Photoelectric conversion element and method for manufacturing photoelectric conversion layer

The integration of a laminated semiconductor structure with titanium oxide and chlorine in the n-type layer allows the photoelectric conversion element to store and discharge electricity, addressing the need for continuous light irradiation and reducing device size by incorporating a power storage function.

JP7591740B2Active Publication Date: 2024-11-29NATIONAL INSTITUTE OF TECHNOLOGY +1
View PDF 11 Cites 0 Cited by

Patent Information

Application Number
JP2023023245
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2023-02-17
Publication Date
2024-11-29
Estimated Expiration
2043-02-17

AI Technical Summary

Technical Problem

Conventional photoelectric conversion elements require continuous light irradiation to generate current, and connecting an external battery increases device size due to separate components.

Method used

A photoelectric conversion element with a laminated structure of p-type and n-type semiconductor layers, where the n-type semiconductor layer is made of titanium oxide and includes a titanium compound with chlorine, and a power storage function is integrated by storing electrons and holes within the photoelectric conversion layer.

Benefits of technology

The element can store electricity generated during light exposure and discharge it after light stops, maintaining current flow without external batteries, thus reducing device size and enhancing energy efficiency.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007591740000001
    Figure 0007591740000001
  • Figure 0007591740000002
    Figure 0007591740000002
  • Figure 0007591740000003
    Figure 0007591740000003
Patent Text Reader

Abstract

To provide a photoelectric conversion element with a power storage function.SOLUTION: A photoelectric conversion element according to the present invention comprises two electrodes, an n-type semiconductor material formed between the two electrodes, and a photoelectric conversion layer containing p-type semiconductor material including carbon allotropes with p-type semiconductor properties, and the region containing a carbon allotrope of the photoelectric conversion layer includes a power storage region for storing electricity generated in the photoelectric conversion layer. The carbon allotrope includes carbon nano-tubes and the region including the carbon nano-tubes includes the power storage region.SELECTED DRAWING: Figure 2
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a photoelectric conversion element and a method for producing a photoelectric conversion layer of the photoelectric conversion element. [Background technology]

[0002] In general, a photoelectric conversion element has a photoelectric conversion layer composed of a p-type semiconductor material and an n-type semiconductor material between an anode and a cathode (see, for example, Patent Document 1). When light is incident on the photoelectric conversion layer, excitons are generated and electrons and holes are generated. The electrons move to the cathode and the holes move to the anode, causing a current to flow in an external circuit connected to the photoelectric conversion element. When the irradiation of the photoelectric conversion layer with light is stopped, electrons and holes are not generated in the photoelectric conversion layer, so that a current does not flow to the external circuit. In other words, a conventional photoelectric conversion element could only pass a current while the irradiation of light to the photoelectric conversion element continues. For this reason, in order to continue supplying a current even after the irradiation of light to the photoelectric conversion element has stopped, an external battery is connected to the photoelectric conversion element, and after the irradiation of light to the photoelectric conversion element has stopped, a current is supplied from the external battery (see, for example, Patent Document 2). [Prior art documents] [Patent documents]

[0003] [Patent Document 1] Patent No. 6005785 [Patent Document 2] Patent Publication No. 2022-168820 Summary of the Invention [Problem to be solved by the invention]

[0004] However, when an external battery is connected to the photoelectric conversion element, the photoelectric conversion element and the external battery are separate, which results in an increase in the size of the device.

[0005] In view of the above circumstances, the present invention provides a photoelectric conversion element having a power storage function and a method for manufacturing the photoelectric conversion element. [Means for solving the problem]

[0006] The photoelectric conversion element of the present invention includes two electrodes and a photodiode formed between the two electrodes, and a photoelectric conversion layer in which a p-type semiconductor layer and an n-type semiconductor layer are laminated, the p-type semiconductor layer being made of carbon nanotubes having p-type semiconductor properties, and the n-type semiconductor layer being made of titanium oxide (TiO 2 The present invention is characterized in that the semiconductor device is made of an n-type semiconductor material including .

[0007] In addition, in the photoelectric conversion element of the present invention, The n-type semiconductor material is characterized by including a titanium compound containing chlorine.

[0008] In addition, in the photoelectric conversion element of the present invention, The photoelectric conversion layer has a function of storing electrons and holes generated in the photoelectric conversion layer. .

[0009] In the photoelectric conversion element of the present invention, the n-type semiconductor material contains a titanium compound containing chlorine.

[0010] In the photoelectric conversion element of the present invention, the photoelectric conversion layer has a laminated structure in which a p-type semiconductor layer containing the p-type semiconductor material and an n-type semiconductor layer containing the n-type semiconductor material are laminated.

[0011] In the photoelectric conversion element of the present invention, the photoelectric conversion layer has a bulk heterojunction structure.

[0012] Further, the method for producing a photoelectric conversion layer of the present invention is a method for producing a photoelectric conversion layer having a laminated structure in which a p-type semiconductor layer containing a p-type semiconductor material and an n-type semiconductor layer containing an n-type semiconductor material are laminated, comprising the steps of: The n-type semiconductor layer forming step includes an n-type semiconductor layer side film forming step of forming a film of a titanium tetrachloride aqueous solution containing titanium tetrachloride, and an n-type semiconductor layer side heating step of heating the film of the titanium tetrachloride aqueous solution formed in the n-type semiconductor layer side film forming step for a predetermined period of time to generate the n-type semiconductor layer. a p-type semiconductor layer forming step of forming the p-type semiconductor layer, wherein the laminated structure is formed by the n-type semiconductor layer forming step and the p-type semiconductor layer forming step, The photoelectric conversion layer has a function of storing electrons and holes generated in the photoelectric conversion layer. .

[0013] Furthermore, in the method for producing a photoelectric conversion layer of the present invention, the n-type semiconductor layer formation step includes an n-type semiconductor layer side film formation step of forming a film of a titanium tetrachloride aqueous solution containing titanium tetrachloride on a surface of an adjacent layer, and an n-type semiconductor layer side heating step of heating the film of the titanium tetrachloride aqueous solution formed in the n-type semiconductor layer side film formation step for a predetermined period of time to produce the n-type semiconductor layer, wherein the n-type semiconductor material containing at least titanium oxide (TiO2) having a crystalline structure is produced from the film in the n-type semiconductor layer side heating step, and the n-type semiconductor layer is produced.

