Blocked isocyanate composition
The use of a stabilizer with a pKa of 2.0 or less in blocked isocyanate compositions addresses storage stability issues and enables effective curing, resulting in high-quality cured films for adhesives and coatings.
Patent Information
- Application Number
- JP2020165091
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2020-09-30
- Publication Date
- 2024-12-03
- Estimated Expiration
- 2040-09-30
AI Technical Summary
Conventional blocked isocyanate compositions suffer from poor storage stability due to gradual decomposition, especially in solutions containing hydroxyl, amino, and thiol groups, and there is a need for improved stability while maintaining effective curing and removal of the blocking agent.
A blocked isocyanate composition is developed using a stabilizer with a pKa of 2.0 or less, such as a salt of para-toluenesulfonic acid, to enhance storage stability and facilitate the removal of the blocking agent during curing, incorporating a blocked isocyanate compound and a stabilizer, along with optional polymerization inhibitors and monomers.
The composition achieves excellent storage stability and effective curing, forming high-quality cured films suitable for adhesives and coatings, with improved removal of the blocking agent, thereby enhancing the performance of isocyanate-based materials.
Smart Images

Figure 0007593033000001 
Figure 0007593033000002 
Figure 0007593033000003
Abstract
Description
[Technical field]
[0001] The present invention relates to a blocked isocyanate composition containing a blocked isocyanate compound, which is a blocked product of a (meth)acrylic acid ester having an isocyanato group, and a stabilizer. [Background technology]
[0002] A blocked isocyanate compound is a compound in which an isocyanato group is reacted with an active hydrogen group-containing compound (blocking agent) to inactivate (block) the reactivity of the isocyanato group, and has the property that when this is heated, the blocking agent dissociates and the isocyanato group is regenerated. For example, when a blocked isocyanate compound is used as a curing agent, by blocking the isocyanato group, it is not necessary to prepare a two-liquid type, for example, one liquid containing a base agent having an active hydrogen group and another liquid containing a compound having an isocyanato group for reacting with the active hydrogen group, and it is possible to premix the base agent having an active hydrogen group and the blocked isocyanate compound into one liquid. Therefore, blocked isocyanate compounds are widely used in adhesives, coating agents, molding materials, etc.
[0003] Cited Document 1 discloses a urethane-formation reaction catalyst used in a urethane-formation reaction between an isocyanate or a blocked isocyanate and a polyol, the urethane-formation reaction catalyst comprising the following components (A), (B) and (C), in which component (A) is in a uniformly dissolved state in component (C): (A) An acetylacetone compound of at least one specific metal element selected from the group consisting of zinc, aluminum, calcium, zirconium and magnesium. (B) Stabilizer (C) Solvent
[0004] Cited Document 2 discloses a polyaniline composition containing a polyaniline complex obtained by doping a substituted or unsubstituted polyaniline molecule with a proton donor, a phenolic compound, a divalent blocked isocyanate compound, and a solvent. [Prior art documents] [Patent documents]
[0005] [Patent Document 1] JP 2015-136678 A [Patent Document 2] JP 2012-158620 A Summary of the Invention [Problem to be solved by the invention]
[0006] In the conventional blocked isocyanate composition, the decomposition of the blocked isocyanate compound proceeds gradually in a solution, particularly in a solution in which a hydroxyl group, an amino group, or a thiol group coexists with the blocked isocyanate compound, so that the storage stability of the blocked isocyanate compound in the blocked isocyanate composition is poor. Therefore, there has been a demand for improving the storage stability of the blocked isocyanate compound in the blocked isocyanate composition. In addition, there has been a demand for a cured film obtained by curing the blocked isocyanate composition well while maintaining the storage stability of the blocked isocyanate compound in the blocked isocyanate composition, and further for a method for producing a composition containing an isocyanate compound, which causes a blocking agent to be released from the blocked isocyanate compound in the blocked isocyanate composition.
[0007] The present invention has been made to solve the above-mentioned problems, and an object of the present invention is to provide a blocked isocyanate composition having excellent storage stability of a blocked isocyanate compound, a cured film obtained by curing the blocked isocyanate composition, and a method for producing a composition containing an isocyanate compound or the like, which comprises removing a blocking agent from the blocked isocyanate compound or the like in the blocked isocyanate composition. [Means for solving the problem]
[0008] As a result of intensive research into the above-mentioned problems, the present inventors have found that the above-mentioned problems can be solved by using a specific stabilizer, which is a salt of a specific blocked isocyanate compound with an acid having a pKa of 2.0 or less, and have completed the present invention. That is, the present invention includes, for example, the following aspects [1] to
[10] . [1] A blocked isocyanate composition comprising a blocked isocyanate compound (A) and a stabilizer (B), a blocked isocyanate composition, wherein the blocked isocyanate compound (A) is a compound formed by urethane bonding between an isocyanato group of a (meth)acrylic ester compound (a1) having an isocyanato group and a hydroxyl group of a phenol compound (a2); and the stabilizer (B) is a salt of a compound (b1) represented by general formula (1) and an acid (b2), and the pKa of the acid (b2) is 2.0 or less. R 1 N=CR 2 -NR 3 R 4 (1) (In the formula, R 2 is a hydrogen atom, a hydrocarbon group having 1 to 20 carbon atoms, or -NR 5 2 R is a group represented by the formula: 1 , R 3 , R 4 and R 5 are each independently a hydrogen atom or a hydrocarbon group having 1 to 20 carbon atoms, and two R 5 may be the same or different. 1 , R 2 , R 3 , R 4 , and two R 5 Any two or more of these may be bonded to form a cyclic structure.) [2] The stabilizer (B) is used in an amount of 100 to 1.00 × 10 relative to the blocked isocyanate compound (A). 5 The blocked isocyanate composition according to [1], wherein the blocked isocyanate composition contains 10 ppm by mass of the blocked isocyanate. [3] The blocked isocyanate composition according to [1] or [2], wherein the (meth)acrylic acid ester compound (a1) having an isocyanato group is 2-acryloyloxyethyl isocyanate, 2-methacryloyloxyethyl isocyanate, 2-(isocyanatoethyloxy)ethyl acrylate, 2-(isocyanatoethyloxy)ethyl methacrylate, or 1,1-bis(acryloyloxymethyl)ethyl isocyanate. [4] The blocked isocyanate composition according to any one of [1] to [3], wherein the compound (b1) is a compound represented by general formula (1-2): R 1a N=CR 2a -NR 3a R 4a (1-2) (In the formula, R 1a , R 2a , R 3a and R 4a is a hydrocarbon group, R 1a and R 4a and R 2a and R 3a and each bond to form a ring structure, and R 1a and R 4a The sum of the carbon numbers is 3 to 20, R 2a and R 3a The sum of the carbon numbers is 3 to 20.) [5] The blocked isocyanate composition according to any one of [1] to [3], wherein the compound (b1) represented by the general formula (1) is 1,8-diazabicyclo[5.4.0]-undecene-7, 1,5-diazabicyclo[4.3.0]-5-nonene, or 1,1,3,3-tetramethylguanidine. [6] The blocked isocyanate composition according to any one of [1] to [5], further comprising a polymer (F) obtained by polymerizing the blocked isocyanate compound (A). [7] The blocked isocyanate composition according to any one of [1] to [6], wherein the acid (b2) is at least one selected from the group consisting of paratoluenesulfonic acid, trifluoromethanesulfonic acid, benzenesulfonic acid, methanesulfonic acid, 10-camphorsulfonic acid, hydrochloric acid, and sulfuric acid. [8] A blocked isocyanate polymer obtained by polymerizing a polymerizable component contained in the blocked isocyanate composition according to any one of [1] to [7]. [9] A cured film obtained by curing the blocked isocyanate composition according to any one of [1] to [7].
