Ferritic Stainless Steel Sheet

A ferritic stainless steel with controlled C, Si, Nb, and N composition precipitates the Laves phase, addressing brazing and corrosion issues in high-temperature treatments, ensuring strength and resistance for automotive heat exchangers.

JP7593357B2Active Publication Date: 2024-12-03JFE STEEL CORP
View PDF 12 Cites 0 Cited by

Patent Information

Application Number
JP2022053244
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2022-03-29
Publication Date
2024-12-03
Estimated Expiration
2042-03-29

AI Technical Summary

Technical Problem

Conventional ferritic stainless steels exhibit insufficient brazing properties, strength, and corrosion resistance when subjected to high-temperature brazing heat treatment, particularly in automotive heat exchangers like exhaust heat recovery units and EGR coolers, due to structural coarsening and sensitization at grain boundaries.

Method used

A ferritic stainless steel composition with controlled amounts of C, Si, Nb, N, and other elements, optimized to precipitate the Laves phase during brazing heat treatment, ensuring excellent brazing properties, strength, and corrosion resistance, with specific element ratios to maintain strength within 25 MPa of the initial tensile strength.

Benefits of technology

The optimized composition achieves excellent brazing properties, maintaining strength and corrosion resistance, preventing structural softening and sensitization, making it suitable for high-temperature brazing applications in automotive heat exchangers.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007593357000001
    Figure 0007593357000001
  • Figure 0007593357000002
    Figure 0007593357000002
Patent Text Reader

Abstract

To provide a ferritic stainless steel sheet that has excellent brazability when being subjected to brazing heat treatment at a high temperature, and also has excellent strength characteristics and corrosion resistance after the brazing heat treatment.SOLUTION: A ferritic stainless steel sheet has a composition including 0.003 to 0.030% C, 0.60 to 1.30% Si, 0.05 to 0.30% Mn, 0.050% or less P, 0.020% or less S, 24.0 to 28.0% Cr, 1.60 to 2.50% Ni, 1.50 to 3.00% Mo, 0.001 to 0.020% Al, 0.20 to 0.80% Nb, 0.030% or less N, each by mass%, and the balance being Fe and unavoidable impurities, while satisfying Expressions (1) and (2); and has an amount of decrease in a tensile strength due to brazing heat treatment of 25 MPa or less. C+N≤0.030%...(1) 3Si+Nb-7C-7N≥2.00%...(2)SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a ferritic stainless steel sheet, and more particularly to a ferritic stainless steel sheet that has excellent brazeability when brazing heat treatment is performed at high temperatures, and also has excellent strength characteristics and corrosion resistance after brazing heat treatment. [Background technology]

[0002] In recent years, in order to comply with stricter exhaust gas regulations in the automotive field, there has been a demand for improved exhaust gas purification performance and fuel efficiency. As a result, the application of automotive heat exchangers such as exhaust heat recovery devices and EGR (Exhaust Gas Recirculation) coolers is expanding.

[0003] The exhaust heat recovery system is a device that warms the coolant from the heat of the exhaust gas through a heat exchanger, improving fuel efficiency and heating performance.The EGR cooler has a mechanism for recirculating exhaust gas, cools the hot exhaust gas on the exhaust side through a heat exchanger, and lowers the combustion temperature by re-inhaling the cooled exhaust gas into the engine, thereby suppressing the generation of nitrogen oxides.

[0004] Many of the heat exchanger parts in exhaust heat recovery devices and EGR coolers have both water passages and exhaust gas passages on the route that recirculates exhaust gas to the intake side of the engine, and are structured by combining pipes, plates, fins, tubes, side plates, etc. Brazing joints using Ni-containing brazing filler metal are used to join and assemble these parts. For this reason, the materials used in heat exchangers are required to have good brazing properties with Ni-containing brazing filler metal and sufficient strength properties after brazing heat treatment.

[0005] Furthermore, exhaust gas contains nitrogen oxides (NOx) and sulfur oxides (SOx), which condense in the heat exchanger and become highly corrosive acidic condensed water. Therefore, materials used in heat exchanger components are required to have high corrosion resistance. In addition, since brazing heat treatment is performed at high temperatures, when a material is subjected to brazing heat treatment, Cr carbonitrides precipitate at the grain boundaries, and a Cr-deficient layer is formed in the vicinity, which may cause a decrease in corrosion resistance, a phenomenon known as sensitization. Therefore, it is necessary to prevent sensitization in order to ensure corrosion resistance after brazing heat treatment.

[0006] For these reasons, austenitic stainless steels such as SUS304L and SUS316L, which have regulated carbon content to suppress the occurrence of sensitization, have been used as materials for the heat exchanger parts of exhaust heat recovery devices and EGR coolers. However, austenitic stainless steels are expensive because they contain a lot of Ni, and because they have a large thermal expansion coefficient, they can be destroyed by thermal fatigue when subjected to restraints accompanied by severe vibrations at high temperatures.

