Thermoelectric conversion module

Flexible heat dissipation members like wires or metal foils address installation challenges in thermoelectric conversion modules, enabling efficient heat dissipation and temperature difference in confined spaces.

JP7591510B2Active Publication Date: 2024-11-28LINTEC CORP
View PDF 9 Cites 0 Cited by

Patent Information

Application Number
JP2021551155
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2019-09-30
Filing Date
2020-09-24
Publication Date
2024-11-28
Estimated Expiration
2040-09-24

AI Technical Summary

Technical Problem

Existing thermoelectric conversion modules with rigid, three-dimensionally bulky fins face installation challenges in narrow spaces, limiting effective use of heat sources.

Method used

Employing flexible heat dissipation members such as wires or metal foils thermally connected to thermoelectric conversion elements, allowing for efficient temperature difference provision even in confined areas.

Benefits of technology

Enhances installation flexibility and efficiency of thermoelectric conversion modules in spaces with limited installation space by effectively dissipating heat and providing a significant temperature difference.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007591510000002
    Figure 0007591510000002
  • Figure 0007591510000003
    Figure 0007591510000003
  • Figure 0007591510000001
    Figure 0007591510000001
Patent Text Reader

Abstract

Provided is a thermoelectric conversion module which has a high degree of freedom with regard to the installation of a heat dissipating member and can be efficiently provided with a temperature difference even when a heat source is in a confined space and the installation space is limited, said module comprising a thermoelectric conversion element and a first heat dissipating member which is thermally connected to one surface of the thermoelectric conversion element, wherein the first heat dissipating member is either a wire or a metal foil.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a thermoelectric conversion module. [Background technology]

[0002] 2. Description of the Related Art Conventionally, one of the effective means for recovering unused waste heat energy generated from fossil fuel resources used in buildings, factories, etc. as a heat source is a thermoelectric conversion module that uses a thermoelectric conversion material having a thermoelectric effect such as the Seebeck effect or the Peltier effect to directly convert thermal energy into electrical energy. As the thermoelectric conversion module, the use of so-called π-type thermoelectric conversion elements is known. The π-type is configured by providing a pair of electrodes spaced apart from each other on a substrate, for example, providing a P-type thermoelectric element on one electrode and an N-type thermoelectric element on the other electrode, also spaced apart from each other, and connecting the upper surfaces of both thermoelectric materials to the electrodes of the opposing substrate. Also, the use of so-called in-plane type thermoelectric conversion elements is known. The in-plane type is configured by alternately providing P-type thermoelectric elements and N-type thermoelectric elements in the in-plane direction of the substrate, for example, by connecting the lower parts of the junctions between the two thermoelectric elements in series with an electrode interposed therebetween. Under these circumstances, from the viewpoint of improving thermoelectric performance, a heat dissipation member is usually provided on the low-temperature side of the thermoelectric conversion element in order to efficiently apply a temperature difference to the thermoelectric conversion element. Patent Document 1 discloses that when using a thermoelectric conversion element, a heat sink (hereinafter sometimes referred to as a "heat dissipation member") is provided to the thermoelectric conversion element and part of the heat sink is connected to a heat storage material, etc., so that electricity can be generated efficiently based on the temperature difference generated between the heat storage material and the heat sink. [Prior art documents] [Patent documents]

[0003] [Patent Document 1] International Publication No. 2016 / 132533 Summary of the Invention [Problem to be solved by the invention]

[0004] However, the thermoelectric conversion module of Patent Document 1 uses rigid, three-dimensional bulky fins or the like as heat dissipation members. For example, in a location where the heat source is located in a narrow space and installation space is limited, it may be difficult to install the thermoelectric conversion module and it may be difficult to use the heat source effectively and efficiently.

[0005] In view of the above, an object of the present invention is to provide a thermoelectric conversion module that allows a high degree of freedom in the installation of heat dissipation members and can efficiently create a temperature difference, even in places where a heat source is located in a narrow space and installation space is limited. [Means for solving the problem]

[0006] As a result of extensive research into solving the above-mentioned problems, the inventors discovered that in the configuration of a thermoelectric conversion module, by using a flexible wire or metal foil as the first heat dissipation member thermally connected to one side of the thermoelectric conversion element, it is possible to provide a high degree of freedom in the installation of the first heat dissipation member even in places where the heat source is located in a narrow space and installation space is limited, and it is possible to efficiently create a temperature difference, thereby completing the present invention. That is, the present invention provides the following (1) to (13). (1) A thermoelectric conversion module comprising a thermoelectric conversion element and a first heat dissipation member thermally connected to one surface of the thermoelectric conversion element, the first heat dissipation member being a wire or a metal foil. (2) The thermoelectric conversion module according to (1) above, further comprising a connection member thermally connected to an end of the first heat dissipation member opposite to an end connected to one surface of the thermoelectric conversion element. (3) The thermoelectric conversion module according to (1) above, further comprising a housing thermally connected to an end of the first heat dissipation member opposite to an end connected to one surface of the thermoelectric conversion element. (4) The thermoelectric conversion module according to (3) above, wherein the temperature difference between one surface of the thermoelectric conversion element and the temperature of the casing is 10° C. or more. (5) The thermoelectric conversion module according to any one of (1) to (4) above, wherein the first heat dissipation member is made of a highly thermally conductive material. (6) The thermoelectric conversion module according to (5) above, wherein the highly thermally conductive material is selected from the group consisting of gold, copper, silver, iron, nickel, aluminum and brass. (7) The thermoelectric conversion module according to (3) or (4) above, wherein the material of the housing is selected from rubber, resin, and metal. (8) The thermoelectric conversion module according to any one of (1) to (7) above, wherein a heat capacity Mh of the casing is larger than a heat capacity Mw of the first heat dissipation member. (9) The thermoelectric conversion module according to any one of the above (1) to (8), wherein a ratio (Mh / Mw) of a heat capacity Mh of the casing to a heat capacity Mw of the first heat dissipation member is 2 to 5,000. (10) The thermoelectric conversion module according to any one of (1) to (9) above, further comprising a second heat dissipation member thermally connected between one surface of the thermoelectric conversion element and the first heat dissipation member. (11) The thermoelectric conversion module according to any one of (1) to (10) above, further comprising a heat transfer member thermally connected to the other surface of the thermoelectric conversion element. (12) The thermoelectric conversion module according to any one of (1) to (11) above, wherein the thermoelectric conversion elements are π-type thermoelectric conversion elements or in-plane type thermoelectric conversion elements. (13) The thermoelectric conversion module according to (12) above, wherein the configuration of the π-type thermoelectric conversion element or the in-plane type thermoelectric conversion element is used for power generation. Effect of the Invention

[0007] According to the present invention, a thermoelectric conversion module can be provided that allows high freedom in the installation of heat dissipation members and can efficiently create a temperature difference, even in places where the heat source is located in a narrow space and the installation space is limited. [Brief description of the drawings]

[0008] [Figure 1]FIG. 2 is a cross-sectional view illustrating an example of the configuration of a thermoelectric conversion module of the present invention. [Diagram 2] FIG. 4 is a cross-sectional view illustrating another example of the configuration of a thermoelectric conversion module of the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0009] [Thermoelectric conversion module] The thermoelectric conversion module of the present invention comprises a thermoelectric conversion element and a first heat dissipation member thermally connected to one surface of the thermoelectric conversion element, the first heat dissipation member being a wire or a metal foil. In the thermoelectric conversion module of the present invention, by making the first heat dissipation member that constitutes the thermoelectric conversion module a flexible wire or metal foil, heat dissipation from one side of the thermoelectric conversion element originating from the heat source can be efficiently conducted, and not only can an efficient temperature difference be applied to the thermoelectric conversion element, as in the case of a configuration using rigid, three-dimensional, bulky heat dissipation fins, etc., but also the degree of freedom in maneuvering for installing heat dissipation members, etc. can be increased even in places where the heat source is located in a narrow space and the installation space for the thermoelectric conversion module is limited.