[10] A method for producing a composition containing an isocyanate compound or an isocyanato group-containing (co)polymer, and a stabilizer (B), comprising: maintaining the blocked isocyanate composition according to any one of [1] to [7] at 30°C or higher for 10 days or more, and then maintaining it at 80°C or higher for 0.5 hours or more to eliminate the phenol compound (a2) from the blocked isocyanate compound (A) or polymer (F). Effect of the Invention
[0009] According to the present invention, it is possible to provide a blocked isocyanate composition having excellent storage stability of the blocked isocyanate compound. It is also possible to provide a cured film obtained by satisfactorily curing the blocked isocyanate composition containing the blocked isocyanate compound having excellent storage stability, and an adhesive, a coating agent, and a molding material utilizing the formation of the cured film. It is also possible to provide a method for producing a composition containing an isocyanate compound or the like, which comprises releasing a blocking agent from the blocked isocyanate compound or the like having excellent storage stability in the blocked isocyanate composition. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0010] Hereinafter, embodiments of the present invention will be described in detail, however, the present invention is not limited to the embodiments described below. In the present invention, (meth)acrylic acid means acrylic acid or methacrylic acid. For example, a (meth)acrylic acid ester compound means an acrylic acid ester compound or a methacrylic acid ester compound.
[0011] <Blocked isocyanate composition> The blocked isocyanate composition according to one embodiment of the present invention contains a blocked isocyanate compound (A) and a stabilizer (B). The blocked isocyanate composition may contain a polymer (F). If necessary, the blocked isocyanate composition may contain at least one of a polymerization inhibitor (C), a monomer (D) having an ethylenically unsaturated bond, and another polymer (E). The blocked isocyanate composition according to this embodiment forms a cured film by polymerization and curing by irradiation with light or heating.
[0012] [Blocked isocyanate compound (A)] The blocked isocyanate compound (A) used in the present invention is a compound in which the isocyanato group of a (meth)acrylic acid ester compound (a1) having an isocyanato group is bonded to a hydroxyl group of a phenol compound (a2) as a blocking agent through a urethane bond. The blocked isocyanate compound (A) is preferably a compound represented by the following general formula (2).
[0013] (R 6 -COO) n R 7 (NH-C(=O)OPh) m (2) In formula (2), R 6 CH 2 =CH(CH 3 )- or CH 2 =CH-.
[0014] R 7 R is a linear or branched aliphatic hydrocarbon group having 1 to 7 carbon atoms, preferably 2 to 6, more preferably 2 to 5, and even more preferably 2, with an m+n valence, or an aromatic hydrocarbon group having 6 to 7 carbon atoms which may have a substituent such as a methyl group. 7 R may contain an ether bond. 7 is preferably -CH from the viewpoint of availability of raw materials. 2 -, -CH 2 CH 2 -, or -CH 2 CH 2 OCH 2 CH 2-, more preferably -CH 2 CH 2 -It is.
[0015] m and n are each independently an integer of 1 or 2, and from the viewpoint of ease of production, each is preferably 1. Ph represents a phenyl group. A part or all of the hydrogen atoms of the phenyl group may be substituted with a substituent having 1 to 20 carbon atoms. Examples of the substituent include a methoxy group, an acetyl group, a propionyl group, a formyl group, a methoxycarbonyl group, an ethoxycarbonyl group, a benzyloxycarbonyl group, a methyl group, an ethyl group, an n-propyl group, an n-butyl group, an n-pentyl group, an n-hexyl group, an isopropyl group, an isobutyl group, a sec-butyl group, a tert-butyl group, and a phenyl group, and preferable examples thereof include a methoxy group, an acetyl group, a propionyl group, a formyl group, a methoxycarbonyl group, an ethoxycarbonyl group, and a benzyloxycarbonyl group.
[0016] Since the blocked isocyanate compound (A) has an ethylenically unsaturated hydrocarbon group, it can form a homopolymer or a copolymer with other monomers such as a monomer (D) having an ethylenically unsaturated bond.
[0017] ((Meth)acrylic acid ester compound (a1) having an isocyanato group) The (meth)acrylic acid ester compound (a1) having an isocyanato group (-NCO) is a compound represented by the following formula (3).
[0018] (R 6 -COO) n R 7 (NCO) m (3) In formula (3), R 6 , R 7 , m and n have the same meanings as the respective symbols in formula (2).
[0019] Examples of the (meth)acrylic acid ester compound (a1) having an isocyanato group represented by formula (3) include 2-methacryloyloxyethyl isocyanate, 3-methacryloyloxy-n-propyl isocyanate, 2-methacryloyloxyisopropyl isocyanate, 4-methacryloyloxy-n-butyl isocyanate, 2-methacryloyloxy-tert-butyl isocyanate, 2-methacryloyloxybutyl-4-isocyanate, 2-methacryloyloxybutyl-3-isocyan ... Acryloyloxybutyl-2-isocyanate, 2-methacryloyloxybutyl-1-isocyanate, 5-methacryloyloxy-n-pentyl isocyanate, 6-methacryloyloxy-n-hexyl isocyanate, 7-methacryloyloxy-n-heptyl isocyanate, 2-(isocyanatoethyloxy)ethyl methacrylate, 3-methacryloyloxyphenyl isocyanate, 4-methacryloyloxyphenyl isocyanate, 2-acryloyloxyethyl isocyanate, 3-acryloyloxy -n-propyl isocyanate, 2-acryloyloxyisopropyl isocyanate, 4-acryloyloxy-n-butyl isocyanate, 2-acryloyloxy-tert-butyl isocyanate, 2-acryloyloxybutyl-4-isocyanate, 2-acryloyloxybutyl-3-isocyanate, 2-acryloyloxybutyl-2-isocyanate, 2-acryloyloxybutyl-1-isocyanate, 5-acryloyloxy-n-pentyl isocyanate, 6-acryloyloxy-n-hexyl Isocyanate, 7-acryloyloxy-n-heptyl isocyanate, 2-(isocyanatoethyloxy)ethyl acrylate, 3-acryloyloxyphenyl isocyanate, 4-acryloyloxyphenyl isocyanate, 1,1-bis(methacryloyloxymethyl)methyl isocyanate, 1,1-bis(methacryloyloxymethyl)ethyl isocyanate, 1,1-bis(acryloyloxymethyl)methyl isocyanate, 1,1-bis(acryloyloxymethyl)ethyl isocyanate.
[0020] Among these, from the viewpoint of ease of production and / or ease of availability of raw materials, 2-acryloyloxyethyl isocyanate, 2-methacryloyloxyethyl isocyanate, 2-(isocyanatoethyloxy)ethyl acrylate, 2-(isocyanatoethyloxy)ethyl methacrylate, or 1,1-bis(acryloyloxymethyl)ethyl isocyanate is preferred, 2-acryloyloxyethyl isocyanate or 2-methacryloyloxyethyl isocyanate is more preferred, and 2-acryloyloxyethyl isocyanate is even more preferred.
