Method for manufacturing semi-solidified slurry, method for manufacturing compact, and compact
Patent Information
- Application Number
- JP2023553801
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2021-10-12
- Publication Date
- 2024-11-29
- Estimated Expiration
- 2041-10-12
AI Technical Summary
【0009】 請求項1記載の半凝固スラリーの製造方法によれば、攪拌工程において、溶湯の中に入れた棒を棒の長さ方向に往復運動して溶湯を攪拌するから、高い固相率であっても溶湯が凝固するときの固相と液相とを均質に攪拌し易い。さらに、溶湯の最も固相率の低い部分における固相率が80%以上になるまで攪拌するから、凝固して固相に成長する液相部分を少なくしながら、固相の周りの液相の分布のばらつきを小さくする。よって得られる半凝固スラリーの部位ごとの固相率のばらつきを小さくし、さらに結晶粒の大きさのばらつきを小さくできる。
Smart Images

Figure 0007592186000001 
Figure 0007592186000002 
Figure 0007592186000003
Abstract
Description
[Technical field]
[0001] The present invention relates to a method for producing a semi-solidified slurry, a method for producing a molded body, and the molded body. [Background technology]
[0002] In a method for producing a semi-solidified slurry of a metal consisting of a solid phase and a liquid phase, Patent Document 1 discloses a technique for producing a semi-solidified slurry by swirling and rotating (rotating) a plurality of rods in molten metal. [Prior art documents] [Patent documents]
[0003] [Patent Document 1] JP 2018-15771 A Summary of the Invention [Problem to be solved by the invention]
[0004] In the prior art, the molten metal is stirred by rotating and swirling a rod (spinning), but the solid and liquid phases do not mix sufficiently, resulting in variations in the solid phase ratio at different locations in the resulting semi-solidified slurry.
[0005] The present invention has been made to solve this problem, and an object of the present invention is to provide a method for producing a semi-solidified slurry that can reduce the variation in solid phase ratio from part to part of the semi-solidified slurry, a method for producing a molded body that can reduce the variation in crystal grain size, and the molded body. [Means for solving the problem]
[0006] In order to achieve this object, the method for producing a semi-solidified slurry of the present invention includes a preparation step of putting a molten metal into a bottomed vessel, and a step of pouring the molten metal into the vessel. The lowest solid fraction portion In and a stirring process in which a rod immersed in the molten metal is reciprocated in the length direction of the rod to stir the molten metal until the solid fraction reaches 80% or more.
[0007] The method for producing a green body of the present invention includes a molding step of obtaining a semi-solidified slurry by the above-described method for producing a semi-solidified slurry, and then pressurizing and deforming the semi-solidified slurry to form it.
[0008] The molded body of the present invention is The longest line is drawn among the two points of the outline projected onto a plane perpendicular to the pressure direction, and the longest line is cut along multiple cutting planes that intersect perpendicularly to the line and divide the line into six equal parts. The eutectic area ratio, which is the ratio of the area of the eutectic appearing in a field of view on a specified cross section to the area of the field, is calculated for each field. Measured When the eutectic area fraction is determined, the coefficient of variation obtained by dividing the standard deviation of the eutectic area fraction by the average value of the eutectic area fraction is 0.15 or less. Effect of the Invention
[0009] According to the method for producing a semi-solidified slurry described in claim 1, in the stirring step, the rod placed in the molten metal is reciprocated in the direction of the length of the rod to stir the molten metal, so that even if the molten metal has a high solid fraction, the solid and liquid phases can be easily stirred homogeneously when the molten metal solidifies. In the area with the lowest solid fraction The mixture is stirred until the solid fraction reaches 80% or more, which reduces the amount of liquid that solidifies and grows into a solid phase, while minimizing the variation in the distribution of the liquid around the solid phase. This reduces the variation in the solid fraction of each part of the resulting semi-solidified slurry, and also reduces the variation in the size of the crystal grains.
[0010] According to the method for producing a semi-solidified slurry described in claim 2, since the position perpendicular to the length direction of the rod when the rod reciprocates is different from the previous position in the method for producing a semi-solidified slurry described in claim 1, it is easy to homogeneously mix the solid phase and liquid phase when the molten metal solidifies at multiple positions perpendicular to the length direction of the molten metal, and therefore it is possible to further reduce the variation in the solid phase ratio at each part of the obtained semi-solidified slurry.
[0011] According to the method for producing a semi-solidified slurry described in claim 3, in the method for producing a semi-solidified slurry described in claim 1 or 2, in a cross section perpendicular to the longitudinal direction of the rods, a plurality of rods are present at intervals from each other, and the center of one of the two adjacent rods is located within a circle whose radius is 7 times the thickness of the other rod and whose center is the center of the other rod, so that the reciprocating motion of the rods affects the molten metal between the rods, and the solid phase and liquid phase are easily stirred homogeneously when the molten metal solidifies. This makes it possible to further reduce the variation in the solid fraction at each part of the obtained semi-solidified slurry.
[0012] According to the method for producing a semi-solidified slurry of claim 4, in the method for producing a semi-solidified slurry of any one of claims 1 to 3, an electromagnetic stirring step is provided prior to or simultaneously with the stirring step, so that the crystal grain size of the obtained semi-solidified slurry can be further reduced by the electromagnetic stirring step.
