Polymer gels in the formation of polymer brushes
The use of swellable and removable polymer gels in the polymerization medium addresses the challenges of uniform reactant distribution and complete polymer brush formation on surfaces, enabling controlled and large-scale production of homogeneous polymer brush-coated surfaces.
Patent Information
- Application Number
- JP2022522830
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2019-10-15
- Filing Date
- 2020-10-09
- Publication Date
- 2024-11-29
- Estimated Expiration
- 2040-10-09
AI Technical Summary
The preparation of polymer brushes is a specialized task that faces challenges such as achieving uniform distribution of reactants, avoiding solvent evaporation, and ensuring complete formation on large or complex surfaces, which can result in non-uniform polymer brush products.
The use of swellable and removable polymer gels in the polymerization medium to facilitate uniform distribution and formation of polymer brushes, allowing for controlled polymerization on surfaces of any shape by swelling in the medium and adhering to the surface during reaction, while being easily removable after brush formation.
This method enables uniform and controlled polymer brush formation on various surfaces, including large or complex shapes, with improved adhesion and minimal interference with the polymerization process, allowing for large-scale production of homogeneous polymer brush-coated surfaces.
Smart Images

Figure 0007592080000001 
Figure 0007592080000002 
Figure 0007592080000003
Abstract
Description
[Technical field]
[0001] The present invention relates to the use of polymer gels in the formation of polymer brushes. In particular, the present invention relates to a polymer gel swollen in a polymerization medium, the swollen polymer gel being applied during the formation of the polymer brush. The present invention further relates to the use of polymer gels in the formation of polymer brushes on a surface. In particular, the polymer gels used in the present invention are such that they can be swelled in a polymerization medium and can be removed after the formation of the polymer brush on the surface. The present invention provides an improved method for the formation of polymer brushes on a surface, allowing for easy large-scale production of surfaces covered with polymer brushes and the formation of specific polymer brushes. In particular, the present invention allows the application of the polymerization medium to surfaces of any shape. [Background technology]
[0002] The formation of polymer brushes is well known. Polymer brushes are polymer structures tethered at one end to a substrate such as a metal, plastic or ceramic material. Using specific preparation techniques and specific monomers, it is possible to design and synthesize polymer brushes with specific properties, such as chemical composition, thickness, grafting density and structure.
[0003] In particular, polymer brushes are used to join incompatible materials, i.e., materials that cannot be easily combined by adhesion or traditional interlocking methods. One major feature that polymer brushes have is that they can join materials in a virtually invisible manner.
[0004] There are several known methods for forming polymer brushes on a surface. When forming a polymer brush, a polymerization initiator is first formed on the surface on which the polymer brush is to be formed. The surface can then be contacted with a suitable monomer, catalyst, ligand, and, if necessary, a solvent, or with a suitable monomer, catalyst, ligand, oxygen scavenger, and, if necessary, a solvent, thereby forming the polymer brush using specific reaction conditions. The polymerization initiator and monomer are selected to suit the purpose and properties of the resulting polymer brush. The polymer brush can also be formed as a multi-layer polymer brush, for example, by repeating the formation of the polymer brush using different starting monomers. This can be done due to the controlled nature of the polymerization, which leaves initiation sites at the ends of the polymer brush. Summary of the Invention [Problem to be solved by the invention]
[0005] Nevertheless, the preparation of polymer brushes and the handling of reagents remain specialized tasks. Furthermore, the production of large polymer brush-coated surfaces poses various challenges, such as obtaining a uniform distribution of reactants on the surface on which the polymer brushes are formed, and avoiding the reactants forming depressions on the surface or areas where no reactants are present. Another challenge is dealing with the evaporation of solvent during the formation process, which results in a product with an apparently non-uniform distribution of polymer brushes. Similarly, areas where no polymer brushes are present can also be problematic, which leads to poor quality of the polymer brush product. To ensure complete formation of the polymer brushes on the surface, the surface can be completely immersed in the reactants, but this approach may not be possible for large surfaces or substrates.
[0006] Therefore, there is a need to improve and ensure uniform distribution of reactants for forming polymer brushes.
[0007] Polymer gels are well-known materials. They are used in many applications, ranging from disposable diapers, to contact lenses and implants, to tissue engineering. They are three-dimensional polymer networks capable of absorbing large amounts of water (hydrogels) or organic solvents (organogels), up to 500 times their own weight. They are obtained by crosslinking polymers into a crosslinked polymer matrix. These crosslinkable sites can be divided into reversible and irreversible crosslinks. Reversibly crosslinked polymer gels can result from various interactions or bonds, such as ionic attraction, hydrogen bonding, or metal coordination. Exposure of reversible polymer gels to certain stimuli results in cleavage of the crosslinks. Irreversibly crosslinked polymer gels have a network of covalent bonds, resulting in a permanent gel network.
[0008] Polymer gels have many useful characteristics, in particular a viscoelastic response to mechanical deformation. In particular, polymer gels have been proposed for a variety of applications, such as artificial muscles, purification or separation systems, tissue engineering, biosensors, shape memory materials, transport systems, and molecular recognition systems. Thus, polymer gels can absorb or respond to other compounds.
[0009] In recent years, hydrogels (polymer gels swollen in water) have been proposed for use in drug delivery due to their affinity for water and the possibility of controlled sustained drug release, e.g., by diffusion, swelling, chemicals, or the environment. However, despite the promise, very few products have been marketed, possibly because it is difficult to release drugs from hydrogels without degrading them, thereby creating a risk of toxicity due to the potential harm of degraded hydrogels to human health. To avoid the accumulation of hydrogels in the body, one approach is to synthesize enzymatically degradable drug delivery hydrogels.
[0010] Hydrogels have been combined with polymer brushes in the form of polymer brush-gels (see S. Demirci, Polymers 2018, 10, 956). Crosslinkers react or combine with brush-forming monomers to form brush-gels (or crosslinked polymer brush networks) from which other compounds can be released (e.g., methylene blue). In S. Demirci, cyclodextrin was incorporated as a crosslinker into polymers, such as poly(2-N-morpholinoethyl methacrylate), resulting in a crosslinked cyclodextrin methacrylate (CDMA) polymer on silicon wafers. This CDMA polymer was then used to reversibly capture / release methylene blue from the brush-gels.
[0011] Thus, although hydrogels are widely used in many applications and polymer gels can find applications as well, they have some drawbacks as a medium for generating polymer brushes. For example, depending on the polymer gel, the polymer brush reactants may be absorbed into the polymer gel, thereby preventing the migration of the reactants to the interface, resulting in poor formation of the polymer brush. Furthermore, crosslinking sites on the polymer gel may react with the polymer brush reactants, adversely affecting the polymer brush formation. Furthermore, some crosslinking sites may act as radical scavengers, thereby affecting the polymer brush formation. Furthermore, some crosslinking sites may act as metal coordinators, meaning that the metal catalyst utilized in the polymerization may be absorbed, thereby distorting the polymerization process.
[0012] Notwithstanding the above, hydrogels have been used in conjunction with polymer brushes. From EP 3 385 340 A1 a coating of a polysaccharide hydrogel layer and a polymer brush layer is known. The coating is prepared by a) providing a hydrogel layer on a substrate, b) attaching an initiator having radically transferable atoms on the hydrogel layer, and c) reacting a monomer with the initiator to form a polymer brush attached to the hydrogel layer. As a result, the hydrogel becomes an integral part of the polymer brush and the hydrogel is functionalized by the polymer brush.
[0013] The present inventors have surprisingly found that certain polymer gels can promote uniform distribution of the polymerization reactants and further promote the formation of polymer brushes. [Means for solving the problem]
[0014] The present invention relates to the formation of polymer brushes. In particular, the present invention relates to the use of polymer gels in the formation of polymer brushes. The polymer gels used in the present invention are swellable in a polymerization medium and removable after the formation of the polymer brush on the surface. Thus, the polymer gel serves as a "container" for the polymerization medium containing the reactants required for the formation (or growth) of the polymer brush. The polymer gel offers many advantages, such as easy application of the reactants required for the formation of the polymer brush. When swollen in the polymerization medium, the polymer gel has a dense structure, which can allow good contact between the polymerization medium and the surface on which the polymer brush is to be formed. Furthermore, after the formation of the polymer brush, the polymer gel and excess polymerization medium can be easily removed from the surface. Thus, the polymer gel does not react with any functional groups immobilized on the surface or with the components of the polymerization medium, leaving a pure polymer brush after the removal of the polymer gel.
[0015] Thus, in a first aspect, the present invention relates to a method for forming a polymer brush on a surface, comprising contacting a surface having a polymerization initiator immobilized thereon with a polymerization medium, in which a swellable and removable polymer gel is used during the formation of the polymer brush. One major advantage of using a polymerization medium in combination with a polymer gel is that the polymer gel swells in the polymerization medium, thereby providing a semi-solid or dense carrier for the polymerization medium and thereby a carrier for the polymer brush-forming components of the polymerization medium. This allows the formation of polymer brushes on surfaces of any shape and orientation, since the swollen polymerization medium adheres to the surface during the polymerization reaction. Another advantage is that the polymer gel slows the transfer of oxygen from the ambient atmosphere to the polymer gel-surface interphase, providing a greater degree of control over the polymerization reaction that results in the polymer brush.
[0016] Thus, the present invention particularly relates to a method in which the polymer gel is capable of swelling in the polymerization medium, and in which the polymer gel is removable after formation of the polymer brushes on the surface.
[0017] Previously, polymer brushes were formed by a dip-coating process, limiting the formation of polymer brushes into larger or more complex structures. In the present invention, the polymerization reaction can proceed easily without the need to fully immerse the surface / structure in the polymerization medium. A further advantage of the present invention is that the formation of polymer brushes can be directed only to specific sites, whereas traditional dip-coating can result in undesirable formation of polymer brushes if immobilized initiator is present at all sites of the surface / structure.
