Purple zirconia sintered body and its manufacturing method

A zirconia sintered body with controlled Al2O3, Y2O3, and Nd2O3 composition and tetragonal crystal structure addresses the lack of translucency and color stability in existing purple zirconia, ensuring long-term color consistency and strength.

JP7593389B2Active Publication Date: 2024-12-03TOSOH CORP
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
JP2022194602
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2016-02-09
Filing Date
2022-12-06
Publication Date
2024-12-03
Estimated Expiration
2036-12-21

AI Technical Summary

Technical Problem

Existing purple zirconia sintered bodies lack translucency and exhibit significant color tone changes due to deterioration over time, affecting their aesthetic and functional longevity.

Method used

A zirconia sintered body composition comprising specific amounts of Al2O3, Y2O3, and Nd2O3, with a tetragonal crystal structure, is developed to provide translucency and maintain a stable purple color tone during long-term use.

Benefits of technology

The solution achieves a translucent, purple-colored zirconia sintered body with minimal color tone change, maintaining aesthetic appeal and mechanical strength.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007593389000001
    Figure 0007593389000001
  • Figure 0007593389000002
    Figure 0007593389000002
  • Figure 0007593389000003
    Figure 0007593389000003
Patent Text Reader

Abstract

Provided is a raw material powder from which a translucent, purple-colored zirconia sintered body can be produced, which exhibits little change in color tone over long-term use. [Solution] The raw material powder is zirconia containing 0.01% by weight or more and 1.0% by weight or less of aluminum oxide, and the remainder being 1.2 mol% or more and 3.5 mol% or less of yttria and 0.01 mol% or more and 2 mol% or less of neodia.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a purple zirconia sintered body. [Background technology]

[0002] Zirconia sintered bodies can exhibit any color by containing lanthanoid rare earth oxides or transition metals as colorants (Patent Document 1). When the zirconia sintered body contains a colorant, it has high designability in addition to the high-class feel and mechanical strength inherent to zirconia. Therefore, the zirconia sintered body containing a colorant (hereinafter also referred to as "colored zirconia sintered body") is being applied to a wide range of applications, such as decorative members and exterior members, in addition to conventional optical applications, medical applications, and mechanical applications. With the expansion of applications, more differentiated designability is being demanded for the colored zirconia sintered body. Furthermore, among colored zirconia sintered bodies, zirconia sintered bodies that exhibit bright colors such as red, pink, orange, purple, light blue, and light gray have a particularly strong effect on designability, so the demands for color tone are increasing.

[0003] For example, the following have been reported as purple zirconia sintered bodies.

[0004] Patent Document 1 describes a purple zirconia sintered body called Y 2 O 3 , MgO or CaO, and CoO 2 or Nd 2 O 3 A zirconia sintered body containing

[0005] In addition, as a purple zirconia sintered body that is not bluish or reddish, a zirconia sintered body containing cobalt oxide, nickel oxide and titanium oxide, or neodymium oxide has been reported (Patent Document 2). [Prior art documents] [Patent documents]

[0006] [Patent Document 1] Japanese Patent Application Publication No. 62-59571 [Patent Document 2] JP 2011-020877 A Summary of the Invention [Problem to be solved by the invention]

[0007] The purple sintered bodies disclosed in Patent Documents 1 and 2 do not exhibit translucency. The color tone of the opaque sintered body is expressed only by the reflected light on the surface. The color tone of these sintered bodies changes significantly due to the deterioration of the sintered body over a long period of use. Even if there is no decrease in strength, the lifespan of these sintered bodies as components is shortened due to changes in aesthetics.

[0008] Furthermore, the color tone of a translucent sintered body is affected not only by the reflected light on the surface but also by the scattered light and transmitted light inside the sintered body. Therefore, the color tone of a translucent sintered body changes more significantly with deterioration than an opaque sintered body.

[0009] In view of these problems, the present invention aims to provide a zirconia sintered body that has translucency and is purple in color and exhibits little change in color tone over long-term use. [Means for solving the problem]

[0010] The present inventors have investigated discoloration due to deterioration during use in a colored zirconia sintered body and the prevention of discoloration. As a result, they have found a zirconia sintered body that has translucency by using a specific composition and exhibits a purple color with almost no change in color tone during use.

