Method for making a homogeneous mixture of polyolefin and liquid organic acid

By using polyolefin granules and controlled mixing in a pressurizable device, the method addresses mixer fouling and loading limits, achieving homogeneous mixtures with higher hydrocarbylsulfonic acid content, thereby improving thermal aging performance of polyethylene formulations.

JP7591524B2Active Publication Date: 2024-11-28DOW GLOBAL TECHNOLOGIES LLC
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
JP2021574920
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2019-06-27
Filing Date
2020-06-22
Publication Date
2024-11-28
Estimated Expiration
2040-06-22

AI Technical Summary

Technical Problem

The challenge of creating homogeneous mixtures of polyolefins and liquid organic acids, particularly hydrocarbylsulfonic acids, is hindered by mixer fouling and limited loading due to immiscibility and shear heating, which restricts the incorporation of these acids beyond 2 weight percent, leading to equipment contamination and reduced thermal aging performance.

Method used

A method involving the use of polyolefin granules and controlled temperature and mixing stages in a pressurizable mixer device to incorporate liquid hydrocarbylsulfonic acid, ensuring it is added below the polyolefin's melting point, followed by targeted temperature increases to achieve a homogeneous mixture with up to 6 weight percent incorporation, minimizing equipment fouling and enhancing thermal stability.

Benefits of technology

The method allows for the creation of homogeneous mixtures with higher acid loading, preventing mixer fouling and improving thermal aging performance, as demonstrated by enhanced retention of tensile strength and elongation in the resulting polyethylene formulations.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007591524000001
    Figure 0007591524000001
  • Figure 0007591524000002
    Figure 0007591524000002
  • Figure 0007591524000003
    Figure 0007591524000003
Patent Text Reader

Abstract

A method for making a homogeneous mixture comprising a liquid hydrocarbyl sulfonic acid and a polyolefin, comprising multiple stages of adding ingredients, mixing, and monitoring temperature. The method allows for the production of embodiments of the homogeneous mixture in which greater than 3 weight percent of the liquid hydrocarbyl sulfonic acid is incorporated into the polyolefin, and prevents fouling of mixer equipment.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] Mixture of polyolefins and additives.

[0002] Introduction Publications of patents and patent applications in or regarding this field include CN206899549U, EP0775719A2, US4,490,323, US5,516,814, US6,172,138B1, US6,448,310B1, US2006 / 0281850A1, WO2002 / 088239A1, and WO2006 / 101754A1.

[0003] The moisture-curable polyethylene formulation includes a (hydrolyzable silyl group) functional polyethylene copolymer (HSG-FP copolymer) and a silanol condensation catalyst, which can be an organic acid effective to catalyze the moisture-based condensation cure of the hydrolyzable silyl groups to form crosslinked polyethylene as a networked polymer. Summary of the Invention

[0004] A loading limit problem was encountered when incorporating liquid silanol condensation catalysts into polyethylene carrier resins to make catalyst masterbatches. The silanol condensation catalyst, also known as moisture cure catalyst, may be provided to moisture curable polyethylene formulations in the form of a catalyst masterbatch that includes a carrier resin and a silanol condensation catalyst. An embodiment of the resulting moisture curable polyethylene formulation includes an HSG-FP copolymer, a carrier resin, and a silanol condensation catalyst. The carrier resin is typically a polyolefin, such as polyethylene or polypropylene. All other things being equal, a higher loading of the silanol condensation catalyst into the catalyst masterbatch increases the final loading of the silanol condensation catalyst that can be reached in the moisture curable polyethylene formulation, allowing greater flexibility in using the catalyst masterbatch to prepare moisture curable polyethylene formulations at a wide range of loading levels of the silanol condensation catalyst. Because they tend to be immiscible with one another - the polyolefin carrier resin is a non-polar hydrocarbon and the silanol condensation catalyst is typically a polar aprotic acid such as a liquid organic acid (e.g., a carboxylic acid or a hydrocarbyl sulfonic acid) - it is difficult to make homogeneous mixtures with loading levels much greater than 2 weight percent of the liquid organic acid in the polyolefin.

[0005] Problems with mixer fouling were also encountered when attempting to use mixer equipment to mix liquid hydrocarbyl sulfonic acid into polyolefin pellets to produce a homogeneous mixture of polyolefin and liquid hydrocarbyl sulfonic acid. The mixer equipment generates shear heating during the mixing operation. The shear heating increases the temperature of the material in the mixer equipment, eventually melting the polyolefin pellets. However, unmixed portions of the liquid hydrocarbyl sulfonic acid remain, fouling the mixer equipment. The fouling was visible to the naked eye as a dark colored residue from the hydrocarbyl sulfonic acid on the surfaces of the mixer equipment. The mixer equipment required periodic cleaning to prevent the residue from building up and shutting down production, and this cleaning would render the mixer equipment temporarily unusable. Additionally, homogeneous mixtures could not be achieved at loading levels above 2 weight percent of liquid hydrocarbyl sulfonic acid in polyolefin.

[0006] Attempts were made to solve both the loading limit and mixer fouling problems by trying one of the following actions: (a) reducing the mixing temperature and / or shortening the mixing period, (b) increasing the mixing temperature and / or lengthening the mixing period, (c) limiting the maximum loading of the liquid hydrocarbyl sulfonic acid, (d) changing the point of addition of one or more stabilizer additives (e.g., antioxidants) to the polyolefin, or (e) replacing the polyolefin pellets with polyolefin granules, which are a more finely divided physical form. However, these actions alone did not solve at least one of the loading limit and mixer fouling problems. For example, attempts to solve the mixer fouling problem by (a) reducing the mixing temperature (cooling the mixer equipment) or shortening the mixing time resulted in less effective mixing and a concomitant higher level of the unmixed portion of the liquid hydrocarbyl sulfonic acid. (b) Attempting to solve the loading limit problem by consuming too much of the stabilizer additives (e.g., antioxidants) in the polyolefin by increasing the mixing temperature (heating the mixing equipment) and / or increasing the mixing period reduced the heat aging performance of the homogeneous mixture in the end-use application. The mixer fouling problem was also exacerbated. Therefore, it was decided not to allow the mixing temperature to exceed 170 degrees Celsius (°C) to minimize the consumption of the stabilizer additives (e.g., antioxidants) in the polyolefin. (c) Attempting to solve the mixer fouling problem by limiting the maximum loading of liquid organic acid per unit weight of polyolefin exacerbated the loading limit problem. (d) Attempting to solve the heat aging problem by changing the time of addition of one or more stabilizer additives to the polyolefin polymer did not prevent the mixer fouling problem, but negated the flexibility and limited the usefulness of the homogeneous mixture as a catalyst masterbatch for various end-use applications with different stabilizer requirements. (e) Attempts to solve the fouling problem by replacing polyolefin pellets with polyolefin granules failed to prevent the accumulation of unmixed liquid hydrocarbyl sulfonic acid and did not solve the mixer fouling problem.

[0007] A method has been discovered for producing a homogenous mixture comprising a liquid hydrocarbyl sulfonic acid and a polyolefin in a mixer apparatus. The method uses granular polyolefin and includes the following steps carried out in the mixer apparatus (within the mixing chamber thereof): mixing the recently added liquid hydrocarbyl sulfonic acid into an initial polyolefin formulation consisting essentially of mostly, but not all, polyolefin to obtain a first mixture, the polyolefin being in the form of granules, and from the time the liquid hydrocarbyl sulfonic acid is added until the start of mixing, the temperature of the initial polyolefin formulation is in a first target temperature range that allows the liquid hydrocarbyl sulfonic acid to be incorporated into the polyolefin, below the melting temperature of the polyolefin, and continuing mixing until the temperature of the first mixture increases (e.g., as a result of heat generated by mixing, i.e., heat of mixing) to a second target temperature range that is higher than the first target temperature range; adding a small portion of the polyolefin in the form of granules to the first mixture; mixing to obtain a second mixture while monitoring the temperature of the second mixture as shear heating increases its temperature until the temperature of the second mixture reaches a final target temperature range of 145°C to 150°C, thereby producing a homogenous mixture, wherein all of the liquid hydrocarbyl sulfonic acid is incorporated into the polyolefin in the mixer apparatus. The method allows for the production of embodiments of a homogeneous mixture in which greater than 3 weight percent of liquid hydrocarbyl sulfonic acid is incorporated into the polyolefin, and prevents fouling of mixer equipment. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0008] 1. A method of making a homogenous mixture comprising a liquid hydrocarbyl sulfonic acid and a polyolefin in a mixer apparatus, comprising steps (1)-(3): (1) mixing a recently added liquid hydrocarbyl sulfonic acid with an initial polyolefin formulation consisting essentially of most, but not all, of a polyolefin to obtain a first mixture, the polyolefin being in the form of granules, and from the time the liquid hydrocarbyl sulfonic acid is added to the initial polyolefin formulation until the start of mixing, the temperature of the initial polyolefin formulation is in a first target temperature range that enables the liquid hydrocarbyl sulfonic acid to be incorporated into the polyolefin, and (2) obtaining a mixture at a temperature below the melting temperature of the olefin and continuing mixing until the temperature of the first mixture increases (e.g., as a result of heat of mixing) to a second target temperature range higher than the first target temperature range; (3) adding a small portion of the polyolefin in granular form to the first mixture to obtain a second mixture; and (4) mixing the second mixture until the temperature of the second mixture increases to a final target temperature range of 145°C to 150°C, thereby producing a homogenous mixture in the mixer apparatus, wherein all of the liquid hydrocarbyl sulfonic acid is incorporated into the polyolefin.

