Resin composition
Patent Information
- Application Number
- JP2023021405
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2023-02-15
- Publication Date
- 2024-12-03
- Estimated Expiration
- 2036-12-02
Smart Images

Figure 0007593426000006 
Figure 0007593426000001 
Figure 0007593426000002
Abstract
Description
[Technical field]
[0001] The present invention relates to a resin composition. The present invention further relates to a sheet-like substrate, an adhesive film, a printed wiring board, and a semiconductor device each containing the resin composition. [Background technology]
[0002] A known manufacturing technique for printed wiring boards is a build-up method in which insulating layers and conductor layers are alternately stacked on an inner layer circuit board. Insulating layers are generally formed by curing a resin composition. For example, Patent Document 1 describes a resin composition that is characterized by containing (A) a radical polymerizable compound, (B) an epoxy resin, (C) a curing agent, and (D) a roughening component. [Prior art documents] [Patent documents]
[0003] [Patent Document 1] JP 2014-034580 A Summary of the Invention [Problem to be solved by the invention]
[0004] Many epoxy resin compositions suitable for forming insulating layers of inner layer circuit boards have been proposed, including the resin composition described in Patent Document 1. However, in recent years, there has been an increasing demand for resin compositions capable of forming insulating layers with excellent low dielectric tangent. In addition, as electronic devices become smaller and more powerful, build-up layers are being multiplied in multilayer printed wiring boards, and finer and denser wiring is being required.
[0005] In order to achieve finer and denser wiring, there is a demand for resin compositions with good compatibility that provide insulating layers with a low dielectric tangent, good plating adhesion and undercoat adhesion, and excellent smear removal properties; however, at present, all of these requirements have not yet been satisfied.
[0006] The object of the present invention is to provide a resin composition having good compatibility which provides an insulating layer having a low dielectric tangent, good plating adhesion and base adhesion, and excellent smear removability; a sheet-like substrate containing the resin composition; an adhesive film containing the resin composition; and a printed wiring board and a semiconductor device having an insulating layer formed using the resin composition. [Means for solving the problem]
[0007] The present inventors have found that in conventional general resin compositions, the lower the dielectric tangent, the poorer the smear removability, i.e., there is a trade-off between the dielectric tangent and the smear removability. As a result of intensive research aimed at solving the above problem, the present inventors have found that by incorporating (A) an epoxy resin, (B) a curing agent, and a predetermined amount of (C) a compound having a cyclic ether structure with five or more members in a resin composition, an insulating layer having a low dielectric tangent, good plating adhesion and base adhesion, and excellent smear removability can be obtained, and have completed the present invention.
[0008] That is, the present invention includes the following. [1] A resin composition comprising (A) an epoxy resin, (B) a curing agent, and (C) a compound having a cyclic ether structure having five or more members, A resin composition, in which the content of the component (C) is 1% by mass to 50% by mass, relative to 100% by mass of the resin component. [2] The resin composition according to [1], wherein the content of the component (A) is 5% by mass to 50% by mass, relative to 100% by mass of the resin component. [3] The resin composition according to [1] or [2], wherein the content of the component (B) is 5% by mass to 60% by mass, relative to 100% by mass of the resin component. [4] The resin composition according to any one of [1] to [3], wherein the component (B) is an active ester curing agent. [5] The resin composition according to any one of [1] to [4], further comprising (D) an inorganic filler. [6] The resin composition according to [5], wherein the content of component (D) is 50% by mass or more, based on 100% by mass of the non-volatile components of the resin composition. [7] The resin composition according to any one of [1] to [6], wherein the component (C) contains a dioxane structure. [8] The resin composition according to any one of [1] to [7], wherein the component (C) has a carbon-carbon unsaturated bond. [9] The resin composition according to any one of [1] to [8], wherein the component (C) has a carbon-carbon double bond.
[10] The resin composition according to any one of [1] to [9], wherein the component (C) has one or more functional groups selected from the group consisting of a vinyl group, a methacrylic group, an acrylic group, an allyl group, a styryl group, and a propenyl group.
[11] The resin composition according to any one of [1] to
[10] , wherein the component (C) has a vinyl group.
[12] The resin composition according to any one of [1] to
[11] , wherein the component (C) is the following compound: [ka]
[13] The resin composition according to any one of [1] to
[12] , which is for forming an insulating layer of a printed wiring board.
[14] The resin composition according to any one of [1] to
[12] , which is for forming an interlayer insulating layer of a printed wiring board.
[15] A sheet-like substrate comprising the resin composition according to any one of [1] to
[14] .
[16] An adhesive film comprising a support and a resin composition layer formed on the support from the resin composition according to any one of [1] to
[14] .
[17] A printed wiring board including a first conductor layer, a second conductor layer, and an insulating layer formed between the first conductor layer and the second conductor layer, The insulating layer of the printed wiring board is a cured product of the resin composition according to any one of [1] to
[14] .
[18] A semiconductor device comprising the printed wiring board according to
[17] . Effect of the Invention
[0009] According to the present invention, it is possible to provide a resin composition having good compatibility which provides an insulating layer having a low dielectric tangent, good plating adhesion and base adhesion, and excellent smear removal properties; a sheet-like substrate containing the resin composition; an adhesive film containing the resin composition; and a printed wiring board and a semiconductor device having an insulating layer formed using the resin composition. [Brief description of the drawings]
[0010] [Figure 1] FIG. 1 is a partial cross-sectional view that illustrates an example of a printed wiring board. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0011] The resin composition, sheet-like substrate, adhesive film, printed wiring board, and semiconductor device of the present invention will be described in detail below.
[0012] [Resin composition] The resin composition of the present invention is a resin composition containing (A) an epoxy resin, (B) a curing agent, and (C) a compound having a cyclic ether structure with 5 or more members, and the content of the component (C) is 1% by mass to 50% by mass when the resin component is taken as 100% by mass. This makes it possible to provide a resin composition with good compatibility that provides an insulating layer with a low dielectric tangent, good plating adhesion and base adhesion, and excellent smear removal properties.
[0013] The term "resin component" refers to the non-volatile components constituting the resin composition, excluding the inorganic filler (D) described below. Each component contained in the resin composition will be described in detail below.
[0014] <(A) Epoxy resin> The resin composition contains an epoxy resin (A). Examples of the epoxy resin (A) include fluorine-containing epoxy resins such as bisphenol AF type epoxy resins and perfluoroalkyl type epoxy resins; bisphenol A type epoxy resins; bisphenol F type epoxy resins; bisphenol S type epoxy resins; bixylenol type epoxy resins; dicyclopentadiene type epoxy resins; trisphenol type epoxy resins; naphthol novolac type epoxy resins; phenol novolac type epoxy resins; tert-butyl-catechol type epoxy resins; naphthalene type epoxy resins; naphthol type epoxy resins; anthracene type epoxy resins; glycidylamine type epoxy resins; glycidyl ester type epoxy resins; cresol novolac type epoxy resins; biphenyl type epoxy resins; linear aliphatic epoxy resins; epoxy resins having a butadiene structure; alicyclic epoxy resins; heterocyclic epoxy resins; spiro ring-containing epoxy resins; cyclohexane dimethanol type epoxy resins; naphthylene ether type epoxy resins; trimethylol type epoxy resins; tetraphenylethane type epoxy resins, etc. The epoxy resins may be used alone or in combination of two or more.