[0011] That is, the present invention is Al 2 O 3The zirconia sintered body has a content of 0.01% by weight or more and 1.0% by weight or less, with the remainder being zirconia containing 1.2 mol % or more and 3.5 mol % or less of yttria and 0.01 mol % or more and 2 mol % or less of neodia.

[0012] The zirconia sintered body of the present invention will be described below.

[0013] The sintered body of the present invention is Al 2 O 3 The content is 0.01% by weight or more and 1.0% by weight or less, preferably 0.03% by weight or more and 0.8% by weight or less, and more preferably 0.04% by weight or more and 0.6% by weight or less. If the alumina content is less than 0.01% by weight, the sintered body will have low strength. 2 O 3 If the content exceeds 1.0% by weight, the density of the sintered body tends to decrease. This results in greater individual variation in color tone. 2 O 3 The content can be 0.05% by weight or more and 0.3% by weight or less.

[0014] In the present invention, Al 2 O 3 The content is the Al content relative to the weight of the sintered body of the present invention. 2 O 3 It can be calculated from the weight ratio of

[0015] The sintered body of the present invention is made of yttria (Y 2 O 3 ) and Neodia (Nd 2 O 3 The content of the Y / Nd-containing zirconia is 99% by weight or more and 99.99% by weight or less, preferably 99.2% by weight or more and 99.97% by weight or less, and more preferably 99.4% by weight or more and 99.96% by weight or less.

[0016] In the present invention, the content of Y / Nd-containing zirconia can be determined from the weight ratio of Y / Nd-containing zirconia to the weight of the sintered body of the present invention.

[0017] Y / Nd-containing zirconia is 2 O 3 and Nd 2 O 3 It is zirconia containing.

[0018] Yttrium functions as a stabilizer without coloring zirconia. The yttria content of zirconia is 1.2 mol% or more and 3.5 mol% or less, preferably 1.3 mol% or more and 3.2 mol% or less, and more preferably 1.5 mol% or more and 3.0 mol% or less. If the yttria content is less than 1.2 mol%, the sintered body is likely to break during production or under hydrothermal conditions. On the other hand, if the yttria content exceeds 3.5 mol%, not only does the strength of the sintered body decrease, but the transparency becomes too high. If the transparency becomes too high, the coloring becomes weak, and the coloring tends to be different from purple.

[0019] In the present invention, the yttria content (mol%) is the molar ratio of yttria to the total of yttria, neodia, and zirconia in zirconia (Y 2 O 3 / (Y 2 O 3 +Nd 2 O 3 +ZrO 2 )) can be obtained.

[0020] Neodymium mainly functions as a colorant. The zirconia contains neodia, which gives the sintered body of the present invention a purple color. The neodia content is preferably 0.01 mol% or more and 2 mol% or less, more preferably 0.03 mol% or more and 1.8 mol% or less, and even more preferably 0.05 mol% or more and 1.5 mol% or less.

[0021] In the present invention, the neodia content (mol%) is the molar ratio of neodia to the total of yttria, neodia, and zirconia in zirconia (Nd2 O 3 / (Y 2 O 3 +Nd 2 O 3 +ZrO 2 )) can be obtained.

[0022] The molar ratio of the yttria content (mol%) to the neodymium content (mol%) in zirconia (hereinafter referred to as "Y 2 O 3 / Nd 2 O 3 The ratio of yttria to neodia is preferably 0.8 or more, and more preferably 1 or more. Both yttria and neodia have the effect of stabilizing the crystal phase of zirconia. However, the stabilizing effect of yttria is stronger than that of neodia. Therefore, by using more yttria than neodia, the sintered body of the present invention has a more stabilized crystal phase and is purple in color. Y 2 O 3 / Nd 2 O 3 The ratio is arbitrary as long as the above yttria content and the above neodymium content are satisfied. 2 O 3 / Nd 2 O 3 The upper limit of the ratio may be 50, or even 10, or even 5.

