Polymer composition and cured product thereof

A polymer composition with carbon nanotubes of varying diameters addresses the challenge of high viscosity in existing compositions by maintaining antistatic performance and moldability, using a reduced amount of carbon nanotubes to achieve suitable surface resistance for electronic components.

JP7593063B2Active Publication Date: 2024-12-03OSAKA SODA CO LTD
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
JP2020188214
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2020-11-11
Publication Date
2024-12-03
Estimated Expiration
2040-11-11

AI Technical Summary

Technical Problem

Existing polymer compositions used for electrical and electronic components to prevent static electricity damage require high amounts of carbon nanotubes, which compromise moldability due to increased viscosity.

Method used

A polymer composition comprising carbon nanotubes with different outer diameters in a specific ratio, where one type has an outer diameter less than 3.0 nm and the other 3.0 nm or more, maintaining excellent antistatic performance while reducing the overall amount of carbon nanotubes, thereby improving moldability.

Benefits of technology

The composition achieves excellent antistatic performance with reduced carbon nanotube content, maintaining low viscosity and high moldability, resulting in a cured product with a surface resistance suitable for electronic components.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007593063000002
    Figure 0007593063000002
  • Figure 0007593063000001
    Figure 0007593063000001
Patent Text Reader

Abstract

To provide a polymer composition which, even though an added amount of carbon nanotubes is reduced, can exhibit excellent anti-static performance after curing and, further, has excellent moldability.SOLUTION: A polymer composition comprises carbon nanotubes (A), carbon nanotubes (B), and a polymer. where an outer diameter of the carbon nanotubes (A) is less than 3.0 nm, an outer diameter of the carbon nanotubes (B) is 3.0 nm or more, and a content ratio (mass ratio) of the carbon nanotubes (A) and the carbon nanotubes (B), A:B, is 1:400 to 1:0.25.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a polymer composition and a cured product thereof. [Background technology]

[0002] Conventionally, electrical and electronic components, such as semiconductor components such as IC chips, hard disks, and silicon wafers, as well as the materials used to handle these components (e.g., carrier trays, IC sockets, connectors, and wafer tweezers), have the problem of being electrically destroyed when charged with static electricity.

[0003] As members that suppress electrical breakdown due to static electricity, antistatic molded articles made by adding conductive materials such as carbon black, ketjen black, and acetylene black to a resin composition are known. [Prior art documents] [Patent documents]

[0004] [Patent Document 1] JP 2007-296725 A Summary of the Invention [Problem to be solved by the invention]

[0005] The main object of the present invention is to provide a polymer composition that exhibits excellent antistatic performance after curing and has excellent moldability, even though the amount of carbon nanotubes is reduced. Another object of the present invention is to provide a cured product of the polymer composition. [Means for solving the problem]

[0006] The present inventors have conducted extensive research to solve the above problems, and have found that by using carbon nanotubes having a relatively small outer diameter and carbon nanotubes having a large outer diameter in a specific ratio, a polymer composition can be obtained that exhibits excellent antistatic properties after curing, even though the amount of carbon nanotubes is reduced, and that has excellent moldability without becoming too viscous.

[0007] The present disclosure has been completed through further investigation based on the above findings.

[0008] That is, the present invention can be described as follows.

[0009] Item 1. A polymer composition comprising carbon nanotubes (A), carbon nanotubes (B), and a polymer, The outer diameter of the carbon nanotube (A) is less than 3.0 nm, The outer diameter of the carbon nanotube (B) is 3.0 nm or more, A polymer composition, wherein the content ratio (mass ratio) of the carbon nanotubes (A) to the carbon nanotubes (B) is (A):(B)=1:400 to 1:0.25. Item 2. The content of the carbon nanotubes (A) is 0.0005% by mass or more and less than 0.005% by mass; Item 2. The polymer composition according to item 1, wherein the content of the carbon nanotubes (B) is 0.0005% by mass or more and less than 0.2% by mass. Item 3. The polymer composition according to item 1 or 2, wherein the polymer is a curable resin. Item 4. The polymer composition according to any one of Items 1 to 3, further comprising a curing agent. Item 5. A cured product of the polymer composition according to any one of items 1 to 4. Item 6. Surface resistance is 10 6 Ω / sq. or more 10 11 Item 6. The cured product according to item 5, having a hardness of less than Ω / sq. Item 7. The cured product according to item 5 or 6, which is an electric or electronic part. Effect of the Invention