[0018] In a second aspect, the present invention relates to the use of a swellable and removable polymer gel in the formation of polymer brushes. In this aspect, the polymer gel is also swellable in the polymerization medium and removable after the formation of the polymer brushes. The use of the polymer gel provides a uniform distribution of the polymerization medium on the surface on which the polymerization initiator is fixed. The use of the polymer gel has the advantageous effect that the swollen polymerization medium (swollen gel) can be easily applied to surfaces with complex shapes and various orientations, since the polymer gel swells in the polymerization medium, thereby allowing the swollen polymerization medium (swollen gel) to adhere better to the surface.
[0019] It has also been surprisingly found that swelling of the polymer gel in the polymerization medium does not interfere with the polymerization reaction (ie, the formation of polymer brushes on the surface).
[0020] The present invention will be more fully understood from the detailed description given in this disclosure. The accompanying drawings are provided for illustrative purposes only and therefore are not intended to limit the present invention. [Brief description of the drawings]
[0021] [Figure 1] FIG. 1 illustrates a method of the present invention in which a surface on which a polymerization initiator is immobilized (first step) is contacted with a polymer gel swollen in a polymerization medium (second step), leading to the development and formation of polymer brushes from the polymerization initiator (third step). [Diagram 2] FIG. 2 illustrates the method of the present invention of contacting a surface with a polymer gel swollen in a polymerization medium (see Example 4) and further shows that the medium can adhere to the surface even when tilted vertically during a 1 hour polymerization. [Diagram 3] Figure 3 visually shows a homogenous polymer brush film only where the polymer gel swollen in the polymerization medium was deposited on the surface (sample in Figure 2 after 1 hour). Along the edges, the aluminum sample still only has immobilized initiator and no polymer brushes have formed. [Figure 4]FIG. 4 shows the swollen polymer gel of Example 5 smeared onto a 10 cm×10 cm stainless steel plate. [Diagram 5] Figure 5 shows the sample after polymerization and cleaning, see Example 5. [Figure 6] FIG. 6 shows the swollen polymer gel of Example 6. [Figure 7] Figure 7 shows the formation of polymer brushes in areas where the swollen polymer gel contacted the polymerization initiator, see Example 6. [Figure 8] FIG. 8 shows the swollen polymer gel of Example 7. [Figure 9] FIG. 9 shows the swollen polymer gel of Example 8. [Figure 10] Figure 10 shows the polymer gel swollen in the polymerization medium (left) and transferred to a plate (right). See Example 10. [Figure 11] Figure 11 shows the IRRAS spectrum after forming the PMMA polymer brush. [Figure 12] Figure 12 shows the polymer gel swollen in the polymerization medium (left) and the swollen polymer gel transferred to a plate (right), see Example 11. [Figure 13] Figure 13 shows the IRRAS spectrum after formation of the PMMA polymer brushes, see Example 11. [Figure 14] Figure 14 shows the polymer gel swollen in the polymerization medium (left) and the swollen polymer gel transferred to a plate (right), see Example 12. [Figure 15] Figure 15 shows the IRRAS spectrum after formation of PMMA polymer brushes, see Example 12. [Figure 16] Figure 16 shows the polymer gel swollen in polymerization medium (left) and transferred to a plate (right), see Example 13. [Figure 17] Figure 17 shows the IRRAS spectrum after formation of PMMA polymer brushes, see Example 13. [Figure 18]Figure 18 shows the polymer gel swollen in polymerization medium (left) and transferred to a plate (right), see Example 14. [Figure 19] Figure 19 shows the IRRAS spectrum after formation of PMMA polymer brushes, see Example 14. [Figure 20] Figure 20 shows the polymer gel swollen in polymerization medium (left) and the swollen polymer gel transferred to a plate (right), see Example 15. [Figure 21] Figure 21 shows the polymer gel swollen in polymerization medium (left) and the swollen polymer gel transferred to a plate (right), see Example 16. [Figure 22] 22 shows the water contact angle between a plate on which the polymer brushes are formed and a water droplet (see Example 16). [Diagram 23] Figure 23 shows the polymer gel swollen in polymerization medium (left) and the swollen polymer gel transferred to a plate (right), see Example 17. [Figure 24] 24 shows the water contact angle between a plate on which the polymer brushes are formed and a water droplet (see Example 17). [Diagram 25] Figure 25 visually illustrates the polymer gel swollen in the polymerization medium (left) and the homogenous polymer brush film only where the polymer gel swollen in the polymerization medium was placed on the surface (right). See Example 18. [Figure 26] Figure 26 shows the IRRAS spectrum after formation of the PGMA polymer brushes, see Example 18. [Figure 27] Figure 27 shows the XPS survey spectrum of PMMA polymer brushes, see Example 21. [Figure 28] Figure 28 shows a high-resolution spectrum of the carbon peaks of PMMA polymer brushes. See Example 21. [Figure 29] Figure 29 shows the XPS survey spectrum of PS polymer brushes, see Example 25. [Diagram 30] Figure 30 shows a high-resolution spectrum of the carbon peaks of PS polymer brushes. See Example 25. [Diagram 31] Figure 31 shows the XPS survey spectrum of PHEMA polymer brushes, see Example 26. [Diagram 32] Figure 32 shows a high-resolution spectrum of the carbon peaks of PHEMA polymer brushes. See Example 26. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0022] The invention and its aspects are described in more detail below.
[0023] The present invention relates to a method of forming polymer brushes on a surface by contacting a surface having a polymerization initiator immobilized thereon with a polymerization medium, in which a polymer gel is swollen in the polymerization medium during the formation of the polymer brushes, after which the polymer gel can be removed from the surface.
[0024] As used herein, the terms "a polymer gel" and "the polymer gel" are intended to include one or more polymer gels. The more than one polymer gel may suitably be two, three, four or five polymer gels.
[0025] The polymer gel applied in the present invention is preferably one which is swellable in water, in a mixture of water and an alcohol, in a mixture of water and an aprotic solvent, or in an aprotic solvent other than the polymerization medium.
[0026] In a preferred embodiment of the invention, the polymer gel is such that the cross-linking of the polymer gel is reversible, and therefore the swelling of the polymer gel in the polymerization medium (swollen gel) can be reversed by an external stimulus.
[0027] The polymer gels used in the present invention are such that they can absorb the organic solvent / water solvent system used in the polymerization medium. The polymer gels used in the present invention are preferably reversible polymer gels, i.e., polymer gels that can change between a gelled form and a liquid form. In particular, the polymer gels used in the methods of the present invention can be hydrogels. Suitable polymer gels are reversibly crosslinked polymer gels having a single network (one type of polymer and crosslinks) or a double network (two types of polymer and crosslinks). Examples of suitable polymer gels include, but are not limited to, polyallylamine (PAH), poly(2-hydroxyethyl methacrylate phosphate ester), polyvinylimidazole, polyacrylic acid, PEG, collagen, gelatin, agarose, and polysaccharides such as chitosan, cyclodextrins (e.g., a combination of β-CD polymer and PEG-cholesterol polymer), alginates, sodium alginate, and xanthan gum, as well as cysteine-based polymer gels. It is expected that xanthan gum will be a very suitable polysaccharide to be used as a polymer gel for the purposes of the present invention. A crosslinking agent for forming a crosslinked polymer gel may be incorporated into the system as part of the polymer gel or may be added as an additive.
[0028] In one embodiment, the polymer gel has metal chelating sites, thereby allowing metal coordination. Incorporation of molecules containing metal chelating sites, such as tannic acid (TA), can provide crosslinking of the polymer with coordination of metal ions, such as Cu(II), Fe(III), and Al(III).
[0029] In another embodiment, cross-linking of the polymer gel relies on hydrophobic interactions, for example, achieved by guest-host interactions (e.g., small hydrophobic molecules with cyclodextrins).
[0030] In another embodiment, the cross-linking of the polymer gel relies on sulfur cross-linking, which then occurs through disulfide bonds generated within one polymer (e.g., polycysteine).
[0031] In another embodiment, the polymer gel has hydrogen bond acceptors and / or donors, whereby cross-linking is facilitated by hydrogen bonds. Examples of this include gelatin and agarose, which are advantageously thermoresponsive polymer gels.
[0032] The polymer gels used in the present invention are preferably reversibly crosslinked. Reversibility is obtained by responsiveness to external stimuli such as pH, temperature, light exposure, sonication, solvent polarity or oxidation potential. One example of a pH-responsive polymer gel is a PAH / TA / Fe(III) polymer gel (hydrogel). At low pH (less than 7), the polymer gel is in liquid form, and at high pH (7 or higher), the polymer gel is dense or semi-solid. Another example is a hydrogel of poly(phosphate 2-hydroxyethyl methacrylate ester), which gels at high pH but liquefies by sonication in water (or at low pH). In particular, the swollen polymer gel can be removable by adjusting pH or temperature, by light exposure, or by changing the polarity of the solvent mixture. In some methods, sonication is performed in a suitable solvent, optionally as a series of rinsing steps.
[0033] One example where cross-linking is driven by hydrophobic interactions is cyclodextrin, which is incorporated into the site chain of one polymer. Another polymer is then designed to have hydrophobic sites. By mixing these two polymers in a hydrophilic environment, gelation occurs. Energetic considerations attract the hydrophobic moieties to the hydrophobic interior of the cyclodextrin, thus driving cross-linking. This bond can be reversed by changing to a solvent of a different polarity.
[0034] After swelling of the polymer gel in the polymerization medium, the resulting medium (gel) is transferred to a surface where the polymer brushes are formed.
[0035] Generally, the formation of the polymer brushes is carried out at room temperature, but it should be understood that other temperatures may be applied. The temperature may be related to the particular method used to form the polymer brushes. Additionally, elevated temperatures may be used as a stimulus to liquefy the polymer gel after polymer brush formation, thereby facilitating removal of the polymer gel.
[0036] Typically, polymer brushes are synthesized by SIP (Surface-Initiated Polymerisation). Examples of suitable methods for forming polymer brushes include ARGET ATRP (Activators Regenerated by Electron Transfer Atom Transfer Radical Polymerisation), conventional ATRP, SARA ATRP (Supplemental Activation Reducing Agent Atom Transfer Radical Polymerisation), and SET LRP (Single-Electron Transfer Living Radical Polymerisation). These methods are well known in the art. Some methods are described in WO 2019 / 196999 A1.