[0023] The zirconia crystal structure of the sintered body of the present invention preferably contains tetragonal crystals, and the main phase of the crystal structure is preferably tetragonal. In order for the sintered body of the present invention to have translucency and a purple color, tetragonal crystals that scatter grain boundary light are essential. In addition, the zirconia crystal structure of the sintered body of the present invention may contain cubic crystals or may be a mixed crystal of tetragonal and cubic crystals, as long as the main phase is tetragonal, that is, the tetragonal content is 50% or more, further 80% or more, or further 90% or more.

[0024] When the average crystal grain size is appropriately small, the sintered body of the present invention has the strength to be used in various components, etc. Therefore, the average crystal grain size of the sintered body of the present invention is 0.3 μm or more and 0.5 μm or less, and preferably 0.3 μm or more and 0.45 μm or less.

[0025] The sintered body of the present invention preferably has a relative density of 99.7% or more, more preferably 99.75% or more, and even more preferably 99.80% or more. When the relative density is 99.7% or more, the sintered body of the present invention is more likely to have translucency. In the present invention, the relative density is the ratio of the actually measured density to the theoretical density. For the theoretical density, the density of the HIP-treated body obtained by subjecting a molded body having the same composition to the primary sintering and HIP treatment was used.

[0026] The measured density of the sintered body of the present invention varies depending on the composition, but is 6.075 g / cm 3 More than 6.155g / cm 3 Below that, 6.080g / cm 3 More than 6.150g / cm 3 or less, or even 6.085 g / cm 3 More than 6.145g / cm 3 The following are some of the reasons:

[0027] The sintered body of the present invention has translucency. The sintered body of the present invention exhibits a more aesthetic color tone than the color tone exhibited by only surface reflected light, by exhibiting a color tone that is expressed by not only surface reflected light but also surface reflected light such as scattered light and transmitted light inside the sintered body and other light. In order to enhance aesthetics, the sintered body of the present invention preferably has a total light transmittance (hereinafter also simply referred to as "total light transmittance") of 10% or more, further 13% or more, or even 15% or more for a sample thickness of 1.0 mm, relative to a light source D65. On the other hand, if the translucency is too high, the color tone tends to be weak. Therefore, the total light transmittance is preferably less than 40%. A preferred total light transmittance is 10% or more and less than 40%, further 10% or more and 35% or less, or further 10% or more and 25% or less.

[0028] The sintered body of the present invention exhibits a purple color.* a * b * In the color system, lightness L * is between 45 and 85, a * is between -5 and 20 and b * The more desirable color tone can be confirmed by checking that the lightness L is between -25 and 5. * is between 50 and 80, a * is between -3 and 15 and b * is between -20 and 0, and the lightness L * is between 54 and 75, a * is between -1 and 12 and b * is between -18 and -5.

[0029] The sintered body of the present invention does not change in color even after long-term use. The absence of color change can be confirmed by measuring the color of the sintered body before and after use. In particular, the absence of color change can be confirmed by measuring the color of the sintered body after immersing in hot water at 140°C for 24 hours and the color of the sintered body before immersion, using the color difference calculated by the following formula:

[0030] Color tone difference ΔE={(L 1 * -L 2 * ) 2 +(a 1 * -a 2 * ) 2 +(b 1 * -b 2 * ) 2} 0.5 In the above formula, L 1 * , a 1 * and b 1 * are the lightness values ​​of the sintered bodies before immersion, respectively. * , saturation a * and b * It is. 2 * , a 2 * and b2 * are the lightness values ​​of the sintered bodies after immersion, respectively. * , saturation a * and b * It is.

[0031] The sintered body of the present invention has a ΔE value calculated by the above formula of 2.0 or less, preferably 1.8 or less, and more preferably 1.0 or less. If ΔE is 2.0 or less, no change in aesthetics can be recognized by visual observation. Theoretically, the lower limit of ΔE is 0, but taking into account measurement errors, etc., ΔE should be 0.2 or more.

[0032] The three-point bending strength of the sintered body of the present invention can be 1000 MPa or more, and further 1050 MPa or more. If the strength is too high, the workability decreases, so the three-point bending strength of the zirconia sintered body of the present invention may be 1300 MPa or less, and further 1250 MPa or less.

[0033] In the present invention, the three-point bending strength can be measured by a method in accordance with IS R 1601.

[0034] Next, a method for producing the sintered body of the present invention will be described.