[0010] According to the present invention, it is possible to provide a polymer composition which exhibits excellent antistatic properties after curing and has excellent moldability, even though the blending amount of carbon nanotubes is reduced. Furthermore, according to the present invention, it is also possible to provide a cured product of the polymer composition. [Brief description of the drawings]

[0011] [Figure 1] 1 is an optical microscope photograph of the cured product of the polymer composition obtained in Example 1. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0012] The polymer composition of the present invention comprises carbon nanotubes (A), carbon nanotubes (B), and a polymer, the carbon nanotubes (A) having an outer diameter of less than 3.0 nm, the carbon nanotubes (B) having an outer diameter of 3.0 nm or more, and the content ratio (mass ratio) of the carbon nanotubes (A) to the carbon nanotubes (B) being (A):(B)=1:400 to 1:0.25. The polymer composition of the present invention has this constitution, and therefore, even though the amount of carbon nanotubes is reduced, it can exhibit excellent antistatic performance after curing, and further, a polymer composition having excellent moldability without excessively increasing viscosity can be obtained. The polymer composition of the present invention and its cured product will be described in detail below.

[0013] In this specification, a numerical value connected with "~" means a numerical range including the numerical values ​​before and after "~" as the lower and upper limits. When multiple lower limits and multiple upper limits are listed separately, any lower limit and upper limit may be selected and connected with "~" (however, when an upper limit value written as "less than" is connected with "~", the numerical value after "~" (i.e., the upper limit value) is not included in the numerical range).

[0014] 1. Polymer composition The polymer composition of the present invention is a polymer composition containing carbon nanotubes (A), carbon nanotubes (B), and a polymer. The outer diameter of the carbon nanotubes (A) is less than 3.0 nm. On the other hand, the outer diameter of the carbon nanotubes (B) is 3.0 nm or more. That is, the polymer composition of the present invention contains two or more types of carbon nanotubes with different outer diameters (thicknesses).

[0015] From the viewpoint of more suitably exerting the effects of the present invention, it is preferable that the difference in the outer diameter between the carbon nanotube (A) and the carbon nanotube (B) is large. Specifically, the outer diameter of the carbon nanotube (A) is preferably 2.7 nm or less, more preferably 2.5 nm or less, and even more preferably 2.0 nm or less. The lower limit of the outer diameter of the carbon nanotube (A) is preferably 1.0 nm. On the other hand, the outer diameter of the carbon nanotube (B) is preferably 4.0 nm or more, more preferably 5.0 nm or more, even more preferably 6.0 nm or more, even more preferably 8.0 nm or more, and even more preferably 9.0 nm or more. The upper limit of the outer diameter of the carbon nanotube (B) is preferably 150 nm or less, more preferably 120 nm or less, and even more preferably 100 nm or less. The outer diameter (average value) of the carbon nanotube can be measured as an average value by using a Raman spectrometer and a transmission electron microscope depending on the diameter. Specific measurement methods are as described in the examples.

