Method for synthesizing polymers by controlled radical inverse emulsion polymerization

Inverse emulsion polymerization using a water-soluble precursor in an inverse emulsion system addresses the challenges of conventional radical polymerization by producing water-soluble polymers with controlled molecular weight and low polydispersity.

JP7592010B2Active Publication Date: 2024-11-29SPSM SA
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
JP2021524203
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2018-11-06
Filing Date
2019-11-04
Publication Date
2024-11-29
Estimated Expiration
2039-11-04

AI Technical Summary

Technical Problem

Conventional radical polymerization methods struggle to achieve controlled chain lengths and narrow molecular weight distribution, leading to high variance and compositional drift, especially in the synthesis of water-soluble polymers.

Method used

A method for inverse emulsion polymerization using a water-soluble precursor in an inverse emulsion system, combining a water-soluble monomer with a lipophilic solvent and surfactant, followed by radical polymerization to produce polymers with controlled molecular weight and low polydispersity.

Benefits of technology

The method enables the production of water-soluble polymers with high molecular weight and low polydispersity index, typically below 2, by controlling the molecular weight and minimizing compositional heterogeneity.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007592010000007
    Figure 0007592010000007
  • Figure 0007592010000008
    Figure 0007592010000008
  • Figure 0007592010000001
    Figure 0007592010000001
Patent Text Reader

Abstract

The present invention relates to a method for preparing a polymer by reverse-phase emulsion polymerization, comprising the steps of: a) preparing an aqueous phase containing at least one water-soluble monomer and at least one water-soluble precursor of formula (I); b) preparing an organic phase containing a lipophilic solvent and at least one water-in-oil surfactant; c) stirring and mixing the aqueous phase and the organic phase to form a reverse emulsion; and d) after the reverse emulsion has been formed, adding a radical polymerization initiator to the reverse emulsion and polymerizing at least one water-soluble monomer to obtain a polymer. TIFF2022506667000008.tif51156
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a novel process for radical polymerization in inverse emulsion. [Background technology]

[0002] Conventional radical polymerization is an ideal route to synthesize high molecular weight polymers on an industrial scale because it is easy to carry out: in fact, it is applicable to a wide range of monomers, is tolerant of the functional groups carried by the monomers and impurities present in the reaction medium, is reproducible, is compatible in homogeneous and heterogeneous media, and can be carried out in protic solvents, including water.

[0003] However, this technique does not allow accurate chain length. Moreover, different sizes of chains would show a fairly high dispersion. During conventional radical copolymerization of two monomers, composition drift also occurs if one type of monomer is consumed faster than the other. Obtaining polymers with macromolecular architecture and controlled microstructure proves difficult in that case.

[0004] Although it is possible to achieve controlled architectures with living ionic polymerization, it is difficult to carry out and requires stringent conditions, such as a medium free of impurities, water and / or traces of oxygen.

[0005] Reversible deactivation radical polymerization (RDRP) combines the ease of implementation of conventional radical polymerization with the liveliness of ionic polymerization.

[0006] RDRP is a combination of techniques such as iodine transfer polymerization (ITP), NMP (nitroxide mediated polymerization), which is polymerization controlled by nitroxides, ATRP (atom transfer radical polymerization), which is polymerization controlled by atom transfer, RAFT (reversible addition-fragmentation chain transfer polymerization), which includes MADIX technology (MACromolecular Design by Interchange of Xanthates), OMRP (organometallic mediated radical polymerization), which are various variations of polymerization using organometallic compounds, and radical polymerization controlled by heteroatom-containing compounds (organoheteroatom mediated radical polymerization (OHRP)).

[0007] All of these techniques are based on the reversible equilibrium between dormant and active species (propagating macroradicals), as shown in Figure 1.

