Thermosetting resin composition
The thermosetting resin composition, with a specific blend of polyalkenylphenol, polymaleimide, and polyethylene glycol compounds, addresses the challenges of adhesion, reflow resistance, and moldability in semiconductor packaging, ensuring high heat resistance and reduced peeling.
Patent Information
- Application Number
- JP2022527499
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2020-05-28
- Filing Date
- 2021-01-27
- Publication Date
- 2024-12-03
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
Existing thermosetting resin compositions used in semiconductor packaging face challenges in achieving high heat resistance without compromising adhesion to metals, moldability, and reflow resistance, often leading to issues like peeling and mold release problems due to stress and thermal stress.
A thermosetting resin composition comprising a polyalkenylphenol compound, a polymaleimide compound, a polyethylene glycol compound, and a radical initiator, with specific molecular structures and ratios, to enhance adhesion, reflow resistance, and moldability while maintaining heat resistance.
The composition provides a cured product with excellent adhesion to metals, improved reflow resistance, and good moldability without sacrificing heat resistance, addressing the trade-offs in existing resin systems.
Smart Images

Figure 0007593402000016 
Figure 0007593402000017 
Figure 0007593402000001
Abstract
Description
[Technical field]
[0001] The present invention relates to a thermosetting resin composition, a cured product thereof, a method for producing a structure using the thermosetting resin composition, and a structure including the cured product. [Background technology]
[0002] In recent years, with the increasing density of electronic components, semiconductor packages used in electronic devices and industrial equipment are required to have higher wiring density, smaller size, thinner profile, higher heat resistance, higher heat dissipation, etc. Therefore, the encapsulating material, which is a plastic material, is also required to have high heat resistance.
[0003] Transfer molding is a method in which the material is heated and softened in a plunger, then the heated and softened material is forced into a heated mold cavity through passages in the mold such as gates, sprues, and runners, and hardened inside the mold cavity. Since the material is injected into the cavity in a highly fluid state, molding can be done at low pressure.
[0004] Transfer molding is characterized by being less likely to damage the insert than other molding methods that require high pressure. Transfer molding allows for miniaturization and fine processing, and has high productivity, making it known as a representative molding method for encapsulating power semiconductors and ICs.
[0005] Conventionally, epoxy-phenolic thermosetting resin materials have been used as sealing materials in transfer molding. However, it is difficult to meet the recent demand for high heat resistance with conventional materials. In order to meet the demand for high heat resistance, sealing materials with various resin systems have been proposed, such as thermosetting resin compositions containing a large amount of polyfunctional epoxy resin, and thermosetting resin compositions containing highly heat-resistant structures such as bismaleimide, triazine skeleton, benzoxazine skeleton, and silsesquioxane skeleton.
[0006] Patent Document 1 (JP Patent Publication No. 11-140277) describes an epoxy resin composition for semiconductor encapsulation, characterized in that the essential components are (A) a phenolic resin containing, based on the total phenolic resin amount, 30 to 100 parts by mass of a phenolic resin having a novolac structure containing a biphenyl derivative and / or a naphthalene derivative in the molecule, (B) an epoxy resin containing, based on the total epoxy resin amount, 30 to 100 parts by mass of an epoxy resin having a novolac structure containing a biphenyl derivative and / or a naphthalene derivative in the molecule, (C) an inorganic filler, and (D) a curing accelerator.
[0007] Patent Document 2 (JP Patent Publication 5-43630 A) describes an aromatic bismaleimide resin composition containing N,N'-(alkyl-substituted diphenylmethane)bismaleimide and polyallylphenol obtained by condensing salicylaldehyde with phenol.
[0008] Patent Document 3 (JP Patent Publication No. 5-6869) describes a semiconductor device in which a semiconductor element is encapsulated with a resin composition containing (A) a maleimide compound having two or more maleimide groups in one molecule, (B) an allylated phenol resin having a specific repeating unit, and (C) a curing catalyst.
[0009] Patent Document 4 (JP Patent Publication No. 6-93047) describes a curable resin composition obtained by blending a maleimide compound, an alkenylphenol compound having a specific structure, and an epoxy group-containing organosilane compound in a specific ratio. [Prior art documents] [Patent documents]
[0010] [Patent Document 1] Japanese Patent Application Publication No. 11-140277 [Patent Document 2] Japanese Patent Application Publication No. 5-43630 [Patent Document 3] Japanese Patent Application Publication No. 5-6869 [Patent Document 4] Japanese Patent Application Publication No. 6-93047 Summary of the Invention [Problem to be solved by the invention]
[0011] In material development, when the resin system is changed significantly, problems may occur in balancing the performances that are in a trade-off relationship. For example, methods for increasing the heat resistance of materials include increasing the number of functional groups in epoxy resins to increase the crosslink density (Patent Document 1) and using maleimide resins as other resins (Patent Documents 2-4). The more the heat resistance of the material is increased by these methods, the denser the crosslink structure of the cured product of the thermosetting resin becomes, so the material becomes harder and stronger, and the elastic modulus of the cured product tends to increase. As a result, when the cured product is used in close contact with a different material, such as when the thermosetting resin is used as an encapsulant, problems such as the material peeling off due to the stress generated at the interface are likely to occur. In particular, in devices that are repeatedly and intensely subjected to stress and / or thermal stress, peeling is likely to occur between the cured product that constitutes them and other members.
[0012] In addition, in resin moldings that include metal inserts, a trade-off is likely to occur between moldability, such as bleed-out and releasability, and adhesion to internal parts. These properties tend to change significantly when the skeleton and polarity of the main resin are changed.
[0013] Therefore, there is a demand for materials that have excellent adhesion to other members such as metals, and excellent reflow resistance and heat cycle resistance without compromising heat resistance and moldability. In order to resolve the above trade-off, it is useful to use additives that are suitable for the resin system.