[0007] Therefore, the use of steels other than austenitic stainless steel in the heat exchanger parts of exhaust heat recovery devices and EGR coolers is being considered.

[0008] For example, Patent Document 1 discloses a ferritic stainless steel as a material for exhaust heat recovery devices and EGR coolers, in which an oxide film containing 16.0% or more Nb in cationic fraction is formed after brazing, thereby ensuring corrosion resistance.

[0009] Patent Document 2 discloses a ferritic stainless steel as a material for exhaust heat recovery devices and EGR coolers, in which the amounts of Al, Ti, and Si added are controlled to ensure corrosion resistance.

[0010] Patent Document 3 discloses a ferritic stainless steel as a material for exhaust heat recovery devices and EGR coolers, in which corrosion resistance is ensured by controlling the Al, Si, and Cr concentrations in the oxide film after an annealing process.

[0011] Patent Documents 4 and 5 disclose ferritic stainless steels in which Cr, Mo, and other components are added in a certain relational formula, and the amounts of Al and Ti added are controlled to ensure excellent condensed water corrosion resistance and brazability.

[0012] Patent Document 6 discloses a ferritic stainless steel that ensures excellent condensed water corrosion resistance and brazeability by adding components such as Si and Ni according to a certain relational formula and by suppressing the amount of Al added. [Prior art documents] [Patent documents]

[0013] [Patent Document 1] Patent No. 6157664 [Patent Document 2] Patent No. 6159775 [Patent Document 3] JP 2020-63499 A [Patent Document 4] Patent No. 6517371 [Patent Document 5] Patent No. 6583517 [Patent Document 6] Patent No. 6699670 Summary of the Invention [Problem to be solved by the invention]

[0014] However, in the ferritic stainless steels of Patent Documents 1 to 6, the structure of the steel is coarsened by high-temperature brazing heat treatment using a Ni-containing brazing filler metal, which softens the steel and results in insufficient strength. Furthermore, depending on the brazing filler metal and brazing conditions, brazing properties may be insufficient. Thus, the conventional techniques have not been able to provide good corrosion resistance and good brazing properties at high temperatures using a Ni-containing brazing filler metal, and to ensure sufficient material strength after brazing heat treatment.

[0015] The present invention has been made in consideration of the above circumstances, and has an object to provide a ferritic stainless steel sheet that has excellent brazeability when brazing heat treatment is performed at high temperatures, and also has excellent strength characteristics and corrosion resistance after brazing heat treatment.

[0016] In this specification, the brazing heat treatment (high-temperature brazing heat treatment) refers to the following heat treatment. In a nitrogen carrier gas atmosphere of 0.2 Torr, the sample is heated from room temperature to 970°C at an average heating rate of 18°C / min, held at 970°C for 30 minutes, then heated from 970°C to 1180°C at an average heating rate of 18°C / min, and held at 1180°C for 10 minutes. Then, in the same atmosphere as the above, the sample is cooled at an average cooling rate of 11°C / min in the temperature range from 1180°C to 800°C, an average cooling rate of 6°C / min in the temperature range from 800°C to 600°C, an average cooling rate of 4°C / min in the temperature range from 600°C to 400°C, and an average cooling rate of 2°C / min in the temperature range from 400°C to 200°C. Then, the sample is cooled from 200°C to room temperature in an air atmosphere.

[0017] In addition, in this specification, excellent brazing property means that after the above-mentioned brazing heat treatment is performed on a steel plate having a Ni-containing brazing material applied to its surface, the ratio of the circular equivalent diameter of the brazing material after the brazing heat treatment to the circular equivalent diameter of the brazing material before the brazing heat treatment (spreadability of the brazing material) is 150% or more.

[0018] In this specification, excellent corrosion resistance after brazing heat treatment means that test pieces are taken from the steel plate that has been subjected to the above-mentioned brazing heat treatment, and in accordance with ASTM G48 Method C, the test pieces are immersed for 72 hours in a mixed aqueous solution of 6 mass % FeCl3 + 1 mass % HCl at each temperature (20°C, 25°C, 30°C, 35°C, 40°C, 45°C, 50°C) that is changed from 20°C to 50°C in increments of 5°C and held at a constant temperature. The surface of each test piece is then observed, and the minimum temperature at which pitting corrosion occurs on the surface of the test piece (critical pitting corrosion initiation temperature) is 35°C or higher.

