Resin particles, aqueous dispersion of resin particles, and method for preparing aqueous dispersion of resin particles

Resin particles with disulfide bonds and surfactants are produced via an emulsion process, enabling efficient light-induced softening for applications in photoresist agents and functional coatings.

JP7593044B2Active Publication Date: 2024-12-03RESONAC CORP
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
JP2020173285
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2020-10-14
Publication Date
2024-12-03
Estimated Expiration
2040-10-14

AI Technical Summary

Technical Problem

Existing photosoftening compositions do not effectively utilize resin particles with disulfide bonds to achieve efficient light-induced softening properties.

Method used

Resin particles containing a compound with disulfide bonds and a surfactant are produced through an emulsion process, where an organic solvent solution with the disulfide compound is added to an aqueous solution containing a surfactant, followed by solvent removal, forming an aqueous dispersion.

Benefits of technology

The resulting resin particles exhibit photosoftening properties, allowing them to soften upon light irradiation, facilitating applications in photoresist agents, softeners, tackifiers, and other functional coatings.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007593044000002
    Figure 0007593044000002
  • Figure 0007593044000001
    Figure 0007593044000001
Patent Text Reader

Abstract

To provide resin particles having light softening properties, a dispersion of resin particles, and a method for making a water dispersion of resin particles.SOLUTION: The present invention discloses resin particles containing a compound having a disulfide bond and a surfactant, a water dispersion of resin particles containing a compound having a disulfide bond and a surfactant, and a method for making a water dispersion of resin particles.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present disclosure relates to resin particles, an aqueous dispersion of resin particles, and a method for preparing an aqueous dispersion of resin particles. [Background technology]

[0002] Photosoftening compositions that are softened by irradiation with light are used in a variety of applications. For example, Patent Document 1 discloses an image forming apparatus equipped with a recording member having a photosoftening resin layer made of a photosoftening resin. [Prior art documents] [Patent documents]

[0003] [Patent Document 1] Japanese Patent Application Publication No. 11-190883 Summary of the Invention [Problem to be solved by the invention]

[0004] A primary object of the present disclosure is to provide photosoftenable resin particles, an aqueous dispersion of resin particles, and a method for preparing an aqueous dispersion of resin particles. [Means for solving the problem]

[0005] One aspect of the present disclosure relates to a resin particle comprising a compound having a disulfide bond and a surfactant.

[0006] Another aspect of the present disclosure relates to an aqueous dispersion of resin particles, comprising a compound having a disulfide bond and a surfactant.

[0007] Another aspect of the present disclosure relates to a method for preparing an aqueous dispersion of resin particles, the method including the steps of: adding an organic solvent solution containing a compound having a disulfide bond to an aqueous solution containing a surfactant to prepare an emulsion; and removing the organic solvent from the emulsion. Effect of the Invention

[0008] According to the present disclosure, there are provided photosoftenable resin particles, an aqueous dispersion of resin particles, and a method for producing an aqueous dispersion of resin particles. [Brief description of the drawings]

[0009] [Figure 1] FIG. 2 is an image diagram showing a cross section of a resin particle according to the present embodiment. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0010] Hereinafter, embodiments of the present disclosure will be described, however, the present disclosure is not limited to the following embodiments.

[0011] In this specification, "photosoftening" refers to a property that viscosity decreases, modulus decreases, loss tangent (tan δ) increases, hardness decreases, etc., due to light irradiation. In this specification, the term "process" includes not only an independent process, but also a process that cannot be clearly distinguished from other processes, as long as the intended effect of the process is achieved. In this specification, a numerical range indicated using "~" indicates a range including the numerical values ​​described before and after "~" as the minimum and maximum values, respectively. In the numerical ranges described in stages in this specification, the upper limit or lower limit of a numerical range of a certain stage may be replaced by the upper limit or lower limit of a numerical range of another stage. In the numerical ranges described in this specification, the upper limit or lower limit of the numerical range may be replaced by the value shown in the examples. In addition, the upper limit and lower limit values ​​described individually can be arbitrarily combined.

