Injection molded body, its manufacturing method, and raw materials used therein
Combining plant-derived polyethylene and fossil fuel-derived polypropylene resins with controlled melt flow rates addresses gate residue in injection molding, enabling environmentally friendly production with existing molds.
Patent Information
- Application Number
- JP2020095406
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2020-06-01
- Publication Date
- 2024-12-03
- Estimated Expiration
- 2040-06-01
AI Technical Summary
Injection molding using plant-derived raw materials results in molding defects at the gate portion, known as gate residue, despite contributing to global environmental conservation.
Combining a plant-derived polyethylene resin with a low melt flow rate and fossil fuel-derived polypropylene resin to suppress molding defects, with specific ratios and melt flow rates to ensure adequate fluidity and suppress gate residue.
Manufactures injection molded articles that contribute to environmental conservation while effectively reducing molding defects, particularly gate residue, using existing cold runner molds without the need for hot runner molds.
Smart Images

Figure 0007592982000003 
Figure 0007592982000004 
Figure 0007592982000005
Abstract
Description
[Technical field]
[0001] The present disclosure relates to an injection molded article and a method for producing the same, as well as raw materials used therein. [Background technology]
[0002] From the viewpoint of protecting the global environment, the development of plastic materials using raw materials derived from plants is being promoted. Patent Document 1 discloses a method for producing one or more olefins from the residues of renewable natural raw materials (e.g., sugar cane), and also discloses polymers using these olefins. [Prior art documents] [Patent documents]
[0003] [Patent Document 1] Special Publication No. 2010-511634 Summary of the Invention [Problem to be solved by the invention]
[0004] In the field of injection molding using plastic materials as raw materials, using plant-derived raw materials as part of the raw materials contributes to global environmental conservation. Therefore, the inventors prepared a raw material by blending plant-derived polyethylene resin and fossil fuel-derived polypropylene resin, and supplied this to a cold runner type mold to manufacture an injection molded product. However, solidified resin remained at the gate of the molded product when it was removed from the mold. This is a type of molding defect and is called a gate residue.
[0005] The gate residue will be explained with reference to Fig. 1(a) and Fig. 1(b). Fig. 1(a) is a cross-sectional view showing a state in which a cavity C defined by a pair of molds 1a and 1b is filled with plastic material P. The plastic material P is supplied into the cavity C through a cold runner R provided in the mold 1b. In this state, the cold runner R is also filled with the plastic material P. The tip opening of the cold runner R corresponds to the gate portion. Fig. 1(b) is a cross-sectional view showing a schematic view of an injection-molded body 10 recovered from the molds 1a and 1b. The injection-molded body 10 has a protrusion 10a (gate residue) of the plastic material P at the gate portion.
[0006] The present disclosure has been made in consideration of the above problems, and provides a method for producing an injection-molded article that contributes to global environmental conservation and can suppress the occurrence of molding defects, as well as raw materials used therein. [Means for solving the problem]
[0007] The present inventors have experimentally found that the occurrence of the above molding defects can be suppressed by selecting and using a plant-derived polyethylene resin having a relatively small melt flow rate at 190°C (relatively high melt viscosity) for use in combination with a fossil fuel-derived polypropylene resin. The present disclosure below is based on this finding.
[0008] A method for producing an injection molded body according to one aspect of the present disclosure includes the steps of preparing a raw material containing a plant-derived polyethylene resin and a fossil fuel-derived polypropylene resin, and supplying the raw material into a mold, wherein the raw material contains 5 to 95 mass% plant-derived polyethylene resin and 95 to 5 mass% fossil fuel-derived polypropylene resin, based on the total mass of the plant-derived polyethylene resin and the fossil fuel-derived polypropylene resin, and the plant-derived polyethylene resin has a melt flow rate of 15 g / 10 min or less at 190°C.
[0009] According to the above manufacturing method, since a plant-derived resin material is used as part of the raw material, it can contribute to global environmental conservation. Furthermore, according to the above manufacturing method, even when a cold runner type mold is used, the occurrence of molding defects can be sufficiently suppressed. Note that the melt flow rate value in this disclosure refers to a value measured under conditions of a specified temperature (190°C or 230°C described below) and a load of 2.16 kg in accordance with the method described in JIS K7210-1:2014.