[0010] 1 is a cross-sectional view for explaining an example of the configuration of the thermoelectric conversion module of the present invention. The thermoelectric conversion module 1A is configured as a so-called π-type thermoelectric conversion element, and includes a first substrate 2a and an opposing second substrate 2b, a P-type thermoelectric element layer 4 and an N-type thermoelectric element layer 5 formed between the first substrate 2a and the opposing second substrate 2b, a first electrode 3a formed on the first substrate 2a, and a second electrode 3b formed on the opposing second substrate 2b. A wire 7 is thermally connected to the surface of the second substrate 2b opposite to the second electrode 3b side via a bonding material portion 6a as a first heat dissipation member, and the wire 7 extends to an end 8.

[0011] The first heat dissipation member used in the present invention is a wire or a metal foil. The wire is not particularly limited as long as it has flexibility, and the cross-sectional shape may be circular, elliptical, rectangular, etc. The wire may be a single wire or a twisted wire, or a combination of these may be used, or a plurality of each may be used independently. The metal foil is not particularly limited as long as it has flexibility. In addition, the metal foil may be used alone or in combination of multiple sheets.

[0012] The wire used in the present invention is preferably made of a highly thermally conductive material. As the highly thermally conductive material, from the viewpoint of having flexibility and efficiently conducting heat dissipated from one side of the thermoelectric conversion element originating from the heat source, preferred are single metals such as gold, copper, silver, iron, nickel, and aluminum, and alloys such as brass, and more preferred are copper (including oxygen-free copper) and aluminum.

[0013] The cross-sectional area of ​​each wire used in the present invention is appropriately selected depending on the material used, but is not particularly limited as long as it has flexibility and can maintain mechanical strength. 2 and preferably 0.5 to 20.0 mm 2 , more preferably 1.0 to 10.0 mm 2 , and more preferably 2.0 to 5.0 mm 2 If the cross-sectional area of ​​the wire is within the above range, the degree of freedom in handling as a heat dissipation member can be increased even in a place where the heat source is in a narrow space and the installation space for the thermoelectric conversion module is limited. The length of each wire used in the present invention is not particularly limited, but is appropriately selected according to the housing to be connected, as described below, and is usually about 1 cm to 100 cm.

[0014] The metal foil used in the present invention is not particularly limited as long as it is a metal, and from the viewpoint of having flexibility and efficiently conducting heat dissipated from one side of the thermoelectric conversion element originating from the heat source, preferred are single metals such as gold, copper, silver, iron, nickel, and aluminum, and alloys such as brass, and more preferred are copper (including oxygen-free copper) and aluminum.

[0015] The thickness of the metal foil used in the present invention is usually 0.1 μm to 500 μm, preferably 1 μm to 300 μm, more preferably 2 μm to 200 μm, and further preferably 3 μm to 100 μm. If the thickness of the metal foil is within the above range, the flexibility is further improved, and the degree of freedom in handling as a heat dissipation member can be increased even in a place where the heat source is in a narrow place and the installation space for the thermoelectric conversion module is limited. The length of each metal foil used in the present invention is not particularly limited, but is appropriately selected according to the housing to be connected, as described below, and is usually about 1 cm to 100 cm.

[0016] As another example of the thermoelectric conversion module of the present invention, it is preferable to provide a housing thermally connected to the end of the first heat dissipation member opposite the end connected to one surface of the thermoelectric conversion element. The housing is used to efficiently receive the heat conducted from the first heat dissipation member, thereby lowering the temperature of one side of the thermoelectric conversion element and increasing the temperature difference with the other side of the thermoelectric conversion element on the heat source side.

[0017] 2 is a cross-sectional view illustrating another example of the configuration of the thermoelectric conversion module of the present invention. The thermoelectric conversion module 1B has the same configuration as the thermoelectric conversion module 1A, except that the end 8 of the wire 7 is thermally connected to the housing 9 via the bonding material part 6b in the thermoelectric conversion module 1A.

[0018] From the viewpoint of efficient heat dissipation, the housing used in the present invention preferably has a heat capacity Mh (J / K) larger than the heat capacity Mw (J / K) of the first heat dissipation member. The material of the housing may be the same as or different from the highly thermally conductive material used as the first heat dissipation member. From the viewpoint of installation in a narrow space (reducing the size of the housing), it is more preferable to use a material having a higher specific heat than the highly thermally conductive material used. Examples of such housing materials include rubber, resin, metal, etc., and can be appropriately selected depending on the highly thermally conductive material used.

[0019] The ratio (Mh / Mw) of the heat capacity Mh of the casing to the heat capacity Mw of the first heat dissipation member depends on the heat capacity of the first heat dissipation member used, but is preferably greater than 1, more preferably 2 to 5000, even more preferably 4 to 5000, and particularly preferably 8 to 5000. When the ratio is set to this value, heat dissipated from one surface of the thermoelectric conversion element is conducted through the first heat dissipation member and efficiently stored in the casing, thereby lowering the temperature of one surface of the thermoelectric conversion element and increasing the temperature difference with the other surface of the thermoelectric conversion element on the heat source side.

[0020] From the viewpoint of efficiently dissipating heat from one side of the thermoelectric conversion element originating from a heat source, it is preferable to provide a second heat dissipation member (not shown) between one side of the thermoelectric conversion element (for example, the side of the second substrate 2b opposite to the electrode side in FIG. 1) and the end of the wire (for example, the end opposite to the end 8 of the wire in FIG. 1), which is thermally connected to both. The second heat dissipation member is not particularly limited, but it is preferable to use a highly thermally conductive material. From the viewpoint of efficiently conducting heat dissipation from one side of the thermoelectric conversion element, examples of the highly thermally conductive material include single metals such as copper, silver, iron, nickel, chromium, and aluminum, and alloys such as stainless steel and brass (brass). Among these, copper (including oxygen-free copper), aluminum, and stainless steel are preferable, and copper is more preferable because of its high thermal conductivity and easy processability. In addition, a plurality of the single metals or alloys may be combined and stacked for use. When the second heat dissipation member is in the form of a sheet, the thickness is preferably 3 to 200 μm, more preferably 5 to 100 μm, and further preferably 10 to 50 μm. As a method for forming the second heat dissipation member, from the viewpoint of process simplicity, electrolytic plating, electroless plating, or a combination of these, or a method of providing a metal foil on a substrate by a deposition method are preferable. It is also preferable to form a predetermined pattern on the highly thermally conductive material by subjecting it to a known chemical treatment mainly based on photolithography, for example by subjecting a patterned portion of a photoresist to a wet etching treatment and then removing the photoresist.

[0021] In addition, in order to efficiently connect to the heat source, it is preferable to provide a heat transfer member (not shown) on the other surface of the thermoelectric conversion element (for example, in FIG. 1, the surface of the second substrate 2a opposite to the electrode side). The heat transfer member is not particularly limited, but is preferably a highly heat conductive material. From the viewpoint of efficiently conducting heat radiation from a heat source to the other surface of a thermoelectric conversion element, the highly heat conductive material is preferably a single metal such as gold, copper, silver, iron, nickel, or aluminum, or an alloy such as stainless steel or brass, and more preferably copper (including oxygen-free copper) or aluminum. A combination of a plurality of the above single metals may also be used. The thickness of the heat transfer member is preferably 3 to 200 μm, more preferably 5 to 100 μm, and further preferably 10 to 50 μm. The heat transfer member can be formed in the same manner as the above-mentioned method for forming the second heat dissipation member.

