Method for producing transfer sheet and laminate
The laminate structure with a UV laser patterning method addresses the incomplete layer removal issue in transfer sheets, ensuring clean separation and maintaining product appearance by selectively removing the base color layer while preserving the anchor and release layers.
Patent Information
- Application Number
- JP2021064453
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2021-04-05
- Publication Date
- 2024-11-28
- Estimated Expiration
- 2041-04-05
AI Technical Summary
Conventional patterning methods using infrared lasers for transfer sheets result in incomplete removal of layers, leading to peeling marks and poor appearance due to partial peeling between the base sheet and release layer during laser patterning.
A laminate structure is used with a base sheet, a release layer, an anchor layer, and a block layer containing a transparent resin that does not easily absorb UV wavelengths, along with a base color layer, where the patterning is performed using a UV laser to selectively remove the base color layer while minimizing energy transfer to the anchor and release layers.
This method prevents peeling between the base sheet and release layer, ensuring a clean separation and maintaining the appearance of the decorated product by selectively removing the base color layer without affecting the underlying layers.
Smart Images

Figure 0007591455000001 
Figure 0007591455000002 
Figure 0007591455000003
Abstract
Description
[Technical field]
[0001] The present invention relates to a method for producing a transfer sheet and a laminate. [Background technology]
[0002] A method of using a decorative sheet when manufacturing molded products such as a cover panel for a home appliance or an interior panel for an automobile is known. When expressing a pattern such as an arbitrary character, symbol, or figure on a decorative sheet, there is a method of patterning a printed layer of the decorative sheet with a laser. With reference to FIG. 11(a), for example, Patent Document 1 describes a method of forming an arbitrary pattern by irradiating an infrared laser from the surface on which the light-shielding layer 230 is formed on a laminate in which a colored layer 220 and a light-shielding layer 230 are laminated in order on a base sheet 210. According to this method, even if it becomes necessary to add or change a pattern, or both, it is not necessary to prepare a new printing plate, and it is possible to easily manufacture a small amount of a wide variety of molded products.
[0003] However, the conventional patterning method is intended for a decorative sheet in which the base sheet remains in the molded product, and no patterning technology has yet been proposed for a transfer sheet in which the base sheet does not remain in the molded product. Therefore, it is conceivable to pattern a laminate in which the decorative sheet described in Patent Document 1 is replaced with a transfer sheet configuration by a laser. Referring to FIG. 11(b), the laminate 300 to be processed is formed by laminating a peeling layer 240, an anchor layer 250, a colored layer 220, and a light-shielding layer 230 on a base sheet 210 in this order. The peeling layer 240 is a layer for facilitating peeling of the base sheet 210, and the anchor layer 250 is a layer for bonding the peeling layer 240 and the colored layer 220 together. Referring to FIG. 11(c), when an infrared laser is irradiated from the surface on which the light-shielding layer 230 is formed, a transfer sheet 200 on which an arbitrary pattern is formed can be obtained. [Prior art documents] [Patent documents]
[0004] [Patent Document 1] JP 2001-30290 A Summary of the Invention [Problem to be solved by the invention]
[0005] However, in conventional patterning using an infrared laser, it is difficult to control the removal of only a desired layer (for example, the light-shielding layer 230), and as shown in FIG. 11(c), all layers from the light-shielding layer 230 to the peeling layer 240 are removed. At this time, partial peeling occurs between the base sheet 210 and the peeling layer 240 due to the impact when the peeling layer 240 is removed by the infrared laser. In this state, if the transfer sheet 200 and an injection-molded product are integrated by, for example, a simultaneous molding and decoration method and the base sheet 210 is peeled off, a peeling mark will be left on the decorated product. In other words, the use of a transfer sheet that has been subjected to conventional patterning using an infrared laser can cause poor appearance of the decorated product.
[0006] The present invention has been made to solve the above-mentioned problems, and aims to provide a laminate in which peeling is less likely to occur between a base sheet and a release layer during laser patterning, and a method for manufacturing a transfer sheet using such a laminate. [Means for solving the problem]
[0007] In order to achieve the above-mentioned object, the first invention is a method for manufacturing a transfer sheet, which includes a laminate formation process including at least the steps of laminating a release layer on a base sheet, laminating an anchor layer on the release layer, laminating a block layer containing a transparent resin that does not easily absorb UV wavelengths on the anchor layer, and laminating a base color layer on the block layer, and a process of forming an arbitrary pattern having holes that penetrate the base color layer by irradiating a UV laser onto the base color layer from the side of the laminate on which the base color layer is formed.