[0012] In this specification, the content of each component in the composition means the total amount of the multiple substances present in the composition when the composition contains multiple substances corresponding to each component, unless otherwise specified. In addition, the exemplified materials may be used alone or in combination of two or more types, unless otherwise specified. "A or B" may contain either A or B, or may contain both. In this specification, "(meth)acryloyl group" means an acryloyl group or a methacryloyl group, and other similar expressions are the same.

[0013] [Resin particles] The resin particles according to this embodiment contain a compound having a disulfide bond (hereinafter, sometimes referred to as "component (A)") and a surfactant (hereinafter, sometimes referred to as "component (B)").

[0014] The average particle size (D50) of the resin particles is preferably 50 to 1000 nm, more preferably 50 to 500 nm, further preferably 60 to 400 nm, and particularly preferably 65 to 300 nm. The average particle size can be calculated by measuring the particle size distribution of the resin particles by dynamic light scattering.

[0015] 1 is a conceptual diagram showing a cross section of a resin particle 10 according to this embodiment. The resin particle 10 is composed of a polymer particle 1 containing component (A) and a surfactant 2 present in the vicinity of the surface of the polymer particle 1.

[0016] Component (A): Compound having a disulfide bond The component (A) has a disulfide bond capable of generating a thiyl radical upon irradiation with light. The component (A) is not particularly limited as long as it is a compound having a disulfide bond (-SS-), but since the component (A) is reduced in molecular weight upon irradiation with light, it may be a high molecular weight component of a polymer or oligomer. The component (A) may be used alone or in combination of two or more types. It is preferable that the component (A) has multiple (two or more) disulfide bonds.

[0017] The component (A) may be, for example, a copolymer obtained by reacting a monomer having a disulfide bond and a functional group (hereinafter sometimes referred to as "component (A-1)") with a monomer having a substituent capable of reacting with the functional group (hereinafter sometimes referred to as "component (A-2)"), in other words, a reaction product of component (A-1) and component (A-2), i.e., a copolymer containing monomer units of component (A-1) and monomer units of component (A-2).

[0018] Examples of the functional group in the (A-1) component include a thiol group, a carboxy group, a hydroxyl group, an amino group, and an allyl group. The functional group in the (A-1) component may be, for example, at least one selected from the group consisting of a thiol group, a carboxy group, a hydroxyl group, an amino group, and an allyl group. The number of functional groups in the (A-1) component may be 2 or more from the viewpoint of increasing the molecular weight. On the other hand, the lower the degree of crosslinking of the (A) component, the easier it tends to be to soften the photosoftenable resin composition to a liquid state (liquid) when irradiated with light. Therefore, it is preferable to use a monomer having two functional groups as the (A-1) component, and when multiple monomers having different functional groups are used, it is preferable to increase the proportion of the monomer having two functional groups. The proportion of the monomer having two functional groups may be 75 to 100 mass%, 85 to 100 mass%, or 90 to 100 mass% based on the total amount of the (A-1) component. The proportion of monomers having three or more functional groups may be 0 to 10 mass %, 0 to 15 mass %, or 0 to 25 mass % based on the total amount of the component (A-1).

[0019] Examples of commercially available products of the component (A-1) include the Thiokol LP series (polysulfide polymer, manufactured by Toray Fine Chemicals Co., Ltd.), 3,3'-dithiodipropionic acid (manufactured by Tokyo Chemical Industry Co., Ltd.), dithiodiethanol (manufactured by Tokyo Chemical Industry Co., Ltd.), cystamine hydrochloride (manufactured by Tokyo Chemical Industry Co., Ltd.), and diallyl disulfide (manufactured by Tokyo Chemical Industry Co., Ltd.). These components (A-1) may be used alone or in combination of two or more.