[0015] The epoxy resin preferably contains an epoxy resin having two or more epoxy groups in one molecule. When the non-volatile components of the epoxy resin are taken as 100 mass%, it is preferable that at least 50 mass% of the epoxy resin is an epoxy resin having two or more epoxy groups in one molecule. The epoxy resin is preferably an epoxy resin having two or more epoxy groups in one molecule and being liquid at a temperature of 20°C (hereinafter referred to as "liquid epoxy resin"), and / or an epoxy resin having three or more epoxy groups in one molecule and being solid at a temperature of 20°C (hereinafter referred to as "solid epoxy resin"). As the epoxy resin, a liquid epoxy resin and a solid epoxy resin may be used in combination.
[0016] As the liquid epoxy resin, bisphenol A type epoxy resin, bisphenol F type epoxy resin, bisphenol AF type epoxy resin, naphthalene type epoxy resin, glycidyl ester type epoxy resin, glycidyl amine type epoxy resin, phenol novolac type epoxy resin, alicyclic epoxy resin having an ester skeleton, cyclohexane dimethanol type epoxy resin, glycidyl amine type epoxy resin, and epoxy resin having a butadiene structure are preferred, and glycidyl amine type epoxy resin, bisphenol A type epoxy resin, bisphenol F type epoxy resin, bisphenol AF type epoxy resin, and naphthalene type epoxy resin are more preferred. Specific examples of liquid epoxy resins include DIC's "HP4032", "HP4032D", and "HP4032SS" (naphthalene type epoxy resins), Mitsubishi Chemical's "828US", "jER828EL" (bisphenol A type epoxy resin), "jER807" (bisphenol F type epoxy resin), "jER152" (phenol novolac type epoxy resin), "630", and "630LSD" (glycidylamine type epoxy resin), Nippon Steel & Sumitomo Metal Chemical's "ZX1059" (a mixture of bisphenol A type epoxy resin and bisphenol F type epoxy resin), and Nippon Steel & Sumitomo Metal Chemical's "YD-8 Examples of the epoxy resins include "125G" (bisphenol A type epoxy resin), "EX-721" (glycidyl ester type epoxy resin) manufactured by Nagase ChemteX Corporation, "Celloxide 2021P" (alicyclic epoxy resin having an ester skeleton) manufactured by Daicel Corporation, "PB-3600" (epoxy resin having a butadiene structure), "ZX1658" and "ZX1658GS" (liquid 1,4-glycidylcyclohexane) manufactured by Nippon Steel Chemical Co., Ltd., "630LSD" (glycidylamine type epoxy resin) manufactured by Mitsubishi Chemical Corporation, and "E-7432" and "E-7632" (perfluoroalkyl type epoxy resin) manufactured by Daikin Industries, Ltd. These may be used alone or in combination of two or more types.
[0017] As the solid epoxy resin, naphthalene-type tetrafunctional epoxy resin, cresol novolac-type epoxy resin, dicyclopentadiene-type epoxy resin, trisphenol-type epoxy resin, naphthol-type epoxy resin, biphenyl-type epoxy resin, naphthylene ether-type epoxy resin, anthracene-type epoxy resin, bisphenol A-type epoxy resin, and tetraphenylethane-type epoxy resin are preferred, and naphthalene-type tetrafunctional epoxy resin, naphthol-type epoxy resin, and biphenyl-type epoxy resin are more preferred. Specific examples of solid epoxy resins include "HP4032H" (naphthalene type epoxy resin), "HP-4700", "HP-4710" (naphthalene type tetrafunctional epoxy resin), "N-690" (cresol novolac type epoxy resin), "N-695" (cresol novolac type epoxy resin), "HP-7200", "HP-7200HH", "HP-7200H" (dicyclopentadiene type epoxy resin), "EXA-7311", "EXA-7311-G3", "EXA-7311-G4", "EXA-7311-G4S", "HP6000" (naphthylene ether type epoxy resin), and "EPPN-502H" (trisphenol type epoxy resin), "NC7000L" (naphthol novolac type epoxy resin), "NC3000H", "NC3 Examples of epoxy resins include "000", "NC3000L", and "NC3100" (biphenyl type epoxy resins), "ESN475V" (naphthalene type epoxy resin) and "ESN485" (naphthol novolac type epoxy resin) manufactured by Nippon Steel & Sumitomo Metal Chemical Co., Ltd., "YX4000H", "YL6121" (biphenyl type epoxy resin), "YX4000HK" (bixylenol type epoxy resin), and "YX8800" (anthracene type epoxy resin) manufactured by Mitsubishi Chemical Co., Ltd., "PG-100" and "CG-500" manufactured by Osaka Gas Chemical Co., Ltd., "YL7800" (fluorene type epoxy resin) manufactured by Mitsubishi Chemical Co., Ltd., "jER1010" (solid bisphenol A type epoxy resin), "jER1031S" (tetraphenylethane type epoxy resin), and "YL7760" (bisphenol AF type epoxy resin) manufactured by Mitsubishi Chemical Co., Ltd.
[0018] When a liquid epoxy resin and a solid epoxy resin are used in combination as the epoxy resin, the mass ratio thereof (liquid epoxy resin:solid epoxy resin) is preferably in the range of 1:0.1 to 1:15, more preferably 1:0.1 to 1:10, and even more preferably 1:0.3 to 1:3.
[0019] From the viewpoint of obtaining an insulating layer exhibiting good tensile breaking strength and insulating reliability, the content of the epoxy resin in the resin composition is preferably 5% by mass or more, more preferably 10% by mass or more, and even more preferably 20% by mass or more, when the resin component is taken as 100% by mass. The upper limit of the content of the epoxy resin is not particularly limited as long as the effects of the present invention are exhibited, but is preferably 50% by mass or less, more preferably 40% by mass or less.
[0020] The epoxy equivalent of the epoxy resin is preferably 50 to 5000, more preferably 50 to 3000, even more preferably 80 to 2000, and even more preferably 110 to 1000. Within this range, the crosslink density of the cured product of the resin composition layer is sufficient, and an insulating layer with small surface roughness can be obtained. The epoxy equivalent can be measured according to JIS K7236, and is the mass of a resin containing one equivalent of an epoxy group.
[0021] The weight average molecular weight of the epoxy resin is preferably 100 to 5000, more preferably 250 to 3000, and further preferably 400 to 1500. Here, the weight average molecular weight of the epoxy resin is a polystyrene-equivalent weight average molecular weight measured by gel permeation chromatography (GPC).
[0022] <(B) Hardener> The resin composition contains a curing agent (B). The curing agent is not particularly limited as long as it has the function of curing the epoxy resin (A), and examples thereof include phenol-based curing agents, naphthol-based curing agents, active ester-based curing agents, benzoxazine-based curing agents, cyanate ester-based curing agents, and carbodiimide-based curing agents. The curing agents may be used alone or in combination of two or more. The component (B) is preferably one or more selected from phenol-based curing agents, naphthol-based curing agents, active ester-based curing agents, carbodiimide-based curing agents, and cyanate ester-based curing agents, and is preferably an active ester-based curing agent from the viewpoint of lowering the dielectric loss tangent.
[0023] As the phenol-based curing agent and naphthol-based curing agent, from the viewpoint of heat resistance and water resistance, a phenol-based curing agent having a novolac structure or a naphthol-based curing agent having a novolac structure is preferable. Also, from the viewpoint of adhesion to the conductor layer, a nitrogen-containing phenol-based curing agent is preferable, and a triazine skeleton-containing phenol-based curing agent is more preferable.
