiment contains a conductive inorganic filler, the content of the conductive inorganic filler is an amount that allows the molded article to exhibit electrical insulation, specifically, an amount that allows the molded article to exhibit volume resistivity at room temperature (23°C) of 1 x 10 14It is preferable to use an amount that can maintain the conductivity at Ω·cm or more. The term "conductive inorganic filler" is well known to those skilled in the art, and means an inorganic filler having conductivity such as carbon-based fillers (carbon black, carbon fiber, graphite, etc.), metal-based fillers (metal fibers having conductivity such as SUS fiber, metal or metal oxide powder having conductivity, etc.), and metal surface-coated fillers. In one embodiment, the content of these conductive inorganic fillers is, for example, 10 mass % or less of the entire PAS resin composition of this embodiment, preferably 6 mass % or less, and more preferably 4 mass % or less. The content at which the conductive inorganic filler can exhibit conductivity may vary depending on the type, shape, and conductivity of the conductive inorganic filler, so even if the content is more than the above amount, good There are cases like this.

[0036] [Other ingredients] In this embodiment, in addition to the above-mentioned components, in order to impart desired properties according to the purpose, known additives generally added to thermoplastic resins and thermosetting resins, namely, elastomers, release agents, lubricants, plasticizers, flame retardants, colorants such as dyes and pigments, crystallization accelerators, crystal nucleating agents, various antioxidants, heat stabilizers, weather resistance stabilizers, corrosion inhibitors, etc. may be blended within a range that does not impair the effects of the composition. Although the generation of burrs can be suppressed by the PAS resin composition of this embodiment, a burr suppressor such as an alkoxysilane compound may be used in combination, if necessary.

[0037] The method for producing a molded article using the PAS resin composition of the present embodiment is not particularly limited, and any known method can be used. For example, the PAS resin composition of the present embodiment can be fed into an extruder, melt-kneaded and pelletized, and the pellets can be fed into an injection molding machine equipped with a predetermined mold and injection molded to produce a molded article.

[0038] Examples of molded articles obtained by molding the PAS resin composition of the present embodiment include materials for electric / electronic equipment parts, materials for automobile equipment parts, materials for chemical equipment parts, materials for water-related parts, etc. Specific examples include various cooling system parts for automobiles, ignition-related parts, distributor parts, various sensor parts, various actuator parts, throttle parts, power module parts, ECU parts, various connector parts, piping joints (pipe joints), joints, etc. Other applications include electrical and electronic components such as LEDs, sensors, sockets, terminal blocks, printed circuit boards, motor parts, ECU cases, lighting components, television components, rice cooker components, microwave oven components, iron components, copier-related components, printer-related components, facsimile-related components, heaters, air conditioner components, and other home and office electrical appliance components. EXAMPLES

[0039] The present embodiment will be described in more detail below with reference to examples, but the present embodiment is not limited to the following examples. Unless otherwise specified, commercially available products were used as raw materials.

[0040] [Examples 1 to 7, Comparative Examples 1 to 2] In each of the Examples and Comparative Examples, the raw material components shown in Table 1 were dry blended and then fed into a twin-screw extruder with a cylinder temperature of 320°C (glass fiber was two-axis The components were added separately through the side feed of the extruder, melt-kneaded, and pelletized. In Table 1, the numerical values ​​for each component indicate parts by mass. The details of each raw material component used are shown below.

[0041] (1)PAS resin PPS resin: Fortron KPS, manufactured by Kureha Corporation (melt viscosity: 30 Pa·s (shear rate: 1200 sec -1 , 310℃)

[0042] (Melt viscosity measurement of PPS resin) The melt viscosity of the PPS resin was measured as follows. A Capillograph manufactured by Toyo Seiki Seisakusho Co., Ltd. was used, and a flat die of 1 mm diameter x 20 mm length was used as the capillary. The barrel temperature was 310°C, and the shear rate was 1200 sec. -1 The melt viscosity at 100° C. was measured.