[0008] This activation-deactivation process allows the chains to grow at the same rate until the monomer is completely consumed, thus allowing the molecular weight of the polymer to be controlled to obtain a narrow molecular weight distribution. It would also be possible to minimize compositional heterogeneity. Reversible deactivation of the growing chains is at the origin of minimizing irreversible termination reactions. Most polymer chains remain in a dormant form and can therefore be reactivated. It is possible to functionalize the chain ends to further initiate other polymerization regimes or to extend the chains. This is the key to obtain high molecular weights with controlled composition and structure.

[0009] Controlled radical polymerization therefore has the following characteristic features: 1. The number of polymer chains is fixed throughout the duration of the reaction. 2. All polymer chains grow at the same rate, Linear increase in molecular weight Tight molecular weight distribution results. 3. The average molecular weight is controlled by the monomer / precursor molar ratio.

[0010] The controlled properties are more pronounced when the rate of radical chain reactivation is very high compared to the rate of chain propagation. However, in some cases, the rate of radical chain reactivation is greater than or equal to the rate of propagation. In these cases, conditions 1 and 2 are not observed, and as a result, it becomes impossible to control the molecular weight.

[0011] Patent EP 991 683 describes direct emulsion-controlled radical polymerization. This type of polymerization requires a step to recover the polymer, such as vacuum deposition. The polymers described in patent EP 991 683 are obtained by polymerization of lipophilic monomers. In the case of emulsion polymerization, the emulsion is thus a direct emulsion, and the monomers are polymerized in the dispersed or organic phase. The presented procedure results in block polymers of low molecular weight.

[0012] In patent application WO 2012 / 042167 a gel polymerization route is used: water-soluble precursors are used, but this approach does not make it possible to obtain polymers with high molecular weights. [Prior art documents] [Patent documents]

[0013] [Patent Document 1] Patent EP 991 683 [Patent Document 2] Patent application WO 2012 / 042167 [Patent Document 3] Patent FR 2 868 783 Summary of the Invention [Problem to be solved by the invention]

[0014] The problem that the Applicant proposes to solve is to obtain water-soluble polymers that are of high molecular weight and at the same time have a low polydispersity index, advantageously lower than 2. [Means for solving the problem]

[0015] The present invention relates to a method for preparing a polymer by inverse emulsion polymerization, comprising the steps of: a) preparing an aqueous phase comprising at least one water-soluble monomer and at least one water-soluble precursor of formula (I); Precursor

[0016] [ka]

[0017] (In the formula, Z is O, S or N; R 1 and R 2 are the same or different, an optionally substituted alkyl, acyl, alkenyl or alkynyl group (i), or a saturated or unsaturated, optionally substituted, carbon-based ring (ii) or an aromatic carbon-based ring (ii); or represents a saturated or unsaturated, optionally substituted heterocycle (iii), or an aromatic heterocycle (iii), These groups and rings (i), (ii) and (iii) may be substituted by substituted aromatic groups, or alkoxycarbonyl or aryloxycarbonyl (-COOR), carboxy (-COOH), acyloxy (-OCR), carbamoyl (-CONR), cyano (-CN), alkylcarbonyl, alkylarylcarbonyl, arylcarbonyl, arylalkylcarbonyl, phthalimido, maleimido, succinimido, amidino, guanidino, hydroxy (-OH), amino (-NR), halogen, allyl, epoxy, alkoxy (-OR), S-alkyl, S-aryl, hydrophilic or ionic groups such as alkali metal salts of carboxylic acids, alkali metal salts of sulfonic acids, polyalkylene oxide chains (POE, POP), cationic substituents (quaternary ammonium salts); R represents an alkyl or aryl group; A is a linear or structured polymer chain containing n identical or different monomers, n is an integer between 1 and 500, advantageously between 2 and 500 b) preparing an organic phase comprising a lipophilic solvent and at least one water-in-oil surfactant; c) mixing the aqueous phase and the organic phase by stirring to form an inverse emulsion; d) after formation of the inverse emulsion, adding a radical polymerization initiator to said inverse emulsion to polymerize at least one water-soluble monomer to obtain a polymer; The present invention relates to a method comprising the steps of:

[0018] In formula (I), R 1 and R 2are identical or different and advantageously represent a group of (i) (alkyl, acyl, alkenyl or alkynyl), more advantageously selected from a linear or branched alkyl group containing from 1 to 20 carbon atoms, preferably from 1 to 10 carbon atoms, a linear or branched acyl group containing from 2 to 20 carbon atoms, preferably from 2 to 10 carbon atoms, a linear or branched alkenyl group containing from 2 to 20 carbon atoms, preferably from 2 to 10 carbon atoms, or a linear or branched alkynyl group containing from 2 to 20 carbon atoms, preferably from 2 to 10 carbon atoms, which groups may further comprise one or more substituted aromatic groups, optionally containing from 4 to 7 carbon atoms, or alkoxycarbonyl or or aryloxycarbonyl (-COOR), carboxy (-COOH), acyloxy (-OCR), carbamoyl (-CONR), cyano (-CN), alkylcarbonyl, alkylarylcarbonyl, arylcarbonyl, arylalkylcarbonyl, phthalimide, maleimide, succinimide, amidino, guanidino, hydroxy (-OH), amino (-NR), halogen, allyl, epoxy, alkoxy (-OR), S-alkyl, S-aryl, hydrophilic or ionic groups, for example, alkali metal salts of carboxylic acids, alkali metal salts of sulfonic acids, polyalkylene oxide chains (POE, POP), and cationic substituents (quaternary ammonium salts).

[0019] R advantageously represents a linear or branched alkyl group containing from 1 to 20 carbon atoms, preferably from 1 to 10 carbon atoms, or an aryl group containing from 6 to 10 carbon atoms.

[0020] Advantageously, carbocyclic ring (ii) contains from 6 to 10 carbon atoms, while heterocyclic ring (iii) advantageously contains from 5 to 9 carbon atoms.

[0021] The groups containing carbon atoms are hydrocarbon groups which may also contain heteroatoms. Furthermore, the heterocycles contain one or more heteroatoms, preferably N, O, S or P.

[0022] Monomer means a molecule capable of forming a polymer by polymerization, advantageously a molecule having vinyl unsaturation (CH2=CH- and its derivatives formed by the replacement of at least one hydrogen).In order not to affect the clarity of the description, the term monomer also refers to the monomer in its polymerized form.That is, acrylamide monomer shows not only CH2=CH-C(=O)NH2 but also -(CH2-CH(C(=O)NH2))- pattern.

[0023] In an NR2 functional group, the two R groups may be the same or different.

[0024] Step d) makes it possible to obtain a water-soluble polymer, which may be a homopolymer or a copolymer.

[0025] The expression "inverse emulsion" refers to both inverse emulsions and inverse microemulsions, which are water-in-oil emulsions in which the aqueous phase is dispersed in the form of droplets or small droplets in the organic phase.

[0026] The expression "water-soluble precursor" denotes a precursor which is soluble in water to a proportion of at least 50 g / l at a temperature of 25° C. This definition also relates to other water-soluble compounds (polymers, monomers, etc.) mentioned.

[0027] Generally, the polymer chain A comprises at least one nonionic monomer and / or at least one anionic monomer and / or at least one cationic monomer. Advantageously, A comprises at least two identical monomers.

[0028] The following various types of monomers can be used as monomers in the aqueous phase or in the polymer chain A of the precursor:

[0029] The nonionic monomer that can be used within the framework of the present invention can be specifically selected from the group that comprises vinyl monomers that dissolve in water.Preferred monomers that belong to this class are, for example, acrylamide, methacrylamide, N-isopropylacrylamide, N,N-dimethylacrylamide, N,N-diethylacrylamide, N-methylolacrylamide, N-vinylformamide, N-vinylacetamide, N-vinylpyridine, N-vinylpyrrolidone, acryloylmorpholine (ACMO), glycidyl methacrylate, glyceryl methacrylate and diacetone acrylamide.Preferred nonionic monomer is acrylamide.