[0019] In this specification, "excellent strength characteristics after brazing heat treatment" means that, in accordance with JIS Z 2241:2011, a tensile test is performed at room temperature using JIS No. 13B test pieces taken parallel to the rolling direction from the steel sheet that has been subjected to the brazing heat treatment and the steel sheet before the brazing heat treatment, at a test speed of 10 mm / min, and the value obtained by subtracting the tensile strength (MPa) after the brazing heat treatment from the tensile strength (MPa) before the brazing heat treatment (reduction in tensile strength due to the brazing heat treatment) is within 25 MPa. [Means for solving the problem]

[0020] The present inventors have conducted extensive research into the relationship between the constituent elements of various stainless steels and precipitates when performing high-temperature Ni-containing brazing heat treatment. As a result, they have discovered that by adding an appropriate amount of Si and further controlling the contents of C, N, and Nb appropriately, the Laves phase can be sufficiently precipitated during the cooling process during brazing heat treatment, and strength properties after brazing heat treatment can be secured.

[0021] The gist and configuration of the present invention are as follows. [1] In mass percent, C: 0.003 to 0.030%, Si: 0.60-1.30%, Mn: 0.05 to 0.30%, P: 0.050% or less, S: 0.020% or less, Cr: 24.0-28.0%, Ni: 1.60-2.50%, Mo: 1.50-3.00%, Al: 0.001 to 0.020%, Nb: 0.20-0.80%, N: 0.030% or less, and satisfying the following formulas (1) and (2), with the balance being Fe and unavoidable impurities: A ferritic stainless steel plate in which the decrease in tensile strength due to brazing heat treatment is within 25 MPa. C+N≦0.030% (1) 3Si+Nb-7C-7N≧2.00% (2) (In formulas (1) and (2), C, N, Si, and Nb represent the contents (mass%) of each element.) [2]Further, in mass percent: Cu: 0.01 to 1.00%, Co: 0.01 to 1.00%, W: 0.01 to 2.00%, The ferritic stainless steel sheet according to [1], containing one or more selected from the following: [3] Furthermore, in mass percent: Ti: 0.01 to 0.10%, V: 0.01 to 0.20%, Zr: 0.01 to 0.10%, Mg: 0.0005~0.0050%, Ca: 0.0005 to 0.0050%, B: 0.0005~0.0050%, REM (rare earth metal): 0.001~0.100%, Sn: 0.001~0.100%, Sb: 0.001 to 0.100%, The ferritic stainless steel sheet according to [1] or [2], containing one or more selected from the following: [4] A ferritic stainless steel sheet according to any one of [1] to [3], which is used for an exhaust heat recovery device or an EGR cooler, in which one or more joints are assembled by brazing heat treatment. Effect of the Invention

[0022] According to the present invention, it is possible to obtain a ferritic stainless steel sheet which has excellent brazeability when brazing heat treatment is performed at high temperatures, and which has excellent strength characteristics and corrosion resistance after brazing heat treatment. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0023] The present invention will be specifically described below.

[0024] First, the reason why the composition of the steel is limited to the above range in the present invention will be explained. Note that the unit of the content of elements in the composition of the steel is "mass%", but hereinafter, it will be simply expressed as "%" unless otherwise specified.

[0025] C: 0.003 to 0.030% A high C content improves strength, while a low C content improves workability. Here, in order to obtain sufficient strength, the C content must be 0.003% or more. However, if the C content exceeds 0.030%, the workability is significantly reduced, and Cr carbides are precipitated at the grain boundaries, causing sensitization and reducing corrosion resistance. Therefore, the C content is set to a range of 0.003 to 0.030%. The C content is preferably 0.005% or more. The C content is preferably 0.025% or less, more preferably 0.020% or less, and even more preferably 0.010% or less.

[0026] Silicon: 0.60-1.30% Silicon is an element that has the effect of promoting the precipitation of the Laves phase during brazing heat treatment. This effect is obtained with a silicon content of 0.60% or more. However, if the silicon content exceeds 1.30%, silicon oxide is formed on the steel sheet surface during brazing heat treatment, and brazeability is reduced. Therefore, the silicon content is set to a range of 0.60 to 1.30%. The silicon content is preferably 0.65% or more, and more preferably 0.70% or more. The silicon content is preferably 1.00% or less, and more preferably 0.80% or less.

[0027] Mn: 0.05 to 0.30% Mn has a deoxidizing effect, and this effect can be obtained with a Mn content of 0.05% or more. However, if the Mn content exceeds 0.30%, the corrosion resistance deteriorates. Therefore, the Mn content is set to a range of 0.05 to 0.30%. The Mn content is preferably 0.10% or more, and more preferably 0.15% or more. Moreover, the Mn content is preferably 0.25% or less, and more preferably 0.20% or less.

[0028] P:0.050% or less P is an element that is inevitably contained in steel, and excessive content of P makes intergranular corrosion more likely to occur. This tendency becomes more pronounced when the P content exceeds 0.050%. Therefore, the P content is set to 0.050% or less. Preferably, the P content is 0.030% or less. There is no particular lower limit for the P content. However, since excessive de-P leads to increased costs, the P content is preferably 0.005% or more.