[0020] The (A-2) component is a monomer having a substituent capable of reacting with a functional group, and can be used without any particular limitation as long as it has a substituent capable of reacting with a functional group. Examples of the substituent include a group containing a cyclic ether (e.g., a glycidyl group, etc.), an isocyanate group, a (meth)acryloyl group, an aldehyde group, an amino group, a hydroxyl group, a carboxyl group, and an alkoxysilyl group. The substituent in the (A-2) component may be, for example, at least one selected from the group consisting of a group containing a cyclic ether, an isocyanate group, and a (meth)acryloyl group. The number of substituents in the (A-2) component may be two or more from the viewpoint of increasing the molecular weight. On the other hand, the lower the degree of crosslinking of the (A) component, the easier it tends to be to soften the photosoftenable resin composition to a liquid state (liquid) when irradiated with light, so it is preferable to use a monomer having two substituents as the (A-2) component, and when multiple monomers having different numbers of substituents are used, it is preferable to increase the proportion of the monomer having two substituents.

[0021] In one embodiment of the (A-2) component, the proportion of monomers having three or more substituents may be 20% by mass or more, 30% by mass or more, 40% by mass or more, or 50% by mass or more, and 90% by mass or less or 75% by mass or less, based on the total amount of the (A-2) component. The proportion of monomers having two substituents may be 10% by mass or more or 25% by mass or more, and 80% by mass or less, 70% by mass or less, 60% by mass or less, or 50% by mass or less, based on the total amount of the (A-2) component.

[0022] In another embodiment of the component (A-2), the proportion of monomers having two substituents may be 75 to 100 mass%, 85 to 100 mass%, or 90 to 100 mass%, based on the total amount of the component (A-2). The proportion of monomers having three or more substituents may be 0 to 10 mass%, 0 to 15 mass%, or 0 to 25 mass%, based on the total amount of the component (A-2).

[0023] Examples of the component (A-2) include a monomer having two or more cyclic ether-containing groups in one molecule; a monomer having two or more isocyanate groups in one molecule; a monomer having two or more (meth)acryloyl groups in one molecule; a monomer having two or more amino groups in one molecule, a monomer having two or more isocyanate groups and (meth)acryloyl groups in one molecule; a monomer having a cyclic ether-containing group and two or more alkoxysilyl groups in one molecule; a compound having two or more isocyanate groups in one molecule, or a monomer having two or more cyclic ether-containing groups in one molecule. Examples of the monomer include a combination of a compound having a group containing one or more cyclic ethers and a compound having an amino group, an acid anhydride skeleton, or a thiol group, and an alkoxyl group in one molecule; a monomer that is a combination of a compound having two or more isocyanate groups in one molecule and a compound having a hydroxyl group and a (meth)acryloyl group in one molecule; a monomer that is a combination of a compound having a group containing two or more cyclic ethers in one molecule and a compound having a carboxyl group and a (meth)acryloyl group in one molecule. These (A-2) components may be used alone or in combination of two or more.

[0024] Suitable combinations of the (A-1) component and the (A-2) component include, for example, a combination of a monomer having a disulfide bond and a thiol group or a hydroxyl group, and at least one selected from the group consisting of a monomer having two or more cyclic ether-containing groups in one molecule, a monomer having two or more (meth)acryloyl groups in one molecule, and a monomer having two or more isocyanate groups in one molecule; and a combination of a monomer having a disulfide bond and a carboxy group, and at least one selected from the group consisting of a monomer having two or more cyclic ether-containing groups in one molecule, a monomer having two or more amino groups in one molecule, and a monomer having two or more isocyanate groups in one molecule.

[0025] When the copolymer (A) is obtained by reacting the (A-1) component with the (A-2) component, the reaction ratio of these components can be appropriately adjusted based on the functional group equivalent of the (A-1) component and the substituent equivalent of the (A-2) component. The reaction between the (A-1) component and the (A-2) component may be carried out while heating. The reaction temperature may be, for example, 0 to 200°C, and the reaction time may be, for example, 0.1 to 240 hours.

