Polycarbonate resin composition and method for producing polycarbonate resin composition

A balanced polycarbonate resin composition with aromatic polycarbonate, polyester, and epoxy-containing polymers addresses hydrolysis and impact resistance, enhancing molded article performance.

JP7591877B2Active Publication Date: 2024-11-29SUMITOMO CHEM CO LTD
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
JP2020111769
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2020-06-29
Publication Date
2024-11-29
Estimated Expiration
2040-06-29

AI Technical Summary

Technical Problem

Polycarbonate resin compositions lack hydrolysis resistance and have an imbalance between rigidity and impact resistance, leading to issues with surface peeling in molded articles.

Method used

A polycarbonate resin composition comprising aromatic polycarbonate, polyester, a polymer with epoxy groups, and a copolymer derived from a conjugated diene and aromatic vinyl hydrocarbon, with specific mass content ratios, is produced through melt-kneading and mixing to achieve a balanced blend.

Benefits of technology

The composition exhibits hydrolysis resistance, excellent rigidity and impact resistance, and reduces surface peeling in molded articles.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007591877000001
    Figure 0007591877000001
  • Figure 0007591877000002
    Figure 0007591877000002
  • Figure 0007591877000003
    Figure 0007591877000003
Patent Text Reader

Abstract

To provide a polycarbonate resin composition capable of forming a molding which has hydrolysis resistance, an excellent balance between rigidity and impact resistance, and high surface impact strength and causes less surface layer peeling, and a method for producing the same.SOLUTION: The polycarbonate resin composition contains (a) an aromatic polycarbonate, (b) a polyester, (c) a polymer having an epoxy group, and (d) a copolymer having a monomer unit derived from a conjugated diene and a monomer unit derived from an aromatic vinyl hydrocarbon. The content of the polyester is 9.0 mass% or less based on the total amount of the aromatic polycarbonate, the polyester, the polymer having an epoxy group, and the copolymer.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a polycarbonate resin composition and a method for producing a polycarbonate resin composition. [Background technology]

[0002] In order to improve the impact resistance of a resin composition containing an aromatic polycarbonate, for example, a copolymer mainly composed of an α-olefin and a glycidyl ester of an α,β-unsaturated acid is sometimes blended into the resin composition (for example, Patent Document 1). [Prior art documents] [Patent documents]

[0003] [Patent Document 1] Patent No. 2893185 Summary of the Invention [Problem to be solved by the invention]

[0004] Polycarbonate resin compositions containing aromatic polycarbonates as a main component may have insufficient hydrolysis resistance, and it is desirable for the polycarbonate resin composition to have an improved balance between rigidity and impact resistance, so as to form molded articles having high dart impact strength and little surface peeling.

[0005] An object of one aspect of the present invention is to provide a polycarbonate resin composition capable of forming a molded article that has hydrolysis resistance, an excellent balance between rigidity and impact resistance, high dart impact strength, and little surface peeling, and a production method thereof. [Means for solving the problem]

[0006] One aspect of the present invention provides a polycarbonate resin composition containing (a) an aromatic polycarbonate, (b) a polyester, (c) a polymer having an epoxy group, and (d) a copolymer having a monomer unit derived from a conjugated diene and a monomer unit derived from an aromatic vinyl hydrocarbon, wherein the content of the polyester is 9.0 mass% or less based on the total amount of the aromatic polycarbonate, the polyester, the polymer having an epoxy group, and the copolymer.

[0007] Another aspect of the present invention provides a method for producing a polycarbonate resin composition, comprising the steps of melt-kneading (b) a polyester, (c) a polymer having an epoxy group, and (d) a copolymer having a monomer unit derived from a conjugated diene and a monomer unit derived from an aromatic vinyl hydrocarbon to obtain a mixture, and kneading the mixture with (a) an aromatic polycarbonate to prepare a polycarbonate resin composition, wherein the content of the polyester is 9.0 mass% based on the total amount of the aromatic polycarbonate, the polyester, the polymer having an epoxy group, and the copolymer. Effect of the Invention

[0008] The present invention can provide a polycarbonate resin composition capable of forming a molded article that has hydrolysis resistance, an excellent balance between rigidity and impact resistance, high dart impact strength, and little surface peeling, and a production method thereof. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0009] Hereinafter, several embodiments of the present invention will be described in detail, however, the present invention is not limited to the following embodiments.