[0029] S: 0.020% or less S is an element that is inevitably contained in steel, and an S content of more than 0.020% promotes the precipitation of MnS and reduces corrosion resistance. Therefore, the S content is set to 0.020% or less. The S content is preferably 0.015% or less. The lower limit of the S content is not particularly limited. However, since excessive de-S leads to an increase in costs, the S content is preferably 0.0005% or more.

[0030] Cr: 24.0~28.0% Cr is an important element for ensuring the corrosion resistance of stainless steel. If the Cr content is less than 24.0%, sufficient corrosion resistance cannot be obtained. On the other hand, if the Cr content exceeds 28.0%, the material becomes hard and the workability decreases. Therefore, the Cr content is set to a range of 24.0 to 28.0%. The Cr content is preferably 25.0% or more. Moreover, the Cr content is preferably 27.0% or less, and more preferably 26.0% or less.

[0031] Ni: 1.60~2.50% By containing Ni at 1.60% or more, it is possible to suppress the precipitation of the σ phase during brazing heat treatment, which causes a decrease in corrosion resistance after brazing heat treatment. On the other hand, if the Ni content exceeds 2.50%, the stress corrosion cracking susceptibility increases. Therefore, the Ni content is set to a range of 1.50 to 2.50%. The Ni content is preferably 1.70% or more, and more preferably 1.80% or more. In addition, the Ni content is preferably 2.30% or less, and more preferably 2.20% or less.

[0032] Mo: 1.50-3.00% Mo stabilizes the passivation film of stainless steel to improve corrosion resistance. This effect is obtained when the Mo content is 1.50% or more. However, if the Mo content exceeds 3.00%, the σ phase precipitates during brazing heat treatment, lowering the corrosion resistance. Therefore, the Mo content is set to the range of 1.50 to 3.00%. The Mo content is preferably 1.70% or more, and more preferably 1.80% or more. Moreover, the Mo content is preferably 2.50% or less, and more preferably 2.00% or less.

[0033] Al: 0.001 to 0.020% Al is a useful element for deoxidization, and this effect can be obtained with an Al content of 0.001% or more. However, Al is an element active against oxygen, and if the Al content exceeds 0.020%, oxides mainly composed of Al are generated on the surface of the steel during brazing heat treatment. These oxides significantly reduce brazing properties. Therefore, the Al content is set to the range of 0.001 to 0.020%. The Al content is preferably 0.015% or less, and more preferably 0.010% or less.

[0034] Nb: 0.20-0.80% Nb is an element that suppresses the decrease in corrosion resistance (sensitization) caused by the precipitation of Cr carbonitrides during brazing heat treatment by combining with C and N. In addition, it contributes to improving strength by the precipitation of Laves phase. This effect is obtained when the Nb content is 0.20% or more. On the other hand, when the Nb content exceeds 0.80%, the precipitation of Laves phase becomes excessive and the workability is reduced. Therefore, the Nb content is set to the range of 0.20 to 0.80%. The Nb content is preferably 0.25% or more, more preferably 0.30% or more. In addition, the Nb content is preferably 0.60% or less, more preferably 0.40% or less.

[0035] N: 0.030% or less If the N content exceeds 0.030%, the corrosion resistance and workability are reduced. Therefore, the N content is set to 0.030% or less. The N content is preferably 0.025% or less, and more preferably 0.015% or less. Although there is no particular restriction on the lower limit of the N content, excessive reduction of the N content leads to an increase in costs, so the N content is preferably set to 0.003% or more.

[0036] C+N≦0.030% (1) In formula (1), C and N represent the content (mass %) of each element. Excessive C and N content reduces corrosion resistance. Therefore, the C content and N content are set within the above-mentioned ranges, and C+N (the sum of the C content and the N content) is set to 0.030% or less. C+N is preferably 0.024% or less, and more preferably 0.019% or less.

[0037] 3Si+Nb-7C-7N≧2.00% (2) In the formula (2), Si, Nb, C, and N represent the content (mass%) of each element. In the present invention, the contents of Si, Nb, C and N are each set to a predetermined value in order to precipitate a sufficient amount of Laves phase during brazing heat treatment. Furthermore, the inventors have conducted extensive research and found that if 3Si+Nb-7C-7N is less than 2.00%, the amount of Laves phase precipitated after brazing heat treatment is insufficient and the strength after brazing heat treatment decreases significantly. The reason for this is that Si and Nb promote the precipitation of the Laves phase, but an increase in C+N increases the amount of Nb carbonitride precipitated, which consumes Nb and causes a decrease in the amount of Laves phase precipitated, so that the balance of these elements is considered to have a significant effect on the precipitation of the Laves phase. Therefore, the contents of Si, Nb, C and N are each set within the above-mentioned ranges, and 3Si+Nb-7C-7N is set to 2.00% or more. 3Si+Nb-7C-7N is preferably 3.00% or more.

[0038] The basic components (essential components) of the ferritic stainless steel sheet of the present invention have been described above. The balance other than the above basic components can be Fe and unavoidable impurities.