[0037] The ATRP method is a method that generates radicals by an atom transfer process, usually using a transition metal complex as a catalyst and an alkyl halide as a polymerization initiator (RX). At the same time, the transition metal is oxidized to a higher oxidation state. This results in a growing polymer chain from the monomer. The ATRP method requires the following reactants: monomer, (solvent), initiator (immobilized on the surface on which the polymer brush is grown), catalyst, and ligand. In the ARGET ATRP method, a reducing agent such as hydrazine, phenols, sugars, and ascorbic acid is used to regenerate the activator by electron transfer to regenerate Cu(I). In the SARA ATRP method, Cu(0) is used as an auxiliary activator and reducing agent, which directly activates the alkyl halide, which further reduces Cu(II) to Cu(I), thereby regenerating the Cu(I) activator. In the SIP method, an immobilized polymerization initiator is activated by a catalyst in the presence of a monomer to form a polymer brush on the surface. SET-LRP utilizes alkyl halides as initiators, similar to ATRP, ARGET ATRP, and SARA ATRP. In the presence of monomer, (solvent), and ligand, the polymerization is catalyzed by a catalyst derived from the bulk moiety of Cu(0) that provides a constant supply of Cu(0) as catalyst.
[0038] All of the above mentioned methods are suitable for preparing polymer brushes on a surface. These and other methods for forming polymer brushes on a surface not specifically mentioned in this disclosure are equally suitable for the purposes of the present invention.
[0039] Reaction conditions, such as temperature, reaction time, washing, etc., are generally known to those skilled in the art. Similarly, those skilled in the art will know how to select the polymerization medium, i.e., monomers, catalysts / ligands, solvents, etc., required to form the polymer brushes depending on the method of polymer brush formation.
[0040] Generally, the polymerization medium used in the present method includes a solvent or combination of solvents, monomers, ligands, catalysts, and / or activators. In some cases, it may be advantageous to add an activator to the polymer gel prior to swelling of the polymer gel and the polymerization medium. Thereby, the reactants of the polymerization medium are activated only when the polymer gel and the polymerization medium are combined. In some cases, an anti-caking agent, such as sodium bicarbonate or silicon dioxide, may be used to ensure uniform gelation of the polymerization medium. In some cases, a surfactant, such as an anionic, zwitterionic or nonionic surfactant, may be used to facilitate distribution of the polymerization medium through the polymer gel.
[0041] In the present invention, suitable solvents include alcohols such as methanol, ethanol, and isopropanol. Aprotic solvents such as dimethylsulfoxide (DMSO), acetone, dimethylformamide, tetrahydrofuran, propylene carbonate, methylene carbonate, ethylene carbonate, ethyl lactate alcohol, and ionic liquids (salts dissolved in liquids) can also be used in the method of the present invention. The alcohol and / or aprotic solvent is preferably mixed with water in a suitable ratio, for example water and alcohol are preferably mixed in an alcohol / aprotic solvent:water ratio of 5% by volume:95% by volume, 10% by volume:90% by volume, 15% by volume:85% by volume, 20% by volume:80% by volume, 25% by volume:75% by volume, 30% by volume:70% by volume, 35% by volume:65% by volume, 40% by volume:60% by volume, 45% by volume:55% by volume, 50% by volume:50% by volume, 55% by volume:45% by volume, 60% by volume:40% by volume, 65% by volume:35% by volume, 70% by volume:30% by volume, 75% by volume:25% by volume, 80% by volume:20% by volume, 85% by volume:15% by volume, 90% by volume:10% by volume or 5% by volume:95% by volume. In a preferred embodiment, the ratio is 50%:50% alcohol / aprotic solvent:water by volume.
[0042] Examples of suitable monomers include, but are not limited to, acrylates, methacrylates, halogen-substituted alkenes, acrylamides, methacrylamides, and styrenes, and mixtures thereof. Specific acrylate monomers include, but are not limited to, methyl acrylate, ethyl acrylate, and lauryl acrylate. Specific methacrylate monomers include, but are not limited to, methyl methacrylate (MMA), 2-hydroxy-ethyl-methacrylate (HEMA), glycidyl methacrylate (GMA), ethyl methacrylate, butyl methacrylate, and lauryl methacrylate. Specific halogen-substituted alkene monomers include, but are not limited to, vinyl chloride, vinylidene difluoride, tetrafluoroethylene, chlorotrifluoroethylene, and hexafluoropropylene. Specific acrylamide-based monomers include, but are not limited to, acrylamide, N-isopropylacrylamide, N-tert-butylacrylamide, and N-hydroxyethylacrylamide. Specific methacrylamide monomers include, but are not limited to, N-isopropyl methacrylamide, methacrylamide, N-tert-butyl-methacrylate, N-hydroxy-ethyl methacrylate.Specific styrenic monomers include, but are not limited to, styrene, 4-methylstyrene, 2,3,4,5,6-pentafluorostyrene, p-divinylbenzene, and 4-chlorostyrene.
[0043] Examples of suitable ligands include, but are not limited to, nitrogen-containing ligands such as N,N,N',N'',N'''-pentamethyldiethylenetriamine (PMDETA), tris[2-(dimethylamino)ethyl]amine (Me6TREN), tris(2-aminoethyl)amine (TREN), tris(2-pyridylmethyl)amine (TPMA), and 2,2'-bipyridyl (BiPy).
[0044] Examples of suitable catalysts include, but are not limited to, metal catalysts derived from copper (Cu), iron (Fe) and nickel (Ni), with Cu being particularly preferred.
[0045] Examples of suitable activators include, but are not limited to, sodium ascorbate (NaAsc), ascorbic acid (Asc), hydrazine, hydrazine hydrate, sodium hypophosphite, a mixture of iron powder and sodium chloride, bicarbonate, citric acid, and pyrogallic acid, and mixtures thereof. In particular, NaAsc, Asc, and hydrazine are suitable for the purposes of the present invention.
[0046] In the method of the invention, the polymer brushes are formed on a surface, typically on the surface of a solid material. Such surfaces can be suitably made of metals (e.g., aluminum, steel, titanium, nickel, gold, silver, platinum, chromium, copper, iron, and alloys of various metals), glass, carbon, carbon fibers, graphene or graphite, ceramics, composites, or other materials, including plastics, rubber, or outer coatings of such materials. The surface can be conductive or non-conductive. The surface has a polymerization initiator immobilized thereon. Methods for immobilizing the polymerization initiator are well known in the art. The polymerization initiator can have a predetermined surface chemistry to allow immobilization to the surface, depending on the material from which the surface is made, but also on the properties of the polymer brushes to be formed.
[0047] The concentration of each of the components (monomer, ligand, catalyst, activator) is typically in the range of 0.1 nM to 35 M. Specific examples include, but are not limited to, 1 nM, 5 nM, 10 nM, 50 nM, 1 M, 5 M, 10 M, 20 M, and 30 M. It should be understood that the concentration of each component may be the same or different. In certain embodiments, the concentration of the monomer may be 0.01 M to 5 M. In certain embodiments, the concentration of the activator may be 0.010 to 0.045 M. In certain embodiments, the concentration of the ligand is 0.05 mM to 0.1 M. In certain embodiments, the concentration of the solvent is 0.1 to 35 M. In certain embodiments, the concentration of the catalyst is 1.0 ppb to 500.0 ppm.
[0048] In a preferred embodiment of the present invention, the polymer gel is a reversibly crosslinked polymer gel. Such reversible polymer gels can be preferably composed mainly of polymers with specific crosslinkers either incorporated into the polymer side chains or added as additives (e.g., tannic acid) to the polymer gel solution. These crosslinkers can be preferably metal-coordinating, for example, using pyrogallol (tannic acid) structures. The choice of metal coordination is important, since undesired coordination of metals to the metal coordination sites can distort the polymerization reaction and thus the formation of polymer brushes. Preferred polymer gels are those that swell in the polymerization medium.
[0049] In another embodiment of the present invention, the polymer gel is thixotropic. Xanthan gum is a suitable example of a thixotropic polymer gel.
[0050] In the method of the invention, a polymer gel is swollen in a polymerization medium. After swelling, the final polymerization medium typically contains 0.1 to 20% by weight of polymer. The swollen gel is then applied to a surface on which a polymerization initiator is immobilized. The swollen gel can suitably be brushed / painted, laid or poured onto the surface. Polymerization and formation of polymer brushes are then allowed to proceed.
[0051] The surface and the swollen gel (combined polymer gel and polymerization medium) are typically kept in contact with each other for a suitable time, such as, for example, 0.1 seconds to 5 hours. Suitable times include, but are not limited to, 1 second, 2 seconds, 30 seconds, 1 minute, 5 minutes, 30 minutes, 1 hour, 2 hours, 3 hours, 4 hours, and 5 hours. The formation of the polymer brush can be carried out at ambient temperature (room temperature) or may be carried out with cooling or heating. Suitable reaction temperatures are from -20°C to 120°C, such as, for example, from room temperature (about 20°C) to 120°C. Specific temperatures include, but are not limited to, -20°C, 0°C, room temperature (about 20°C), 30°C, 50°C, 60°C, 70°C, 80°C, 90°C, 100°C, 110°C, and 120°C.
[0052] After the formation of the polymer brushes, the swollen gel is removed from the surface. This can be done by sonicating the surface, preferably in an acidic environment, if necessary. An example of a pH-responsive polymer gel is PAH / TA / Fe(III), which is in a liquid phase below pH 7 and in a gel state above pH 7. When the polymer gel is immersed in an acidic solution, such as an HCl solution, the metal coordination changes, which changes the viscosity of the gel and makes it liquid. When the gel is in a liquid state, it can be easily removed from the polymer brushes, for example by sonication.