[0035] The sintered body of the present invention can be produced by a production method including a sintering step of sintering a molded body which is zirconia containing 0.01% by weight or more and 1.0% by weight or less of aluminum oxide, and the remainder being 1.2 mol% to 3.5 mol% of yttria and 0.01 mol% to 2 mol% of neodiamondia, at 1350°C to 1500°C.

[0036] The molded body to be subjected to the sintering step is zirconia containing 0.01% to 1.0% by weight of aluminum oxide, and the balance being 1.2% to 3.5% by weight of yttria and 0.01% to 2% by weight of neodia. A more preferred molded body is zirconia containing 0.03% to 0.8% by weight of aluminum oxide, and the balance being 1.3% to 3.2% by weight of yttria and 0.03% to 1.8% by weight of neodia.

[0037] The aluminum oxide content is alumina (Al 2 O 3 The ratio of alumina (Al) to the total weight of aluminum oxide (calculated as 0.01%) and zirconia containing yttria and neodymium (Y / Nd-containing zirconia) was calculated as 0.01%. 2 O 3 The weight percentage of aluminum oxide can be calculated by converting the weight percentage of aluminum oxide into the mass fraction of aluminum oxide.

[0038] The shape of the molded body is arbitrary, and examples thereof include at least one type selected from the group consisting of a disk shape, a column shape, a plate shape, a sphere shape, and a roughly sphere shape.

[0039] The compact is obtained by compacting a raw material powder containing Y / Nd-containing zirconia and aluminum oxide in the above-mentioned composition.

[0040] The raw material powder has the above composition, and the average particle size is preferably 0.35 μm to 0.60 μm, and more preferably 0.40 μm to 0.55 μm. The BET specific surface area is 5 to 15 m. 2 / g, and even 7~13m 2 It is preferable that the molecular weight is 1 / g.

[0041] The raw powder is preferably a spray-granulated powder granule (hereinafter simply referred to as "powder granule"), and is preferably a powder granule containing an organic binder. By making the raw powder into a powder granule, the flowability during formation of a compact is increased, and pores are easily eliminated from the compact. This makes it difficult for bubbles to form in the sintered body.

[0042] The organic binder may be at least one of the commonly used organic binders selected from the group consisting of polyvinyl alcohol, polyvinyl butyrate, wax, and acrylic. The content of the organic binder in the powder granules may be 1% by weight or more and 5% by weight or less based on the raw material powder.

[0043] When the raw powder is made into powder granules, the average granule size is preferably 30 μm or more and 80 μm or less, and the bulk density is 1.10 g / cm 3 More than 1.40g / cm 3 It is preferable that:

[0044] The Y / Nd-containing zirconia contained in the raw material powder is yttria (Y 2 O 3 ) and Neodia (Nd 2 O 3 ) may be used. Furthermore, the Y / Nd-containing zirconia may be at least two kinds of powders selected from the group consisting of yttria-containing zirconia, neodia-containing zirconia, and yttria-neodia-containing zirconia, or may be a mixed powder of yttria-containing zirconia and yttria-neodia-containing zirconia. Compared with a mixed powder of yttria powder, neodia powder, and zirconia powder, or a mixed powder of yttria-containing zirconia powder and neodia powder, the color tone of the obtained sintered body is more likely to be uniform by using zirconia powder containing yttria and neodia before sintering. It is particularly preferable that the Y / Nd-containing zirconia is at least one of a mixed powder of yttria-containing zirconia and yttria-neodia-containing zirconia, or a yttria-neodia-containing zirconia powder.

[0045] The Y / Nd-containing zirconia powder preferably has an yttria content of 1.2 mol% to 3.5 mol%, more preferably 1.3 mol% to 3.2 mol%, and more preferably has a neodia content of 0.01 mol% to 2 mol%, more preferably 0.03 mol% to 1.8 mol%. When the Y / Nd-containing zirconia contains yttria-containing zirconia powder, the yttria content of the yttria-containing zirconia powder may be 2 mol% to 4 mol%, more preferably 2 mol% to 3.5 mol%. When the Y / Nd-containing zirconia contains neodia-containing zirconia powder, the neodia content of the neodia-containing zirconia powder may be 0.02 mol% to 4 mol%.