[0030] The anionic monomers are preferably selected from acrylic acid, methacrylic acid, itaconic acid, crotonic acid, maleic acid, fumaric acid, 2-acrylamido-2-methylpropanesulfonic acid, vinylsulfonic acid, vinylphosphonic acid, allylsulfonic acid, allylphosphonic acid, styrenesulfonic acid, said anionic monomers being unsalted, partially salified or fully salified, and the salts of 3-sulfopropyl methacrylate. The salt forms advantageously correspond to alkali metal (Li, Na, K, etc.), alkaline earth metal (Ca, Mg, etc.) or ammonium salts, in particular quaternary ammonium salts.

[0031] The cationic monomers that can be used in the context of the present invention can be selected in particular from acrylamide, acrylic, vinyl, allyl or maleic type monomers, which have a quaternary ammonium function by salification or quaternization, including, but not limited to, quaternized dimethylaminoethyl acrylate (ADAME), quaternized dimethylaminoethyl methacrylate (MADAME), dimethyldiallylammonium chloride (DADMAC), acrylamidopropyltrimethylammonium chloride (APTAC) and methacrylamidopropyltrimethylammonium chloride (MAPTAC), said cationic monomers being unsalted, partially or completely salified.

[0032] The cationic monomers can also be chosen from associative cationic monomers, as described in patent FR 2 868 783.

[0033] The monomers may optionally be zwitterionic monomers of the acrylamide, acrylic, vinyl, allyl or maleic type, which have an amine or quaternary ammonium function and an acidic function of the carboxylic acid, sulfonic acid or phosphoric acid type, such as 2-((2-(acryloyloxy)ethyl)dimethylammonio)ethane-1-sulfonate, 3-((2-(acryloyloxy)ethyl)dimethylammonio)propane-1-sulfonate, 4-((2-(acryloyloxy)ethyl)dimethylammonio)butane-1-sulfonate, derivatives of dimethylaminoethyl acrylate such as [2-(acryloyloxy)ethyl](dimethylammonio)acetate, Derivatives of dimethylaminoethyl methacrylate such as 2-((2-(methacryloyloxy)ethyl)dimethylammonio)ethane-1-sulfonate, 3-((2-(methacryloyloxy)ethyl)dimethylammonio)propane-1-sulfonate, 4-((2-(methacryloyloxy)ethyl)dimethylammonio)butane-1-sulfonate, and [2-(methacryloyloxy)ethyl](dimethylammonio)acetate; 2- Derivatives of dimethylaminopropyl acrylamide such as ((3-acrylamidopropyl)dimethylammonio)ethane-1-sulfonate, 3-((3-acrylamidopropyl)dimethylammonio)propane-1-sulfonate, 4-((3-acrylamidopropyl)dimethylammonio)butane-1-sulfonate, [3-(acryloyloxy)propyl)](dimethylammonio)acetate, 2-((3-methacrylamidopropyl)dimethylammonio)ethane-1-sulfonate, 3-((3-methacrylamidopropyl)dimethylammonio)propane-1-sulfonate, 4-((3-methacrylamidopropyl)dimethylammonio)butane-1-sulfonate, and derivatives of dimethylaminopropyl methylacrylamide such as [3-(methacryloyloxy)propyl)](dimethylammonio)acetate, but are not limited to these.

[0034] The monomers may optionally have LCST or UCST groups.

[0035] According to the general knowledge of the skilled person, the group at LCST corresponds to those groups whose solubility in water for a given concentration changes above a certain temperature and which changes depending on the salt concentration. This group is the group that exhibits a transition temperature that determines the lack of compatibility with the solvent medium upon heating. The lack of compatibility with the solvent leads to opacification, i.e. loss of transparency, which can be due to precipitation, aggregation, gelation or viscosification of the medium. The lowest transition temperature is called the "LCST" (Lower Critical Solution Temperature). For each concentration of group that exhibits LCST, a heating transition temperature is observed. It is higher than the LCST, which is the minimum point of the curve. Below this temperature the polymer dissolves in water and above this temperature the polymer loses its solubility in water.