[0022] As yet another example of the thermoelectric conversion module of the present invention, it is preferable that the first heat dissipation member is provided with a connecting member thermally connected to an end opposite to the end connected to one surface of the thermoelectric conversion element. 1, for example, a connection member (not shown) is provided at an end 8 of a wire 7 serving as a first heat dissipation member. By connecting the connection member to a metal body or the like with a large heat capacity that is present around a heat source, heat can be efficiently dissipated from the end 8 of the wire 7, and the same effect as the example in which a housing is provided as described above can be obtained. There are no particular limitations on the connecting member as long as it is capable of thermal connection, and general-purpose members such as clips, solder, conductive paste, conductive adhesive, bonding agent, etc. can be used, and they can be selected appropriately depending on the nature of the objects to be connected.

[0023] The temperature difference between the temperature of one surface of the thermoelectric conversion element and the temperature of the housing is preferably 10° C. or more, more preferably 20° C. or more, even more preferably 30° C. or more, and particularly preferably 40° C. or more. The upper limit of the temperature difference is usually 100° C. or less. By installing the thermoelectric conversion module in such an environment, a higher output can be obtained.

[0024] <Substrate> The thermoelectric conversion module of the present invention preferably includes a first substrate having a first electrode. As described above, when configured as a π-type thermoelectric conversion element, it preferably includes a second substrate having a second electrode facing the first substrate having the first electrode. When configured as an in-plane type thermoelectric conversion element, it preferably includes a second substrate facing the first substrate having the first electrode. The first substrate and the second substrate facing the first substrate may be the same or different. The first and second substrates are not particularly limited, and can be made of glass, ceramics, plastic film, etc., independently. Among these, plastic film is preferred from the viewpoint of flexibility and freedom of installation on the surface of the heat source. Furthermore, polyimide film, polyamide film, polyetherimide film, polyaramid film, polyamideimide film, polysulfone film are preferred from the viewpoint of high heat resistance and low outgas generation, and polyimide film is particularly preferred from the viewpoint of high versatility.

[0025] The thickness of the first and second substrates is preferably from 1 to 1000 μm, more preferably from 10 to 500 μm, and further preferably from 20 to 100 μm, from the viewpoints of heat resistance and flexibility. The first and second substrates preferably have a 5% weight loss temperature measured by thermogravimetric analysis of 300°C or higher, more preferably 400°C or higher. The thermal dimensional change rate measured at 200°C in accordance with JIS K7133 (1999) is preferably 0.5% or less, more preferably 0.3% or less. The linear expansion coefficient in the planar direction measured in accordance with JIS K7197 (2012) is 0.1 ppm·°C or less. -1 ~50ppm·℃ -1 and 0.1 ppm·℃ -1 ~30ppm·℃ -1 It is more preferable that:

[0026] <Electrode> The thermoelectric conversion module of the present invention preferably includes a first electrode. When configured as a π-type thermoelectric conversion element, it is preferable that a second electrode is further included on a second substrate facing the first substrate having the first electrode. The first electrode and the second electrode of the second substrate facing the first substrate may be the same or different. Furthermore, when configured as an in-plane type thermoelectric conversion element, the second electrode may or may not be present as long as there is a first electrode. The metal materials used for the first electrode and the second electrode are not particularly limited, but are preferably copper, gold, nickel, aluminum, rhodium, platinum, chromium, palladium, stainless steel, molybdenum, or an alloy containing any of these metals, and may be formed as a single layer or a multilayer structure by combining a plurality of layers. The thickness of the first electrode layer and the second electrode layer is preferably 10 nm to 200 μm, more preferably 30 nm to 150 μm, and further preferably 50 nm to 120 μm. If the thickness of the first electrode layer and the second electrode layer is within the above range, the electrical conductivity is high and the resistance is low, and sufficient strength as an electrode is obtained.

[0027] The first electrode and the second electrode are formed using the above-mentioned metal material. The method of forming the first electrode and the second electrode includes a method of forming an electrode without a pattern on a substrate, and then processing the electrode into a predetermined pattern shape by a known physical or chemical treatment mainly based on a photolithography method, or a combination of these, or a method of directly forming an electrode pattern by a screen printing method, an inkjet method, or the like. Methods for forming an electrode without a pattern include dry processes such as PVD (physical vapor deposition) methods such as vacuum deposition, sputtering, and ion plating, or CVD (chemical vapor deposition) methods such as thermal CVD and atomic layer deposition (ALD), or wet processes such as various coating methods and electrodeposition methods such as dip coating, spin coating, spray coating, gravure coating, die coating, and doctor blade methods, silver halide plating, electrolytic plating, electroless plating, and lamination of metal foils, and are appropriately selected depending on the material of the electrode. From the viewpoint of thermoelectric performance, high electrical conductivity and high thermal conductivity are required, so it is preferable to use electrodes formed by plating or vacuum film formation. Vacuum film formation methods such as vacuum deposition and sputtering, as well as electrolytic plating and electroless plating are preferable because they can easily achieve high electrical conductivity and high thermal conductivity. Depending on the size and dimensional accuracy of the formed pattern, a hard mask such as a metal mask can be used to easily form a pattern.

[0028] <Thermoelectric element layer> The thermoelectric element layer used in the present invention preferably comprises a thermoelectric semiconductor composition containing thermoelectric semiconductor particles, a heat-resistant resin, and one or both of an ionic liquid and an inorganic ionic compound, on a substrate.

[0029] (Thermoelectric semiconductor particles) The thermoelectric semiconductor particles used in the thermoelectric element layer are preferably prepared by pulverizing a thermoelectric semiconductor material to a predetermined size using a fine pulverizer or the like.

[0030] As the materials constituting the P-type thermoelectric element layer and the N-type thermoelectric element layer used in the present invention, there is no particular limitation as long as they are materials capable of generating a thermoelectromotive force by applying a temperature difference. For example, bismuth-tellurium-based thermoelectric semiconductor materials such as P-type bismuth telluride and N-type bismuth telluride; telluride-based thermoelectric semiconductor materials such as GeTe and PbTe; antimony-tellurium-based thermoelectric semiconductor materials; zinc-antimony-based thermoelectric semiconductor materials such as ZnSb, Zn 3 Sb 2、 Zn 4 Sb 3 ; silicon-germanium-based thermoelectric semiconductor materials such as SiGe; bismuth selenide-based thermoelectric semiconductor materials such as Bi 2 Se 3 ; silicide-based thermoelectric semiconductor materials such as β-FeSi 2 、CrSi 2 、MnSi 1.73 、Mg 2 Si; oxide-based thermoelectric semiconductor materials; Heusler materials such as FeVAl, FeVAlSi, FeVTiAl, and sulfide-based thermoelectric semiconductor materials such as TiS 2 are used.

[0031] Among these, the thermoelectric semiconductor materials used in the present invention are preferably bismuth-tellurium-based thermoelectric semiconductor materials such as P-type bismuth telluride or N-type bismuth telluride. The P-type bismuth telluride has holes as carriers and a positive Seebeck coefficient. For example, those represented by Bi X Te 3 Sb 2-X are preferably used. In this case, X is preferably 0 < X ≤ 0.8, more preferably 0.4 ≤ X ≤ 0.6. When X is greater than 0 and less than or equal to 0.8, the Seebeck coefficient and electrical conductivity increase, and the characteristics as a P-type thermoelectric conversion material are maintained, which is preferable. Also, the N-type bismuth telluride has electrons as carriers and a negative Seebeck coefficient. For example, those represented by Bi 2 Te 3-Y Se Y are preferably used. In this case, Y is preferably 0 ≤ Y ≤ 3 (when Y = 0: Bi2 Te 3 ) and more preferably 0.1 < Y ≤ 2.7. When Y is 0 or more and 3 or less, the Seebeck coefficient and the electrical conductivity increase, and the characteristics as an N-type thermoelectric conversion material are maintained, which is preferable.