[0053] The use of polymer gels for the formation of polymer brushes has been shown to achieve a number of advantages. The polymer gel acts as a container for the polymerization medium, providing a stable environment for the formation of the polymer brushes, which can then diffuse freely within the polymer gel and promote the formation of the polymer brushes at the surface. The polymer gel further provides a viscous environment, thereby allowing the formation of polymer brushes on surfaces that are not planar oriented (horizontally aligned) during the formation of the polymer brushes, or on surfaces where the formation of a particular polymer brush is desired. Furthermore, the use of polymer gels during the formation of the polymer brushes minimizes the supply of oxygen during the formation of the polymer brushes, ensuring controlled polymerization. These advantages further enable large-scale production of polymer brush-coated surfaces.
[0054] The present invention therefore further relates to the use of a polymer gel in the formation of a polymer brush to uniformly distribute a polymerization medium over a surface having a polymerization initiator immobilized thereon. The polymer gel and its method of use in the formation of a polymer brush are as described above.
[0055] The use according to the invention involves swelling the polymer gel in a polymerization medium.
[0056] Polymer brushes are useful for many applications such as bonding rubbers, composites and plastics to and between metals and glass for sealing applications, bonding functional thermoplastic materials to glass for sensor applications, efficient bonding of polymer brush coated composite fillers such as carbon fibers, graphene, particles, etc. to a matrix of polymer, e.g., thermoplastic material, to create functional surfaces such as antibacterial, low friction or superhydrophobic self-cleaning surfaces on glass, metals, plastics, etc.
[0057] The invention is further illustrated by the following non-limiting examples. EXAMPLES
[0058] Example 1 Preparation of catalyst / Me6TREN solutions for polymerization media A catalyst / Me6TREN solution (polymerization medium without oxygen scavenger activator and monomer) was prepared in the following manner. 250 ml of DI water (deionized water) and 2.40 ml of N-tris[2-(dimethylamino)ethyl]amine (Me6TREN - acting as ligand) were mixed in a round bottom flask equipped with a copper-wire-wrapped Teflon magnet. The solution was stirred for 8 days to liberate Cu(0) into solution. Cu(0) acts as a dormant / inactive catalyst and can be activated by adding an activator. UV-vis spectroscopy was used to determine the Cu(0) catalyst concentration. The Cu catalyst / Me6TREN stock solution was diluted with water to obtain catalyst concentrations of 73 mg / l, 93.8 mg / l, 333 mg / l or 427 mg / l.
[0059] Example 2 Preparation of catalyst / PMDETA solutions for polymerization media A catalyst / PMDETA stock solution (polymerization medium without polymerization activator) was prepared as follows: 2000 ml of DI water (deionized water) and 44 ml of N,N,N',N'',N''-pentamethyldiethylenetriamine (PMDETA - acting as a ligand) were mixed in an Erlenmeyer flask. Using a peristaltic pump and silicone tubing, this solution was passed through a Cu tube (10 m long, 2.8 mm inner diameter, 4 mm outer diameter) at a flow rate of 10 ml / min. This resulted in liberating Cu(0) into the solution. Cu(0) acts as a dormant / inactive catalyst and can be activated by the addition of an activator. UV-vis spectroscopy was used to determine the Cu(0) catalyst concentration. The Cu catalyst / PMDETA stock solution was then diluted with DI water to obtain a catalyst concentration of approximately 30 mg / l.
[0060] Example 3 pH-Responsive Polymer Gels: Preparation of Poly(2-hydroxyethyl methacrylate phosphate ester) 2.27 g of 2-hydroxyethyl methacrylate phosphate ester (monomer) was combined with 8 ml of the catalyst / PDETA stock solution from Example 2 and 10 μL of ethyl α-bromoisobutyrate (initiator). The solution was purged with argon for 5 minutes. 32.7 mg of sodium ascorbate (NaAsc, activator) was added and the solution was purged for another 5 minutes. The reaction was allowed to proceed overnight. The polymer was isolated by suction filtration and washed briefly with water, followed by ethanol. This cleaning step removes, for example, excess NaAsc. This resulted in a non-swollen polymer gel, poly(2-hydroxyethyl methacrylate phosphate ester).
[0061] Example 4 Formation of polymer brushes using the polymer gel, poly(2-hydroxyethyl methacrylate phosphate ester) Poly(2-hydroxyethyl methacrylate phosphate ester) gel (prepared in Example 3) was swelled in the polymerization medium to produce polyacrylamide brushes, and the resulting gel was applied to a surface on which a polymerization initiator was immobilized (see below) to form a polyacrylamide brush.
[0062] First, a polymerization medium (without oxygen scavenger as an activator) was prepared by mixing 4 ml of DI water, 50 μl of Me6TREN / catalyst stock solution (prepared in Example 1) and 0.29 g of acrylamide. Next, the polymer gel was swollen in the polymerization medium by dissolving 195.5 mg of poly(phosphate 2-hydroxyethyl methacrylate ester) of Example 3 in 1 ml of the polymerization medium by ultrasonication for 5 minutes. At this stage, the polymer gel solution combined with the polymerization medium was acidic and therefore in its liquid form. To gel the polymer gel, the pH of the solution was increased to above pH 7 by adding NaOH solution. It is noteworthy that the polymerization medium was simultaneously activated by adding the oxygen scavenger activator NaAsc (sodium ascorbate) combined with the NaOH solution, allowing the formation of polymer brushes. Therefore, 10.2 mg of NaAsc was added to 1 ml of 1 M NaOH, and this solution was added to the solution of polymer gel in the polymerization medium.
[0063] The polymer gel (mixed with the polymerization medium) started to gel within 3 minutes. A pea-sized piece of gel was placed on a 25x25mm aluminum plate on which a polymerization initiator (3-(trimethoxysilyl)propyl 2-bromo-2-methylpropanoate deposited on the aluminum) was fixed. The swollen polymerization medium (combination of polymerization medium and polymer gel) was smeared onto the plate. This is shown in Figure 2. As can be seen from Figure 2, the adhesion of the swollen gel (swollen polymerization medium) to the plate was good and the gel remained in place even when tilted vertically as shown.
[0064] The swollen polymer gel in the polymerization medium was left at room temperature for 1 hour to develop polymer brushes on the surface. The polymer gel / polymerization medium was then removed by sonicating the plate in water for 10 minutes. The sonication "dissolved" the swollen polymer gel, i.e., it became liquid (the swollen gel was reversible). The plate was then cleaned by sonication in acetone for 10 minutes to remove physisorbed material.
[0065] The formation of a homogeneous polymer brush coating was observed only in the areas where the polymer gel / polymerization medium was in contact with the surface (visually confirmed, shown in Figure 3). The distinction between the two distinct regions was also confirmed by water contact angle measurements.
[0066] Example 5 Formation of polymer brushes on large stainless steel substrates using a polymer gel, poly(2-hydroxyethyl methacrylate phosphate ester) This example is similar to the previous Example 4 in that polyacrylamide brushes were formed by swelling a poly(2-hydroxy-ethyl methacrylate phosphate ester) gel (the polymer gel prepared in Example 3) in a polymerization medium to produce a polyacrylamide brush, and applying the resulting gel to a surface on which a polymerization initiator was immobilized (see below). However, in this example, it was applied to a large stainless steel plate to demonstrate the scalability of the method.
[0067] First, a polymerization medium (without oxygen scavenger as an activator) was prepared by mixing 4 ml of DI water, 50 μl of Me6TREN / catalyst stock solution (prepared in Example 1), and 0.31 g of acrylamide. Next, the polymer gel was swollen in the polymerization medium by dissolving 603 mg of poly(phosphate 2-hydroxyethyl methacrylate ester) of Example 3 in 2 ml of the polymerization medium by sonication for 5 minutes. At this stage, the polymer gel solution combined with the polymerization medium was acidic and therefore in its liquid form. To gel the polymer gel, the pH of the solution was increased to above pH 7 by adding NaOH solution. It is noteworthy that the polymerization medium was simultaneously activated by adding the oxygen scavenger activator NaAsc combined with the NaOH solution, allowing the formation of polymer brushes. Therefore, 11.9 mg of NaAsc was added to 2 ml of 1 M NaOH, and this solution was added to the solution of polymer gel in the polymerization medium.
[0068] The polymer gel (mixed with the polymerization medium) started to gel within 3 minutes. The gel was placed on a 100×100 mm stainless steel plate on which a polymerization initiator (3-(trimethoxysilyl)propyl 2-bromo-2-methylpropanoate deposited on stainless steel) was fixed. The polymer gel swollen in the polymerization medium was smeared on multiple portions of the plate. This is shown in FIG. 4.
[0069] The swollen polymerization medium / polymer gel was left to react at room temperature for 1 hour. The polymer gel / polymerization medium was then removed by sonicating the plate in water for 10 minutes. The sonication "dissolved" the swollen polymer gel, i.e., it became liquid (the swollen gel was reversible). The plate was then cleaned by sonication in acetone for 10 minutes to remove physisorbed material.
[0070] A homogeneous polymer brush coating was observed to form only in the areas where the swollen polymerization medium was in contact with the surface, as confirmed by spraying water on the surface and observing that the surface was wet only in the coated areas, as shown in Figure 5. The distinction between the two different areas was also confirmed by water contact angle measurements.
[0071] Example 6 Formation of polymer brushes using polymer gel, PAH / TA / Fe(III) Poly(glycidyl methacrylate) brushes were formed by swelling the PAH / TA / Fe(III) polymer gel in the polymerization medium to produce poly(glycidyl methacrylate) brushes, where the PAH was purchased (while the poly(2-hydroxyethyl methacrylate phosphate ester) used in Examples 3 and 4 was synthesized).
[0072] First, a polymerization medium was prepared by mixing 172 μl DI water, 172 μl EtOH, 100 μl PMDETA / catalyst stock solution (prepared in Example 2) and 52 μl glycidyl methacrylate. Next, a PAH / TA / Fe(III) polymer gel was prepared by mixing 0.5 ml 40% PAH in water, 15.9 mg tannic acid and 0.17 ml 0.00865 M FeCl3 in DI water. The polymerization medium and the polymer gel were then combined to obtain a dark blue solution. At this stage, the polymer gel combined with the polymerization medium was acidic and therefore in its liquid form.