[0013] According to the method for producing a green body described in claim 5, a semi-solidified slurry having small variations in solid fraction and small variations in crystal grain size from one part to another can be obtained by the method for producing a semi-solidified slurry described in any one of claims 1 to 4. This semi-solidified slurry is pressurized, deformed, and formed, so that a green body having stable yield strength can be obtained in every part.
[0014] According to the molded article of claim 6, The longest line segment is drawn among the lines connecting two points of the outline projected onto a plane perpendicular to the pressure direction, and the longest line segment is cut into multiple cut planes that intersect perpendicularly to the line segment and divide the line segment into six equal parts. The eutectic area ratio, which is the ratio of the area of the eutectic appearing in a specified cross-section to the area of the field of view, is measured for each field of view. Since the coefficient of variation of the eutectic area ratio of the molded body is 0.15 or less, the variation in the yield strength, which is correlated with the eutectic area ratio, from one part to another can be reduced, and therefore a molded body having stable yield strength in every part can be obtained. [Brief description of the drawings]
[0015] [Figure 1] (a) is a cross-sectional view of the vessel when the rod is out of the molten metal, and (b) is a cross-sectional view of the vessel when the rod is immersed in the molten metal. [Diagram 2](a) is a cross-sectional view of the vessel when the rod is out of the molten metal at a different horizontal position than in Figure 1(a), and (b) is a cross-sectional view of the vessel when the rod is immersed in the molten metal at a different horizontal position than in Figure 1(b). [Diagram 3] 1(b) is a cross-sectional view of the vessel taken along line IIIa-IIIa in FIG. 1(b), and FIG. 2(b) is a cross-sectional view of the vessel taken along line IIIb-IIIb in FIG. 2(b). [Figure 4] IVb(a) is a cross-sectional view of the semi-solidified slurry taken along the line IVb in FIG. [Diagram 5] FIG. 2 is a schematic diagram showing the movement of a solid phase and a liquid phase in a molten metal during a stirring process. [Figure 6] 1A is a perspective view of the molded body, and FIG. 1B is a projection of the molded body drawn on a plane perpendicular to line A in FIG. [Figure 7] FIG. 13 is a diagram showing the relationship between the stirring method and the solid fraction. [Figure 8] FIG. 1 is a diagram showing the relationship between the stirring method and the eutectic area ratio. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0016] A preferred embodiment of the present invention will be described below with reference to the accompanying drawings. A method for producing a semi-solidified slurry 40 and a method for producing a molded body 100 in one embodiment will be described with reference to Fig. 1(a) to Fig. 4. Fig. 1(a) is a cross-sectional view of a vessel 20 when a rod 30 is sticking out of the molten metal 10. Fig. 1(b) is a cross-sectional view of a vessel 20 when a rod 30 is in the molten metal 10. In Fig. 1(a) and Fig. 1(b), the up-down direction, the left-right direction, and the direction perpendicular to the plane of the paper are respectively referred to as the up-down direction, the left-right direction, and the front-rear direction of the vessel 20 (the same applies to Fig. 2(a), Fig. 2(b), and Fig. 5(a) to Fig. 5(d)).
[0017] As shown in FIG. 1(a), molten metal 10 is placed in a vessel 20 with a bottom. The molten metal 10 is a molten metal, such as an aluminum alloy, a magnesium alloy, a copper alloy, or an iron alloy. The molten metal 10 may be a mixture of molten metal and powder or fiber. Examples of materials for the powder or fiber include ceramics such as SiC and Al2O3, and carbon. In a preparation process, the molten metal 10 is placed in the vessel 20 by pouring it from a spout of a high-temperature furnace (not shown) capable of maintaining a molten state, or by placing a container in the furnace and pouring it from the container into the vessel 20.
[0018] The metal is preferably a heat-treatable alloy whose mechanical properties (especially yield strength) are improved by solution treatment and aging treatment. The metal is, for example, heat-treatable alloy of aluminum alloy A6000 series A6051, A6061, A2000 series A2011, A2017, A2618 and A7000 series. The metal may also be based on systems such as magnesium alloy Mg-Zn(-Zr) (ZK series), Mg-Zn-Cu (ZC series), Mg-Zn-RE (ZE and EZ series; here RE means rare earth element), Mg-Zn-Mn(-Al) (ZM series), Mg-Al-Zn(Mn) (AZ and AM series), Mg-Y-RE(-Zr) (WE series), Mg-Ag-RE(-Zr) (QE and EQ series), Mg-Sn(-Zn,Al,Si)-based alloys. Other examples of the metal that can be used include copper alloys and iron alloys. In this embodiment, the metal is a heat-treated aluminum alloy.
[0019] The vessel 20 can be made of either metal or nonmetal, so long as it has high-temperature strength against the temperature of the molten metal 10 and does not react with the molten metal 10. The vessel 20 is open at the top, has a bottom 21 at the bottom, and has a rectangular cross section perpendicular to the up-down direction. In the left-right and front-to-back directions of the vessel 20 (hereinafter referred to as the "horizontal direction"), flat walls 22 are arranged to the right, left, front, and rear, and are connected to each other. The lower end of each wall 22 is connected to the respective end of the bottom 21 in the horizontal direction.