[0008] In addition, in order to achieve the above-mentioned object, a second invention is a method for manufacturing a transfer sheet, which includes the steps of preparing a laminate in which at least a release layer, an anchor layer, a block layer containing a transparent resin that does not easily absorb UV wavelengths, and a base color layer are laminated in that order on a base sheet, and forming an arbitrary pattern having holes that penetrate the base color layer by irradiating a UV laser onto the base color layer from the side of the laminate on which the base color layer is formed.
[0009] When configured as in the first or second invention, the energy of the UV laser attenuated by removing the base color layer is absorbed by the block layer and further attenuated, but the attenuated energy does not remove the anchor layer and the release layer, and only the base color layer is removed. Since the release layer laminated on the base sheet is not removed, peeling is unlikely to occur between the base sheet and the release layer.
[0010] A third invention is a method for producing a transfer sheet according to the first or second invention, wherein the base color layer is black-based and the block layer is one layer. In this configuration, most of the UV laser energy is absorbed by the base color layer and used to remove the base color layer. In other words, most of the UV laser energy is attenuated by the base color layer. The remaining energy is then attenuated to a level that does not remove the anchor layer and release layer by passing through the blocking layer, which does not easily absorb UV wavelengths. This makes it possible to more reliably prevent peeling between the base sheet and the release layer.
[0011] A fourth invention is a method for producing a transfer sheet according to the first or second invention, wherein the base color layer is white-based and the block layer is two or more layers. In this configuration, the UV laser energy is not easily absorbed by the base color layer, i.e., is not easily attenuated by the base color layer, so most of the UV laser energy reaches the block layer. However, the UV laser energy is attenuated to a degree that does not remove the anchor layer and the release layer by passing through multiple block layers that do not easily absorb UV wavelengths. Therefore, peeling between the base sheet and the release layer can be more reliably prevented.
[0012] A fifth invention is a method for producing a transfer sheet, in any of the first to fourth inventions, wherein the transparent resin contained in the block layer is one selected from the group consisting of vinyl chloride-vinyl acetate copolymer resin, polyacetal resin, polycarbonate resin, and acrylic resin.
[0013] The sixth invention is a method for manufacturing a transfer sheet, which includes a step of forming a pattern color layer of a different color from the base color layer on top of a base color layer of a laminate on which a pattern is formed, so as to fill the holes, in any of the first to fifth inventions. In this configuration, the holes are formed by a UV laser, so the edges are clear, and the holes are filled with a pattern color layer that is a different color from the base color layer, making it easier to see any pattern.
[0014] In addition, in order to achieve the above-mentioned object, a seventh invention is a laminate including a base sheet, a release layer laminated on the base sheet, an anchor layer laminated on the release layer, a block layer laminated on the anchor layer and containing a transparent resin that does not easily absorb UV wavelengths, and a base color layer laminated on the block layer.
[0015] With this configuration, when a UV laser is irradiated from the side where the base color layer is formed to form an arbitrary pattern, the energy of the UV laser attenuated by removing the base color layer is further attenuated by passing through the block layer, which does not easily absorb UV wavelengths, and the attenuated energy does not remove the anchor layer and release layer, but only the base color layer. Because the release layer laminated on the base sheet is not removed, peeling is unlikely to occur between the base sheet and the release layer. Effect of the Invention
[0016] According to the laminate of the present invention and the method for producing a transfer sheet using the same, peeling is unlikely to occur between the base sheet and the release layer during patterning by laser. [Brief description of the drawings]