[0014] The present disclosure describes a thermosetting resin composition that gives a cured product that has excellent adhesion to metals and excellent reflow resistance without impairing moldability and the heat resistance of the cured product. [Means for solving the problem]
[0015] That is, the present invention relates to the following [1] to
[15] . [1] A thermosetting resin composition comprising a polyalkenylphenol compound (A), a polymaleimide compound (B), a polyethylene glycol compound (C), and a radical initiator (D), The polyethylene glycol compound (C) has a structural unit represented by formula (1), and the structural unit represented by formula (1) accounts for 90 mol % to 100 mol % of all structural units. Thermosetting resin composition. [ka] [2] The thermosetting resin composition according to [1], wherein the content of the polyethylene glycol compound (C) is 1 to 10 mass% based on the total content of the polyalkenylphenol compound (A), the polymaleimide compound (B), and the polyethylene glycol compound (C). [3] The thermosetting resin composition according to [1] or [2], wherein the polyethylene glycol compound (C) has a number average molecular weight Mn of 2,000 to 50,000. [4] The thermosetting resin composition according to any one of [1] to [3], wherein the content of the polyalkenylphenol compound (A) is 5 to 200 parts by mass per 100 parts by mass of the polymaleimide compound (B). [5] The thermosetting resin composition according to any one of [1] to [4], wherein the polyethylene glycol compound (C) is polyethylene glycol. [6] The polyalkenylphenol compound (A) is represented by the formula (2)-1: [ka] and optionally formula (2)-2: [ka] A polyalkenylphenol compound having a structural unit represented by the formula: In formula (2)-1 and formula (2)-2, R1 each independently represents a hydrogen atom, an alkyl group having 1 to 5 carbon atoms, or an alkoxy group having 1 to 5 carbon atoms; R 2 are each independently expressed by the formula (3): [ka] In the formula (3), R 3 , R 4 , R 5 , R 6 , and R 7 are each independently a hydrogen atom, an alkyl group having 1 to 5 carbon atoms, a cycloalkyl group having 5 to 10 carbon atoms, or an aryl group having 6 to 12 carbon atoms, * in formula (3) represents a bond to a carbon atom constituting an aromatic ring, R 1 and R 2 may be the same or different in each phenol skeleton unit, and each Q independently represents a group of the formula -CR 8 R 9 -, a cycloalkylene group having 5 to 10 carbon atoms, a divalent organic group having an aromatic ring, a divalent organic group having an alicyclic condensed ring, or a divalent organic group combining these, R 8 and R 9 each independently represents a hydrogen atom, an alkyl group having 1 to 5 carbon atoms, an alkenyl group having 2 to 6 carbon atoms, a cycloalkyl group having 5 to 10 carbon atoms, or an aryl group having 6 to 12 carbon atoms. The thermosetting resin composition according to any one of [1] to [5]. [7] The thermosetting resin composition according to [6], wherein p is a real number of 1.1 to 35, p+q is a real number of 1.1 to 35, and q is a real number such that the value of the formula: p / (p+q) is 0.4 to 1, where p is an average number of structural units represented by formula (2)-1 per molecule, and q is an average number of structural units represented by formula (2-2) per molecule. [8] The thermosetting resin composition according to any one of [1] to [7], wherein the polymaleimide compound (B) is an aromatic bismaleimide compound. [9] The thermosetting resin composition according to any one of [1] to [8], wherein the radical initiator (D) is an organic peroxide.
[10] The thermosetting resin composition according to any one of [1] to [9], further comprising a filler (E).
[11] The thermosetting resin composition according to
[10] , wherein the filler (E) is at least one selected from the group consisting of silica, alumina, magnesium oxide, and solid rubber particles.
[12] The thermosetting resin composition according to
[10] or
[11] , wherein a content of the filler (E) is 200 to 1900 parts by mass per 100 parts by mass in total of the polyalkenylphenol compound (A), the polymaleimide compound (B), the polyethylene glycol compound (C), and the radical initiator (D).
[13] A cured product of the thermosetting resin composition according to any one of [1] to
[12] .
[14] A method for producing a structure, comprising molding the thermosetting resin composition according to any one of [1] to
[12] .
[15] A structure comprising the cured product according to
[13] . Effect of the Invention
[0016] According to the present invention, it is possible to obtain a thermosetting resin composition which gives a cured product having excellent adhesion to metals and excellent reflow resistance without impairing moldability and the heat resistance of the cured product. [Brief description of the drawings]
[0017] [Figure 1] FIG. 2 is a schematic diagram of a molding die, a top plate, and a bottom plate used in evaluating demolding properties. [Diagram 2] FIG. 2 is a schematic diagram of a sample used for evaluating releasability. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0018] The present invention will be described in detail below. A thermosetting resin composition according to one embodiment contains a polyalkenylphenol compound (A), a polymaleimide compound (B), a polyethylene glycol compound (C), and a radical initiator (D).
[0019] [Polyalkenylphenol compound (A)] The polyalkenylphenol compound (A) is a compound having at least two phenol skeletons in the molecule, and having 2-alkenyl groups bonded to some or all of the aromatic rings forming the phenol skeletons in the molecule. The 2-alkenyl group is preferably a group having a structure represented by formula (3).
[0020] [ka]
[0021] In formula (3), R 3 , R 4 , R 5 , R 6 , and R 7 are each independently a hydrogen atom, an alkyl group having 1 to 5 carbon atoms, a cycloalkyl group having 5 to 10 carbon atoms, or an aryl group having 6 to 12 carbon atoms. * in formula (3) represents a bond to a carbon atom constituting an aromatic ring.
[0022] R in Equation (3) 3 , R 4 , R 5 , R 6 , and R 7Specific examples of the alkyl group having 1 to 5 carbon atoms constituting the formula (1) include a methyl group, an ethyl group, an n-propyl group, an isopropyl group, an n-butyl group, a sec-butyl group, a tert-butyl group, and an n-pentyl group. Specific examples of the cycloalkyl group having 5 to 10 carbon atoms include a cyclopentyl group, a cyclohexyl group, a methylcyclohexyl group, and a cycloheptyl group. Specific examples of the aryl group having 6 to 12 carbon atoms include a phenyl group, a methylphenyl group, an ethylphenyl group, a biphenyl group, and a naphthyl group. The 2-alkenyl group represented by formula (3) is an allyl group, that is, R 3 , R 4 , R 5 , R 6 , and R 7 are preferably all hydrogen atoms.
[0023] In the polyalkenylphenol compound (A), 2-alkenyl groups are bonded to preferably 40 to 100%, more preferably 60 to 100%, and even more preferably 80 to 100% of the aromatic rings constituting the phenol skeleton.
[0024] The basic skeleton of the polyalkenylphenol compound (A) may be that of a known phenol resin such as a phenol novolac resin, a cresol novolac resin, a triphenylmethane type phenol resin, a phenol aralkyl resin, a biphenyl aralkyl phenol resin, a phenol-dicyclopentadiene copolymer resin, etc. Among them, a polyalkenylphenol compound (A) having a structural unit shown in the following formula (2)-1 and optionally the formula (2)-2 can be preferably used.