[0026] When reacting the (A-1) component with the (A-2) component, a curing catalyst may be used as necessary. The curing catalyst can be selected arbitrarily according to the type of functional group of the (A-1) component and the type of substituent of the (A-2) component. When reacting a monomer having a thiol group or a hydroxyl group as a functional group as the (A-1) component with a monomer having an isocyanate group as a substituent as the (A-2) component, the curing catalyst may be, for example, a tin-based catalyst or an amine-based catalyst. When reacting a monomer having a carboxyl group as a functional group as the (A-1) component with a monomer having a group containing a cyclic ether as a substituent as the (A-2) component, the curing catalyst component may be, for example, an amine-based catalyst or a phosphorus-based catalyst. When a monomer having a thiol group or a hydroxyl group as a functional group as the component (A-1) is reacted with a monomer having a (meth)acryloyl group as a substituent as the component (A-2), an amine catalyst that promotes the Michael addition reaction between the thiol group or the hydroxyl group and the (meth)acryloyl group may be used.

[0027] Examples of tin-based catalysts include dibutyltin dilaurate, dibutyltin dichloride, dibutyltin oxide, dibutyltin dibromide, dibutyltin dimaleate, dioctyltin dilaurate, dibutyltin diacetate, dibutyltin sulfide, tributyltin sulfide, tributyltin oxide, tributyltin acetate, triethyltin ethoxide, tributyltin ethoxide, dioctyltin oxide, tributyltin chloride, tributyltin trichloroacetate, and tin 2-ethylhexanoate.

[0028] Examples of the amine catalyst include triethylamine, triethylenediamine, 1,8-diazabicyclo[5.4.0]undecene-7 (DBU), and 1,5-diazabicyclo[4.3.0]nonene-5 (DBN).

[0029] Examples of phosphorus-based catalysts include triphenylphosphine and its addition reaction products, (4-hydroxyphenyl)diphenylphosphine, bis(4-hydroxyphenyl)phenylphosphine, and tris(4-hydroxyphenyl)phosphine.

[0030] The content of the curing catalyst may be 0.005 to 10 mass %, 0.01 to 5 mass %, or 0.02 to 3 mass % based on the total of the components (A-1) and (A-2).

[0031] The molecular weight or weight average molecular weight (Mw) of the component (A) may be 200 to 10,000,000, 1,000 to 2,000,000, or 2,500 to 1,000,000. Mw is a polystyrene-equivalent value obtained by gel permeation chromatography (GPC) using a calibration curve with standard polystyrene.

[0032] (B) Component: Surfactant The surfactant may be an anionic surfactant, a cationic surfactant, a nonionic surfactant, or an amphoteric surfactant.

[0033] Examples of anionic surfactants include fatty acid oils such as sodium oleate and castor oil potassium, alkyl sulfate ester salts such as sodium lauryl sulfate and ammonium lauryl sulfate, alkyl benzene sulfonates such as sodium dodecylbenzene sulfonate, alkyl naphthalene sulfonates, alkanesulfonates, dialkyl sulfosuccinates such as sodium dioctyl sulfosuccinate, alkenyl succinates (dipotassium salts), alkyl phosphate ester salts, naphthalene sulfonate-formaldehyde condensates, polyoxyethylene alkyl ether sulfates such as polyoxyethylene alkyl phenyl ether sulfate ester salts and sodium polyoxyethylene lauryl ether sulfate, polyoxyethylene alkyl sulfate ester salts, polyoxyethylene lauryl ether acetates such as sodium polyoxyethylene lauryl ether acetate, alkyl benzene sulfonic acids such as dodecylbenzene sulfonic acid, alpha olefin sulfonates such as sodium tetradecene sulfonate, alkyl sulfate ester salts, alkyl ether sulfate ester salts, alaninates such as N-lauroyl-N-methyl-β-alanine sodium salt and their salts, and fatty acid soaps.

[0034] Examples of cationic surfactants include alkylamine salts such as laurylamine acetate and stearylamine acetate; and quaternary ammonium salts such as cetyltrimethylammonium bromide, cetyltrimethylammonium chloride, lauryltrimethylammonium bromide and lauryltrimethylammonium chloride.