[0009] The method may further include a preliminary step prior to step (1), the preliminary step including adding a liquid hydrocarbyl sulfonic acid to the initial polyolefin formulation in the mixer apparatus immediately prior to the start of mixing in step (1), the initial polyolefin formulation being in a first target temperature range, i.e., the majority of the polyolefin does not contact the liquid hydrocarbyl sulfonic acid unless the temperature of the majority of the polyolefin is already in the first target temperature range.

[0010] The method allows for the creation of embodiments of homogeneous mixtures in which greater than 3 weight percent of liquid hydrocarbyl sulfonic acid is incorporated into the polyolefin, preventing fouling of mixer equipment. Without being bound by theory, if the polyolefin is used in pellet form, and / or if the polyolefin is not divided into its major and minor portions and used separately, a sufficient amount of liquid hydrocarbyl sulfonic acid will not be incorporated into the polyolefin, and the amount of the minor portion of the polyolefin will be insufficient to absorb all of the remaining pooled or unincorporated liquid hydrocarbyl sulfonic acid, and the resulting non-uniform mixed material will have a too low load limit and foul the mixer equipment. Similar problems will occur if the liquid hydrocarbyl sulfonic acid is added to the heated material before the temperature of the heated material reaches the first target temperature range, if the liquid hydrocarbyl sulfonic acid is added to a completely molten material, and / or if the temperature of the mixture does not reach 145°C. If the temperature of the second mixed material exceeds 150°C, the resulting heat aging may impair the performance of the second mixed material in the end-use application.

[0011] The phrase "the initial polyolefin blend consists essentially of a majority of polyolefin in the form of granules" means that the initial polyolefin blend does not contain a minor portion of polyolefin and does not contain liquid hydrocarbyl sulfonic acid.

[0012] The phrase "effective for incorporating the liquid hydrocarbyl sulfonic acid and below the melting temperature of the polyolefin" means a temperature hot enough that at least 90 weight percent of the liquid hydrocarbyl sulfonic acid, in granular form, can be absorbed into the bulk of the polyolefin. This temperature can be between 95 and 105 degrees Celsius (°C).

[0013] The term "granules" means that the average particle size is between 0.2 millimeters (mm) and 1.5 mm, alternatively between 0.20 mm and 0.80 mm.

[0014] The method may further include a preliminary step of heating the initial polyolefin formulation from a temperature lower than the first target temperature range (e.g., from ambient temperature) to the first target temperature range before the step of adding the liquid hydrocarbyl sulfonic acid to the initial polyolefin formulation in the mixer device. The term "heating" means increasing the temperature of the material. Heating may be achieved by exchanging heat from an external heat source to the initial polyolefin formulation through the mixer device, or by mixing the initial polyolefin formulation in the mixer device, thereby generating heat of mixing, or a combination thereof. Typically, heating is achieved by mixing the initial polyolefin formulation (essentially consisting of granules of the main part of polyolefin) in the mixer device, thereby generating heat of mixing.

[0015] The expressions "majority of polyolefins" and "minority of polyolefins" refer to larger and smaller weight fractions, respectively, of the total amount of polyolefins in a homogeneous mixture. For example, if the total amount of polyolefins in a homogeneous mixture is said to be 100 parts by weight (relative amount), the majority of polyolefins may be 90-99 parts by weight and the minority of polyolefins may be 10-1 parts by weight, respectively. The majority of polyolefins may be additive-free and free of any other polymers, or the majority of polyolefins may contain at least one additive and free of any other polymers. The minority of polyolefins may be additive-free and free of any other polymers, or the minority of polyolefins may contain at least one additive and free of any other polymers. The at least one additive of the embodiment of the majority of polyolefins may be the same as or different from the at least one additive of the embodiment of the minority of polyolefins. The polyolefin of the majority may be the same as or different from the polyolefin of the minority. The polyolefin may be a high density polyethylene.

[0016] The expression "a second target temperature range higher than the first target temperature range" means that the lower limit of the second target temperature range is higher than the upper limit of the first target temperature range.

[0017] The term "liquid" means a state of matter characterized at 25°C as an amorphous fluid having a definite volume but no definite shape, somewhere between that of a gas and a solid. The term "solid" means a state of matter characterized at 25°C as having a definite volume and shape.

[0018] Melting refers to changing a substance from a solid state to a liquid state. Typically, melting means that the change is complete such that the liquid state of the substance contains no unmelted material.

[0019] By "recently added" it is meant that the liquid hydrocarbyl sulfonic acid may be in contact with the majority of the polyolefin without mixing for up to 1 hour, alternatively up to 30 minutes, alternatively up to 5 minutes, alternatively up to 30 seconds, alternatively 0 seconds. In the latter embodiment, the liquid hydrocarbyl sulfonic acid is added during the mixing of step (1) or is added at a measured rate (metered) during the mixing of step (1).

[0020] Mixing includes mechanically actuated means that initiate motion by applying a direct contact force, either manually or through a machine, where a physical object (e.g., a stirrer paddle, screw, plunger, or blender) contacts and thereby moves the material. Examples of mechanically actuated forces include stirring, rotor mixing, screw mixing, plunger mixing, blender mixing, and other direct physical contact. Contact forces do not include electromagnetic, gravitational, acoustic, or convective forces.

[0021] The method may further include the feature of substantially or completely not soaking (or absorbing) the liquid hydrocarbyl sulfonic acid into the polyolefin granules. Soaking requires miscibility of the liquid hydrocarbyl sulfonic acid in the polyolefin granules and effective soaking conditions. Such soaking conditions include a period of time (e.g., 8-16 hours) and a sufficiently high temperature (e.g., 60°C-90°C) to transfer the liquid hydrocarbyl sulfonic acid into the polyolefin granules.