[0039] In the present invention, one or more elements selected from Cu, Co and W may further be contained within the following ranges.

[0040] Cu: 0.01 to 1.00% Cu is an element that enhances corrosion resistance. This effect is obtained when the Cu content is 0.01% or more. However, when the Cu content exceeds 1.00%, the hot workability is reduced. Therefore, when Cu is contained, the Cu content is set to a range of 0.01 to 1.00%. When Cu is contained, the Cu content is preferably 0.10% or more. Moreover, when Cu is contained, the Cu content is preferably 0.80% or less, and more preferably 0.60% or less.

[0041] Co: 0.01 to 1.00% Co is an element that enhances corrosion resistance. This effect is obtained when the Co content is 0.01% or more. However, when the Co content exceeds 1.00%, the workability decreases. Therefore, when Co is contained, the Co content is set to a range of 0.01 to 1.00%. When Co is contained, the Co content is more preferably 0.05% or more. Furthermore, when Co is contained, the Co content is more preferably 0.70% or less.

[0042] W: 0.01 to 2.00% W is an element that enhances corrosion resistance. This effect is obtained when the W content is 0.01% or more. However, when the W content exceeds 2.00%, the workability decreases. Therefore, when W is contained, the W content is set to a range of 0.01 to 2.00%. When W is contained, the W content is more preferably 0.05% or more. Moreover, when W is contained, the W content is more preferably 1.00% or less.

[0043] In the present invention, one or more elements selected from Ti, V, Zr, Mg, Ca, B, REM, Sn, and Sb may further be contained within the following ranges.

[0044] Ti: 0.01 to 0.10% Ti combines with C and N contained in steel and has the effect of preventing sensitization. This effect is obtained with a Ti content of 0.01% or more. On the other hand, Ti is an element active against oxygen, and if the Ti content exceeds 0.10%, oxides mainly composed of Ti are formed on the steel surface during brazing heat treatment. These oxides reduce brazeability. Therefore, when Ti is contained, the Ti content is set to a range of 0.01 to 0.10%. When Ti is contained, the Ti content is more preferably 0.05% or less.

[0045] V: 0.01 to 0.20% Like Ti, V bonds with C and N contained in the steel to prevent sensitization. These effects are obtained when the V content is 0.01% or more. On the other hand, if the V content exceeds 0.20%, the workability decreases. Therefore, when V is contained, the V content is set to a range of 0.01 to 0.20%. When V is contained, the V content is more preferably 0.15% or less, and further preferably 0.10% or less.

[0046] Zr: 0.01 to 0.10% Like Ti and Nb, Zr is an element that combines with C and N contained in steel to suppress sensitization. This effect is obtained when the Zr content is 0.01% or more. On the other hand, when the Zr content exceeds 0.10%, the workability decreases. Therefore, when Zr is contained, the Zr content is set to a range of 0.01 to 0.10%. When Zr is contained, the Zr content is more preferably 0.03% or more. Moreover, when Zr is contained, the Zr content is more preferably 0.05% or less.

[0047] Mg: 0.0005~0.0050% Mg acts as a deoxidizer. This effect is obtained when the Mg content is 0.0005% or more. However, if the Mg content exceeds 0.0050%, the toughness of the steel decreases, and manufacturability decreases. Therefore, when Mg is contained, the Mg content is set to a range of 0.0005 to 0.0050%. When Mg is contained, the Mg content is more preferably 0.0020% or less.

[0048] Ca: 0.0005~0.0050% Ca improves the penetration of the welded portion and improves the weldability. This effect is obtained when the Ca content is 0.0005% or more. However, when the Ca content exceeds 0.0050%, Ca combines with S to generate CaS, which reduces the corrosion resistance. Therefore, when Ca is contained, the Ca content is set to a range of 0.0005 to 0.0050%. When Ca is contained, the Ca content is more preferably 0.0010% or more. Furthermore, when Ca is contained, the Ca content is more preferably 0.0025% or less.

[0049] B: 0.0005~0.0050% B is an element that improves secondary work embrittlement. This effect is manifested when the B content is 0.0005% or more. However, when the B content exceeds 0.0050%, ductility decreases due to solid solution strengthening. Therefore, when B is contained, the B content is set to a range of 0.0005 to 0.0050%. When B is contained, the B content is more preferably 0.0025% or less.

[0050] REM (rare earth metal): 0.001~0.100% REM (rare earth metals: elements with atomic numbers 57 to 71, such as La, Ce, and Nd) are effective elements for deoxidization. The effect can be obtained when the REM content is 0.001% or more. However, when the REM content exceeds 0.100%, the hot workability decreases. Therefore, when REM is contained, the REM content is set to the range of 0.001 to 0.100%. When REM is contained, the REM content is more preferably 0.005% or more. Moreover, when REM is contained, the REM content is more preferably 0.050% or less. Note that REM is a collective term for 15 elements, including Sc, Y, and lanthanum (La) with atomic number 57 to lutetium (Lu) with atomic number 71, and the REM content here is the total content of these elements.