[0021] (Phenol compound (a2)) The phenol compound (a2) is used as a blocking agent for the (meth)acrylic acid ester compound (a1) having an isocyanato group, and is represented by the following general formula (4).
[0022] HOPh···(4) In formula (4), Ph represents a phenyl group. The hydrogen atom of the phenyl group may be substituted with a substituent having 1 to 20 carbon atoms. Examples of the substituent include the substituent of the phenyl group in formula (2).
[0023] Among these, ketone compounds such as o-hydroxyacetophenone, m-hydroxyacetophenone, p-hydroxyacetophenone, o-hydroxypropiophenone, m-hydroxypropiophenone, p-hydroxypropiophenone, salicylaldehyde, 3-hydroxybenzaldehyde, and 4-hydroxybenzaldehyde, as well as methyl salicylate, methyl m-hydroxybenzoate, methyl p-hydroxybenzoate, benzyl salicylate, benzyl m-hydroxybenzoate, benzyl p-hydroxybenzoate, isoamyl salicylate, isoamyl m-hydroxybenzoate, isoamyl p-hydroxybenzoate, methyl 5-acetylsalicylate, methyl 6-acetylsalicylate, vanillin, 2-hydroxy-3 Preferred are ester compounds such as o-hydroxybenzaldehyde, 2-hydroxy-5-methoxybenzaldehyde, 3-hydroxy-4-methoxybenzaldehyde, and 2-hydroxy-4-methoxybenzaldehyde, and more preferred are ketone compounds such as o-hydroxyacetophenone, p-hydroxyacetophenone, o-hydroxypropiophenone, p-hydroxypropiophenone, salicylaldehyde, and 3-hydroxybenzaldehyde, and ester compounds such as methyl salicylate, methyl p-hydroxybenzoate, benzyl salicylate, benzyl p-hydroxybenzoate, isoamyl salicylate, isoamyl p-hydroxybenzoate, methyl 5-acetylsalicylate, and vanillin, and even more preferred are methyl salicylate and p-hydroxyacetophenone.
[0024] The blocked isocyanate compound (A) is contained in the blocked isocyanate composition in an amount of preferably 1% by mass or more, more preferably 10% by mass or more, and further preferably 50% by mass or more.
[0025] The blocked isocyanate compound (A) can be produced by a known method, for example, by reacting a (meth)acrylic acid ester compound (a1) having an isocyanato group with a phenol compound (a2) in a reaction vessel as follows.
[0026] The order of adding these compounds to the reactor is not particularly limited. As a method for producing the blocked isocyanate compound (A), for example, the following methods (1) to (3) can be adopted. (1) A method in which a phenol compound (a2) is charged into a reactor, and a (meth)acrylic acid ester compound (a1) having an isocyanato group is added thereto under stirring to cause a reaction. (2) A method in which a (meth)acrylic ester compound (a1) having an isocyanato group is charged into a reactor, and a phenol compound (a2) is added thereto under stirring to cause a reaction. (3) A method in which a phenol compound (a2) and a (meth)acrylic acid ester compound (a1) having an isocyanato group are simultaneously added to a reactor under stirring to cause a reaction.
[0027] The reaction temperature of the (meth)acrylic acid ester compound (a1) having an isocyanato group and the phenol compound (a2) is preferably from -10°C to 90°C, more preferably from 5°C to 70°C, and even more preferably from 10°C to 40°C. If the reaction temperature is -10°C or higher, the reaction rate can be improved, and the blocked isocyanate compound (A) can be obtained with good productivity, which is preferable. Also, if the reaction temperature is 90°C or lower, the reverse reaction is unlikely to proceed, and the compound can be obtained with high purity, which is preferable.
[0028] The reaction is usually carried out until the (meth)acrylic ester compound (a1) or the phenol compound (a2) having an isocyanato group disappears. The reaction time is not particularly limited, but is usually preferably 30 minutes or more and 168 hours or less. The disappearance of the phenol compound (a2) is considered to be when, for example, the result of high performance liquid chromatography analysis shows that the phenol compound (a2) is 2 parts by mass or less based on 100 parts by mass of the blocked isocyanate compound (A). On the other hand, the disappearance of the (meth)acrylic ester compound (a1) having an isocyanato group is considered to be when, for example, the result of IR measurement shows that the (meth)acrylic ester compound (a1) having an isocyanato group is 2% by mass or less based on the absorption due to the isocyanato group. The reaction time also includes the time for adding the (meth)acrylic ester compound (a1) having an isocyanato group and the phenol compound (a2) by dropwise addition, etc.
[0029] In the above production, when m=1 in the above formula (3), the phenol compound (a2) is preferably contacted with the (meth)acrylic acid ester compound (a1) having an isocyanato group at 0.1 to 4.0 times by mole, more preferably at 0.5 to 3.0 times by mole, even more preferably at 0.75 to 1.25 times by mole, and particularly preferably at 1.00 times by mole. The reaction ratio of these compounds is theoretically 1:1 (molar ratio), but the reaction can be smoothly carried out by contacting them at a molar ratio within the above range. In addition, when m=2 in the above formula (3), the amount of the phenol compound (a2) contacted with the (meth)acrylic acid ester compound (a1) having an isocyanato group may be twice the amount of the above m=1.
[0030] It is also preferable to add a polymerization inhibitor (C) to the reaction system for producing the blocked isocyanate compound (A), which will be described later. The polymerization inhibitor (C) may be used after the production of the blocked isocyanate compound (A), but it is more preferable to use it during the production of the blocked isocyanate compound (A). The polymerization inhibitor quickly reacts with the radical generated from the (meth)acryloyl group in the blocked isocyanate compound (A) in the radical polymerization reaction, and therefore can stabilize the blocked isocyanate compound (A) so that the polymerization reaction by the (meth)acryloyl group does not proceed. The polymerization inhibitor will be described in detail later.
[0031] The method of adding the polymerization inhibitor (C) is not particularly limited, and examples thereof include a method of adding it to the reactor together with the phenol compound (a2); a method of mixing it with the (meth)acrylic acid ester compound (a1) having an isocyanato group and adding it to the reactor; a method of adding it to both the phenol compound (a2) and the (meth)acrylic acid ester compound (a1) having an isocyanato group and adding each of them to the reactor; and a method of adding it to the generated blocked isocyanate compound (A) after the reaction is completed.
[0032] In the above-mentioned method for producing the blocked isocyanate compound (A), the blocked isocyanate compound (A) can be used as a solvent or dispersion medium, the reaction can be carried out without a solvent, or a known organic solvent can be used as the solvent or dispersion medium. The solvent is not particularly limited, but examples thereof include alcohol-based solvents such as cellosolve, methyl cellosolve, butyl cellosolve, propylene glycol monomethyl ether, methanol, ethanol, propanol, isopropanol, butanol, pentanol, hexanol, octanol, nonanol, decanol, benzyl alcohol, and hexylene glycol; ketone-based solvents such as acetone, methyl ethyl ketone, methyl isobutyl ketone, and cyclohexanone; ester-based solvents such as ethyl acetate, butyl acetate, ethyl lactate, γ-butyrolactone, propylene glycol monomethyl ether acetate, and propylene glycol monobutyl ether acetate; ether-based solvents such as ethylene glycol dimethyl ether, ethylene glycol dibutyl ether, and diethylene glycol dimethyl ether; aromatic hydrocarbon-based solvents such as benzene, toluene, and xylene; and amide-based solvents such as dimethylformamide, dimethylacetamide, and N-methylpyrrolidone. Halogen-substituted compounds of these solvents may also be used. Among these, ester solvents such as propylene glycol monomethyl ether acetate and ketone solvents such as acetone are preferred, and propylene glycol monomethyl ether acetate is more preferred. These may be used alone or in combination of two or more.