[0046] The aluminum oxide contained in the raw material powder is preferably at least one powder selected from the group consisting of alumina, hydrated alumina, alumina sol, aluminum hydroxide, aluminum chloride, aluminum nitrate, and aluminum sulfate, and more preferably at least one powder selected from the group consisting of alumina, hydrated alumina, and alumina sol.

[0047] The raw material powder may be prepared by mixing Y / Nd-containing zirconia and aluminum oxide by any method.

[0048] The raw material powder may have an aluminum oxide content of 0.01% by weight or more and 1.0% by weight or less, with the remainder being Y / Nd-containing zirconia, and further may have an aluminum oxide content of 0.03% by weight or more and 0.8% by weight or less, with the remainder being Y / Nd-containing zirconia.

[0049] Particularly preferred raw material powders are a mixed powder of yttria-containing zirconia and yttria-neodia-containing zirconia, or a mixed powder of at least one of yttria-neodia-containing zirconia powder and alumina powder.

[0050] The molded body can be obtained by molding the raw material powder, which may be crushed and then molded. The molding method may be any method capable of molding the raw material powder into a desired shape, and may be, for example, at least one method selected from the group consisting of die pressing, cold isostatic pressing, slip casting, and injection molding.

[0051] In the sintering step, the compact is sintered in an oxidizing atmosphere at a sintering temperature of 1350° C. to 1500° C. In this way, the sintered body of the present invention is obtained.

[0052] Sintering is performed in an oxidizing atmosphere. By sintering in an oxidizing atmosphere, the sintered body of the present invention has translucency and exhibits a purple color. The oxidizing atmosphere can be either an oxygen gas atmosphere or an air atmosphere. For convenience, an air atmosphere is preferable.

[0053] The sintering temperature is preferably 1400°C or higher and 1490°C or lower, more preferably 1410°C or higher and 1480°C or lower, and even more preferably 1420°C or higher and 1470°C or lower.

[0054] The heating rate is 800° C. / hour or less, and further 650° C. / hour or less. A preferred heating rate is 50° C. / hour to 800° C. / hour or less, and further 100° C. / hour to 700° C. / hour or less. This makes it possible to suppress the progress of sintering during the heating process and sinter the molded body at the sintering temperature.

[0055] The holding time at the sintering temperature (hereinafter also simply referred to as "holding time") may be any time depending on the sintering temperature. The holding time can be, for example, 5 hours or less, further 3 hours or less, or further 2 hours or less.

[0056] The sintering method is preferably pressureless sintering. Pressureless sintering is a method of sintering a molded body by simply heating it without applying an external force. A specific example of pressureless sintering is sintering under atmospheric pressure.

[0057] The manufacturing method of the present invention may include at least one of a polishing step of polishing the sintered body or a processing step of processing the shape. The polishing step polishes the surface of the sintered body after sintering. By polishing, the sintered body can be made to have a surface state suitable for the intended use, such as imparting a glossy feel to the surface. The processing step processes the sintered body into an arbitrary shape. This allows the sintered body to have a shape according to the use. Either the polishing step or the processing step may be performed first. Effect of the Invention

[0058] According to the present invention, it is possible to provide a zirconia sintered body which has translucency and is purple in color and shows little change in color tone over long-term use. EXAMPLES

[0059] The present invention will be specifically described below with reference to examples, but the present invention is not limited to these examples.

[0060] (Average particle size) The average particle size of the powder sample was measured using a Microtrac particle size distribution analyzer (device name: 9320-HRA, manufactured by Honeywell). As a pretreatment, the sample powder was suspended in distilled water to prepare a slurry, which was then dispersed for 3 minutes using an ultrasonic homogenizer (device name: US-150T, manufactured by Nippon Seiki Seisakusho).

[0061] In the present invention, the "average particle size" of the zirconia powder refers to the diameter of a sphere having the same volume as a particle at the median value of the cumulative curve of the particle size distribution expressed on a volume basis (median diameter; particle size corresponding to 50% of the cumulative curve), and is measured using a particle size distribution measuring device using a laser diffraction method.

[0062] (Average granule diameter) The average granule size of the granule samples was determined by a sieve test method.