[0010] [Polycarbonate resin composition] The polycarbonate resin composition according to one embodiment contains (a) an aromatic polycarbonate (hereinafter sometimes referred to as "component (a)"), (b) a polyester (hereinafter sometimes referred to as "component (b)"), (c) a polymer having an epoxy group (hereinafter sometimes referred to as "component (c)"), and (d) a copolymer having a monomer unit derived from a conjugated diene and a monomer unit derived from an aromatic vinyl hydrocarbon (hereinafter sometimes referred to as "component (d)"). The content of the polyester in the polycarbonate resin composition is 9.0 mass% or less based on the total amount of components (a), (b), (c), and (d).

[0011] The polycarbonate resin composition according to the present embodiment contains the components (a), (b), (c), and (d) as essential components, and by setting the content of the component (b) within a specific range, it is possible to form a molded article that has hydrolysis resistance, an excellent balance between rigidity and impact resistance, high dart impact strength, and little surface peeling.

[0012] The tensile modulus of elasticity of a molded article formed from the polycarbonate resin composition may be, for example, 1500 MPa or more, 1800 MPa or more, or 2000 MPa or more at 23° C. The upper limit of the tensile modulus of elasticity may be, for example, 2800 MPa or less.

[0013] Hereinafter, each component constituting the polycarbonate resin composition will be described in detail.

[0014] (Component (a)) The polycarbonate resin composition contains (a) an aromatic polycarbonate as a main component. From the viewpoint of maintaining the rigidity of the polycarbonate resin composition, the content of the aromatic polycarbonate may be 75 mass% or more, 80 mass% or more, or 85 mass% or more based on the total amount of the (a) component, the (b) component, the (c) component, and the (d) component. From the viewpoint of improving the impact resistance of the polycarbonate resin composition, the content of the aromatic polycarbonate may be 98 mass% or less, 95 mass% or less, or 93 mass% or less.

[0015] Aromatic polycarbonates are polymers, which may be linear or branched, that contain monomer units derived from aromatic dihydroxy compounds and carbonyl groups. Aromatic polycarbonates are generally produced by the polymerization reaction of aromatic dihydroxy compounds with carbonyl chloride (phosgene), carbonic acid diesters (e.g., dimethyl carbonate, diphenyl carbonate), or carbon monoxide or carbon dioxide.

[0016] The aromatic dihydroxy compound constituting the aromatic polycarbonate may be, for example, a bis(hydroxyaryl)alkane, a bis(hydroxyaryl)cycloalkane, a cardo structure-containing bisphenol, a dihydroxydiaryl ether, a dihydroxydiaryl sulfide, a dihydroxydiaryl sulfoxide, a dihydroxydiaryl sulfone, 4,4′-dihydroxydiphenyl, hydroquinone, resorcinol, or a combination thereof.

[0017] Examples of bis(hydroxyaryl)alkanes include 2,2-bis(4-hydroxyphenyl)propane, 2,2-bis(3,5-dibromo-4-hydroxyphenyl)propane, bis(4-hydroxyphenyl)methane, 1,1-bis(4-hydroxyphenyl)ethane, 2,2-bis(4-hydroxyphenyl)butane, 2,2-bis(4-hydroxyphenyl)octane, 2,2-bis(4-hydroxy-3-methylphenyl)propane, 1,1-bis(3-tert-butyl-4-hydroxyphenyl)propane, 2,2-bis(4-hydroxy-3,5-dimethylphenyl)propane, 2,2-bis(3-bromo-4-hydroxyphenyl)propane, 2,2-bis(3,5-dichloro-4-hydroxyphenyl)propane, 2,2-bis(3 1,1-bis(4-hydroxyphenyl)propane, 2,2-bis(3-cyclohexyl-4-hydroxyphenyl)propane, 1,1-bis(4-hydroxyphenyl)-1-phenylethane, bis(4-hydroxyphenyl)diphenylmethane, 2,2-bis(4-hydroxyphenyl)-1,1,1-trichloropropane, 2,2-bis(4-hydroxyphenyl)-1,1,1,3,3,3-hexachloropropane, 2,2-bis(4-hydroxyphenyl)-1,1,1,3,3,3-hexafluoropropane, 1,1-bis(4-hydroxy-3-tert-butylphenyl)propane, 2,2-bis(4-hydroxy-3-bromophenyl)propane, and 2,2-bis(4-hydroxy-3,5-dibromophenyl)propane. 2,2-bis(4-hydroxyphenyl)propane and 2,2-bis(3,5-dibromo-4-hydroxyphenyl)propane are sometimes called bisphenol A and tetrabromobisphenol A, respectively.

[0018] Examples of bis(hydroxyaryl)cycloalkanes include 1,1-bis(4-hydroxyphenyl)cyclopentane, 1,1-bis(4-hydroxyphenyl)cyclohexane, and 1,1-bis(4-hydroxyphenyl)-3,3,5-trimethylcyclohexane.