[0020] A plurality of rods 30 are connected to one surface of the base 32 with a gap between them. The tip of the rod 30 opposite to the tip connected to the base 32 has a pointed, cone-shaped tip 31. The cross-sectional shape of the rod 30 may be a circle, ellipse, square, triangle, polygon or star. The cross-sectional shape of the rod 30 is preferably a circle with few protruding parts on the outside.
[0021] The rods 30 are arranged parallel to one another. The length of the rods 30 is set to be longer than the distance from the liquid surface 11 of the molten metal 10 in the vessel 20 to the bottom 21 of the vessel 20. In the preparation process, the rods 30 are located outside the liquid surface 11 of the molten metal 10.
[0022] The rod 30 is made of a metal or nonmetallic material that can withstand the temperature of the molten metal 10. At least the surface of the rod 30 is coated with a coating such as DLC (diamond-like carbon). The coating prevents the rod 30 from being worn down due to friction with the molten metal 10 and prevents the molten metal 10 from adhering to the rod 30.
[0023] 1(b), in the stirring step, the molten metal 10 is inserted into the vessel 20 immediately after it is placed therein, or after the vessel 20 is held (exposed) to the atmosphere, a vacuum, or an inert gas such as argon gas or nitrogen gas for a predetermined time after it is placed therein, and then the rod 30 is inserted from the liquid surface 11 of the molten metal 10 toward the bottom 21 (downward) of the vessel 20. The rod 30 is then moved back and forth in its lengthwise direction to stir the molten metal 10. The predetermined time for holding the molten metal 10 in the atmosphere, vacuum, or inert gas is appropriately set depending on the amount of molten metal 10, the type of metal in the molten metal 10, the shape and size of the vessel 20, the atmospheric temperature of the atmosphere, vacuum, or inert gas, and the like.
[0024] Figure 2(a) is a cross-sectional view of vessel 20 when rod 30 is out of molten metal 10 at a horizontal position different from that of Figure 1(a), and Figure 2(b) is a cross-sectional view of vessel 20 when rod 30 is in molten metal 10 at a horizontal position different from that of Figure 1(b).
[0025] The horizontal position of rod 30 in Fig. 2(a) is a position moved to the right by a distance a from the horizontal position of rod 30 in Fig. 1(a). As shown in Fig. 1(b), rod 30 is once inserted toward the bottom 21 of vessel 20, and then rises from the bottom 21 of vessel 20 toward the liquid surface 11 of molten metal 10, returning to the position of rod 30 in Fig. 1(a). Then, as shown in Fig. 2(a), rod 30 moves to the right by a distance a.
[0026] Next, as shown in Fig. 2(b), rod 30 is moved a distance a to the right to a horizontal position, from which rod 30 is inserted from the liquid surface 11 of molten metal 10 toward the bottom 21 of vessel 20. After that, rod 30 further rises from the bottom 21 of vessel 20 toward the liquid surface 11 of molten metal 10, and returns to the position of rod 30 in Fig. 2(a).
[0027] Fig. 3(a) is a cross-sectional view of the vessel 20 taken along line IIIa-IIIa in Fig. 1(b), and Fig. 3(b) is a cross-sectional view of the vessel 20 taken along line IIIb-IIIb in Fig. 2(b). In Fig. 3(a) and Fig. 3(b), the up-down direction, left-right direction, and perpendicular direction to the paper correspond to the front-rear direction, left-right direction, and up-down direction, respectively, of the vessel 20. In Fig. 3(b), the dotted lines show four representative cross sections of the multiple rods 30 in Fig. 3(a), and indicate the positions before moving horizontally by a distance a.
[0028] As shown in Fig. 3(a), in a cross section perpendicular to the longitudinal direction of the rod 30, a plurality of rods 30 are present with a gap between them. Of two adjacent rods 30, the center of one rod 30 is located within a circle whose radius is a length L2 that is 7 times the thickness L1 of the other rod 30 and whose center is the center of the other rod 30. The thicknesses of the adjacent rods 30 may be different from each other or the same.
[0029] Distance a is a variable value (including a value having the same magnitude) whose magnitude changes with each reciprocating motion of rod 30. The direction in which distance a operates also varies with each reciprocating motion of rod 30, either left and right, front and back, or both. Therefore, in the stirring process, rod 30 can perform reciprocating motion at a horizontal position different from the immediately preceding reciprocating motion, making it easy to homogeneously stir solid phase 50 (described later) and liquid phase 60 (described later) when molten metal 10 solidifies, at multiple positions in the horizontal direction of molten metal 10.
[0030] The rod 30 repeats the reciprocating motion shown in Figures 1(a) to 3(b) until the solid fraction in any part of the molten metal 10 becomes 80% or more. Note that "until the solid fraction in any part of the molten metal 10 becomes 80% or more" means that the solid fraction in the part of the molten metal 10 with the lowest solid fraction becomes 80% or more.