[0010] One aspect of the present disclosure relates to a raw material used in the method for producing the injection-molded article, the raw material containing a plant-derived polyethylene resin and a fossil fuel-derived polypropylene resin, the plant-derived polyethylene resin content being 5 to 95 mass% and the fossil fuel-derived polypropylene resin content being 95 to 5 mass% based on the total mass of the plant-derived polyethylene resin and the fossil fuel-derived polypropylene resin, and the plant-derived polyethylene resin has a melt flow rate of 15 g / 10 min or less at 190°C.
[0011] One aspect of the present disclosure relates to an injection-molded article, which contains a plant-derived polyethylene resin and a fossil fuel-derived polypropylene resin, the plant-derived polyethylene resin content is 5 to 95 mass% and the fossil fuel-derived polypropylene resin content is 95 to 5 mass% based on the total mass of the plant-derived polyethylene resin and the fossil fuel-derived polypropylene resin, and the plant-derived polyethylene resin has a melt flow rate of 15 g / 10 min or less at 190°C.
[0012] In the present disclosure, from the viewpoint of further reducing the above molding defects, the melt flow rate of the fossil fuel-derived polypropylene resin at 230°C is preferably 15g / 10min or less. From the same viewpoint, the ratio (B / A) of the melt flow rate value B of the fossil fuel-derived polypropylene resin at 230°C to the melt flow rate value A of the plant-derived polyethylene resin at 190°C is preferably 1.1 or more and 2.0 or less. From the viewpoint of the fluidity of the raw material, the melt flow rate of the plant-derived polyethylene resin at 190°C is preferably 3g / 10min or more. From the same viewpoint, the melt flow rate of the fossil fuel-derived polypropylene resin at 230°C is preferably 5g / 10min or more. Effect of the Invention
[0013] According to the present disclosure, there are provided a method for producing an injection-molded article, which contributes to the preservation of the global environment and can sufficiently suppress the occurrence of molding defects, and raw materials used therein. [Brief description of the drawings]
[0014] [Figure 1] FIG. 1(a) is a cross-sectional view showing a schematic diagram of a state in which plastic material is supplied into a cold runner type mold, and FIG. 1(b) is a cross-sectional view showing a schematic diagram of a molded body with solidified resin remaining at the gate portion. [Diagram 2] FIG. 2 is a cross-sectional view that illustrates the injection molded articles produced in the examples and comparative examples. [Diagram 3] FIG. 3 is a perspective view that typically shows a mold used in the examples and comparative examples. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0015] Hereinafter, embodiments of the present disclosure will be described in detail. Note that the present invention is not limited to the following embodiments.
[0016] <Manufacturing method of injection molded article> The method for producing an injection molded article according to this embodiment includes the following steps. (A) A process for preparing a raw material containing a plant-derived polyethylene resin and a fossil fuel-derived polypropylene resin. (B) A step of supplying the above-mentioned raw material into a mold.
[0017] (Raw material for manufacturing injection molded products) First, the raw material for manufacturing injection molded bodies will be described. As described above, this raw material includes plant-derived polyethylene resin and fossil fuel-derived polypropylene resin. An example of a plant-derived polyethylene resin is that manufactured by Braskem. Braskem manufactures and sells linear low-density polyethylene (LLDPE), high-density polyethylene (HDPE), and low-density polyethylene (LDPE) from renewable natural raw materials. The plant-derived LLDPE has an α-olefin with 4 or 6 carbon atoms in the side chain, which is represented as C4-LLDPE or C6-LLDPE.
[0018] The melt flow rate of the plant-derived polyethylene resin at 190°C is 15g / 10min or less, preferably 12g / 10min or less, and more preferably 10g / 10min or less. When this value is 15g / 10min or less, even if the plant-derived polyethylene resin is used in combination with the fossil fuel-derived polypropylene resin, the occurrence of molding defects can be sufficiently suppressed. This value is preferably 3g / 10min or more, more preferably 5g / 10min or more, and even more preferably 7g / 10min or more. When this value is 3g / 10min or more, even if the ratio of the plant-derived polyethylene resin in the raw material is relatively high, the fluidity of the raw material can be sufficiently maintained. In addition, even if the plant-derived polyethylene resin and the fossil fuel-derived polypropylene are blended, the basic functions such as drop strength as an injection molded product can be satisfied.