[0024] Specific examples of phenol-based curing agents and naphthol-based curing agents include, for example, "MEH-7700", "MEH-7810", and "MEH-7851" manufactured by Meiwa Kasei Co., Ltd., "NHN", "CBN", and "GPH" manufactured by Nippon Kayaku Co., Ltd., "SN170", "SN180", "SN190", "SN475", "SN485", "SN495", "SN-495V", "SN375", and "SN395" manufactured by Nippon Steel & Sumitomo Metal Corporation, and "TD-2090", "LA-7052", "LA-7054", "LA-1356", "LA-3018-50P", and "EXB-9500" manufactured by DIC Corporation.
[0025] The active ester curing agent is not particularly limited, but generally, compounds having two or more highly reactive ester groups in one molecule, such as phenol esters, thiophenol esters, N-hydroxyamine esters, and esters of heterocyclic hydroxy compounds, are preferably used. The active ester curing agent is preferably one obtained by a condensation reaction between a carboxylic acid compound and / or a thiocarboxylic acid compound and a hydroxy compound and / or a thiol compound. In particular, from the viewpoint of improving heat resistance, an active ester curing agent obtained from a carboxylic acid compound and a hydroxy compound is preferred, and an active ester curing agent obtained from a carboxylic acid compound and a phenol compound and / or a naphthol compound is more preferred. Examples of the carboxylic acid compound include benzoic acid, acetic acid, succinic acid, maleic acid, itaconic acid, phthalic acid, isophthalic acid, terephthalic acid, and pyromellitic acid. Examples of phenol compounds or naphthol compounds include hydroquinone, resorcin, bisphenol A, bisphenol F, bisphenol S, phenolphthaline, methylated bisphenol A, methylated bisphenol F, methylated bisphenol S, phenol, o-cresol, m-cresol, p-cresol, catechol, α-naphthol, β-naphthol, 1,5-dihydroxynaphthalene, 1,6-dihydroxynaphthalene, 2,6-dihydroxynaphthalene, dihydroxybenzophenone, trihydroxybenzophenone, tetrahydroxybenzophenone, phloroglucin, benzenetriol, dicyclopentadiene-type diphenol compounds, phenol novolac, etc. Here, the term "dicyclopentadiene-type diphenol compounds" refers to diphenol compounds obtained by condensing one molecule of dicyclopentadiene with two molecules of phenol.
[0026] Specifically, active ester compounds containing a dicyclopentadiene-type diphenol structure, active ester compounds containing a naphthalene structure, active ester compounds containing an acetylated product of phenol novolac, and active ester compounds containing a benzoylated product of phenol novolac are preferred, and among these, active ester compounds containing a naphthalene structure and active ester compounds containing a dicyclopentadiene-type diphenol structure are more preferred. The "dicyclopentadiene-type diphenol structure" refers to a divalent structural unit consisting of phenylene-dicyclopentylene-phenylene.
[0027] Commercially available active ester curing agents include "EXB9451", "EXB9460", "EXB9460S", "HPC-8000-65T", "HPC-8000H-65TM", and "EXB-8000L-65TM" (manufactured by DIC Corporation) as active ester compounds containing a dicyclopentadiene-type diphenol structure, "EXB9416-70BK" (manufactured by DIC Corporation) as an active ester compound containing a naphthalene structure, and "EXB9416-70BK" (manufactured by DIC Corporation) as an active ester compound containing an acetylated product of phenol novolac. Examples of active ester-based hardeners that are benzoyl derivatives of phenol novolac include "DC808" (manufactured by Mitsubishi Chemical Corporation) as an active ester compound containing a benzoyl derivative of phenol novolac, "YLH1026" (manufactured by Mitsubishi Chemical Corporation) as an active ester-based hardener that is an acetylated derivative of phenol novolac, and "YLH1026" (manufactured by Mitsubishi Chemical Corporation), "YLH1030" (manufactured by Mitsubishi Chemical Corporation), and "YLH1048" (manufactured by Mitsubishi Chemical Corporation) as active ester-based hardeners that are benzoyl derivatives of phenol novolac.
[0028] Specific examples of benzoxazine-based curing agents include "HFB2006M" manufactured by Showa Polymer Co., Ltd., and "Pd" and "Fa" manufactured by Shikoku Chemical Industry Co., Ltd.
[0029] Examples of the cyanate ester curing agent include bifunctional cyanate resins such as bisphenol A dicyanate, polyphenol cyanate, oligo(3-methylene-1,5-phenylene cyanate), 4,4'-methylenebis(2,6-dimethylphenyl cyanate), 4,4'-ethylidene diphenyl dicyanate, hexafluorobisphenol A dicyanate, 2,2-bis(4-cyanate)phenylpropane, 1,1-bis(4-cyanate phenylmethane), bis(4-cyanate-3,5-dimethylphenyl)methane, 1,3-bis(4-cyanate phenyl-1-(methylethylidene))benzene, bis(4-cyanate phenyl)thioether, and bis(4-cyanate phenyl)ether; polyfunctional cyanate resins derived from phenol novolac and cresol novolac; and prepolymers in which these cyanate resins are partially converted to triazine. Specific examples of cyanate ester-based curing agents include "PT30" and "PT60" (phenol novolac type multifunctional cyanate ester resins), "ULL-950S" (multifunctional cyanate ester resin), "BA230", and "BA230S75" (prepolymers in which part or all of bisphenol A dicyanate has been converted to triazine to form a trimer), all of which are manufactured by Lonza Japan.
[0030] Specific examples of carbodiimide-based curing agents include "V-03" and "V-07" manufactured by Nisshinbo Chemical Inc.
[0031] The ratio of the amount of epoxy resin to the curing agent is preferably 1:0.01 to 1:3, more preferably 1:0.015 to 1:2, and even more preferably 1:0.02 to 1:1.5, in terms of the ratio of [total number of epoxy groups in the epoxy resin] to [total number of reactive groups in the curing agent]. Here, the reactive groups in the curing agent are active hydroxyl groups, active ester groups, etc., and vary depending on the type of curing agent. The total number of epoxy groups in the epoxy resin is the value obtained by dividing the solid content mass of each epoxy resin by the epoxy equivalent, and the total number of reactive groups in the curing agent is the value obtained by dividing the solid content mass of each curing agent by the reactive group ...
[0032] The content of the curing agent is not particularly limited, but is preferably 60% by mass or less, more preferably 55% by mass or less, and even more preferably 50% by mass or less, assuming that the resin component is 100% by mass. The lower limit is not particularly limited, but is preferably 5% by mass or more, more preferably 10% by mass or more, and even more preferably 20% by mass or more. By making the content of the curing agent 5% by mass or more, it is possible to improve the plating adhesion and the base adhesion. Furthermore, by making it 60% by mass or less, it is possible to improve the smear removal property in the case of an active ester-based curing agent, and to lower the dielectric tangent in the case of a phenol-based curing agent and a naphthol-based curing agent.
[0033] <(C) Compounds having a cyclic ether structure with five or more members> The resin composition contains 1 to 50 mass % of (C) a compound having a cyclic ether structure having five or more members, when the resin component is taken as 100 mass %.
[0034] As mentioned above, conventionally, there has been a trade-off between dielectric tangent and smear removability, but by including a predetermined amount of (C) a compound having a cyclic ether structure of 5 or more members, it is possible to lower the dielectric tangent and improve the smear removability. Cyclic ethers of 5 or more members have the property of having a low dielectric tangent because the movement of the molecules is restricted. In addition, cyclic ethers of 5 or more members have a certain degree of hydrophilicity because of their polarity. The hydrophilicity makes it easier to remove smears, improving the smear removability. Furthermore, the polarity and hydrophilicity are thought to improve compatibility, plating adhesion, and substrate adhesion. However, the technical scope of the present invention is not limited by the explanation of the mechanism by which the effects described here are obtained.