[0022] Additional inventive aspects follow, some of which are numbered below for ease of reference. Aspect 1. A method of making a homogenous mixture comprising 1-6 parts by weight of liquid hydrocarbyl sulfonic acid per 100 parts by weight of polyolefin in a mixer apparatus, comprising steps (1)-(3): (1) mixing a recently added liquid hydrocarbyl sulfonic acid in a pressure mixing operation carried out in a pressurizable mixer apparatus with an initial polyolefin blend consisting essentially of 90-98 parts by weight of polyolefin to obtain a first mixture, wherein the polyolefin is in the form of granules, and wherein the temperature of the initial polyolefin blend is in a first target temperature range of 95° C. to 105° C. from the time the liquid hydrocarbyl sulfonic acid is added to the start of mixing. (2) adding 10-2 parts by weight of polyolefin in the form of granules to the first mixture to obtain a second mixture; and (3) mixing the second mixture in a pressure mixing operation carried out in a pressurizable mixer apparatus until the temperature of the second mixture increases to a final target temperature range of 145°C to 150°C, thereby creating a homogenous mixture in the mixer apparatus, wherein all of the liquid hydrocarbyl sulfonic acid is incorporated into the 100 parts by weight of polyolefin. When the temperature of the first mixture reaches the second target temperature range and immediately prior to commencing step (3), it is possible that some fraction of the 1-6 parts by weight of the liquid hydrocarbyl sulfonic acid will not be incorporated into the polyolefin. This may be visually observed as an accumulation or pool of unincorporated fractions underneath or on the surface of the first mixture. The method may further include a preliminary step prior to step (1), which includes adding a liquid hydrocarbyl sulfonic acid to the initial polyolefin formulation in a mixer apparatus, the mixer apparatus being at a first target temperature range during the addition temperature of the initial polyolefin formulation. The mixer apparatus may further be a mixer apparatus described below, such as a twin rotor batch mixer apparatus. Aspect 2. The method of aspect 1, wherein step (3) comprises mixing the first mixture with 10-2 parts by weight of polyolefin in a first direction to obtain a second mixture, continuing mixing until the temperature of the second mixture increases to a third target temperature range of 135°C to 140°C, and subsequently mixing the second mixture in a second direction until the temperature of the second mixture increases to a final target range of 145°C to 150°C, the second mixing direction being orthogonal to the first mixing direction. By orthogonal, for example, when represented by three axes x, y, and z, the first direction of mixing can be along the axis of the mixing element (e.g., rotor or screw) and the second direction of mixing can be perpendicular to the axis of the mixing element. Orthogonal mixing can further include mixing in a third direction that is circular around the axis of the mixing element (e.g., around the circumference of the rotor or screw). Certain mixer equipment is designed to accommodate orthogonal mixing operations. In some embodiments, the mixing in the first direction and the mixing in the second direction comprise pressure mixing operations carried out in a pressurizable mixer apparatus used in step (3) of Embodiment 1. Aspect 3. The method of aspect 2, wherein after mixing in a first direction and prior to mixing in a second direction, step (3) is interrupted by a non-pressurized mixing operation step performed in a non-pressurizable mixer apparatus, comprising relaxing the second mixture for a period of time during which the second mixture is subjected to non-pressurized mixing, and during relaxation, the temperature of the second mixture can remain in a third target temperature range or be reduced to a minimum of 120°C. Aspect 4. The method of any one of aspects 1-3, wherein the initial polyolefin formulation further consists essentially of at least one first solid additive or a melt thereof, the first mixture further consists essentially of at least one first solid additive or a melt thereof, and the homogenous mixture comprises 100 parts by weight of polyolefin, 1-6 parts by weight of a liquid hydrocarbyl sulfonic acid, and the at least one first solid additive. Aspect 5. The method of any one of aspects 1-3, wherein step (2) further comprises adding at least one second solid additive to the first mixture, wherein the second mixture further comprises at least one second solid additive, or a melt thereof, and wherein the homogeneous mixture comprises 100 parts by weight of a polyolefin, 1-6 parts by weight of a liquid hydrocarbyl sulfonic acid, and the at least one second solid additive. Aspect 6. The method of any one of aspects 1-3, wherein the initial polyolefin formulation further consists essentially of at least one first solid additive or a melt thereof, the first mixture further consists essentially of at least one first solid additive or a melt thereof, step (2) further comprises adding at least one second solid additive to the first mixture, the second mixture further comprises at least one second solid additive or a melt thereof, and the homogenous mixture comprises 100 parts by weight of polyolefin, 1-6 parts by weight of liquid hydrocarbyl sulfonic acid, the at least one first solid additive, and the at least one second solid additive. In some embodiments, at least one, or all but one, or each of the at least one first solid additive is compositionally distinct from at least one, or all but one, or each of the at least one second solid additive. Aspect 7. The method of any one of aspects 1-6, wherein the number of parts by weight of the liquid hydrocarbyl sulfonic acid is from 2 to 6, alternatively from 3 to 6, alternatively from 3 to 5, alternatively from 3.5 to 4.1, per every 100 parts by weight of the polyolefin. Aspect 8. The method of any one of aspects 1-7, further comprising, after step (3), mixing at least a portion of the step (4) homogeneous mixture with (A) (hydrolyzable silyl group)-functional polyethylene copolymer (HSG-FP copolymer) to result in a moisture-curable polyethylene formulation comprising at least a portion of the homogeneous mixture and (A) HSG-FP copolymer. In preparing the moisture-curable polyethylene formulation, at least a portion of the homogeneous mixture can function as a catalyst masterbatch comprising a liquid hydrocarbyl sulfonic acid as a silanol condensation catalyst and a polyolefin as a carrier resin. The mixing of step (4) can comprise a pressurized mixing operation carried out in a pressurizable mixer apparatus or a non-pressurized mixing operation carried out in a pressurizable mixer apparatus. Aspect 9. A homogenous mixture made by the method of any one of claims 1-7. Example 10. A moisture curable polyethylene formulation made by the method of example 8.

[0023] The method can be carried out in the mixing chamber of any mixer apparatus that is effective to generate shear heating during a mixing operation carried out therein, to make a polyolefin blend, and to monitor its temperature during at least a portion of the mixing operation in the mixer apparatus. The mixer apparatus can be further configured as a pressurizable mixer apparatus, which is a mixer apparatus that is separately configurable to carry out pressurized and non-pressurized mixing operations. The mixer apparatus can be further configured for orthogonal mixing operations, as described below. The mixer apparatus can be further configured as a batch mixer apparatus for carrying out batch mixing operations. The mixer apparatus can be a pressurizable batch mixer apparatus configured to carry out pressurized and non-pressurized batch mixing operations.

[0024] The process employs a mixer apparatus. The mixer apparatus used in the mixing step (1) of the process can be the same or different as the mixer apparatus used in the mixing step (3) of the process and / or the same or different as the mixer apparatus used in the non-pressurized mixing step (if any). The mixer apparatus used in the mixing step (4) can be the same or different as the mixer apparatus used in steps (1), (3), and any non-pressurized mixing steps. The addition step (2) can be carried out in the mixer apparatus used in steps (1) or (2), or both.

[0025] The mixer apparatus may include a mixing chamber for holding the materials to be mixed, at least one mixing element for mixing the materials in the mixing chamber, a sealing element movable from an open position for performing a non-pressurized mixing operation to a closed position for performing a pressurized mixing operation (and vice versa) for sealing and increasing the pressure in the mixing chamber, a temperature sensor for measuring the temperature of the materials during the pressurized mixing operation, and a discharge door movable from a closed position for performing a mixing operation to an open position (and vice versa) for discharging the mixed materials from the mixer apparatus. The temperature sensor may be disposed within the sealing element such that when the sealing element is in its closed position, the temperature sensor is positioned to sense the temperature of the materials in the mixing chamber. The mixer apparatus may further include an external jacket that substantially surrounds the mixing chamber and defines a channel through which a heat transfer fluid can be circulated to regulate the temperature of the walls of the mixing chamber and, in turn, regulate the temperature of the contents of the mixing chamber. Typically, during the mixing operation, no heat transfer fluid is circulated, an ambient temperature heat transfer fluid is circulated, or a cooled heat transfer fluid is circulated.

[0026] Each of the at least one mixing element may be independently a rotor or a screw element. Each rotor or screw element may be independently rotatable. Each rotor or screw element may independently define an internal heat transfer channel through which a heat transfer fluid may be circulated to regulate the temperature of the rotor or screw element during the mixing operation. The at least one mixing element may consist of up to two mixing elements, for example, up to two rotors or two screw elements.

[0027] The mixing steps (1) and (3) of the method may comprise a pressurized mixing operation performed in a pressurizable mixer apparatus with the sealing element and discharge door of the mixer apparatus in their closed positions, such as the pressurized mixing operations of steps (1) and (3) of embodiment 1. Step (3) of the method may be divided into two separate pressurized mixing operations performed consecutively in a pressurizable mixer apparatus, such as those operations described in embodiment 2. The embodiment of step (3) that is divided into two separate pressurized mixing operations may be interrupted by an intermediate step that comprises a non-pressurized mixing operation performed in a pressurizable mixer apparatus with the sealing element in its open position and the discharge door in its closed position, e.g., the non-pressurized mixing operation described in embodiment 3.

[0028] The pressurizable mixer apparatus of the preceding paragraph may be a twin rotor batch mixer apparatus. In the twin rotor batch mixer apparatus, at least one mixing element may consist of twin rotors arranged parallel to each other and rotatable in opposite directions in the mixing chamber. For example, one of the twin rotors may be a first rotor rotatable in a clockwise direction, and the other of the twin rotors may be a second rotor rotatable in a counterclockwise direction. The mixing chamber may be subdivided into a first and a second half chamber in fluid communication with each other. During a pressurized mixing operation when the mixing chamber of the pressurizable mixer apparatus is sealed by a sealing element (e.g., the ram is in a down position) and the pressure in the mixing chamber is greater than the ambient pressure (at the ram pressure), the material in the first half chamber may be mixed by the first rotor and the material in the second half chamber may be mixed by the second rotor, but with relatively little or no transfer of material between the first and second half chambers. During a non-pressurized or "relaxed" mixing operation when the mixing chamber of the pressurizable mixer apparatus is not sealed by a sealing element (e.g., the ram is in the up position) and the pressure in the mixing chamber is about ambient pressure, the material in the first half-chamber can be mixed by the first rotor, the material in the second half-chamber can be mixed by the second rotor, and further portions of the material can be transferred between the first and second half-chambers. The first rotor of the twin rotor can be located in the first half-chamber and the second rotor of the twin rotor can be located in the second half-chamber. The twin rotor batch mixer apparatus can have orthogonal mixing capabilities. Orthogonal mixing can occur simultaneously in both the x-axis and y-axis directions, meaning that the material being mixed flows in both directions along the y-axis between the first and second half-chambers, as well as along the rotor axis in a particular half-chamber (each rotor axis is along the x-axis).In a pressurized mixing operation, the sealing element is lowered, the mixing chamber is sealed by the sealing element and pressurized (e.g., the ram is in the down position), the material is given less room to rotate or flow between the first and second half-chambers, and therefore the flow rate between the first and second half-chambers is less than in a non-pressurized mixing operation. In a non-pressurized mixing operation, the sealing element is in a raised or relaxed position, the mixing chamber is sealed by the sealing element and pressurized (e.g., the ram is in the up position), the material is given more room to rotate or flow between the first and second half-chambers, and therefore the flow rate between the first and second half-chambers is greater than in a non-pressurized mixing operation.