[0031] Fig. 4(a) is a perspective view of the semi-solidified slurry 40, and Fig. 4(b) is a cross-sectional view of the semi-solidified slurry 40 shown in Fig. 4(a) in the arrow IVb direction. The semi-solidified slurry 40 in Fig. 4(a) is the semi-solidified slurry 40 that is taken out of the vessel 20 by stirring the molten metal 10 in the stirring step and then turning the vessel 20 upside down. In the semi-solidified slurry 40, a solid phase 50 and a liquid phase 60 coexist.
[0032] As shown in Fig. 4(a) and Fig. 4(b), the solid fraction of the molten metal 10 after the stirring process, i.e., the semi-solidified slurry 40, can be obtained by taking out the semi-solidified slurry 40 immediately after the stirring process from the vessel 20, quenching it in water, and observing 15 cross sections with a metallurgical microscope (200x). The 15 cross sections of the semi-solidified slurry 40 are 15 cross sections in total, including five cross sections from the upper part 41, the central part 42, and the lower part 43 of the semi-solidified slurry 40 that were in contact with the wall 22 of the vessel 20 toward the inside, i.e., the wall side parts 44, 44, the middle parts 45, 45, and the central part 46. The part that is quenched and solidified is the liquid phase 60 of the semi-solidified slurry 40. The solid fraction (%) can be obtained by dividing the area of the solid phase 50 that appears in the field of view on the cross section by the area of the field of view and multiplying it by 100 in each of the 15 cross sections. The field of view is a rectangular area 450 μm long and 600 μm wide.
[0033] The solid fraction of the molten metal 10 in the stirring step can be determined, for example, by preparing a graph showing the correlation between the kinetic viscosity of the molten metal 10 and the solid fraction in advance, providing a viscosity measuring device on the rod 30, and measuring the kinetic viscosity of the molten metal 10 during stirring, thereby obtaining a semi-solidified slurry 40 with a desired solid fraction. Alternatively, a graph showing the correlation between stirring time and the solid fraction can be prepared in advance, and stirring can be performed until the time at which the desired solid fraction is obtained from the graph, thereby obtaining a semi-solidified slurry 40 with a desired solid fraction.
[0034] The tip 31 is disposed with its pointed end facing away from the liquid surface 11 of the molten metal 10 toward the bottom 21 of the vessel 20. Because the tip 31 is pointed, it is easy to insert the rod 30 into the molten metal 10 even if the molten metal 10 has a high solid fraction of 80% or more.
[0035] In the stirring process, two adjacent rods 30 are positioned such that the center of one rod 30 is located within a circle whose radius is a length L2 that is 7 times the thickness L1 of the other rod 30 and whose center is the center of the other rod 30, and the two rods are stirred until the solid fraction reaches a high solid fraction of 80% or more.Therefore, even if the distance from the center to the center of adjacent rods 30 is long, the molten metal 10 between them can be sufficiently stirred.
[0036] Next, the movement of the solid phase 50 and the liquid phase 60 in the molten metal 10 in the stirring step will be described with reference to Fig. 5(a) to Fig. 5(d). Fig. 5(a) is a schematic diagram of the molten metal 10 when it enters the vessel 20 in the preparation step. Fig. 5(b) is a schematic diagram showing the state of the molten metal 10 when the rod 30 is inserted into the molten metal 10 in the stirring step. Fig. 5(c) is a schematic diagram showing the state of the molten metal 10 a predetermined time after Fig. 5(b). Fig. 5(d) is a schematic diagram showing the state of the molten metal 10 a further predetermined time after Fig. 5(c).
[0037] In Figures 5(a) to 5(d), the solid phase 50 represented by a square and the liquid phase 60 represented by a triangle are schematic representations of the distribution of the solid phase 50 and the liquid phase 60 in the molten metal 10. In Figures 5(a) to 5(d), the portion of the liquid surface 11 of the molten metal 10 where there is a large amount of solid phase 50 is omitted. In Figures 5(b) to 5(d), in order to simplify the drawings, all but one of the rods 30 are omitted.
[0038] As shown in FIG. 5(a), the molten metal 10 poured from the furnace into the vessel 20 is cooled from the portion closer to the wall 22 and bottom 21 of the vessel 20 than the horizontal center portion of the vessel 20, and a first layer 70 containing more solid phase 50 is formed from the portion closer to the wall 22 and bottom 21 of the vessel 20. A second layer 80 containing more liquid phase 60 than the first layer 70 is formed inside the first layer 70. A third layer 90 containing more liquid phase 60 than the second layer 80 is formed further inside the second layer 80, including the horizontal center portion of the vessel 20. All of the first layer 70 to the third layer 90 include the vicinity of the liquid surface 11 of the molten metal 10 (excluding the portion of the liquid surface 11 of the molten metal 10 where the solid phase 50 is more abundant). Note that the boundary between the first layer 70 and the second layer 80 and the boundary between the second layer 80 and the third layer 90 are not clearly defined, but a boundary line is provided for the purpose of explanation.
[0039] 5(b), the rod 30 is inserted from the liquid surface 11 toward the bottom 21 while pushing aside the solid phase 50 and liquid phase 60 in the molten metal 10 to the outside of the rod 30. The pushed-aside solid phase 50 and liquid phase 60 are present around the rod 30.