[0035] Examples of nonionic surfactants include polyvinyl alcohol, polyethylene glycol alkyl ethers, polyethylene glycol alkylaryl ethers, polyethylene glycol esters, polyethylene glycol sorbitan esters, perfluoroalkyl glycols, polyoxyethylene lauryl ethers, polyethylene-polyoxypropylene decyl ethers, and polyoxyethylene isoalcohol ethers.

[0036] Examples of amphoteric surfactants include hydrocarbon surfactants such as lauryl dimethylamine oxide, phosphate surfactants, phosphite surfactants, and betaines such as lauric acid amidopropyl dimethylaminoacetic acid betaine.

[0037] As component (B), from the viewpoint of dispersion stability of the resin particles in water, it is preferable to use a surfactant having an ionic group, it is more preferable to use an anionic surfactant, and it is even more preferable to use a combination of an anionic surfactant and a nonionic surfactant.

[0038] The amount of the component (B) added may be 0.01 to 50 parts by mass, 0.05 to 40 parts by mass, or 0.1 to 30 parts by mass per 100 parts by mass of the component (A), from the viewpoint of further enhancing the water dispersibility of the resin particles.

[0039] Component (C): Photoradical generator The resin particles according to this embodiment may contain a photoradical generator as component (C). In this case, component (C) is contained in polymer particle 1 together with component (A). The photoradical generator may be a component that reacts with a thiyl radical generated when the resin composition is irradiated with light, or a component that generates a photoinduced radical. As the photoradical generator, a photoradical polymerization initiator or the like can be used.

[0040] Examples of the photoradical generator include an intramolecular cleavage type photoradical polymerization initiator and a hydrogen abstraction type photoradical polymerization initiator. Examples of the intramolecular cleavage type photoradical polymerization initiator include a benzyl ketal type photoradical polymerization initiator; an α-hydroxyacetophenone type photoradical polymerization initiator; a benzoin type photoradical polymerization initiator; an aminoacetophenone type photoradical polymerization initiator; an oxime ketone type photoradical polymerization initiator; an acylphosphine oxide type photoradical polymerization initiator; a titanocene type photoradical polymerization initiator; a thiobenzoic acid S-phenyl polymerization initiator; and high molecular weight derivatives thereof. Examples of the hydrogen abstraction type photoradical polymerization initiator include a benzophenone type photoradical polymerization initiator, a thioxanthone type photoradical polymerization initiator, and an anthraquinone type photoradical polymerization initiator.

[0041] The content of the (C) component may be 1 part by mass or more, 5 parts by mass or more, or 10 parts by mass or more, and may be 40 parts by mass or less, 30 parts by mass or less, or 25 parts by mass or less, per 100 parts by mass of the (A) component.

[0042] [Aqueous dispersion of resin particles] The resin particles according to this embodiment can be used as an aqueous dispersion in which resin particles containing a compound having a disulfide bond and a surfactant are dispersed in water.

[0043] The aqueous dispersion of resin particles according to this embodiment can be prepared by a method including the steps of: adding an organic solvent solution containing a compound having a disulfide bond, component (A), to an aqueous solution containing a surfactant, component (B), to prepare an emulsion; and removing the organic solvent from the emulsion.

[0044] Examples of the organic solvent include aromatic hydrocarbons such as benzene, xylene, and toluene; ketones such as cyclohexanone and methyl ethyl ketone; cyclic ethers such as dioxane and tetrahydrofuran; and esters such as ethyl acetate, butyl acetate, and propyl acetate.

[0045] After adding an organic solvent solution containing component (A) to an aqueous solution containing component (B), the solution is dispersed in water using a dispersing device such as a homogenizer to form polymer particles, and an emulsion of resin particles having a surfactant attached to the surface of the polymer particles can be obtained. The temperature at which the emulsion is prepared may be 0 to 80°C, and from the viewpoint of preventing particle aggregation, 40°C or less is more preferable.

[0046] The organic solvent solution may contain a photoradical generator (C) as component (A) together with component (A). When component (C) is added to prepare resin particles, it is preferable to handle component (C) under light-shielded conditions in order to prevent decomposition of component (C) due to light.