[0025] [ka] [ka]
[0026] The structural units shown in formula (2)-1 and formula (2)-2 are preferred phenol skeleton units constituting the polyalkenylphenol compound (A), and the bonding order of these phenol skeleton units is not particularly limited. 1 each independently represents a hydrogen atom, an alkyl group having 1 to 5 carbon atoms, or an alkoxy group having 1 to 5 carbon atoms; and in formula (2)-1, R 2 R is each independently a 2-alkenyl group represented by formula (3). 1 and R 2 may be the same or different in each phenol skeleton unit. Q independently represents a group of the formula -CR 8 R 9 -, a cycloalkylene group having 5 to 10 carbon atoms, a divalent organic group having an aromatic ring, a divalent organic group having an alicyclic condensed ring, or a divalent organic group combining these, 8 and R 9 each independently represents a hydrogen atom, an alkyl group having 1 to 5 carbon atoms, an alkenyl group having 2 to 6 carbon atoms, a cycloalkyl group having 5 to 10 carbon atoms, or an aryl group having 6 to 12 carbon atoms.
[0027] When the average number of structural units shown in formula (2)-1 per molecule is p and the average number of structural units shown in formula (2)-2 per molecule is q, preferably, p is a real number of 1.1 to 35, p+q is a real number of 1.1 to 35, and q is a real number such that the value of the formula: p / (p+q) is 0.4 to 1.
[0028] R 1 Specific examples of the alkyl group having 1 to 5 carbon atoms include a methyl group, an ethyl group, an n-propyl group, an isopropyl group, an n-butyl group, a sec-butyl group, a tert-butyl group, an n-pentyl group, etc. Specific examples of the alkoxy group having 1 to 5 carbon atoms include a methoxy group, an ethoxy group, an n-propoxy group, an isopropoxy group, an n-butoxy group, a sec-butoxy group, a tert-butoxy group, an n-pentoxy group, etc.
[0029] Formula-CR 8R 9 R is an alkylene group represented by - 8 and R 9 In the above, specific examples of the alkyl group having 1 to 5 carbon atoms include a methyl group, an ethyl group, an n-propyl group, an isopropyl group, an n-butyl group, a sec-butyl group, a tert-butyl group, and an n-pentyl group. Specific examples of the alkenyl group having 2 to 6 carbon atoms include a vinyl group, an allyl group, a butenyl group, a pentenyl group, and a hexenyl group. Specific examples of the cycloalkyl group having 5 to 10 carbon atoms include a cyclopentyl group, a cyclohexyl group, a methylcyclohexyl group, and a cycloheptyl group. Specific examples of the aryl group having 6 to 12 carbon atoms include a phenyl group, a methylphenyl group, an ethylphenyl group, a biphenyl group, and a naphthyl group.
[0030] Specific examples of the cycloalkylene group having 5 to 10 carbon atoms constituting Q include a cyclopentylene group, a cyclohexylene group, a methylcyclohexylene group, and a cycloheptylene group. Specific examples of the divalent organic group having an aromatic ring include a phenylene group, a tolylene group, a naphthylene group, a biphenylene group, a fluorenylene group, an anthracenylene group, a xylylene group, and a 4,4-methylenediphenyl group. The number of carbon atoms of the divalent organic group having an aromatic ring can be 6 to 20 or 6 to 14. Specific examples of the divalent organic group having an alicyclic condensed ring include a dicyclopentadienylene group. The number of carbon atoms of the divalent organic group having an alicyclic condensed ring can be 7 to 20 or 7 to 10.
[0031] It is preferable that Q is a dicyclopentadienylene group, a phenylene group, a methylphenylene group, a xylylene group, or a biphenylene group, in terms of high mechanical strength of the cured product.It is preferable that Q is -CH2-, since the viscosity of the polyalkenylphenol compound (A) is low and it is advantageous to mix it with the polymaleimide compound (B).
[0032] p is preferably a real number from 1.1 to 35, more preferably a real number from 2 to 30, and further preferably a real number from 3 to 10. When p is 1.1 or more, the thermal decomposition onset temperature when a cured product of the thermosetting resin composition is placed in a high-temperature environment is appropriate, and when p is 35 or less, the viscosity of the thermosetting resin composition is in a range suitable for processing during molding.
[0033] p+q is preferably a real number of 1.1 to 35, more preferably a real number of 2 to 30, and further preferably a real number of 3 to 10. When p+q is 1.1 or more, the thermal decomposition onset temperature when a cured product of the thermosetting resin composition is placed in a high-temperature environment is appropriate, and when p+q is 35 or less, the viscosity of the thermosetting resin composition is in a range suitable for processing during molding.
[0034] q is preferably a real number that makes the value of the formula: p / (p+q) 0.4 to 1, more preferably a real number that makes the value of the formula: p / (p+q) 0.6 to 1, and even more preferably a real number that makes the value of the formula: p / (p+q) 0.8 to 1. When the value of the formula: p / (p+q) is 1, q is 0. That is, in this embodiment, the polyalkenylphenol compound (A) does not contain the structural unit shown in formula (2)-2. The polyalkenylphenol compound (A) can have only the structural unit shown in formula (2)-1. If q is a value that satisfies the above condition, the degree of curing of the thermosetting resin composition can be made sufficient depending on the application.
[0035] The number average molecular weight Mn of the polyalkenylphenol compound (A) is preferably 300 to 5000, more preferably 400 to 4000, and further preferably 500 to 3000. When the number average molecular weight Mn is 300 or more, the thermal decomposition starting temperature is appropriate when the cured product of the thermosetting resin composition is placed in a high-temperature environment, and when it is 5000 or less, the viscosity of the thermosetting resin composition falls within a range suitable for processing during molding.
[0036] The polyalkenylphenol compound (A) can be obtained by converting a part of the hydroxyl groups of the raw phenolic resin into alkenyl ethers, and then rearranging the 2-alkenyl groups by the Claisen rearrangement reaction. As the raw phenolic resin, a known phenolic resin having a structural unit represented by the following formula (2)-2 can be preferably used. [ka]
[0037] Specific examples of the raw material phenol resin for the polyalkenylphenol compound (A) include phenol novolac resin, cresol novolac resin, triphenylmethane type phenol resin, phenol aralkyl resin, biphenyl aralkyl resin, and phenol-dicyclopentadiene copolymer resin.
[0038] As the 2-alkenyl etherification reaction of the raw material phenol resin, there can be mentioned two methods: (i) a known method of reacting a halogenated 2-alkenyl compound such as allyl chloride, methallyl chloride, allyl bromide, etc. with a phenol compound, and (ii) a known method of reacting a 2-alkenyl carboxylate compound such as allyl acetate, etc. with a phenol compound. For the 2-alkenyl etherification reaction using a halogenated 2-alkenyl compound, for example, the method described in JP-A-2-91113 can be used. For the method of reacting a 2-alkenyl carboxylate compound with a phenol resin, for example, the method described in JP-A-2011-26253 can be used.
