Copolymer, resin composition for injection molding, molded article, and method for producing copolymer
A copolymer with controlled molecular weight distribution and composition ensures high transparency and strength in molded products, addressing defects in conventional copolymers, suitable for high-design applications.
Patent Information
- Application Number
- JP2023512934
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2021-04-08
- Filing Date
- 2022-03-24
- Publication Date
- 2024-11-28
- Estimated Expiration
- 2042-03-24
AI Technical Summary
Conventional copolymers containing aromatic vinyl and cyano monomer units do not meet the increasing demands for transparency, reduction in defects in terms of strength and hue, and appearance quality in molded products.
A copolymer with specific molecular weight distribution characteristics, where the ratio of peak intensities detected at UV254 nm and differential refractive index detector in the peak half-width is controlled to 0.15 or less, and a resin composition comprising this copolymer, produced through controlled polymerization methods to ensure uniform composition distribution.
The copolymer achieves excellent strength, chemical resistance, and transparency in molded articles, suitable for high-design applications such as cosmetic containers and stationery.
Smart Images

Figure 0007591646000001
Abstract
Description
[Technical field]
[0001] The present invention relates to a copolymer containing an aromatic vinyl monomer unit and a cyano-based monomer unit, an injection molding resin composition containing the copolymer, and a molded article molded from the resin composition. [Background technology]
[0002] Copolymers containing aromatic vinyl monomer units and cyano monomer units have excellent properties such as chemical resistance, rigidity, and moldability, and are therefore used in a wide range of fields. These copolymers can be produced by various polymerization methods such as emulsion polymerization, suspension polymerization, bulk polymerization, and solution polymerization. However, since an emulsifier is used in the case of emulsion polymerization, and a dispersant is used in the case of suspension polymerization, there are problems with the appearance quality in terms of transparency and coloring and discoloration of the polymerization product. Therefore, non-aqueous bulk polymerization or solution polymerization is often adopted from the perspectives of quality, cost, and environment.
[0003] When bulk polymerization or solution polymerization is carried out continuously on an industrial production scale, the latent heat of vaporization is utilized, that is, heat is removed by evaporation from the gas-liquid interface between the gas phase and the polymerization liquid, or, if necessary, the evaporated solvent and unreacted monomers are cooled in a condenser outside the reaction vessel and refluxed into the reaction vessel, thereby enabling polymerization at a high conversion rate, and therefore this method is widely used as an industrial production scale polymerization method.
[0004] Disclosed are a method in which the concentration of the condensed liquid refluxing from the condenser of the polymerization vessel is adjusted and this is sprayed back into the gas phase part of the polymerization vessel (Patent Document 1), and a method in which the raw material liquid is sprayed into the upper gas phase part of the reaction vessel using a spray nozzle or the like and the condensed liquid refluxing from the condenser is mixed with the raw material liquid and supplied to the polymerization vessel (Patent Document 2). [Prior art documents] [Patent documents]
[0005] [Patent Document 1] JP 2000-226417 A [Patent Document 2] JP 2004-262987 A Summary of the Invention [Problem to be solved by the invention]
[0006] However, it cannot be said that the copolymers obtained by the above-mentioned conventional techniques necessarily provide satisfactory results in terms of the recently increasing demand for reducing the incidence of defects in terms of physical properties including transparency, strength, hue, etc.