[0014] In addition, the manufacturing method of the photoelectric conversion layer of the present invention includes a film formation process for forming a coating of a mixed solution containing a carbon allotrope having p-type semiconductor properties, and a heating process for heating the coating of the mixed solution formed in the film formation process to form a photoelectric conversion layer having a bulk heterojunction structure, wherein the heating process is characterized in that a storage region for storing electricity generated in the photoelectric conversion layer is formed in at least a part of the region containing the carbon allotrope of the photoelectric conversion layer.

[0015] In the method for producing a photoelectric conversion layer of the present invention, the mixed solution contains titanium tetrachloride, and in the heating step, an n-type semiconductor material containing at least titanium oxide (TiO2) having a crystalline structure is produced by heating the titanium tetrachloride.

[0016] In addition, the manufacturing method of the photoelectric conversion layer of the present invention includes a film formation process for forming a film of a mixed solution containing an n-type semiconductor material and a carbon allotrope having p-type semiconductor properties, and a heating process for heating the film of the mixed solution formed in the film formation process to form a photoelectric conversion layer with a bulk heterojunction structure, wherein the heating process is characterized in that a storage region for storing electricity generated in the photoelectric conversion layer is formed in at least a part of the region containing the carbon allotrope of the photoelectric conversion layer. Effect of the Invention

[0017] The photoelectric conversion element of the present invention can provide the excellent effect of storing electricity. [Brief description of the drawings]

[0018] [Figure 1] 1A is a schematic cross-sectional view of a photoelectric conversion element according to an embodiment of the present invention, and FIG. 1B is a schematic cross-sectional view of a modified example of the photoelectric conversion element according to an embodiment of the present invention. [Diagram 2] 1A is a schematic cross-sectional view of a photoelectric conversion layer of a photoelectric conversion element according to a first embodiment of the present invention, and FIG. 1B is a schematic cross-sectional view of a modified example of a power storage region of the photoelectric conversion layer of a photoelectric conversion element according to a first embodiment of the present invention. [Diagram 3] 1A is a SEM image of a junction (boundary) between an n-type semiconductor layer and a p-type semiconductor layer of a photoelectric conversion element according to a first embodiment of the present invention, observed with a scanning electron microscope (SEM) at a magnification of 100,000. 1B is a SEM image of a surface of a cathode of a photoelectric conversion element according to a first embodiment of the present invention, observed with a scanning electron microscope (SEM) at a magnification of 100,000. [Figure 4] 1A is an enlarged schematic cross-sectional view of a photoelectric conversion layer of a photoelectric conversion element according to a first embodiment of the present invention, showing a state in which the convex portions are fitted into the concave portions so that the entire convex surfaces of the convex portions and the entire concave surfaces of the concave portions are in contact with each other. FIG. 1B is an enlarged schematic cross-sectional view of a photoelectric conversion layer of a photoelectric conversion element according to a first embodiment of the present invention, showing a state in which the convex portions are fitted into the concave portions so that part of the convex surfaces of the convex portions and part of the concave surfaces of the concave portions are in contact with each other. [Diagram 5] 3 is a flowchart showing a flow of manufacturing the photoelectric conversion element (laminate structure) according to the first embodiment of the present invention. [Figure 6] Graph (A) shows the change in the current-voltage characteristic curve of the photoelectric conversion element of Example 1 of the present invention for each light irradiation time, and graph (B) shows the change in the current-voltage characteristic curve of the photoelectric conversion element of Example 1 of the present invention for each elapsed time after the end of light irradiation. [Figure 7] 4 is a current-voltage characteristic curve of a photoelectric conversion element of a comparative example in Example 1 of the present invention. [Figure 8]1A is a schematic cross-sectional view of a photoelectric conversion element (bulk heterojunction structure) according to a second embodiment of the present invention, and FIG. 1B is a schematic cross-sectional view of a modified example of the electricity storage region of the photoelectric conversion layer of the photoelectric conversion element according to the second embodiment of the present invention. [Figure 9] 10 is a flowchart showing a flow of manufacturing a photoelectric conversion element (bulk heterojunction structure) according to a second embodiment of the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0019] DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS Hereinafter, an embodiment of the present invention will be described with reference to the accompanying drawings. Figures 1 to 9 show an example of an embodiment of the present invention, and in the drawings, parts with the same reference numerals represent the same items.

[0020] <Overall configuration of photoelectric conversion element> A photoelectric conversion element 1 according to an embodiment of the present invention will be described with reference to Figs. 1 and 2. As shown in Fig. 1(A), the photoelectric conversion element 1 according to the embodiment of the present invention includes an anode (first electrode) 2, a cathode (second electrode) 3, and a photoelectric conversion layer 4. The photoelectric conversion element 1 is formed by stacking the cathode (second electrode) 3, the photoelectric conversion layer 4, and the anode (first electrode) 2 in this order on one surface of a substrate 5. The direction in which the layers of the photoelectric conversion element 1 are stacked is defined as the stacking direction K. The stacking direction K is parallel to the thickness direction of the photoelectric conversion layer 4.

[0021] In addition, the photoelectric conversion element 1 in this embodiment is assumed to be a thin-film photoelectric conversion element having a film thickness of, for example, about 5 to 50 (μm), but is not limited to this and may be a photoelectric conversion element having a film thickness in another range.

[0022] <Substrate> The substrate 5 is, for example, a plate-like member made of a transparent material having insulating properties. The substrate 5 may be made of a deformable material (for example, a material having flexibility), or may be made of a material that is not deformable. Specific examples of the material of the substrate 5 include glass such as borosilicate glass, white plate glass, and quartz glass, and insulating materials such as polyethylene terephthalate (PET), polyethylene naphthalate (PEN), polycarbonate (PC), and polyethersulfone (PES). The thickness of the substrate 5 is not particularly limited, but may be, for example, in the range of 100 μm to 100 mm.

[0023] <Anode (first electrode)> The anode 2 may be made of at least a material having electrical conductivity. Examples of materials constituting the anode 2 include conductive polymer compounds, metals such as platinum, gold, silver, copper, and aluminum, and mixtures of the above, but are not limited thereto, and may be made of other materials. Examples of conductive polymer compounds include PEDOT-PSS, but are not limited thereto, and may be polythiophene, polyaniline, polypyrrole, and derivatives thereof. PEDOT-PSS is an abbreviation for a composite of poly(3,4-ethylenedioxythiophene) (PEDOT), which is a substituted polythiophene containing ions to which a polyanion has been added, and which is made of polystyrene sulfonic acid (PSS).