[0032] The blending amount of the thermoelectric semiconductor particles in the thermoelectric semiconductor composition is preferably 30 to 99% by mass. More preferably, it is 50 to 96% by mass, and still more preferably, it is 70 to 95% by mass. If the blending amount of the thermoelectric semiconductor particles is within the above range, the Seebeck coefficient (the absolute value of the Peltier coefficient) is large, the decrease in electrical conductivity is suppressed, and only the thermal conductivity decreases, so that high thermoelectric performance is exhibited, and a film having sufficient film strength and flexibility is obtained, which is preferable.

[0033] The average particle size of the thermoelectric semiconductor particles is preferably 10 nm to 200 μm, more preferably 10 nm to 30 μm, still more preferably 50 nm to 10 μm, and particularly preferably 1 to 6 μm. If it is within the above range, uniform dispersion becomes easy and the electrical conductivity can be increased. The method for obtaining thermoelectric semiconductor particles by pulverizing the thermoelectric semiconductor material is not particularly limited, and it may be pulverized to a predetermined size by a known fine pulverization device such as a jet mill, a ball mill, a bead mill, a colloid mill, a conical mill, a disk mill, an edge mill, a powder mill, a hammer mill, a pellet mill, a Wiley mill, a roller mill, etc. The average particle size of the thermoelectric semiconductor particles was obtained by measuring with a laser diffraction particle size analyzer (Master Sizer 3000, manufactured by Malvern) and used as the median of the particle size distribution.

[0034] In addition, the thermoelectric semiconductor particles are preferably annealed (hereinafter, sometimes referred to as "annealing treatment A"). By carrying out the annealing treatment A, the crystallinity of the thermoelectric semiconductor particles is improved, and further, the surface oxide film of the thermoelectric semiconductor particles is removed, so that the Seebeck coefficient (absolute value of the Peltier coefficient) of the thermoelectric conversion material increases, and the thermoelectric figure of merit can be further improved. The annealing treatment A is not particularly limited, but is preferably carried out under an inert gas atmosphere such as nitrogen or argon, a reducing gas atmosphere such as hydrogen, or under vacuum conditions with a controlled gas flow rate, before preparing the thermoelectric semiconductor composition, so as not to adversely affect the thermoelectric semiconductor particles, and more preferably under a mixed gas atmosphere of an inert gas and a reducing gas. The specific temperature conditions depend on the thermoelectric semiconductor particles used, but it is usually preferable to carry out the annealing treatment at a temperature below the melting point of the particles and at 100 to 1500°C for several minutes to several tens of hours.

[0035] (Heat-resistant resin) The heat-resistant resin used in the present invention acts as a binder between thermoelectric semiconductor particles to enhance the flexibility of the thermoelectric element layer. There are no particular limitations on the heat-resistant resin, but a heat-resistant resin is used that maintains various physical properties such as mechanical strength and thermal conductivity as a resin without being impaired when the thermoelectric semiconductor particles are crystal-grown by annealing a thin film made of a thermoelectric semiconductor composition. Examples of the heat-resistant resin include polyamide resin, polyamideimide resin, polyimide resin, polyetherimide resin, polybenzoxazole resin, polybenzimidazole resin, epoxy resin, and copolymers having the chemical structure of these resins. The heat-resistant resin may be used alone or in combination of two or more. Among these, polyamide resin, polyamideimide resin, polyimide resin, and epoxy resin are preferred because they have higher heat resistance and do not adversely affect the crystal growth of thermoelectric semiconductor particles in the thin film, and polyamide resin, polyamideimide resin, and polyimide resin are more preferred because they have excellent flexibility. When a polyimide film is used as the support, polyimide resin is more preferred as the heat-resistant resin because of adhesion to the polyimide film. In the present invention, polyimide resin is a general term for polyimide and its precursor.

[0036] The heat-resistant resin preferably has a decomposition temperature of 300° C. or higher. If the decomposition temperature is within the above range, the thermoelectric semiconductor composition does not lose its function as a binder and can maintain the flexibility of the thermoelectric element layer, even when the thin film made of the thermoelectric semiconductor composition is annealed, as described below.

[0037] The heat-resistant resin preferably has a mass loss rate of 10% or less, more preferably 5% or less, and even more preferably 1% or less at 300° C. as measured by thermogravimetry (TG). If the mass loss rate is within the above range, the thermoelectric element layer can maintain its flexibility without losing its function as a binder, even when a thin film made of the thermoelectric semiconductor composition is annealed, as described below.

[0038] The amount of the heat-resistant resin in the thermoelectric semiconductor composition is preferably 0.1 to 40 mass%, more preferably 0.5 to 20 mass%, and further preferably 1 to 20 mass%. When the amount of the heat-resistant resin is within the above range, a film having both high thermoelectric performance and high film strength can be obtained.

[0039] (Ionic Liquid) The ionic liquid used in the present invention is a molten salt formed by combining a cation and an anion, and refers to a salt that can exist in a liquid state in any temperature range of -50 to 400°C. In other words, the ionic liquid is an ionic compound having a melting point in the range of -50°C to less than 400°C. The melting point of the ionic liquid is preferably -25°C to 200°C, more preferably 0°C to 150°C. The ionic liquid has characteristics such as extremely low vapor pressure and non-volatility, excellent thermal stability and electrochemical stability, low viscosity, and high ionic conductivity, and therefore can effectively suppress the reduction in electrical conductivity between thermoelectric semiconductor particles as a conductive auxiliary. In addition, the ionic liquid exhibits high polarity based on an aprotic ionic structure and has excellent compatibility with heat-resistant resins, so that the electrical conductivity of the thermoelectric element layer can be made uniform.

[0040] The ionic liquid may be a known or commercially available one. For example, a mixture of a cationic component such as a pyridinium, pyrimidinium, pyrazolium, pyrrolidinium, piperidinium, imidazolium, etc., and a derivative thereof; a tetraalkylammonium-based amine-based cation and a derivative thereof; a phosphine-based cation such as a phosphonium, trialkylsulfonium, tetraalkylphosphonium, etc., and a derivative thereof; a lithium cation and a derivative thereof; and a mixture of a Cl cation and ... - , Br - , I - , AlCl 4 - , Al 2 Cl 7 - , B.F. 4 - , PF6 - , ClO4 - , NO 3 - , C.H. 3 COO - , C.F. 3 COO - , C.H. 3 SO 3 - , C.F. 3 SO 3 - , (FSO2 ) 2 N - , (CF 3 SO 2 ) 2 N - , (CF 3 SO 2 ) 3 C - , AsF 6 - , SbF 6 - , NbF 6 - , TaF 6 - , F(HF)n - , (CN) 2 N - , C 4 F 9 SO 3 - , (C 2 F 5 SO 2 ) 2 N - , C 3 F 7 COO - , (CF 3 SO 2 )(CF 3 CO)N - and an anion component such as the above.

[0041] Of the above ionic liquids, from the viewpoints of high-temperature stability, compatibility with thermoelectric semiconductor particles and resins, suppression of a decrease in the electrical conductivity in the gaps between thermoelectric semiconductor particles, and the like, it is preferred that the cationic component of the ionic liquid contains at least one selected from pyridinium cations and derivatives thereof, and imidazolium cations and derivatives thereof.