[0033] A catalyst and additives may be added to the reaction system for producing the blocked isocyanate compound (A). Examples of the catalyst include dibutyltin dilaurate.
[0034] [Stabilizer (B)] The stabilizer (B) used in the present invention is a salt of a compound (b1) represented by the following general formula (1) and an acid (b2), and the pKa of the acid (b2) is 2.0 or less.
[0035] R 1 N=CR2 -NR 3 R 4 (1) In the formula, R 2 is a hydrogen atom, a hydrocarbon group having 1 to 20 carbon atoms, or -NR 5 2 R is a group represented by the formula: 1 , R 3 , R 4 and R 5 is a hydrogen atom or a hydrocarbon group having 1 to 20 carbon atoms, and two R 5 may be the same or different. 1 , R 2 , R 3 , R 4 , and two R 5 Any two or more of the groups may be bonded to form a cyclic structure.
[0036] The compound (b1) may be a compound represented by the general formula (1-2).
[0037] R 1a N=CR 2a -NR 3a R 4a (1-2) In the formula, R 1a , R 2a , R 3a and R 4a is a hydrocarbon group, R 1a and R 4a and R 2a and R 3a and each bond to form a ring structure, and R 1a and R 4a The sum of the carbon numbers of R is 3 to 20, preferably 5 to 10. 2a and R 3a The sum of the carbon numbers is 3 to 20, and preferably 5 to 10.
[0038] Of the compounds (b1) represented by general formula (1), 1,8-diazabicyclo[5.4.0]-undecene-7, 1,5-diazabicyclo[4.3.0]-5-nonene, and 1,1,3,3-tetramethylguanidine are preferred, and 1,8-diazabicyclo[5.4.0]-undecene-7 is more preferred.
[0039] The acid (b2) is an acid having a pKa of 2.0 or less at 25° C. Among the acids having a pKa of 2.0 or less, paratoluenesulfonic acid, trifluoromethanesulfonic acid, benzenesulfonic acid, methanesulfonic acid, 10-camphorsulfonic acid, hydrochloric acid and sulfuric acid are preferred, and paratoluenesulfonic acid is more preferred. The acids having a pKa of 2.0 or less at 25° C. include those having a pKa of 2.0 or less in an aqueous solution and those that are too acidic to be measured in an aqueous solution and have a pKa of 2.0 or less in an aqueous solution calculated from the measurement results in an organic solvent.
[0040] In the blocked isocyanate composition, the amount of the stabilizer (B) is 100 ppm by mass or more to 1.00 × 10 5 Mass ppm or less is preferable, and 1.00 x 10 3 Mass ppm or more 1.00×10 4 It is more preferable that the amount of the stabilizer (B) is 100 ppm by mass or more relative to the blocked isocyanate compound (A) because the blocked isocyanate compound (A) is stable during storage. It is preferable that the amount of the stabilizer (B) is 1.00 × 10 5 If it is not more than ppm by mass, the blocking agent is easily desorbed when the blocked isocyanate compound (A) is heated, which is preferable.
[0041] [Polymerization inhibitor (C)] The blocked isocyanate composition in one embodiment of the present invention may contain a polymerization inhibitor (C).
[0042] As the polymerization inhibitor (C), a commonly used one such as phenothiazine, p-methoxyphenol, or 2,6-di-tert-butyl-4-methylphenol (hereinafter also referred to as "BHT") can be used.
[0043] The amount of the polymerization inhibitor (C) used varies depending on the types of the phenol compound (a2) and the (meth)acrylic acid ester compound (a1) having an isocyanato group, but is preferably 10 ppm by mass or more and 2.00×10 or less as the total amount during and after the production of the blocked isocyanate compound (A). 4 Preferably, 50 ppm by mass or less, and 1.00×10 4 ppm by mass is more preferable, and 100 ppm by mass or more is 1.00×10 3 Parts per million by weight is more preferred.
[0044] [Monomer (D) having an ethylenically unsaturated bond] The blocked isocyanate composition in one embodiment of the present invention may contain a monomer (D) having an ethylenically unsaturated bond. The monomer (D) having an ethylenically unsaturated bond does not include the blocked isocyanate compound (A) and the (meth)acrylic acid ester compound (a1) having an isocyanato group.
[0045] The monomer (D) having an ethylenically unsaturated bond is not particularly limited as long as it has an ethylenically unsaturated bond and is a compound capable of copolymerizing with the blocked isocyanate compound (A).
[0046] Examples of the monomer (D) having an ethylenically unsaturated bond include (meth)acrylic acid esters and derivatives thereof, styrene and derivatives thereof, vinyl acetate and derivatives thereof, (meth)acrylonitrile and derivatives thereof, vinyl esters of organic carboxylic acids and derivatives thereof, allyl esters of organic carboxylic acids and derivatives thereof, dialkyl esters of fumaric acid and derivatives thereof, dialkyl esters of itaconic acid and derivatives thereof, N-vinylamide derivatives of organic carboxylic acids, maleic acid and derivatives thereof, terminally unsaturated hydrocarbons and derivatives thereof, and the like.
[0047] Examples of (meth)acrylic acid esters and derivatives thereof include methyl (meth)acrylate, ethyl (meth)acrylate, n-propyl (meth)acrylate, isopropyl (meth)acrylate, n-butyl (meth)acrylate, isobutyl (meth)acrylate, sec-butyl (meth)acrylate, hexyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, decyl (meth)acrylate, isobornyl (meth)acrylate, cyclohexyl (meth)acrylate, phenyl (meth)acrylate, benzyl (meth)acrylate, ) Monofunctional (meth)acrylates such as 2-hydroxyethyl acrylate, 2-hydroxypropyl (meth)acrylate, 3-hydroxypropyl (meth)acrylate, 2-hydroxybutyl (meth)acrylate, 2-hydroxyphenylethyl (meth)acrylate, 4-hydroxybutyl (meth)acrylate, N,N-dimethyl (meth)acrylamide, N,N-diethyl (meth)acrylamide, and N-acryloylmorpholine; and polyfunctional (meth)acrylates such as ethylene glycol di(meth)acrylate, propylene glycol di(meth)acrylate, 1,4 butanediol di(meth)acrylate, diethylene glycol di(meth)acrylate, triethylene glycol di(meth)acrylate, trimethylolpropane di(meth)acrylate, trimethylolpropane tri(meth)acrylate, pentaerythritol penta(meth)acrylate, and pentaerythritol hexa(meth)acrylate.
[0048] Examples of styrene and its derivatives include styrene, 2,4-dimethyl-α-methylstyrene, o-methylstyrene, m-methylstyrene, p-methylstyrene, 2,4-dimethylstyrene, 2,4,6-trimethylstyrene, o-chlorostyrene, 2-vinylbiphenyl, 1-vinylanthracene, p-isopropenyltoluene, divinylbenzene, and divinylbiphenyl.
[0049] Examples of vinyl esters of organic carboxylic acids and their derivatives include vinyl acetate, vinyl propionate, vinyl butyrate, vinyl benzoate, and vinyl adipate.