[0035] From the viewpoint of significantly obtaining the desired effects of the present invention, the number of oxygen atoms contained in the cyclic ether structure is preferably 1 or more, more preferably 2 or more. The lower limit is not particularly limited, but is preferably 5 or less, more preferably 4 or less, and even more preferably 3 or less.
[0036] The cyclic ether structure having 5 or more members is not particularly limited as long as it is 5 or more members, and may be a monocyclic ring, a polycyclic ring, or a condensed ring. The component (C) may have a plurality of cyclic ether structures. The cyclic ether structure is preferably a 5- to 10-membered ring, more preferably a 5- to 8-membered ring, and even more preferably a 5- to 6-membered ring. Specific examples of the cyclic ether structure having 5 or more members include a furan structure, a tetrahydrofuran structure, a dioxolane structure, a pyran structure, a dihydropyran structure, a tetrahydropyran structure, and a dioxane structure. Among these, from the viewpoint of improving compatibility, it is preferable that the compound having a cyclic ether structure having 5 or more members includes a dioxane structure. The dioxane structure is a concept including a 1,2-dioxane structure, a 1,3-dioxane structure, and a 1,4-dioxane structure, and the 1,3-dioxane structure is preferable.
[0037] The cyclic ether structure having 5 or more members may have a substituent such as an alkyl group or an alkoxy group bonded thereto. The number of carbon atoms in these substituents is usually 1 to 6 (preferably 1 to 3).
[0038] From the viewpoint of lowering the dielectric tangent, the (C) component preferably has a carbon-carbon unsaturated bond, more preferably a carbon-carbon double bond. The carbon-carbon unsaturated bond may be present within the cyclic ether structure or outside the cyclic ether structure, and is preferably present as a functional group described below. The (C) component may have a plurality of carbon-carbon unsaturated bonds.
[0039] From the viewpoint of lowering the dielectric tangent and facilitating the reaction with the (A) component, the (C) component preferably has one or more functional groups selected from the group consisting of vinyl groups, methacryl groups, acrylic groups, allyl groups, styryl groups, and propenyl groups, and more preferably has a vinyl group. The functional group may be present in any one of the (C) components, and may be present within the cyclic ether structure or outside the cyclic ether structure. The functional group may be present in more than one part.
[0040] The compound having a cyclic ether structure having five or more members is preferably represented by the following general formula (1). [ka] (In formula (1), ring A represents a divalent group having a cyclic ether structure of 5 or more members, and B 1 and B. 2 each independently represents a single bond or a divalent linking group; C 1 and C 2 each independently represents a functional group.)
[0041] Ring A represents a divalent group having a cyclic ether structure of 5 or more members. The cyclic ether structure of 5 or more members is the same as the cyclic ether structure of 5 or more members described above, and the preferred range is also the same.
[0042] Specific examples of the divalent group having a cyclic ether structure having 5 or more members include a furan-2,5-diyl group, a tetrahydrofuran-2,5-diyl group, a dioxolane-2,5-diyl group, a pyran-2,5-diyl group, a dihydropyran-2,5-diyl group, a tetrahydropyran-2,5-diyl group, a 1,2-dioxane-3,6-diyl group, a 1,3-dioxane-2,5-diyl group, a 1,4-dioxane-2,5-diyl group, and a 5-ethyl-1,3-dioxane-2,5-diyl group, of which a 5-ethyl-1,3-dioxane-2,5-diyl group is preferred.
[0043] B 1 and B. 2 each independently represents a single bond or a divalent linking group, and a divalent linking group is preferable. Examples of the divalent linking group include an alkylene group which may have a substituent, an alkynylene group which may have a substituent, an arylene group which may have a substituent, a heteroarylene group which may have a substituent, an ester bond, an ether bond, an amide bond, a urea bond, a urethane bond, a group represented by -C(=O)-, -S-, -SO-, or -NH-, and the like, and may be a group formed by combining a plurality of these groups.
[0044] The alkylene group which may have a substituent is preferably an alkylene group having 1 to 10 carbon atoms, more preferably an alkylene group having 1 to 6 carbon atoms, and further preferably an alkylene group having 1 to 5 carbon atoms or an alkylene group having 1 to 3 carbon atoms. The alkylene group may be linear, branched, or cyclic. Examples of such alkylene groups include a methylene group, an ethylene group, a propylene group, a butylene group, a pentylene group, a hexylene group, and a 1,1-dimethylethylene group, and the like. A methylene group, an ethylene group, and a 1,1-dimethylethylene group are preferred.
[0045] The alkylene group may have a substituent. The substituent is not particularly limited, and examples of the substituent include a halogen atom, -OH, -OC 1-6 Alkyl group, -N(C 1-6 Alkyl group) 2, C 1-6 Alkyl group, C 6-10An aryl group, -NH2, -CN, -C(O)O-C 1-6 Examples include an alkyl group, -COOH, -C(O)H, -NO2, etc.
[0046] Here, the term "C p-q "(where p and q are positive integers and p < q) represents that the number of carbon atoms in the organic group described immediately after this term is p to q. For example, the expression "C 1-6 alkyl group" indicates an alkyl group having 1 to 6 carbon atoms.
[0047] The above substituents may further have a substituent (hereinafter sometimes referred to as a "secondary substituent"). As the secondary substituent, the same ones as the above substituents may be used unless otherwise specified.
[0048] As the alkynylene group which may have a substituent, an alkynylene group having 2 to 10 carbon atoms is preferable, an alkynylene group having 2 to 6 carbon atoms is more preferable, and an alkynylene group having 2 to 5 carbon atoms is even more preferable. Examples of the alkynylene group include an ethynylene group, a propynylene group, a butynylene group, a pentynylene group, and a hexynylene group. The substituents that the alkynylene group may have are the same as those that the alkylene group may have.
[0049] As the arylene group which may have a substituent, an arylene group having 6 to 14 carbon atoms is preferable, and an arylene group having 6 to 10 carbon atoms is more preferable. Examples of the arylene group include a phenylene group, a naphthylene group, and an anthracenylene group. The substituents that the arylene group may have are the same as those that the alkylene group may have.
[0050] The heteroarylene group which may have a substituent is preferably a heteroarylene group having 3 to 15 carbon atoms, more preferably a heteroarylene group having 3 to 9 carbon atoms, and further preferably a heteroarylene group having 3 to 6 carbon atoms. Examples of the heteroarylene group include a furandiyl group, a pyridinediyl group, and a thiophenediyl group. The substituent which the heteroarylene group may have is the same as the substituent which the alkylene group may have.
[0051] Among these, B 1 and B. 2 is preferably a group obtained by combining one or more selected from an alkylene group which may have a substituent, an alkynylene group which may have a substituent, an ester bond, and an ether bond, and more preferably a group obtained by combining one or more selected from an alkylene group which may have a substituent, and an ester bond.
[0052] C 1 and C 2 each independently represents a functional group. Examples of the functional group include a vinyl group, a methacryl group, an acryl group, an allyl group, a styryl group, a propenyl group, and an epoxy group, and a vinyl group is more preferable.
[0053] Specific examples (exemplary compounds) of the component (C) are shown below, but the component (C) is not limited to these. [ka]
[0054] As the component (C), a commercially available product may be used, for example, “A-DOG” manufactured by Shin-Nakamura Chemical Co., Ltd. (the compound of the specific example above) and “KAYARAD R-604” manufactured by Nippon Kayaku Co., Ltd. (the compound of the specific example above) can be mentioned.