[0016] In the polymer composition of the present invention, two or more kinds of carbon nanotubes (A) and (B) having different outer diameters (thickness) are contained in a predetermined ratio. That is, the outer diameter of the carbon nanotube (A) is less than 3.0 nm, the outer diameter of the carbon nanotube (B) is 3.0 nm or more, and the content ratio (mass ratio) of the carbon nanotubes (A) and the carbon nanotubes (B) is (A):(B)=1:400 to 1:0.25. In the polymer composition of the present invention, in addition to the carbon nanotubes (B) having a large outer diameter, the carbon nanotubes (A) having a small outer diameter are contained in a predetermined ratio and content, respectively, so that the polymer composition can exhibit excellent antistatic performance after curing, even though the blending amount of the carbon nanotubes is reduced, and furthermore, a polymer composition having excellent moldability without excessively high viscosity can be obtained. The mechanism of this can be considered as follows. That is, a structure is formed in which the carbon nanotubes (A) with a small outer diameter bridge between the carbon nanotubes (B) with a large outer diameter dispersed in the polymer composition of the present invention, and when this polymer composition is cured, the electrical conductivity of the cured product is increased, resulting in a small surface resistance value of the cured product and excellent antistatic properties. In particular, since the carbon nanotubes (A) are very thin with an outer diameter of less than 3.0 nm, they tend to form curled (curved) shapes, and it can be said that the curled carbon nanotubes (A) are easily entangled between the carbon nanotubes (B) with a large outer diameter to form a conductive path. Furthermore, when a large amount of carbon nanotubes (B) having a large outer diameter are blended, the electrical conductivity of the cured product of the polymer composition can be increased, but the viscosity of the polymer composition becomes very high, which causes the problem of reduced moldability. However, in the polymer composition of the present invention, by using carbon nanotubes (A) having a small outer diameter in combination with carbon nanotubes (B) having a large outer diameter, the amount of carbon nanotubes (B) having a large outer diameter used (and even the total amount of carbon nanotubes used in the polymer composition) can be reduced, while the electrical conductivity of the cured product of the polymer composition can be increased, and the viscosity of the polymer composition does not become too high, thereby exhibiting excellent moldability.

[0017] From the viewpoint of more suitably exerting the effects of the present invention, in the polymer composition of the present invention, the lower limit of the content of the carbon nanotubes (A) is, for example, 0.0005 mass% or more, preferably 0.00075 mass% or more, more preferably 0.001 mass% or more, and the upper limit is, for example, less than 0.005 mass%, preferably 0.004 mass% or less, more preferably 0.003 mass% or less. From the same viewpoint, the lower limit of the content of the carbon nanotubes (B) is, for example, 0.0005 mass% or more, preferably 0.00075 mass% or more, more preferably 0.001 mass% or more, and the upper limit is, for example, less than 0.2 mass%, preferably 0.15 mass% or less, more preferably 0.1 mass% or less. Furthermore, the lower limit of the total content of all carbon nanotubes contained in the polymer composition of the present invention is, for example, 0.001 mass% or more, preferably 0.0015 mass% or more, more preferably 0.002 mass% or more, and the upper limit is, for example, less than 0.205 mass%, preferably 0.155 mass% or less, more preferably 0.105 mass% or less. From the viewpoint of more suitably exerting the effects of the present invention, in the content ratio (mass ratio) of carbon nanotubes (A) to carbon nanotubes (B), the upper limit of the ratio of carbon nanotubes (B) is 1:400 (carbon nanotubes (A):carbon nanotubes (B)), preferably 1:300, more preferably 1:250, even more preferably 1:200, and even more preferably 1:150. In addition, the lower limit of the ratio of carbon nanotubes (B) is 1:0.25 (carbon nanotubes (A):carbon nanotubes (B)), preferably 1:0.3, more preferably 1:0.5, and even more preferably 1:0.75.

[0018] The origin of the carbon nanotubes (A) and (B) is not particularly limited, and they may be formed by any manufacturing method, but examples of the method include arc discharge, laser evaporation, and chemical vapor deposition (CVD), and the chemical vapor deposition (CVD) method is preferable. The type of the carbon nanotubes (A) and (B) is not particularly limited, and they may be single-walled carbon nanotubes, double-walled carbon nanotubes, or multi-walled carbon nanotubes.

[0019] The intensity ratio G / D of the G band to the D band of the carbon nanotubes (A) and (B) is not particularly limited, but in the carbon nanotube (A), the lower limit is, for example, 10 or more, preferably 20 or more, and more preferably 30 or more, and the upper limit is, for example, 200 or less, preferably 190 or less, and more preferably 180 or less. In the carbon nanotube (B), the lower limit is, for example, 0.001 or more, preferably 0.01 or more, and more preferably 0.1 or more, and the upper limit is, for example, 10 or less, preferably 9 or less, and more preferably 8 or less. G / D is measured by a Raman spectrometer, and in a Raman spectrum measured by a resonance Raman scattering method (excitation wavelength 532 nm), the G band (1590 cm -1 around 1300 cm -1 The higher the G / D ratio, the fewer the defects in the carbon nanotube structure.