[0036] Usually, the LCST can be measured visually. It determines the temperature at which the lack of compatibility with the solvent occurs, i.e. the cloud point, which corresponds to the opacification or loss of transparency of the solution.

[0037] The LCST can also be determined depending on the type of phase transition, for example by DSC (differential scanning calorimetry), transmittance measurements, or viscosity measurements.

[0038] Preferably, the LCST is determined by determining the cloud point by transmittance according to the following protocol.

[0039] The transition temperature is measured for a compound exhibiting an LCST in a solution of said compound at a mass concentration of 1% by weight in deionized water. The cloud point corresponds to the temperature at which the solution exhibits a transmittance of light having a wavelength between 400 and 800 nm equal to 85%.

[0040] That is, the temperature at which the solution exhibits a transmittance equal to 85% corresponds to the lowest LCST transition temperature of the compound exhibiting an LCST, in this case the macromonomer.

[0041] Generally, a transparent composition will exhibit a maximum light transmittance value of at least 85%, preferably at least 90%, at any wavelength between 400 and 800 nm, via a 1 cm thick sample, which is the basis for the cloud point corresponding to 85% transmittance.

[0042] According to the general knowledge of the skilled artisan, the UCST group corresponds to a group whose solubility in water for a given concentration changes below a certain temperature and that changes depending on the salt concentration. This group is a group that has a cooling transition temperature that defines the boundary of the lack of affinity with the solvent medium. The lack of affinity with the solvent leads to opacification, i.e. loss of transparency, which can be due to precipitation, aggregation, gelation or high viscosity of the medium. The maximum transition temperature is called "UCST" (Upper Critical Solution Temperature). For each concentration of UCST group, a cooling transition temperature is observed, which is higher than the UCST, the minimum point of the curve. Above this temperature the polymer dissolves in water and below this temperature the polymer loses its solubility in water.

[0043] The invention and the advantages it brings will become more apparent from the following figures and examples, which are provided to illustrate the invention without limiting it. [Brief description of the drawings]

[0044] [Figure 1] FIG. 1 shows the reversible equilibrium between dormant and active species in a radical polymerization process with reversible deactivation. [Diagram 2] FIG. 2 shows the proton nuclear magnetic resonance spectrum (H NMR) of the water-soluble precursor of formula (I) in Example 1. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0045] According to a preferred embodiment, the precursor is of formula (I), wherein Z is O.

[0046] According to another preferred embodiment, the precursor is of formula (I), wherein Z is O, A is a linear or structured polymer chain resulting from 1 to 100 (preferably 2 to 100) monomers, including at least one nonionic monomer and / or at least one anionic monomer and / or at least one cationic monomer.

[0047] According to another preferred embodiment, the precursor is of formula (I), wherein Z is O, A is a linear or structured polymer chain obtained from 1 to 100 (preferably 2 to 100) monomers, including at least one nonionic monomer and / or at least one anionic monomer and / or at least one associative cationic monomer.

[0048] According to another preferred embodiment, the precursor is of formula (I), wherein Z is O, A is a linear or structured polymer chain obtained from 1 to 100 (preferably 2 to 100) monomers, including at least one nonionic monomer and / or at least one anionic monomer and / or at least one monomer containing a group exhibiting an LCST.

[0049] Advantageously, A consists of n identical non-ionic monomers. More preferably, A is a polyacrylamide.

[0050] According to another preferred embodiment, the precursor has the following formula (II):

[0051] [ka]

[0052] (In the formula, "n" represents an integer between 1 and 100, preferably between 1 and 50.) It is.

[0053] According to another embodiment, in formula (I) or formula (II), "n" represents an integer between 2 and 100, preferably between 3 and 100, more preferably between 4 and 50.

[0054] According to the invention, the amount of precursor in the emulsion is 5.10 times the weight of the emulsion. -7 Between 5% and 5%, preferably 5.10 -4 % to 5.10 -2 %.

[0055] The molar ratio of water-soluble monomer / precursor in the aqueous phase is advantageously between 12,500:1 and 300,000:1, preferably between 27,500:1 and 250,000:1, more preferably between 27,500:1 and 10,000:1.