[0051] Sn: 0.001 to 0.100% Sn is an element effective in suppressing roughness of the surface during processing. This effect can be obtained when the Sn content is 0.001% or more. However, when the Sn content exceeds 0.100%, the hot workability is reduced. Therefore, when Sn is contained, the Sn content is set to a range of 0.001 to 0.100%. When Sn is contained, the Sn content is more preferably 0.050% or less.

[0052] Sb: 0.001 to 0.100% Sb, like Sn, is an element that is effective in suppressing roughness of the surface during machining. This effect is obtained when the Sb content is 0.001% or more. However, when the Sb content exceeds 0.100%, the workability decreases. Therefore, when Sb is contained, the Sb content is set to a range of 0.001 to 0.100%. When Sb is contained, the Sb content is more preferably 0.050% or less.

[0053] The chemical composition of the ferritic stainless steel sheet according to the present invention has been explained above. In addition, it is important for materials for exhaust heat recovery devices and EGR coolers to minimize the decrease in strength of the material after brazing heat treatment at high temperatures.

[0054] The decrease in tensile strength due to brazing heat treatment is within 25 MPa The decrease in tensile strength due to brazing heat treatment [MPa] = tensile strength before brazing heat treatment [MPa] - tensile strength after brazing heat treatment [MPa]. As described above, in order to precipitate a sufficient amount of Laves phase during brazing heat treatment, the respective contents of Si, Nb, C, and N were set to predetermined values, and control of the amount of strength loss was examined. As a result, it was found that if the amount of loss in tensile strength due to brazing heat treatment is within 25 MPa, damage due to softening during use of exhaust heat recovery devices and EGR coolers manufactured by brazing heat treatment can be prevented in advance. The amount of loss in tensile strength due to brazing heat treatment is preferably within 15 MPa.

[0055] Next, a preferred method for producing the ferritic stainless steel sheet of the present invention will be described.

[0056] The method for producing the ferritic stainless steel sheet of the present invention is not particularly limited, but for example, a steel slab having the above-mentioned composition is hot-rolled to form a hot-rolled sheet, which is annealed as necessary, and then cold-rolled to form a cold-rolled sheet of a desired thickness, which is annealed as necessary, to produce a ferritic stainless steel sheet having the above-mentioned composition. Note that the conditions for hot rolling, cold rolling, hot-rolled sheet annealing, cold-rolled sheet annealing, etc. are not particularly limited, and may be in accordance with conventional methods.

[0057] In the steelmaking process for producing steel, it is preferable to perform secondary refining of steel melted in a converter or electric furnace by a VOD (Vacuum Oxygen Decarburization) method or the like to produce steel containing the above-mentioned essential components and components added as necessary. The produced molten steel can be made into a steel material by a known method, but from the viewpoint of productivity and quality, it is preferable to use a continuous casting method. The steel material is then preferably heated to 1050 to 1250°C and hot-rolled into a hot-rolled sheet of a desired thickness. Of course, it can also be hot-worked into other products besides sheet materials. The hot-rolled sheet is then preferably subjected to continuous annealing at a temperature of 900 to 1150°C as necessary, and then descaled by pickling or the like to produce a hot-rolled product. Note that, if necessary, scale may be removed by shot blasting or a grinding brush before pickling.

[0058] Furthermore, the above hot rolled product (hot rolled annealed sheet, etc.) may be subjected to a process such as cold rolling to produce a cold rolled product. In this case, cold rolling may be performed once, but may be performed twice or more with intermediate annealing in between in terms of productivity and required quality. The total reduction ratio of one or more cold rollings is preferably 60% or more, more preferably 70% or more. The cold rolled steel sheet is then preferably subjected to continuous annealing (finish annealing) at a temperature of 900 to 1150°C, more preferably 950 to 1150°C, pickled, and produced as a cold rolled product. Note that continuous annealing may be performed as bright annealing, and pickling may be omitted. Furthermore, depending on the application, after finish annealing, skin pass rolling or the like may be performed to adjust the shape, surface roughness, and material properties of the steel sheet.

[0059] The ferritic stainless steel sheet of the present invention described above is suitable for use in exhaust heat recovery devices and EGR coolers (exhaust gas recirculation devices) in which one or more joints are assembled by brazing heat treatment, and is particularly suitable for use as heat exchanger members for the exhaust heat recovery devices and EGR coolers. EXAMPLES

[0060] Steel having the chemical composition shown in Table 1 was melted in a vacuum melting furnace and heated at 1150°C for 1 hour, after which a hot-rolled sheet having a thickness of 4.2 mm was produced by hot rolling, and the hot-rolled sheet was held at 1080°C for 30 seconds or more for hot-rolled sheet annealing. Furthermore, after removing scale from the surface of the steel sheet by grinding, the steel sheet was cold-rolled to a thickness of 1.2 mm to produce a cold-rolled sheet, which was then held at 1040°C for 30 seconds for finish annealing to produce a cold-rolled annealed sheet.