[0029] The mixing conditions of a pressurizable mixer apparatus, including a twin rotor batch mixer apparatus, can be controlled by setting the pressure in the mixing chamber, the rotational speed of the rotors, and the temperature of the heat transfer fluid (if any) circulating through the rotors. The pressure in the pressurizable mixer apparatus of any given pressurized mixing step (e.g., step (1)) can independently be the same or different than the pressure in the pressurizable mixer apparatus of another pressurized mixing step (e.g., step (3)). The temperature of the materials in the mixing chamber can be monitored by a temperature sensor. The temperature of the materials in any given mixing step (pressurized or non-pressurized) can independently be the same or different than the temperature of the materials in another mixing step (pressurized or non-pressurized).

[0030] When the sealing element is in its open position, solid materials can be added to the mixing chamber of the pressurizable mixer apparatus. The pressurizable mixer apparatus can be configured with a liquid injection system having a metering function for adding liquid to the mixing chamber at a measured rate.

[0031] A mixer apparatus (e.g., a pressurizable mixer apparatus) may be placed in material transfer communication with the extruder / pelletizer apparatus such that a homogenous mixture may be created in the mixing chamber and then transferred to the extruder for pelletization. A mixer apparatus placed in communication with an extruder / pelletizer apparatus may be referred to herein as a mixer / extruder / pelletizer system. The mixer / extruder / pelletizer system may be a Banbury Type 1D mixer / extruder / pelletizer system as described below in the Examples.

[0032] In some embodiments, the ingredients may be added sequentially to the mixing chamber in the following order: the first majority half (e.g., 45-49 parts by weight) of the polyolefin, then any optional metal deactivators, then any optional first antioxidants, then any optional second antioxidants, then the second majority half (e.g., 45-49 parts by weight) of the polyolefin.

[0033] Each heat transfer fluid can independently be a gas, a vapor, or a liquid. The starting temperature of the heat transfer fluid can be ambient (e.g., air or water from a natural source), higher than ambient (heated air or steam), or lower than ambient (e.g., cold air, cold water, cold brine, or cold glycol).

[0034] The temperature of the contents of the mixing chamber (e.g., the initial polyolefin blend, the first mixture, or the second mixture) can be continuously or intermittently monitored by a temperature sensor. The temperature sensor can be a thermometer, a thermocouple probe, or an infrared sensor, or a thermocouple probe.

[0035] Parts by weight are relative amounts. For example, 100 parts by weight of polyolefin may be equal to 1,000 grams (g) of polyolefin, in which case 6 parts by weight of liquid hydrocarbyl sulfonic acid is equal to 60 g of liquid hydrocarbyl sulfonic acid (0.06 x 1,000). Or, 100 parts by weight of polyolefin may be equal to 5,060 kilograms (kg) of polyolefin, in which case 4 parts by weight of liquid hydrocarbyl sulfonic acid is equal to 202 g of liquid hydrocarbyl sulfonic acid (0.04 x 5,060).

[0036] Prior to the process, the target 100 parts by weight of polyolefin in the homogeneous mixture is separated as a major portion, such as 90-98, alternatively 92-95, alternatively 95-98 parts by weight, and a minor portion, such as 10-2 parts by weight, alternatively 8-5 parts by weight, alternatively 5-2 parts by weight.

[0037] The 90-98 parts by weight polyolefin and the 10-2 parts by weight polyolefin may independently be an ethylene-based polymer or a propylene-based polymer. The ethylene-based polymer may be a polyethylene homopolymer ethylene / (C4-C 20 The propylene-based polymer may be a polypropylene homopolymer, a propylene / ethylene copolymer, or a blend of any two or more thereof. The polyolefin may be, independently, an ethylene-based polymer. The ethylene-based polymer may be a polyethylene homopolymer or an ethylene / (C4-C 20 The ethylene-based polymer may be a hydrocarbon such as high density polyethylene (HDPE), which has a relatively high degree of crystallinity and is useful as a carrier resin.

[0038] Ethylene-based polymers contain 51-100 wt% of ethylene units derived from the polymerization of ethylene and 49-0 wt% of comonomer units derived from the polymerization of one or more olefin-functional monomers (comonomers) selected from propylene, 1-butene, 1-hexene, 1-octene, etc. (C4-C6) 20 ) alpha-olefins, or unsaturated carboxylic acid esters. The propylene-based polymers contain 51-100 wt% of propylene units derived from the polymerization of propylene, and 49-0 wt% of comonomer units derived from the polymerization of one or two olefin-functional monomers (comonomers) selected from propylene, (C4-C8) alpha-olefins such as 1-butene, 1-hexene, 1-octene, or unsaturated carboxylic acid esters. (C4-C 20 Examples of alpha-olefins are (C4-C8) alpha-olefins such as 1-butene, 1-hexene, or 1-octene, and (C 10 -C 20 ) alpha-olefins.

[0039] The polyolefin granules can be porous or non-porous.

[0040] Liquid hydrocarbyl sulfonic acid. A compound of formula R-SO3H, where R is (C1-C 40 ) hydrocarbyl group, the compound has a definite volume at 25°C but does not have a definite (fixed) shape. (C1-C 40 ) The hydrocarbyl group is (C1-C 40 ) alkyl group, (C3-C 40 ) cycloalkyl group, (C6-C 40 ) aryl groups, (C1-C 10 )Alkyl-(C6-C 10 ) aryl group or (C6-C 10 )Aryl-(C2-C 20) alkyl groups. The liquid hydrocarbyl sulfonic acids may have temperature characteristics of (i) or (ii): (i) a freezing point below 0° C., alternatively between 0° C. and 20.0° C., or (ii) a melting point between 20.1° C. and 99° C., alternatively between 30.0° C. and 79.9° C., alternatively between 40.0° C. and 69.9° C. The liquid hydrocarbyl sulfonic acids may be provided as anhydrides, hydrates, or organic solvates.

[0041] The present methods and the homogeneous mixtures produced thereby independently may contain only one liquid hydrocarbyl sulfonic acid or a combination of two or more different liquid hydrocarbyl sulfonic acids.

[0042] The present method and the homogeneous mixtures independently produced thereby can contain only one liquid additive that is a liquid hydrocarbyl sulfonic acid, or the present method and the homogeneous mixtures independently produced thereby can contain a liquid hydrocarbyl sulfonic acid and at least one liquid additive that is not a liquid hydrocarbyl sulfonic acid.

[0043] The method and the homogeneous mixture produced thereby may further include at least one solid additive different from the polyolefin. Such additives may be independently inorganic or organic. Examples include carbon black, carbon nanotubes, diamond powder, graphite, graphene, powdered metals, powdered metal oxides, solid flame retardants, silica, alumina, and silicate glass beads.

[0044] The moisture curable polyethylene formulation may include (A) an HSG-FP copolymer, a homogeneous mixture, and optionally any zero, one or more additives (B) through (H): (B) metal deactivators, (C) antioxidants, (D) colorants, (E) anti-scorching agents, (F) stabilizers, (G) processing aids, (H) flame retardants.

[0045] (A) (Hydrolyzable Silyl Group)-Functional Polyethylene (HSG-FP) Copolymers. (A) HSG-FP copolymers are made by copolymerizing monomers including ethylene and, optionally, an olefin-functional comonomer, where at least one olefin-functional comonomer is an olefin-functional hydrolyzable silane. The composition of the (A) HSG-FP copolymers may be characterized by constitutional units selected from ethylene units, alkylene hydrolyzable silyl group units, optionally propylene units, and optionally comonomer units derived from an olefin comonomer. Optionally, the zero, one, or more olefin comonomers are selected from the group consisting of (C4-C 20) alpha-olefins, olefinically unsaturated carboxylic acids, olefinically unsaturated carboxylic esters, olefinically unsaturated carboxylic anhydrides, and combinations thereof. The carboxylic acids can be mono- or dicarboxylic acids. The carboxylic esters can be mono-, di- or di-carboxylic acid monoesters, or di-carboxylic acid diesters. The olefinically unsaturated carboxylic acids can be terminally unsaturated (C2-C8) carboxylic acids, or (meth)acrylic acids, or unsaturated dicarboxylic acids. The olefinically unsaturated carboxylic esters can be vinyl (C2-C8) carboxylate esters, or vinyl (C2-C5) carboxylate esters (e.g., vinyl acetate, vinyl propionate, or vinyl butanoate), or (C1-C8) alkyl (meth)acrylate esters. Alternatively, it may be a (C1-C3) alkyl (meth)acrylate ester, or a di(C1-C8) alkyl diester of an unsaturated dicarboxylic acid, or a mono(C1-C8) alkyl ester of an unsaturated dicarboxylic acid, or a mono(C1-C8) alkyl ester of maleic acid. By meth)acrylate, it is meant H2C=CHCO2- or H2C=C(CH3)CO2-. The CTA may be acetone, methyl ethyl ketone, propionaldehyde, 2-propanol, ethyl acetate, isobutene, butane, 2-methylpropane, ISOPARTM-C, ISOPARTM-E, ISOPARTM-H, or a combination of any two or more thereof. If present, the CTA may be 0.03 to 10% by weight of the polymerization reaction mixture.