[0056] The radical polymerization initiator can be selected from the initiators conventionally used in radical polymerization. The radical polymerization initiator can be, for example, one of the following initiators: - hydrogen peroxides such as those selected from the group comprising tert-butyl hydroperoxide, cumene hydroperoxide, t-butyl peroxyacetate, t-butyl peroxybenzoate, t-butyl peroxyoctoate, t-butyl peroxyneodecanoate, t-butyl peroxyisobutyrate, lauroyl peroxide, t-amyl peroxypivalate, t-butyl peroxypivalate, dicumyl peroxide, benzoyl peroxide, potassium persulfate, and ammonium persulfate; - 2-2'-azobis(isobutyronitrile), 2,2'-azobis(2-butanenitrile), 4,4'-azobis(4-pentanoic acid), 1,1'-azobis(cyclohexanecarbonitrile), 2-(t-butylazo)-2-cyanopropane, 2,2'-azobis[2-methyl-N-(1,1)-bis(hydroxymethyl)-2-hydroxyethyl]propionamide, 2,2'-azobis(2-methyl-N-hydroxyethyl)propionamide, 2,2'-azobis(N,N'-dimethyleneisobutylamidine)dichloride, 2,2'- azo compounds such as those selected from the group including azobis(2-amidinopropane) dichloride, 2,2'-azobis(N,N'-dimethyleneisobutyramide), 2,2'-azobis(2-methyl-N-[1,1-bis(hydroxymethyl)-2-hydroxyethyl]propionamide), 2,2'-azobis(2-methyl-N-[1,1-bis(hydroxymethyl)ethyl]propionamide), 2,2'-azobis(2-methyl-N-(2-hydroxyethyl)propionamide], and 2,2'-azobis(isobutyramide) dihydrate; - A reducing system comprising a combination of such as those selected from the group including: a) hydrogen or alkyl peroxides, peresters, or percarbonates, etc.; b) any salt of iron, titanium, zinc formaldehyde sulfoxylate, or sodium formaldehyde sulfoxylate; and c) mixtures of reducing sugars; Alkali metal or ammonium persulfates, perborates or perchlorates in combination with alkali metal bisulfites, such as sodium metabisulfite, and reducing sugars; Alkali metal persulfates in combination with arylphosphonic acids such as benzenephosphonic acid and reducing sugars.

[0057] The various monomers used in the aqueous phase can be selected from the lists given above in the description also relating to the precursor polymer sequence A. Advantageously, the monomers are selected from the group comprising nonionic monomers, anionic monomers and mixtures of nonionic and anionic monomers.

[0058] Advantageously, the polymers obtained according to the invention have a molecular weight between 1,250,000 and 30,000,000 (thirty million) g / mol, preferably between 2,750,000 and 25,000,000 g / mol, molecular weight being understood as weight average molecular weight.

[0059] The polydispersity index (Ip) of the polymers obtained according to the invention is advantageously at most 2 (≦2), preferably at most 1.5 (≦1.5). The polydispersity index is determined by the following formula: Ip=Mw / Mn Mw is the weight average molecular weight. Mn is the number average molecular weight.

[0060] The determination of the average molecular weight by weight (Mw) and the average molecular weight by number (Mn) is carried out in a conventional manner, advantageously by size exclusion chromatography (CES) coupled with a multi-angle light scattering detector on a Dawn Heleos II 18 angles (Wyatt technology).

[0061] According to another aspect, the invention relates to the use of the polymers obtained by the polymerization process described above in the oil and gas industry, hydraulic fracturing, paper, water treatment, construction, mining, cosmetics, textiles or detergents. Preferably, the polymers are used in the field of enhanced oil and gas recovery. EXAMPLES

[0062] Synthesis of water-soluble precursors 2 kg of O-ethyl-S-(1-methoxycarbonyl)ethyl dithiocarbonate, 10 kg of acrylamide, 12 kg of water, 20 kg of acetic acid and 140 g of azo initiator (V 044) were charged into a 50 kg reactor at room temperature (20° C.). The mixture was degassed by bubbling with nitrogen and then heated to 60° C. with stirring. The polymerization reaction was carried out for 3 hours with stirring.