[0020] The length of each of the carbon nanotubes (A) and (B) is not particularly limited, but from the viewpoint of more suitably exerting the effects of the present invention, it may be 10 nm or more, 10 μm or more, 1 mm or more, or 10 mm or more, and although there is no particular upper limit, it is 100 mm or less. The measurement method is also not particularly limited, and it may be the length of a single carbon nanotube, or the state in which the carbon nanotubes are aggregated together and formed into a bundle (bundle state).

[0021] The carbon purity of the carbon nanotubes (A) is not particularly specified, but is, for example, 95% or more, preferably 98% or more, and more preferably 99% or more. By removing impurities such as metals as much as possible, the dispersibility of the carbon nanotubes (A) can be improved. By improving the dispersibility, a structure in which the carbon nanotubes (A) bridge between the carbon nanotubes (B) can be more efficiently formed, and the effect of the present invention can be enhanced. In addition, the carbon purity of the carbon nanotubes (B) is not particularly specified, but is, for example, 80% or more, preferably 85% or more, and more preferably 90% or more.

[0022] The polymer contained in the polymer composition of the present invention is not particularly limited as long as the effects of the present invention are achieved, and examples thereof include resins, rubbers, etc. Examples of the resins include curable resins such as thermosetting resins and ionizing radiation curable resins, and thermoplastic resins.

[0023] Specific examples of thermosetting resins include epoxy resins, polyurethane resins (including two-component curing polyurethanes), unsaturated polyester resins, aminoalkyd resins, phenolic resins, urea resins, diallyl phthalate resins, melamine resins, guanamine resins, melamine-urea co-condensation resins, silicon resins, polysiloxane resins, etc. These thermosetting resins can be used alone or in combination of two or more.

[0024] The ionizing radiation curable resin is a resin that is crosslinked and cured by irradiation with ionizing radiation. Specifically, it is a mixture of at least one of prepolymers, oligomers, and monomers having polymerizable unsaturated bonds or epoxy groups in the molecule. Here, the ionizing radiation means electromagnetic waves or charged particle beams that have an energy quantum capable of polymerizing or crosslinking molecules, and usually ultraviolet rays (UV) or electron beams (EB) are used, but it also includes electromagnetic waves such as X-rays and γ-rays, charged particle beams such as α-rays and ion beams. Specific examples of the ionizing radiation curable resin include acrylic resins. These ionizing radiation curable resins can be used alone or in combination of two or more.

[0025] A curing agent such as a crosslinking agent or a polymerization initiator, and a polymerization accelerator can be added to the curable resin. For example, as a curing agent, an organic amine can be added to an epoxy resin, and an isocyanate, an organic sulfonate, etc. can be added to an unsaturated polyester resin, a polyurethane resin, etc. Peroxides such as methyl ethyl ketone peroxide and radical initiators such as azoisobutylnitrile can be added to an unsaturated polyester resin.

[0026] Specific examples of thermoplastic resins include polyethylene resins, polypropylene resins, polystyrene resins, rubber-modified polystyrene resins, acrylonitrile-butadiene-styrene (ABS) resins, acrylonitrile-styrene (AS) resins, polymethyl methacrylate resins, acrylic resins, polyvinyl chloride resins, polyvinylidene chloride resins, polyethylene terephthalate resins, ethylene vinyl alcohol resins, cellulose acetate resins, ionomer resins, polyacrylonitrile resins, polyamide resins, polyacetal resins, polybutylene terephthalate resins, polylactic acid resins, polyphenylene ether resins, modified polyphenylene ether resins, polycarbonate resins, polysulfone resins, polyphenylene sulfide resins, polyetherimide resins, polyethersulfone resins, polyarylate resins, thermoplastic polyimide resins, polyamideimide resins, polyetheretherketone resins, polyketone resins, liquid crystal polyester resins, fluororesins, syndiotactic polystyrene resins, and cyclic polyolefin resins. These thermoplastic resins can be used alone or in combination of two or more.