[0046] The (A) HSG-FP copolymer may be characterized by a total hydrolyzable silyl group content of 0.43 to 0.99 mole percent. The total mole percent hydrolyzable silyl group content is calculated from the weight percent values ​​of the hydrolyzable silyl group content, the weight percent values ​​being determined according to the X-ray fluorescence (XRF) test method described below. For example, if the at least one alkenyl-functional hydrolyzable silane is vinyltrimethoxysilane (VTMS), its molecular weight is 148.23 g / mole, and the comonomer content is 2.0 weight percent, then the mole percent = 0.38 mole percent. If the VTMS comonomer content is 5.0 weight percent, then the mole percent = 0.99 mole percent. The mole percent hydrolyzable silyl group content at any given weight percent hydrolyzable silyl group content value varies inversely with the molecular weight of the at least one alkenyl-functional hydrolyzable silane from which the hydrolyzable silyl group is derived.

[0047] (A) The HSG-FP copolymer contains hydrolyzable silyl groups. These groups are independently represented by the formula (R 2 ) m (R 3 ) 3-m Si- where subscript m is an integer 1, 2, or 3, and each R 2 are independently H, HO-, (C1-C8)alkoxy, (C2-C6)carboxy, phenoxy, (C1-C6)alkyl-phenoxy, (C1-C6)alkyl(H)N-, ((C1-C6)alkyl)2N-, (C1-C6)alkyl(H)C=NO-, or ((C1-C6)alkyl)2C=NO-, each R 3 is independently (C1-C8) alkyl or phenyl. 2 may be free of H and HO-, or free of phenoxy and (C-C) alkyl-phenoxy. 2 are independently (C1-C6)alkoxy, (C2-C6)carboxy, ((C1-C6)alkyl) 2It can be N-, (C1-C6) alkyl(H)C=NO-, or ((C1-C6) alkyl)2C=NO-, or (C1-C6) alkoxy, or (C2-C6) carboxy, or ((C1-C6) alkyl)2N-, or (C1-C6) alkyl(H)C=NO-, or ((C1-C6) alkyl)2C=NO-. A) All of the hydrolyzable silyl groups of the HSG-FP copolymer can be the same. The hydrolyzable silyl groups are derived from the hydrolyzable silyl groups of at least one alkenyl-functional hydrolyzable silane (comonomer) from which the comonomer units of the HSG-FP copolymer containing such groups are made.

[0048] Optional Additive (B) Metal Deactivator. Examples include hydrazine derivatives such as oxalyl bis(benzylidene hydrazide) (OABH) and 1,2-bis(3,5-di-tert-butyl-4-hydroxyhydrocinnamoyl)hydrazine and 2,2'-oxamido-bis-(ethyl-3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate. The moisture curable polyethylene formulation may be free of (B). (B) Antioxidant, if present, may be 0.01 to 1.5 wt. % of the total weight of the moisture curable polyethylene formulation, alternatively 0.1 to 1.0 wt. %.

[0049] Optional Additive (C) Antioxidant: An organic molecule, or collection of such molecules, that inhibits oxidation. The (C) antioxidant is compositionally distinct from the (F) stabilizer, i.e., when the moisture curable polyethylene formulation contains both (C) and (F), the compound used as (C) will be distinct from the compound used as (F). The (C) antioxidant functions to provide antioxidant properties to the moisture curable polyethylene formulation and / or to the cured polymeric product produced by curing the moisture curable polyethylene formulation.Examples of suitable (C) include bis(4-(1-methyl-1-phenylethyl)phenyl)amine (e.g., NAUGARD 445), 2,2'-methylene-bis(4-methyl-6-t-butylphenol) (e.g., VANOX MBPC), 2,2'-thiobis(2-t-butyl-5-methylphenol) (also known as 4,4'-thiobis(6-tert-butyl-m-cresol), CAS No. 96-69-5, commercially available from LOWINOX TBM-6), 2,2'-thiobis(6-t-butyl-4-methylphenol) (CAS No. 90-66-4, commercially available from LOWINOX TBM-6), and the like. TBP-6), tris[(4-tert-butyl-3-hydroxy-2,6-dimethylphenyl)methyl]-1,3,5-triazine-2,4,6-trione (e.g., CYANOX 1790), pentaerythritol tetrakis(3-(3,5-bis(1,1-dimethylethyl)-4-hydroxyphenyl)propionate (e.g., IRGANOX 1010, CAS number 6683-19-8), 3,5-bis(1,1-dimethylethyl)-4-hydroxybenzenepropanoic acid 2,2'-thiodiethanediyl ester (e.g., IRGANOX 1035, CAS number 41484-35-9), distearyl thiodipropionate ("DSTDP"), dilauryl thiodipropionate (e.g., IRGANOX PS 800), stearyl 3-(3,5-di-t-butyl-4-hydroxyphenyl)propionate (e.g., IRGANOX 1076), 2,4-bis(dodecylthiomethyl)-6-methylphenol (IRGANOX 1726), 4,6-bis(octylthiomethyl)-o-cresol (e.g., IRGANOX 1520), and 2',3-bis[[3-[3,5-di-tert-butyl-4-hydroxyphenyl]propionyl]]propionohydrazide (IRGANOX 1024).(C) is 4,4'-thiobis(2-t-butyl-5-methylphenol) (also known as 4,4'-thiobis(6-tert-butyl-m-cresol)), 2,2'-thiobis(6-t-butyl-4-methylphenol, tris[(4-tert-butyl-3-hydroxy-2,6-dimethylphenyl)methyl]-1,3,5-triazine-2,4,6-trione, distearyl thiodipropionate, or dilauryl thiodipropionate, or any of these. The combination may be any combination of two or more of the above. The combination may be tris[(4-tert-butyl-3-hydroxy-2,6-dimethylphenyl)methyl]-1,3,5-triazine-2,4,6-trione and distearyl thiodipropionate. The moisture-curable polyethylene formulation may be free of (C) peroxides. The (C) antioxidant, if present, may be 0.01 to 1.5 wt. %, alternatively 0.1 to 1.0 wt. %, of the total weight of the moisture-curable polyethylene formulation.

[0050] Optional Additive (D) A colorant, such as a pigment or dye. For example, carbon black or titanium dioxide. Carbon black may be provided as a carbon black masterbatch, which is a blend of poly(1-butene-co-ethylene) copolymer (95% to less than 100% by weight of the total weight of the masterbatch) and carbon black (0% to 5% by weight of the total weight of the masterbatch). Carbon black is a microcrystallized form of quasicrystalline carbon and has a high surface area to volume ratio, but less than that of activated carbon. Examples of carbon black are furnace carbon black, acetylene carbon black, conductive carbon (e.g., carbon fiber, carbon nanotubes, graphene, graphite, and expanded graphite platelets). The moisture-curable polyethylene formulation may be free of (D). If present, (D) is 0.1 to 35% by weight of the moisture-curable polyethylene formulation, alternatively 1 to 10% by weight.

[0051] Optional Additive (E) Scorch Retardant. (E) Scorch retardant functions to inhibit premature moisture cure of the moisture curable polyethylene formulation, where premature moisture cure would occur from premature or prolonged exposure of the formulation to ambient air or when the mixture is at ambient or elevated temperatures (e.g., during later melt extrusion). Examples of (E) are octyltriethoxysilane and octyltrimethoxysilane and vinyltrimethoxysilane. The moisture curable polyethylene formulation may be free of (E). (E), when present, may be 0.001-5.0% by weight of the moisture curable polyethylene formulation, alternatively 0.01-3.0% by weight, alternatively 0.10-1.5% by weight, alternatively 0.15-1.0% by weight.

[0052] Optional Additives (F) Stabilizers for stabilizing moisture curable polyethylene formulations against ultraviolet light (UV stabilizers). (F) stabilizers are compositionally distinct from (C) antioxidants, meaning that if a mixture contains both (C) and (F), the compound used as (C) will be different from the compound used as (F). Examples include hindered amine light stabilizers (HALS), benzophenones, or benzotriazoles. (F) UV stabilizers can be molecules, or aggregates of such molecules, that contain a basic nitrogen atom bonded to at least one sterically bulky organic group and function as inhibitors of degradation or decomposition. HALS are compounds that have sterically hindered amino functional groups and can inhibit oxidative degradation and also increase the shelf life of formulation embodiments that contain organic peroxides. Examples of suitable (F) are butanedioic acid dimethyl ester, polymer containing 4-hydroxy-2,2,6,6-tetramethyl-1-piperidine-ethanol (CAS No. 65447-77-0, commercially available LOWILITE 62), and N,N'-bisformyl-N,N'-bis(2,2,6,6-tetramethyl-4-piperidinyl)-hexamethylenediamine (CAS No. 124172-53-8, commercially available Uvinul 4050H). The moisture curable polyethylene formulation may be free of (F). When present, the (F) UV stabilizer may be 0.001 to 1.5% by weight, alternatively 0.002 to 1.0% by weight, alternatively 0.05 to 0.1% by weight of the moisture curable polyethylene formulation.