[0007] Therefore, an object of the present invention is to provide a copolymer containing an aromatic vinyl monomer unit and a cyano-based monomer unit, which has excellent strength, chemical resistance, hue and transparency when made into a molded article, and an injection molding resin containing the copolymer. [Means for solving the problem]
[0008] As a result of intensive research aimed at solving the above problems, the present inventors have found that when a copolymer containing an aromatic vinyl monomer unit and a cyano monomer unit satisfies the following constitution in terms of the molecular weight distribution of the copolymer, the resulting molded article has excellent strength, chemical resistance, hue and transparency, and have completed the present invention. That is, the present invention provides (1) A copolymer containing an aromatic vinyl monomer unit and a cyano monomer unit, in which, when the peak intensity detected at UV 254 nm within the peak half-width of the weight-average molecular weight MwRI of the copolymer determined by gel permeation chromatography using a differential refractive index detector is P(UV), and the peak intensity detected by the differential refractive index detector within the peak half-width of MwRI is P(RI), the difference between the maximum and minimum values of P(UV) / P(RI) is 0.15 or less. (2) The copolymer according to (1), which contains 50 to 90 mass% of the aromatic vinyl monomer units and 10 to 50 mass% of the cyano monomer units, when the total of the aromatic vinyl monomer units and the cyano monomer units is taken as 100 mass%. (3) The copolymer according to (1) or (2), wherein the aromatic vinyl monomer unit is a styrene monomer unit, and the cyano monomer unit is an acrylonitrile monomer unit. (4) A resin composition for injection molding, comprising the copolymer according to any one of (1) to (3). (5) A molded article molded from the resin composition for injection molding according to (4), and (6) A method for producing a copolymer containing an aromatic vinyl monomer unit and a cyano-based monomer unit, comprising the steps of: feeding a feed liquid containing an aromatic vinyl monomer and a cyano-based monomer into a liquid phase of a polymerization liquid in a reaction vessel; and condensing an evaporated gas generated in the reaction vessel with a heat exchanger outside the reaction vessel and returning the obtained condensate to the liquid phase of the reaction vessel. Regarding. Effect of the Invention
[0009] According to the present invention, there is provided a copolymer which is excellent in strength, chemical resistance, hue and transparency when molded into a molded article. The resin composition according to the present invention can be suitably used for containers for cosmetics and the like, miscellaneous goods such as stationery, which require high designability. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0010] <Specification of molecular weight distribution of copolymer> In the copolymer containing aromatic vinyl monomer units and cyano monomer units according to the present embodiment, when the peak intensity detected at UV254 nm in the peak half-width of the weight average molecular weight MwRI determined by a differential refractive index detector in gel permeation chromatography (hereinafter sometimes abbreviated as "GPC") is P(UV), and the peak intensity detected by a differential refractive index detector in the peak half-width of MwRI is P(RI), the difference between the maximum and minimum values of P(UV) / P(RI) is 0.15 or less, preferably 0.10 or less. Specifically, for example, it is 0.15 or less, 0.13 or less, 0.11 or less, 0.10 or less, 0.09 or less, 0.08 or less, 0.07 or less, 0.06 or less, or 0.05 or less. If the difference between the maximum and minimum values of P(UV) / P(RI) exceeds 0.15, the color of the molded product may be poor. A copolymer in which the difference between the maximum and minimum values of P(UV) / P(RI) is 0.15 or less can be obtained, for example, by the production method described below, but is not limited thereto.
[0011] In the GPC measurement, tetrahydrofuran (hereinafter, sometimes abbreviated as "THF") can be used as the mobile phase. MwRI is a value calculated in terms of polystyrene, and can be measured under the following conditions. Device name: SYSTEM-21 Shodex (Showa Denko Co., Ltd.) Column: Three PL gel MIXED-B columns (Polymer Laboratories) in series Temperature: 40℃ Solvent: Tetrahydrofuran Concentration: 0.4% by mass Calibration curve: Created using standard polystyrene (PS) (Polymer Laboratories)
[0012] In the GPC measurement in this embodiment, a GPC device is used that has a differential refractive index detector and an absorptiometric detector and can simultaneously perform measurements using these detectors. The absorptiometric detector is configured to be able to measure absorbance at a wavelength of 254 nm. In the molecular weight distribution obtained by the GPC measurement, the concentration of each component contained in each molecular weight in the distribution is measured by the differential refractive index detector, and the absorbance of each molecular weight component (measurement wavelength 254 nm) is measured by the absorptiometric detector. The measurement wavelength 254 nm is derived from the structure of the benzene ring. The absorptiometric detector may be a detector that measures the absorption of ultraviolet light of a specific wavelength, or a detector that performs spectroscopic measurement of the absorption of ultraviolet light of a specific range of wavelengths.
[0013] The peak half-width of the weight-average molecular weight MwRI refers to the width of the elution times before and after the peak, among the elution times that give half the value of the highest peak intensity, which is taken as the peak in the chromatogram obtained by plotting the values measured by a differential refractive index detector. Note that even when the peak is multimodal, the elution time that gives the highest peak intensity is used as the reference. In addition, there may be more than two elution times that give half the value of the highest peak intensity, and among such elution times, the width of the elution times before and after the peak that are the furthest from the peak is referred to.
[0014] The peak intensities P(RI) and P(UV) indicate peak intensities in the half-width ranges mentioned above in a chromatogram obtained by plotting the values measured with a refractive index detector and the values measured with an absorptiometry detector (measurement wavelength 254 nm) against the molecular weight of the resin converted from the GPC elution volume.
[0015] <Copolymer containing aromatic vinyl monomer units and cyano monomer units> The copolymer according to the present embodiment contains an aromatic vinyl monomer unit and a cyano-based monomer unit, and may contain a monomer unit other than the aromatic vinyl monomer unit and the cyano-based monomer unit as long as the effect of the present invention is not impaired. The monomer units constituting the copolymer containing aromatic vinyl monomer units and cyano monomer units according to this embodiment will be described below.