[0019] Examples of cardo structure-containing bisphenols include 9,9-bis(4-hydroxyphenyl)fluorene and 9,9-bis(4-hydroxy-3-methylphenyl)fluorene.

[0020] Examples of dihydroxydiaryl ethers include 4,4'-dihydroxydiphenyl ether and 4,4'-dihydroxy-3,3'-dimethyldiphenyl ether.

[0021] Examples of dihydroxydiaryl sulfides include 4,4'-dihydroxydiphenyl sulfide and 4,4'-dihydroxy-3,3'-dimethyldiphenyl sulfide.

[0022] Examples of dihydroxydiaryl sulfoxides include 4,4'-dihydroxydiphenyl sulfoxide, and 4,4'-dihydroxy-3,3'-dimethyldiphenyl sulfoxide.

[0023] Examples of dihydroxydiarylsulfones include 4,4'-dihydroxydiphenylsulfone and 4,4'-dihydroxy-3,3'-dimethyldiphenylsulfone.

[0024] The aromatic polycarbonate may contain monomer units derived from one or more aromatic dihydroxy compounds selected from these. The aromatic polycarbonate may particularly contain monomer units derived from 2,2-bis(4-hydroxyphenyl)propane.

[0025] The branched aromatic polycarbonates contain monomer units derived from polyhydroxy compounds such as, for example, phloroglysine, 2,6-dimethyl-2,4,6-tris(4-hydroxyphenyl)-3-heptene, 4,6-dimethyl-2,4,6-tris(4-hydroxyphenyl)-2-heptene, 1,3,5-tris(2-hydroxyphenyl)benzene, 1,1,1-tris(4-hydroxyphenyl)ethane, 2,6-bis(2-hydroxy-5-methylbenzyl)-4-methylphenol, and α,α′,α″-tris(4-hydroxyphenyl)-1,3,5-triisopropylbenzene, or 3,3-bis(4-hydroxyaryl)oxindole (isatin bisphenol), 5-chloruisatin bisphenol, 5,7-dichloruisatin bisphenol, or 5-bromoisatin bisphenol.

[0026] The viscosity average molecular weight of the aromatic polycarbonate may be 10000 to 100000, 14000 to 50000, or 16000 to 30000. The viscosity average molecular weight here is a converted value from the melt viscosity measured at a temperature of 20° C. using methylene chloride as a solvent.

[0027] The aromatic polycarbonate can be synthesized by a conventional method such as an interfacial polymerization method, a pyridine method, an ester exchange method, etc. Commercially available aromatic polycarbonates can also be used.

[0028] ((b) component) The content of the (b) polyester in the polycarbonate resin composition is 9.0 mass% or less, and may be less than 8.0 mass%, less than 5.0 mass%, or less than 4.0 mass% based on the total amount of the (a), (b), (c), and (d) components from the viewpoint of improving the hydrolysis resistance of the polycarbonate resin composition. The content of the (b) polyester may be 0.1 mass% or more, 0.3 mass% or more, 0.5 mass% or more, or 0.8 mass% or more from the viewpoint of reducing surface peeling and improving dart impact strength of the molded article.

[0029] (b) The polyester may be, in particular, an aromatic polyester which is a condensation polymer of an aromatic dicarboxylic acid and a saturated dihydric alcohol. Examples of aromatic polyesters include polyethylene terephthalate, polypropylene terephthalate, polytetramethylene terephthalate (also called "polybutylene terephthalate"), polyhexamethylene terephthalate, polycyclohexane-1,4-dimethylol terephthalate, and polyneopentyl terephthalate.

[0030] (b) The polyester may contain polybutylene terephthalate, polyethylene terephthalate, or a combination thereof, preferably polybutylene terephthalate, from the viewpoint of further enhancing the hydrolysis resistance of the polycarbonate resin composition. Polybutylene terephthalate may further contain a monomer unit derived from an aromatic dicarboxylic acid other than terephthalic acid, and examples thereof include polybutylene (terephthalate / adipate), polybutylene (terephthalate / sebacate), polybutylene (terephthalate / decanedicarboxylate), polybutylene (terephthalate / naphthalate), and poly(butylene / ethylene) terephthalate. Polyethylene terephthalate may further contain monomer units derived from aromatic dicarboxylic acids other than terephthalic acid, examples of which include polyethylene(terephthalate / adipate), polyethylene(terephthalate / sebacate), polyethylene(terephthalate / decanedicarboxylate), polyethylene(terephthalate / naphthalate), and poly(butylene / ethylene) terephthalate.