[0055] The content of component (C) is 1% by mass or more, preferably 5% by mass or more, and more preferably 10% by mass or more, based on 100% by mass of the resin component. The upper limit is 50% by mass or less, preferably 48% by mass or less, more preferably 45% by mass or less, and even more preferably 40% by mass or less. By making the content 1% by mass or more, it is possible to lower the dielectric tangent and further improve the smear removal property, and by making it 50% by mass or less, it is possible to improve the plating adhesion and the base adhesion.
[0056] The mass ratio of the epoxy resin to the (C) component (epoxy resin:mass of the (C) component) is preferably in the range of 1:0.01 to 1:100, more preferably in the range of 1:0.1 to 1:90, and still more preferably in the range of 1:0.1 to 1:80. By keeping it within such a range, compatibility can be improved.
[0057] <(D) Inorganic filler> The resin composition may contain (D) an inorganic filler in addition to the components (A) to (C) from the viewpoint of lowering the dielectric tangent and improving smear removal properties.
[0058] The material of the inorganic filler is not particularly limited, and examples thereof include silica, alumina, glass, cordierite, silicon oxide, barium sulfate, barium carbonate, talc, clay, mica powder, zinc oxide, hydrotalcite, boehmite, aluminum hydroxide, magnesium hydroxide, calcium carbonate, magnesium carbonate, magnesium oxide, boron nitride, aluminum nitride, manganese nitride, aluminum borate, strontium carbonate, strontium titanate, calcium titanate, magnesium titanate, bismuth titanate, titanium oxide, zirconium oxide, barium titanate, barium zirconate titanate, barium zirconate, calcium zirconate, zirconium phosphate, and zirconium tungstate phosphate. Among these, silica is particularly suitable. Examples of silica include amorphous silica, fused silica, crystalline silica, synthetic silica, and hollow silica. As the silica, spherical silica is preferable. The inorganic filler may be used alone or in combination of two or more.
[0059] The average particle size of the inorganic filler is preferably 3 μm or less, more preferably 2 μm or less, and even more preferably 1 μm or less, from the viewpoint of obtaining an insulating layer with small surface roughness and improving the formability of fine wiring. The lower limit of the average particle size is not particularly limited, but is preferably 0.01 μm or more, more preferably 0.1 μm or more, and even more preferably 0.3 μm or more. Examples of commercially available inorganic fillers having such an average particle size include "YC100C", "YA050C", "YA050C-MJE", and "YA010C" manufactured by Admatechs Co., Ltd., "UFP-30" manufactured by Denki Kagaku Kogyo Co., Ltd., "Silfill NSS-3N", "Silfill NSS-4N", and "Silfill NSS-5N" manufactured by Tokuyama Corporation, and "SO-C2" and "SO-C1" manufactured by Admatechs Co., Ltd.
[0060] The average particle size of the inorganic filler can be measured by a laser diffraction / scattering method based on the Mie scattering theory. Specifically, a particle size distribution of the inorganic filler is created on a volume basis using a laser diffraction / scattering particle size distribution measuring device, and the median diameter is taken as the average particle size. The measurement sample is preferably an inorganic filler dispersed in methyl ethyl ketone using ultrasonic waves. Examples of laser diffraction / scattering particle size distribution measuring devices that can be used include the LA-500 manufactured by Horiba, Ltd. and the SALD-2200 manufactured by Shimadzu Corporation.
[0061] From the viewpoint of improving moisture resistance and dispersibility, the inorganic filler is preferably treated with one or more surface treatment agents such as the above-mentioned fluorine compounds, such as a fluorine-containing silane coupling agent, an aminosilane coupling agent, an epoxysilane coupling agent, a mercaptosilane coupling agent, a silane coupling agent, an alkoxysilane, an organosilazane compound, and a titanate coupling agent, and is more preferably treated with a fluorine-containing silane coupling agent. Examples of commercially available surface treatment agents include Shin-Etsu Chemical Co., Ltd.'s "KBM403" (3-glycidoxypropyltrimethoxysilane), Shin-Etsu Chemical Co., Ltd.'s "KBM803" (3-mercaptopropyltrimethoxysilane), Shin-Etsu Chemical Co., Ltd.'s "KBE903" (3-aminopropyltriethoxysilane), Shin-Etsu Chemical Co., Ltd.'s "KBM573" (N-phenyl-3-aminopropyltrimethoxysilane), Shin-Etsu Chemical Co., Ltd.'s "SZ-31" (hexamethyldisilazane), Shin-Etsu Chemical Co., Ltd.'s "KBM103" (phenyltrimethoxysilane), Shin-Etsu Chemical Co., Ltd.'s "KBM-4803" (long-chain epoxy-type silane coupling agent), and Shin-Etsu Chemical Co., Ltd.'s "KBM-7103" (3,3,3-trifluoropropyltrimethoxysilane).
[0062] From the viewpoint of improving the dispersibility of the inorganic filler, the degree of surface treatment with the surface treatment agent is preferably 0.2 to 5 parts by mass of the surface treatment agent per 100 parts by mass of the inorganic filler, more preferably 0.2 to 3 parts by mass, and even more preferably 0.3 to 2 parts by mass.
[0063] The degree of surface treatment with the surface treatment agent can be evaluated by the amount of carbon per unit surface area of the inorganic filler. From the viewpoint of improving the dispersibility of the inorganic filler, the amount of carbon per unit surface area of the inorganic filler is set to 0.02 mg / m 2 More than 0.1 mg / m is preferable. 2 More preferably, 0.2 mg / m or more 2 On the other hand, from the viewpoint of suppressing an increase in the melt viscosity of the resin varnish and the melt viscosity in the form of a sheet, it is more preferable that the content is 1 mg / m 2Less than 0.8 mg / m is preferred. 2 Less than 0.5 mg / m is more preferable. 2 The following is even more preferred:
[0064] The amount of carbon per unit surface area of the inorganic filler can be measured after the surface-treated inorganic filler is washed with a solvent (e.g., methyl ethyl ketone (MEK)). Specifically, a sufficient amount of MEK as a solvent is added to the inorganic filler that has been surface-treated with a surface treatment agent, and ultrasonic cleaning is performed at 25°C for 5 minutes. After removing the supernatant and drying the solid content, the amount of carbon per unit surface area of the inorganic filler can be measured using a carbon analyzer. The carbon analyzer that can be used is the "EMIA-320V" manufactured by Horiba, Ltd.
[0065] When the resin composition contains an inorganic filler, the content of the inorganic filler is preferably 50% by mass or more, more preferably 55% by mass or more, even more preferably 60% by mass or more, 65% by mass or more, or 70% by mass or more, based on 100% by mass of the non-volatile components in the resin composition, from the viewpoint of reducing the dielectric tangent and improving the smear removability. The upper limit of the content of the inorganic filler in the resin composition is preferably 90% by mass or less, more preferably 85% by mass or less, even more preferably 80% by mass or less, or 75% by mass or less, based on the mechanical strength of the insulating layer.
[0066] <(E) Curing accelerator> In one embodiment, the resin composition may contain (E) a curing accelerator. Examples of the curing accelerator include phosphorus-based curing accelerators, amine-based curing accelerators, imidazole-based curing accelerators, guanidine-based curing accelerators, metal-based curing accelerators, and organic peroxide-based curing accelerators. Phosphorus-based curing accelerators, amine-based curing accelerators, imidazole-based curing accelerators, and metal-based curing accelerators are preferred, and imidazole-based curing accelerators and organic peroxide-based curing accelerators are more preferred. The curing accelerator may be used alone or in combination of two or more.