[0024] The anode 2 may be a single layer or a laminate of multiple materials. The anode 2 may be made of a material having electrical conductivity and optical transparency. In this case, the anode 2 may be made of any of the materials for the cathode 3 described below.

[0025] <Cathode (second electrode)> The cathode 3 is preferably composed of a material having conductivity and light transmissivity. Examples of the material having light transmissivity include, for example, a transparent material. Specifically, examples of the material constituting the cathode 3 include conductive metal oxides such as tin-doped indium oxide (ITO), fluorine-doped tin oxide (FTO), antimony-doped tin oxide (ATO), aluminum-doped zinc oxide (AZO), and gallium-doped zinc oxide (GZO).

[0026] Further, the cathode 3 may be in a single layer or a mode in which a plurality of materials are laminated. Further, the cathode 3 may be composed of the material of the anode 2 described above.

[0027] <Photovoltaic conversion layer> The photovoltaic conversion layer 4 generates electrons and holes due to light incident from the outside. And the photovoltaic conversion layer 4 is formed between the anode 2 and the cathode 3. As shown in FIG. 1(A), when light is incident on the photovoltaic element 1, excitons are generated in the photovoltaic conversion layer 4, and electrons and holes are generated. Then, the electrons move to the cathode 3 side and the holes move to the anode 2 side. As a result, a current (photoexcitation current) flows through an external circuit (not shown) connected to the anode 2 and the cathode 3. The photovoltaic conversion layer 4 as described above contains a p-type semiconductor material and an n-type semiconductor material.

[0028] <p-type semiconductor material> The p-type semiconductor material in the photovoltaic conversion layer 4 includes a carbon allotrope having p-type semiconductor characteristics (hereinafter referred to as a p-type carbon allotrope). Examples of the p-type carbon allotrope include, for example, carbon nanotubes. The carbon nanotubes may be single-layer ones (single-walled carbon nanotubes) or multi-layer ones (multi-walled nanotubes).

[0029] In addition to the above p-type carbon allotropes, other electron-donating compounds may be included in the p-type semiconductor material in the photoelectric conversion layer 4. Examples of other electron-donating compounds include p-type organic semiconductor materials such as polyvinylcarbazole and its derivatives, polysilane and its derivatives, polysiloxane derivatives having aromatic amines in the side chain or main chain, polyaniline and its derivatives, polythiophene and its derivatives (e.g., P3HT (poly(3-hexylthiophene))), polypyrrole and its derivatives, polyphenylene vinylene and its derivatives, polythienylene vinylene and its derivatives, polyfluorene and its derivatives. When an unavoidable component that is inadvertently included during the process of providing a mixture with the above p-type carbon allotropes is contained, such a material is also included in the p-type semiconductor material.

[0030] <n-type semiconductor material> The n-type semiconductor material in the photoelectric conversion layer 4 is selected in consideration of the energy difference from the above p-type carbon allotropes. Examples of such n-type semiconductor materials include products formed when an aqueous solution of titanium tetrachloride at a predetermined concentration is heated and fired at a predetermined temperature for a predetermined time. The product contains titanium oxide (TiO2), but may further contain a precursor of titanium oxide (TiO2) and unavoidable impurities. Examples of the precursor of titanium oxide (TiO2) include TiO (2-X) (0 ≦ X < 2), and a titanium compound containing chlorine (TiCl Y O (Z-0.5Y) )(0 < Y < 4, 0 < Z ≦ 2, 0 < (Z - 0.5Y) ≦ 2) may be included. Incidentally, titanium oxide (TiO2) may also be referred to as titanium dioxide. Note that it is preferable that the ratio of titanium oxide (TiO2) in the above product is 95% or more and the ratio of the precursor of titanium oxide (TiO2) is 5% or less. Also, the ratio of titanium oxide (TiO2) in the above product may be 90% or more and the ratio of the precursor of titanium oxide (TiO2) may be 10% or less. Further, titanium oxide (TiO2) as the above product preferably has a crystal structure. Also, the precursor of titanium oxide (TiO2) preferably has a crystal structure.

[0031] The n-type semiconductor material in the photoelectric conversion layer 4 may be, for example, an oxide semiconductor (for example, zinc oxide) and other electron-accepting compounds, or a mixture of at least two of the above. Even in this case, if the product or the mixture contains an unavoidable component that is unintentionally contained in the process of providing the mixture, the material is also included in the n-type semiconductor material.

[0032] The output voltage of the photoelectric conversion element 1 is determined by the difference between the LUMO value of the n-type semiconductor material and the HOMO value of the p-type semiconductor material. Since the values ​​of LUMO and HOMO are band gap energies, if the band gap energy of the above product as the n-type semiconductor material is large, the LUMO of the n-type semiconductor material becomes large, making it possible to obtain a high output voltage.

[0033] <Photoelectric conversion layer structure> 2(A) and (B), the photoelectric conversion layer 4 in this embodiment has a laminated structure in which a p-type semiconductor layer 41 containing a p-type semiconductor material and an n-type semiconductor layer 42 containing an n-type semiconductor material are laminated in a lamination direction K (thickness direction of the photoelectric conversion layer 4). In the photoelectric conversion layer 4 having this laminated structure, the boundary surface where the p-type semiconductor layer 41 and the n-type semiconductor layer 42 contact each other becomes a pn junction interface 43. When light hits the pn junction interface 43, electrons and holes are generated there, and a current flows.

[0034] The region containing the p-type carbon allotrope as the p-type semiconductor material includes a storage region 44 that stores electricity generated in the photoelectric conversion layer 4. As shown in FIG. 2(A), the storage region 44 may extend over the entire region of the p-type semiconductor layer 41. As shown in FIG. 2(B), the storage region 44 may extend over a portion of the p-type semiconductor layer 41. In this case, a plurality of storage regions 44 may be formed in the p-type semiconductor layer 41 (see FIG. 2(B)), or only one storage region 44 may be formed. As shown in FIG. 2(B), the storage region 44 may extend across the p-type semiconductor layer 41 and the n-type semiconductor layer 42. The storage region 44 may extend over the entire regions of the p-type semiconductor layer 41 and the n-type semiconductor layer 42.

[0035] When the p-type carbon allotrope contains carbon nanotubes, the carbon nanotubes are preferably distributed in a fibrous, dispersed state in the region containing the carbon nanotubes.