[0016] <Aromatic vinyl monomer unit> The monomer that gives the aromatic vinyl monomer unit contained in the copolymer according to the present embodiment is not particularly limited, and examples thereof include substituted styrenes having a substituent such as styrene, α-methylstyrene, p-methylstyrene, 3,5-dimethylstyrene, 4-methoxystyrene, and 2-hydroxystyrene, halogenated styrenes such as α-bromostyrene and 2,4-dichlorostyrene, and 1-vinylnaphthalene, etc. Among these, styrene is preferred from the viewpoints of polymerizability, moldability, mechanical properties, etc.
[0017] <Cyano monomer unit> The monomer that gives the cyano monomer unit contained in the copolymer according to the present embodiment is not particularly limited, and examples thereof include acrylonitrile, methacrylonitrile, α-chloroacrylonitrile, α-ethylacrylonitrile, etc. Among these, acrylonitrile is preferred from the viewpoints of polymerizability, mechanical properties, etc.
[0018] The content ratio of the aromatic vinyl monomer unit and the cyano monomer unit in the copolymer in this embodiment can be selected arbitrarily, but the amount of the aromatic vinyl monomer unit contained in 100% by mass of the copolymer is preferably 50% by mass to 90% by mass, more preferably 55% by mass to 88% by mass, and even more preferably 60% by mass to 85% by mass. Specifically, for example, it may be 50% by mass, 55% by mass, 60% by mass, 65% by mass, 70% by mass, 75% by mass, 80% by mass, 85% by mass, or 90% by mass, and may be within a range between any two of the numerical values exemplified here. The amount of the cyanide vinyl monomer contained in 100% by mass of the copolymer is preferably 10% by mass to 50% by mass, more preferably 12% by mass to 45% by mass, and even more preferably 15% by mass to 40% by mass. Specifically, for example, the content is 10 mass%, 15 mass%, 20 mass%, 25 mass%, 30 mass%, 35 mass%, 40 mass%, 45 mass%, or 50 mass%, and may be within a range between any two of the numerical values exemplified here. If each monomer is outside the above composition range, it may be difficult to achieve the appearance, chemical resistance, transparency, mechanical properties, etc. of the molded article that are the object of the present invention.
[0019] <Monomer units other than aromatic vinyl monomer units and cyano monomer units> In the copolymer of the present embodiment, a copolymerizable monomer other than the vinyl cyanide monomer and the aromatic vinyl monomer may be copolymerized to the extent that the effect of the present invention is not impaired. Examples of other vinyl compounds copolymerizable with the vinyl cyanide monomer and the aromatic vinyl monomer include acrylic acid esters such as methyl methacrylate, ethyl methacrylate, methyl acrylate, ethyl acrylate, and butyl acrylate, unsaturated carboxylic acids or anhydrides such as acrylic acid, methacrylic acid, maleic anhydride, and itaconic acid, and maleimide compounds such as N-phenylmaleimide and N-cyclohexylmaleimide, and more preferably ethyl acrylate and butyl acrylate, and two or more of these may be mixed and used.
[0020] The content of these monomer units contained in the copolymer in this embodiment is 0% by mass to 20% by mass, preferably 0% by mass to 5% by mass, assuming that the total of the vinyl cyanide monomer units, the aromatic vinyl monomer units, and the monomer units derived from monomers copolymerizable therewith is 100% by mass.
[0021] <Resin composition> The resin composition in this embodiment is a resin composition containing a copolymer containing an aromatic vinyl monomer unit and a cyano-based monomer unit. In the resin composition, the content of the copolymer of the aromatic vinyl monomer unit and the cyano-based monomer unit in 100% by mass of the resin composition is, for example, 50% by mass or more. In one aspect, the content of the copolymer in the resin composition is preferably 80% by mass or more, more preferably 90% by mass or more. Specifically, for example, it is 50, 55, 60, 65, 70, 75, 80, 85, or 90% by mass or more. In one aspect, the resin composition may be substantially composed of only a copolymer containing an aromatic vinyl monomer unit and a cyano-based monomer unit.
[0022] The resin composition in this embodiment may contain mineral oil within a range that does not impair the effects of the present invention. In addition, additives such as internal lubricants such as stearic acid and ethylene bisstearylamide, phenol-based antioxidants, phosphorus-based antioxidants, sulfur-based antioxidants, lactone-based antioxidants, ultraviolet absorbers, hindered amine-based stabilizers, antistatic agents, and external lubricants may be included. These additives may be added and mixed in the polymerization process, the devolatilization process, and the granulation process, or added and mixed in an extruder or an injection molding machine during molding, and are not particularly limited.