[0067] Examples of the phosphorus-based curing accelerator include triphenylphosphine, phosphonium borate compounds, tetraphenylphosphonium tetraphenylborate, n-butylphosphonium tetraphenylborate, tetrabutylphosphonium decanoate, (4-methylphenyl)triphenylphosphonium thiocyanate, tetraphenylphosphonium thiocyanate, butyltriphenylphosphonium thiocyanate, and the like, with triphenylphosphine and tetrabutylphosphonium decanoate being preferred.
[0068] Examples of the amine curing accelerator include trialkylamines such as triethylamine and tributylamine, 4-dimethylaminopyridine, benzyldimethylamine, 2,4,6-tris(dimethylaminomethyl)phenol, and 1,8-diazabicyclo(5,4,0)-undecene, with 4-dimethylaminopyridine and 1,8-diazabicyclo(5,4,0)-undecene being preferred.
[0069] Examples of the imidazole curing accelerator include 2-methylimidazole, 2-undecylimidazole, 2-heptadecylimidazole, 1,2-dimethylimidazole, 2-ethyl-4-methylimidazole, 1,2-dimethylimidazole, 2-ethyl-4-methylimidazole, 2-phenylimidazole, 2-phenyl-4-methylimidazole, 1-benzyl-2-methylimidazole, 1-benzyl-2-phenylimidazole, 1-cyanoethyl-2-methylimidazole, 1-cyanoethyl-2-undecylimidazole, 1-cyanoethyl-2-ethyl-4-methylimidazole, 1-cyanoethyl-2-phenylimidazole, 1-cyanoethyl-2-undecylimidazolium trimellitate, 1-cyanoethyl-2-phenylimidazolium trimellitate, 2,4-diamino-6-[2'-methylimidazolyl-(1')]-ethyl-s-triazine, 2, 4-Diamino-6-[2'-undecylimidazolyl-(1')]-ethyl-s-triazine, 2,4-diamino-6-[2'-ethyl-4'-methylimidazolyl-(1')]-ethyl-s-triazine, 2,4-diamino-6-[2'-methylimidazolyl-(1')]-ethyl-s-triazine isocyanuric acid adduct, 2-phenylimidazole isocyanuric acid adduct, 2-phenyl-4,5-dihydroxymethylimidazole, 2-furan Examples of the imidazole compounds include imidazole compounds such as 2-ethyl-4-methyl-5-hydroxymethylimidazole, 2,3-dihydro-1H-pyrrolo[1,2-a]benzimidazole, 1-dodecyl-2-methyl-3-benzylimidazolium chloride, 2-methylimidazoline, and 2-phenylimidazoline, as well as adducts of imidazole compounds and epoxy resins. Of these, 2-ethyl-4-methylimidazole and 1-benzyl-2-phenylimidazole are preferred.
[0070] As the imidazole-based curing accelerator, a commercially available product may be used, for example, "P200-H50" manufactured by Mitsubishi Chemical Corporation.
[0071] Examples of the guanidine curing accelerator include dicyandiamide, 1-methylguanidine, 1-ethylguanidine, 1-cyclohexylguanidine, 1-phenylguanidine, 1-(o-tolyl)guanidine, dimethylguanidine, diphenylguanidine, trimethylguanidine, tetramethylguanidine, pentamethylguanidine, 1,5,7-triazabicyclo[4.4.0]dec-5-ene, and 7-methyl-1,5,7-triazabicyclo[4.4.0]dec-5-ene. Examples of such biguanide include o-[4.4.0]dec-5-ene, 1-methylbiguanide, 1-ethylbiguanide, 1-n-butylbiguanide, 1-n-octadecylbiguanide, 1,1-dimethylbiguanide, 1,1-diethylbiguanide, 1-cyclohexylbiguanide, 1-allylbiguanide, 1-phenylbiguanide, and 1-(o-tolyl)biguanide. Of these, dicyandiamide and 1,5,7-triazabicyclo[4.4.0]dec-5-ene are preferred.
[0072] Examples of metal-based curing accelerators include organometallic complexes or organometallic salts of metals such as cobalt, copper, zinc, iron, nickel, manganese, and tin. Specific examples of organometallic complexes include organocobalt complexes such as cobalt(II) acetylacetonate and cobalt(III) acetylacetonate, organocopper complexes such as copper(II) acetylacetonate, organozinc complexes such as zinc(II) acetylacetonate, organoiron complexes such as iron(III) acetylacetonate, organonickel complexes such as nickel(II) acetylacetonate, and organomanganese complexes such as manganese(II) acetylacetonate. Examples of organometallic salts include zinc octylate, tin octylate, zinc naphthenate, cobalt naphthenate, tin stearate, and zinc stearate.
[0073] Examples of the organic peroxide curing accelerator include dicumyl peroxide, cyclohexanone peroxide, tert-butyl peroxybenzoate, methyl ethyl ketone peroxide, dicumyl peroxide, tert-butylcumyl peroxide, di-tert-butyl peroxide, diisopropylbenzene hydroperoxide, cumene hydroperoxide, tert-butyl hydroperoxide, etc. As the organic peroxide curing accelerator, commercially available products may be used, for example, "Percumyl D" manufactured by NOF Corporation.
[0074] When the resin composition contains a curing accelerator, the content of the curing accelerator is preferably 0.01% by mass to 1% by mass, more preferably 0.01% by mass to 0.5% by mass, and even more preferably 0.01% by mass to 0.1% by mass, based on 100% by mass of the non-volatile components in the resin composition.
[0075] <(F) Indene Coumarone Resin> In one embodiment, the resin composition may contain (F) an indene coumarone resin. Examples of the indene coumarone resin include a copolymer of indene and coumarone, and a copolymer of indene, coumarone, and styrene.
[0076] The content of the coumarone component in the indene coumarone resin is preferably 5 mol% or more, more preferably 8 mol% or more, and even more preferably 10 mol% or more. The upper limit is preferably 40 mol% or less, more preferably 35 mol% or less, and even more preferably 30 mol% or less.
[0077] The content of the indene component in the indene coumarone resin is preferably 30 mol% or more, more preferably 35 mol% or more, and even more preferably 40 mol% or more. The upper limit is preferably 80 mol% or less, more preferably 75 mol% or less, and even more preferably 70 mol% or less.
[0078] When the indene coumarone resin is a copolymer of indene, coumarone and styrene, the content of the styrene component is preferably 20 mol% or more, more preferably 25 mol% or more, and even more preferably 30 mol% or more. The upper limit is preferably 70 mol% or less, more preferably 65 mol% or less, and even more preferably 60 mol% or less.
[0079] Specific examples of indene coumarone resins include "H-100," "V-120S," and "V-120," both manufactured by Nippon Paint Chemical Co., Ltd.
[0080] When the resin composition contains an indene coumarone resin, from the viewpoint of improving compatibility, the content of the indene coumarone resin is preferably 0.1 to 3 mass%, more preferably 0.3 to 2 mass%, and even more preferably 0.5 to 1.5 mass%, based on 100 mass% of the non-volatile components in the resin composition.
[0081] <(G)Thermoplastic resin> In one embodiment, the resin composition may contain (G) a thermoplastic resin. Examples of the thermoplastic resin include phenoxy resin, polyvinyl acetal resin, polyolefin resin, polybutadiene resin, polyimide resin, polyamideimide resin, polyetherimide resin, polysulfone resin, polyethersulfone resin, polyphenylene ether resin, polycarbonate resin, polyetheretherketone resin, and polyester resin, and phenoxy resin is preferred. The thermoplastic resin may be used alone or in combination of two or more.