[0027] Specific examples of rubber include synthetic rubbers such as isoprene rubber, butadiene rubber, styrene-butadiene rubber, chloroprene rubber, nitrile rubber, polyisobutylene rubber, ethylene propylene rubber, chlorosulfonated polyethylene, acrylic rubber, fluororubber, epichlorohydrin rubber, urethane rubber, and silicone rubber.

[0028] In the polymer composition of the present invention, the content of the polymer is preferably 90.0 mass% or more, more preferably 95 mass% or more, and further preferably 97 mass% or more. The polymer composition of the present invention may be a polymer composition substantially containing only carbon nanotubes (A), carbon nanotubes (B), and a polymer.

[0029] In addition, the polymer composition of the present invention may contain other compounding agents, so long as they do not impair the effects of the present invention, and these can be appropriately selected from known compounds depending on the application of the polymer composition of the present invention and the cured product, such as antioxidants, heat stabilizers, light stabilizers, ultraviolet absorbers, pigments, colorants, foaming agents, antistatic agents, flame retardants, lubricants, softeners, tackifiers, plasticizers, release agents, deodorants, fragrances, dispersants, diluents, etc. The content of additives contained in the polymer composition of the present invention is preferably 5% by mass or less, more preferably 3% by mass or less.

[0030] The polymer composition of the present invention can be produced by mixing the carbon nanotubes (A) and (B) and a polymer.

[0031] The polymer composition of the present invention has a shear viscosity at a temperature of 30°C and a shear rate of 0.1 [1 / sec] that is preferably 0.5 to 24.5 times, more preferably 0.8 to 20.0 times, and even more preferably 0.9 to 15.0 times, the shear viscosity of the polymer contained in the polymer composition. The shear viscosity is a value measured by the method described in the Examples. In addition, the viscosity of a polymer composition that is solid at room temperature may be measured using a known measurement method.

[0032] 2.Cured product of polymer composition The cured product of the present invention is a cured product of the polymer composition of the present invention. When curing the polymer composition of the present invention, a curing agent may be used. For example, when the polymer contained in the polymer composition of the present invention is an epoxy resin, the polymer composition of the present invention is mixed with a curing agent to make the polymer composition of the present invention a curable polymer composition, which is then cured to obtain a cured product. The amount of the curing agent used is preferably 50 parts by mass or less, more preferably 30 parts by mass or less, relative to 100 parts by mass of the polymer composition. In the cured product of the polymer composition of the present invention, it is preferable that the content of carbon nanotubes (A) is 0.00025% by mass or more and less than 0.005% by mass, and the content of carbon nanotubes (B) is 0.0025% by mass or more and less than 0.02% by mass. The ratio of carbon nanotubes (A) to carbon nanotubes (B) is the same as that of the polymer composition of the present invention.

[0033] It is not always necessary to use a curing agent to harden the polymer composition of the present invention. For example, when the polymer contained in the polymer composition of the present invention is a thermoplastic resin, the polymer composition of the present invention that has been heated and is in a fluid state may be cooled and solidified (hardened) to form the cured product of the present invention.

[0034] The surface resistance of the cured product of the present invention is preferably 10 6 ~10 10 Ω / sq., more preferably 10 6 ~10 9 Ω / sq., and more preferably 10 6 ~10 8 Ω / sq. As described above, the cured product of the present invention contains two or more types of carbon nanotubes (A) and (B) having different outer diameters (thickness) at a predetermined ratio, so that even a small amount of the carbon nanotubes easily forms a conductive path between the carbon nanotubes, and the cured product has such a low surface resistance and can exhibit antistatic properties. The method for measuring the surface resistance is as follows, and the method described in the examples can be used as a specific measuring method.