[0042] Specific examples of ionic liquids in which the cationic component contains a pyridinium cation and a derivative thereof include 4-methyl-butylpyridinium chloride, 3-methyl-butylpyridinium chloride, 4-methyl-hexylpyridinium chloride, 3-methyl-hexylpyridinium chloride, 4-methyl-octylpyridinium chloride, 3-methyl-octylpyridinium chloride, 3,4-dimethyl-butylpyridinium chloride, 3,5-dimethyl-butylpyridinium chloride, 4-methyl-butylpyridinium tetrafluoroborate, 4-methyl-butylpyridinium hexafluorophosphate, 1(or N)-butylpyridinium bromide, 1-butyl-4-methylpyridinium bromide, and 1-butyl-4-methylpyridinium hexafluorophosphate. Of these, 1(or N)-butylpyridinium bromide, 1-butyl-4-methylpyridinium bromide, and 1-butyl-4-methylpyridinium hexafluorophosphate are preferred.

[0043] Specific examples of ionic liquids in which the cationic component contains an imidazolium cation and a derivative thereof include [1-butyl-3-(2-hydroxyethyl)imidazolium bromide], [1-butyl-3-(2-hydroxyethyl)imidazolium tetrafluoroborate], 1-ethyl-3-methylimidazolium chloride, 1-ethyl-3-methylimidazolium bromide, 1-butyl-3-methylimidazolium chloride, 1-hexyl-3-methylimidazolium chloride, 1-octyl-3-methylimidazolium chloride, 1-decyl-3-methylimidazolium chloride, and 1-decyl-3-methylimidazolium chloride. Examples of the imidazolium bromide include 1-dodecyl-3-methylimidazolium chloride, 1-tetradecyl-3-methylimidazolium chloride, 1-ethyl-3-methylimidazolium tetrafluoroborate, 1-butyl-3-methylimidazolium tetrafluoroborate, 1-hexyl-3-methylimidazolium tetrafluoroborate, 1-ethyl-3-methylimidazolium hexafluorophosphate, 1-butyl-3-methylimidazolium hexafluorophosphate, 1-methyl-3-butylimidazolium methyl sulfate, and 1,3-dibutylimidazolium methyl sulfate. Among these, [1-butyl-3-(2-hydroxyethyl)imidazolium bromide] and [1-butyl-3-(2-hydroxyethyl)imidazolium tetrafluoroborate] are preferred.

[0044] The above ionic liquid has an electrical conductivity of 10 -7 If the electrical conductivity is in the above range, the conductive additive can effectively suppress the decrease in electrical conductivity between thermoelectric semiconductor particles.

[0045] The ionic liquid preferably has a decomposition temperature of 300° C. or higher. If the decomposition temperature is within the above range, the effect as a conductive auxiliary agent can be maintained even when a thin film made of the thermoelectric semiconductor composition is annealed, as described below.

[0046] The ionic liquid preferably has a mass loss rate of 10% or less, more preferably 5% or less, and even more preferably 1% or less at 300° C. as measured by thermogravimetry (TG). If the mass loss rate is within the above range, the ionic liquid can maintain its effect as a conductive auxiliary even when a thin film made of the thermoelectric semiconductor composition is annealed, as described below.

[0047] The amount of the ionic liquid in the thermoelectric semiconductor composition is preferably 0.01 to 50% by mass, more preferably 0.5 to 30% by mass, and further preferably 1.0 to 20% by mass. When the amount of the ionic liquid is within the above range, a decrease in electrical conductivity is effectively suppressed, and a film having high thermoelectric performance is obtained.

[0048] (Inorganic ionic compounds) The inorganic ionic compound used in the present invention is a compound composed of at least a cation and an anion. The inorganic ionic compound is a solid at room temperature, has a melting point at any temperature in the temperature range of 400 to 900°C, and has characteristics such as high ionic conductivity, so that it can suppress the decrease in electrical conductivity between thermoelectric semiconductor particles as a conductive auxiliary.

[0049] As the cation, a metal cation is used. Examples of the metal cation include alkali metal cations, alkaline earth metal cations, typical metal cations and transition metal cations, with alkali metal cations and alkaline earth metal cations being more preferred. Examples of alkali metal cations include Li + , Na + , K + , Rb + , Cs + and Fr + etc. Examples of alkaline earth metal cations include Mg 2+ , Ca 2+ , Sr 2+ and Ba 2+ etc.

[0050] The anion may be, for example, F - , Cl - , Br - , I - , O.H. - , C.N. - , NO 3 - , NO 2 - , ClO - , ClO 2 - , ClO 3 - , ClO 4 - , CrO 4 2- , HSO 4 - , SCN - , B.F. 4 - , P.F. 6 - etc.

[0051] The inorganic ionic compound may be any known or commercially available inorganic ionic compound. For example, a cationic component such as potassium cation, sodium cation, or lithium cation and a Cl - , AlCl 4 - , Al 2 Cl 7 - , ClO 4 - Chloride ions such as Br - bromide ions, such as I - Iodide ions such as BF 4 - , P.F. 6 - Fluoride ions such as F(HF) n - Halide anions such as NO 3 - , O.H. - , C.N. - and an anion component such as the above.

[0052] Among the above inorganic ionic compounds, from the viewpoints of high temperature stability, compatibility with thermoelectric semiconductor particles and resin, and suppression of a decrease in the electrical conductivity of the gaps between thermoelectric semiconductor particles, it is preferable that the cationic component of the inorganic ionic compound contains at least one selected from potassium, sodium, and lithium. In addition, it is preferable that the anionic component of the inorganic ionic compound contains a halide anion, and Cl is preferably 0.01 to 0.01. - , Br - , and I - It is more preferable that the composition contains at least one selected from the following:

[0053] Specific examples of inorganic ionic compounds whose cationic component contains potassium cations include KBr, KI, KCl, KF, KOH, and K 2 CO 3 Among these, KBr and KI are preferred. Specific examples of inorganic ionic compounds in which the cationic component contains a sodium cation include NaBr, NaI, NaOH, NaF, and Na 2 CO 3 Among these, NaBr and NaI are preferred. Specific examples of inorganic ionic compounds in which the cationic component contains a lithium cation include LiF, LiOH, and LiNO 3 Among these, LiF and LiOH are preferred.

[0054] The above inorganic ionic compounds have an electrical conductivity of 10 -7 S / cm or more is preferable, and 10 -6 If the electrical conductivity is in the above range, the conductive additive can effectively suppress the decrease in electrical conductivity between thermoelectric semiconductor particles.

[0055] The inorganic ionic compound preferably has a decomposition temperature of 400° C. or higher. If the decomposition temperature is within the above range, the effect as a conductive auxiliary agent can be maintained even when a thin film made of the thermoelectric semiconductor composition is annealed, as described later.

[0056] The inorganic ionic compound preferably has a mass loss rate of 10% or less, more preferably 5% or less, and even more preferably 1% or less at 400° C. as measured by thermogravimetry (TG). If the mass loss rate is within the above range, the compound can maintain its effect as a conductive auxiliary even when a thin film made of the thermoelectric semiconductor composition is annealed, as described below.

[0057] The amount of the inorganic ionic compound in the thermoelectric semiconductor composition is preferably 0.01 to 50 mass%, more preferably 0.5 to 30 mass%, and further preferably 1.0 to 10 mass%. When the amount of the inorganic ionic compound is within the above range, the decrease in electrical conductivity can be effectively suppressed, and as a result, a film with improved thermoelectric performance can be obtained. In addition, when an inorganic ionic compound and an ionic liquid are used in combination, the total content of the inorganic ionic compound and the ionic liquid in the thermoelectric semiconductor composition is preferably 0.01 to 50 mass%, more preferably 0.5 to 30 mass%, and even more preferably 1.0 to 10 mass%.

[0058] The thickness of the thermoelectric element layer is not particularly limited, but from the standpoint of thermoelectric performance and film strength, it is preferably 100 nm to 1000 μm, more preferably 300 nm to 600 μm, and even more preferably 5 to 400 μm.