[0036] As long as light irradiation continues, power generation continues, and power continues to be stored in the power storage area 44. When light irradiation stops, power generation stops, and electricity is discharged from the power storage area 44 over time.

[0037] 3(A) shows a SEM image of the junction surface 42A (see FIGS. 2(A) and (B)) of the n-type semiconductor layer 42 with the p-type semiconductor layer 41 observed at a magnification of 100,000 times using a scanning electron microscope (SEM). FIG. 3(B) shows a SEM image of the surface of the cathode 3 of the substrate 5 with the cathode 3 before the n-type semiconductor layer 42 is provided, observed at a magnification of 100,000 times using a scanning electron microscope (SEM). Comparing the SEM images of FIGS. 3(A) and (B), a plurality of granular white spots are uniformly distributed on the junction surface 42A of the n-type semiconductor layer 42. The granular white spots are convex portions 45 that are convex from the flat portion 42B of the surface of the n-type semiconductor layer 42 toward the p-type semiconductor layer 41 along the stacking direction K, as shown in FIG. 4(A). That is, when the junction surface 42A of the n-type semiconductor layer 42 with the p-type semiconductor layer 41 is observed from the side opposite to the junction surface 42A using a scanning electron microscope (SEM), a plurality of minute protrusions 45 are formed on the junction surface 42A of the n-type semiconductor layer 42 with the p-type semiconductor layer 41, which are displayed as white spots in the SEM image. In the region of the junction surface 42A of the n-type semiconductor layer 42 shown in the photograph of the SEM image in FIG. 3(A), the protrusions 45 (each white dot constituting the white spot) are distributed almost uniformly, but this is not limited thereto, and they may be distributed unevenly. Note that the plurality of protrusions 45 may include protrusions having various heights and widths, or may include protrusions having approximately the same height or width.

[0038] The p-type semiconductor layer 41 is bonded (contacted) to the n-type semiconductor layer 42 at a bonding surface 41A of the p-type semiconductor layer 41. The p-type semiconductor layer 41 has a recess 46 that fits (engages) with a protrusion 45 of the n-type semiconductor layer 42, as shown in FIG. 4(A). The p-type semiconductor layer 41 is engaged (contacted) with the n-type semiconductor layer 42 in a state in which the recess 46 fits into the protrusion 45 and covers the protrusion 45 (engaged state). In order to ensure a large contact area at the bonding surfaces 42A and 41A of the n-type semiconductor layer 42 and the p-type semiconductor layer 41, it is preferable to provide many regions where the recess 46 fits into the protrusion 45 so that the entire convex surface of the protrusion 45 and the entire concave surface of the recess 46 are in contact with each other, as shown in FIG. 4(A). In addition, as shown in Figure 4 (B), there may be an area where recess 46 fits into convex portion 45, with part of the convex surface of convex portion 45 and part of the concave surface of concave portion 46 in contact, and the remaining part of the convex surface of convex portion 45 and the remaining part of the concave surface of concave portion 46 not in contact.

[0039] When light strikes the pn junction interface 43 where the junction surfaces 41A and 42A are in contact, electrons and holes are generated there, causing a current to flow. Compared to the contact area of ​​the virtual n-type semiconductor layer and the virtual p-type semiconductor layer where the pn junction interface 43 is smooth, the contact area of ​​the junction surface 42A of the n-type semiconductor layer 42 and the junction surface 41A of the p-type semiconductor layer 41 in this embodiment is larger. Therefore, the photoelectric conversion element 1 in this embodiment generates a large amount of electrons and holes when struck by light. As a result, the photoelectric conversion element 1 in this embodiment has better current-voltage characteristics than a photoelectric conversion element having a virtual n-type semiconductor layer and a virtual p-type semiconductor layer.

[0040] In the present invention, the n-type semiconductor layer 42 does not necessarily have to have the protrusion 45. Such a structure is also within the scope of the present invention.

[0041] <Method of manufacturing photoelectric conversion element> Next, an example of a method for manufacturing the photoelectric conversion element 1 in this embodiment will be described with reference to FIG.

[0042] <Cathode formation process> First, a cathode 3 is formed on a substrate 5 (cathode formation step: step S100). Specifically, for example, a film of the material described in the above <cathode (second electrode)> is provided (cathode-side film formation step). More specifically, for example, the material described in the above <cathode (second electrode)> is made into a paste and printed on the substrate 5 by a printing apparatus to provide a film. Note that a film may be provided on the substrate 5 by a sputtering method, a vapor deposition method, or other film formation methods using the material described in the above <cathode (second electrode)>.

[0043] Then, an annealing process of heating the substrate 5 on which the film is formed at a predetermined temperature (for example, 130°C) for a predetermined time (for example, 10 minutes) is performed (cathode-side heating step). Thereby, the cathode 3 is formed on the substrate 5.

[0044] <n-type semiconductor layer formation step> Subsequently, an n-type semiconductor layer 42 is formed on the cathode 3 (n-type semiconductor layer formation step). Specifically, first, a film of an aqueous titanium tetrachloride solution is formed on the cathode 3 (n-type semiconductor layer-side film formation step: step S101). More specifically, for example, at least the cathode 3 side of the substrate 5 is immersed in an aqueous titanium tetrachloride solution diluted to a predetermined concentration for a predetermined time (for example, 10 minutes to 30 minutes). Thereby, a film of the aqueous titanium tetrachloride solution is formed on the cathode 3 side of the substrate 5. Note that the film of the aqueous titanium tetrachloride solution may be provided on the substrate 5 by a spin coating method, or may be provided by printing or other film formation methods.

[0045] <n-type semiconductor layer-side heating step> The substrate 5 on which the film of the aqueous titanium tetrachloride solution is formed is dried in an atmosphere at a predetermined temperature for a predetermined time. That is, the film of the aqueous titanium tetrachloride solution is heated to evaporate (remove) moisture from the film of the aqueous titanium tetrachloride solution (first heating step: step S102). Note that the first heating step may be regarded as a moisture removal step in the sense of evaporating (removing) moisture from the film of the aqueous titanium tetrachloride solution.