[0035] (Surface resistance measurement) Under standard conditions (23°C, 50% RH), a high resistance resistivity meter (e.g., Hiresta-UX MCP-HT800 (manufactured by Mitsubishi Chemical Analytical Co., Ltd.)) is used to press a probe (e.g., USR probe MCP-HTP14) with a load of 2 kg against the surface of the cured material, and the surface resistance value is measured using a constant voltage application / leakage current measurement method.

[0036] The shape of the cured product of the present invention is not particularly limited and can be any shape. For example, when the polymer composition of the present invention is molded in a mold and cured, the cured product has a shape corresponding to the shape of the mold.

[0037] The cured product of the present invention has a low surface resistivity and excellent antistatic properties, and therefore can be suitably used, for example, as electrical parts and electronic parts. EXAMPLES

[0038] The present invention will be described in more detail below with reference to examples, but the following examples are not intended to limit the scope of the invention. In the present invention, "parts" refers to "parts by mass" and "%" refers to "% by mass".

[0039] The measurement methods used in the examples and comparative examples are as follows.

[0040] (Raman spectrometer) Measurements were performed using a laser Raman microscope (RAMANtouch VIS-NIR-DIS, Nanophoton Co., Ltd.) with a laser wavelength of 532 nm. -1 From 300cm -1 The outer diameter was calculated from the G band (1590 cm). Note that this method cannot detect carbon nanotubes with an outer diameter of more than 2.5 nm, so the outer diameter was calculated from the G band and D band observations, which will be described later. The G / D intensity ratio, which indicates the crystallinity of carbon nanotubes, is calculated from the G band (1590 cm). -1 around 1300 cm-1 The intensity ratio was calculated from the peak intensity ratio of the

[0041] (Transmission electron microscope observation) Observations were performed using a transmission electron microscope (Hitachi High-Technologies Corporation, FEG-equipped transmission electron microscope HF-2000) at an accelerating voltage of 200 kV. The observation sample was prepared by dispersing in an alcohol-based solvent, fixing the dispersion liquid to a microgrid by blotting, and vacuum drying. The field of view was enlarged 1,000,000 times, and the outer diameter (average value) of 50 observed carbon nanotubes was calculated.

[0042] (Measurement of shear viscosity and evaluation of moldability) The viscosity of the polymer composition was measured using a rheometer (manufactured by Thermo Fisher Scientific, product name: HAAKE MARSIII). The temperature condition was standardized at 30°C, and a C35 / 2° cone was used. The representative value was the shear viscosity at a shear rate of 0.1 [1 / s]. Using the shear viscosity (5.6 Pa·s) of a polymer not containing carbon nanotubes at 30°C as a standard, if the shear viscosity was less than 24.5 times the standard, it could be molded in the same way as a polymer not containing carbon nanotubes, and the moldability was evaluated as good "〇". If the shear viscosity was 24.5 times or more the standard, it was difficult to mold in the same way as a polymer not containing carbon nanotubes, and the moldability was evaluated as poor "×".

[0043] (Measurement of surface resistance and evaluation of antistatic properties) Under standard conditions (23°C, 50% RH), a high resistance resistivity meter (Hiresta-UX MCP-HT800, manufactured by Mitsubishi Chemical Analytical Co., Ltd.) was used to press a USR probe MCP-HTP14 with a load of 2 kg against the surface of the cured product of the polymer composition (cured epoxy resin product) and measure the surface resistance value by a constant voltage application / leakage current measurement method. When the surface resistance value was 1×10 11 When the surface resistance is less than 1×10 Ω / sq., the antistatic property is evaluated as good (○). 11When the resistance was Ω / sq. or more, the antistatic property was evaluated as poor (×).

[0044] Details of the raw materials used in the examples and comparative examples are as follows.