[0023] The ultraviolet absorbent has a function of suppressing deterioration or coloration caused by ultraviolet rays, and examples thereof include ultraviolet absorbents based on benzophenones, benzotriazoles, triazines, benzoates, salicylates, cyanoacrylates, anilide oxalates, malonic esters, formamidines, etc. These may be used alone or in combination of two or more kinds, and may be used in combination with a light stabilizer such as a hindered amine.
[0024] In order to express various designs, the resin composition in this embodiment may contain various dyes and pigments within a range that does not impair the effects of the present invention. For example, coumarin fluorescent dyes, benzopyran fluorescent dyes, perylene fluorescent dyes, anthraquinone fluorescent dyes, thioindigo fluorescent dyes, xanthene fluorescent dyes, xanthone fluorescent dyes, thioxanthene fluorescent dyes, thioxanthone fluorescent dyes, thiazine fluorescent dyes, and diaminostilbene fluorescent dyes can be mentioned. The content of the dyes and pigments is preferably 0.00001 to 1 part by mass, more preferably 0.00003 to 0.3 parts by mass, based on 100 parts by mass of additives such as the resin composition and antioxidants in total.
[0025] <Method for producing a copolymer containing aromatic vinyl monomer units and cyano monomer units> In the present embodiment, the copolymer containing aromatic vinyl monomer units and cyano monomer units can be produced by a suspension polymerization method, a solution polymerization method, a bulk polymerization method, or the like. However, in order to prevent the inclusion of a dispersant or the like in the resin, the solution polymerization method or the bulk polymerization method is preferably used.
[0026] <Polymerization equipment> The polymerization apparatus used in this embodiment comprises a complete mixed tank type polymerization vessel (I) equipped with a heat exchanger for condensing vapor from the gas phase, or the polymerization vessel (I) and one or more polymerization vessels (II) connected thereto. The polymerization vessel (II) may be a complete mixed tank type polymerization vessel, a tubular type polymerization vessel, an extruder type polymerization vessel, a kneader type polymerization vessel, or the like.
[0027] The embodiment for making the polymerization liquid in the polymerization vessel (I) substantially uniform is not particularly limited, and in addition to stirring and mixing using ribbon-type stirring blades such as helical ribbon blades, turbine-type stirring blades, screw-type stirring blades, anchor blades, paddle blades such as inclined paddle blades and flat paddle blades, Full Zone blades (product name), Max Blend blades (product name), Sun Mellor blades (product name), or the like, it is also possible to combine this with circulation mixing using a pump or the like provided outside the polymerization vessel (I), for example.
[0028] Examples of the heat exchanger used in this embodiment include a spray condenser and a shell-and-tube condenser.
[0029] The solvent used in the present embodiment is an inactive polymerization solvent that is usually used in radical polymerization, and examples thereof include aromatic hydrocarbons such as ethylbenzene, toluene, xylene, o-xylene, m-xylene, p-xylene, cumene, n-propylbenzene, isopropylbenzene, etc., ketones such as 2-butanone, methyl isobutyl ketone, etc., and amide compounds such as N,N-dimethylformamide, N,N-dimethylacetamide, N-methylpyrrolidone, etc. Among these solvents, ethylbenzene is preferred from the viewpoints of devolatilization and economic efficiency.
[0030] The amount of the solvent used is preferably 5 to 40 parts by mass, more preferably 10 to 35 parts by mass, based on 100 parts by mass of the monomer mixture. If it is less than 5 parts by mass, the viscosity of the polymerization liquid increases, so that the polymerization rate cannot be increased sufficiently, resulting in poor productivity. On the other hand, if it exceeds 40 parts by mass, the amount of devolatilized solvent increases, which is not economical.
[0031] The polymerization initiator added in this embodiment may be a known polymerization initiator, and examples of such initiators include ketone peroxides such as methyl ethyl ketone peroxide, peroxyketals such as 1,1-bis(t-butylperoxy)3,3,5-trimethylcyclohexane and 2,2-bis(4,4-di-t-butylperoxycyclohexyl)propane, hydroperoxides such as cumene hydroperoxide, dialkyl peroxides such as dicumyl peroxide, and diacyl peroxides such as benzoyl peroxide. Examples of the polymerization initiator include peroxides, peroxydicarbonates such as diisopropyl peroxydicarbonate, peroxyesters such as t-butylperoxyisopropyl carbonate, azonitriles such as 2,2'-azobisisobutyronitrile and 1,1'-azobis(cyclohexane-1-carbonitrile), and organic peroxides such as t-butylperoxyallyl carbonate, t-butyltrimethylsilyl peroxide, and 3,3',4,4'-tetra(t-butylperoxycarbonyl)benzophenone. Among these polymerization initiators, t-butylperoxyisopropyl carbonate is preferred from the viewpoint of color and economic efficiency. These polymerization initiators may be used alone or in combination of two or more.