[0082] The polystyrene-equivalent weight average molecular weight of the thermoplastic resin is preferably 8,000 or more, more preferably 10,000 or more, even more preferably 20,000 or more, and particularly preferably 40,000 or more. The upper limit is not particularly limited, but is preferably 70,000 or less, more preferably 60,000 or less. The polystyrene-equivalent weight average molecular weight of the thermoplastic resin is measured by gel permeation chromatography (GPC). Specifically, the polystyrene-equivalent weight average molecular weight of the thermoplastic resin is measured at a column temperature of 40° C. using a measuring device LC-9A / RID-6A manufactured by Shimadzu Corporation, a column Shodex K-800P / K-804L / K-804L manufactured by Showa Denko K.K., chloroform or the like as a mobile phase, and can be calculated using a calibration curve of standard polystyrene.
[0083] Examples of the phenoxy resin include phenoxy resins having one or more skeletons selected from the group consisting of bisphenol A skeleton, bisphenol F skeleton, bisphenol S skeleton, bisphenolacetophenone skeleton, novolac skeleton, biphenyl skeleton, fluorene skeleton, dicyclopentadiene skeleton, norbornene skeleton, naphthalene skeleton, anthracene skeleton, adamantane skeleton, terpene skeleton, and trimethylcyclohexane skeleton. The terminal of the phenoxy resin may be any functional group such as a phenolic hydroxyl group or an epoxy group. The phenoxy resin may be used alone or in combination of two or more. Specific examples of phenoxy resins include "1256" and "4250" (both of which are phenoxy resins containing a bisphenol A skeleton), "YX8100" (phenoxy resin containing a bisphenol S skeleton), and "YX6954" (phenoxy resin containing a bisphenol acetophenone skeleton) manufactured by Mitsubishi Chemical Corporation. Other examples include "FX280" and "FX293" manufactured by Nippon Steel & Sumikin Chemical Co., Ltd., and "YL7500BH30", "YX6954BH30", "YX7553", "YX7553BH30", "YL7769BH30", "YL6794", "YL7213", "YL7290", and "YL7482" manufactured by Mitsubishi Chemical Corporation.
[0084] Examples of polyvinyl acetal resin include polyvinyl formal resin and polyvinyl butyral resin, and polyvinyl butyral resin is preferred.Specific examples of polyvinyl acetal resin include "Denka Butyral 4000-2", "Denka Butyral 5000-A", "Denka Butyral 6000-C", and "Denka Butyral 6000-EP" manufactured by Denki Kagaku Kogyo Co., Ltd., and S-LEC BH series, BX series (e.g. BX-5Z), KS series (e.g. KS-1), BL series, and BM series manufactured by Sekisui Chemical Co., Ltd.
[0085] Specific examples of polyimide resins include "Rikacoat SN20" and "Rikacoat PN20" manufactured by New Japan Chemical Co., Ltd. Specific examples of polyimide resins also include modified polyimides such as linear polyimides obtained by reacting bifunctional hydroxyl-terminated polybutadiene, a diisocyanate compound, and a tetrabasic acid anhydride (polyimides described in JP-A-2006-37083), and polysiloxane skeleton-containing polyimides (polyimides described in JP-A-2002-12667 and JP-A-2000-319386, etc.).
[0086] Specific examples of polyamide-imide resins include "Viromax HR11NN" and "Viromax HR16NN" manufactured by Toyobo Co., Ltd. Specific examples of polyamide-imide resins also include modified polyamide-imides such as "KS9100" and "KS9300" (polysiloxane skeleton-containing polyamide-imide) manufactured by Hitachi Chemical Co., Ltd.
[0087] A specific example of a polyethersulfone resin is "PES5003P" manufactured by Sumitomo Chemical Co., Ltd. A specific example of a polyphenylene ether resin is "OPE-2St 1200", an oligophenylene ether-styrene resin having a vinyl group manufactured by Mitsubishi Gas Chemical Co., Ltd.
[0088] Specific examples of polysulfone resins include polysulfones "P1700" and "P3500" manufactured by Solvay Advanced Polymers.
[0089] Among them, the thermoplastic resin is preferably a phenoxy resin or a polyvinyl acetal resin. Therefore, in a preferred embodiment, the thermoplastic resin includes at least one selected from the group consisting of phenoxy resin and polyvinyl acetal resin. Among them, the thermoplastic resin is preferably a phenoxy resin, and more preferably a phenoxy resin having a weight average molecular weight of 40,000 or more. By using a phenoxy resin having a weight average molecular weight of 40,000 or more, it is possible to miniaturize the wiring circuit.
[0090] When the resin composition contains a thermoplastic resin, the content of the thermoplastic resin is preferably 1 to 10 mass%, more preferably 1.5 to 5 mass%, and even more preferably 2 to 5 mass%, based on 100 mass% of the non-volatile components in the resin composition.
[0091] <(H) Flame retardants> In one embodiment, the resin composition may contain a flame retardant (H). Examples of the flame retardant include organic phosphorus flame retardants, organic nitrogen-containing phosphorus compounds, nitrogen compounds, silicone flame retardants, metal hydroxides, etc. The flame retardants may be used alone or in combination of two or more.
[0092] As the flame retardant, commercially available products may be used, such as "HCA-HQ" manufactured by Sankosha and "PX-200" manufactured by Daihachi Chemical Industry Co., Ltd. As the flame retardant, those which are difficult to hydrolyze are preferred, such as 10-(2,5-dihydroxyphenyl)-10-hydro-9-oxa-10-phosphaphenanthrene-10-oxide.
[0093] When the resin composition contains a flame retardant, the content of the flame retardant is preferably 0.5 to 20 mass%, more preferably 0.5 to 15 mass%, and even more preferably 0.5 to 10 mass%, based on 100 mass% of the non-volatile components in the resin composition.
[0094] <(I) Organic filler> In one embodiment, the resin composition may contain (I) an organic filler. By containing the component (I), the tensile breaking strength of the cured product of the resin composition layer of the adhesive film can be improved. As the organic filler, any organic filler that can be used when forming an insulating layer of a printed wiring board may be used, and examples thereof include rubber particles, polyamide fine particles, silicone particles, etc.
[0095] As the rubber particles, commercially available products may be used, for example, "EXL2655" manufactured by Dow Chemical Japan, "AC3401N" and "AC3816N" manufactured by Aica Kogyo Co., Ltd.
[0096] When the resin composition contains an organic filler, the content of the organic filler is preferably 0.1 to 20 mass%, more preferably 0.2 to 10 mass%, even more preferably 0.3 to 5 mass%, or even more preferably 0.5 to 3 mass%, based on 100 mass% of the non-volatile components in the resin composition.
[0097] <(J) Optional Additives> In one embodiment, the resin composition may further contain other additives as necessary. Examples of such other additives include organometallic compounds such as organocopper compounds, organozinc compounds, and organocobalt compounds, as well as resin additives such as thickeners, defoamers, leveling agents, adhesion promoters, and colorants.
[0098] <Physical properties and applications of resin compositions> The resin composition of the present invention can provide an insulating layer having a low dielectric tangent, good plating adhesion and base adhesion, and excellent smear removal properties, and also has good compatibility. Therefore, the resin composition of the present invention can be suitably used as a resin composition for forming an insulating layer of a printed wiring board (resin composition for insulating layer of printed wiring board), and can be more suitably used as a resin composition for forming an interlayer insulating layer of a printed wiring board (resin composition for insulating layer of printed wiring board). In addition, the resin composition of the present invention can be suitably used when the printed wiring board is a circuit board with built-in components, since it provides an insulating layer with good component embedding properties.