[0061] (1) Brazeability evaluation A test piece of 50×50 mm was taken from the prepared cold-rolled annealed sheet, and the surface was polished with #600 emery paper, and then degreased with acetone. A Ni-containing brazing filler metal (main components (remainder): Ni-29mass%Cr-6mass%P-4mass%Si) with a diameter of 12 mmΦ and a thickness of 1 mm was placed on the polished surface. Then, the brazing heat treatment described below was performed with the surface on which the Ni-containing brazing filler metal was placed facing up and the steel sheet surface horizontal. Then, the circle equivalent diameter of the brazing filler metal on the surface of the test piece (the circle equivalent diameter of the brazing filler metal after the brazing heat treatment) was measured. Then, the ratio of the circle equivalent diameter of the brazing filler metal after the brazing heat treatment to the diameter of the brazing filler metal before the brazing heat treatment (12mmΦ, the circle equivalent diameter is also the same) was calculated (spreadability of the brazing filler metal), and evaluated according to the following criteria. Spreadability of the brazing filler metal after brazing heat treatment to that before brazing heat treatment = (equivalent circle diameter of the brazing filler metal after brazing heat treatment / equivalent circle diameter of the brazing filler metal before brazing heat treatment) x 100 (%) ○(Pass): 150% or more × (Fail): Less than 150% In this test, a brazing material having a spreading rate of 150% or more after the brazing heat treatment relative to before the brazing heat treatment was evaluated as having excellent brazeability.

[0062] <Brazing heat treatment> In a nitrogen carrier gas atmosphere of 0.2 Torr, the temperature range from room temperature to 970 ° C. was heated at an average heating rate of 18 ° C. / min, and then held at 970 ° C. for 30 minutes, and then heated at an average heating rate of 18 ° C. / min in the temperature range from 970 ° C. to 1180 ° C., and held at 1180 ° C. for 10 minutes. Then, in the same atmosphere as the above atmosphere, the temperature range from 1180 ° C. to 800 ° C. was cooled at an average cooling rate of 11 ° C. / min, the temperature range from 800 ° C. to 600 ° C. was cooled at an average cooling rate of 6 ° C. / min, the temperature range from 600 ° C. to 400 ° C. was cooled at an average cooling rate of 4 ° C. / min, and the temperature range from 400 ° C. to 200 ° C. was cooled at an average cooling rate of 2 ° C. / min. Then, it was cooled from 200 ° C. to room temperature in an air atmosphere.

[0063] (2) Evaluation of corrosion resistance The prepared cold-rolled annealed sheet was subjected to the brazing heat treatment. Then, a test piece of 50 mm × 30 mm was taken from the cold-rolled annealed sheet subjected to the brazing heat treatment, and the surface was polished with #600 emery paper and then degreased with acetone. Then, in accordance with ASTM G48 Method C, the test piece was immersed for 72 hours in a 6 mass% FeCl3 + 1 mass% HCl mixed aqueous solution at each temperature (20 ° C, 25 ° C, 30 ° C, 35 ° C, 40 ° C, 45 ° C, 50 ° C) that was changed from 20 ° C to 50 ° C in 5 ° C increments and held at a constant temperature. The surface of each test piece was observed with a magnifying glass to confirm the presence or absence of pitting corrosion. The minimum temperature at which pitting corrosion occurred was defined as the critical pitting corrosion occurrence temperature, and was evaluated according to the following criteria. ◎ (Pass, especially good): Critical pitting temperature is 45℃ or higher ○(Pass): Critical pitting temperature is 35℃ or higher and less than 45℃ × (Fail): Critical pitting temperature is less than 35°C In this test, materials with a minimum temperature at which pitting corrosion occurred (critical pitting corrosion temperature) of 35°C or higher were rated as having excellent corrosion resistance after brazing heat treatment.

[0064] (3) Strength characteristic evaluation after brazing heat treatment The prepared cold-rolled annealed sheet was subjected to the brazing heat treatment. Then, a tensile test was performed at room temperature at a test speed of 10 mm / min using JIS 13B test pieces taken parallel to the rolling direction from each of the steel sheets after the brazing heat treatment and before the brazing heat treatment in accordance with JIS Z 2241:2011, and the tensile strength was evaluated according to the following criteria based on the value obtained by subtracting the tensile strength (MPa) after the brazing heat treatment from the tensile strength (MPa) before the brazing heat treatment (amount of reduction in tensile strength due to the brazing heat treatment). Decrease in tensile strength due to brazing heat treatment [MPa] = tensile strength before brazing heat treatment [MPa] - tensile strength after brazing heat treatment [MPa] ◎ (Pass, especially good): Within 15MPa ○(Pass): Over 15MPa ~ Within 25MPa ×(Fail): Over 25MPa In this test, a material with a tensile strength reduction of 25 MPa or less due to brazing heat treatment was evaluated as having excellent strength characteristics after brazing heat treatment.