[0032] The amount of polymerization initiator used is advantageously large in that it increases the reaction rate within the range where the removal of reaction heat in the polymerization apparatus can be controlled, but a high reaction rate can cause problems such as coloration. The practical amount used varies depending on the type of polymerization initiator and the polymerization temperature, but is preferably 0.005 to 0.5 parts by mass, more preferably 0.01 to 0.4 parts by mass, per 100 parts by mass of the total amount of monomers.
[0033] In the production of the copolymer according to this embodiment, for example, t-dodecyl mercaptan, n-dodecyl mercaptan, unsaturated dimer of α-methylstyrene, terpinolene, octyl thioglycolate, or the like may be used as a chain transfer agent.
[0034] The amount of the chain transfer agent used varies depending on the type of the chain transfer agent, but is preferably 5 parts by mass or less, more preferably more than 0 and 3 parts by mass or less, and even more preferably 1 to 0.001 parts by mass, relative to 100 parts by mass of the total amount of the monomers. If the amount exceeds 5 parts by mass, the molecular weight of the copolymer of the aromatic vinyl monomer unit and the cyano monomer unit becomes too small, causing problems such as failure to achieve practical strength.
[0035] The polymerization of the copolymer according to this embodiment is carried out, for example, as follows.
[0036] <Preparation of Feed Solution> First, a supply liquid containing a solvent, a polymerization monomer, a polymerization initiator, a chain transfer agent, etc. in a given ratio is prepared.
[0037] <Supply of feed liquid to reaction tank> The feed liquid is continuously fed to the liquid phase of the polymerization liquid to be fed to the reaction vessel. The feed rate when feeding the feed liquid to the liquid phase of the polymerization liquid depends on the temperature and the polymerization rate to be controlled, which will be described later, but it is preferable to adjust the residence time in the polymerization vessel to 2 to 6 hours. If the residence time is too short, the color may deteriorate, and if the residence time is too long, problems with productivity may occur.
[0038] <Polymerization of Monomer> The polymerization temperature is maintained within a predetermined range to carry out the polymerization. The polymerization temperature varies depending on the type of initiator used, but is preferably 120 to 180° C. If the polymerization temperature is within this range, the polymerization can be easily controlled, and the polymerization rate can be increased while preventing deterioration of the color tone.
[0039] <Control of reaction solution filling rate> The filling rate of the reaction liquid is maintained within a predetermined range, and the reaction liquid is continuously withdrawn in an amount equal to the amount of the supply liquid. The filling rate of the reaction liquid in the reaction tank is preferably 50 to 100 vol%, and by carrying out the polymerization within this range, excellent productivity is achieved.
[0040] <Condensation of evaporated gas> The evaporated gas generated in the reactor passes through the vapor line into a heat exchanger outside the reactor, where it condenses into a condensate, which is returned to the liquid phase of the reactor through a feed line.
[0041] <Recovery of copolymer> The withdrawn reaction liquid is degassed to remove unreacted monomers and organic solvent, and the copolymer is recovered as pellets.
[0042] When the peak intensity detected by UV 254 nm within the peak half width of the weight average molecular weight MwRI is P(UV), and the peak intensity detected by a differential refractive index detector within the peak half width of MwRI is P(RI), the copolymer in this embodiment, for example, produced by the above-mentioned production method, has a difference between the maximum and minimum values of P(UV) / P(RI) of 0.15 or less.
[0043] The difference between the maximum and minimum values of P(UV) / P(RI) represents the composition distribution of aromatic vinyl monomer units and cyano monomer units in the resin. The peak intensity of P(UV) detected by absorbance (measurement wavelength 254 nm) changes with the concentration of monomers with benzene rings, i.e., aromatic vinyl monomer units. On the other hand, since P(RI) depends on the concentration of the entire molecule, the fact that P(UV) / P(RI) shows a constant value regardless of molecular weight indicates that there is no difference in the composition distribution even if the molecular weight changes.