[0031] The intrinsic viscosity of the polyester may be 0.50 to 2.00 dl / g, 0.60 to 1.90 dl / g, or 0.80 to 1.80 dl / g. The intrinsic viscosity here is a value determined by measuring the viscosity of a solution in which the polyester is dissolved in a mixed solvent of phenol and tetrachloroethane (mass ratio 5:5) at 30°C.

[0032] The polyester can be synthesized, for example, by a conventional polymerization method using an aromatic dicarboxylic acid and a saturated dihydric alcohol. Commercially available polyesters can also be used.

[0033] ((c) component) (c) The polymer having an epoxy group is generally a thermoplastic resin, and may be, for example, a copolymer containing a monomer unit derived from a monomer having an epoxy group. Examples of the monomer having an epoxy group include α,β-unsaturated carboxylic acid glycidyl ester and glycidyl ether having an unsaturated group.

[0034] The unsaturated carboxylic acid glycidyl ester may be a compound represented by the following formula (1): 1 represents an alkenyl group having 2 to 18 carbon atoms which may have one or more substituents. Examples of the compound represented by formula (1) include glycidyl acrylate, glycidyl methacrylate, and glycidyl itaconic acid ester. [ka]

[0035] The glycidyl ether having an unsaturated group may be a compound represented by the following formula (2): 2 represents an alkenyl group having 2 to 18 carbon atoms which may have one or more substituents, and X is CH2-O (CH2 is R 2 ) or an oxygen atom. Examples of the compound represented by formula (2) include allyl glycidyl ether, 2-methylallyl glycidyl ether, and styrene-p-glycidyl ether. [ka]

[0036] The copolymerization monomer copolymerized with the monomer having an epoxy group may be, for example, ethylene, an α-olefin, styrene, acrylonitrile, an unsaturated carboxylic acid ester (ethyl acrylate, methyl methacrylate, butyl acrylate, etc.), acrylic acid, an unsaturated vinyl ester (vinyl acetate, vinyl propionate, etc.), or a combination thereof.

[0037] The polymer having an epoxy group may be an olefin copolymer containing a monomer unit having an epoxy group and a monomer unit derived from ethylene or an α-olefin (such as propylene). The proportion of the monomer units derived from ethylene or an α-olefin (the total proportion of the monomer units derived from ethylene and the monomer units derived from an α-olefin) may be 50 to 99.9% by mass based on the mass of the polymer having an epoxy group.

[0038] Examples of olefin copolymers having epoxy groups include ethylene-glycidyl (meth)acrylate copolymers, ethylene-glycidyl (meth)acrylate-methyl (meth)acrylate copolymers, ethylene-glycidyl (meth)acrylate-ethyl (meth)acrylate copolymers, ethylene-glycidyl (meth)acrylate-normal propyl (meth)acrylate copolymers, ethylene-glycidyl (meth)acrylate-isopropyl (meth)acrylate copolymers, ethylene-glycidyl (meth)acrylate-normal butyl (meth)acrylate copolymers, ethylene-glycidyl (meth)acrylate-isobutyl (meth)acrylate copolymers, ethylene-glycidyl (meth)acrylate-2-ethylhexyl (meth)acrylate copolymers, and ethylene-glycidyl (meth)acrylate-vinyl acetate copolymers. The (c) component preferably contains an ethylene-glycidyl (meth)acrylate copolymer. An example of a commercially available ethylene-glycidyl (meth)acrylate copolymer is "Bondfast" (product name) manufactured by Sumitomo Chemical.

[0039] Other examples of copolymers containing a monomer unit having an epoxy group include a glycidyl methacrylate-styrene copolymer, a glycidyl methacrylate-acrylonitrile-styrene copolymer, and a glycidyl methacrylate-propylene copolymer.

[0040] The polymer having an epoxy group may have a polymer chain made of polyethylene, polypropylene, polystyrene, ethylene-α-olefin copolymer, or a hydrogenated or non-hydrogenated styrene-conjugated diene polymer, and a graft chain containing a monomer having an epoxy group bonded to the polymer chain. The monomer having an epoxy group can be graft polymerized by, for example, solution or melt kneading.

[0041] The proportion of the monomer unit having an epoxy group in the polymer having an epoxy group may be 0.1 mass% or more, 0.5 mass% or more, 1 mass% or more, or 3 mass% or more based on the mass of the polymer having an epoxy group. The proportion of the monomer unit having an epoxy group may be 30 mass% or less, 20 mass% or less, 15 mass% or less, or 10 mass% or less, or more than 6 mass%, based on the mass of the polymer having an epoxy group. When the proportion of the monomer unit having an epoxy group is high, the hydrolysis resistance of the polycarbonate resin composition and the molded article tends to be further improved.