[0063] (Average grain size of sintered body) The average crystal grain size of the sintered body samples was determined by the planimetric method from SEM photographs taken with a field emission scanning electron microscope (FESEM). That is, the mirror-polished sintered body samples were thermally etched and observed with a field emission scanning electron microscope (instrument name: JSM-T220, manufactured by JEOL Ltd.). The average crystal grain size was calculated from the obtained SEM photographs by the planimetric method.

[0064] (density of sintered body) The measured density of the sintered body sample was determined by Archimedes' method. A HIP-treated body with the same composition as the sintered body sample was prepared, and the measured density of the HIP-treated body was determined by Archimedes' method, which was used as the theoretical density. The relative density of the sintered body sample was calculated from the ratio of the measured density of the sintered body to the theoretical density.

[0065] (Total light transmittance) The total light transmittance of the sintered body sample was measured using a turbidity meter (device name: NDH2000, manufactured by Nippon Denshoku Co., Ltd.) according to a method conforming to JIS K7361. A double-sided polished disk-shaped sintered body having a thickness of 1 mm was used as the measurement sample.

[0066] (color tone) The color tone of the sintered body sample was measured by a method conforming to JIS Z 8729. For the measurement, a color difference meter (device name: Z-300, manufactured by Nippon Denshoku Industries Co., Ltd.) was used.

[0067] For the measurement, a disk-shaped sintered body having a thickness of 2.8 mm and polished on one side was used. The color tone was measured on the polished surface of the sintered body.

[0068] (strength) The three-point bending strength of the sintered samples was measured by the three-point bending method according to JIS R 1601.

[0069] Example 1 A hydrated zirconia sol was obtained by hydrolyzing an aqueous solution of zirconium oxychloride. Yttria (Y 2 O 3) and Neodia (Nd 2 O 3 ) was added to the hydrated zirconia sol, which was then dried and calcined to obtain calcined zirconia powder containing yttria and neodia. The calcination conditions were 1170°C for 2 hours in air. The calcined powder obtained was washed with distilled water and then dried to obtain Y / Nd-containing zirconia powder. The ratio of Al to the weight of the Y / Nd-containing zirconia powder was 2 O 3 α-alumina having an average particle size of 0.3 μm was added to the Y / Nd-containing zirconia powder so that the content was 0.05 wt % to prepare a mixed powder.

[0070] Distilled water was added to the mixed powder to obtain a slurry with a powder content of 45% by weight, which was then pulverized in a ball mill using zirconia balls with a diameter of 2 mm as the pulverization medium in water for 16 hours.

[0071] The average particle size and BET specific surface area of ​​the powder in the slurry after the pulverization process (hereinafter also referred to as the "pulverized slurry") were measured. The BET specific surface area was measured on the zirconia powder after the pulverized slurry was dried at 110°C in the air. The average particle size was 0.45 μm and the BET specific surface area was 12.3 m. 2 / g.

[0072] After adding 3% by weight of an organic binder to the ground slurry, the mixture was spray-dried to obtain powder granules. The powder granules had an average granule diameter of 46 μm and a loose bulk density of 1.23 g / cm. 3 It was.

[0073] The obtained granules were preformed in a uniaxial press at 19.6 MPa, and then molded by cold isostatic pressing (hereinafter also referred to as "CIP") at 196 MPa to obtain a molded body. The obtained molded body was sintered under atmospheric pressure at a sintering temperature of 1450°C, a heating rate of 600°C / hr, and a holding time of 2 hours in an air atmosphere to obtain a zirconia sintered body of this example. The obtained zirconia sintered body had translucency and was purple in color.

[0074] The composition of the Y / Nd-containing zirconia powder is shown in Table 1, and the evaluation results of the zirconia sintered body of this example are shown in Tables 2 and 3.

[0075] Example 2 A pulverized slurry and powder granules were obtained in the same manner as in Example 1, except that yttria and neodia were added to the hydrated zirconia sol so that the yttria concentration was 1.59 mol% and the neodia concentration was 1.48 mol%, and the calcination temperature was 1210°C.

[0076] The powder in the crushed slurry has an average particle size of 0.43 μm and a BET specific surface area of ​​13.8 m 2 / g, and the powder granules have an average granule diameter of 43 μm and a light bulk density of 1.26 g / cm 3 It was.