[0040] 5(c), when the rod 30 is raised from the bottom 21 of the molten metal 10 toward the liquid surface 11, the liquid phase 60, which has higher fluidity and is easier to move than the solid phase 50, flows into the portion of the molten metal 10 where the rod 30 was before the solid phase 50. The liquid phase 60 flows in greater quantity and faster than the solid phase 50 into the portion closer to the bottom 21 where the rod 30 was, so the molten metal 10 with more liquid phase 60 moves to the portion closer to the bottom 21.
[0041] 5(d), the molten metal 10 containing a large amount of liquid phase 60 flows into the portion where the rod 30 was present, and then the molten metal 10 containing a large amount of solid phase 50 flows in. The solid phase 50 of the first layer 70 where a large amount of solid phase 50 was present can be pushed aside, and the molten metal 10 containing a large amount of liquid phase 60 can be poured into that portion, so that the solid phase 50 and the liquid phase 60 can be easily mixed.
[0042] The molten metal 10 with a large amount of liquid phase 60 that has moved to the first layer 70 is located in the first layer 70 closer to the wall 22 and the bottom 21 than the second layer 80 and the third layer 90, and is therefore more likely to cool and become a solid phase 50. The molten metal 10 with a large amount of liquid phase 60 that was present in the second layer 80 and the third layer 90, which are less likely to become a solid phase 50, moves to the first layer 70, which is more likely to become a solid phase 50, and therefore can be homogeneously turned into a solid phase 50 without leaving any portion with a large amount of liquid phase 60. Thus, a semi-solidified slurry 40 with little variation in the solid phase ratio from one portion to another can be obtained.
[0043] In the stirring process, the molten metal 10 is stirred by reciprocating motion of the rod 30 until the solid fraction reaches 80% or more, thereby reducing the amount of liquid phase 60 present around the solid phase 50 and reducing the variation in distribution of the liquid phase 60 around the solid phase 50. The liquid phase 60 with small distribution variation uses the nearby solid phase 50 as a nucleus to further grow the solid phase 50, thereby reducing the variation in size of the particles (crystal grains) of the solid phase 50.
[0044] In the embodiment, the speed of the reciprocating motion of the rod 30 depends on the magnitude of the reciprocating motion, but is preferably, for example, 200 mm / sec to 300 mm / sec, and two or more reciprocating motions are performed per second. Since two or more reciprocating motions are performed per second, the negative pressure generated in the part where the rod 30 was present when the rod 30 rises from the bottom 21 of the molten metal 10 toward the liquid surface 11 is increased compared to the case where the speed is slower, and the flow of the solid phase 50 and the liquid phase 60 is promoted. Therefore, the stirring time can be shortened.
[0045] Since the horizontal position where the rod 30 reciprocates is different from the horizontal position of the previous reciprocation, the effect of the reciprocation can be obtained at a plurality of different horizontal positions in the molten metal 10. At any horizontal position of the molten metal 10, the solid phase 50 and the liquid phase 60 tend to mix, and the distribution of the solid phase 50 and the liquid phase 60 in the semi-solidified slurry 40 tends to become uniform. Therefore, the variation in the solid phase ratio at each portion of the semi-solidified slurry 40 can be reduced.
[0046] The surface temperature of the rod 30 before it comes into contact with the molten metal 10 is lower than that of the molten metal 10. Therefore, the molten metal 10 that comes into contact with the surface of the rod 30 tends to solidify quickly. Since there is almost no difference in the surface temperatures of the multiple rods 30, the molten metal 10 near the horizontal center of the vessel 20 and the molten metal 10 near the wall 22 of the vessel 20 are cooled regardless of the distance to the wall 22 of the molten metal 10. This makes it possible to reduce the variation in the solid fraction from one portion to another.
[0047] In the stirring process, when the rod 30 is moved up from the bottom 21 of the vessel 20 toward the liquid surface 11 of the molten metal 10 during the reciprocating motion of the rod 30, at least a part of the rod 30 is exposed to the atmosphere, etc., and the rod 30 is cooled. When the part of the rod 30 exposed to the atmosphere, etc. and the cooled part come into contact with the molten metal 10, the generation of the solid phase 50 is promoted. Therefore, the time required for the molten metal 10 to solidify can be shortened.
[0048] In the stirring step, when the rod 30 is raised from the bottom 21 of the vessel 20 toward the liquid surface 11 of the molten metal 10 during the reciprocating motion of the rod 30, the rod 30 has a small portion protruding from its outer shape, so the molten metal 10 is unlikely to adhere to the rod 30. Therefore, a semi-solidified slurry 40 with a stable volume can be repeatedly obtained. In the stirring step, the rod 30 may be vibrated while reciprocating. In this case, when the rod 30 is raised from the bottom 21 of the vessel 20 toward the liquid surface 11 of the molten metal 10, the vibration can make it even more difficult for the molten metal 10 to adhere to the rod 30. The direction of vibration is preferably the length direction of the rod 30. Even if the molten metal 10 adheres to the rod 30, the adhering molten metal 10 can be easily blown off with air or the like. After the preparation step, an electromagnetic stirring step of electromagnetically stirring the molten metal 10 may be performed before the stirring step or simultaneously with the stirring step. When electromagnetic stirring is performed before the stirring step, it is preferable to perform the stirring step without any time gap after the electromagnetic stirring step.