[0039] The amount of the 2-alkenyl halide compound or 2-alkenyl carboxylate compound used relative to the phenolic hydroxyl group is preferably 0.4 to 5.0 equivalents, more preferably 0.6 to 4.0 equivalents. When the amount is 0.4 equivalents or more, the number of reaction sites with the polymaleimide compound (B) after the Claisen rearrangement is more appropriate, and a cured product having better heat resistance can be obtained.
[0040] The 2-alkenyl etherification reaction is carried out by mixing the 2-alkenyl compound with the raw material phenolic resin and reacting for 4 to 40 hours. In the 2-alkenyl etherification reaction, a solvent in which the raw material phenolic resin dissolves can be used. The reaction can also be carried out without a solvent by using a 2-alkenyl carboxylic acid compound capable of dissolving the raw material phenolic resin.
[0041] The 2-alkenyl etherification rate of the raw material phenol resin can also be controlled by suppressing the reaction rate (conversion rate) of the 2-alkenyl compound low by using a larger amount of the 2-alkenyl halogenated compound or the 2-alkenyl carboxylate compound than the above-mentioned amount and adjusting the reaction time to be shorter than the above-mentioned reaction time.
[0042] The target polyalkenylphenol compound (A) can be obtained by subjecting the polyalkenyl ether compound produced by the method described in (i) or (ii) above to a Claisen rearrangement reaction. The Claisen rearrangement reaction can be carried out by heating the polyalkenyl ether compound to a temperature of 100 to 250°C and reacting for 1 to 20 hours. The Claisen rearrangement reaction can be carried out using a high boiling point solvent or without a solvent. In order to promote the rearrangement reaction, an inorganic salt such as sodium thiosulfate or sodium carbonate can be added. Details are disclosed in, for example, JP-A-2-91113.
[0043] [Polymaleimide compound (B)] The polymaleimide compound (B) is a compound having two or more maleimide groups represented by formula (4). By blending the polymaleimide compound (B), the heat resistance of the cured product can be improved. [ka]
[0044] In formula (4), * represents a bond to an organic group containing an aromatic ring or a straight-chain, branched-chain, or cyclic aliphatic hydrocarbon group.
[0045] Examples of the polymaleimide compound (B) include bismaleimides such as bis(4-maleimidophenyl)methane, trismaleimides such as tris(4-maleimidophenyl)methane, tetrakismaleimides such as bis(3,4-dimaleimidophenyl)methane, and polymaleimides such as poly(4-maleimidostyrene). Examples of the polymaleimide compound (B) include aromatic polymaleimide compounds and aliphatic polymaleimide compounds, and aromatic polymaleimide compounds are preferred in that the flame retardancy of the resulting cured product is particularly excellent.
[0046] The aromatic polymaleimide compound is a compound having two or more maleimide groups represented by formula (4), and these maleimide groups are bonded to the same or different aromatic rings. Specific examples of the aromatic ring include a single ring such as benzene, and a condensed ring such as naphthalene and anthracene. Since they are mixed well in the curable resin composition, the polymaleimide compound (B) is preferably an aromatic bismaleimide compound or an aliphatic bismaleimide compound, and more preferably an aromatic bismaleimide compound.
[0047] Specific examples of the aromatic bismaleimide compound include bis(4-maleimidophenyl)methane, bis(3-maleimidophenyl)methane, bis(3-methyl-4-maleimidophenyl)methane, bis(3,5-dimethyl-4-maleimidophenyl)methane, bis(3-ethyl-4-maleimidophenyl)methane, bis(3,5-diethyl-4-maleimidophenyl)methane, bis(3-propyl-4-maleimidophenyl)methane, bis(3,5-dipropyl-4-maleimidophenyl)methane, bis(3-butyl-4-maleimidophenyl)methane, bis (3,5-dibutyl-4-maleimidophenyl)methane, bis(3-ethyl-4-maleimido-5-methylphenyl)methane, 2,2-bis(4-maleimidophenyl)propane, 2,2-bis[4-(4-maleimidophenyloxy)phenyl]propane, bis(4-maleimidophenyl)ether, bis(3-maleimidophenyl)ether, bis(4-maleimidophenyl)ketone, bis(3-maleimidophenyl)ketone, bis(4-maleimidophenyl)sulfone, bis(3-maleimidophenyl)sulfone, bis[4-(4-maleimidophenyl) 1,4-Bis(4-maleimidophenyl)cyclohexane, 1,4-dimaleimido naphthalene, 2,3-dimaleimido naphthalene, 1,5-dimaleimido naphthalene, 1,8-dimaleimido naphthalene, 2,6-dimaleimido naphthalene, 2,7-dimaleimido naphthalene, 4,4'-dimaleimido biphenyl, 3,3'-di Maleimido biphenyl, 3,4'-dimaleimido biphenyl, 2,5-dimaleimido-1,3-xylene, 2,7-dimaleimido fluorene, 9,9-bis(4-maleimidophenyl)fluorene, 9,9-bis(4-maleimido-3-methylphenyl)fluorene, 9,9-bis(3-ethyl-4-maleimidophenyl)fluorene, 3,7-dimaleimido-2-methoxyfluorene, 9,10-dimaleimidophenanthrene, 1,2-dimaleimido anthraquinone, 1,5-dimaleimido anthraquinone, 2,6-dimaleimido anthraquinone, 1,Examples of the dimaleimidobenzene include 2-dimaleimidobenzene, 1,3-dimaleimidobenzene, 1,4-dimaleimidobenzene, 1,4-bis(4-maleimidophenyl)benzene, 2-methyl-1,4-dimaleimidobenzene, 2,3-dimethyl-1,4-dimaleimidobenzene, 2,5-dimethyl-1,4-dimaleimidobenzene, 2,6-dimethyl-1,4-dimaleimidobenzene, 4-ethyl-1,3-dimaleimidobenzene, 5-ethyl-1,3-dimaleimidobenzene, 4,6-dimethyl-1,3-dimaleimidobenzene, 2,4,6-trimethyl-1,3-dimaleimidobenzene, 2,3,5,6-tetramethyl-1,4-dimaleimidobenzene, and 4-methyl-1,3-dimaleimidobenzene.
[0048] Specific examples of the aliphatic bismaleimide compound include bis(4-maleimidocyclohexyl)methane, bis(3-maleimidocyclohexyl)methane, etc. Among them, bis(4-maleimidophenyl)methane and 2,2-bis[4-(4-maleimidophenyloxy)phenyl]propane are preferred. Commercially available products include, for example, the BMI (trade name, Daiwa Chemical Industry Co., Ltd.) series.
[0049] When the polymaleimide compound (B) is taken as 100 parts by mass, the amount of the polyalkenylphenol compound (A) is preferably 5 to 200 parts by mass, more preferably 10 to 150 parts by mass, and even more preferably 30 to 100 parts by mass. If the amount is 5 parts by mass or more, the flowability during molding is better. On the other hand, if the amount is 200 parts by mass or less, the heat resistance of the cured product is better.