[0059] The P-type thermoelectric element layer and the N-type thermoelectric element layer as thin films made of the thermoelectric semiconductor composition are preferably further annealed (hereinafter, sometimes referred to as "annealing treatment B"). By carrying out the annealing treatment B, the thermoelectric performance can be stabilized and the thermoelectric semiconductor particles in the thin film can be crystallized, thereby further improving the thermoelectric performance. The annealing treatment B is not particularly limited, but is usually carried out under an inert gas atmosphere such as nitrogen or argon, under a reducing gas atmosphere, or under vacuum conditions with a controlled gas flow rate, and is carried out at 100 to 500°C for several minutes to several tens of hours, depending on the heat resistance temperature of the resin and ionic compound used.

[0060] The thermoelectric conversion module of the present invention is not particularly limited, but is preferably composed of a π-type thermoelectric conversion element or an in-plane type thermoelectric conversion element. It is also preferable to use the π-type thermoelectric conversion element or the in-plane type thermoelectric conversion element for power generation.

[0061] (Method of manufacturing thermoelectric conversion module) The thermoelectric conversion module of the present invention can be manufactured by a method including a step of forming electrodes on a substrate (hereinafter sometimes referred to as an "electrode formation step"), a step of applying and drying the thermoelectric semiconductor composition to form a thermoelectric element layer (hereinafter sometimes referred to as a "thermoelectric element layer formation step"), a step of annealing the thermoelectric element layer (hereinafter sometimes referred to as an "annealing step"), a step of bonding the annealed substrate to another substrate (hereinafter sometimes referred to as a "bonding step"), and a step of connecting a heat dissipation member to the substrate (hereinafter sometimes referred to as a "heat dissipation member connection step"). Hereinafter, the steps included in the method for producing a thermoelectric conversion module of the present invention will be described in order.

[0062] (Electrode formation process) The electrode formation step is, for example, a step of forming a pattern made of the above-mentioned metal material on a first substrate, and the method of forming the pattern on the substrate and the method of forming the pattern are as described above. In particular, when manufacturing the above-mentioned π-type thermoelectric conversion module, the electrode formation step includes a step of forming a pattern made of the above-mentioned metal material on a second substrate facing the first substrate.

[0063] (Thermoelectric element layer formation process) The thermoelectric element layer forming step is, for example, a step of applying the thermoelectric semiconductor composition onto an electrode. Methods for applying the thermoelectric semiconductor composition onto an electrode on a first substrate include known methods such as screen printing, flexographic printing, gravure printing, spin coating, dip coating, die coating, spray coating, bar coating, doctor blade, etc., and are not particularly limited. When forming a coating film in a pattern, a screen printing method, a slot die coating method, etc., which can easily form a pattern using a screen plate having a desired pattern, are preferably used. The coating film thus obtained is then dried to form a thermoelectric element layer, and the drying method may be a conventionally known drying method such as hot air drying, hot roll drying, infrared irradiation, etc. The heating temperature is usually 80 to 150° C., and the heating time varies depending on the heating method, but is usually several seconds to several tens of minutes. When a solvent is used in the preparation of the thermoelectric semiconductor composition, the heating temperature is not particularly limited as long as it is within a temperature range in which the solvent used can be dried. The same applies when the thermoelectric semiconductor composition is applied onto an electrode on a second substrate.

[0064] Another example of the thermoelectric element layer forming step is a method in which the thermoelectric element layer is previously produced as chips of a thermoelectric conversion material, and a plurality of the obtained chips are placed and bonded on predetermined electrodes on a substrate. As a method for producing a chip of a thermoelectric conversion material, for example, a chip of a thermoelectric conversion material made of a thermoelectric semiconductor composition can be produced by the following method. First, a sacrificial layer is formed on a substrate such as glass, and a thermoelectric element layer (hereinafter, sometimes referred to as a "chip of thermoelectric conversion material") is formed on the obtained sacrificial layer by the method described above. Next, the obtained chip of thermoelectric conversion material is annealed, and the chip of thermoelectric conversion material is peeled off from the sacrificial layer on the substrate, thereby manufacturing the chip of thermoelectric conversion material as an individual piece. The sacrificial layer may be made of a resin such as polymethylmethacrylate or polystyrene, or a release agent such as a fluorine-based release agent or a silicone-based release agent.

[0065] (Annealing process) The annealing step is, for example, a step of annealing the thermoelectric element layer in a configuration having the first substrate, the electrode, and the thermoelectric element layer obtained above in this order. The annealing step is performed in the annealing step B described above.

[0066] (Laminating process) The bonding process is, for example, a process of bonding a first substrate having an electrode and a thermoelectric element layer obtained in the annealing process to an opposing second substrate or a second substrate having a second electrode, to produce a thermoelectric conversion module. In the case of a second substrate having a second electrode, the laminating agent used for the lamination may be a conductive paste, etc. Examples of the conductive paste include copper paste, silver paste, nickel paste, etc., and in the case of using a binder, examples of the conductive paste include epoxy resin, acrylic resin, urethane resin, etc. In addition, in the case of the second substrate not having a second electrode, a resin material can be used. The resin material preferably contains a polyolefin resin, an epoxy resin, or an acrylic resin. Furthermore, the resin material preferably has adhesive properties, low water vapor permeability, and insulating properties. In this specification, having adhesive properties means that the resin material has adhesive properties, adhesion properties, and pressure-sensitive adhesive properties that can be bonded by pressure at the initial stage of attachment. Methods for applying the laminating agent onto the substrate include known methods such as screen printing and dispensing.

[0067] When a solder material layer is used for bonding to the electrodes in the bonding step, a solder-receiving layer can be used to improve the bonding strength. For example, a method for forming a solder-receiving layer on a chip of a thermoelectric conversion material obtained by the above-mentioned manufacturing method is as follows. After forming a solder-receiving layer on all surfaces of the thermoelectric conversion material chip, which has an upper surface, a lower surface, and a side surface, the solder-receiving layer formed on the side surface of the thermoelectric conversion material chip is entirely removed or part of the resulting solder-receiving layer is removed to form the solder-receiving layer. The solder-receiving layer preferably contains a metal material. The metal material is preferably at least one selected from gold, silver, rhodium, platinum, chromium, palladium, tin, nickel, and an alloy containing any of these metal materials. Among these, a two-layer structure of gold, silver, nickel, tin and gold, or nickel and gold is more preferable, and silver is even more preferable from the viewpoints of material cost, high thermal conductivity, and bonding stability. The solder-receiving layer is required to have high electrical conductivity and high thermal conductivity in order to maintain thermoelectric performance, and from the viewpoint of reducing the contact resistance at the interface with the thermoelectric conversion material chip, it is preferable to use a solder-receiving layer formed by a plating method or a vacuum film formation method. The solder material constituting the solder material layer may be appropriately selected taking into consideration the heat resistance temperature of the heat-resistant resin contained in the resin film and the chip of the thermoelectric conversion material, as well as electrical conductivity and thermal conductivity, and examples of such known materials include Sn, Sn / Pb alloy, Sn / Ag alloy, Sn / Cu alloy, Sn / Sb alloy, Sn / In alloy, Sn / Zn alloy, Sn / In / Bi alloy, Sn / In / Bi / Zn alloy, Sn / Bi / Pb / Cd alloy, Sn / Bi / Pb alloy, Sn / Bi / Cd alloy, Bi / Pb alloy, Sn / Bi / Zn alloy, Sn / Bi alloy, Sn / Bi / Pb alloy, Sn / Pb / Cd alloy, and Sn / Cd alloy. From the viewpoints of lead-free and / or cadmium-free, melting point, electrical conductivity, and thermal conductivity, alloys such as 43Sn / 57Bi alloy, 42Sn / 58Bi alloy, 40Sn / 56Bi / 4Zn alloy, 48Sn / 52In alloy, and 39.8Sn / 52In / 7Bi / 1.2Zn alloy are preferred. Methods for applying the solder material onto the electrodes of the substrate include known methods such as screen printing and dispensing.