[0050] Examples of allyl esters of organic carboxylic acids and derivatives thereof include allyl acetate, allyl benzoate, diallyl adipate, diallyl terephthalate, diallyl isophthalate, and diallyl phthalate.
[0051] Examples of dialkyl esters of fumaric acid and derivatives thereof include dimethyl fumarate, diethyl fumarate, di-2-ethylhexyl fumarate, dibenzyl fumarate, and the like.
[0052] Examples of dialkyl esters of maleic acid and derivatives thereof include dimethyl maleate, diethyl maleate, di-2-ethylhexyl maleate, and dibenzyl maleate.
[0053] Examples of dialkyl esters of itaconic acid and derivatives thereof include dimethyl itaconate, diethyl itaconate, 2-ethylhexyl itaconate, dibenzyl itaconate, and the like.
[0054] An example of the N-vinylamide derivative of an organic carboxylic acid is N-methyl-N-vinylacetamide.
[0055] Examples of maleimide and its derivatives include N-phenylmaleimide and N-cyclohexylmaleimide.
[0056] Terminally unsaturated hydrocarbons and their derivatives include 1-butene, 1-pentene, 1-hexene, vinylcyclohexane, vinyl chloride, allyl alcohol, and the like.
[0057] Of these, (meth)acrylic acid esters and derivatives thereof are preferred, and methyl (meth)acrylate, ethyl (meth)acrylate, n-propyl (meth)acrylate, isopropyl (meth)acrylate, n-butyl (meth)acrylate, isobutyl (meth)acrylate, and sec-butyl (meth)acrylate are more preferred.
[0058] The monomer (D) having an ethylenically unsaturated bond may be used alone or in combination of two or more kinds.
[0059] The total amount of the monomer (D) having an ethylenically unsaturated bond relative to the blocked isocyanate compound (A) is 0 mol% or more and 5.0 × 10 4 mol% or less is preferable, and 50mol% or more is 1×10 4 mol% or less is more preferable, and 100mol% or more 2×10 3 It is more preferably mol % or less.
[0060] [Other polymers (E)] The blocked isocyanate composition in one embodiment of the present invention may contain another polymer (E). The other polymer (E) is a polymer other than the polymer (F) obtained by polymerizing the blocked isocyanate compound (A). The other polymer is not particularly limited, and examples thereof include polyols, polyamines, polythiols, etc.
[0061] The polyol is not particularly limited, and various known polyols can be used.Specific examples include alkyl polyols such as ethylene glycol, 1,4-butanediol, 1,5-pentanediol, 1,6-hexanediol, trimethylolpropane, ditrimethylolpropane, and dipentaerythritol, polyester polyols, polycarbonate diols, polybutadiene diols, trishydroxyethyl isocyanurate, bisphenol A, perfluoropolyols, and the so-called ethylene oxide-modified polyols, propylene oxide-modified polyols, and caprolactone-modified polyols in which the alkyl chains of these polyols are extended using ethylene oxide, propylene oxide, caprolactone, or the like.
[0062] The polyamine is not particularly limited, and various known polyamines can be used.Specific examples include ethylenediamine, 1,3-diaminopropane, 1,4-diaminobutane, 1,5-diaminopentane, 1,6-diaminohexane, spermidine, spermine, N,N'-bis(2-aminoethyl)-1,3-propanediamine, N,N'-bis(3-aminopropyl)-1,4-butanediamine, N,N'-bis(3-aminopropyl)ethylenediamine, agmatine, 3,3'-diaminodipropylamine, and diethylenetriamine.
[0063] The polythiol is not particularly limited, and various known ones can be used.Specific examples include 1,2-ethanedithiol, 1,3-propanedithiol, 1,4-butanedithiol, 2,3-butanedithiol, 1,5-pentanedithiol, 1,6-hexanedithiol, 1,7-heptanedithiol, 1,8-octanedithiol, 1,9-nonanedithiol, 1,10-decanedithiol, 4,4'-thiobisbenzenethiol, tris[2-(3-mercaptopropionyloxy)ethyl]isocyanurate, 1,3,5-benzenetrithiol, pentaerythritol tetrakis(mercaptoacetate), ethylene glycol bis(3-mercaptopropionate), 4,5-bis(mercaptomethyl)-o-xylene, 4,4'-biphenanthroline, and the like. nyldithiol, ethylene bis(thioglycolate), pentaerythritol tetra(3-mercaptopropionate), 1,4-butanediol bis(thioglycolate), 1,3-benzenedithiol, dithiothreitol, dithioerythritol, 1,4-benzenedithiol, bis(2-mercaptoethyl)sulfide, 1,5-dimercaptonaphthalene, 3,7-dithia-1,9-nonanedithiol, 3,6-dioxa-1,8-octanedithiol, trimethylolpropane tris(3-mercaptopropionate), dipentaerythritol hexakis(3-mercaptopropionate), trimethylolpropane tris(thioglycolate).
[0064] The amount of the other polymer (E) is preferably 10 to 10,000 parts by mass, more preferably 20 to 1,000 parts by mass, based on 100 parts by mass of the total of the blocked isocyanate compound (A) and the polymer (F). In the blocked isocyanate polymer described below, the amount of the other polymer (E) is preferably 10 to 10,000 parts by mass, more preferably 20 to 1,000 parts by mass, based on 100 parts by mass of the polymer derived from the blocked isocyanate compound (A).
[0065] [Polymer (F)] The blocked isocyanate composition may contain a polymer (F) obtained by polymerizing the blocked isocyanate compound (A). The polymer (F) includes a homopolymer of the blocked isocyanate compound (A) and a copolymer obtained by copolymerizing the blocked isocyanate compound (A) with a monomer (D) having an ethylenically unsaturated bond, which will be described later. The polymerization can be carried out by a known method such as photopolymerization, radical polymerization, or thermal polymerization. In the case of radical polymerization, a radical polymerization initiator exemplified in the section [Blocked isocyanate polymer], which will be described later, can be used.
[0066] [Storage conditions] The storage temperature of the blocked isocyanate composition is preferably from 0° C. to 50° C. For example, the temperature inside a container during container transport is usually within this temperature range, so that the blocked isocyanate compound is unlikely to decompose during transport, and changes in viscosity of the blocked isocyanate composition are suppressed.
[0067] [Application] The blocked isocyanate composition can be used as a raw material for adhesives, coating agents, molding materials, etc. For example, the blocked isocyanate composition can be used for a cured film produced by polymerizing a polymerizable component in the blocked isocyanate composition to produce a blocked isocyanate polymer, and then curing the polymer.
[0068] <Blocked isocyanate polymer> One embodiment of the present invention is a blocked isocyanate polymer obtained by polymerizing the polymerizable components in the blocked isocyanate composition described above. Polymerization also includes copolymerization. The polymerizable components in the blocked isocyanate composition include a blocked isocyanate compound (A) and a monomer (D) having an ethylenically unsaturated bond. The blocked isocyanate polymer may include a polymer (F) present in the blocked isocyanate composition.