[0017] [Figure 1] 1A is a schematic cross-sectional view showing a first embodiment of a laminate, and FIG. 1B is a schematic cross-sectional view showing a first embodiment of a method for producing a transfer sheet. [Diagram 2] The left side is a schematic cross-sectional view showing how the laminate of the first embodiment is patterned with a UV laser, and the right side is a schematic view showing the attenuation tendency of the UV laser energy. [Diagram 3] 1A is a schematic cross-sectional view showing a second embodiment of a laminate, and FIG. 1B is a schematic cross-sectional view showing a second embodiment of a method for producing a transfer sheet. [Figure 4] The left side is a schematic cross-sectional view showing how the laminate of the second embodiment is patterned with a UV laser, and the right side is a schematic view showing the attenuation tendency of the UV laser energy. [Diagram 5] FIG. 2 is a schematic cross-sectional view showing an example of a decorative product using the transfer sheet of the first embodiment. [Figure 6] FIG. 11 is a schematic cross-sectional view showing an example of a decorative product using the transfer sheet of the second embodiment. [Figure 7] FIG. 11 is a schematic cross-sectional view showing another embodiment of the transfer sheet. [Figure 8] FIG. 11 is a schematic cross-sectional view showing another embodiment of the transfer sheet. [Figure 9]FIG. 11 is a schematic cross-sectional view showing another embodiment of the transfer sheet. [Figure 10] FIG. 11 is a schematic cross-sectional view showing another embodiment of the transfer sheet. [Figure 11] (a) A schematic cross-sectional view showing a conventional method for producing a decorative sheet, (b) A schematic cross-sectional view in which the decorative sheet shown in (a) is replaced with a transfer sheet structure, and (c) A schematic cross-sectional view showing a method for producing a transfer sheet in which the laminate shown in (b) is patterned with an infrared laser. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0018] (First embodiment) Referring to FIG. 1(a), the laminate 3 includes a base sheet 31, a release layer 32 laminated on the base sheet 31, an anchor layer 33 laminated on the release layer 32, a block layer 34 containing a transparent resin that does not easily absorb UV wavelengths laminated on the anchor layer 33, and a base color layer 35 laminated on the block layer 34. Referring to Figure 1(b), the manufacturing method of the transfer sheet 1 includes a step of forming the above-mentioned laminate 3, and a step of forming an arbitrary pattern 5 having a hole portion 35a penetrating the base color layer 35 by irradiating a UV laser onto the base color layer 35 from the side of the laminate 3 on which the base color layer 35 is formed.
[0019] After the transfer sheet 1 is transferred to the object, the base sheet 31 is peeled off from the object. What is transferred from the laminate 3 to the object is a transfer layer 36 including a release layer 32, an anchor layer 33, a block layer 34, and a base color layer 35. Examples of materials for the base sheet 31 include thermoplastic resins such as polypropylene resins, polyethylene resins, polyamide resins, acrylic resins, olefin resins, polyester resins, vinyl chloride resins, polycarbonate resins, and ABS resins, as well as laminates of these resins.
[0020] The release layer 32 is a layer that becomes the outermost surface of the transfer target decorated by the transfer layer 36 by transferring the transfer sheet 1 to the transfer target and peeling off the base sheet 31. The release layer 32 is transparent. The release layer 32 is formed over the entire surface of the base sheet 31. The material of the release layer 32 can be, for example, a thermoplastic resin such as an acrylic resin, a polystyrene resin, a polyamide resin, a chlorinated polyolefin resin, a chlorinated ethylene-vinyl acetate copolymer resin, a cyclized rubber, or a coumarone-indene resin. When the release layer is formed from such a thermoplastic resin, it can provide the transfer target with chemical resistance or the like. In addition, as other materials, it can be formed by including any of, for example, a photocurable resin such as an ultraviolet curable resin, a radiation curable resin such as an electron beam curable resin, or a thermosetting resin. Examples of such resins include urethane acrylate resins, cyanoacrylate resins, epoxy acrylate resins, polyester acrylate resins, and resins obtained by adding additives such as isocyanate to these resins. When the release layer is formed from the above-mentioned curable resin, it is possible to impart physical properties such as durability and abrasion resistance to the transfer object. The thickness of the release layer 32 can be set to 2 μm or more and 12 μm or less.
[0021] The anchor layer 33 is a layer for improving the adhesion between the release layer 32 and the block layer 34. The anchor layer 33 is transparent. The anchor layer 33 is formed over the entire surface of the release layer 32. The material of the anchor layer 33 may be, for example, a urethane resin, an acrylic resin, or an epoxy resin. The thickness of the anchor layer 33 may be 1 μm or more and 3 μm or less.