[0019] The density of the plant-derived polyethylene resin is, for example, 0.910 to 0.960 g / cm 3 0.915~0.918g / cm 3 or 0.953~0.959g / cm 3When the density of the plant-derived polyethylene resin is within this range, the occurrence of molding defects can be sufficiently suppressed even when the plant-derived polyethylene resin is used in combination with a fossil fuel-derived polypropylene resin.
[0020] Examples of polypropylene resins derived from fossil fuels include homopolypropylene, block polypropylene, random polypropylene, and modified polypropylene. The block polypropylene here generally has a structure in which a rubber component and polyethylene are dispersed in homopolypropylene at the polymerization stage. When a combination of block polypropylene and random polypropylene is used as the polypropylene resin, the mass ratio of the block polypropylene to the random polypropylene (block polypropylene / random polypropylene) is preferably 20 / 80 to 80 / 20, and more preferably 40 / 60 to 60 / 40.
[0021] The modified polypropylene is obtained by graft-modifying polypropylene with an unsaturated carboxylic acid derivative component derived from, for example, an unsaturated carboxylic acid, an acid anhydride of an unsaturated carboxylic acid, an ester of an unsaturated carboxylic acid, or the like. In addition, modified polypropylene such as hydroxyl group-modified polypropylene or acrylic-modified polypropylene can also be used as the polypropylene resin. Examples of the α-olefin component used to obtain the propylene-based copolymer include 1-butene, 1-pentene, 1-hexene, 1-heptene, 1-octene, and 4-methyl-1-pentene.
[0022] The melt flow rate of the fossil fuel-derived polypropylene resin at 230°C may be, for example, 30g / 10min or less or 20g / 10min or less, and is preferably 15g / 10min or less. By having this value of 15g / 10min or less, even if the ratio of plant-derived polyethylene resin in the raw material is relatively high, the occurrence of molding defects can be sufficiently suppressed. This value is preferably 3g / 10min or more, more preferably 5g / 10min or more, and even more preferably 7g / 10min or more. By having this value of 3g / 10min or more, even if the ratio of fossil fuel-derived polypropylene resin in the raw material is high, the fluidity of the raw material can be sufficiently maintained.
[0023] The density of polypropylene resin derived from fossil fuels is, for example, 0.900 to 0.910 g / cm 3 When the density of the fossil fuel-derived polypropylene resin is in this range, the occurrence of molding defects can be sufficiently suppressed even when the plant-derived polyethylene resin is used in combination with the fossil fuel-derived polypropylene resin.
[0024] From the viewpoint of further reducing the above-mentioned molding defects, the ratio (B / A) of the melt flow rate value B of the fossil fuel-derived polypropylene resin at 230°C to the melt flow rate value A of the plant-derived polyethylene resin at 190°C is, for example, 1.1 to 4.0, and may be 1.1 to 2.0 or 2.0 to 4.0, and from the viewpoint of further suppressing molding defects, it is preferably 1.1 to 2.0.
[0025] Based on the total mass of the plant-derived polyethylene resin and the fossil fuel-derived polypropylene resin, the content of the plant-derived polyethylene resin in the raw material is 5% by mass or more, preferably 10% by mass or more, and more preferably 25% by mass or more. Having this value of 5% by mass or more contributes to global environmental conservation in terms of carbon neutrality. On the other hand, based on the same standard, the content of the fossil fuel-derived polypropylene resin in the raw material is 5% by mass or more, preferably 50% by mass or more, and more preferably 70% by mass or more. Having this value of 5% by mass or more allows the effects attributable to the polypropylene resin (for example, excellent moldability and physical properties) to be fully exhibited.
[0026] The total amount of the plant-derived polyethylene resin and the fossil fuel-derived polypropylene resin relative to the total mass of the raw material is, for example, 90% by mass or more, and may be 95% by mass or more or 98% by mass or more. In addition to the plant-derived polyethylene resin and the fossil fuel-derived polypropylene resin, the raw material may contain, for example, additives that are blended into the raw material of the injection molded body.