[0069] In order to radically polymerize the polymerizable components in the blocked isocyanate composition, it is preferable to use a radical polymerization initiator. The radical polymerization initiator is not particularly limited, but examples thereof include organic peroxides such as benzoyl peroxide, lauroyl peroxide, caproyl peroxide, tert-butyl peroxyoctoate, and diacetyl peroxide; azobisisobutyronitrile, azobis-α,γ-dimethylvaleronitrile, 2,2'-azobis(isobutyric acid) dimethyl, azobisisobutyronitrile, 1,1'-azobis(cyclohexane-1-carbonitrile), 2,2'-azobis(2-methylbutyronitrile), 2,2'-azobis(4-methoxy-2,4-dimethylvaleronitrile), 2,2'-azobis(2,4-dimethylvaleronitrile), 2,2'-azobis(isobutyronitrile), 2,2'-azobis(2-methylbutyronitrile), 2,2'-azobis[2-(2-imidazolin-2-yl)propane], and the like. 2,2'-azobis[2-(2-imidazolin-2-yl)propane]dihydrochloride, 2,2'-azobis[2-(2-imidazolin-2-yl)propane]disulfate dihydrate, 2,2'-azobis[2-(2-imidazolin-2-yl)propane], 2,2'-azobis(2-methylpropionamidine)dihydrochloride, 2,2'-azobis[N-(2-carboxyethyl)-2-methylpropionamidine]nhydrate, 2,2'-azobis[2-methyl-N-( azo compounds such as 2,2'-azobis[N-(2-hydroxyethyl)propionamide], 2,2'-azobis(N-(2-propenyl)-2-methylpropionamide], 2,2'-azobis(N-butyl-2-methylpropionamide), and 4,4'-azobis(4-cyanovaleric acid); dialkyl peroxydicarbonates such as diisopropyl peroxycarbonate, and redox initiators.
[0070] The radical polymerization initiator is preferably used in the range of 0.01 to 15 parts by mass, more preferably 0.1 to 10 parts by mass, per 100 parts by mass of the blocked isocyanate compound (A) monomer in the blocked isocyanate composition.
[0071] The polymerization can be carried out by a known method, but if the reaction is carried out at a temperature higher than necessary, the blocking agent (phenol compound (a2)) of the (meth)acrylic acid ester compound (a1) having an isocyanato group may partially dissociate from the blocked isocyanate compound (A), and the dissociated blocking agent may act as a chain transfer agent, resulting in a broadening of the molecular weight distribution, and the resin may gel due to crosslinking derived from the isocyanato group of the (meth)acrylic acid ester compound (a1) having a free isocyanato group and the amino group generated by decomposition of the isocyanato group. Therefore, it is preferable to carry out the polymerization at a temperature of 120°C or less.
[0072] The weight average molecular weight of the blocked isocyanate polymer is preferably 100,000 or less, more preferably 50,000 or less, and particularly preferably 30,000 or less, in order to suppress an increase in the viscosity of the polymer. The weight average molecular weight of the blocked isocyanate polymer is preferably 1,000 or more. The weight average molecular weight can be measured by gel permeation chromatography (GPC method).
[0073] <Cured film> One embodiment of the present invention is a cured film obtained by curing the above-mentioned blocked isocyanate composition at a predetermined temperature. When curing, it is preferable to add a base to the blocked isocyanate composition in order to improve the curing speed.
[0074] The base is not particularly limited, and examples thereof include primary, secondary, and tertiary amines such as ammonia, methylamine, ethylamine, monoethanolamine, cyclohexylamine, dimethylamine, diethylamine, methylethanolamine, diethanolamine, ethylenediamine, and triethylamine; 1,5-diazabicyclo[4.3.0]-nonene-5, 1,8-diazabicyclo[5.4.0]-undecene-7, 1,5-diazabicyclo[4.3.0]-nonene-5, 1,8-diazabicyclo[5.4.0]-undecene-7, and ... hardening accelerator compounds that become bases when heated, such as salts of 1,8-diazabicyclo[5.4.0]-undecene-7 and the like phenol salts, 1,8-diazabicyclo[5.4.0]-undecene-7 phenol salts, 1,8-diazabicyclo[5.4.0]-undecene-7 octylate salts, 1,8-diazabicyclo[5.4.0]-undecene-7 paratoluenesulfonate salts, and 1,8-diazabicyclo[5.4.0]-undecene-7 formate salts, and inorganic compounds such as sodium hydroxide and potassium hydroxide. Of these, 1,8-diazabicyclo[5.4.0]-undecene-7 and its phenol salts are preferred.
[0075] The reaction temperature during curing is not particularly limited, but is preferably from 60° C. to 140° C., and more preferably from 80° C. to 120° C. The reaction time during curing is not particularly limited, but is preferably from 0.5 hours to 5 hours.
[0076] Since the blocked isocyanate composition can form a cured film in this manner, it can be suitably used as an adhesive, a coating agent, a molding material, and the like.
[0077] <Method for producing a composition containing an isocyanate compound or an isocyanato group-containing (co)polymer, etc.> One embodiment of the present invention is a method for producing a composition containing an isocyanate compound or an isocyanato group-containing (co)polymer and a stabilizer (B), which comprises holding the above-mentioned blocked isocyanate composition at 25° C. or higher for 10 days or more (hereinafter referred to as "first-stage holding"), and then holding the composition at 80° C. or higher for 0.5 hours or more (hereinafter referred to as "second-stage holding") to eliminate the phenol compound (a2) from the blocked isocyanate compound (A) or polymer (F). The isocyanate compound is a compound in which the phenol compound (a2) has been eliminated from the blocked isocyanate compound (A). The isocyanato group-containing (co)polymer means an isocyanato group-containing polymer or an isocyanato group-containing copolymer. The isocyanato group-containing polymer is a polymer in which the phenol compound (a2) has been eliminated from a homopolymer of the blocked isocyanate compound (A). The isocyanato group-containing copolymer is a copolymer in which the phenol compound (a2) is eliminated from a copolymer of a blocked isocyanate compound (A) and a monomer (D) having an ethylenic unsaturated bond. The first-stage holding and the second-stage holding are preferably carried out under dry air (dew point 0°C). The first-stage holding is preferably carried out at 25°C or higher and 50°C or lower for 10 days or longer and 45 days or shorter. The second-stage holding is preferably carried out at 80°C or higher and 200°C or lower for 0.5 hours or longer and 20 hours or shorter. In terms of improving the elimination rate, it is preferable to add a base during the second-stage holding. Here, the base may be, for example, the base described in the above [Cured Film] section. EXAMPLES
[0078] The present invention will be described in more detail below with reference to examples and comparative examples, but the present invention is not limited to the following examples. In the examples, measurements and tests were carried out by the following methods.
[0079] [viscosity] The viscosity was measured under the following conditions using a B-type viscometer specified in JIS K 5600-2-3:2014. The sample was placed in the viscometer and the viscosity was recorded after 10 minutes. Viscometer type: Cone-plate type Cone type: CPA-52Z Cone angle: 3° Cone diameter: 12mm Sample volume: 0.5mL Rotation speed: 50 rpm Temperature: 23℃
[0080] [Storage stability test] The blocked isocyanate composition was left to stand in a sealed container and exposed to dry air (dew point: 0° C.) and kept at 40° C. for 2 weeks, and the residual rate of the blocked isocyanate compound was determined. The residual rate (%) was calculated by (amount of the compound to be measured at the end of the storage stability test)÷(amount of the compound to be measured at the start of the storage stability test)×100.
[0081] [Deblocking test] The blocked isocyanate composition was heated at 100° C. for 1 hour while exposed to dry air (dew point: 0° C.) in a closed container, and the conversion rate of the blocked isocyanate compound was determined. The conversion rate (%) was calculated by {(amount of the compound to be measured at the start of the deblocking test)-(amount of the compound to be measured at the end of the deblocking test)}÷(amount of the compound to be measured at the start of the deblocking test)×100.