[0044] Although the mechanism by which the difference between the maximum and minimum values of P(UV) / P(RI) of the copolymer becomes 0.15 or less by such a production method has not been fully elucidated, it is considered that the reason is that, in the production method of the prior art, the copolymer composition distribution occurs due to the presence of supply from the gas phase, whereas in the production method according to the present embodiment, the feed liquid is supplied to the liquid phase of the polymerization liquid and the condensate is returned to the liquid phase of the reaction vessel, so there is no supply from the gas phase, and therefore the composition distribution of the copolymer becomes smaller, and the difference in composition distribution caused by the change in the molecular weight of the copolymer becomes smaller.
[0045] <Method for producing a resin composition containing a copolymer containing an aromatic vinyl monomer unit and a cyano monomer unit> A resin composition is obtained by adding mineral oil, additives, dyes and pigments, etc., as necessary, to the copolymer of aromatic vinyl monomer units and cyano monomer units obtained as described above. The additives may be added and mixed in the polymerization process, the devolatilization process, or the granulation process, or in an extruder or an injection molding machine during molding, but is not limited thereto.
[0046] The molded article obtained by molding the resin composition according to this embodiment can be processed into miscellaneous goods such as stationery, cosmetic containers, housings for home appliances, etc., which require high design quality. The resin composition according to this embodiment is preferably used alone or as a mixed resin blended with other resins such as ABS resin and PC resin. EXAMPLES
[0047] The following detailed description will be given using examples, but the present invention is not limited to the following examples.
[0048] <Example 1> The feed liquid to be fed to a 50L reactor was prepared to be 70 parts by mass of styrene, 15 parts by mass of acrylonitrile, 15 parts by mass of ethylbenzene, 0.02 parts by mass of t-butylperoxyisopropyl carbonate as a polymerization initiator, and 0.01 parts by mass of n-dodecyl mercaptan as a chain transfer agent. This feed liquid was bubbled with nitrogen gas, passed through a mixer, and then continuously fed to the reactor at a rate of 10.8 L / hour into the liquid phase of the polymerization liquid, so that the polymerization temperature was kept at 145°C and the filling rate of the reaction liquid in the reactor was kept at 70 vol%, and the reaction liquid was continuously extracted in an amount equal to the amount of the feed liquid. The evaporated gas generated in the reactor was condensed in a heat exchanger outside the reactor, and the condensate was returned to the liquid phase of the reactor. The extracted reaction liquid was introduced into a devolatilizer maintained at 250°C and a high vacuum of 10 mmHg, where unreacted monomers and organic solvents were degassed and recovered, and the copolymer was recovered as pellets.
[0049] <Example 2> The feed liquid to be supplied to a 50L reaction vessel was prepared to contain 58 parts by mass of styrene, 22 parts by mass of acrylonitrile, 20 parts by mass of ethylbenzene, 0.02 parts by mass of t-butylperoxyisopropyl carbonate as a polymerization initiator, and 0.04 parts by mass of n-dodecyl mercaptan as a chain transfer agent. After bubbling this feed liquid with nitrogen gas, it passed through a mixer and was continuously supplied to the reaction vessel at a rate of 8L / hour to the liquid phase of the polymerization liquid, so that the polymerization temperature was kept at 145°C and the filling rate of the reaction liquid in the reaction vessel was kept at 60vol%, and the reaction liquid was continuously extracted in an amount equal to the amount of the feed liquid. The evaporated gas generated in the reaction vessel was condensed in a heat exchanger outside the reaction vessel, and the condensate was returned to the liquid phase of the reaction vessel. The extracted reaction liquid was introduced into a devolatilizer under the same conditions as in Example 1, and the unreacted monomer and organic solvent were degassed and recovered, and the copolymer was recovered as pellets.
[0050] <Example 3> The feed liquid to be fed to a 50L reaction vessel was prepared to contain 49 parts by mass of styrene, 29 parts by mass of acrylonitrile, 23 parts by mass of ethylbenzene, 0.02 parts by mass of t-butylperoxyisopropyl carbonate as a polymerization initiator, and 0.12 parts by mass of n-dodecyl mercaptan as a chain transfer agent. After bubbling this feed liquid with nitrogen gas, it passed through a mixer and was continuously fed to the reaction vessel at a rate of 9.8 L / hour to the liquid phase of the polymerization liquid, so that the polymerization temperature was kept at 145°C and the filling rate of the reaction liquid in the reaction vessel was kept at 80 vol%, and the reaction liquid was continuously extracted in an amount equal to the amount of the feed liquid. The evaporated gas generated in the reaction vessel was condensed in a heat exchanger outside the reaction vessel, and the condensate was returned to the liquid phase of the reaction vessel. The extracted reaction liquid was introduced into a devolatilizer under the same conditions as in Example 1, and the unreacted monomer and organic solvent were degassed and recovered, and the copolymer was recovered as pellets.