[0073] To gel the polymerization medium combined with the polymer gel (i.e., the swollen polymerization medium / polymer gel), the pH of the solution was raised to above pH 7 by adding NaOH solution. The polymerization medium was simultaneously activated by adding the oxygen scavenger activator NaAsc combined with the NaOH solution, allowing the formation of polymer brushes. Therefore, 5.5 mg of NaAsc was added to 0.33 ml of 1 M NaOH, and this solution was added to the combined polymer gel and polymerization medium. This resulted in the polymer gel swelling in the polymerization medium to form a polymer gel containing the polymerization medium, resulting in a dark red dense solution.
[0074] The swollen polymer gel / polymerization medium was placed on a 25×25 mm aluminum plate onto which the polymerization initiator (3-(trimethoxysilyl)propyl 2-bromo-2-methylpropanoate deposited on aluminum) was immobilized, as shown in FIG.
[0075] After 1 h of polymerization, the plate with the swollen polymer gel was immersed in 0.01 M HCl and sonicated for 10 min. The acidic pH was the stimulus to "dissolve" the swollen polymer gel, i.e., the medium became liquid (swelling is reversible). The plate was then sonicated for 10 min, first in water and then in acetone, to remove physisorbed material.
[0076] The formation of a homogeneous polymer brush coating was observed only in the area where the polymerization medium containing the polymer gel was in contact with the surface, as confirmed by optical microscopy and shown in Figure 7. The distinction between the two distinct areas was also confirmed by water contact angle measurements.
[0077] In FIG. 7, a clear boundary can be seen between the polymer brush-coated areas, where the polymerization medium and polymer gel were in contact with the surface, and the blank aluminum substrate, where only the initiator was immobilized.
[0078] Example 7 Formation of polymer brushes using polymer gels, PAH / TA / Fe(III) in a more dense form This example is similar to Example 6 above in that poly(glycidyl methacrylate) polymer brushes were formed by swelling a PAH / TA / Fe(III) polymer gel in the polymerization medium to produce poly(glycidyl methacrylate) polymer brushes. In this example, a denser swollen gel (polymer gel and polymerization medium) was obtained by adding a smaller amount of polymerization medium.
[0079] First, a polymerization medium (not yet containing an oxygen scavenger as a polymerization activator) was prepared by mixing 104 μl DI water, 104 μl EtOH, 60 μl PMDETA / catalyst stock solution (prepared in Example 2), and 31 μl glycidyl methacrylate. Next, a PAH / TA / Fe(III) polymer gel was prepared by mixing 0.5 ml of 40% PAH in water, 14.8 mg tannic acid, and 0.17 ml of 0.00865 M FeCl3 in DI water. The polymerization medium and the polymer gel were then combined to obtain a dark blue solution in which the polymer gel was swollen by the polymerization medium. At this stage, the polymer gel combined with the polymerization medium was acidic and therefore in its liquid form.
[0080] To gel this mixture, the pH of the solution was raised to above pH 7 by adding NaOH solution. It is noteworthy that the addition of the oxygen scavenger activator NaAsc combined with the NaOH solution simultaneously activated the polymerization medium, allowing the formation of polymer brushes. Therefore, 4.3 mg of NaAsc was added to 0.33 ml of 1 M NaOH, and this solution was added to the mixture of polymer gel and polymerization medium. This resulted in a dark red dense solution of the polymerization medium contained in the polymer gel.
[0081] This swollen gel (a combination of polymer gel and polymerization medium) was placed on a 25x25mm aluminum plate onto which the polymerization initiator (3-(trimethoxysilyl)propyl 2-bromo-2-methylpropanoate deposited on the aluminum) was fixed. The medium was so dense that the sample could be placed vertically while the medium remained fixed. This is shown in Figure 8.
[0082] After 1 hour of polymerization, the plate with swollen polymer gel / polymerization medium was immersed in 0.01M HCl and sonicated for 10 minutes. The acidic pH was the stimulus to "dissolve" the gelation medium, i.e., it became liquid. The plate was then sonicated for 10 minutes, first in water and then in acetone, to remove physisorbed material.
[0083] The formation of a homogeneous polymer brush coating was observed only in the areas where the swollen dense polymer gel was in contact with the surface (as confirmed by optical microscopy), and the distinction between the two distinct regions was also confirmed by water contact angle measurements.
[0084] Furthermore, it was concluded that even when using a very dense swollen gel of polymerization medium and polymer gel, the components of the medium were indeed able to react with the polymerization initiator immobilized on the surface. Thus, the components important for the formation of the polymer brushes were freely accessible for the formation of the polymer brushes.
[0085] Example 8 Formation of polymer brushes using polymer gels, PAH / TA / Fe(III) in a more dense form This example is similar to Examples 6 and 7 in that poly(glycidyl methacrylate) brushes were formed by swelling a PAH / TA / Fe(III) polymer gel in the polymerization medium to produce poly(glycidyl methacrylate) polymer brushes, but in this example, a smaller amount of polymerization medium was added to obtain a denser swollen gel (polymer gel and polymerization medium).
[0086] First, a polymerization medium was prepared by mixing 35 μl DI water, 35 μl EtOH, 20 μl PMDETA / catalyst stock solution (prepared in Example 2) and 10 μl glycidyl methacrylate (but not yet containing a polymerization activator). Next, a PAH / TA / Fe(III) polymer gel was prepared by mixing 0.5 ml of 40% PAH in water, 14.1 mg tannic acid and 0.17 ml of 0.00865 M FeCl3 in DI water. The polymerization medium and the polymer gel were then combined to obtain a dark blue solution. At this stage, the polymer gel combined with the polymerization medium was acidic and therefore in its liquid form.
[0087] To gel the polymer gel and polymerization medium, the pH of the solution was raised to above pH 7 by adding NaOH solution. It is noteworthy that the addition of oxygen scavenger activator NaAsc combined with NaOH solution simultaneously activated the polymerization medium, allowing the formation of polymer brushes. Therefore, 4.6 mg of NaAsc was added to 0.33 ml of 1 M NaOH, and this solution was added to the combination of polymer gel and polymerization medium. This resulted in a dark red dense solution due to the formation of a semi-solid form of swollen polymer gel.
[0088] The swollen polymerization medium / polymer gel was placed on a 25x25mm aluminum plate onto which the polymerization initiator (3-(trimethoxysilyl)propyl 2-bromo-2-methylpropanoate deposited on aluminum) was fixed. The medium was so dense that the sample could be placed vertically while the medium remained fixed. This is shown in Figure 9.
[0089] After 1 hour of polymerization, the plate was immersed in 0.01M HCl and sonicated for 10 minutes. The acidic pH was the stimulus to "dissolve" the swollen polymerization medium / polymer gel, i.e., it became liquid. Then, to remove the bioadsorbates, the plate was sonicated first in water for 10 minutes and then in acetone for 10 minutes.
[0090] The formation of a homogeneous polymer brush coating was observed only in the areas where the gelled polymer gel (polymerization medium and polymer gel) was in contact with the surface (as confirmed by optical microscopy), and water contact angle measurements also confirmed the difference between the two distinct regions.
[0091] Furthermore, it was concluded that even in the denser swollen gels, components of the medium were indeed able to react with the surface-immobilized initiator, and thus the components important for polymer brush formation were freely accessible for polymer brush formation.
[0092] Example 9 Preparation of sodium alginate polymer gel Various polymer gels of sodium alginate were prepared by mixing 4 g, 5 g, 6 g and 8 g of sodium alginate in 100 ml of DI water to form 4 w%v%, 5 w% / v%, 6 w% / v% and 8 w% / v% sodium alginate polymer gels, respectively. The resulting polymer gels were viscous liquids in all cases.
[0093] Example 10 Formation of polymer brushes using sodium alginate polymer gel in a 14% ethanol solvent system First, a polymer gel was prepared by dissolving 150.1 mg of sodium ascorbate (NaAsc, activator) in 17 ml of sodium alginate solution (4 w% / v%) prepared according to Example 9. The mixture became a light brown thick liquid. The activator-containing polymer gel was stored in a container.
[0094] In a separate vessel, 1.6 ml of methyl methacrylate (MMA) was mixed with 7.1 ml of the Cu catalyst / Me6TREN solution ([Cu]=93.8 mg / l) and 4.3 ml of ethanol to form the polymerization medium.
[0095] The polymerization medium was poured into the sodium alginate polymer gel under stirring. Upon mixing, the solution turned light blue, and after about 5 minutes the mixture turned white. Thus, the polymer gel was swelled in the polymerization medium.
[0096] The resulting polymer gel swollen in the polymerization medium was transferred to a 10x10mm stainless steel plate (304 steel alloy) on which the polymerization initiator (4-(chloromethyl)phenyltrimethoxysilane deposited on the stainless steel) was fixed. The polymer gel swollen in the polymerization medium was very dense and covered the plate well and uniformly. The plate was left for 10 minutes to allow the formation of polymer brushes on the plate. The plate was then placed in a beaker of DI water. The change in polarity of the solvent was the stimulus to "dissolve" the swollen polymer gel / polymerization medium and remove it from the plate. The plate was further rinsed by sonication in water for 5 minutes, followed by sonication in acetone for 5 minutes.
[0097] The formed polymer brushes were determined to have a thickness of 57±7 nm by ellipsometry. The macromolecular structure of the formed polymer brushes was further confirmed by infrared reflection absorption spectroscopy (IRRAS).
[0098] Figure 10 shows the polymer gel swollen in the polymerization medium (left) and the swollen polymer gel transferred to a plate (right). Figure 11 shows the IRRAS spectrum after the formation of the polymer brush. Importantly, the peaks at 2974, 1739, 1273, 1244, 1195 and 1153 cm -1 The peaks at 10 and 11 confirm the presence of sp3 hybridized carbon-hydrogen, carbonyl, and carbon-oxygen bonds, respectively, consistent with those expected for PMMA polymer brushes.
[0099] Example 11 Formation of polymer brushes using sodium alginate polymer gel in a 63% ethanol solvent system The procedure was carried out as described in Example 10 using 150 mg of sodium ascorbate (active agent) and 17 ml of sodium alginate solution (4 w% / v%) prepared according to Example 9. The mixture became a light brown thick liquid. The active agent-loaded polymer gel was stored in a container.