[0027] The raw material can be prepared by mixing or kneading a plant-derived polyethylene resin, a fossil fuel-derived polypropylene resin, and other components as necessary (step (A)). An injection molded article can be obtained through a step (step (B)) of supplying the molten raw material into the cavity of a mold. The preparation of the raw material and the supply of the raw material to the mold may be carried out by a kneading extruder. For example, when a kneading extruder having a screw is used, the screw temperature may be adjusted according to the melt flow rate (melt viscosity) of the raw material. The screw temperature may be, for example, 190 to 220°C. The injection speed of the raw material into the cavity of the mold may be, for example, 30 to 80 mm / sec. When a raw material with a relatively small melt flow rate (relatively high melt viscosity) is used, the filling property of the raw material into the cavity may be improved by moving the VP switching position in the kneading extruder closer to the nozzle (discharge port) side.
[0028] The mold may be of the cold runner type or the hot runner type, but according to this embodiment, even when a cold runner type mold is used, which is more likely to cause gate residue compared to the hot runner type, the occurrence of gate residue can be sufficiently suppressed. This has the advantage that an injection molded article that is considerate of the global environment can be manufactured by simply using an existing cold runner type mold and replacing the conventional resin raw material derived from fossil fuels with the raw material according to this embodiment. In other words, there is an advantage that, for example, there is no need to newly introduce a hot runner type mold.
[0029] According to the above embodiment, it is possible to efficiently manufacture an injection molded article that contributes to global environmental conservation and can sufficiently suppress the occurrence of molding defects. Specific examples of the injection molded article include plastic caps, containers, and plugs.
[0030] Although the embodiments of the present disclosure have been described in detail above, the present invention is not limited to the above-mentioned embodiments. For example, in the above-mentioned embodiments, a case where an injection molded article is manufactured using a cold runner type mold is illustrated, but an injection molded article may be manufactured using a hot runner type mold.
[0031] In the above embodiment, the case where the plant-derived polyethylene resin and the fossil fuel-derived polypropylene resin are used in combination is exemplified, but the injection molded article may be manufactured using the fossil fuel-derived polyethylene resin instead of the plant-derived polyethylene resin. The physical properties (e.g., melt flow rate and density at 190°C) of the fossil fuel-derived polyethylene resin are preferably in the same range as those of the above-mentioned plant-derived polyethylene resin. EXAMPLES
[0032] The present disclosure will be described below based on examples and comparative examples. Note that the present invention is not limited to the following examples.
[0033] The following materials were used to prepare the raw materials for the comparative examples and examples. <Plant-derived polyethylene resin (Bio-PE)> BioPE1: HDPE manufactured by Braskem (Melt flow rate at 190℃: 20.0g / 10min) BioPE2: Braskem HDPE (Melt flow rate at 190℃: 30.0g / 10min) BioPE3: Braskem LDPE (Melt flow rate at 190℃: 8.3g / 10min) BioPE4: Braskem LDPE (Melt flow rate at 190℃: 7.2g / 10min) <Polypropylene resin (PP) derived from fossil fuels> PP1: PP manufactured by SunAllomer (Melt flow rate at 230℃: 25.0g / 10min) PP2: PP manufactured by SunAllomer (Melt flow rate at 230℃: 14.0g / 10min) PP3: PP manufactured by SunAllomer (Melt flow rate at 230℃: 9.5g / 10min)
[0034] The following injection molded articles according to the comparative examples and examples were produced under the conditions shown in Tables 1 and 2, respectively. Injection molded body: Cap with hinge (diameter: 68.4 mm, height: 22.2 mm) Fig. 2 is a cross-sectional view showing the caps (injection molded articles) produced in the examples and comparative examples. As shown in this figure, the cap 20 includes an upper cover 20a, a cap body 20b, and a hinge 20c that allows the upper cover 20a to be opened and closed relative to the cap body 20b. "Gate height" in Tables 1 and 2 means the height of the remaining gate (see Fig. 1(b)).
[0035] An injection molding machine manufactured by Sumitomo Heavy Industries, Ltd. was used as the molding machine. A cold runner type mold was used as the mold. FIG. 3 is a perspective view showing a mold used in the examples and comparative examples. As shown in this figure, mold 5 has three parts 5a, 5b, and 5c. With mold 5, a total of eight caps 20 can be manufactured simultaneously. Part 5a has an opening 6. Molten resin is supplied into mold 5 from opening 6. Part 5b has a cold runner 7. Part 5c, together with part 5b, has a recess 8 that forms a cavity.