[0053] Optional Additives (G) Processing Aids: Molecules that reduce adhesion of the polymer melt in manufacturing equipment such as extruders and dies, and subsequently melt fracture of the material in embodiments where the moisture-curable polyethylene formulation is used therein. (G) can be fluoropolymers, polyorganosiloxanes, metal salts of fatty carboxylic acids, fatty carboxamides, waxes, ethylene oxide (co)polymers, and non-ionic surfactants. The moisture-curable polyethylene formulation may be free of (G). (G) Processing Aids, if present, may be 0.05-5% by weight of the moisture-curable polyethylene formulation.

[0054] Optional Additives (H) Flame Retardants. (H) Flame retardants are compounds that inhibit or slow the spread of fire by inhibiting chemical reactions in a flame. (H) Flame retardants can be (H1) minerals, (H2) organic halogen compounds, (H3) (organic) phosphorus compounds, (H4) halogenated silicones, (H5) a combination of any two or more of (H1)-(H4), or (H6) a combination of any one of (H1)-(H4) with a flame retardant synergist (e.g., antimony trioxide). The moisture curable polyethylene formulation may be free of (H). (H) Flame retardants, if present, can be 0.1-80.0 wt.%, alternatively 1-50.0 wt.%, alternatively 5-30.0 wt.% of the moisture curable polyethylene formulation.

[0055] The homogeneous mixture may optionally further comprise any zero, one or more of the optional additives (B) through (H).

[0056] The homogeneous mixtures and moisture curable polyethylene formulations can be used to make articles of manufacture, such as coatings on substrates, tapes, films, layers of laminates, foams, and pipes.

[0057] Moisture curable polyethylene formulations can be moisture cured to produce a cured polymer product by exposure to ambient air or by immersion in hot water at 70°C to 95°C. The degree of crosslinking of the cured polymer product can be characterized by measuring the percent hot creep.

[0058] or precedes a different embodiment. May is not required but confers latitude for choice. Optional (optionally): Absent (or excluded) or present (or included).

[0059] Density: Measured according to ASTM D792-13, Standard Test Method for Density and Specific Gravity (Relative Density) of Plastics by Displacement, Method B (for testing solid plastics in liquids other than water, e.g., in liquid 2-propanol). Units of grams per cubic centimeter (g / cm3 ).

[0060] Melt Index ("I2"): Measured in accordance with ASTM D1238-13 using the 190°C / 2.16 kg condition, formerly known as "Condition E". In grams per 10 minutes (g / 10 min).

[0061] Wire preparation method: Reactor copolymer of ethylene and VTMS (1.5% vinyltrimethoxysilane). Available as Dow DFDB-5451 silane copolymer. The copolymer also contained 0.5% immersed octyltriethoxysilane as a moisture scavenger. In all comparative and inventive examples, 95% by weight of the immersed copolymer was mixed with 5% or 9% by weight of a homogenous mixture (catalyst masterbatch) containing the remaining additives in a wireline extruder to form a 0.635 millimeter (mm, 25 mil) wall wire with a 14 AWG conductor. The wire was then immersed in a 90°C water bath for 3 hours for moisture curing and crosslinking.

[0062] Hot creep test method: After crosslinking, the wire sample prepared by the wire preparation method is peeled off to remove the conductor, and then the crosslinking degree of the peeled off insulation is measured at 20 Newtons per square meter (N / m 2 ) for 15 minutes at 200°C. The higher the degree of crosslinking, the lower the sample will elongate under load and therefore the lower the hot creep %.

[0063] After crosslinking, the mechanical properties of tensile strength and elongation were measured on an Instron machine using fully crosslinked wire samples prepared by the wire preparation method. The conductor was removed from the sample with a length of 12.7 cm (5 in). The samples were tested according to IEC 60502 at 25.4 cm per minute (cm / min, 10 in / min). The minimum values ​​for tensile strength and elongation according to the IEC 60502 specifications are 12 MPa (1800 pounds per square inch (psi)) and 200%, respectively.

[0064] Unaged and Aged Tensile and Elongation Test Method. This is a heat aged performance test without a conductor: The conductor was removed from the crosslinked samples and the samples were heat aged in an oven at 135°C for 168 hours according to IEC-60502. At the end of the aging period, the heat aged samples were removed from the oven and allowed to cool under ambient conditions for a minimum of 16 hours. The tensile strength and elongation of the heat aged samples were then compared to that of the unaged samples. According to IEC-60502, if the difference in tensile strength and elongation between the heat aged and unaged samples is less than 25%, the sample passes the test.

[0065] Mandrel Bend Test Method. This is a heat aging test on copper. IEC-60502-2 specifies that if after heat aging it is difficult to remove the insulation without damaging the conductor, the mandrel bend test should be performed. For the mandrel test, unstripped wire (both conductor and insulation) prepared by the wire preparation method was heat aged at 150°C for 10 days. The heat aged wire was left at room temperature for a minimum of 16 hours before being wound around a mandrel at a speed of 5 seconds per revolution. The recommendations in IEC-60502-2 for the number of turns based on the mandrel diameter and core thickness were followed. If there are no cracks in the insulation, the sample passes the test. EXAMPLES

[0066] The following comparative and inventive examples were made using a Banbury Type 1D mixer / extruder / pelletizer system, including a Banbury Type 1D mixer apparatus, an extruder apparatus, and a pelletizer apparatus, in a sequential material flow communication. The Banbury 1D batch mixer is available from HF Mixing Group, Freudenberg, Germany. The Banbury 1D batch mixer includes a mixing chamber with a solids feed inlet for accepting solids to be mixed into the mixing chamber, a liquid injector for adding liquid to the mixing chamber, and a drop door for allowing the prepared batch mixture to exit the mixing chamber and be transferred directly to the extruder / pelletizer apparatus. The Banbury 1D batch mixer also includes a feed hopper for feeding solids to the mixing chamber via the feed inlet. The Banbury 1D batch mixer also includes a ram that is movable from an up position to a down position and vice versa. When the ram is in the up position, the feed inlet of the mixing chamber is open, allowing the mixing chamber to receive solids from the feed hopper. When the ram is in the down position, it seals the feed inlet of the mixing chamber and presses the material contained in the mixing chamber, the amount of pressing being controllable by setting the ram pressure. The Banbury 1D batch mixer also includes a variable speed rotor (rotatable mixing element) disposed within the mixing chamber and effective for mixing the solid and liquid materials contained within the mixing chamber, the rotor designed to mix in a second direction perpendicular to the first direction. The Banbury 1D batch mixer also includes a heat exchanger jacket in heat exchange communication with the mixing chamber, the rotor, and the drop door. The Banbury 1D batch mixer has a mixing chamber volume of 16.1 liters (L) and a batch capacity of 12 kilograms (kg), using a specific gravity of 1 gram per milliliter (g / mL) and a packing ratio of 0.75. The mixing conditions can be controlled by setting the ram pressure and the rotational speed of the mixing element. The preferred ram pressure is 0.138 to 0.552 megapascals (MPa).The preferred rotation speed is 40 to 100 revolutions per minute (rpm).The extruder / pelletizer is configured with the following series of screens for screening the batch mixture: 20 mesh / 150 mesh / 80 mesh / 60 mesh / 20 mesh.

[0067] Polyolefin 1: Density is 0.965g / cm 3 High density polyethylene pellets with a melt index (I2) of 7.5 to 8.5 g / 10 min. Available from The Dow Chemical Company as DGDA-6944.

[0068] Polyolefin 2: Density 0.955g / cm 3 High density polyethylene pellets having a melt index (I2) of 1.2 to 1.8 g / 10 min. Available from The Dow Chemical Company as DMDC-1250.

[0069] Polyolefin 3: Density 0.945g / cm 3 High density polyethylene granules having a melt index (I2) of 0.87 to 1.07 g / 10 min. Available from The Dow Chemical Company as DFH-4593H.

[0070] Liquid hydrocarbyl sulfonic acid 1: Viscosity 2700mm 2 / sec NACURE CD 2180 M (available from King Industries).

[0071] Metal deactivator (B)-1: Oxalyl bis(benzylidene)hydrazide (OABH).

[0072] Antioxidant (C)-1: NAUGARD 445 is 4-(1-methyl-1-phenylethyl)-N-[4-(1-methyl-1-phenylethyl)phenyl]aniline.

[0073] Antioxidant (C)-2: LOWINOX 22IB46 is 4,4-thiobis(6-tert-butyl-m-cresol).

[0074] Antioxidant (C)-3: DSTDP is distearyl thiodipropionate.