[0042] Examples of a method for producing a polymer having an epoxy group include a method of copolymerizing a monomer having an epoxy group with another monomer by a high-pressure radical polymerization method, a solution polymerization method, an emulsion polymerization method, etc., and a method of graft polymerizing a monomer having an epoxy group onto an ethylene-based polymer or the like.

[0043] From the viewpoint of further improving the hydrolysis resistance of the polycarbonate resin composition, the content of the component (c) in the polycarbonate resin composition may be 0.1 part by mass or more, 0.5 part by mass or more, or 1 part by mass or more, and may be 20 parts by mass or less, 15 parts by mass or less, or 10 parts by mass or less, relative to 100 parts by mass of the component (a).

[0044] ((d) component) The polycarbonate resin composition contains, as component (d), a copolymer having monomer units derived from a conjugated diene and monomer units derived from an aromatic vinyl hydrocarbon, from the viewpoint of increasing the dart impact strength of a molded article and reducing surface peeling. The copolymer may be a hydrogenated copolymer. Component (d) is a copolymer having no epoxy groups and is different from component (c).

[0045] Examples of conjugated dienes include 1,3-butadiene, isoprene, 1,3-pentadiene, 2,3-dimethyl-1,3-butadiene, 3-butyl-1,3-octadiene, and 1,3-hexadiene. The conjugated diene compound is preferably 1,3-butadiene. Examples of aromatic vinyl hydrocarbons include styrene, α-methylstyrene, tert-butylstyrene, vinyltoluene, vinylnaphthalene, divinylbenzene, trivinylbenzene, and divinylnaphthalene. The aromatic vinyl hydrocarbon is preferably styrene.

[0046] Component (d) may further comprise a monomer based on a monomer selected from the group consisting of α-olefins, vinyl esters, unsaturated carboxylic acid esters, cyclic olefins, and vinyl cyanide compounds.

[0047] Examples of α-olefins include propylene, butene-1, pentene-1, hexene-1, heptene-1, octene-1, nonene-1, decene-1, undecene-1, dodecene-1, tridecene-1, tetradecene-1, pentadecene-1, hexadecene-1, heptadecene-1, octadecene-1, nonadecene-1, eicosene-1, 3-methyl-1-butene, 3-methyl-1-pentene, 3-ethyl-1-pentene, 4-methyl-1-pentene, 4-methyl-1-hexene, 4,4-dimethyl-1-hexene, 4,4-dimethyl-1-pentene, 4-ethyl-1-hexene, 3-ethyl-1-hexene, 9-methyl-1-decene, 11-methyl-1-dodecene, and 12-ethyl-1-tetradecene. Examples of vinyl esters include vinyl acetate and vinyl propionate. Examples of unsaturated carboxylic acid esters include methyl acrylate, ethyl acrylate, methyl methacrylate, and ethyl methacrylate. Examples of cyclic olefins include 2-norbornene and 5-methyl-2-norbornene. Examples of vinyl cyanide compounds include acrylonitrile and methacrylonitrile.

[0048] From the viewpoint of further increasing the dart impact strength of the molded article, the component (d) preferably contains a copolymer or a hydrogenated copolymer of a conjugated diene and an aromatic vinyl hydrocarbon, and more preferably contains a hydrogenated copolymer of a conjugated diene and an aromatic vinyl hydrocarbon. That is, the component (d) may contain a copolymer having only monomer units derived from a conjugated diene and monomer units derived from an aromatic vinyl hydrocarbon, or a hydrogenated polymer obtained by hydrogenating the copolymer. Examples of the hydrogenated copolymer include a hydrogenated styrene-butadiene-styrene copolymer and a hydrogenated styrene-isoprene-styrene copolymer.

[0049] From the viewpoint of the balance between rigidity and impact resistance, the content of the (d) component may be 1 part by mass or more, 2 parts by mass or more, or 3 parts by mass or more, and may be 30 parts by mass or less, 20 parts by mass or less, or 10 parts by mass or less, per 100 parts by mass of the (a) component.

[0050] The copolymer of a conjugated diene and an aromatic vinyl hydrocarbon can be synthesized, for example, by copolymerizing a conjugated diene and an aromatic vinyl hydrocarbon in a hydrocarbon solvent in the presence of an alkali metal catalyst. The hydrogenated copolymer can be prepared by hydrogenating the copolymer in the presence of a hydrogenation catalyst. A commercially available product can also be used as the component (d).