[0043] (2) Inorganic nanotubes Applied Minerals, "Halloysite G (685445)" (average diameter: 50 nm, average inner diameter: 15 nm)

[0044] (3) Non-conductive inorganic filler Glass fiber: Owens Corning Gu Ji Japa N Manufactured by the same company, chopped strand, fiber diameter: 10.5 μm, length: 3 mm

[0045] [evaluation] The pellets obtained in each of the Examples and Comparative Examples were evaluated as follows. (1) Burr length Using a mold with a disk-shaped cavity, with a burr measurement section with a 20μm mold gap on the outer periphery, injection molding was performed at a cylinder temperature of 320℃, a mold temperature of 150℃, and the minimum pressure required to completely fill the cavity, and the burr length generated in that section was measured under magnification using a projection device. The measurement results are shown in Table 1.

[0046] (2) Melt Viscosity of Resin Composition A Capillograph manufactured by Toyo Seiki Seisakusho Co., Ltd. was used, and a flat die of 1 mm diameter x 20 mm length was used as the capillary. The barrel temperature was 310°C, and the shear rate was 1000 sec. -1 The melt viscosity (MV) was measured at 100°C. The measurement results are shown in Table 1. A melt viscosity of 500 Pa·s or less can be said to have excellent fluidity.

[0047] (3) Charpy impact strength Test pieces (width 10 mm, thickness 4 mmt) were prepared according to ISO3167 by injection molding at a cylinder temperature of 320°C and a mold temperature of 150°C. Using these test pieces, the Charpy impact strength (kJ / m2 The measurement results are shown in Table 1.

[0048] [Table 1]

[0049] From Table 1, it can be seen that the generation of burrs is suppressed in Examples 1 to 7 compared to Comparative Example 1. Also, the Charpy impact strength in Examples 1 to 7 is slightly lower than that in Comparative Example 1, but is within an acceptable range. On the other hand, in Comparative Example 2 in which an excessive amount of inorganic nanotubes was added, it can be seen that the generation of burrs is suppressed, but the Charpy impact strength is significantly reduced. From the above, it can be seen that by adding a specified amount of inorganic nanotubes to a PAS resin composition, it is possible to suppress the occurrence of burrs and also to suppress a decrease in Charpy impact strength.

Claims

1. Temperature 310℃ and shear rate 1200sec -1 A polyarylene sulfide resin composition comprising 100 parts by weight of a polyarylene sulfide resin having a melt viscosity of 5 to 500 Pa·s as measured by a method according to claim 1, and 0.01 parts by weight or more and less than 10 parts by weight of inorganic nanotubes (limited to those containing no carbon atoms) (excluding polyphenylene sulfide resin compositions consisting of 100 parts by weight of a polyphenylene sulfide resin and 0.01 to 100 parts by weight of boron nitride nanotubes).

2. 2. The polyarylene sulfide resin composition according to claim 1, wherein the inorganic nanotubes are one selected from the group consisting of aluminosilicate nanotubes, boron nitride nanotubes, titanium oxide nanotubes, metal sulfide nanotubes, and metal halide nanotubes.

3. The polyarylene sulfide resin composition according to claim 2, wherein the aluminosilicate nanotubes are halloysite nanotubes or metahalloysite nanotubes.

4. The polyarylene sulfide resin composition according to any one of claims 1 to 3, further comprising 5 to 250 parts by mass of a non-conductive inorganic filler (excluding the inorganic nanotubes) per 100 parts by mass of the polyarylene sulfide resin.

5. 5. The polyarylene sulfide resin composition according to claim 4, wherein the non-conductive inorganic filler is one or more selected from the group consisting of glass fibers, glass beads, glass flakes, calcium carbonate and talc.

6. A method for suppressing burrs in a polyarylene sulfide resin composition, comprising adding 0.01 part by mass or more and less than 10 parts by mass of inorganic nanotubes (limited to those containing no carbon atoms) to 100 parts by mass of a polyarylene sulfide resin having a melt viscosity of 5 to 500 Pa·s measured at a temperature of 310° C. and a shear rate of 1,200 sec -1 .

Citation Information

Patent Citations

  • Intrinsic type PPS / glass fiber / epoxy resin / nerchinskite micro-nano composite flame-retardance cable material and preparation method thereof

    CN106280456A

  • Polyphenylene sulfide resin composition and its production

    JP1989146955A

  • Wafer prober, IC prober, and their probing methods

    JP1994021169A

  • Polyphenylene sulfide resin composition for precision molding

    JP1997157525A

  • Polyarylene sulfide resin composition

    JP2006143827A