[0077] Except for using the obtained powder granules, the zirconia sintered body of this example was obtained by molding and sintering in the same manner as in Example 1. The obtained zirconia sintered body had translucency and was purple in color.

[0078] The composition of the Y / Nd-containing zirconia powder is shown in Table 1, and the evaluation results of the zirconia sintered body of this example are shown in Tables 2 and 3.

[0079] Example 3 A pulverized slurry and powder granules were obtained in the same manner as in Example 1, except that yttria and neodia were added to the hydrated zirconia sol so that the yttria concentration was 1.59 mol% and the neodia concentration was 1.48 mol%, and the calcination temperature was 1210°C.

[0080] The powder in the crushed slurry has an average particle size of 0.43 μm and a BET specific surface area of ​​13.8 m 2 / g, and the powder granules have an average granule diameter of 43 μm and a light bulk density of 1.26 g / cm 3 It was.

[0081] A zirconia sintered body of this example was obtained by molding and sintering in the same manner as in Example 1, except that the obtained powder granules were used and the sintering temperature was set to 1500° C. The obtained zirconia sintered body had translucency and was purple in color.

[0082] The composition of the Y / Nd-containing zirconia powder is shown in Table 1, and the evaluation results of the zirconia sintered body of this example are shown in Tables 2 and 3.

[0083] Example 4 A hydrated zirconia sol was obtained by hydrolysis of an aqueous solution of zirconium oxychloride. Yttria was added to the hydrated zirconia sol so that the yttria concentration was 3 mol%, and then the sol was dried and calcined to obtain calcined zirconia powder containing yttria. The calcination conditions were 1100°C for 2 hours in air. The calcined powder obtained was washed with distilled water and dried to obtain yttria-containing zirconia powder.

[0084] A pulverized slurry and powder granules were obtained in the same manner as in Example 1, except that the obtained yttria-containing zirconia powder was used.

[0085] The powder in the crushed slurry has an average particle size of 0.42 μm and a BET specific surface area of ​​13.1 m 2 / g, the average granule diameter of the powder granules is 45 μm and the light bulk density is 1.27 g / cm 3 It was.

[0086] The obtained powder granules and powder granules obtained in the same manner as in Example 1 were mixed by stirring to obtain a mixed powder granule having the following composition.

[0087] Al 2 O 3 :0.05% by weight Y / Nd-containing zirconia: balance In addition, the composition of the Y / Nd-containing zirconia in the mixed powder granules is Y. 2 O 3 2.3mol%, Nd 2 O 3 0.74 mol% and the balance is ZrO 2It was.

[0088] Except for using the obtained mixed powder granules, molding and sintering were performed in the same manner as in Example 1 to obtain a sintered body of this example. The obtained zirconia sintered body had translucency and was purple in color.

[0089] The composition of the Y / Nd-containing zirconia in the mixed powder granules is shown in Table 1, and the evaluation results of the zirconia sintered body of this example are shown in Tables 2 and 3.

[0090] Example 5 The sintered body of this example was obtained in the same manner as in Example 4, except that the mixed powder granules had the following composition.

[0091] Al 2 O 3 :0.05% by weight Y / Nd-containing zirconia: balance In addition, the composition of the Y / Nd-containing zirconia in the mixed powder granules is Y. 2 O 3 2.93mol%, Nd 2 O 3 0.07mol%, and the balance is ZrO 2 It was.

[0092] The obtained zirconia sintered body had translucency and was purple in color.

[0093] The composition of the Y / Nd-containing zirconia in the mixed powder granules is shown in Table 1, and the evaluation results of the zirconia sintered body of this example are shown in Tables 2 and 3.

[0094] Comparative Example 1 Neodia-containing zirconia powder, crushed slurry, and powder granules were obtained in the same manner as in Example 1, except that neodia was added to the hydrated zirconia sol so that the neodia concentration was 3 mol %, and that no yttria was added.

[0095] The powder in the crushed slurry has an average particle size of 0.41 μm and a BET specific surface area of ​​14.1 m 2 / g, and the powder granules have an average granule diameter of 43 μm and a light bulk density of 1.22 g / cm 3 It was.