[0051] (Other Ingredients) The polycarbonate resin composition according to one embodiment may further contain other components in addition to the components (a), (b), (c), and (d) without departing from the spirit of the present invention. Examples of other components include various additives such as heat stabilizers, antioxidants, colorants, release agents, softeners, antistatic agents, impact modifiers, fillers, lubricants, dyes, and flame retardants. The polycarbonate resin composition may further contain polymers other than the components (a), (b), (c), and (d). In the case of a polycarbonate resin composition used for applications in which flame retardancy is not very important, the content of the flame retardant may be 0 to 20 parts by mass, and the total content of the components (b), (c), (d), and the flame retardant may be less than 25 parts by mass relative to 100 parts by mass of the component (a).

[0052] The content of Ti (titanium) in the polycarbonate resin composition may be 0.01 to 30 ppm based on the mass of the polycarbonate resin composition. When the content of Ti is within this range, the hydrolysis resistance and scratch recovery of the polycarbonate resin composition and the molded article tend to be further improved. Ti may be, for example, a trace component derived from a polyester polymerization catalyst.

[0053] [Method for producing polycarbonate resin composition] The polycarbonate resin composition can be obtained, for example, by a method including melt-kneading each component. A method for producing a polycarbonate resin composition according to one embodiment includes a step (1) of melt-kneading (b) polyester, (c) a polymer having an epoxy group, and (d) a copolymer having a monomer unit derived from a conjugated diene and a monomer unit derived from an aromatic vinyl hydrocarbon to obtain a mixture, and a step (2) of kneading the mixture with (a) an aromatic polycarbonate to prepare a polycarbonate resin composition. The content of the (d) component is 9.0 mass% or less and may be less than 5.0 mass% based on the total amount of the (a), (b), (c) and (d) components.

[0054] By using such a production method, it is possible to obtain a polycarbonate resin composition that can be used to form a molded article that has hydrolysis resistance, an excellent balance between rigidity and impact resistance, high dart impact strength, and little surface peeling.

[0055] In step (1), a mixture of components (b), (c), and (d) can be obtained. The kneading temperature in step (1) may be, for example, 230 to 300°C. In step (2), a polycarbonate resin composition containing components (a), (b), (c), and (d) can be obtained. The kneading temperature in step (2) is not particularly limited and may be, for example, 230 to 350°C. For example, a twin-screw kneading extruder can be used to knead each component.

[0056] The polycarbonate resin composition may be in the form of pellets. The molded article made of the polycarbonate resin composition according to the present embodiment can be produced, for example, by a method including molding the pellet-shaped polycarbonate resin composition into a desired shape by a conventional means such as injection molding. The shape of the molded article is not particularly limited. The molded article can be used for applications such as electric and electronic devices, communication devices, precision machinery, and automobile parts. EXAMPLES

[0057] The present invention will be described in more detail below with reference to examples, although the present invention is not limited to these examples.

[0058] 1. Raw materials The following raw materials were prepared for preparing a polycarbonate resin composition. (a) Ingredients Aromatic polycarbonate (PC): SD POLYCA200-13 (product name, manufactured by Sumika Polycarbonate Co., Ltd., viscosity average molecular weight: 21,000) (b) Component Polybutylene terephthalate (PBT): Toraycon 1401 X06 (product name, manufactured by Toray Industries, Inc., inherent viscosity: 1.74) (c) Component E-GMA-1: Bondfast E (product name, manufactured by Sumitomo Chemical Co., Ltd., a copolymer of 88 parts by mass of ethylene and 12 parts by mass of glycidyl methacrylate) E-GMA-2: Bondfast 7M (product name, manufactured by Sumitomo Chemical Co., Ltd., a copolymer of 67 parts by mass of ethylene, 6 parts by mass of glycidyl methacrylate, and 27 parts by mass of methyl acrylate) (d) Ingredients SEBS-1: Kraton G1651 (product name, manufactured by Kraton Corporation, hydrogenated styrene-butadiene-styrene copolymer) SEBS-2: Kraton G1633 (product name, manufactured by Kraton Corporation, hydrogenated styrene-butadiene-styrene copolymer) (others) EOR: Engage 8842 (trade name, manufactured by The Dow Chemical Company, ethylene-octene-1 copolymer, density: 0.857 g / cm 3 )

[0059] 2. Polycarbonate resin composition and molded body Example 1 A co-rotating twin-screw kneading extruder (KZW20TW, Technobel Co., Ltd.) having a main feeder, a sub-feeder, and a nozzle head provided on the extruder side was prepared. This twin-screw kneading extruder had nine barrels C1 to C9 provided along the extrusion direction from the hopper side. The temperature of each barrel was set as follows. C1: 50℃ C2: 200℃ C3~C9: 260℃ 50 parts by mass of SEBS-1 was fed from the main feeder to the hopper port provided on barrel C1 of the twin-screw kneading extruder, and 40 parts by mass of E-GMA-1 and 10 parts by mass of PBT were fed from the sub-feeder. The nozzle head temperature was set to 260°C, the screw rotation speed to 300 rpm, and the discharge rate to 3 kg / hour, and SEBS-1, E-GMA-1, and PBT were melt-kneaded. The molten mixture discharged from the twin-screw extruder was cut with a pelletizer to obtain pellets of a mixture of SEBS-1, E-GMA-1, and PBT.