[0050] [Polyethylene glycol compound (C)] The polyethylene glycol compound (C) is a compound having a structural unit of formula (1), in which the structural unit of formula (1) accounts for 90 mol % to 100 mol % of all structural units. [ka] The structural unit of formula (1) is preferably from 95 mol % to 100 mol %, and more preferably from 97 mol % to 100 mol %.
[0051] Without being bound by any theory, the polyethylene glycol compound (C) has good miscibility with both the polyalkenylphenol compound (A) and the polymaleimide compound (B), and therefore adding the polyethylene glycol compound (C) can improve the compatibility of the polyalkenylphenol compound (A) and the polymaleimide compound (B). In addition, when a release agent is used, the polyethylene glycol compound (C) itself is moderately compatible and can control the surface separation property of the release agent. This effect can suppress the bleeding out of the release agent and other components. Furthermore, since the high molecular weight polyethylene glycol compound (C) is a stable component even at high temperatures, it can also adjust the flowability of the thermosetting resin composition and the surface wettability of the thermosetting resin composition to the mold during molding. Due to these effects, the addition of the high molecular weight polyethylene glycol compound (C) can further suppress bleeding out.
[0052] The number average molecular weight Mn of the polyethylene glycol compound (C) is preferably 2000 to 50000, more preferably 2500 to 30000, and further preferably 3000 to 25000. When the number average molecular weight Mn is 2000 or more, the bleeding out of the polyethylene glycol compound (C) onto the surface of the cured product after molding can be further suppressed. On the other hand, when the number average molecular weight Mn is 50000 or less, the viscosity of the thermosetting resin composition falls within a range suitable for molding.
[0053] The content of structural units other than the formula (1) in the polyethylene glycol compound (C) is 0 to 10 mol %, preferably 0 to 5 mol %, and more preferably 0 to 3 mol % based on the total structural units. Examples of structural units other than the formula (1) include structural units constituting a branched structure, structural units containing terminal functional groups such as optionally substituted amino groups, carboxy groups, sulfonic acid groups, hydroxy groups, glycidyl groups, azide groups, cyano groups, thiol groups, and unsaturated hydrocarbon groups, and structural units produced as by-products during compound synthesis.
[0054] The polyethylene glycol compound (C) may be polyethylene glycol or a polyethylene glycol derivative. Specific examples of the polyethylene glycol include PEG-4000 and PEG-6000 manufactured by Toho Chemical Industry Co., Ltd., and PEG-10000 and PEG-20000 manufactured by Sanyo Chemical Industries, Ltd. Examples of the polyethylene glycol derivative include polyethylene glycol fatty acid esters such as polyethylene glycol monooleate and polyethylene glycol-di-2-ethylhexoate.
[0055] The content of the polyethylene glycol compound (C) is preferably 1 to 10% by mass, more preferably 1.3 to 7% by mass, and even more preferably 1.5 to 5% by mass, based on the total of the polyalkenylphenol compound (A), the polymaleimide compound (B), and the polyethylene glycol compound (C). If the content of the polyethylene glycol compound (C) is 1% by mass or more, the wet adhesion to the metal surface can be further improved. On the other hand, if the content of the polyethylene glycol compound (C) is 10% by mass or less, the melting point or softening point of the thermosetting resin composition before molding can be appropriately adjusted to improve the handleability, and the bleeding out of the polyethylene glycol compound (C) after curing can be further suppressed.
[0056] [Radical initiator (D)] By blending a radical initiator (D) in the thermosetting resin composition, the curing of the thermosetting resin composition can be promoted. Examples of the radical initiator (D) include thermal radical initiators. The radical initiator (D) is preferably a thermal radical initiator. Examples of the thermal radical initiator include organic peroxides. The organic peroxide is preferably an organic peroxide having a 10-hour half-life temperature of 100 to 170°C, and specific examples thereof include dicumyl peroxide, 2,5-dimethyl-2,5-di(tert-butylperoxy)hexane, tert-butylcumyl peroxide, di-tert-butyl peroxide, 1,1,3,3-tetramethylbutyl hydroperoxide, and cumene hydroperoxide.
[0057] The amount of the radical initiator (D) used is preferably 0.01 to 10 parts by mass, more preferably 0.05 to 7.5 parts by mass, and even more preferably 0.1 to 5 parts by mass, based on 100 parts by mass in total of the polyalkenylphenol compound (A), the polymaleimide compound (B), and the polyethylene glycol compound (C). When the amount of the radical initiator (D) used is 0.01 part by mass or more, the curing reaction proceeds sufficiently, and when it is 10 parts by mass or less, the storage stability of the thermosetting resin composition is better.
[0058] [Filler (E)] The thermosetting resin composition may further include a filler (E). The type of the filler (E) is not particularly limited, and examples thereof include solid rubber particles such as solid silicone rubber particles, organic fillers such as silicone powder, and inorganic fillers such as silica, alumina, magnesium oxide, and boron nitride, and can be appropriately selected depending on the application. In one embodiment, the filler (E) is at least one selected from the group consisting of silica, alumina, magnesium oxide, and solid rubber particles.
[0059] For example, when the thermosetting resin composition is used for semiconductor sealing, it is preferable to mix an insulating inorganic filler in order to obtain a cured product with a low thermal expansion coefficient. The inorganic filler is not particularly limited, and known fillers can be used. Specific examples of the inorganic filler include particles of silica such as amorphous silica and crystalline silica, alumina, boron nitride, aluminum nitride, silicon nitride, and the like. From the viewpoint of reducing viscosity, spherical amorphous silica is desirable. The inorganic filler may be surface-treated with a silane coupling agent or the like, but may not be surface-treated.
[0060] The average particle size of the filler (E) is preferably 0.1 to 30 μm, and the maximum particle size is preferably 100 μm or less, particularly preferably 75 μm or less. When the average particle size is within this range, the viscosity of the thermosetting resin composition during use is appropriate, and the injectability into narrow-pitch wiring parts or narrow gap parts is also appropriate. The average particle size referred to here is the volume cumulative particle size D measured by a laser diffraction scattering type particle size distribution measuring device. 50 It is.
[0061] The content of the filler (E) in the thermosetting resin composition can be appropriately determined depending on the application. The content of the filler (E) in the thermosetting resin composition is preferably 200 to 1900 parts by mass, more preferably 300 to 1000 parts by mass, and even more preferably 300 to 600 parts by mass, relative to 100 parts by mass in total of the polyalkenylphenol compound (A), the polymaleimide compound (B), the polyethylene glycol compound (C), and the radical initiator (D).