[0022] The block layer 34 is a layer that prevents the anchor layer 33 and the release layer 32 from being patterned by a UV laser when the base color layer 35 is patterned by a UV laser. In the first embodiment, one block layer 34 is formed. The block layer 34 is formed over the entire surface of the anchor layer 33. The action and function of the block layer 34 will be described in detail later. The block layer 34 is a transparent layer formed containing a transparent resin that does not easily absorb UV wavelengths. In other words, the block layer 34 is formed containing a transparent resin that easily transmits UV wavelengths. In further other words, the block layer 34 is formed containing a transparent resin whose molecular bonds are not easily broken by UV wavelengths. As such a transparent resin, any one of vinyl chloride-vinyl acetate copolymer resin, polyacetal resin, polycarbonate resin, and acrylic resin may be used. The block layer 34 may be formed by adding an additive that improves hardness to these resins. The thickness of the blocking layer 34 may be set to be not less than 2 μm and not more than 30 μm. Note that the blocking layer 34 does not contain particles that diffuse the UV laser.
[0023] The base color layer 35 is a colored layer. The base color layer 35 is formed over the entire surface on the block layer 34. In the first embodiment, the color of the base color layer 35 is blackish. Here, blackish is preferably black, but includes a relatively dark color close to black. For example, it includes a color in a range in which the values indicating the lightness and chroma in the Munsell color system are both below the median value. An arbitrary pattern 5 is formed by irradiating the base color layer 35 with a UV laser. The pattern 5 has a hole 35a penetrating the base color layer 35. The arbitrary pattern 5 is, for example, a character, a symbol, a figure, or a combination of these. After the transfer layer 36 is transferred to the transfer target and the base sheet 31 is peeled off, the color of the base color layer 35 and the arbitrary pattern 5 are visible through transparent layers such as the block layer 34, the anchor layer 33, and the peeling layer 32. As the material of the base color layer 35, an ink in which a black pigment or dye is dispersed in a binder resin can be used. The thickness of the base color layer 35 may be set to be not less than 2 μm and not more than 20 μm. The base color layer 35 may be formed on only a part of the surface of the block layer 34, rather than on the entire surface.
[0024] The above layers can be formed by a known layer forming method. For example, a coating method or a printing method can be used. Coating methods include, for example, a gravure coating method, a roll coating method, and a comma coating method. Printing methods include, for example, a gravure printing method, an offset printing method, a screen printing method, and a lamination method.
[0025] The UV laser is a laser having an ultraviolet wavelength. In the first embodiment, the wavelength of the UV laser is 355 nm. When a UV laser with a wavelength of 355 nm is used, the focused diameter can be approximately 25 μm. In this way, the UV laser can have a smaller focused diameter compared to an infrared laser with a longer wavelength, and therefore it is possible to precisely focus and perform very fine processing while maintaining excellent positional accuracy. UV lasers have a large photon energy, so when they are irradiated onto a material with weak bonds, they can perform photodecomposition processing, which directly dissociates the molecular bonds. Photodecomposition processing uses light (UV laser) to break molecular bonds, so it generates less heat in the workpiece compared to thermal processing using lasers with long wavelengths such as infrared lasers. In addition, because the UV energy that hits the workpiece is mainly used for decomposition rather than heating, it has the advantage of producing an extremely sharp processed surface and leaving little processing residue.
[0026] With reference to FIG. 2, the details of the UV laser processing in the first embodiment and the action and function of the blocking layer 34 will be described. As shown in FIG. 1(a), the laminate 3, which is the object to be processed, has one block layer 34 and the base color layer 35 is blackish. Referring to the left side of FIG. 2, the UV laser light L is irradiated from the side where the base color layer 35 is formed. The UV laser light L is focused at a focal point f by a lens (not shown) in the UV laser machine (not shown). Also, as shown on the right side of FIG. 2, the value of the UV laser energy at the focal point f is E1, which is the highest. The reason for this is as follows. That is, the focused diameter, i.e., the focused area, is the smallest at the focal point f, so that the laser energy (energy density) per unit area is the largest at the focal point f. Here, since the base color layer 35 is blackish, it is easy to absorb the wavelength of the UV laser light L. Therefore, when the position of the focal point f is adjusted to the vicinity of the surface of the base color layer 35, the base color layer 35 absorbs the UV laser light L well, and the molecular bonds are cut by the energy, and the base color layer 35 is removed. Then, as shown by the two-dot chain line on the left side of Fig. 2, a hole 35a is formed in the base color layer 35. In this way, when the base color layer 35 is blackish, the base color layer 35 absorbs the wavelength of the UV laser light L well and can be processed with the maximum UV laser energy value E1, so that the processing efficiency of the base color layer 35 is good.