[0060] Next, the temperatures of the barrels of the twin-screw kneading extruder were set as follows. C1: 100℃ C2: 240℃ C3~C9: 280℃ 90 parts by mass of PC was fed from the main feeder and 10 parts by mass of the above mixture pellets were fed from the sub-feeder to the hopper port provided on the barrel C1 of the twin-screw kneading extruder. The temperature of the nozzle head was set to 280°C, the screw rotation speed to 300 rpm, and the discharge rate to 5 kg / hour, respectively, and PC, SEBS-1, E-GMA-1, and PBT were melt-kneaded. The molten mixture discharged from the twin-screw extruder was cut with a pelletizer to obtain a pellet-shaped polycarbonate resin composition.

[0061] The pellet-like polycarbonate resin composition was injection molded using an injection molding machine (Sumitomo Heavy Industries, SE100EV) under conditions of a mold temperature of 90°C, a cylinder temperature of 300°C, and an injection speed of 15 mm / sec to produce a molded body A having a thickness of 3.2 mm. The pellet-like polycarbonate resin composition was injection molded using an injection molding machine under conditions of a mold temperature of 80°C, a cylinder temperature of 300°C, and an injection speed of 30 mm / sec to produce a molded body B having a length of 150 mm, a width of 90 mm, and a thickness of 2 mm.

[0062] Example 2 A polycarbonate resin composition and a molded article were produced under the same conditions as in Example 1, except that SEBS-1 was changed to SEBS-2 and E-GMA-1 was changed to E-GMA-2.

[0063] Example 3 Polycarbonate resin compositions and molded articles were produced under the same conditions as in Example 1, except that the blending ratio of SEBS-1 and SEBS-2 was changed as shown in Table 1.

[0064] (Examples 4 to 5) Polycarbonate resin compositions and molded articles were produced under the same conditions as in Example 1, except that the blending ratio of PC to PBT was changed as shown in Table 1.

[0065] Comparative Example 1 PC was molded alone under the same conditions as in Example 1 to produce a molded body.

[0066] Comparative Example 2 A polycarbonate resin composition and a molded article were produced under the same conditions as in Example 1, except that SEBS-1 was changed to EOR.

[0067] Comparative Example 3 A polycarbonate resin composition and a molded article were produced under the same conditions as in Example 1, except that PBT was not used and the blending ratio was changed as shown in Table 2.

[0068] Comparative Example 4 A polycarbonate resin composition and a molded article were produced under the same conditions as in Example 1, except that E-GMA-1 was not used and the blending ratio was changed as shown in Table 2.

[0069] Comparative Example 5 A pellet-shaped polycarbonate resin composition and a molded product were produced under the same conditions as in Example 1, except that the blending ratio of PC and PBT was changed as shown in Table 2.

[0070] 3. Evaluation Tables 1 and 2 show the blend ratios (parts by mass) of each polycarbonate resin composition and the evaluation results.

[0071] (Hydrolysis resistance) The pellet-shaped polycarbonate resin composition was stored for 72 hours using a pressure cooker (EHS-221(M) manufactured by Espec) under conditions of a test temperature of 120°C and a humidity of 100%RH. The melt flow index (MFR) of the pellets before and after storage was measured using a melt flow tester. The melt flow index was measured under conditions of a temperature of 280°C and a load of 2.16 kgf. The presence or absence of an increase in the MFR of the pellets after storage in the pressure cooker compared to the MFR of the pellets before storage, and the increase rate of the MFR were measured. If no increase in MFR was observed or the increase rate was small, it can be said that the polycarbonate resin composition has excellent hydrolysis resistance.

[0072] (Izod impact test) A notched test piece having a length of 63.5 mm, a width of 12.7 mm, and a thickness of 3.2 mm was prepared from the molded body A. Using this test piece, the Izod impact strength (kJ / m 2 The Izod impact test was carried out in an atmosphere of 23°C and with a test piece temperature of -40°C.