[0049] Electromagnetic stirring reduces the size of the particles (crystal grains) of the solid phase 50 in the resulting semi-solidified slurry 40. When the size of the particles of the solid phase 50 is reduced, the area of contact between the solid phase 50 and the liquid phase 60 is increased, and the amount of eutectic crystallized between the solid phases 50 can be increased.
[0050] Next, the obtained semi-solidified slurry 40 is placed in a mold from the vessel 20. The mold is closed, and the semi-solidified slurry 40 is pressurized to deform the semi-solidified slurry 40 and form a compact 100 (described later). The mold is opened, and the compact 100 is removed. Thereafter, the compact 100 is subjected to a solution treatment and an artificial aging treatment (collectively referred to as "T6 treatment").
[0051] During molding, the liquid phase 60 of the semi-solidified slurry 40 is divided into a portion that exists around the primary crystal (solid phase 50) and grows the primary crystal, and a portion that becomes a eutectic containing the components of the primary crystal (solid phase 50) and other elements. The eutectic portion contains elements of the primary crystal and elements different from the primary crystal. Since a certain amount of elements other than the primary crystal are present around the primary crystal in the eutectic, when the molded body 100 is molded and then subjected to solution treatment and aging treatment, a precipitation phase, which is a strengthening mechanism, precipitates (generates) around the primary crystal. When the precipitation phase is generated, the movement of the primary crystal due to slip between particles is suppressed by the precipitation phase, improving the mechanical properties (especially the yield strength) of the molded body 100.
[0052] The obtained molded body 100 was molded using the semi-solidified slurry 40 with a high solid fraction and little variation in the solid fraction from one part to another, so there is little variation in the distribution of eutectic crystallized between the solid phases 50 (primary crystals). Therefore, the molded body 100 that has been subjected to the T6 treatment has little variation in the distribution of the precipitated phase, and it is possible to obtain a molded body 100 with little variation in the distribution of mechanical properties (especially proof stress).
[0053] The molded body 100 is a press-molded product used for, for example, a housing. For press molding, a drawing process using a mold, a forging process, or the like is adopted. The molded body 100 has continuous fiber flows (grain flows), which are flows of the crystal structure of metal.
[0054] Next, a method for determining the eutectic area ratio and the variation coefficient of the eutectic area ratio of the molded body 100 will be described with reference to Fig. 6(a) and Fig. 6(b). Fig. 6(a) is a perspective view of the molded body 100 that has been pressed in a mold, taken out, and subjected to T6 treatment. Line A in Fig. 6(a) is a line along the direction in which the molded body 100 is pressed in the mold. The direction in which the molded body 100 is pressed may be from the upper surface 101 toward the lower surface 102, from the lower surface 102 toward the upper surface 101, or from both the upper surface 101 and the lower surface 102. In addition, the upper surface 101 and the lower surface 102 may have irregularities, and the shape of the upper surface 101 and the shape of the lower surface 102 may be different.
[0055] Fig. 6(b) is a projection of the molded body 100 drawn on a plane perpendicular to line A in Fig. 6(a). As shown in Fig. 6(b), first, the longest line segment 112 is drawn among the line segments connecting two points 110 and 111 on the outline 103 of the projection of the molded body 100. Next, a line segment 112 that intersects perpendicularly with the line segment 112 and divides the line segment 112 into six equal parts is drawn. 5 The molded body 100 is cut at six cut surfaces 113. The eutectic area ratio of each part can be obtained from the cross section of a sample obtained from each of the six equal parts. In this embodiment, the molded body 100 is divided into six equal parts at the cut surfaces 113, and the eutectic area ratio is obtained from the cross section of the sample of each of the six equal parts. 7 The eutectic area ratio may be determined from the cross section of each of equal or more portions of the sample.
[0056] The eutectic area ratio is the ratio of the area of the eutectic appearing in a field of view on a cross section to the area of the field of view. When the eutectic area ratio of the molded body 100 is measured multiple times for each field of view, the coefficient of variation obtained by dividing the standard deviation of the eutectic area ratio by the average value of the eutectic area ratio is 0.15 or less. When the longitudinal direction exists in the orthogonal direction of the molded body 100, the cross section of the molded body 100 is a cross section obtained from six or more parts obtained by equally dividing the distance of the molded body 100 in the longitudinal direction. The field of view on the cross section is a rectangular region of 450 μm in length and 600 μm in width.
[0057] Since the coefficient of variation of the eutectic area ratio of the molded body 100 is 0.15 or less, it is possible to obtain a molded body 100 with little variation in the eutectic area ratio relative to the average value of the eutectic area ratio, and it is possible to reduce the variation in the yield strength, which is correlated with the eutectic area ratio, from one part to another. Therefore, it is possible to obtain a molded body 100 with stable yield strength in each part. EXAMPLES
[0058] The present invention will be described in more detail with reference to examples, but the present invention is not limited to these examples.