[0046] Incidentally, the predetermined temperature in the first heating step (moisture removal step) may be any temperature (boiling point of water) that can evaporate (remove) moisture from the coating of the titanium tetrachloride aqueous solution, and is preferably within the range of 70°C to 100°C, and more preferably within the range of 80°C to 90°C. In addition, the predetermined temperature in the first heating step (moisture removal step) may be constant for a predetermined time or may be changed. In addition, the predetermined time in the first heating step (moisture removal step) may be any time that can evaporate (remove) moisture from the coating of the titanium tetrachloride aqueous solution. In this step, the predetermined time is preferably about 60 minutes when the predetermined temperature is 80°C.

[0047] Furthermore, even if another heating step is performed between the first heating step and the second heating step (calcination step), if the moisture is evaporated (removed) from the coating of the titanium tetrachloride aqueous solution in that heating step, that heating step may also be considered to be included in the moisture removal step. In other words, the moisture removal step may be composed of a plurality of heating steps.

[0048] At a heating temperature of 200° C. or less, titanium oxide (TiO2) having a crystalline structure or a precursor of titanium oxide (TiO2) having a crystalline structure is hardly generated. In this state, the electron transport property is extremely low, so that the charge-separated electrons can hardly be transported to the electrode. On the other hand, titanium oxide (TiO2) having a crystalline structure has a high electron transport property. Therefore, in order to generate titanium oxide (TiO2) having a crystalline structure, at least the coating side of the substrate 5 that has been subjected to the first heating step (moisture removal step) is heated and baked at a predetermined temperature (e.g., 500° C.) for a predetermined time (e.g., 45 minutes) (second heating step (baking step): step S103). That is, the coating from which moisture has been removed on the substrate 5 is baked on the cathode 3 of the substrate 5. The second heating step may be regarded as a baking step, with the second heating step being taken as meaning that at least the coating side of the substrate 5 that has been subjected to the moisture removal step is heated and baked for a predetermined time.

[0049] During the firing process, the coating from which moisture has been removed undergoes a chemical reaction such as oxidation, and the predetermined product already described is generated on the cathode 3 of the substrate 5. Then, during the firing process, the predetermined product forms the n-type semiconductor layer 42, and at the same time, a plurality of protrusions 45 are formed on the bonding surface 42A of the n-type semiconductor layer 42. To repeat, the predetermined product contains titanium oxide (TiO2), and may contain a precursor of titanium oxide (TiO2) and unavoidable impurities depending on the firing conditions.

[0050] In addition, the predetermined temperature (baking temperature) in the second heating step (baking step) may be any temperature at which the coating from which moisture has been removed can be baked onto the substrate 5, and is preferably, for example, 450°C to 550°C. If the predetermined temperature (baking temperature) exceeds 450°C, titanium oxide (TiO2) and the precursor of titanium oxide (TiO2) will definitely have an anatase crystal structure, and if the predetermined temperature (baking temperature) exceeds 550°C, the resistivity of the cathode 3 may increase. Incidentally, it is presumed that if the predetermined temperature (baking temperature) is 500°C to 550°C, titanium oxide (TiO2) and the precursor of titanium oxide (TiO2) will include not only those with an anatase crystal structure but also those with a rutile crystal structure.

[0051] Furthermore, even if another heating step is performed after the second heating step, if the heating step is for baking the coating, the heating step may also be considered to be included in the baking step. In other words, the baking step may be composed of a plurality of heating steps.

[0052] For convenience of explanation, the first heating step (moisture removal step) and the second heating step (baking step) are collectively defined as the n-type semiconductor layer side heating step in this embodiment. The reason why the n-type semiconductor layer side heating step is divided into two steps is that if the first heating step (moisture removal step) is omitted and the second heating step (baking step) is performed, the n-type semiconductor layer 42 may crack due to thermal expansion due to heating at a high temperature, and this is to be avoided. By dividing the n-type semiconductor layer side heating step into two steps as in this embodiment, it is possible to provide an n-type semiconductor layer 42 that is free of cracks and has a plurality of fine protrusions 45 distributed on the bonding surface 42A. The titanium tetrachloride aqueous solution may further contain an electron-accepting compound, which is the n-type semiconductor material described above.

[0053] Furthermore, there may be an additional step having a different main purpose in providing the n-type semiconductor layer 42 before the first heating step (moisture removal step), between the first heating step (moisture removal step) and the second heating step (baking step), or after the second heating step (baking step). Although the additional step is not the main purpose, it may or may not ultimately achieve the purpose of the moisture removal step or the baking step. As in the manufacturing method of the photoelectric conversion element of this embodiment, if at least the first heating step and the second heating step are included, the n-type semiconductor layer 42 can be provided by performing moisture removal and baking.

[0054] In the conventional manufacturing method of a dye-sensitized photoelectric conversion element, the semiconductor layer (titanium oxide layer) is treated with an aqueous titanium tetrachloride solution in order to improve the bonding (necking) between semiconductor particles in the semiconductor layer (titanium oxide layer) that has already been provided. On the other hand, in the manufacturing method of a photoelectric conversion element in this embodiment, an existing semiconductor layer is not treated with an aqueous titanium tetrachloride solution, but the aqueous titanium tetrachloride solution is used as a main material to form the semiconductor layer (n-type semiconductor layer 42) itself. In other words, the two manufacturing methods are completely different, since the aqueous titanium tetrachloride solution is used in the improvement treatment of the semiconductor layer in one method (the conventional manufacturing method of a dye-sensitized photoelectric conversion element) and in the treatment of making the semiconductor layer itself in the other method (the manufacturing method of a photoelectric conversion element in this embodiment).

[0055] Furthermore, in the method for manufacturing a photoelectric conversion device according to the present embodiment, convex portions 45 are formed in the n-type semiconductor layer 42, thereby increasing the contact area between the n-type semiconductor layer 42 and the p-type semiconductor layer 41, and increasing the amounts of electrons and holes generated when light hits. That is, the method for manufacturing a photoelectric conversion device according to the present embodiment is premised on this laminated structure. On the other hand, a conventional dye-sensitized photoelectric conversion device generates electricity by causing electron transfer between a semiconductor layer and an electrolytic solution when light hits, which is completely different from the power generation principle in this laminated structure.

[0056] Note that if the n-type semiconductor layer 42 can be formed to have a plurality of convex portions 45 on the cathode 3 using an aqueous titanium tetrachloride solution diluted to a predetermined concentration, it may be provided by other processing methods.