[0100] 1.6 ml of methyl methacrylate (MMA) was mixed with 2 ml of Cu catalyst / Me6TREN solution ([Cu]=333 mg / l) and 9.4 ml of ethanol to form the polymerization medium.
[0101] The polymerization medium was poured into the sodium alginate polymer gel under stirring. Upon mixing, the solution turned pale blue, and after about 5 minutes the mixture turned pale yellow. Thus, the polymer gel was swollen in the polymerization medium.
[0102] The resulting polymer gel swollen in the polymerization medium was transferred to a 10x10mm stainless steel plate (304 steel alloy) on which the polymerization initiator (4-(chloromethyl)phenyltrimethoxysilane deposited on the stainless steel) was fixed. The polymer gel swollen in the polymerization medium was very dense and covered the plate well and uniformly. The plate was left for 10 minutes to allow the formation of polymer brushes on the plate. The plate was then placed in a beaker of DI water. The change in the polarity of the solvent was the stimulus to "dissolve" the swollen polymer gel and remove it from the plate. The plate was further rinsed by ultrasonication in water for 5 minutes, followed by ultrasonication in acetone for 5 minutes.
[0103] The formed polymer brushes were determined to have a thickness of 78±7 nm by ellipsometry. The macromolecular structure of the formed polymer brushes was further confirmed by infrared reflection absorption spectroscopy (IRRAS).
[0104] Figure 12 shows the polymer gel swollen in the polymerization medium (left) and the swollen polymer gel transferred to the plate (right). Figure 13 shows the IRRAS spectrum after the formation of the polymer brush. Importantly, the peaks at 2974, 1741, 1271, 1243, 1197 and 1154 cm -1 The peaks at 10 and 11 confirm the presence of sp3 hybridized carbon-hydrogen, carbonyl, and carbon-oxygen bonds, respectively, consistent with those expected for PMMA polymer brushes.
[0105] Example 12 Formation of sodium alginate polymer gels and polymer brushes using aprotic solvents as polymerization media. 150.3 mg of sodium ascorbate (active agent) was dissolved in 17 ml of sodium alginate polymer gel (5 w% / v%) and the procedure was carried out as in Example 10. The mixture was stirred to obtain a light brown thick liquid.
[0106] The polymerization medium was a mixture of 1.5 ml of Cu catalyst / Me6TREN solution ([Cu]=427 mg / l), 1.6 ml of methyl methacrylate (MMA) mixed with 0.5 ml of DI water and 9.4 ml of DMSO solvent.
[0107] The polymerization medium was poured into the polymer gel / activator liquid and stirred. Upon mixing, the combined solution turned pale blue in color, and after approximately 5 minutes the combined solution became thick and clear.
[0108] The polymerized gel swollen in the polymerization medium was transferred to a 10×10 mm stainless steel plate (304 steel alloy) on which the polymerization initiator (4-(chloromethyl)phenyltrimethoxysilane deposited on stainless steel) was fixed and left for 10 min for the conversion of the polymer brushes. The plate was rinsed as described in Example 10.
[0109] The formed polymer brushes were determined to have a thickness of 64±32 nm by ellipsometry. The macromolecular structure of the formed polymer brushes was further confirmed by infrared reflection absorption spectroscopy (IRRAS).
[0110] Figure 14 shows the polymer gel swollen in the polymerization medium (left) and the swollen polymer gel transferred to a plate (right). Figure 15 shows the IRRAS spectrum after the formation of the polymer brush. Importantly, the peaks at 2967, 1741, 1273, 1243, 1197 and 1154 cm -1 The peaks at 10 and 11 confirm the presence of sp3 hybridized carbon-hydrogen, carbonyl, and carbon-oxygen bonds, respectively, consistent with those expected for PMMA polymer brushes.
[0111] Example 13 Formation of polymer brushes using 5 w% / v% sodium alginate polymer gel in ethanol solvent The procedure was carried out similarly to Example 10, using 150 mg of sodium ascorbate (active agent) dissolved in 17 ml of sodium alginate polymer gel (5 w% / v%). The mixture was stirred to obtain a light brown thick liquid.
[0112] The polymerization medium was a mixture of 1.5 ml of Cu catalyst / Me6TREN solution ([Cu]=427 mg / l), 1.6 ml of methyl methacrylate (MMA) mixed with 0.5 ml of DI water and 9.4 ml of ethanol solvent.
[0113] The polymerization medium was poured into the polymer gel / activator solution and stirred. Upon mixing, the combined solution turned light blue, and after about 5 minutes, the combined solution became a bright white dense gel. The polymerization gel swollen in the polymerization medium was transferred to a 10×10 mm stainless steel plate (304 steel alloy) on which the polymerization initiator (4-(chloromethyl)phenyltrimethoxysilane deposited on stainless steel) was fixed and left for 10 minutes for conversion of the polymer brushes. The plate was rinsed as described in Example 10.
[0114] The formed polymer brushes were determined to have a thickness of 64±6 nm by ellipsometry. The macromolecular structure of the formed polymer brushes was further confirmed by infrared reflection absorption spectroscopy (IRRAS).
[0115] Figure 16 shows the polymer gel swollen in the polymerization medium (left) and the swollen polymer gel transferred to a plate (right). Figure 17 shows the IRRAS spectrum after the formation of the polymer brush. Importantly, the peaks at 2974, 1739, 1273, 1243, 1197 and 1154 cm -1 The peaks at 10 and 11 confirm the presence of sp3 hybridized carbon-hydrogen, carbonyl, and carbon-oxygen bonds, respectively, consistent with those expected for PMMA polymer brushes.
[0116] Example 14 Formation of polymer brushes using 6 w% / v% sodium alginate polymer gel in ethanol solvent The procedure was carried out similarly to Example 10, using 150 mg of sodium ascorbate (active agent) dissolved in 17 ml of sodium alginate polymer gel (6 w% / v%). The mixture was stirred to obtain a light brown thick liquid.
[0117] The polymerization medium was a mixture of 1.5 ml of Cu catalyst / Me6TREN solution ([Cu]=427 mg / l), 1.6 ml of methyl methacrylate (MMA) mixed with 0.5 ml of DI water and 9.4 ml of ethanol solvent.
[0118] The polymerization medium was poured into the polymer gel / activator solution and stirred. Upon mixing, the combined solution turned light blue, and after about 5 minutes, the combined solution became a bright white dense gel. The polymerization gel swollen in the polymerization medium was transferred to a 10×10 mm stainless steel plate (304 steel alloy) on which a polymerization initiator (4-(chloromethyl)phenyltrimethoxysilane deposited on stainless steel) was fixed and left for 10 minutes for the formation of polymer brushes. The plate was rinsed as described in Example 10.
[0119] The formed polymer brushes were determined to have a thickness of 56±10 nm by ellipsometry. The macromolecular structure of the formed polymer brushes was further confirmed by infrared reflection absorption spectroscopy (IRRAS).
[0120] Figure 18 shows the polymer gel swollen in the polymerization medium (left) and the swollen polymer gel transferred to a plate (right). Figure 19 shows the IRRAS spectrum after the formation of the polymer brush. Importantly, the peaks at 2974, 1739, 1273, 1243, 1197 and 1154 cm -1 Peaks at 100 nm and 150 nm confirm the presence of sp3 hybridized carbon-hydrogen, carbonyl, and carbon-oxygen bonds, respectively, consistent with those expected for PMMA brushes.
[0121] Example 15 Formation of polymer brushes using 8 w% / v% sodium alginate polymer gel in ethanol solvent The procedure was carried out similarly to Example 10, using 150 mg of sodium ascorbate (active agent) dissolved in 17 ml of sodium alginate polymer gel (8 w% / v%). The mixture was stirred to obtain a light brown thick liquid.
[0122] The polymerization medium was a mixture of 1.5 ml of Cu catalyst / Me6TREN solution ([Cu]=427 mg / l), 1.6 ml of methyl methacrylate (MMA) mixed with 0.5 ml of DI water and 9.4 ml of ethanol solvent.
[0123] The polymerization medium was poured into the polymer gel / activator liquid and stirred. Upon mixing, the combined solution turned pale blue, and after approximately 5 minutes the combined solution became a white thick gel.
[0124] The polymerized gel swollen in the polymerization medium was transferred to a 10×10 mm stainless steel plate (304 steel alloy) on which the polymerization initiator (4-(chloromethyl)phenyltrimethoxysilane deposited on stainless steel) was fixed and left for 10 min for the formation of polymer brushes. The plate was rinsed as described in Example 10.
[0125] The formed polymer brushes were determined to have a thickness of 37±10 nm by ellipsometry. The macromolecular structure of the formed polymer brushes was further confirmed by infrared reflection absorption spectroscopy (IRRAS).
[0126] FIG. 20 shows a polymer gel swollen in polymerization medium (left) and the swollen polymer gel transferred to a plate (right).
[0127] Example 16 Formation of poly(styrene) polymer brushes using sodium alginate polymer gels The procedure was carried out similarly to Example 10, using 150.2 mg of sodium ascorbate (active agent) dissolved in 17 ml of sodium alginate polymer gel (5 w% / v%). The mixture was stirred to give a light brown thick liquid.
[0128] The polymerization medium was a mixture of 1.5 ml of Cu catalyst / Me6TREN solution ([Cu]=427 mg / l), 1.6 ml of styrene (monomer) mixed with 0.5 ml of DI water and 9.4 ml of ethanol solvent. This polymerization medium was poured into the polymer gel / activator solution and stirred. Upon mixing, the combined solution turned a light blue color, and after approximately 5 minutes the combined solution became a white thick gel.
[0129] The polymerized gel swollen in the polymerization medium was transferred to a 10×10 mm stainless steel plate (304 steel alloy) on which the polymerization initiator (4-(chloromethyl)phenyltrimethoxysilane deposited on stainless steel) was fixed and left for 10 min for the formation of polymer brushes. The plate was rinsed as described in Example 10.