[0059] Samples 1-3 of semi-solidified slurries were produced by stirring the molten metal 10 using different stirring methods. The metal used was A6061, a heat-treated aluminum alloy. The vessel 20 to hold the molten metal 10 was a stainless steel rectangular vessel with a bottom, measuring 60 mm wide, 60 mm long, 50 mm high, and 0.8 mm thick. In Samples 2 and 3, the speed at which the rod 30 was moved was approximately the same, between 200 mm / sec and 300 mm / sec. All other conditions were the same.
[0060] Sample 1 is a semi-solidified slurry obtained by performing only electromagnetic stirring for 10 seconds without any time gap after the preparation process. Sample 2 is a semi-solidified slurry obtained by performing electromagnetic stirring for 10 seconds without any time gap after the preparation process, and then stirring by rotating the rod 30 for 30 seconds without any time gap. Sample 3 is a semi-solidified slurry obtained by performing electromagnetic stirring for 10 seconds without any time gap after the preparation process, and then stirring by reciprocating the rod 30 for 30 seconds without any time gap after the preparation process.
[0061] The obtained samples 1-3 were quenched in water, and the cross sections of 15 locations, including the top, center, and bottom of each sample, and the wall side, middle, and center of each sample, which were in contact with the wall 22 of the vessel 20, were observed with a metal microscope (200x) to determine the solid fraction. The quenched and solidified portions are the liquid phase 60 of each sample. The solid fraction (%) was calculated by dividing the area of the solid phase 50 that appeared in the field of view on each cross section by the area of the field of view and multiplying it by 100. The field of view was a rectangular area of 450 μm in length and 600 μm in width for each of the 15 locations. Figure 7 is a diagram showing the relationship between each sample with different stirring methods and the solid fraction.
[0062] As shown in Figure 7, the solid fraction of sample 1 ranged from 55% to 100%, with a standard deviation of 13.51%. The solid fraction of sample 2 ranged from 36% to 100%, with a standard deviation of 19.40%. The solid fraction of sample 3 ranged from 85.2% to 100%, with a standard deviation of 4.10%. Even in the lowest solid fraction area, the solid fraction of sample 3 was 80% or more.
[0063] Next, Sample 1 and Sample 3 were each molded by applying a pressure of about 70 MPa to 140 MPa in a mold using a press machine equipped with a mold to obtain a molded body. After the obtained molded bodies were subjected to solution treatment and artificial aging treatment, six tensile test pieces were made from each molded body, and the 0.2% proof stress was measured. The six tensile test pieces were made from each part obtained by dividing the molded body into six equal parts in the longitudinal direction in the orthogonal direction perpendicular to the direction in which each sample was pressed. The measurement of the 0.2% proof stress was in accordance with JIS Z2241:2011. The tensile test pieces were No. 14B test pieces in accordance with JIS Z2241:2011. The 0.2% proof stress of Sample 1 was in the range of 78 MPa to 271 MPa, with a standard deviation of 81.58 MPa. The 0.2% proof stress of Sample 3 was in the range of 220 MPa to 255 MPa, with a standard deviation of 8.54 MPa.
[0064] Next, the fracture surfaces of the six tensile test pieces in the tensile test were polished and observed under a metal microscope (200x), and the eutectic area ratios were measured. Specifically, rectangular regions of 450μm length and 600μm width were arbitrarily set on the fracture surfaces of the six tensile test pieces, and the eutectic area ratios within those regions were measured. Figure 8 shows the relationship between the eutectic area ratios and the samples with different stirring methods.
[0065] As shown in Figure 8, the eutectic area ratio of sample 1 was in the range of 0.4%-1.5%, with a standard deviation of 0.41% and an average value of 1.09%. The coefficient of variation of the eutectic area ratio of sample 1 was 0.38. The eutectic area ratio of sample 3 was in the range of 1.1%-1.6%, with a standard deviation of 0.20% and an average value of 1.41%. The coefficient of variation of the eutectic area ratio of sample 3 was 0.15.
[0066] Compared to Samples 1 and 2, it is presumed that Sample 3 is able to homogeneously stir the solid phase 50 and liquid phase 60 in the molten metal 10 by the up and down reciprocating motion of the rod 30, thereby reducing the variation in the solid phase ratio from one portion to another.
[0067] In sample 3, the variation in the eutectic area ratio from one region to another is small, and therefore the variation in the distribution of eutectic between primary crystals is also small. It is presumed that the small variation in the distribution of eutectic between primary crystals reduces the variation in the distribution of precipitated phases obtained by solution treatment and artificial aging treatment, and reduces the variation in the 0.2% proof stress from one region to another.
[0068] The present invention has been described above based on the embodiments and examples, but the present invention is not limited to the above embodiments and examples, and it can be easily inferred that various improvements and modifications are possible within the scope of the present invention without departing from the spirit of the present invention.
[0069] In the embodiment, the molten metal 10 put into the vessel 20 is the molten metal 10 of heat-treated aluminum alloy A6061, but the present invention is not necessarily limited to this. As long as the metal can produce the semi-solidified slurry 40, other heat-treated alloys and non-heat-treated alloys can be used. In this case, even if the metal is a non-heat-treated alloy, the molded body 100 molded by pressurizing the semi-solidified slurry 40 obtained by the stirring step does not produce a precipitation phase, which is a strengthening mechanism between primary crystals, but the variation in crystal grain size is small and the variation in distribution of primary crystals and eutectic is small, so that the molded body 100 with stable yield strength can be obtained in all parts.