[0063] The water-soluble precursor thus obtained corresponds to formula (I), in which Z is O, R 1 is CH2-CH3, A is (CH(C(=O)NH2)-CH2) n and n is 7, R 2 is CH(CH3)-C(=O)-O-CH3.

[0064] This precursor was specifically characterized by its 1H NMR spectrum (300.13 MHz) in D2O (Figure 2). EXAMPLES

[0065] Synthesis of polymer P1 in inverse emulsion according to the invention Preparation of the aqueous phase: 400 g of acrylamide (50% by weight in water), 90 g of acrylic acid, 150 g of water, and 0.0015% by weight of the emulsion of the water-soluble precursor of Example 1 were mixed. The aqueous phase was neutralized with 90 g of sodium hydroxide (50% by weight in water).

[0066] Preparation of the organic phase: All water-in-oil surfactants (2.5% by weight of the alkanolamides relative to the emulsion, and 3% by weight of the stearyl methacrylate relative to the emulsion) were mixed in 200 g of ISOPAR type oil (Isopar N and L).

[0067] The aqueous and organic phases were mixed to form an emulsion, which was then degassed for 60 minutes before polymerization was initiated by the addition of the reducing agent, sodium metabisulfite (SMB).

[0068] At the end of the polymerization, the resulting polymer is recovered by precipitation in acetone. EXAMPLES

[0069] Synthesis of P2 polymer in inverse emulsion Polymer P2 is synthesized as in Example 2, substituting sodium hypophosphite for the water-soluble precursor. EXAMPLES

[0070] Synthesis of inverse emulsion polymer P3 Polymer P3 can be prepared by reacting a water-soluble precursor with a compound of formula (I) where Z is O and R 1 is CH2-CH3, R 2 is CH3 and A is CH-(CH3)C(=O)-O-), but in this case (and contrary to the invention) A is not present in the monomer.

[0071] [ka] EXAMPLES

[0072] Characterization of polymers P1, P2 and P3 The three polymers P1, P2 and P3 were analyzed by size exclusion chromatography (CES) under the following conditions: one Shodex SB807-G precolumn and two Shodex OHpak columns in series (SB-807 HQ and SB-805 HQ) coupled with a refractive index detector (Optilab T-rEX, Wyatt Technology, and Dawn Heleos II 18 angles, Wyatt Technology).

[0073] [Table 1]

[0074] At number equivalent molecular weights, the polydispersity of polymers in the presence of hydrophilic precursors is much lower than that of polymers prepared by conventional radical polymerization. It was difficult to control the molecular weight of polymer P3 because the precursor used was not soluble in water, which corresponds to a polymerization without a precursor.

Claims

1. 1. A method for preparing a polymer by inverse emulsion polymerization, comprising: a) preparing an aqueous phase comprising at least one water-soluble monomer and at least one water-soluble precursor of formula (I); [Formula 1] (In the formula, Z is O or S; R 1 and R 2 are the same or different, an optionally substituted alkyl, acyl, alkenyl or alkynyl group (i), or a saturated or unsaturated, optionally substituted carbon-based ring (ii) or an aromatic carbon-based ring (ii), or - represents a saturated or unsaturated, optionally substituted heterocycle (iii) or an aromatic heterocycle (iii), These groups and rings (i), (ii) and (iii) may be substituted aromatic groups or alkoxycarbonyl or aryloxycarbonyl (-COOR), carboxy (-COOH), acyloxy (-O 2 CR), carbamoyl (-CONR 2 ), cyano (-CN), alkylcarbonyl, alkylarylcarbonyl, arylcarbonyl, arylalkylcarbonyl, phthalimido, maleimido, succinimido, amidino, guanidino, hydroxy (-OH), amino (-NR 2 ), halogen, allyl, epoxy, alkoxy (-OR), S-alkyl, S-aryl, hydrophilic or ionic groups; R represents an alkyl or aryl group; A is a linear or structured polymer chain containing n identical or different monomers, (n is an integer between 4 and 500) b) preparing an organic phase comprising a lipophilic solvent and at least one water-in-oil surfactant; c) mixing the aqueous phase and the organic phase by stirring to form an inverse emulsion; d) after the inverse emulsion is formed, adding a radical polymerization initiator to said inverse emulsion to polymerize at least one water-soluble monomer to obtain a polymer; Including, 10. A process characterized in that the aqueous phase has a water soluble monomer / precursor ratio between 12,500:1 and 300,000:1 and the molecular weight of the resulting polymer is between 1,250,000 and 30,000,000 by mass.