[0057] Incidentally, although it is repetitive, the n-type semiconductor layer 42 may not have a plurality of convex portions 45. The n-type semiconductor material used in the n-type semiconductor formation step may be different from the above, and examples thereof include oxide semiconductors (for example, zinc oxide) and other electron-accepting compounds.

[0058] <p-type semiconductor layer formation step> Next, the p-type semiconductor layer 41 is formed on the n-type semiconductor layer 42 (p-type semiconductor layer forming step). Specifically, first, a film of a p-type semiconductor material is formed on the n-type semiconductor layer 42 (p-type semiconductor layer side film forming step: step S104). Note that, here, carbon nanotubes, which are p-type carbon allotropes, are used as the p-type semiconductor material. A carbon nanotube coating liquid in which carbon nanotubes are dispersed in a predetermined organic solvent is applied onto the n-type semiconductor layer 42, and a coating of the coating liquid is provided on the n-type semiconductor layer 42 by a spin coating method. Examples of the predetermined organic solvent include dimethyl sulfoxide (DMSO) and ethylene glycol. Note that, the coating of the carbon nanotube coating liquid may be provided by immersing at least the n-type semiconductor layer 42 side of the substrate 5 in the carbon nanotube coating liquid, as in the case of the n-type semiconductor layer side film forming step, or may be provided on the n-type semiconductor layer 42 by printing or other film forming methods.

[0059] Then, an annealing process is performed on the substrate 5 on which the carbon nanotube coating liquid film has been formed, at a predetermined temperature (e.g., 100° C.) for a predetermined time (e.g., 10 minutes) (p-type semiconductor layer side heating process: step S105). This completes the p-type semiconductor layer 41 laminated on the n-type semiconductor layer 42. When the p-type semiconductor layer 41 is formed, the electricity storage region 44 is also formed in the photoelectric conversion layer 4. The p-type semiconductor layer side heating process may be divided into two processes (a moisture removal process and a baking process) in the same manner as in the n-type semiconductor layer side heating process. In this case, the predetermined temperature (baking temperature) in the process corresponding to the moisture removal process may be the same as that in the n-type semiconductor layer side heating process.

[0060] Finally, the anode 2 is formed on the p-type semiconductor layer 41 (anode formation process: step S106). Specifically, first, a coating of the material described in the above <anode (first electrode)> is provided on the p-type semiconductor layer 41 (anode-side film formation process). More specifically, for example, the material described in the above <anode (first electrode)> is made into a paste form, and printed on the substrate 5 by a printing device to provide a coating. Note that the material described in the above <anode (first electrode)> may be used to provide a coating on the p-type semiconductor layer 41 by sputtering, vapor deposition, or other film formation methods.

[0061] Then, the substrate 5 on which the coating has been formed is subjected to an annealing treatment at a predetermined temperature (e.g., 130° C.) for a predetermined time (e.g., 10 minutes) (anode-side heating step). As a result, the anode 2 is formed on the p-type semiconductor layer 41. Through the above steps, the photoelectric conversion element 1 is completed. This photoelectric conversion element 1 is a thin film. Note that the order in the above method for manufacturing the photoelectric conversion element 1 may be reversed, and the anode 2 (anode formation step), p-type semiconductor layer 41 (p-type semiconductor layer formation step), n-type semiconductor layer 42 (n-type semiconductor layer formation step), and cathode 3 (cathode formation step) may be provided in this order.

[0062] <Modification> A modified example of the photoelectric conversion element 1 in this embodiment will be described with reference to Fig. 1(B). As shown in Fig. 1(B), the photoelectric conversion element 1 in this modification is obtained by adding an electron transport layer 6 and a hole transport layer 7 to the photoelectric conversion element 1 in this embodiment.

[0063] The electron transport layer 6 has a function of efficiently transporting electrons generated in the photoelectric conversion layer 4 to the cathode 3. The electron transport layer 6 is provided between the cathode 3 and the photoelectric conversion layer 4 (n-type semiconductor layer 42). The material constituting the electron transport layer 6 is not particularly limited, and examples thereof include titanium (IV) isopropoxide and n-type semiconductors having electron transport properties, such as fullerene and derivatives thereof.

[0064] The hole transport layer 7 has a function of efficiently transporting holes generated in the photoelectric conversion layer 4 to the anode 2. The hole transport layer 7 is preferably formed of a material having high hole mobility. The hole transport layer 7 is provided between the anode 2 and the photoelectric conversion layer 4 (p-type semiconductor layer 41). The material constituting the hole transport layer is not particularly limited, and examples thereof include low molecular weight compounds such as aromatic cyclic acid anhydrides typified by NTCDA, and high molecular weight compounds such as known conductive polymers typified by PEDOT-PSS and poly(3,4-ethylenedioxy)thiophene.

[0065] When the electron transport layer 6 and the hole transport layer 7 are provided in the photoelectric conversion element 1, the electron transport layer 6 and the hole transport layer 7 may be provided by stacking corresponding materials at corresponding positions using a film formation method including a sputtering method, a vapor deposition method, a spin coating method, a printing method, etc.

[0066] The photoelectric conversion element 1 in which only one of the electron transport layer 6 and the hole transport layer 7 is provided and the method for producing the photoelectric conversion element 1 are also included within the scope of the present invention. EXAMPLES

[0067] Next, the inventors of the present application created a photoelectric conversion element as an embodiment of the present invention and two types of photoelectric conversion elements as comparative examples, and conducted an experiment to evaluate the current-voltage characteristics. The photoelectric conversion element as this embodiment was formed by depositing a photoelectric conversion layer 4 and an anode 2 in this order on a glass substrate (manufactured by Asahi Glass) with FTO (fluorine-doped tin oxide transparent conductive film). The FTO portion of the glass substrate with FTO constitutes the cathode, and the glass substrate portion constitutes the substrate.

[0068] Next, an immersion solution is prepared by adjusting a titanium tetrachloride aqueous solution (manufactured by Osaka Titanium Technologies) to 40 mM (molar) using pure water as a solvent, and the glass substrate with FTO is immersed in the immersion solution for 10 minutes. The glass substrate with FTO is then placed in an atmosphere at 80°C for 60 minutes to evaporate (remove) the water in the immersion solution. The glass substrate with FTO is then baked at 500°C for 45 minutes. This completes an n-type semiconductor layer having multiple fine protrusions on the bonding surface. Incidentally, the SEM image in FIG. 3(A) is a photograph of the surface of the n-type semiconductor layer of the photoelectric conversion element in this embodiment.