[0027] The UV laser energy is absorbed by the black base color layer 35 and is consumed to remove the base color layer 35. Therefore, as shown on the right side of FIG. 2, the UV laser energy value is greatly attenuated to E2. The UV laser light L reaches the block layer 34 after forming the hole 35a in the base color layer 35. The block layer 34 is a transparent layer that does not easily absorb UV wavelengths, so it is not easily photodecomposed by the UV laser light L and transmits the UV laser light L. The UV laser light L that has passed through the block layer 34 reaches the anchor layer 33. Here, since the UV laser light L is absorbed to some extent when passing through the block layer 34, the UV laser energy value E2 is further attenuated to E3. As described above, the anchor layer 33 is formed of a transparent resin that is weak against UV wavelengths, such as a urethane resin, an acrylic resin, and an epoxy resin. In other words, a resin that is weak against UV wavelengths is a resin that is easily absorbed by UV wavelengths and whose molecular bonds are easily broken by UV wavelengths. Since the anchor layer 33 has such properties, it is easily processed by absorbing the UV laser light L, but the anchor layer 33 is not photodecomposed at the UV laser energy value E3 that reaches the anchor layer 33. In other words, the anchor layer 33 is not removed by the UV laser energy value E3.
[0028] The UV laser light L passes through the transparent anchor layer 33 and reaches the peeling layer 32. Here, some of the UV laser light L is absorbed when passing through the anchor layer 33, so the UV laser energy value E3 is further attenuated to E4. Since the UV laser energy value E4 is smaller than E3, the peeling layer 32, like the anchor layer 33, is not removed by the UV laser energy value E4.
[0029] In the laminate 3 of the first embodiment, most of the UV laser light L is absorbed by the black base color layer 35, so that most of the UV laser energy (E1-E2) is consumed in removing the black base color layer 35. The block layer 34 located directly below the base color layer 35 does not easily absorb UV wavelengths, in other words, absorbs a small amount of UV laser light L, so it is difficult to be photodecomposed at the UV laser energy value E2. Due to the action and function of the base color layer 35 and the block layer 34, the anchor layer 33 and the release layer 32 located below the block layer 34 are not photodecomposed by the UV laser and remain as they are. Therefore, peeling is unlikely to occur between the base sheet 31 and the release layer 32.
[0030] Second embodiment With reference to FIG. 3(a), the laminate 4 in the second embodiment differs from the first embodiment in that the base color layer 45 is white-based and two block layers 44-1 and 44-2 are provided. The white-based base color layer 45 is preferably white, but also includes a relatively light color close to white. For example, it includes a color in a range in which the value indicating the brightness in the Munsell color system is 8 or more and the value indicating the saturation is 2 or less. An arbitrary pattern 6 is formed by irradiating the base color layer 45 with a UV laser. As a material for the white-based base color layer 45, an ink in which a white-based pigment or dye is dispersed in a binder resin can be used. The thickness of the white-based base color layer 45 can be 2 μm or more and 20 μm or less.
[0031] With reference to FIG. 4, details of the UV laser processing in the second embodiment and the action and function of the blocking layers 44-1 and 44-2 will be described. The laminate 4, which is the object to be processed, has two block layers 44-1 and 44-2, and the base color layer 45 is white. Referring to the left side of FIG. 4, the UV laser light L is irradiated from the side where the base color layer 45 is formed. The UV laser light L is focused at a focal point f by a lens (not shown) in a UV laser machine (not shown). Also, as shown on the right side of FIG. 4, the value of the UV laser energy at the focal point f is E1, which is the highest. Here, since the base color layer 45 is white, it is difficult to absorb the wavelength of the UV laser light L. In other words, the white base color layer 45 is more difficult to process with a UV laser than when it is black. Therefore, it is necessary to adjust the position of the focal point f to a lower position (closer to the base color layer 45) than the position in the first embodiment. By doing so, the highest UV laser energy value E1 hits the white base color layer 45, so that even if the base color layer 45 is white, it is easy to break the molecular bond. Then, as indicated by the two-dot chain line on the left side of FIG. 4, a hole 45a is formed in the base color layer 45.
[0032] Some of the UV laser energy is absorbed by the whitish base color layer 45 and is consumed to remove the base color layer 45. Therefore, as shown on the right side of FIG. 4, the UV laser energy value attenuates to E5. Here, compared to the case where the base color layer is blackish (FIG. 2), E5 is a value larger than E2. This is because the amount of UV laser light L absorbed by the whitish base color layer 45 is less than that of the blackish base color layer 25. In other words, the UV laser energy consumed to remove the whitish base color layer 45 is less than that consumed to remove the blackish base color layer 25.