2. 2. The method of claim 1, wherein Z is O.

3. - Z is O, - A is a linear or structured polymer chain obtained from 1 to 100 monomers, including at least one nonionic monomer and / or at least one anionic monomer and / or at least one cationic monomer; 3. The method according to claim 1 or 2, characterized in that

4. - Z is O, - A is a linear or structured polymer chain obtained from 1 to 100 monomers, including at least one nonionic monomer and / or at least one anionic monomer and / or at least one associative cationic monomer; 3. The method according to claim 1 or 2, characterized in that

5. - Z is O, - A is a linear or structured polymer chain obtained from 1 to 100 monomers, including at least one nonionic monomer and / or at least one anionic monomer and / or at least one monomer containing an LCST group; 3. The method according to claim 1 or 2, characterized in that

6. The precursor is of formula (II) [Case 2] (wherein n is an integer between 1 and 100.) 6. The method according to claim 1 , wherein

7. 7. The method according to claim 1, wherein the water-soluble monomer is selected from the group comprising nonionic monomers, anionic monomers and mixtures of nonionic and anionic monomers.

8. 8. The method according to claim 1, wherein the water-soluble monomer is a non-ionic monomer selected from the group comprising acrylamide, methacrylamide, N-isopropylacrylamide, N,N-dimethylacrylamide, N,N-diethylacrylamide, N-methylol acrylamide, N-vinylformamide, N-vinylacetamide, N-vinylpyridine, N-vinylpyrrolidone, acryloylmorpholine (ACMO), glycidyl methacrylate, glyceryl methacrylate and diacetone acrylamide.

9. 8. The method according to claim 1, characterized in that the water-soluble monomer is an anionic monomer selected from the group comprising acrylic acid, methacrylic acid, itaconic acid, crotonic acid, maleic acid, fumaric acid, 2-acrylamido-2-methylpropanesulfonic acid, vinylsulfonic acid, vinylphosphonic acid, allylsulfonic acid, allylphosphonic acid, styrenesulfonic acid, said anionic monomers in unsalted form, said anionic monomers in partial or complete salification, and salts of 3-sulfopropyl methacrylate.

10. 10. The process according to claim 1, wherein the polymer obtained has a polydispersity of less than or equal to 2.

11. R 1 and R 2are the same or different and are selected from the group comprising linear or branched alkyl groups containing from 1 to 20 carbon atoms, linear or branched acyl groups containing from 2 to 20 carbon atoms, linear or branched alkenyl groups containing from 2 to 20 carbon atoms, linear or branched alkynyl groups containing from 2 to 20 carbon atoms, 11. The process according to claim 1, wherein R represents a linear or branched alkyl group containing from 1 to 20 carbon atoms.

Citation Information

Patent Citations

  • Trithiocarbonate compound containing ethylene, preparation method and application thereof

    CN102382230A

  • Trithiocarbonate compound containing epoxy group, preparation method and application thereof

    CN102746476A

  • Alternate treating device of decontaminating filter screens for open channel

    CN104695385A

  • Method for block polymer synthesis by controlled radical polymerisation

    EP0991683A1

  • new AMPHOTERIC ASSOCIATIVE POLYMERS OF HIGH MOLECULAR WEIGHT AND THEIR APPLICATIONS

    FR2868783A1