[0068] <Heat dissipation component connection process> The heat dissipation member connecting process is a process in which one end of the first heat dissipation member is fixed to the second substrate (however, if the second substrate has a second heat dissipation member described below, the second heat dissipation member) using a solder material layer or the like so that the first heat dissipation member is thermally connected to the second substrate obtained in the bonding process, and the other end of the first heat dissipation member is extended. It is preferable that the method further includes a step of fixing the other end of the first heat dissipation member to the housing by a solder material layer, etc. Fixing by the solder material layer can be performed by a known method.

[0069] (Second heat dissipation member forming process) The method for manufacturing a thermoelectric conversion module preferably includes a step of forming a second heat dissipation member, which is a step of forming the second heat dissipation member, for example, on the second substrate (on the surface opposite to the electrode side, in the case where an electrode is present), using the above-mentioned highly thermally conductive material. The method for forming the second heat dissipation member is as described above.

[0070] (Conductive member forming process) The method for manufacturing a thermoelectric conversion module preferably includes a step of forming a conductive member. The heat transfer member forming step is a step of forming a conductive member on, for example, the first substrate (in the case where an electrode is present, the surface opposite to the electrode side) using the above-mentioned highly thermally conductive material. The method for forming the heat transfer member is as described above.

[0071] According to the manufacturing method of the thermoelectric conversion module of the present invention, even in places where the heat source is located in a narrow space and the installation space is limited, it is possible to obtain a thermoelectric conversion module that allows a high degree of freedom in the installation of the heat dissipation member and can efficiently create a temperature difference. EXAMPLES

[0072] The present invention will now be described in more detail with reference to examples, but the present invention is not limited to these examples in any way.

[0073] The thermoelectric performance of the thermoelectric conversion modules produced in the examples and comparative examples was evaluated by the following method.

[0074] <Thermoelectric performance evaluation> (a) Electrical resistance evaluation of thermoelectric conversion module The electrical resistance R between the extraction electrodes of the obtained thermoelectric conversion module at a set temperature described below was measured in an environment of 25° C.×50% RH using a low resistance measuring device (manufactured by HIOKI EE Corporation, model number: RM3545). (b) Output voltage and maximum output evaluation of thermoelectric conversion module The output voltage V (electromotive force) between the output extraction electrodes of the obtained thermoelectric conversion module at a set temperature described below was measured in an environment of 25° C.×50% RH using a Digital HiTester (manufactured by Hioki E.E. Corporation, model number: 3801-50). In addition, from the obtained electrical resistance R and output voltage V, the maximum output (= V 2 / 4R) was calculated. (c) Evaluation of temperature difference For the obtained thermoelectric conversion module, the temperature difference ΔT between the copper foil in contact with the heat dissipation surface side and the copper foil in contact with the heat absorption surface side was measured using a thermocouple (K type). The heat source was a hot plate, and the other side of the thermoelectric conversion module (heated side: the side that does not have the wire as the first heat dissipation member) was heated to temperatures of 40°C, 50°C, 60°C, 70°C, 80°C, and 90°C (excluding 90°C in Comparative Example 1).The electrical resistance between the extraction electrodes of the thermoelectric conversion module, the output voltage, the maximum output, and the temperature difference between the heated side and the cooled side at each temperature were evaluated.

[0075] Example 1 (1) Preparation of thermoelectric semiconductor composition (Preparation of thermoelectric semiconductor particles) P-type bismuth telluride Bi, a bismuth-tellurium based thermoelectric semiconductor material 0.4 Te 3 Sb 1.6(manufactured by Kojundo Chemical Laboratory, particle size: 90 μm) was pulverized in an air atmosphere using a planetary ball mill (manufactured by Fritsch Japan, Premium line P-7) to produce thermoelectric semiconductor particles T1 with an average particle size of 2.0 μm. In addition, N-type bismuth telluride Bi, a bismuth-tellurium based thermoelectric semiconductor material, 2 Te 3 (manufactured by Kojundo Chemical Laboratory, particle size: 90 μm) was pulverized in the same manner as above to produce thermoelectric semiconductor particles T2 with an average particle size of 2.0 μm. The particle size distribution of the thermoelectric semiconductor particles T1 and T2 obtained by pulverization was measured using a laser diffraction particle size analyzer (Malvern, Mastersizer 3000). (Preparation of Coating Solution of Thermoelectric Semiconductor Composition) Coating liquid (P) The p-type bismuth telluride Bi obtained above 0.4 Te 3.0 Sb 1.6 A coating liquid (P) consisting of a thermoelectric semiconductor composition was prepared by mixing and dispersing 83.3 parts by mass of the particles T1, 2.7 parts by mass of polyamideimide (manufactured by Arakawa Chemical Industries, Ltd., product name: Compocelan AI301, solvent: N-methylpyrrolidone, solid content: 18% by mass) as a heat-resistant resin, and 14 parts by mass of N-butylpyridinium bromide as an ionic liquid. Coating fluid (N) The obtained N-type bismuth telluride Bi 2.0 Te 3.0 A coating liquid (N) consisting of a thermoelectric semiconductor composition was prepared by mixing and dispersing 92.1 parts by mass of the particles T2, 3.0 parts by mass of polyamideimide (manufactured by Arakawa Chemical Industries, Ltd., product name: Compocelan AI301, solvent: N-methylpyrrolidone, solid content: 18% by mass) as a heat-resistant resin, and 4.9 parts by mass of N-butylpyridinium bromide as an ionic liquid. (2) Formation of thin films of thermoelectric conversion materials A sacrificial layer was formed on a 0.7 mm thick glass substrate (product name: blue plate glass, manufactured by Kawamura Kuzo Shoten Co., Ltd.) by spin coating a polymethyl methacrylate resin solution having a solid content of 10 mass %, prepared by dissolving polymethyl methacrylate resin (PMMA) (product name: polymethyl methacrylate, manufactured by Sigma-Aldrich Co., Ltd.) in toluene, so that the thickness after drying was 10.0 μm. Next, the coating solution (P) prepared in (1) above was applied onto the sacrificial layer by screen printing using a metal mask, and dried in air at a temperature of 120°C for 7 minutes to form a thin film with a thickness of 200 μm. Next, the obtained thin film was heated at a heating rate of 5 K / min in an atmosphere of a mixed gas of hydrogen and argon (hydrogen:argon = 3 volume %: 97 volume %) and held at 450°C for 1 hour to anneal the thin film, causing crystal growth of the particles of the thermoelectric semiconductor material, resulting in the formation of P-type bismuth telluride Bi 0.4 Te 3 Sb 1.6 A rectangular parallelepiped chip of thermoelectric conversion material having a top and bottom surface each measuring 1.65 mm×1.65 mm and a thickness of 200 μm was obtained. In addition, the coating solution (N) prepared in (1) above was used, and the coating solution was kept at 360°C for 1 hour for annealing. 2 Te 3 A rectangular parallelepiped chip of thermoelectric conversion material having a top and bottom surface each measuring 1.65 mm×1.65 mm and a thickness of 200 μm was obtained.

[0076] (3) Formation of solder-receiving layer After the annealing treatment, the chips of each thermoelectric conversion material were peeled off from the glass substrate, and a solder-receiving layer [Ni (thickness: 3 μm) laminated with Au (thickness: 40 nm)] was provided on all surfaces of each thermoelectric conversion material chip using an electroless plating method. Next, the solder-receiving layers on the side surfaces of the P-type and N-type thermoelectric conversion material chips were removed by mechanical polishing, i.e., using sandpaper (grit 2000), so that the chips had dimensions of 1.5 mm x 1.5 mm, thereby obtaining P-type and N-type thermoelectric conversion material chips having solder-receiving layers only on the top and bottom surfaces. Note that, in order to completely remove the solder-receiving layers, part of the side walls were also polished.