[0096] A zirconia sintered body of this comparative example was produced by molding and sintering in the same manner as in Example 1, except that the obtained powder granules were used. However, in this comparative example, cracks occurred during sintering, and a sintered body that maintained its shape was not obtained. The results are shown in Tables 1 and 2.

[0097] Comparative Example 2 An yttria-containing zirconia powder, a crushed slurry, and powder granules were obtained in the same manner as in Comparative Example 1, except that neodia was added to the hydrated zirconia sol so that the neodia concentration was 4 mol %.

[0098] The powder in the crushed slurry has an average particle size of 0.42 μm and a BET specific surface area of ​​13.9 m 2 / g, and the powder granules have an average granule diameter of 47 μm and a light bulk density of 1.23 g / cm 3 It was.

[0099] The sintered body of this comparative example was produced by molding and sintering in the same manner as in Comparative Example 1, except that the obtained powder granules were used. However, in this comparative example, cracks occurred during sintering, and a sintered body that maintained its shape was not obtained. The results are shown in Tables 1 and 2.

[0100] Comparative Example 3 A Y / Nd-containing zirconia powder, a crushed slurry, and powder granules were obtained in the same manner as in Comparative Example 1, except that yttria and neodia were added to the hydrated zirconia sol so that the yttria concentration was 1.08 mol %.

[0101] The powder in the crushed slurry has an average particle size of 0.43 μm and a BET specific surface area of ​​13.8 m 2 / g, and the powder granules have an average granule diameter of 48 μm and a light bulk density of 1.26 g / cm 3 It was.

[0102] The sintered body of this comparative example was produced by molding and sintering in the same manner as in Comparative Example 1, except that the obtained powder granules were used and the sintering temperature was set to 1500°C. However, in this comparative example, cracks occurred during sintering, and a sintered body that maintained its shape was not obtained. The results are shown in Tables 1 and 2.

[0103] [Table 1]

[0104] [Table 2]

[0105] [Table 3]

[0106] (Measurement of color change ΔE) The sintered bodies of Examples 1 to 5 were each immersed in hot water at 140° C. for 24 hours, and the color tone of the sintered bodies was measured before and after the immersion to determine the color tone difference ΔE. The results are shown in Table 4.

[0107] [Table 4]

[0108] As can be seen from Table 4, the color difference ΔE was 2.0 or less in all cases, and no change in color was confirmed by visual inspection. [Industrial Applicability]

[0109] The zirconia sintered body of the present invention can be used not only for structural materials such as pulverized members, dental members such as dental prostheses and color-adjusting materials, but also for members such as jewelry and decorative members, for example, watch parts, exterior parts of portable electronic devices, and various other members.

Claims

1. A raw material powder which is zirconia containing 0.01 wt % or more and 1.0 wt % or less of aluminum oxide, and the remainder being 1.2 mol % or more and 3.5 mol % or less of yttria and 0.05 mol % or more and 2 mol % or less of neodia.

2. 2. The raw material powder according to claim 1, wherein the molar ratio of the yttria content to the neodymium content in the zirconia is 0.8 or more.

3. 3. The raw material powder according to claim 1, having an average particle size of 0.35 μm to 0.60 μm.

4. BET specific surface area is 5 to 15 m 2 The raw material powder according to claim 1 or 2, wherein the molecular weight of the raw material powder is 1000 or more.

5. 3. The raw material powder according to claim 1, wherein the aluminum oxide is at least one powder selected from the group consisting of alumina, alumina hydrate, alumina sol, aluminum hydroxide, aluminum chloride, aluminum nitrate, and aluminum sulfate.

6. 3. The raw material powder according to claim 1, wherein the zirconia is at least one of a mixed powder of yttria-containing zirconia and yttria-neodia-containing zirconia, and an yttria-neodia-containing zirconia powder.

7. A molded body comprising zirconia containing 0.01 wt % or more and 1.0 wt % or less of aluminum oxide, and the remainder being 1.2 mol % or more and 3.5 mol % or less of yttria and 0.05 mol % or more and 2 mol % or less of neodia.

Citation Information

Patent Citations

  • Colored zirconia sintered body and its producton

    JP1987059571A

  • Purple zirconia sintered compact

    JP2011020877A

  • Composite plate and method for producing the same

    JP2015089656A

  • Zirconia sintered body and use thereof

    WO2015099048A1