[0036] [Table 1]
[0037] [Table 2] [Explanation of symbols]
[0038] Reference Signs List 1a, 1b, 5... mold, 5a, 5b, 5c... parts, 6... opening, 7, R... cold runner, 8... recess, 10... injection molded body, 10a... protrusion (gate remainder), 20... cap (injection molded body), 20a... upper cover, 20b... cap body, 20c... hinge, C... cavity, P... plastic material
Claims
1. A step of preparing a raw material including a plant-derived polyethylene resin and a fossil fuel-derived polypropylene resin; supplying the raw material into a mold; Including, In the raw material, the content of the plant-derived polyethylene resin is 5 to 95 mass% and the content of the fossil fuel-derived polypropylene resin is 95 to 5 mass% based on the total mass of the plant-derived polyethylene resin and the fossil fuel-derived polypropylene resin, The plant-derived polyethylene resin has a melt flow rate of 5 to 15 g / 10 min at 190° C.; The melt flow rate of the fossil fuel-derived polypropylene resin at 230° C. is 7 to 20 g / 10 min, a ratio (B / A) of a melt flow rate value B of the fossil fuel-derived polypropylene resin at 230°C to a melt flow rate value A of the plant-derived polyethylene resin at 190°C is 1.1 to 2.0; A method for producing an injection molded body, wherein a total amount of the plant-derived polyethylene resin and the fossil fuel-derived polypropylene resin is 90 mass% or more relative to the total mass of the raw materials.
2. The method for producing an injection molded article according to claim 1, wherein the fossil fuel-derived polypropylene resin has a melt flow rate at 230°C of 15 g / 10 min or less.
3. The method for producing an injection molded article according to claim 1 or 2, wherein the mold has a cold runner, and the raw material is supplied into the mold through the cold runner.
4. Plant-derived polyethylene resin, Polypropylene resin derived from fossil fuels and A raw material for manufacturing an injection molded body comprising: the content of the plant-derived polyethylene resin is 5 to 95 mass% and the content of the fossil fuel-derived polypropylene resin is 95 to 5 mass% based on the total mass of the plant-derived polyethylene resin and the fossil fuel-derived polypropylene resin, The plant-derived polyethylene resin has a melt flow rate of 5 to 15 g / 10 min at 190° C.; The melt flow rate of the fossil fuel-derived polypropylene resin at 230° C. is 7 to 20 g / 10 min, a ratio (B / A) of a melt flow rate value B of the fossil fuel-derived polypropylene resin at 230°C to a melt flow rate value A of the plant-derived polyethylene resin at 190°C is 1.1 to 2.0; A raw material for producing injection molded bodies, wherein a total amount of the plant-derived polyethylene resin and the fossil fuel-derived polypropylene resin relative to a total mass of the raw material for producing injection molded bodies is 90 mass% or more.
5. Plant-derived polyethylene resin, Polypropylene resin derived from fossil fuels and An injection molded article comprising: the content of the plant-derived polyethylene resin is 5 to 95 mass% and the content of the fossil fuel-derived polypropylene resin is 95 to 5 mass% based on the total mass of the plant-derived polyethylene resin and the fossil fuel-derived polypropylene resin, The plant-derived polyethylene resin has a melt flow rate of 5 to 15 g / 10 min at 190° C.; The melt flow rate of the fossil fuel-derived polypropylene resin at 230° C. is 7 to 20 g / 10 min, a ratio (B / A) of a melt flow rate value B of the fossil fuel-derived polypropylene resin at 230°C to a melt flow rate value A of the plant-derived polyethylene resin at 190°C is 1.1 to 2.0; an injection-molded article, wherein a total amount of the plant-derived polyethylene resin and the fossil fuel-derived polypropylene resin relative to a total mass of the injection-molded article is 90 mass% or more.
Citation Information
Patent Citations
Propylenic resin composition and its molded article
JP2008255326A
Methods for producing one or more olefins, olefins and polymers
JP2010511634A
Cap having toggle structure containing plant-based polyolefin
JP2013184727A
Resin molded body
JP2016089054A
Plastic cup
JP2019182528A