[0045] Carbon nanotubes (A): Osaka Soda Co., Ltd. Outer diameter: 2.0nm Carbon Purity: 99.7% GD ratio :75

[0046] Carbon nanotubes (B-1): Zeon Nano Technology (product name: ZEONANO SG101) Outer diameter: 4.0nm Carbon Purity: 99.2% GD ratio :8

[0047] Carbon nanotubes (B-2): Nanocyl (product name: NC7000) Outer diameter: 9.5nm Carbon Purity: 90% GD ratio :1

[0048] Polymer: Bisphenol A epoxy resin (product name "JER-828", manufactured by Mitsubishi Chemical Corporation) Shear viscosity: 5.6 [Pa s] (30°C, shear rate 0.1 [1 / s])

[0049] [Examples 1 to 3 and Comparative Examples 1 to 8] Using Nanovater L-ES (manufactured by Yoshida Kikai Kogyo Co., Ltd.), carbon nanotubes (A), carbon nanotubes (B-1), and carbon nanotubes (B-2) were dispersed in bisphenol A type epoxy resin so as to have the composition shown in Table 1, to obtain a polymer composition. The shear viscosity of the obtained polymer composition at 30 ° C. is as shown in Table 1. Next, the polymer composition and an epoxy resin curing agent (modified aromatic amine product name "WA", manufactured by Mitsubishi Chemical Corporation) were weighed in a mass ratio of 4:1, and mixed uniformly using a self-rotating stirring device (product name "Mazerustar KK-250S", manufactured by Kurabo Industries Co., Ltd.), and degassed to obtain a curable polymer composition. Furthermore, the obtained curable polymer composition was poured into a SUS round mold (diameter 50 mm, thickness 2 mm), and then heated in an oven at 120 ° C. for 5 hours to obtain a cured product of the polymer composition (cured epoxy resin product). The surface resistance value of the cured product is as shown in Table 1. Further, an optical microscope photograph was taken to confirm the surface condition of the cured product of the polymer composition of Example 1. The optical microscope photograph of Example 1 is shown in FIG.

[0050] [Table 1]

[0051] In Table 1, "-" means that the ingredient was not included.

[0052] From the results of Examples 1 to 3 in Table 1, it can be seen that sufficient antistatic performance can be obtained with a small amount of carbon nanotubes (A) and (B) by using them in combination. Although it is possible to satisfy the antistatic performance with only carbon nanotubes (B) as in Comparative Example 7, this is not suitable from the viewpoint of practical use because of the extremely high viscosity during molding. Also, from FIG. 1, it can be seen that in the cured product of the polymer composition of Example 1, carbon nanotubes (A) with a small outer diameter are entangled between carbon nanotubes (B) with a large outer diameter to form conductive paths.

Claims

1. A polymer composition comprising carbon nanotubes (A), carbon nanotubes (B), and a polymer, The outer diameter of the carbon nanotube (A) is less than 3.0 nm, The outer diameter of the carbon nanotube (B) is 4.0 nm or more, a content ratio (mass ratio) of the carbon nanotubes (A) to the carbon nanotubes (B) is (A):(B)=1:400 to 1:0.25, The content of the carbon nanotubes (A) is 0.0005% by mass or more and less than 0.005% by mass, The content of the carbon nanotubes (B) is 0.0005% by mass or more and less than 0.2% by mass in the polymer composition.

2. The polymer composition described in claim 1, wherein the outer diameter of the carbon nanotube (B) is 5.0 nm or more.

3. The polymer composition of claim 1 or 2, wherein the polymer is a curable resin.

4. The polymer composition of any one of claims 1 to 3, further comprising a curing agent.

5. A cured product of the polymer composition according to any one of claims 1 to 4.

6. The surface resistance is 10 6 Ω / sq. Above 10 11 The cured product according to claim 5, having a hardness of less than Ω / sq.

7. The cured product according to claim 5 or 6, which is an electrical or electronic part.

Citation Information

Patent Citations

  • Conductive or antistatic molded article and method for producing the same

    JP2007284521A

  • Method for producing conductive injection-molded article

    JP2007296725A

  • Electroconductive resin composition, and electroconductive coating and electroconductive adhesive using the same

    JP2013091783A

  • Injection molding and method for manufacturing the same

    JP2021161256A

  • Carbon nanotube composite material

    WO2013047796A1