[0075] Comparative Examples 1 and 2 (CE1 and CE2): Two non-homogeneous mixtures made separately using a Banbury Type 1D mixer / extruder / pelletizer system with the following ingredients: Polyolefin 1 or 2 (both pellets), Liquid Hydrocarbyl Sulfonic Acid 1, Metal Deactivator (B)-1, Antioxidant (C)-1, Antioxidant (C)-2, and Antioxidant (C)-3. The comparative method had six mixing stages, each defined as a ram-up and ram-down cycle. At the start, the ram position was up and the mixer drop door was closed. Stage 1: Before the ram was fed, ingredients were added sequentially to the mixing chamber in the following order: first 50 parts by weight (total of 100 parts by weight) of Polyolefin 1, then all of the Metal Deactivator (B)-1, then all of the Antioxidant (C)-2, then the remaining 50 parts by weight of Polyolefin 1. The purpose of this first stage was to degas the material. Mixing was initiated using a pressure on the ram (ram pressure) of 0.38 MPa (55 psi) and a rotor speed of 105 revolutions per minute (rpm). After mixing for 30 seconds, the ram was raised, marking the end of the first stage. Stage 2: The ram was sent down again to start the second stage, with the purpose of further mixing the material until it was in liquid form. The ram pressure and rotor speed were kept the same as in the first stage. When the temperature of the mixer contents reached 160°C due to shear heating, the ram was sent up, marking the end of the second stage. Stage 3: At the start of the third stage, the mixer contents had cooled to below 160°C. Antioxidant (C)-1 was added to the mixer and mixing was initiated. The ram pressure was kept the same as in the first stage, but the rotor speed was reduced to 85 rpm to allow for longer mixing times. As in the second stage, the ram was raised when the temperature increased to 160°C due to shear heating, marking the end of the third stage. Stage 4: At the start of the fourth stage, the contents of the mixer had cooled to below 140°C. Antioxidant (C)-3 was charged to the mixer chamber. Mixing began after shear heating increased the temperature to 140°C, indicating the end of the fourth stage. Stage 5: At the start of the fifth stage, the contents of the mixer had cooled to below 160°C. Liquid hydrocarbyl sulfonic acid 1 in a plastic bag was added to the mixer along with the plastic bag.Mixing was started with a ram pressure of 0.31 MPa (45 psi) and rotor speed was 65 rpm for longer mixing time. After the batch temperature reached 160°C, the ram was raised to relax the co-compounds and the material was turned over, indicating the end of the fifth stage. Stage 6: At the start of the sixth stage, the contents of the mixer had cooled to below 160°C. The ram was sent down to start the sixth stage, where the liquid hydrocarbyl sulfonic acid 1 was further mixed with the remaining material at the same processing conditions as the fifth stage. The ram was raised when the temperature increased to 160°C due to shear heating, indicating the end of the sixth stage. The mixer door was opened and the resulting mixture was dripped into the extruder chamber for pelletization. The mixer door was then closed and the mixer was ready for the next process. CE2 was made using the same process as CE1, except that polyolefin 2 was used instead of polyolefin 1 in CE2. The mixing operation conditions, stepwise addition order of CE1 and CE2, mixing operation observations, batch mixture composition, and batch mixture properties are shown later in Tables 1-5.

[0076] Inventive Examples 1 and 2 (IE1 and IE2): Two homogenous mixtures were made separately with the following ingredients using a Banbury Type 1D mixer / extruder / pelletizer system: Polyolefin 3 (granules), Liquid Hydrocarbyl Sulfonic Acid 1, Metal Deactivator (B)-1, Antioxidant (C)-1, Antioxidant (C)-2, and Antioxidant (C)-3. The inventive process used liquid injection of Liquid Hydrocarbyl Sulfonic Acid 1 metered into the mixer chamber from the drive side of the mixer. The process differed from CE1 and CE2. A small portion of Polyolefin 3 (0.9 kg (2 pounds (lbs) of Polyolefin 3) representing 7.4 parts by weight of a total of 12 kg (27 pounds), 100 parts by weight of Polyolefin 3) was set aside. The majority of Polyolefin 3, 11.2 kg (representing 92.6 parts by weight), was split into two equal portions of 46.3 parts by weight each. The inventive process was carried out in three stages. At the start of the process, the ram was in the up position and the mixer door was closed. Stage A: The ingredients were added sequentially to the mixing chamber in the following order: first 46.2 parts by weight of Polyolefin 3, then all of the Metal Deactivator (B)-1, then all of the Antioxidant (C)-2, then all of the Antioxidant (C)-3, then a second 46.2 parts by weight of Polyolefin 3 was added to the mixing chamber. The ram was lowered and mixing began. When the batch temperature reached 100°C due to shear heating, the liquid injection system pump was started and began metering liquid Hydrocarbyl Sulfonic Acid 1 into the mixing chamber. The liquid addition time was approximately 3 minutes (which continued until the second stage described below). In the first stage, the ram pressure was 0.31 MPa (45 psi) and the rotor speed was 85 rpm. When the batch temperature reached 120°C due to shear heating, the ram was raised, indicating the end of the first stage. The material was not yet completely melted. Stage B: At the start of the second stage, all of the antioxidant (C)-3 and 7.4 parts by weight of Polyolefin 3 were fed into the mixing chamber. The ram was then lowered and mixing began. The ram pressure and rotor speed were kept the same as in the first stage. When the batch temperature increased to 140°C due to shear heating, the ram was raised to relax the compound and the material was turned over, indicating the end of the second stage.Stage C: The ram was lowered and mixing was initiated using the same ram pressure and rotor speed as in the second stage. When the batch temperature increased to 145°C due to shear heating, the ram was raised, indicating the end of the third stage. The resulting homogenous mixture was removed from the mixer and dropped into the extruder chamber for pelletization. The mixing operation conditions, addition order per stage, mixing operation observations, batch mixture composition, and batch mixture properties for IE1 and IE2 are shown later in Tables 1-5. [Table 1]

[0077] An advantage of the inventive process is that fewer steps are required to make the inventive homogenous mixtures of IE1 and IE2 (3 steps) compared to the 6 steps required to make the comparative non-homogeneous mixtures of CE1 and CE2. Another advantage is that the inventive homogenous mixtures were made under gentler mixing conditions (maximum rotor speed of 85 rpm, maximum ram pressure of 0.31 MPa, and maximum batch temperature of 145° C.) compared to the comparative mixing conditions (maximum rotor speed of 105 rpm, maximum ram pressure of 0.38 MPa, and maximum batch temperature of 160° C.). [Table 2] [Table 3]

[0078] As shown in Table 3, in CE1, after five batches of CE1 were produced in succession without cleaning the mixer apparatus, the liquid hydrocarbyl sulfonic acid 1 accumulated or pooled in the mixing chamber of the mixer apparatus, leaving a dark stain on the surfaces of the mixer apparatus. Thus, the comparative method was not able to fully incorporate all of the liquid hydrocarbyl sulfonic acid 1 into the batch mixtures at the 4 wt. % loading, but instead left the unincorporated liquid hydrocarbyl sulfonic acid 1 from each batch mixture as a residue, and the residue increased as the number of successive batch mixtures made in the mixer apparatus without cleaning increased to 5. The same results were observed in CE2.

[0079] In contrast to Table 3 for IE1, the liquid hydrocarbyl sulfonic acid 1 did not accumulate or pool in the mixing chamber of the mixer apparatus as no dark stains were observed on the surface of the mixer apparatus after five batch mixtures of IE1 were produced in succession without cleaning the mixer apparatus. Only minimal dark stains were observed as spots on the surface of the mixer apparatus even after making 15 consecutive batch mixtures of IE1 without cleaning the mixer apparatus. Thus, the method of the present invention is able to fully incorporate all the liquid hydrocarbyl sulfonic acid 1 into the batch mixtures at a loading of 4 wt.%, leaving no unincorporated liquid hydrocarbyl sulfonic acid 1 from each batch mixture as a residue. The same results were observed for IE2.

[0080] The improvement is believed to be due to at least two reasons: first, the surface area of ​​the granular resin is greater than that of the pellets, which allows the liquid hydrocarbyl sulfonic acid 1 to be more fully incorporated into the polyolefin 3. Second, the slower addition of the liquid hydrocarbyl sulfonic acid 1 by using a liquid injection system. [Table 4] [Table 5]

[0081] Another advantage of the method of the present invention was the shorter total period of time to make the inventive homogeneous mixture of IE1 and IE2, which (5.5-6 min) was about half the total period of time required to make the heterogeneous mixture of CE1 and CE2 (10-13 min). This is shown in the previous Table 3. Thus, the total exposure time of the antioxidants in the inventive homogeneous mixture of IE1 and IE2 in the mixer apparatus was much shorter than the total exposure time of the relatively heterogeneous mixture of CE1 and CE2 in the mixer apparatus. This means that when the same amount of antioxidants is used, their antioxidant effect is reflected in the extrusion, pelleting, and heat aging tests to a greater extent in IE1 and IE2 than in CE1 and CE2.