[0073] (Tensile test) A test piece for a tensile test in accordance with ASTM D 638 Type 1 was prepared from the molded body A. A tensile test using this test piece was carried out in an atmosphere of 23° C. at a tensile speed of 1 mm / min to measure the tensile modulus (MPa).

[0074] (surface impact test) Using molded body B, a surface impact test was carried out under the conditions of a firing pin diameter of 1 / 2 inch, a sample pressing plate of 1 inch, a firing pin speed of 7 m / sec, and a temperature of 23° C., and the total energy (J) was measured.

[0075] (Surface peeling test) A surface peeling test was carried out using molded body B. 100 slits measuring 2 mm x 2 mm were made with a cutter in the resin inflow section of molded body B, and then Nichiban cellophane tape (CT405AP-24) was attached to the slits. The cellophane tape was forcefully peeled off and the number of peeled off squares at the slits was counted. If the number of peeled off squares is small, it can be said that the surface peeling of the polycarbonate resin composition is small.

[0076] [Table 1]

[0077] [Table 2]

[0078] It was confirmed that the polycarbonate resin composition of each Example had hydrolysis resistance, an excellent balance between rigidity and impact resistance, and was capable of producing a molded article with high dart impact strength and little surface peeling.

Claims

1. (a) an aromatic polycarbonate; (b) a polyester; (c) a polymer having an epoxy group; and (d) a copolymer having monomer units derived from a conjugated diene and monomer units derived from an aromatic vinyl hydrocarbon; A polycarbonate resin composition comprising: the polyester is an aromatic polyester which is a condensation polymer of an aromatic dicarboxylic acid and a saturated dihydric alcohol, and the content of the polyester is 4.0 mass% or less based on the total amount of the aromatic polycarbonate, the polyester, the polymer having an epoxy group, and the copolymer; the content of the aromatic polycarbonate is 75% by mass or more and 98% by mass or less based on the total amount of the aromatic polycarbonate, the polyester, the polymer having an epoxy group, and the copolymer, a content of the polymer having an epoxy group being 0.1 parts by mass or more and 20 parts by mass or less, and a content of the copolymer being 1 part by mass or more and 30 parts by mass or less, relative to 100 parts by mass of the aromatic polycarbonate;

2. The polycarbonate resin composition of claim 1 , wherein the polyester comprises polybutylene terephthalate.

3. 3. The polycarbonate resin composition according to claim 1, wherein the copolymer comprises a copolymer or a hydrogenated copolymer of a conjugated diene and an aromatic vinyl hydrocarbon.

4. 3. The polycarbonate resin composition according to claim 1, wherein the copolymer comprises a hydrogenated copolymer of a conjugated diene and an aromatic vinyl hydrocarbon.

5. 5. The polycarbonate resin composition according to claim 3, wherein the hydrogenated copolymer is a hydrogenated styrene-butadiene-styrene copolymer or a hydrogenated styrene-isoprene-styrene copolymer.

6. The polycarbonate resin composition according to any one of claims 1 to 5, wherein the polymer having an epoxy group comprises an ethylene-glycidyl (meth)acrylate copolymer.

7. (b) a polyester, (c) a polymer having an epoxy group, and (d) a copolymer having a monomer unit derived from a conjugated diene and a monomer unit derived from an aromatic vinyl hydrocarbon, melt-kneading the resulting mixture; and (a) kneading the mixture with an aromatic polycarbonate to prepare a polycarbonate resin composition. the polyester is an aromatic polyester which is a condensation polymer of an aromatic dicarboxylic acid and a saturated dihydric alcohol, and the content of the polyester is 4.0 mass% or less based on the total amount of the aromatic polycarbonate, the polyester, the polymer having an epoxy group, and the copolymer; the content of the aromatic polycarbonate is 75% by mass or more and 98% by mass or less based on the total amount of the aromatic polycarbonate, the polyester, the polymer having an epoxy group, and the copolymer, a content of the polymer having an epoxy group of 0.1 parts by mass or more and 20 parts by mass or less, and a content of the copolymer of 1 part by mass or more and 30 parts by mass or less, relative to 100 parts by mass of the aromatic polycarbonate.

Citation Information

Patent Citations

  • Thermoplastic resin composition

    JP1998017760A

  • Flame retarded thermoplastic resin composition

    JP2000053851A

  • Melt tension improvement agent, polycarbonate-polyester composite resin composition, and molding

    JP2012077240A

  • Thermoplastic resin composition for gas injection molding, resin solid article using the same, molded body and method of manufacturing the same

    JP2016094494A

  • Polycarbonate / Polyester Resin Composition

    JP2893185B2