[0051] <Example 4> The feed liquid to be supplied to the 50 L reaction vessel was prepared such that it contained 78 parts by mass of styrene, 7 parts by mass of acrylonitrile, 15 parts by mass of ethylbenzene, 0.02 parts by mass of t-butyl peroxyisopropyl carbonate as a polymerization initiator, and 0.01 parts by mass of n-dodecyl mercaptan as a chain transfer agent. This feed liquid was bubbled with nitrogen gas, and after passing through a mixer, it was continuously supplied to the liquid phase of the polymerization liquid into the reaction vessel at a rate of 10.8 L / hour. The polymerization temperature was maintained at 145°C, and the filling rate of the reaction liquid in the reaction vessel was maintained at 70 vol%. The same amount of reaction liquid as the feed liquid amount was continuously withdrawn. Incidentally, the evaporation gas generated in the reaction vessel was condensed in a heat exchanger outside the reaction vessel, and the condensate was returned to the liquid phase of the reaction vessel. The withdrawn reaction liquid was introduced into a volatile component removal device under the same conditions as in Example 1, and unreacted monomers and organic solvents were degassed and recovered. The copolymer was recovered as pellets.
[0052] <Comparative Example 1> Resin pellets were obtained in the same manner as in Example 1, except that the feed liquid was continuously introduced from the gas phase of the polymerization liquid.
[0053] <Comparative Example 2> Resin pellets were obtained in the same manner as in Example 1, except that the evaporation gas generated in the reaction vessel was condensed in a heat exchanger outside the reaction vessel, and the condensate was returned to the gas phase of the reaction vessel.
[0054] <Comparative Example 3> Resin pellets were obtained in the same manner as in Example 1, except that the feed liquid was continuously introduced by spraying from the gas phase of the polymerization liquid and from the liquid phase.
[0055] <Comparative Example 4> Resin pellets were obtained in the same manner as in Example 1, except that the feed liquid consisted of only styrene.
[0056] <GPC Measurement> After continuous operation for 360 hours under the conditions described in the examples and comparative examples, the pellets collected were subjected to GPC measurement under the conditions described above, and the maximum value, minimum value, and difference of P(UV) / P(RI) were measured.
[0057] <GPC Measurement Conditions> Device name: SYSTEM-21 Shodex (Showa Denko Co., Ltd.) Column: Three PL gel MIXED-B columns (Polymer Laboratories) in series Temperature: 40℃ Solvent: Tetrahydrofuran Concentration: 0.4% by mass Calibration curve: Created using standard polystyrene (PS) (Polymer Laboratories)
[0058] <Sample preparation> A sample was prepared by dissolving 60 mg of the copolymer in 15 mL of THF (tetrahydrofuran) at room temperature and filtering through a 0.45 μm syringe filter. The injection volume was 10 μL.
[0059] <Measurement of peak intensity P(RI) and P(UV)> The molecular weight of the resin was calculated from the GPC elution volume in the above-mentioned GPC measurement, and the values measured with a refractive index detector and a spectrophotometer (measurement wavelength 254 nm) were plotted against the molecular weight of the resin. In the chromatogram obtained, the peak intensities in the half-width range described above were designated as P(RI) and P(UV), respectively.
[0060] <Preparation of test pieces of resin composition> After 360 hours of continuous operation under the conditions described in the Examples and Comparative Examples, 100% by mass of pellets were collected, and 0.15% by mass of antioxidant 4,4',4''-(1-methylpropanyl-3-ylidene)tris(6-tert-butyl-m-cresol) (ADEKA CORPORATION, Adeka STAB AO-30) and 0.05% by mass of tris(2,4-di-tert-butylphenyl)phosphite (ADEKA CORPORATION, Adeka STAB 2112) were blended, and the mixture was extruded and pelletized using a single-screw extruder (IKG CORPORATION, MS-40). Using these pellets, test pieces were prepared using an injection molding machine, and various physical property values were measured.
[0061] <Charpy impact strength> The pellets thus obtained were used in accordance with JIS K-7111, and measurements were performed using unnotched test pieces, with the impact direction being edgewise, at a relative humidity of 50% and an atmospheric temperature of 23° C. The measuring machine used was a digital impact tester manufactured by Toyo Seiki Seisakusho Co., Ltd.