[0062] [Other additives] Other additives that may be added to the thermosetting resin composition include coupling agents, defoamers, colorants, phosphors, modifiers, leveling agents, light diffusing agents, flame retardants, adhesion promoters, release agents, etc. The other additives do not include compounds that fall under the category of polyalkenylphenol compounds (A), polymaleimide compounds (B), polyethylene glycol compounds (C), radical initiators (D), and fillers (E).
[0063] For example, a coupling agent may be blended from the viewpoint of improving adhesiveness. The coupling agent is not particularly limited, and examples thereof include silane coupling agents such as vinyltriethoxysilane, vinyltrimethoxysilane, 3-glycidoxypropyltrimethoxysilane, γ-methacryloxypropyltrimethoxysilane, γ-aminopropyltrimethoxysilane, and N-phenyl-3-aminopropyltrimethoxysilane. The coupling agent may be used alone or in combination of two or more. The blending amount of the coupling agent in the thermosetting resin composition is preferably 0.1 to 5% by mass. If the blending amount is 0.1% by mass or more, the effect of the coupling agent is fully exerted, and if it is 5% by mass or less, the melt viscosity, the moisture absorption property and the strength of the cured product are better.
[0064] For example, from the viewpoint of improving releasability, a release agent may be blended. The release agent is not particularly limited, and examples thereof include carnauba wax, amide wax, Montan acid ester wax, Montan acid partially saponified ester wax, metal soap such as calcium stearate, polyethylene wax, polypropylene wax, etc. Among them, carnauba wax, Montan acid ester wax, and polyethylene wax are preferable. The release agent may be used alone or in combination of two or more. The blending amount of the release agent in the thermosetting resin composition is preferably 0.01 to 0.5% by mass. If the blending amount is 0.01% by mass or more, the effect of the release agent is fully exerted, and if it is 0.5% by mass or less, bleeding out such as mold staining does not occur and the appearance is good.
[0065] [Method for preparing thermosetting resin composition] The method for preparing the thermosetting resin composition is not particularly limited as long as the polyalkenylphenol compound (A), the polymaleimide compound (B), the polyethylene glycol compound (C), the radical initiator (D), and other optional components can be uniformly mixed and dispersed. A method in which the polyalkenylphenol compound (A), the polymaleimide compound (B), and the polyethylene glycol compound (C) are first melt-mixed, and then the radical initiator (D) and optional additives are added is preferred because each material can be easily mixed uniformly.
[0066] The method of mixing each component is not particularly limited. Each component can be mixed at a predetermined mixing ratio by adding it to a mixer such as a reaction vessel, a pot mill, a two-roll mill, a three-roll mill, a rotary mixer, a twin-screw mixer, a disperser, a single-screw or twin-screw (same-direction or different-direction) extruder, or a kneader, and stirring or kneading it. In a laboratory scale, a rotary mixer is preferred because the stirring conditions can be easily changed, and industrially, a twin-screw mixer is preferred from the viewpoint of productivity. Each mixer can be used by appropriately changing the stirring conditions.
[0067] When powdering a thermosetting resin composition, any method can be used as long as the resin does not melt due to heat generated during the work process, but if the amount is small, a method using an agate mortar is convenient. When using a commercially available grinder, one that generates less heat during grinding is preferred in order to suppress melting of the mixture. The particle size of the powder is preferably 1 mm or less.
[0068] [How to fabricate the structure] The thermosetting resin composition can be melted by heating to a temperature at which the curing reaction does not proceed rapidly. The molten thermosetting resin composition can be molded into any desired shape, cured as necessary, and demolded to produce a structure. As a method for producing the structure, molding, particularly transfer molding and compression molding, are preferred.
[0069] For example, the preferred conditions for transfer molding are a top plate and mold temperature of 170 to 190°C and a holding pressure of 50 to 150 kg / cm for a mold size of 10 mm x 75 mm x 3 mm. 2 As preferable conditions for compression molding, for example, in the case of a mold having a size of 100 mm×75 mm×3 mm thickness, the temperatures of the top plate and mold can be 170 to 190° C., the molding pressure can be 5 to 20 MPa, and the pressure time can be 1.5 to 10 minutes.
[0070] [How to prepare the cured product] The thermosetting resin composition can be cured by heating. The curing temperature is preferably 130 to 300°C, more preferably 150 to 230°C, and further preferably 150 to 200°C. If the curing temperature is 130°C or higher, the thermosetting resin composition before curing can be sufficiently melted and easily filled into a mold, and it is also easy to demold after curing. If the curing temperature is 300°C or lower, thermal deterioration or volatilization of the material can be avoided.
[0071] The heating time can be appropriately changed depending on the thermosetting resin composition and the curing temperature, but is preferably 0.1 to 24 hours from the viewpoint of productivity. This heating may be performed in several steps. When a particularly high degree of curing is required, it is preferable not to cure at an excessively high temperature, but to raise the temperature as the curing progresses, and the final curing temperature is preferably 250°C or less, more preferably 230°C or less.
[0072] [Uses of the cured product] The cured product of the thermosetting resin composition can be used for applications such as semiconductor encapsulation materials, prepregs, interlayer insulating resins, solder resists, and die attach. EXAMPLES
[0073] The present invention will be specifically described below based on examples and comparative examples, but the present invention is not limited to these examples.
[0074] The analytical methods, property evaluation methods, and raw materials used in the examples and comparative examples are as follows.
[0075] <Analysis and Characterization Methods> [Molecular weight] The measurement conditions for GPC are as follows. Equipment name: JASCO LC-2000 plus (JASCO Corporation) Column: Shodex (registered trademark) LF-804 (Showa Denko K.K.) Mobile phase: Tetrahydrofuran Flow rate: 1.0mL / min Detector: JASCO RI-2031 plus (JASCO Corporation) Temperature: 40℃ The number average molecular weight Mn and the weight average molecular weight Mw were calculated using a calibration curve prepared using a polystyrene standard substance under the above measurement conditions.
[0076] [Degree of polymerization] The degree of polymerization P was calculated by the following formula, where Mn is the number average molecular weight calculated by GPC and M is the molecular weight of the repeating unit of the compound. P=Mn / M
[0077] [Glass transition temperature] The heat resistance of the cured product was evaluated in terms of the glass transition temperature (Tg). Specifically, a transfer molding machine was used, and the mold temperature was 180°C and the holding pressure was 100 kg / cm. 2 The thermosetting resin composition was molded under the conditions of 100°C, 100°F, and 3 minutes of holding time to prepare a 5mm×5mm×5mm test piece for measuring the glass transition temperature. The test piece was heated at 200°C for 5 hours to post-cure, and then measured by thermomechanical measurement (TMA). The measurement was performed using a TMA / SS6100 thermomechanical analyzer manufactured by SII Nano Technology Inc. under the conditions of a temperature range of 30 to 300°C, a heating rate of 5°C / min, and a load of 20.0 mN, and the inflection point of the linear expansion coefficient was taken as Tg.