[0082] As a result, pellets made from batch mixtures of IE1 and IE2 had more available antioxidant power and improved heat aging properties compared to pellets made from batch mixtures of CE1 and CE2. This is shown in Table 5, where the retention of tensile strength and elongation at break for CE1 and CE2 was less than 75%, which did not pass the IEC-60502 requirements. For IE1 and IE2, advantageously, the retained tensile strength and retained elongation at break was greater than 80%, which passes the IEC-60502 requirements. The significantly shorter total time required to make the inventive homogenous mixtures of IE1 and IE2 compared to the time required to make the relatively non-homogeneous mixtures of CE1 and CE2 was not expected, leading to a beneficial improvement in the heat aging performance of the inventive homogenous mixtures of IE1 and IE2. The invention as originally claimed in the present application is set forth below. [1] A method for making a homogenous mixture containing 1 to 6 parts by weight of a liquid hydrocarbyl sulfonic acid per 100 parts by weight of polyolefin in a mixer apparatus, comprising steps (1) to (3): (1) mixing a recently added liquid hydrocarbyl sulfonic acid in a pressure mixing operation carried out in a pressurizable mixer apparatus with an initial polyolefin blend consisting essentially of 90 to 98 parts by weight of said polyolefin to obtain a first mixture, said polyolefin being in the form of granules, and wherein the temperature of said initial polyolefin blend from the time of adding said liquid hydrocarbyl sulfonic acid to the start of said mixing is in a first target temperature range of 95°C to 105°C. (2) adding 10 to 2 parts by weight of the polyolefin in granular form to the first mixture to obtain a second mixture; and (3) mixing the second mixture in a pressure mixing operation conducted in a pressurizable mixer apparatus until the temperature of the second mixture increases to a final target temperature range of 145 to 150°C, thereby producing the homogenous mixture in the mixer apparatus, wherein all of the liquid hydrocarbyl sulfonic acid is incorporated into the 100 parts by weight of the polyolefin. [2] The method of [1], wherein step (3) comprises mixing the added 10-2 parts by weight of the polyolefin with the first mixture in a first direction to obtain a second mixture, continuing the mixing until a temperature of the second mixture increases to a third target temperature range of 135°C to 140°C, and subsequently mixing the second mixture in a second direction until a temperature of the second mixture increases to the final target range of 145°C to 150°C, wherein the second mixing direction is perpendicular to the first mixing direction. [3] The method of [2], wherein after mixing in the first direction and prior to mixing in the second direction, step (3) is interrupted by a non-pressurized mixing operation performed in the pressurizable mixer apparatus, comprising relaxing the second mixture for a period of time during which the second mixture is subjected to non-pressurized mixing, and during the relaxation, the temperature of the second mixture remains within the third target temperature range or is reduced to a minimum of 120°C. [4] The method according to any one of [1] to [3], wherein the initial polyolefin formulation of step (1) further consists essentially of at least one first solid additive or a melt thereof, the first mixture further consists essentially of the at least one first solid additive or a melt thereof, and the homogeneous mixture comprises the 100 parts by weight of the polyolefin, the 1 to 6 parts by weight of the liquid hydrocarbyl sulfonic acid, and the at least one first solid additive. [5] The method according to any one of [1] to [3], wherein step (2) further comprises adding the at least one second solid additive to the first mixture, the second mixture further comprising the at least one second solid additive, or a melt thereof, and the homogeneous mixture comprises the 100 parts by weight of the polyolefin, the 1 to 6 parts by weight of the liquid hydrocarbyl sulfonic acid, and the at least one second solid additive. [6] The method according to any one of [1] to [3], wherein the initial polyolefin formulation further consists essentially of at least one first solid additive or a melt thereof, the first mixture further consists essentially of the at least one first solid additive or a melt thereof, step (2) further comprises adding at least one second solid additive to the first mixture, the second mixture further comprises the at least one second solid additive or a melt thereof, and the homogeneous mixture comprises the 100 parts by weight of the polyolefin, the 1 to 6 parts by weight of the liquid hydrocarbyl sulfonic acid, the at least one first solid additive, and the at least one second solid additive. [7] The method according to any one of [1] to [6], wherein the number of parts by weight of the liquid hydrocarbyl sulfonic acid per 100 parts by weight of the polyolefin is from 2 to 6. [8] The method according to any one of [1] to [7], further comprising, after step (3), step (4) of mixing at least a portion of the homogeneous mixture with a (hydrolyzable silyl group)-functional polyethylene copolymer (HSG-FP copolymer) to thereby obtain a moisture-curable polyethylene formulation comprising at least a portion of the homogeneous mixture and the HSG-FP copolymer. [9] A homogeneous mixture prepared by any of the methods described in [1]-[7].

[10] A moisture-curable polyethylene formulation prepared by the method described in [8].

Claims

1. 1. A process for making a homogeneous molten mixture comprising 1 to 6 parts by weight of a liquid hydrocarbyl sulfonic acid per 100 parts by weight of polyolefin in a mixer apparatus, the process comprising steps (1) to (3): (1) in a pressure mixing operation conducted in a pressurizable mixer apparatus, adding and mixing a liquid hydrocarbyl sulfonic acid with an initial polyolefin formulation consisting essentially of 90 to 98 parts by weight of polyolefin to obtain a first mixture, wherein the polyolefin in said initial polyolefin formulation is in the form of granules having an average particle size of 0.2 mm to 1.5 mm, and wherein from the time of adding said liquid hydrocarbyl sulfonic acid to the start of said mixing, the temperature of said initial polyolefin formulation is in a first target temperature range of 95° C. to 105° C., and said mixing is continued until the temperature of said first mixture is increased to a second target temperature range of 115° C. to 125° C.; (2) adding 10 to 2 parts by weight of a polyolefin in the form of granules having an average particle size of 0.2 mm to 1.5 mm to the first mixture to obtain a second mixture; (3) mixing said second mixture in a pressure mixing operation conducted in a pressurizable mixer apparatus until the temperature of said second mixture is increased to a final target temperature range of 145° C. to 150° C., thereby creating said homogeneous molten mixture in said mixer apparatus, wherein all of said liquid hydrocarbyl sulfonic acid is incorporated into said 100 parts by weight of said polyolefin.

2. 2. The method of claim 1, wherein step (3) comprises mixing the added 10 to 2 parts by weight of the polyolefin with the first mixture in a first direction to obtain a second mixture, continuing the mixing until a temperature of the second mixture increases to a third target temperature range of 135° C. to 140° C., and subsequently mixing the second mixture in a second direction until a temperature of the second mixture increases to the final target range of 145° C. to 150° C., wherein the second mixing direction is orthogonal to the first mixing direction.

3. 3. The method of claim 2, wherein after mixing in the first direction and prior to mixing in the second direction, step (3) is interrupted by a non-pressurized mixing operation step performed in the pressurizable mixer apparatus comprising relaxing the second mixture for a period of time during which the second mixture is subjected to non-pressurized mixing, and during said relaxation, the temperature of the second mixture remains in the third target temperature range or is reduced to a minimum of 120°C.

4. 4. The method of any one of claims 1 to 3, wherein the initial polyolefin formulation of step (1) further consists essentially of at least one first solid additive or a melt thereof, the first mixture further consists essentially of the at least one first solid additive or a melt thereof, and the homogeneous molten mixture comprises the 100 parts by weight of the polyolefin, the 1 to 6 parts by weight of the liquid hydrocarbyl sulfonic acid, and the at least one first solid additive.

5. 4. The method of any one of claims 1 to 3, wherein step (2) further comprises adding at least one second solid additive to the first mixture, the second mixture further comprising the at least one second solid additive, or a melt thereof, and the homogeneous molten mixture comprises the 100 parts by weight of the polyolefin, the 1 to 6 parts by weight of the liquid hydrocarbyl sulfonic acid, and the at least one second solid additive.

6. 4. The method of any one of claims 1 to 3, wherein the initial polyolefin formulation further consists essentially of at least one first solid additive or a melt thereof, the first mixture further consists essentially of the at least one first solid additive or a melt thereof, step (2) further comprises adding at least one second solid additive to the first mixture, the second mixture further comprises the at least one second solid additive or a melt thereof, and the homogeneous molten mixture comprises the 100 parts by weight of the polyolefin, the 1 to 6 parts by weight of the liquid hydrocarbyl sulfonic acid, the at least one first solid additive, and the at least one second solid additive.

7. The process according to any one of claims 1 to 6, wherein the number of parts by weight of said liquid hydrocarbyl sulfonic acid is from 2 to 6 per 100 parts by weight of said polyolefin.

8. 8. The method of any one of claims 1 to 7, further comprising, after step (3), step (4) mixing at least a portion of the homogeneous molten mixture with a (hydrolyzable silyl group)-functional polyethylene copolymer (HSG-FP copolymer), resulting in a moisture-curable polyethylene formulation comprising the at least a portion of the homogeneous molten mixture and the HSG-FP copolymer.

Citation Information

Patent Citations

  • UV stabilisation of a cross-linkable polyolefin composition comprising an acidic silanol condensation catalyst

    EP2072568A1

  • Light source lighting device and lighting fixture

    JP2018085241A

  • Semi-crystalline polyolefin additive masterbatch composition

    JP2019535862A