[0062] <Transmittance, YI value> The pellets were used to mold a plate-shaped molded product having a thickness of 127×127×3 mm at a molding temperature of 230° C. using an injection molding machine (J140AD-180H, manufactured by Nippon Steel & Sumitomo Metal Co., Ltd.). A test piece having a thickness of 115×85×3 mm was cut out from the plate-shaped molded product, and the end faces were polished by buffing to prepare a plate-shaped molded product having a mirror surface on the end face. The polished plate-shaped molded product was measured for the spectral transmittance of 350 nm to 800 nm at an optical path length of 115 mm using a UV-visible spectrophotometer V-670 manufactured by JASCO Corporation, with a size of 20×1.6 mm and an incident light with a spread angle of 0°, and the YI value at a field of view of 2° with a wavelength C light source was calculated according to JIS K7105. The transmittance indicates the total light transmittance in the range of 430 to 700 nm. The results are shown in Table 1.
[0063] <haze> In accordance with ASTM D-1003, a plate molded product of 127 x 127 x 3 mm thickness molded under the above-mentioned conditions was used and the haze was measured using a Nippon Denshoku Industries Co., Ltd. haze meter (NDH-2000).
[0064] <Chemical resistance> To eliminate the effects of molding distortion, test pieces were produced by press-molding each pellet at 260°C to a thickness of 4 mm, then cutting into 50mm x 50mm squares. After immersing in each chemical set at 40°C for 14 days, the specimens were classified as follows based on the changes in weight and appearance. Salad oil was used as the chemical. ◎: Almost no change in weight or appearance was observed; ○: Slight cloudiness or discoloration was observed; △: Slight cracking or crazing occurred; ×: Dissolution or significant effect occurred.
[0065] [Table 1]
[0066] Examples 1 to 4, which had a small difference between the maximum and minimum values of P(UV) / P(RI), were excellent in strength, transparency, YI value, and haze value. Comparative Examples 1 to 3, which had a large difference between the maximum and minimum values of P(UV) / P(RI), were low in strength, high in YI value, and poor in hue. [Industrial Applicability]
[0067] The resin composition containing the copolymer of the present invention and the molded article molded from the resin composition have excellent strength, chemical resistance, hue and transparency, and therefore can be suitably used in applications requiring high designability. Specifically, they can be suitably used for applications such as containers for cosmetics and miscellaneous goods such as stationery.< / haze>
Claims
1. A copolymer containing an aromatic vinyl monomer unit and a cyano monomer unit, wherein when P(UV) is a peak intensity detected at UV 254 nm within a peak half-width of a weight average molecular weight MwRI of the copolymer determined by a differential refractive index detector in gel permeation chromatography, and P(RI) is a peak intensity detected by the differential refractive index detector within a peak half-width of MwRI, the difference between the maximum and minimum values of P(UV) / P(RI) is 0.15 or less, A copolymer, wherein a plate-shaped molded product having a size of 127 x 127 x 3 mm in thickness is molded in an injection molding machine at a molding temperature of 230°C using pellets obtained from the copolymer in accordance with ASTM D-1003, and the haze of the molded product is measured using a haze meter and is 0.1 to 0.7%.
2. In accordance with JIS K-7111, a Charpy impact strength of 11.0 kJ / m was measured using an unnotched test piece made by an injection molding machine using pellets obtained from the copolymer, with the impact direction being edgewise, at a relative humidity of 50% and an ambient temperature of 23°C. 2 ~16.0 kJ / m 2 The copolymer according to claim 1 ,
3. The copolymer according to claim 1 or 2, comprising 50 to 90% by mass of the aromatic vinyl monomer units and 10 to 50% by mass of the cyano monomer units, where the total of the aromatic vinyl monomer units and the cyano monomer units is 100% by mass.
4. 4. The copolymer according to claim 1, wherein the aromatic vinyl monomer unit is a styrene monomer unit, and the cyano monomer unit is an acrylonitrile monomer unit.
5. A resin composition for injection molding, comprising the copolymer according to any one of claims 1 to 4.
6. A molded article molded from the resin composition for injection molding according to claim 5.
7. A method for producing a copolymer containing an aromatic vinyl monomer unit and a cyano monomer unit, comprising the steps of: feeding a feed solution containing an aromatic vinyl monomer and a cyano monomer to a liquid phase of the polymerization solution in the reactor; condensing the evaporated gas generated in the reaction vessel in a heat exchanger outside the reaction vessel and returning the obtained condensate to the liquid phase of the reaction vessel; Including, The method for producing a copolymer, wherein the feed liquid and the condensate are not supplied to a gas phase portion in the reaction vessel.
Citation Information
Patent Citations
ABS resin with rubber dispersion particle showing high solution viscosity and manufacture
JP1984080415A
Method for producing styrene-acrylonitrile copolymer
JP1993255448A
Production of acrylonitrile (Co)Polymer
JP1996231643A
Method and device for continuous production of polymer
JP1997012638A
Production of thermoplastic copolymer
JP1998152504A