[0069] Next, 1 (wt%) of carbon nanotubes (manufactured by Thomas Swan & Co. Ltd.) was mixed with pure water as a solvent to prepare a carbon nanotube solution. The carbon nanotube solution was then applied as a coating liquid onto the n-type semiconductor layer, and a coating of the coating liquid was formed on the n-type semiconductor layer by spin coating. The coating was then annealed at 100°C for 10 minutes. This resulted in the formation of a p-type semiconductor layer, completing the photoelectric conversion layer.

[0070] Next, an anode is screen-printed on the p-type semiconductor layer using a conductive paste (Clevios (registered trademark) S V3 Stab), and then an annealing process is performed by heating at 130° C. for 10 minutes. This completes the photoelectric conversion element of this embodiment.

[0071] The two types of photoelectric conversion elements as comparative examples differed from the photoelectric conversion element of this embodiment in the configuration of the p-type semiconductor layer, but the other layers were prepared in the same manner as the photoelectric conversion element of this embodiment.

[0072] The p-type semiconductor layer in the photoelectric conversion element as the first comparative example (hereinafter referred to as the first comparative photoelectric conversion element) was prepared as follows. A copper iodide (I) solution was prepared by adding 0.5 (wt%) copper iodide (I) (CuI) to N,N-dimethylformamide (DMF), and the copper iodide (I) solution was dropped onto a glass substrate with FTO, followed by spin coating at 2000 rpm for 30 seconds. The glass substrate with FTO was then baked at 100°C for 10 minutes. This completed the p-type semiconductor layer of the first comparative photoelectric conversion element.

[0073] The p-type semiconductor layer in the photoelectric conversion element as the second comparative example (second comparative photoelectric conversion element) is prepared as follows. A P3HT solution is prepared by adding 0.5 (wt%) P3HT (poly(3-hexylthiophene)) to chlorobenzene as a solvent, and the P3HT solution is dropped onto a glass substrate with FTO, followed by spin coating at 2000 rpm for 30 seconds. The glass substrate with FTO is then baked at 100°C for 10 minutes. This completes the p-type semiconductor layer of the second comparative photoelectric conversion element.

[0074] A solar simulator (XES-4051 manufactured by Minaeshi Electric Co., Ltd.) was used to measure the current-voltage characteristics of the photoelectric conversion element of this embodiment, the first comparative example photoelectric conversion element, and the second comparative example photoelectric conversion element thus fabricated. The resulting current-voltage characteristics of the photoelectric conversion element of this embodiment, the first comparative example photoelectric conversion element, and the second comparative example photoelectric conversion element are shown in Figures 6(A), (B), and 7.

[0075] As shown in FIG. 6(A), when comparing the current-voltage characteristics of the photoelectric conversion element of this embodiment at the time when light irradiation is started to the photoelectric conversion element of this embodiment and the current-voltage characteristics of the photoelectric conversion element of this embodiment at the time when 3 minutes have passed since the start of light irradiation, the output current of the latter increases more than that of the former as the voltage increases. On the other hand, as shown in FIG. 7, the current-voltage characteristics of the first comparative example photoelectric conversion element and the second comparative example photoelectric conversion element did not change according to the elapsed time from the start of light irradiation. From this, it can be said that it was confirmed that the photoelectric conversion element of this embodiment has a storage region, and electricity generated by light irradiation is stored in the storage region, but the first comparative example photoelectric conversion element and the second comparative example photoelectric conversion element do not have a storage region.

[0076] Furthermore, as shown in FIG. 6(A), the current-voltage characteristics of the photoelectric conversion element of this embodiment 5 or 10 minutes after the start of light irradiation are not significantly different from those 3 minutes after the start of light irradiation. Therefore, it can be inferred that the maximum storage capacity of the storage area of ​​the photoelectric conversion element of this embodiment is reached 3 minutes after the start of light irradiation.

[0077] In addition, as shown in Fig. 6(B), when the light irradiation is stopped after 10 minutes of light irradiation, the output current in the current-voltage characteristic of the photoelectric conversion element of this embodiment gradually decreases as time passes. This is presumably because the electricity stored in the storage region of the photoelectric conversion element of this embodiment is discharged. The graph shown in Fig. 6(B) also supports the fact that the photoelectric conversion element of this embodiment has a storage region.

[0078] The major difference between the photoelectric conversion element of this embodiment and the photoelectric conversion element of the first comparative example and the photoelectric conversion element of the second comparative example is the material of the p-type semiconductor layer. From the above experiments, it was confirmed that the photoelectric conversion element had a storage characteristic by using carbon nanotubes, which are carbon allotropes having p-type semiconductor properties, as the material of the p-type semiconductor layer of the photoelectric conversion element.

[0079] Second Embodiment With reference to FIG. 8, the photoelectric conversion element 1 in the second embodiment of the present invention will be described. As shown in FIG. 8, the photoelectric conversion element 1 in this embodiment has a bulk heterojunction structure (bulk heterojunction structure: the same applies below) in the photoelectric conversion layer 4. More specifically, the bulk heterojunction structure is composed of a mixture in which n-type semiconductor materials and p-type semiconductor materials are randomly mixed. In the bulk heterojunction structure in this embodiment, there are a plurality of p-type semiconductor regions 47 composed of p-type semiconductor materials and a plurality of n-type semiconductor regions 48 composed of n-type semiconductor materials. The p-type semiconductor regions 47 and the n-type semiconductor regions 48 are phase-separated and bonded not only in the thickness direction of the photoelectric conversion layer 4 but also in a direction perpendicular to the thickness direction of the photoelectric conversion layer 4 and / or in a direction inclined to the thickness direction of the photoelectric conversion layer 4. As a result, the bulk heterojunction structure has many pn junction interfaces throughout the entire layer compared to the stacked structure in the first embodiment. Therefore, many of the excitons generated by light absorption can reach the pn junction interface, and the efficiency of charge separation can be improved.