[0078] [Mold releasability] The moldability was evaluated from the viewpoint of releasability from a mold. Specifically, a transfer molding machine equipped with a mold 1 (test piece size: lower diameter: 25 mmφ, upper diameter: 10 mmφ, upper thickness: 7 mm, lower thickness: 7 mm, taper: 2°) and a top plate 2 and a bottom plate 3 shown in Fig. 1 was used, and the mold temperature was 180°C and the holding pressure was 100 kg / cm. 2 The thermosetting resin composition was molded under the conditions of a holding time of 3 minutes, and the demolding force was measured when the composition was pressed from above using a spring scale, as shown in Figure 2. Molding was performed multiple times in succession, and the number of consecutive moldings at which the average value of the demolding force on the left and right sides remained below 40 N was recorded. The evaluation was terminated when the average value exceeded 40 N or when the number of moldings reached 10.
[0079] Appearance (Bleed Out) The moldability was also evaluated from the viewpoint of appearance. Specifically, a transfer molding machine was used, and the mold temperature was 180°C and the holding pressure was 100 kg / cm. 2 The thermosetting resin composition was molded under the conditions of 100°C, 100°F, 100°C, 100°F, 100°C, 150°F, 100°C, 150°F, 100°F, 15 ...
[0080] [Adhesion rate after molding] The material used was rolled oxygen-free copper (C1020), with external dimensions of 52 mm wide, 38 mm long, and 0.5 mm thick, and a lead frame with a bed of 18 mm length and width in the center was used. The bed was enclosed by an external dimension of 30 mm long, 30 mm wide, and 3 mm thick, centered on the center of the lead frame. Sealing was performed at a mold temperature of 180°C and a holding pressure of 100 kg / cm. 2 The thermosetting resin composition was molded using a transfer molding machine under conditions of 100°C, 100°C, and 3 minutes of holding time, and the obtained test piece was post-cured at 200°C for 5 hours. The post-cured test piece was observed for peeling at the interface between the lead frame and the cured thermosetting resin composition using an ultrasonic flaw detection imaging device (Honda Electronics Co., Ltd., HA-60A). Using Image-J software, the area of the non-peeled part was divided by the total area to determine the post-molding adhesion rate.
[0081] [Reflow resistance] Reflow resistance was evaluated by the post-reflow adhesion rate. A reflow test was performed on post-cured test pieces obtained in the same manner as in the post-molding adhesion rate test, using a reflow simulator SRS-1 manufactured by Malcom Co., Ltd., in accordance with the conditions of level 3 of IPC / JEDEC J-STD-020D. The test pieces after the reflow test were analyzed in the same manner as in the post-molding adhesion rate test, and the obtained value was determined as the post-reflow adhesion rate.
[0082] <Ingredients> [Polyalkenylphenol compound (A)] BRG-APO (R in formula (2)-1) 1 = hydrogen atom, Q=-CR 8 R 9 -, R 8 and R 9 = hydrogen atom, R in formula (3) 3 ~R 7 = hydrogen atom) A 1:1 mixture of phenolic novolak resins Shounol (registered trademark) BRG-556 and BRG-558 (Aica Kogyo Co., Ltd.) was used to produce a resin (hydroxyl equivalent 154, number average molecular weight Mn 1000, weight average molecular weight Mw 3000, polymerization degree 6.6, p = 6.6, q = 0, p / (p + q) = 1) in which the ortho- or para-position of the phenolic hydroxyl group was allylated. For the production method, see Example 1 of JP 2016-28129 A.
[0083] HE100C-APO (R of formula (2)-1 and formula (2-2) 1 = hydrogen atom, Q = p-xylylene group, R in formula (3) 3 ~R 7 = hydrogen atom) A resin (hydroxyl equivalent 222, number average molecular weight Mn 900, weight average molecular weight Mw 1900, degree of polymerization 4.0, p = 3.8, q = 0.2, p / (p+q) = 0.95) was produced in which the ortho- or para-position of the phenolic hydroxyl group was allylated using phenol aralkyl resin HE100C-10-15 (Air Water Inc.) in a manner similar to Example 1 of JP2016-28129A.
[0084] [Polymaleimide compound (B)] BMI-4000 (2,2-bis[4-(4-maleimidophenyloxy)phenyl]propane, Daiwa Chemical Industry Co., Ltd.) BMI-1100H (Bis(4-maleimidophenyl)methane, Daiwa Chemical Industry Co., Ltd.)
[0085] [Polyethylene glycol compound (C)] PEG-4000 (polyethylene glycol, Mn 4000, Mw 5000, 100 mol% of the structural unit of formula (1), Toho Chemical Industry Co., Ltd.) PEG-6000 (polyethylene glycol, Mn 6000, Mw 7300, 100 mol% of the structural unit of formula (1), Toho Chemical Industry Co., Ltd.) PEG-10000 (polyethylene glycol, Mn 10000, Mw 14000, 100 mol% of the structural unit of formula (1), Sanyo Chemical Industries, Ltd.) PEG-20000 (polyethylene glycol, Mn 21000, Mw 26000, 100 mol% of the structural unit of formula (1), Sanyo Chemical Industries, Ltd.) Lionon MO-60 (polyethylene glycol monooleate, Mn 7200, Mw 8000, 94 mol% of the structural unit of formula (1), Lion Specialty Chemicals Co., Ltd.)
[0086] [Radical initiator (D)] Percumyl (registered trademark) D (Dicumyl peroxide, NOF Corporation)
[0087] [Filler (E)] Silica filler MSR5100 (spherical silica, average particle size 22.7 μm, Tatsumori Co., Ltd.) was treated with 0.5 mass% of silane coupling agent KBE-403 (Shin-Etsu Chemical Co., Ltd.).