[0082] [Quantitative determination of compound amount] The quantitative measurement of the blocked isocyanate compound, which is the measurement target compound in the storage stability test and the deblocking test, was carried out by HPLC under the following conditions. Equipment: Agilent 1200 Series Column: Showa Denko K.K. Shodex (registered trademark) KF-801+KF-801+KF-801+KF-801 Eluent: Tetrahydrofuran Flow rate: 0.8mL / min Injection volume: 0.01mL Column temperature: 40℃ Detector: RI (Differential Refractive Index) Optical system temperature: 40℃
[0083] [Production Example 1] A 2L separable flask equipped with a stirrer, a thermometer, a dropping funnel, and a reflux condenser was charged with 136.15 g of p-hydroxyacetophenone (Kanto Chemical Co., Ltd.: phenol compound (a2)), 0.07 g of BHT (Oxalis Chemicals Co., Ltd.), 300.05 g of acetone (Kanto Chemical Co., Ltd.), and 1.44 g of dibutyltin dilaurate (hereinafter also referred to as "DBTDL") (Nitto Kasei Co., Ltd.), and cooled to 15°C. 141.08 g of 2-acryloyloxyethyl isocyanate (Showa Denko K.K., AOI-VM (registered trademark): acrylic acid ester compound (a1) having an isocyanato group) was added dropwise using a dropping funnel over a period of 2 hours, and the resulting reaction liquid was aged at 25°C for 2 days. 600 mL of hexane (Kanto Chemical Co., Ltd.) was added to the aged mixture to precipitate a compound represented by the following formula (i) (blocked isocyanate compound (A), hereinafter also referred to as "AOI-PAP"). The precipitated AOI-PAP was filtered, and the AOI-PAP was washed by adding 200 mL of hexane three times, and then dried under reduced pressure at 25°C and 1.0 kPa for 2.5 hours to obtain 181.12 g of AOI-PAP.
[0084] [ka]
[0085] [Comparative Manufacturing Example 1] 579.4g of 3,5-dimethylpyrazole (Otsuka Chemical Co., Ltd.), 0.60g of BHT (Oxalis Chemicals Co., Ltd.), and 775.0g of propylene glycol monomethyl ether acetate (Kanto Chemical Co., Ltd.) were added to a 5L separable flask equipped with a stirrer, a thermometer, a dropping funnel, and a reflux condenser, and cooled to 15°C. After cooling, 867.0g of 2-acryloyloxyethyl isocyanate (Showa Denko K.K., AOI-VM (registered trademark)) was added dropwise over 80 minutes using a dropping funnel. The mixture after the dropping was cooled to 0°C, 1600g of hexane (Kanto Chemical Co., Ltd.) was added, and the mixture was aged for one day. From the mixture after aging, a compound represented by the following formula (ii) (hereinafter also referred to as "AOI-BP") was recovered by filtration, and washing was performed three times using 800g of hexane. The washed AOI-BP was dried under reduced pressure at 40° C. and 1.0 kPa for 5 hours to obtain 1146.55 g of AOI-BP.
[0086] [ka]
[0087] [Example 1] In a 50 mL screw tube, 4.72 g of AOI-PAP produced in Production Example 1, 2.70 g of n-decanol (Kanto Chemical Co., Ltd.), 17.30 g of o-dichlorobenzene (Kanto Chemical Co., Ltd.), 0.0218 g of paratoluenesulfonate of 1,8-diazabicyclo[5.4.0]-undecene-7 (compound (b1) represented by general formula (1)) (U-CAT SA (registered trademark) 506, manufactured by San-Apro Co., Ltd.; stabilizer (B)), and 0.0210 g of BHT (Oxalis Chemicals Co., Ltd.: polymerization inhibitor (C)) were added to prepare a blocked isocyanate composition of the present invention. The ratio of paratoluenesulfonate of 1,8-diazabicyclo[5.4.0]-undecene-7 to AOI-PAP was 4.60 x 10 3The concentration was ppm by mass. A storage stability test was performed using the obtained composition, and the residual rate of AOI-PAP was 98.7%. A deblocking test was performed, and the conversion rate of AOI-PAP was 3.4%. The pKa of paratoluenesulfonic acid (acid (b2)) is -2.8.
[0088] [Comparative Example 1] 4.72 g of AOI-PAP produced in Production Example 1, 2.70 g of n-decanol (Kanto Chemical Co., Ltd.), 17.30 g of o-dichlorobenzene (Kanto Chemical Co., Ltd.), and 0.0224 g of BHT (Oxalis Chemicals Co., Ltd.) were added to a 50 mL screw tube bottle to prepare the composition of Comparative Example 1. When a storage stability test was carried out using the obtained composition, the residual rate of AOI-PAP was 71.5%.
[0089] [Comparative Example 2] 4.72 g of AOI-PAP produced in Production Example 1, 2.70 g of n-decanol (Kanto Chemical Co., Ltd.), 17.31 g of 2-dichlorobenzene (Kanto Chemical Co., Ltd.), 0.0218 g of phenol salt of 1,8-diazabicyclo[5.4.0]-undecene-7 (U-CAT SA (registered trademark) 1, San-Apro Co., Ltd.), and 0.0210 g of BHT (Oxalis Chemicals Co., Ltd.) were added to a 50 mL screw tube bottle to prepare a composition of Comparative Example 2. When a storage stability test was performed using the obtained composition, the residual rate of AOI-PAP was 21.7%. The conversion rate of AOI-PAP was 73.1%. The pKa of phenol is 9.87.
[0090] [Comparative Example 3] 4.72 g of AOI-PAP produced in Production Example 1, 2.70 g of n-decanol (Kanto Chemical Co., Ltd.), 17.31 g of o-dichlorobenzene (Kanto Chemical Co., Ltd.), 0.0218 g of 1,8-diazabicyclo[5.4.0]-undecene-7 (San-Apro Co., Ltd.), and 0.0210 g of BHT (Oxalis Chemicals Co., Ltd.) were added to a 50 mL screw tube bottle to prepare the composition of Comparative Example 3. When a storage stability test was performed using the obtained composition, the residual rate of AOI-PAP was 22.6%.
[0091] [Comparative Example 4] 4.72 g of AOI-PAP produced in Production Example 1, 2.70 g of n-decanol (Kanto Chemical Co., Ltd.), 17.31 g of o-dichlorobenzene (Kanto Chemical Co., Ltd.), 0.020 g of DBTDL (Nitto Kasei Co., Ltd.), and 0.0210 g of BHT (Oxalis Chemicals Co., Ltd.) were added to a 50 mL screw tube bottle to prepare the composition of Comparative Example 4. When a storage stability test was carried out using the obtained composition, the residual rate of AOI-PAP was 50.0%.
[0092] [Comparative Example 5] 4.05 g of AOI-BP produced in Comparative Production Example 1, 2.69 g of n-decanol (Kanto Chemical Co., Ltd.), 17.30 g of o-dichlorobenzene (Kanto Chemical Co., Ltd.), 0.0205 g of U-CAT SA506 (San-Apro Co., Ltd.), and 0.0232 g of BHT (Oxalis Chemicals Co., Ltd.) were added to a 50 mL screw tube bottle to prepare the composition of Comparative Example 5. When a storage stability test was carried out using the obtained composition, the residual rate of AOI-BP was 94.3%.