[0080] In this embodiment, the n-type semiconductor material includes one or more types of materials similar to those in the first embodiment. In this embodiment, the p-type semiconductor material includes a carbon allotrope having p-type semiconductor properties. The carbon allotrope is preferably a carbon nanotube. The p-type semiconductor material may include one or more types of p-type semiconductor materials different from the carbon allotrope having p-type semiconductor properties. The region of the photoelectric conversion layer 4 that includes the carbon allotrope having p-type semiconductor properties includes the electricity storage region 44. The electricity storage region 44 may extend over the entire region of each p-type semiconductor region 47 as shown in FIG. 8(A). Also, as shown in FIG. 8(B), the electricity storage region 44 may extend over a part of each p-type semiconductor region 47. In this case, the electricity storage region 44 may be formed in each p-type semiconductor region 47 in a plurality of regions (see FIG. 9(B)), or only one may be formed. Also, as shown in FIG. 8(B), the electricity storage region 44 may straddle the p-type semiconductor region 47 and the n-type semiconductor region 48. The electricity storage region 44 may extend over the entire regions of each p-type semiconductor region 47 and each n-type semiconductor region 48. Similarly to the first embodiment, the photoelectric conversion element 1 of this embodiment may also have both or one of the electron transport layer 6 and the hole transport layer 7 provided adjacent to the photoelectric conversion layer 4 (see FIG. 1(B)).

[0081] Next, an example of a method for manufacturing the photoelectric conversion element 1 in this embodiment will be described with reference to Fig. 9. As shown in Fig. 9, in the method for manufacturing the photoelectric conversion element 1 in this embodiment, the cathode forming step (step S100), the heating step, and the anode forming step (step S106) are similar to those in the first embodiment, and therefore the same descriptions can be applied as much as possible.

[0082] When the photoelectric conversion layer 4 has a bulk heterojunction structure, in the photoelectric conversion layer formation step (step S107) for providing the photoelectric conversion layer 4, a coating of a mixed solution containing a p-type carbon allotrope (e.g., carbon nanotubes) and an n-type semiconductor material may be formed on an adjacent layer (e.g., the cathode 3 or the anode 2) (film formation step). Also, a coating of a mixed solution containing a p-type carbon allotrope and titanium tetrachloride may be formed on an adjacent layer (e.g., the cathode 3 or the anode 2). The above mixed solution may further contain different types of p-type semiconductor materials and n-type semiconductor materials. That is, the above mixed solution may contain one or more types of p-type semiconductor materials and n-type semiconductor materials. Then, the next heating step may be divided into two steps, for example, as shown in FIG. 9, similar to the first heating step (step S102: moisture removal step) and the second heating step (step S103: baking step) in the first embodiment, or the moisture removal step and the baking step may be performed in one step. However, the predetermined temperature (baking temperature) in the step corresponding to the baking step is preferably determined from the viewpoint of preventing an increase in the resistivity of the crystal structure and other parts in the n-type semiconductor material and the p-type semiconductor material. In addition, in the mixed solution containing the p-type carbon allotrope and titanium tetrachloride, titanium oxide (TiO2) or a precursor of titanium oxide (TiO2) is generated after the above heating step. Titanium oxide (TiO2) and precursors of titanium oxide (TiO2) include those having a crystal structure. Therefore, the n-type semiconductor material of the n-type semiconductor region 48 of the photoelectric conversion layer 4 in this embodiment includes titanium oxide (TiO2). In any case, the substrate with the cathode 3 on which the above coating is formed in the heating step is annealed, and the photoelectric conversion layer 4 of a bulk heterojunction structure is completed on the adjacent layer (for example, the cathode 3 or the anode 2). The order in the above manufacturing method of the photoelectric conversion element 1 may be reversed, and the anode 2 (anode formation step), the photoelectric conversion layer 4 (photoelectric conversion layer formation step), and the cathode 3 (cathode formation step) may be provided in this order. Furthermore, when both or one of the electron transport layer 6 and the hole transport layer 7 are provided adjacent to the photoelectric conversion layer 4 in the photoelectric conversion element 1 of this embodiment, they are provided by the same manufacturing method as in the first embodiment.

[0083] Incidentally, the photoelectric conversion element of the present invention and the method for manufacturing the photoelectric conversion element are not limited to the above-described embodiments, and it goes without saying that various modifications can be made within the scope that does not deviate from the gist of the present invention. [Explanation of symbols]

[0084] 1 Photoelectric conversion element 2 Anode (first electrode) 3 Cathode (second electrode) 4 Photoelectric conversion layer 5 Substrate 6 Electron transport layer 7 Hole transport layer 41 n-type semiconductor layer 41A n-type semiconductor layer junction 42 p-type semiconductor layer 42A p-type semiconductor layer junction 43 pn junction interface 44 Energy storage area 45 Convex 46 Recess 47 p-type semiconductor region 48 n-type semiconductor region

Claims

1. Two electrodes; a photoelectric conversion layer formed between the two electrodes and including a p-type semiconductor layer and an n-type semiconductor layer; Equipped with the p-type semiconductor layer is made of carbon nanotubes having p-type semiconductor properties; The n-type semiconductor layer is made of titanium oxide (TiO 2 ) n-type semiconductor material, The photoelectric conversion layer has a storage function of storing electrons and holes generated in the photoelectric conversion layer. Photoelectric conversion element.

2. The n-type semiconductor material includes a titanium compound containing chlorine. The photoelectric conversion element according to claim 1 .

3. A method for producing a photoelectric conversion layer having a laminated structure in which a p-type semiconductor layer containing a p-type semiconductor material and an n-type semiconductor layer containing an n-type semiconductor material are laminated, comprising the steps of: a film-forming step of forming a film of an aqueous titanium tetrachloride solution containing titanium tetrachloride on an n-type semiconductor layer side; an n-type semiconductor layer side heating step of heating the film of the titanium tetrachloride aqueous solution formed in the n-type semiconductor layer side film forming step for a predetermined period of time to form the n-type semiconductor layer; The n-type semiconductor layer forming step, a p-type semiconductor layer forming step of forming the p-type semiconductor layer using a liquid in which carbon nanotubes having p-type semiconductor characteristics are dispersed; Equipped with the laminated structure is formed by the n-type semiconductor layer forming step and the p-type semiconductor layer forming step, The photoelectric conversion layer has a storage function of storing electrons and holes generated in the photoelectric conversion layer. A method for producing a photoelectric conversion layer.

Citation Information

Patent Citations

  • Self-driven broadband photoelectric detector based on nanotube composite structure

    CN113299834A

  • Prescribed position stop control system of synchronous motor

    JP1985005785A

  • Optical sensor and its manufacturing method

    JP2006190729A

  • Organic photoelectric conversion element and solar cell using the same

    JP2013254912A

  • Organic layer-containing all solid solar cell

    JP2014192480A