[0047] Since the polymer particles in the emulsion contain an organic solvent, an aqueous dispersion of the resin particles can be obtained by removing the organic solvent from the emulsion. The temperature at which the organic solvent is removed may be appropriately set depending on the boiling point of the organic solvent.

[0048] The resin particles according to the present embodiment can be formed into a film shape and used as a photosoftening resin film. In addition, the resin particles can be formed into a block shape and used as a photosoftening resin block. The method for forming the resin particles into a film shape or a block shape is not particularly limited, and a known method can be applied.

[0049] The resin particles according to the embodiment may be mixed with other components to prepare a resin composition. Examples of the other components include thermosetting resins such as epoxy resins, thermoplastic resins, adhesion improvers such as coupling agents, polymerization inhibitors, light stabilizers, antifoaming agents, fillers, chain transfer agents, thixotropy-imparting agents, flame retardants, release agents, surfactants, lubricants, antistatic agents, and other additives.

[0050] The resin particles according to the present embodiment have a property that, by irradiation with light, the disulfide bond (-SS-) in the compound is broken, and the compound having the disulfide bond is reduced in molecular weight and softened. The resin particles can also be softened to a liquid (liquid state). In addition, the resin particles have a property of being easily molded into a film or block shape. By utilizing such a property, the resin particles according to the present embodiment can be applied to, for example, photoresist agents for photolithography, and can be used as a photosensitive resin composition or a photosensitive resin film. The photosensitive resin composition or the photosensitive resin film can be patterned by irradiation with light (exposure), and further can be developed by washing with water after irradiation with light (exposure). The resin particles according to the present embodiment can be suitably used for forming a pattern film.

[0051] The resin particles according to this embodiment can also be used in a variety of applications, such as a softener or easy-removal agent for strong adhesive tapes; an adhesive for weakly adhesive or non-adhesive films; a partial softener for coating materials, adhesives, or adhesives; a partial softener for molding materials; an ultra-low elasticity film that can be punched and obtained by irradiating light after punching; a moisture-proofing agent; a capsule coating that softens and dissolves when irradiated with light; and a thickener that reduces viscosity when irradiated with light.

[0052] By irradiating the resin particles according to the embodiment with light, a softened resin particle can be obtained. The light for light irradiation is not particularly limited, and may be, for example, ultraviolet light or visible light. The wavelength of the light for light irradiation may be 150 to 830 nm. The light irradiation is performed, for example, using a light irradiation device with an irradiation dose of 100 mJ / cm. 2 The irradiation can be performed under the above conditions. The amount of irradiation means the product of illuminance and irradiation time (seconds). Examples of light sources for irradiating ultraviolet light or visible light include low pressure mercury lamps, medium pressure mercury lamps, high pressure mercury lamps, metal halide lamps, LED lamps, etc. The light irradiation may be performed directly on the resin particles or through glass or the like. EXAMPLES

[0053] The present disclosure will be described in more detail below with reference to examples, although the present disclosure is not limited to these examples.

[0054] (Production Example 1) In a sample tube, 0.61 g of Miramer M240 (EO-modified diacrylate of bisphenol A, manufactured by Bigen Specialty Chemical Co., Ltd.), 4.39 g of Thiokol LP-55 (dithiol having a disulfide bond, average molecular weight: 4000, manufactured by Toray Fine Chemical Co., Ltd.), and 7.5 g of toluene were added, and a mixture was obtained by stirring at 80 rpm using a mix rotor. Next, 0.02 g of DBU (1,8-diazabicyclo[5.4.0]undecene-7, manufactured by San-Apro Co., Ltd.) was added to the mixture and mixed, after which the inside of the sample tube was replaced with nitrogen and the reaction was carried out while stirring at 80 rpm using a mix rotor for 30 minutes. Then, 7.5 g of toluene was added to the reactant and stirred at 80 rpm using a mix rotor. As a result, a polymer solution a (polymer concentration: 25% by mass) containing component (A) was obtained.

[0055] (Production Example 2) To 9 g of polymer solution a, 1 g of a toluene solution containing 0.5 g of Omnirad 651 (2,2'-dimethoxy-2-phenylacetophenone, manufactured by IGM Resins BV) was added to obtain a polymer solution b containing components (A) and (C).