[0065] [Table 1]

[0066] [Table 2]

[0067] As shown in Tables 1 and 2, in all of Examples 1 to 26, when brazing heat treatment was performed at high temperatures, ferritic stainless steel sheets were obtained that had excellent brazeability and excellent strength properties and corrosion resistance after brazing heat treatment.

[0068] On the other hand, in Comparative Examples 27 to 37, whose composition was outside the appropriate range, it was not possible to simultaneously satisfy all of the targets for brazeability when brazing heat treatment was performed at high temperatures, and strength properties and corrosion resistance after brazing heat treatment.

[0069] In Comparative Example No. 27, the Al content exceeded the upper limit of the present invention, and therefore excellent brazeability was not obtained. In Comparative Example No. 28, the Si content exceeded the upper limit of the present invention, and therefore excellent brazeability was not obtained. In Comparative Example No. 29, the Mn content exceeded the upper limit of the present invention, and therefore excellent corrosion resistance was not obtained. In Comparative Example No. 30, the Mo content exceeded the upper limit of the present invention, and therefore the σ phase precipitated significantly, failing to provide excellent corrosion resistance. In Comparative Example No. 31, the Si content was below the lower limit of the present invention, so that the Laves phase was not sufficiently produced during the brazing heat treatment, and excellent strength properties were not obtained after the brazing heat treatment. In Comparative Example No. 32, the Cr content was below the lower limit of the present invention, and therefore excellent corrosion resistance was not obtained. In Comparative Example No. 33, the Ni content was below the lower limit of the present invention, and therefore excellent corrosion resistance was not obtained. In Comparative Example No. 34, the Nb content was less than the lower limit of the present invention, so that the Laves phase was not sufficiently produced during the brazing heat treatment, and excellent strength characteristics after the brazing heat treatment were not obtained. In Comparative Example No. 35, since the Mo content was below the lower limit of the present invention, excellent corrosion resistance was not obtained. In Comparative Example No. 36, all of the components were within the specified ranges, but the requirements of formula (1) were not satisfied, so excellent corrosion resistance was not obtained. In Comparative Example No. 37, all the components were within the specified ranges, but did not satisfy the requirements of formula (2). Therefore, the Laves phase was not sufficiently produced during the brazing heat treatment, and excellent strength properties were not obtained after the brazing heat treatment. [Industrial Applicability]

[0070] According to the present invention, a ferritic stainless steel sheet can be obtained that is suitable as a material for heat exchangers such as heat recovery devices and EGR coolers, particularly heat exchangers such as exhaust heat recovery devices and EGR coolers in which one or more joints are assembled by brazing heat treatment, and is therefore extremely useful industrially.

Claims

1. In mass percent, C: 0.003-0.030%, Si: 0.60-1.30%, Mn: 0.05-0.30%, P: 0.050% or less, S: 0.020% or less, Cr: 24.0-28.0%, Ni: 1.60-2.50%, Mo: 1.50-3.00%, Al: 0.001-0.020%, Nb: 0.20-0.80%, N: 0.030% or less, and satisfying the following formulas (1) and (2), with the balance being Fe and unavoidable impurities: A ferritic stainless steel plate in which the amount of decrease in tensile strength due to brazing heat treatment is within 25 MPa. C+N≦0.030%...(1) 3Si+Nb-7C-7N≧2.00%...(2) (In formulas (1) and (2), C, N, Si, and Nb represent the content (mass%) of each element.)

2. Further, in mass percent, Cu: 0.01 to 1.00%, Co: 0.01 to 1.00%, W: 0.01-2.00%, The ferritic stainless steel sheet according to claim 1, comprising one or more selected from the following:

3. Further, in mass percent, Ti: 0.01 to 0.10%, V: 0.01-0.20%, Zr: 0.01 to 0.10%, Mg: 0.0005-0.0050%, Ca: 0.0005-0.0050%, B: 0.0005-0.0050%, REM (rare earth metal): 0.001-0.100%, Sn: 0.001 to 0.100%, Sb: 0.001 to 0.100%, The ferritic stainless steel sheet according to claim 1 or 2, comprising one or more selected from the following:

4. The ferritic stainless steel sheet according to any one of claims 1 to 3, which is used for an exhaust heat recovery device or an EGR cooler, in which one or more joints are assembled by brazing heat treatment.

Citation Information

Patent Citations

  • Thermosetting coating material

    JP1986057664A

  • Semiconductor device

    JP1986059775A

  • Ferritic stainless steel and manufacturing method therefor

    JP2017150016A

  • Multi phase-based stainless steel excellent in steam oxidation resistance

    JP2017206735A

  • Stainless steel

    JP2020063499A