[0130] The formed polymer brushes were determined to have a thickness of 10 ± 2 nm by ellipsometry. Water contact angle measurements after polymerization determined a water contact angle of 84°, confirming that the surfaces of the plates with the polymer brushes were hydrophobic, consistent with PS.
[0131] Figure 21 shows the polymer gel swollen in the polymerization medium (left) and the swollen polymer gel transferred to a plate (right). Figure 22 shows the water contact angle between the plate and the water droplet.
[0132] Example 17 Formation of PHEMA polymer brushes using sodium alginate polymer gel The procedure was carried out similarly to Example 10, using 150.2 mg of sodium ascorbate (active agent) dissolved in 17 ml of sodium alginate polymer gel (5 w% / v%). The mixture was stirred to give a light brown thick liquid.
[0133] The polymerization medium was a mixture of 1.5 ml of Cu catalyst / Me6TREN solution ([Cu]=427 mg / l), 1.6 ml of 2-(hydroxyethyl)-methacrylate (HEMA) (monomer) mixed with 0.5 ml of DI water and 9.4 ml of ethanol solvent. This polymerization medium was poured into the polymer gel / activator solution and stirred. Upon mixing, the combined solution turned pale blue, and after approximately 5 minutes the combined solution became a white thick gel.
[0134] The polymerized gel swollen in the polymerization medium was transferred to a 10×10 mm stainless steel plate (304 steel alloy) on which the polymerization initiator (4-(chloromethyl)phenyltrimethoxysilane deposited on stainless steel) was fixed and left for 10 min for the formation of polymer brushes. The plate was rinsed as described in Example 10.
[0135] The formed polymer brushes were determined to have a thickness of 5±7 nm by ellipsometry. Water contact angle measurements after polymerization determined a water contact angle of 29°, confirming that the surface of the plate with the polymer brushes was hydrophobic, consistent with PHEMA.
[0136] Figure 23 shows the polymer gel swollen in the polymerization medium (left) and the swollen polymer gel transferred to a plate (right). Figure 24 shows the water contact angle between the plate and a water droplet.
[0137] Example 18 Formation of PGMA polymer brushes using sodium alginate polymer gels 18 mg of sodium ascorbate (active agent) was dissolved in 2 ml of sodium alginate polymer gel (4 w% / v%). The mixture was stirred.
[0138] The polymerization medium was a mixture of 104 μl of glycidyl methacrylate (GMA) (monomer) mixed with 135 μl of Cu-catalyst / Me6TREN solution ([Cu]=427 mg / l) and 624 μl of ethanol solvent. 1136 μl of the combined polymer gel / sodium ascorbate solution was transferred to the polymerization solution and stirred. Upon mixing, the combined solution turned pale blue, and after approximately 5 minutes the combined solution became a white dense gel.
[0139] The polymerized gel swollen in the polymerization solution was transferred to a 25×25 mm stainless steel plate (304 steel alloy) on which a polymerization initiator (4-(chloromethyl)phenyltrimethoxysilane deposited on stainless steel) was fixed and left for 30 min for the formation of polymer brushes. The plate was rinsed as described in Example 10.
[0140] The formed polymer brushes were determined to have a thickness of 99±17 nm by ellipsometry. The macromolecular structure of the formed polymer brushes was further confirmed by infrared reflection absorption spectroscopy (IRRAS).
[0141] Figure 25 shows the polymer gel swollen in the polymerization medium (left) and the swollen polymer gel transferred to a plate (right). Figure 26 shows the IRRAS spectrum after the formation of the polymer brush. Importantly, the peaks at 2974, 1737, 1269, 1243, 1173 and 1152 cm -1 The peaks at 908 cm support the presence of sp3 hybridized carbon-hydrogen bonds, carbonyl and carbon-oxygen bonds, respectively. Finally, the peaks at 908 cm -1 Glycidyl epoxy groups were observed at the top and bottom of the PGMA brushes. All of these peaks are consistent with those expected for PGMA polymer brushes.
[0142] Example 19 Preparation of xanthan gum polymer gel Various polymer gels of sodium alginate were prepared by mixing 2g, 3g, 4g, 4.5g and 6g of xanthan gum with 100ml of DI water to form 2w%v%, 3w% / v%, 4w% / v%, 4.5w% / v% and 6w% / v% xanthan gum polymer gels, respectively. The resulting polymer gels were viscous liquids in all cases.
[0143] Example 20 Formation of PMMA polymer brushes using 2 w% / v% xanthan gum 150 mg of sodium ascorbate was dissolved in 17 ml of xanthan gum polymer gel (2 w% / v%) and stirred to give a light brown thick liquid.
[0144] In a separate vessel, 1.6 ml of methyl methacrylate (MMA monomer) was mixed with 1.5 ml of Cu catalyst / Me6TREN-stock solution ([Cu]=427 mg / l), 0.5 mL of water, and 9.4 ml of ethanol (polymerization medium) and poured into the xanthan gum solution under stirring. Upon mixing, the solution (polymer gel swollen in the polymerization medium) became a clear gel.
[0145] The formed polymer gel was transferred to a 10x10mm stainless steel plate (304 steel alloy) on which a polymerization initiator (4-(chloromethyl)phenyltrimethoxysilane deposited on stainless steel) was fixed, and polymerization was carried out for 10 minutes. The plate was then placed in a beaker of DI water. The change in polarity of the solvent was the stimulus to "dissolve" the swollen polymer gel and remove it from the plate. The plate was further rinsed by ultrasonication in water for 5 minutes, followed by ultrasonication in acetone for 5 minutes.
[0146] The polymer brushes formed were determined to have a thickness of 64±6 nm by ellipsometry.
[0147] Example 21 Formation of PMMA polymer brushes using xanthan gum (3 w% / v%) 150 mg of sodium ascorbate was dissolved in 17 ml of xanthan gum solution (3 w% / v%) and stirred to give a light brown thick liquid.
[0148] In a separate vessel, 1.6 ml of methyl methacrylate (MMA monomer) was mixed with 1.5 ml of Cu catalyst / Me6TREN-stock solution ([Cu]=427 mg / l), 0.5 ml of water, and 9.4 ml of ethanol (polymerization medium) and poured into the xanthan gum polymer gel under stirring. Upon mixing, the solution (polymer gel swollen in the polymerization medium) became a clear gel.
[0149] The formed gel was transferred to a 10x10mm stainless steel plate (304 steel alloy) on which a polymerization initiator (4-(chloromethyl)phenyltrimethoxysilane deposited on stainless steel) was fixed, and polymerization was carried out for 10 minutes. The plate was then placed in a beaker of DI water. The change in polarity of the solvent was the stimulus to "dissolve" the swollen polymer gel and remove it from the plate. The plate was further rinsed by sonication in water for 5 minutes, followed by sonication in acetone for 5 minutes.
[0150] The polymer brushes formed were determined to have a thickness of 54±10 nm by ellipsometry. The chemical composition of the PMMA polymer brushes was confirmed by XPS (FIG. 27). Importantly, the peaks at 535 and 287 eV confirm the presence of oxygen and carbon, respectively. The atomic percentage of oxygen of 24.3% and carbon of 75.7% are consistent with the theoretical values for PMMA polymers. FIG. 28 shows a high-resolution spectrum of the carbon peaks demonstrating the chemical structure of the PMMA polymer brushes.
[0151] Example 22 Formation of PMMA polymer brushes using xanthan gum polymer gel (4 w% / v%) 150 mg of sodium ascorbate was dissolved in 17 ml of xanthan gum polymer gel (4 w% / v%) and stirred to give a light brown thick liquid.
[0152] In a separate vessel, 1.6 ml of methyl methacrylate (MMA monomer) was mixed with 1.5 ml of Cu catalyst / Me6TREN-stock solution ([Cu]=427 mg / l), 0.5 ml of water, and 9.4 ml of ethanol (polymerization medium) and poured into the xanthan solution under stirring. Upon mixing, the solution (polymer gel swollen in the polymerization medium) became a clear gel.
[0153] The formed gel was transferred to a 10x10mm stainless steel plate (304 steel alloy) on which a polymerization initiator (4-(chloromethyl)phenyltrimethoxysilane deposited on stainless steel) was fixed, and polymerization was carried out for 10 minutes. The plate was then placed in a beaker of DI water. The change in polarity of the solvent was the stimulus to "dissolve" the swollen polymer gel and remove it from the plate. The plate was further rinsed by sonication in water for 5 minutes, followed by sonication in acetone for 5 minutes.
[0154] The polymer brushes formed were determined to have a thickness of 63±21 nm by ellipsometry.
[0155] Example 23 Formation of PMMA polymer brushes using xanthan gum polymer gel (4.5 w% / v%) 150 mg of sodium ascorbate was dissolved in 17 ml of xanthan gum polymer gel (4.5 w% / v%) and stirred to give a light brown thick liquid.
[0156] In a separate container, 1.6 ml of methyl methacrylate (MMA monomer) was mixed with 1.5 ml of Cu catalyst / Me6TREN-stock solution ([Cu]=427 mg / l), 0.5 ml of water, and 9.4 ml of ethanol (polymerization medium) and poured into the xanthan gum polymer gel under stirring. Upon mixing, the solution became a clear gel.
[0157] The formed gel was transferred to a 10x10mm stainless steel plate (304 steel alloy) on which a polymerization initiator (4-(chloromethyl)phenyltrimethoxysilane deposited on stainless steel) was fixed, and polymerization was carried out for 10 minutes. The plate was then placed in a beaker of DI water. The change in polarity of the solvent was the stimulus to "dissolve" the swollen polymer gel and remove it from the plate. The plate was further rinsed by sonication in water for 5 minutes, followed by sonication in acetone for 5 minutes.
[0158] The PMMA polymer brushes formed were determined to have a thickness of 7±2 nm by ellipsometry.
[0159] Example 24 Formation of PMMA polymer brushes using xanthan gum polymer gel (6 w% / v%) 150 mg of sodium ascorbate was dissolved in 17 ml of xanthan gum polymer gel (6 w% / v%) and stirred to give a light brown thick liquid.