[0070] In the embodiment, the vessel 20 has a rectangular cross section perpendicular to the vertical direction, but this is not necessarily limited to this. It is of course possible to adopt a vessel 20 having a circular, elliptical, or polygonal cross section perpendicular to the vertical direction.
[0071] In the embodiment, the rods 30 are described as being arranged in parallel to one another, but this is not necessarily limited to this. The rods 30 may not be parallel to one another. It is of course possible to set the arrangement of the rods 30 appropriately in accordance with the shape of the vessel 20. It is also of course possible to set the arrangement regardless of the shape of the vessel 20. The rods 30 may be arranged to be spread apart from one another, for example, toward the bottom 21 and wall 22 of the vessel 20.
[0072] In the embodiment, the case where there are a plurality of rods 30 has been described, but the present invention is not necessarily limited to this.
[0073] In the embodiment, the case where the rod 30 moves reciprocally upward until the tip 31 emerges from the liquid surface 11 of the molten metal 10 in the stirring process has been described, but this is not necessarily limited to this. It is of course possible for the rod 30 to repeat reciprocating motion in the up and down direction while the tip 31 remains positioned within the molten metal 10.
[0074] In the embodiment, the method for producing the semi-solidified slurry 40 in which the electromagnetic stirring step is performed before or simultaneously with the stirring step has been described, but the present invention is not necessarily limited to this. It is of course possible to combine a stirring method other than electromagnetic stirring with the stirring step. Examples of stirring methods other than electromagnetic stirring include a method of stirring by ultrasonic vibration, a method of stirring by injecting gas into the molten metal 10, a method of stirring by high-frequency induction, a method of stirring by rotating, revolving, or vibrating the rod 30, and a method of stirring by combining these.
[0075] In the embodiment, the semi-solidified slurry 40 is set in the mold from the vessel 20 and pressurized to be molded in the molding step, but the present invention is not necessarily limited to this. The molten metal 10 may be directly poured into the mold in the preparation step, and the semi-solidified slurry 40 may be obtained in the mold by the stirring step, and then the semi-solidified slurry 40 may be molded by pressing as it is. In this case, the vessel 20 is a mold into which the molten metal 10 is poured. [Explanation of symbols]
[0076] 10 Molten metal 20 vessels 21 bottom 30 bars 40 Semi-solidified slurry 50 solid phase 60 liquid phase 100 Molded body
Claims
1. A method for producing a semi-solidified slurry consisting of a solid phase and a liquid phase, comprising the steps of: The preparation process involves pouring molten metal into a bottomed vessel; and a stirring step of stirring the molten metal by reciprocating a rod immersed in the molten metal in a longitudinal direction of the rod until a solid fraction in a portion of the molten metal in the vessel with a lowest solid fraction reaches 80% or more.
2. 2. The method for producing a semi-solidified slurry according to claim 1, wherein the position of the rod perpendicular to the longitudinal direction in the reciprocating motion in the stirring step is different from the position of the rod perpendicular to the longitudinal direction in the immediately preceding reciprocating motion.
3. In a cross section perpendicular to the longitudinal direction of the rod, The rods are present in a plurality of locations spaced apart from one another, 3. The method for producing a semi-solidified slurry according to claim 1 or 2, wherein the center of one of the two adjacent rods is located within a circle whose radius is 7 times the thickness of the other rod and whose center is the center of the other rod.
4. 4. The method for producing a semi-solidified slurry according to claim 1, further comprising an electromagnetic stirring step of stirring the molten metal in the vessel by electromagnetic stirring after the preparation step and before the stirring step or simultaneously with the stirring step.
5. A method for producing a green body, comprising: a molding step of pressurizing and deforming the semi-solidified slurry obtained by the method for producing a semi-solidified slurry according to any one of claims 1 to 4.
6. A press-molded product, which is a metal molded body consisting of primary crystals and eutectic crystals and in which fiber flow is continuously present, A molded body in which, when the longest line segment among the line segments connecting two points of the outline projected onto a plane perpendicular to the pressure direction is drawn, and the cross section of the sample is obtained by cutting each portion along a plurality of cut planes that intersect perpendicularly to the longest line segment and divide the line segment into six equal parts, a eutectic area ratio, which is the ratio of the area of the eutectic appearing in a visual field on a predetermined cross section to the area of the visual field, is measured for each of the visual fields, and the coefficient of variation, which is the standard deviation of the eutectic area ratio divided by the average value of the eutectic area ratio, is 0.15 or less.
Citation Information
Patent Citations
Method for holding semi-solidified metal slurry
JP1992158952A
Method for forming semi-solidified metal
JP1993050211A
Method for measuring temperature of semi-solidified metal
JP2004105986A
Al ALLOY CASTING AND METHOD FOR PRODUCING THE SAME
JP2010207842A
Deposit fining method of alloy and deposit fining device used in the same
JP2015205340A