[0033] After forming holes 45a in the base color layer 45, the UV laser light L reaches the first block layer 44-1 to which the base color layer 45 is in contact. Here, in the first embodiment, the block layer 34 in contact with the base color layer 35 was not photodecomposed by the UV laser energy value E2. However, in the second embodiment, since the UV laser energy value E5 is greater than E2, the first block layer 44-1 absorbs some UV wavelengths, even though it is a layer that does not easily absorb UV wavelengths, and is photodecomposed by the UV laser energy value E5. Then, holes are formed in the first block layer 44-1 as well, as shown by the two-dot chain line on the left side of FIG. 4.
[0034] The UV laser light L that has passed through the first block layer 44-1 reaches the second block layer 44-2. The UV laser energy of the UV laser light L is attenuated by removing the first block layer 44-1. That is, when the UV laser light L reaches the block layer 44-2, the UV laser energy value E5 has attenuated to E6. This UV laser energy value E6 is a value equivalent to E2 in the first embodiment, and the second block layer 44-2 is not photodecomposed with this energy. Thus, in the second embodiment, the UV laser energy E1 is attenuated to E5 by processing the white-based base color layer 45, and the first block layer 44-1 is processed with the energy value E5, thereby attenuating to a value E6 at which the second block layer 44-2 is not processed.
[0035] The UV laser light L that has passed through the second block layer 44-2 reaches the anchor layer 43. Here, the UV laser light L is absorbed to some extent when passing through the second block layer 44-2, so the UV laser energy value E6 is further attenuated to E7. However, the anchor layer 43 is not removed at the UV laser energy value E7. The UV laser light L passes through the transparent anchor layer 43 and reaches the peeling layer 42. Here, the UV laser light L is absorbed to some extent when passing through the anchor layer 43, so the UV laser energy value E7 is further attenuated to E8. Since the UV laser energy value E8 is smaller than E7, the peeling layer 42, like the anchor layer 43, is not removed at the UV laser energy value E8.
[0036] In the laminate 4 of the second embodiment, the UV laser light L is not easily absorbed by the white-based base color layer 45, so the amount of UV laser energy (E1-E5) consumed to remove the base color layer 45 is smaller than that of the first embodiment. The UV laser energy value E5 is greater than the value E2 at which the block layer is not processed in the first embodiment, so the first block layer 44-1 is processed with the UV laser energy value E5. The second block layer 44-2 located directly below the first block layer 44-1 is not easily absorbed by the UV laser light L, so it is not easily photolytically processed with the UV laser energy value E6. Due to the action and function of the base color layer 45 and the two block layers 44-1 and 44-2, the anchor layer 43 and the peeling layer 42 located below the second block layer 44-2 are not photolytically processed by the UV laser and remain as they are. Therefore, peeling is not easily caused between the base sheet 41 and the peeling layer 42.
[0037] With reference to Figs. 5 and 6, the method of using the transfer sheets 1, 2 of the first and second embodiments will be described. The transfer sheets 1, 2 can be used, for example, in a simultaneous molding and decoration method. The simultaneous molding and decoration method is a method in which the transfer sheets 1, 2 are sandwiched between a pair of dies, the dies are closed, and injection molding is performed in the cavity. When the dies are opened, a molded product is produced in which the transfer sheets 1, 2 and the molded body 7 are integrated. Then, the base sheets 31, 41 are peeled off to obtain the decorated products 8, 9. When the decorated products 8, 9 are viewed from the side where the peeling layers 32, 42 are formed, the arbitrary patterns 5, 6 formed on the base color layers 35, 45 can be visually recognized. The resin used for the material of the molded body 7 may be a transparent resin or a colored transparent resin, and a light source such as an LED may be disposed under the decorative items 8, 9 or inside the molded body 7. In this way, when the light source is turned on, any of the patterns 5, 6 can be lit up, improving the visibility of the patterns 5, 6 and the decorativeness of the decorative items 8, 9.