[0088] [Release agent] Carnauba No. 1 (Carnauba wax, Nikko Rica Corporation) LICOWAX® PE520 (Polyethylene wax, Clariant Chemicals)
[0089] As other resins, the following compounds were used. KF6004 (silicone PEG, Mn 3000, Mw 4500, 50 mol% of structural unit of formula (1), Shin-Etsu Chemical Co., Ltd.) EPPN-501H (triphenylmethane type epoxy resin, Nippon Kayaku Co., Ltd.) CRG-951 (phenol novolac resin, Aica Kogyo Co., Ltd.) ·TPP (triphenylphosphine)
[0090] <Example 1> [Production of Thermosetting Resin Composition] 35 parts by mass of BRG-APO as polyalkenylphenol compound (A), 65 parts by mass of BMI-4000 as polymaleimide compound (B), 2 parts by mass of PEG-6000 as polyethylene glycol compound (C), 1.5 parts by mass of Percumyl D as radical initiator (D), 400 parts by mass of MSR5100 as filler (E), 0.4 parts by mass of carnauba wax as mold release agent and 0.15 parts by mass of PE520 were mixed and melt-kneaded (110 ° C, 10 minutes with two rolls (roll diameter 8 inches) manufactured by Toyo Seiki Seisakusho Co., Ltd.). After cooling at room temperature (25 ° C) for 1 hour to solidify, it was pulverized using a mill mixer (Osaka Chemical Co., Ltd., model WB-1, 25 ° C, 30 seconds) to obtain a powdered thermosetting resin composition.
[0091] [Analysis and Characterization] The above-mentioned analyses were carried out on the obtained thermosetting resin composition, and the composition was compressed into tablets using a tableting machine (Fuji Yakuhin Kikai Co., Ltd.) and then transfer molded to prepare test pieces to be used in the above-mentioned property evaluation, and the properties were evaluated.
[0092] <Examples 2 to 8 and Comparative Examples 1 to 3> Except for changing the types and amounts of raw materials as shown in Table 1, thermosetting resin compositions were produced in the same manner as in Example 1, and analysis and characteristic evaluation were carried out.
[0093] [Table 1]
[0094] Examples 1 to 8 were good in terms of releasability, adhesion rate after molding, adhesion rate after reflow, and appearance. In addition, Examples 1 to 8 were excellent in terms of heat resistance of the cured products. On the other hand, Comparative Examples 1 and 2, which did not contain the polyethylene glycol compound (C), were poor in releasability and appearance, and had a significantly low adhesion rate after reflow. Comparative Example 3, which was based on an epoxy resin, was poor in releasability and appearance, and also had a low adhesion rate after reflow resistance. [Explanation of symbols]
[0095] 1. Mold 2. Tabletop 3 Bottom plate 4 Gate 5 Runner 6 Molded objects
Claims
1. A thermosetting resin composition comprising a polyalkenylphenol compound (A), a polymaleimide compound (B), a polyethylene glycol compound (C), and a radical initiator (D), The polyalkenylphenol compound (A) is a compound having at least two phenol skeletons in the molecule, and having 2-alkenyl groups bonded to some or all of the aromatic rings forming the phenol skeletons in the molecule, The polyethylene glycol compound (C) has a structural unit represented by formula (1), and the structural unit represented by formula (1) accounts for 90 mol % to 100 mol % of all structural units. Thermosetting resin composition. 【Chemistry 1】
2. The content of the polyethylene glycol compound (C) is 1 to 10 mass% based on the total content of the polyalkenylphenol compound (A), the polymaleimide compound (B), and the polyethylene glycol compound (C). The thermosetting resin composition according to claim 1.
3. The thermosetting resin composition according to claim 1 or 2, wherein the polyethylene glycol compound (C) has a number average molecular weight Mn of 2,000 to 50,000.
4. The content of the polyalkenylphenol compound (A) is 5 to 200 parts by mass per 100 parts by mass of the polymaleimide compound (B), The thermosetting resin composition according to any one of claims 1 to 3.
5. The thermosetting resin composition according to any one of claims 1 to 4, wherein the polyethylene glycol compound (C) is polyethylene glycol.
6. The polyalkenylphenol compound (A) is represented by the formula (2)-1: 【Chemistry 2】 and optionally formula (2)-2: 【Chemistry 3】 A polyalkenylphenol compound having a structural unit represented by the formula: In formula (2)-1 and formula (2)-2, R 1 each independently represents a hydrogen atom, an alkyl group having 1 to 5 carbon atoms, or an alkoxy group having 1 to 5 carbon atoms; R 2 each independently represents the formula (3): 【Chemistry 4】 In the formula (3), R 3 , R 4 , R 5 , R 6 , and R 7 are each independently a hydrogen atom, an alkyl group having 1 to 5 carbon atoms, a cycloalkyl group having 5 to 10 carbon atoms, or an aryl group having 6 to 12 carbon atoms, * in formula (3) represents a bond to a carbon atom constituting an aromatic ring, R 1 and R 2 may be the same or different in each phenol skeleton unit, and each Q independently represents a group represented by the formula -CR 8 R 9 -, a cycloalkylene group having 5 to 10 carbon atoms, a divalent organic group having an aromatic ring, a divalent organic group having an alicyclic condensed ring, or a divalent organic group consisting of these, 8 and R 9 each independently represents a hydrogen atom, an alkyl group having 1 to 5 carbon atoms, an alkenyl group having 2 to 6 carbon atoms, a cycloalkyl group having 5 to 10 carbon atoms, or an aryl group having 6 to 12 carbon atoms. The thermosetting resin composition according to any one of claims 1 to 5.
7. The thermosetting resin composition according to claim 6, wherein p is a real number of 1.1 to 35, p+q is a real number of 1.1 to 35, and q is a real number such that the value of the formula: p / (p+q) is 0.4 to 1, where p is an average number of the structural units represented by formula (2)-1 per molecule, and q is an average number of the structural units represented by formula (2-2) per molecule.
8. The thermosetting resin composition according to any one of claims 1 to 7, wherein the polymaleimide compound (B) is an aromatic bismaleimide compound.
9. The thermosetting resin composition according to any one of claims 1 to 8, wherein the radical initiator (D) is an organic peroxide.
10. The thermosetting resin composition according to any one of claims 1 to 9, further comprising a filler (E).
11. The thermosetting resin composition according to claim 10, wherein the filler (E) is at least one selected from the group consisting of silica, alumina, magnesium oxide, and solid rubber particles.
12. The content of the filler (E) is 200 to 1900 parts by mass per 100 parts by mass of the total of the polyalkenylphenol compound (A), the polymaleimide compound (B), the polyethylene glycol compound (C), and the radical initiator (D). The thermosetting resin composition according to claim 10 or 11.
13. A cured product of the thermosetting resin composition according to any one of claims 1 to 12.
14. A method for producing a structure, comprising molding the thermosetting resin composition according to any one of claims 1 to 12.
15. A structure comprising the cured product according to claim 13.
Citation Information
Patent Citations
Semiconductor device
JP1993006869A
Aromatic bismaleimide resin composition
JP1993043630A
Curable resin composition
JP1994093047A
Epoxy resin composition and semiconductor device produced by using the composition
JP1999140277A
Thermosetting resin composition
JP2018095690A