[0160] In a separate vessel, 1.6 ml of methyl methacrylate (MMA monomer) was mixed with 1.5 ml of Cu catalyst / Me6TREN-stock solution ([Cu]=427 mg / l), 0.5 ml of water, and 9.4 ml of ethanol (polymerization medium) and poured into the xanthan gum polymer gel under stirring. Upon mixing, the solution (polymer gel swollen in the polymerization medium) became a clear gel.
[0161] The formed gel was transferred to a 10x10mm stainless steel plate (304 steel alloy) on which a polymerization initiator (4-(chloromethyl)phenyltrimethoxysilane deposited on stainless steel) was fixed, and polymerization was carried out for 10 minutes. The plate was then placed in a beaker of DI water. The change in polarity of the solvent was the stimulus to "dissolve" the swollen polymer gel and remove it from the plate. The plate was further rinsed by sonication in water for 5 minutes, followed by sonication in acetone for 5 minutes.
[0162] The PMMA polymer brushes formed were determined to have a thickness of 50±34 nm by ellipsometry.
[0163] Example 25 Formation of poly(styrene) polymer brushes using xanthan gum polymer gel (4 w% / v%) 150 mg of sodium ascorbate was dissolved in 17 ml of xanthan gum polymer gel (4 w% / v%) and stirred to give a light brown thick liquid.
[0164] In a separate container, 1.6 ml of styrene (monomer) was mixed with 1.5 ml of Cu catalyst / Me6TREN-stock solution ([Cu]=427 mg / l), 0.5 ml of water, and 9.4 ml of ethanol (polymerization medium) and poured into the xanthan gum polymer gel under stirring. Upon mixing, the solution became a clear gel.
[0165] The formed gel was transferred to a 10x10mm stainless steel plate (304 steel alloy) on which a polymerization initiator (4-(chloromethyl)phenyltrimethoxysilane deposited on stainless steel) was fixed, and polymerization was carried out for 10 minutes. The plate was then placed in a beaker of DI water. The change in polarity of the solvent was the stimulus to "dissolve" the swollen polymer gel and remove it from the plate. The plate was further rinsed by sonication in water for 5 minutes, followed by sonication in acetone for 5 minutes.
[0166] The XPS survey analysis is shown in Figure 29. Since no peaks from the sample substrate were observed, it was concluded that a polymer brush thickness of more than 10 nm was achieved (10 nm is the detection limit of XPS). The chemical composition of the poly(styrene) polymer brushes was confirmed by XPS (Figure 31). Importantly, the peaks at 535 and 287 eV confirm the presence of oxygen and carbon, respectively. The atomic percentage of 93.5% for carbon is consistent with PS (a pure carbon-based polymer), with only a small oxygen content (6.5%). Figure 30 shows a high-resolution spectrum of the carbon peaks demonstrating the chemical structure of the poly(styrene) polymer brushes.
[0167] Example 26 Formation of 2-hydroxyethyl methacrylate polymer brushes using xanthan gum polymer gel (4 w% / v%) 150 mg of sodium ascorbate was dissolved in 17 ml of xanthan gum polymer gel (4 w% / v%) and stirred to give a light brown thick liquid.
[0168] In a separate container, 1.6 ml of 2-hydroxyethyl methacrylate (HEMA monomer) was mixed with 1.5 ml of Cu catalyst / Me6TREN-stock solution ([Cu]=427 mg / l), 0.5 ml of water, and 9.4 ml of ethanol (polymerization medium) and poured into the xanthan gum polymer gel under stirring. Upon mixing, the solution (polymer gel swollen in the polymerization medium) became a clear gel.
[0169] The formed gel was transferred to a 10x10mm stainless steel plate (304 steel alloy) on which a polymerization initiator (4-(chloromethyl)phenyltrimethoxysilane deposited on stainless steel) was fixed, and polymerization was carried out for 10 minutes. The plate was then placed in a beaker of DI water. The change in polarity of the solvent was the stimulus to "dissolve" the swollen polymer gel and remove it from the plate. The plate was further rinsed by sonication in water for 5 minutes, followed by sonication in acetone for 5 minutes.
[0170] The XPS survey analysis is shown in Figure 31. Since no peaks from the sample substrate were observed, it was concluded that a polymer brush thickness of more than 10 nm was achieved (10 nm is the detection limit of XPS). The chemical composition of the PHEMA polymer brushes was confirmed by XPS (Figure 31). Importantly, the peaks at 535 and 287 eV confirm the presence of oxygen and carbon, respectively. The atomic percentages of 69.0% for oxygen and 31.0% for carbon are consistent with theoretical values. Figure 32 shows a high-resolution spectrum of the carbon peaks demonstrating the chemical structure of the PHEMA polymer brushes. Some of the embodiments of the invention related to the present invention are given below. [Embodiment 1] 1. A method for forming polymer brushes on a surface, comprising: contacting the surface having the polymerization initiator immobilized thereon with a polymerization medium; The method, wherein a swellable and removable polymer gel is used during formation of the polymer brushes. [Embodiment 2] 2. The method of claim 1, wherein the polymer gel is capable of swelling in the polymerization medium and wherein the polymer gel is removable after formation of the polymer brushes on the surface. [Embodiment 3] 3. The method according to embodiment 1 or 2, wherein the polymer gel is swellable in water, in a mixture of water and an alcohol, or in a mixture of water and an aprotic solvent. [Embodiment 4] 4. The method according to any one of the preceding claims, characterized in that the crosslinking of the polymer gel is reversible. [Embodiment 5] 5. The method according to any one of the preceding claims, characterized in that the polymer gel is polyallylamine (PAH) / tannic acid (TA) / Fe(III), chitosan / TA / Fe(III), collagen / TA / Fe(III), polyvinylimidazole, poly(2-hydroxyethyl methacrylate phosphoric acid ester), or sugars, such as sodium alginate, xanthan gum and cyclodextrin. [Embodiment 6] 5. The method according to any one of the preceding embodiments, wherein the polymer gel has a site for chelating a metal. [Embodiment 7] 7. The method according to any one of the preceding claims, characterized in that the polymer gel is applied to the surface swollen in the polymerization medium. [Embodiment 8] 8. The method according to any one of the preceding embodiments, characterized in that the swollen polymer gel is removable by adjusting the pH or temperature, by exposure to light, or by ultrasonic treatment. [Embodiment 9] Use of a swellable, removable polymer gel in the formation of a polymer brush to uniformly distribute a polymerization medium over a surface having a polymerization initiator immobilized thereon. [Embodiment 10] 10. The use according to embodiment 9, characterized in that the polymer gel is swellable in the polymerization medium and that the polymer gel is removable after formation of the polymer brushes on the surface. [Embodiment 11] Use according to embodiment 8 or 9, characterized in that the polymer gel is polyallylamine (PAH) / tannic acid (TA) / Fe(III), chitosan / TA / Fe(III), collagen / TA / Fe(III), polyvinylimidazole, poly(2-hydroxyethyl methacrylate phosphoric acid ester) or sugars, such as, for example, sodium alginate, xanthan gum and cyclodextrin.
Claims
1. 1. A method for forming polymer brushes on a surface, comprising: contacting the surface having the polymerization initiator immobilized thereon with a polymerization medium; The method, wherein a swellable and removable polymer gel is used during formation of the polymer brushes.
2. 10. The method of claim 1, wherein the polymer gel is swellable in the polymerization medium and the polymer gel is removable after formation of the polymer brushes on the surface.
3. 3. The method according to claim 1 or 2, characterized in that the polymer gel is swellable in water, in a mixture of water and an alcohol, or in a mixture of water and an aprotic solvent.
4. The method according to any one of claims 1 to 3, characterized in that the crosslinking of the polymer gel is reversible.
5. 5. The method according to any one of claims 1 to 4, characterized in that the polymer gel is selected from the group consisting of polyallylamine (PAH) / tannic acid (TA) / Fe(III), chitosan / TA / Fe(III), collagen / TA / Fe(III), polyvinylimidazole, poly(2-hydroxyethyl methacrylate phosphoric acid ester), sugars, and combinations thereof.
6. The method of claim 1, wherein the polymer gel is selected from the group consisting of polyallylamine (PAH) / tannic acid (TA) / Fe(III), chitosan / TA / Fe(III), collagen / TA / Fe(III), polyvinylimidazole, poly(2-hydroxyethyl methacrylate phosphate), sodium alginate, xanthan gum, cyclodextrin, and combinations thereof.
7. The method according to any one of claims 1 to 4, characterized in that the polymer gel has sites for chelating metals.
8. A method according to any one of claims 1 to 7, characterized in that the polymer gel is applied to the surface swollen in the polymerization medium.
9. The method according to any one of claims 1 to 8, characterized in that the swollen polymer gel is removable by adjusting the pH or temperature, by exposure to light or by ultrasonic treatment.
10. Use of a swellable, removable polymer gel in the formation of a polymer brush to uniformly distribute a polymerization medium over a surface having a polymerization initiator immobilized thereon.
11. 11. The use according to claim 10, characterized in that the polymer gel is swellable in the polymerization medium and that the polymer gel is removable after formation of the polymer brushes on the surface.
12. 11. The use according to claim 9 or 10, characterized in that the polymer gel is selected from the group consisting of polyallylamine (PAH) / tannic acid (TA) / Fe(III), chitosan / TA / Fe(III), collagen / TA / Fe(III), polyvinylimidazole, poly(2-hydroxyethyl methacrylate phosphoric acid ester), sugars, and combinations thereof.
13. The use according to claim 9 or 10, characterized in that the polymer gel is selected from the group consisting of polyallylamine (PAH) / tannic acid (TA) / Fe(III), chitosan / TA / Fe(III), collagen / TA / Fe(III), polyvinylimidazole, poly(2-hydroxyethyl methacrylate phosphate), sodium alginate, xanthan gum, cyclodextrin, and combinations thereof.
Citation Information
Patent Citations
Preparation of water-insoluble polymer having definite shape
JP1983045213A
Process for producing water-insoluble polymers of uniform shape from gelled salts of alginic acid
US4520178A
Substrate for polymer brush formation, production method for substrate for polymer brush formation, and precursor liquid for use in production method for substrate for polymer brush formation
WO2019131872A1