[0038] Modifications common to all the embodiments will be described with reference to Figures 7 to 10. Although the following description will be given taking the laminate 3 of the first embodiment as an example, these modifications can also be applied to the laminate 4 of the second embodiment. The manufacturing method of the transfer sheet 1 may include a step of forming a pattern color layer 37 of a color different from the base color layer on the base color layer 35 of the laminate 3 on which the arbitrary pattern 5 is formed, so as to fill the holes 35a. Since the base color layer 35 is black-based, any color different from the base color layer can be used as the pattern color layer 37. With reference to FIG. 7, the pattern color layer 37 of one color may be formed so as to cover the entire base color layer 35. Also, with reference to FIG. 8, the pattern color layers 37, 38 of two or more colors may be formed so as to cover the entire base color layer 35. Also, with reference to FIG. 9, the pattern color layer 37 of one color may be formed so as to cover a part of the base color layer 35. That is, as shown in FIG. 7 to FIG. 9, all the holes 35a formed in the base color layer 35 are filled with the pattern color layer of one color or two or more colors. As the material of the pattern color layers 37, 38, an ink in which a pigment or dye of a color different from the base color layer 35 is dispersed in a binder resin can be used. The pattern color layers 37, 38 may have a thickness of 2 μm or more and 20 μm or less. The pattern color layers 37, 38 may be formed by, for example, a coating method or a printing method. According to this method of manufacturing a transfer sheet, the holes 35a are formed with a UV laser, giving them distinct edges, and the holes 35a are filled with pattern color layers 37, 38 of a different color from the base color layer 35, making any desired pattern 5 easier to see. 10, the method for producing the transfer sheet 1 may include a step of forming an adhesive layer 39 so as to cover the pattern color layer 37. The adhesive layer 39 improves the adhesion of the transfer layer 36 to the transfer target object.
[0039] In the second embodiment, the block layer is two layers, but three or more layers may be formed. Also, in the second embodiment, the block layer may be formed as a single layer with a thickness equivalent to two or more block layers. [Explanation of symbols]
[0040] 1,2: Transfer sheet 3,4: Laminate 31, 41: Base sheet 32, 42: peeling layer 33,43: Anchor layer 34,44: Block layer 44-1: 1st block layer 44-2: Second block layer 35,45: Base color layer 35a, 45a: Hole 36, 46: Transfer layer 37,38: Pattern color layer 39: Adhesive layer 5,6: Pattern 7: Molded body 8,9: Decorations L: UV laser light f :focal point 100:Decorative sheet 200: Transfer sheet 210: Base sheet 220: Colored layer 230: Light shielding layer 240: Peeling layer 250: Anchor layer 300: Laminate
Claims
1. A laminate forming process including at least the steps of: laminating a release layer on a base sheet; laminating an anchor layer on the release layer; laminating a block layer containing a transparent resin that does not easily absorb UV wavelengths on the anchor layer; and laminating a base color layer on the block layer; A method for manufacturing a transfer sheet, comprising a step of forming an arbitrary pattern having holes penetrating the base color layer by irradiating the base color layer with a UV laser from the side of the laminate on which the base color layer is formed.
2. A step of preparing a laminate in which at least a release layer, an anchor layer, a block layer containing a transparent resin that does not easily absorb UV wavelengths, and a base color layer are laminated in this order on a base sheet; A method for manufacturing a transfer sheet, comprising a step of forming an arbitrary pattern having holes penetrating the base color layer by irradiating the base color layer with a UV laser from the side of the laminate on which the base color layer is formed.
3. The method for producing a transfer sheet according to claim 1 or 2, wherein the base color layer is black-based, and the block layer is a single layer.
4. The method for producing a transfer sheet according to claim 1 or 2, wherein the base color layer is white, and the block layer is two or more layers.
5. The method for producing a transfer sheet according to any one of claims 1 to 4, wherein the transparent resin contained in the block layer is one selected from the group consisting of vinyl chloride-vinyl acetate copolymer resin, polyacetal resin, polycarbonate resin, and acrylic resin.
6. A method for manufacturing a transfer sheet according to any one of claims 1 to 5, comprising a step of forming a pattern color layer of a different color from the base color layer on the base color layer of the laminate on which the pattern is formed, so as to fill the holes.
7. A base sheet; a release layer laminated on the base sheet; an anchor layer laminated on the release layer; A blocking layer including a transparent resin that does not easily absorb UV wavelengths, the blocking layer being laminated on the anchor layer; a base color layer laminated on the blocking layer.
Citation Information
Patent Citations
Molding decorated with laser marking and manufacture thereof
JP2001030290A
Transfer material for laser etching, and manufacturing method for multi-color molded article
JP2003175672A
Transfer material for laser etching, and method for manufacturing multicolor molded article
JP2010052277A
Laminate and label
WO2020130130A1