[0077] (Fabrication of thermoelectric conversion module) Using the obtained chips of P-type and N-type thermoelectric conversion materials having solder acceptance layers only on the top and bottom surfaces, a π-type thermoelectric conversion element consisting of 18 pairs each of P-type and N-type thermoelectric conversion material chips was fabricated as follows. First, a substrate with copper foil attached on both sides (manufactured by Ube Exsymo, product name: Upicel N, polyimide substrate, thickness: 12.5 μm, copper foil, thickness: 12 μm) was prepared, and a nickel layer (thickness: 3 μm) and a gold layer (thickness: 40 nm) were laminated in this order on the copper foil of the film substrate by electroless plating, and then an electrode pattern (10 × 10 mm square, 18 pieces, center-to-center distance between adjacent electrodes: 17 mm, 6 columns × 3 rows) was formed only on one side to prepare a substrate with electrodes (lower electrode film). After that, a solder material layer was stencil-printed (thickness: 30 μm) on the electrodes using solder paste 42Sn / 57Bi / Ag alloy (manufactured by Nippon Handa Co., Ltd., product name: PF141-LT7H0) as the solder material. Next, one side of the solder-receiving layer of each of the P-type and N-type thermoelectric conversion material chips obtained above was placed on the solder material layer, and the chips were heated at 180°C for 1 minute and then cooled, thereby placing the P-type and N-type thermoelectric conversion material chips on the electrodes, respectively. Furthermore, the solder paste was printed as a solder material layer on the other side of the solder acceptance layer of each of the P-type and N-type thermoelectric conversion material chips (thickness before heating: 50 μm), and the electrodes of an upper electrode film (an electrode film with electrodes arranged in a pattern so that a π-type thermoelectric conversion element is obtained when it is bonded to the lower electrode film; the substrate, electrode material, thickness, etc. are the same as the lower electrode) were bonded together, and heated at 180°C for 2 minutes (thickness after heating: 30 μm), thereby obtaining a π-type thermoelectric conversion element consisting of 18 pairs each of the P-type and N-type thermoelectric conversion material chips. A wire [SWITCH SCIENCE Corporation, silicone-coated wire; copper wire, thermal conductivity: 400 W / m K, length: 10 cm, diameter: 1.4 mm (cross-sectional area: 1.54 mm)] was attached to the cooling surface of the obtained thermoelectric conversion element with solder interposed therebetween as a first heat dissipation member. 2), heat capacity Mw: 0.53 J / K] was connected to one end of the wire, and the other end of the wire was connected via solder to a case (material: copper, heat capacity Mh: 685 J / K) placed at room temperature (25°C) to form a thermoelectric conversion module. The obtained thermoelectric conversion module was evaluated for electrical resistance, output voltage, maximum output, and temperature difference between the heating surface and the cooling surface at each of the aforementioned temperatures. The evaluation results are shown in Table 1.

[0078] Example 2 In Example 1, the cross-sectional area of ​​the wire was doubled (3.08 mm 2 A thermoelectric conversion module of Example 2 was produced in the same manner as in Example 1, except that the thermal capacity Mw was 1.06 J / K. The obtained thermoelectric conversion module was evaluated for electrical resistance, output voltage, maximum output, and temperature difference between the heating surface and the cooling surface in the same manner as in Example 1. The results are shown in Table 1.

[0079] Comparative Example 1 A thermoelectric conversion module of Comparative Example 1 (including only thermoelectric conversion elements) was produced in the same manner as in Example 1, except that the wires were not connected to the cooling surface and the housing (natural cooling). The obtained thermoelectric conversion module was heated on a hot plate at temperatures of 40° C., 50° C., 60° C., 70° C., and 80° C. The electrical resistance, output voltage, maximum output, and temperature difference between the heating surface and the cooling surface were evaluated at each temperature. The results are shown in Table 1.

[0080] [Table 1]

[0081] It can be seen that the thermoelectric conversion modules of Examples 1 and 2, in which a wire and a housing are thermally connected to one side of a thermoelectric conversion element, provide a larger temperature difference and obtain a higher output than the thermoelectric conversion module of Comparative Example 1, which is configured with natural cooling and no specific heat dissipation means. It is also clear that a higher output can be obtained from the thermoelectric conversion module of Example 2, which has twice the cross-sectional area of ​​the wire (doubles the heat capacity) of the thermoelectric conversion module of Example 1. Furthermore, it is clear that the output increases more significantly as the set temperature increases. [Industrial Applicability]

[0082] The thermoelectric conversion module of the present invention is considered to be applicable to power generation applications in which exhaust heat from various combustion furnaces such as factories, waste incineration furnaces, and cement combustion furnaces, exhaust heat from automobile combustion gases, and exhaust heat from electronic devices are converted into electricity. In particular, when applied to a place where the heat source is located in a narrow space and the installation space for the thermoelectric conversion module is limited, the heat source can be used effectively and efficiently because there is a high degree of freedom in the installation of the heat dissipation member. [Explanation of symbols]

[0083] 1A.1B: Thermoelectric conversion module 2a: First substrate 2b: Second substrate 3a: first electrode 3b: Second electrode 4: P-type thermoelectric element layer 5: N-type thermoelectric element layer 6a, 6b: Joining material part 7: Wire 8: End (wire) 9: Housing

Claims

1. The present invention comprises a thermoelectric conversion element and a first heat dissipation member thermally connected to one surface of the thermoelectric conversion element, the first heat dissipation member being a flexible wire or metal foil, an end portion of the first heat dissipation member opposite to an end portion connected to one surface of the thermoelectric conversion element is provided so as to be directly thermally connected to a surface of a housing; The material of the housing is selected from rubber, resin, and metal. Thermoelectric conversion module.

2. The thermoelectric conversion module according to claim 1 , wherein a temperature difference between one surface of the thermoelectric conversion element and the casing is 10° C. or more.

3. The thermoelectric conversion module according to claim 1 , wherein the first heat dissipation member is made of a highly thermally conductive material.

4. 4. The thermoelectric conversion module according to claim 3, wherein the highly thermally conductive material is selected from the group consisting of gold, copper, silver, iron, nickel, aluminum and brass.

5. 5. The thermoelectric conversion module according to claim 1, wherein a heat capacity Mh of the housing is larger than a heat capacity Mw of the first heat dissipation member.

6. 6. The thermoelectric conversion module according to claim 1, wherein a ratio (Mh / Mw) of a heat capacity Mh of the housing to a heat capacity Mw of the first heat dissipation member is 2 to 5000.

7. The thermoelectric conversion module according to any one of claims 1 to 6, further comprising a second heat dissipation member thermally connected between one surface of the thermoelectric conversion element and the first heat dissipation member.

8. The thermoelectric conversion module according to any one of claims 1 to 7, further comprising a heat transfer member thermally connected to the other surface of the thermoelectric conversion element.

9. The thermoelectric conversion module according to any one of claims 1 to 8, wherein the thermoelectric conversion element is a π-type thermoelectric conversion element or an in-plane type thermoelectric conversion element.

10. The thermoelectric conversion module according to claim 9 , wherein the configuration of the π-type thermoelectric conversion element or the in-plane type thermoelectric conversion element is used for power generation.

Citation Information

Patent Citations

  • Thermoelectric conversion module, sensor module, and information processing system

    EP3261137A1

  • Body temperature utilization generator, and intracochlea implant system using the same

    JP2006204646A

  • Electronic circuit and electronic apparatus

    JP2006261221A

  • Radiation structure of solid-state imaging device

    JP2008205783A

  • Artificial inner ear and thermoelectric generator therefor

    US20060169314A1