[0056] [Preparation of resin particles] In order to prepare the resin particles, the following materials were prepared. Anionic surfactant: Neopelex G-15 (sodium dodecylbenzenesulfonate (soft type): 16% by mass, water: 84% by mass, manufactured by Kao Corporation) Nonionic surfactant: Gohsenol GH-23 (polyvinyl alcohol: 93.5% by mass or more, methanol: less than 3% by mass, methyl acetate: less than 1% by mass, manufactured by Mitsubishi Chemical Corporation)

[0057] Example 1 82.8g of pure water, 4.5g of 2% GH-23-containing aqueous solution, and 2.7g of G-15 were mixed to prepare 90g of an aqueous solution of surfactant. 10g of polymer solution a was slowly dropped into the aqueous solution of surfactant at room temperature, and while cooling the solution in an ice bath, ultrasonically dispersed for 5 minutes using a homogenizer to obtain 100g of emulsion. Then, toluene was removed while heating the emulsion at an internal temperature of 85°C, and an aqueous dispersion of resin particles was obtained.

[0058] Example 2 An emulsion and an aqueous dispersion of resin particles were obtained in the same manner as in Example 1, except that the polymer solution a was changed to the polymer solution b.

[0059] (particle size distribution) The particle size distribution of the resin particles contained in the emulsion and the aqueous dispersion was measured by dynamic light scattering using an ELSZ-2000S manufactured by Otsuka Electronics Co., Ltd. The measurement was carried out at 25°C using pure water as the solvent. The results are shown in Table 1.

[0060] [Table 1]

[0061] (Photosoftening) The aqueous dispersion of the resin particles of Example 2 was dropped onto the release-treated surface of a polyethylene terephthalate film (PET) as a support film, and dried at room temperature for 1.5 hours to obtain a resin film. The resin film was then exposed to UV light using a UV conveyor-type exposure machine (EYEGRANDAGE, manufactured by EYE GRAPHICS Co., Ltd.) at an output of 1.5 kW, a speed of 1.5 m / min, and a peak intensity of 96 mW / cm. 2 , cumulative light intensity 3880mJ / cm 2 After exposure, the resin film had a reduced viscosity and gave off an odor due to the cleavage of the photoradical generator. [Explanation of symbols]

[0062] 1...polymer particle, 2...surfactant, 10...resin particle.

Claims

1. The present invention relates to a surfactant comprising a compound having a disulfide bond and a surfactant containing an anionic surfactant and a nonionic surfactant, The resin particles, wherein the compound having a disulfide bond is a high molecular weight component of a polymer or oligomer having a disulfide bond.

2. The resin particles according to claim 1 , further comprising a photoradical generator.

3. The present invention relates to a surfactant comprising a compound having a disulfide bond and a surfactant containing an anionic surfactant and a nonionic surfactant, The aqueous dispersion of resin particles, wherein the compound having a disulfide bond is a high molecular weight component of a polymer or oligomer having a disulfide bond.

4. The aqueous dispersion according to claim 3 , wherein the resin particles further contain a photoradical generator.

5. A step of preparing an emulsion by adding an organic solvent solution containing a compound having a disulfide bond to an aqueous solution containing a surfactant including an anionic surfactant and a nonionic surfactant; and removing the organic solvent from the emulsion. The method for preparing an aqueous dispersion of resin particles, wherein the compound having a disulfide bond is a high molecular weight component of a polymer or oligomer having a disulfide bond.

6. The method of claim 5 , wherein the organic solvent solution further comprises a photoradical generator.

Citation Information

Patent Citations

  • Modified epoxy resin emulsion and fiber bundling agent using the same

    JP1993039407A

  • Image forming device and recording material

    JP1999190883A

  • Primer composition

    JP1999193355A

  • Particle and contrast agent for optical imaging having the particle

    JP2012224610A

  • Aggregate of resin particles, organic solvent dispersion of resin particles, and method for making aggregate of resin particles

    JP2022064577A