[0093] [Comparative Example 6] 4.05 g of AOI-BP produced in Comparative Production Example 1, 2.69 g of n-decanol (Kanto Chemical Co., Ltd.), 17.30 g of o-dichlorobenzene (Kanto Chemical Co., Ltd.), and 0.0232 g of BHT (Oxalis Chemicals Co., Ltd.) were added to a 50 mL screw tube bottle to prepare the composition of Comparative Example 6. When a storage stability test was carried out using the obtained composition, the residual rate of AOI-BP was 93.6%. The results of the residual ratio of the blocked isocyanate compound in Example 1 and Comparative Examples 1 to 6 are shown in Table 1.
[0094] [Table 1]
[0095] [Example 2] 312 g of propylene glycol monomethyl ether acetate (Kanto Chemical Co., Ltd.) was added to a 1 L separable flask and heated to 90°C. A mixed solution consisting of 60 g of AOI-PAP produced in Production Example 1, 111 g of methyl methacrylate (Kanto Chemical Co., Ltd., monomer (D) having an ethylenic unsaturated bond), 129 g of butyl acrylate (Kanto Chemical Co., Ltd., monomer (D) having an ethylenic unsaturated bond), and 12.00 g of 2,2'-azobis(isobutyrate)dimethyl (FUJIFILM Wako Pure Chemical Co., Ltd., hereinafter also referred to as "V-601") was dropped thereto over 2 hours. The resulting reaction solution was aged for 30 minutes, and then a mixed solution consisting of 3.00 g of V-601 and 12 g of propylene glycol monomethyl ether acetate (Kanto Chemical Co., Ltd.) was added to the reaction solution and aged for another 3 hours. This was cooled to room temperature to obtain an AOI-PAP copolymer (polymer (F)).
[0096] 32.27 g of the above AOI-PAP copolymer, 3.03 g of polyethylene glycol (PEG600, manufactured by Kanto Chemical Co., Ltd., compound (E) having active hydrogen), and 0.0276 g of U-CAT SA (registered trademark) 506 (manufactured by San-Apro Co., Ltd.) were mixed to prepare a homogeneous solution, thereby preparing a blocked isocyanate composition of the present invention. The resulting solution was kept at 40°C and allowed to stand for 3 weeks. The viscosity of the solution before and after standing was measured at room temperature, and was found to be 250.0 mPa s and 256.0 mPa s, respectively.
[0097] [Comparative Example 7] 32.28 g of the AOI-PAP copolymer synthesized in Example 2 and 3.03 g of polyethylene glycol (PEG600, manufactured by Kanto Chemical Co., Ltd.) were mixed to prepare a homogeneous solution, thereby obtaining the composition of Comparative Example 7. The resulting solution was kept at 40°C and stored for three weeks. The viscosity of the solution before and after standing was measured at room temperature, and was found to be 246.1 mPa s and 307.6 mPa s, respectively.
[0098] [Comparative Example 8] 32.26 g of the AOI-PAP copolymer synthesized in Example 2, 3.02 g of polyethylene glycol (PEG600, manufactured by Kanto Chemical Co., Ltd.), and 0.0279 g of acetic acid (manufactured by Kanto Chemical Co., Ltd.) were mixed to prepare a homogeneous solution, thereby obtaining a composition of Comparative Example 8. The resulting solution was kept at 40°C and stored for three weeks. The viscosity of the solution before and after standing was measured at room temperature, and was found to be 236.1 mPa s and 315.5 mPa s, respectively. The pKa of acetic acid is 4.76. Table 2 shows the results of the viscosity before and after standing in Example 2 and Comparative Examples 7 and 8.
[0099] [Table 2]
[0100] [Example 3] In a 50 mL eggplant flask, 4.72 g of AOI-PAP synthesized in Production Example 1, 2.71 g of n-decanol (Kanto Chemical Co., Ltd.), 17.30 g of o-dichlorobenzene (Kanto Chemical Co., Ltd.), 0.0236 g of U-CAT SA (registered trademark) 506 (San-Apro Co., Ltd.), 0.0237 g of U-CAT SA (registered trademark) 1 (San-Apro Co., Ltd.), and 0.0215 g of BHT (Oxalis Chemicals Co., Ltd.) were mixed to prepare a blocked isocyanate composition of the present invention. When a deblocking test was performed using the obtained composition, the conversion rate of AOI-PAP was 69.2%.
Claims
1. A blocked isocyanate composition comprising a blocked isocyanate compound (A) and a stabilizer (B), the blocked isocyanate compound (A) is a compound formed by urethane bonding between an isocyanato group of a (meth)acrylic ester compound (a1) having an isocyanato group and a hydroxyl group of a phenol compound (a2); the stabilizer (B) is a salt of a compound (b1) represented by general formula (1) and an acid (b2), and the pKa of the acid (b2) is 2.0 or less; the (meth)acrylic acid ester compound (a1) having an isocyanato group is 2-acryloyloxyethyl isocyanate, 2-methacryloyloxyethyl isocyanate, 2-(isocyanatoethyloxy)ethyl acrylate, 2-(isocyanatoethyloxy)ethyl methacrylate, or 1,1-bis(acryloyloxymethyl)ethyl isocyanate; the phenol compound (a2) is o-hydroxyacetophenone, m-hydroxyacetophenone, or p-hydroxyacetophenone; The compound (b1) is 1,8-diazabicyclo[5.4.0]-undecene-7 or 1,5-diazabicyclo[4.3.0]-5-nonene, The acid (b2) is paratoluenesulfonic acid. Blocked isocyanate composition. R 1 N=CR 2 -NR 3 R 4 ・・・(1) (In the formula, R 2 is a hydrogen atom, a hydrocarbon group having 1 to 20 carbon atoms, or -NR 5 2 R is a group represented by the formula: 1 , R 3 , R 4 and R 5 are each independently a hydrogen atom or a hydrocarbon group having 1 to 20 carbon atoms, and two R 5 may be the same or different. 1 , R 2 , R 3 , R 4 , and two R 5 Any two or more of these may be bonded to form a cyclic structure.)
2. The stabilizer (B) is 100 to 1.00×10 relative to the blocked isocyanate compound (A). 5 The blocked isocyanate composition of claim 1 , wherein the blocked isocyanate composition is present in an amount of about 100 ppm by weight.
3. The blocked isocyanate composition according to claim 1 or 2, further comprising a polymer (F) obtained by polymerizing the blocked isocyanate compound (A).
4. A blocked isocyanate polymer obtained by polymerizing a polymerizable component contained in the blocked isocyanate composition according to any one of claims 1 to 3.
5. A cured film obtained by curing the blocked isocyanate composition according to any one of claims 1 to 3.
6. A method for producing a composition comprising an isocyanate compound or an isocyanato group-containing (co)polymer and a stabilizer (B), comprising: holding the blocked isocyanate composition according to any one of claims 1 to 3 at 25°C or higher for 10 days or more, and then holding it at 80°C or higher for 0.5 hours or more to eliminate the phenol compound (a2) from the blocked isocyanate compound (A) or polymer (F).
Citation Information
Patent Citations
Plastiol composition
JP1994025588A
Aromatic polyisocyanurate resin and its production
JP1995149859A
Catalyst for producing two component polyurethane sealant
JP2002187927A
Polyaniline composition and molded article comprising the same
JP2012158620A
Urethanization reaction catalyst and curable composition containing urethanization reaction catalyst