[0099] The cured product obtained by thermally curing the resin composition at 190°C for 90 minutes exhibits the characteristic of a low dielectric loss tangent. That is, an insulating layer with a low dielectric loss tangent is obtained. The dielectric loss tangent is preferably 0.005 or less, more preferably 0.0045 or less, and even more preferably 0.004 or less. The lower limit is not particularly limited, but may be 0.0001 or more. The dielectric loss tangent can be measured according to the method described below in <Measurement of dielectric loss tangent>.
[0100] The resin composition is thermally cured at 190°C for 90 minutes to produce a cured product that exhibits excellent adhesion to a conductor layer (plating adhesion) such as a plating. That is, an insulating layer exhibiting good plating adhesion is obtained. The plating adhesion is preferably greater than 0.3 kgf / cm, more preferably 0.31 kgf / cm or more, and even more preferably 0.32 kgf / cm or more. There is no particular upper limit, but it may be 10 kgf / cm or less, or 1 kgf / cm or less, for example. The plating adhesion can be measured according to the method described below in <Measurement of plating adhesion>.
[0101] The cured product obtained by thermally curing the resin composition at 190°C for 90 minutes exhibits the property of excellent adhesion to copper foil and the like (substrate adhesion). That is, an insulating layer exhibiting good substrate adhesion is obtained. The substrate adhesion is preferably more than 0.3 kgf / cm, more preferably 0.31 kgf / cm or more, and even more preferably 0.32 kgf / cm or more. The upper limit is not particularly limited, but may be 10 kgf / cm or less, or 1 kgf / cm or less, etc. The substrate adhesion can be measured according to the method described below in <Substrate Adhesion Measurement>.
[0102] The cured product obtained by thermally curing the resin composition at 190°C for 90 minutes exhibits the property that smears generated during via hole formation are easily removed (excellent smear removability). That is, an insulating layer exhibiting good smear removability is obtained. Since the smear removability is excellent, the maximum smear length measured from the wall side of the bottom of the via hole is preferably less than 3 μm, more preferably 2.5 μm or less, and even more preferably 2 μm or less. The lower limit is not particularly limited, but may be 0.01 μm or more. The smear removability can be measured according to the method described below in <Evaluation of smear removability at the bottom of the via hole>.
[0103] The resin composition exhibits excellent compatibility due to the inclusion of a predetermined amount of component (C). Due to the excellent compatibility, the resin composition is free of precipitation of coarse particles of preferably 30 μm or more (more preferably 40 μm or more, and even more preferably 50 μm or more) and oil droplets.
[0104] [Sheet-type substrate] The resin composition of the present invention can be used by coating in the form of a varnish, but in general, it is industrially preferable to use the resin composition in the form of a sheet-like substrate containing the resin composition. As the sheet-like substrate, the adhesive film and prepreg shown below are preferred.
[0105] <Adhesive film> In one embodiment, the adhesive film includes a support and a resin composition layer provided on the support, and the resin composition layer is formed from the resin composition of the present invention.
[0106] From the viewpoint of thinning the printed wiring board, the thickness of the resin composition layer is preferably 100 μm or less, more preferably 80 μm or less, even more preferably 60 μm or less, and even more preferably 50 μm or less or 40 μm or less. The lower limit of the thickness of the resin composition layer is not particularly limited, but can usually be 1 μm or more, 5 μm or more, 10 μm or more, etc.
[0107] Examples of the support include films made of plastic materials, metal foils, and release papers, with films made of plastic materials and metal foils being preferred.
[0108] When a film made of a plastic material is used as the support, examples of the plastic material include polyesters such as polyethylene terephthalate (hereinafter sometimes abbreviated as "PET") and polyethylene naphthalate (hereinafter sometimes abbreviated as "PEN"), polycarbonate (hereinafter sometimes abbreviated as "PC"), acrylics such as polymethyl methacrylate (PMMA), cyclic polyolefins, triacetyl cellulose (TAC), polyether sulfide (PES), polyether ketone, polyimide, etc. Among these, polyethylene terephthalate and polyethylene naphthalate are preferred, and inexpensive polyethylene terephthalate is particularly preferred.
[0109] When a metal foil is used as the support, examples of the metal foil include copper foil, aluminum foil, etc., and copper foil is preferred. As the copper foil, a foil made of a single metal, copper, or an alloy of copper and another metal (e.g., tin, chromium, silver, magnesium, nickel, zirconium, silicon, titanium, etc.) may be used.
[0110] The surface of the support to be bonded to the resin composition layer may be subjected to a matte treatment, a corona treatment, or an antistatic treatment.
[0111] In addition, as the support, a support with a release layer having a release layer on the surface to be bonded to the resin composition layer may be used. The release agent used in the release layer of the support with a release layer may be, for example, one or more release agents selected from the group consisting of alkyd resins, polyolefin resins, urethane resins, and silicone resins. The support with a release layer may be a commercially available product, for example, "SK-1", "AL-5", and "AL-7" manufactured by Lintec Corporation, "Lumirror T60" manufactured by Toray Industries, "Purex" manufactured by Teijin Ltd., and "Unipeel" manufactured by Unitika Ltd., which are PET films having a release layer mainly composed of an alkyd resin-based release agent.
[0112] The thickness of the support is not particularly limited, but is preferably in the range of 5 μm to 75 μm, and more preferably in the range of 10 μm to 60 μm. When a support with a release layer is used, it is preferable that the total thickness of the support with a release layer is in the above range.
[0113] The adhesive film can be produced, for example, by preparing a resin varnish by dissolving the resin composition in an organic solvent, applying this resin varnish onto a support using a die coater or the like, and then drying it to form a resin composition layer.
[0114] Examples of the organic solvent include ketones such as acetone, methyl ethyl ketone (MEK) and cyclohexanone, acetates such as ethyl acetate, butyl acetate, cellosolve acetate, propylene glycol monomethyl ether acetate and carbitol acetate, carbitols such as cellosolve and butyl carbitol, aromatic hydrocarbons such as toluene and xylene, amide solvents such as dimethylformamide, dimethylacetamide (DMAc) and N-methylpyrrolidone, etc. The organic solvents may be used alone or in combination of two or more.
[0115] Drying may be performed by a known method such as heating or hot air blowing. Drying conditions are not particularly limited, but drying is performed so that the content of organic solvent in the resin composition layer becomes 10 mass % or less, preferably 5 mass % or less. Although it varies depending on the boiling point of the organic solvent in the resin varnish, for example, when a resin varnish containing 30 mass % to 60 mass % of organic solvent is used, the resin composition layer can be formed by drying at 50°C to 150°C for 3 minutes to 10 minutes.
[0116] In the adhesive film, a protective film equivalent to the support can be further laminated on the surface of the resin composition layer that is not bonded to the support (i.e., the surface opposite to the support). The thickness of the protective film is not particularly limited, but is, for example, 1 μm to 40 μm. By laminating the protective film, it is possible to prevent adhesion of dirt and the like to the surface of the resin composition layer and scratches. The adhesive film can be wound up in a roll and stored. When the adhesive film has a protective film, it can be used by peeling off the protective film.
[0117] <Prepreg> In one embodiment, the prepreg is formed by impregnating a sheet-like fiber substrate with the resin composition of the present invention.
[0118] The sheet-like fiber substrate used for the prepreg is not particularly limited, and can be a substrate commonly used for prepreg, such as glass cloth, aramid nonwoven fabric, or liquid crystal polymer nonwoven fabric. From the viewpoint of thinning the printed wiring board, the thickness of the sheet-like fiber substrate is preferably 50 μm or less, more preferably 40 μm or less, even more preferably 30 μm or less, and even more preferably 20 μm or less. The lower limit of the thickness of the sheet-like fiber substrate is not particularly limited, but is usually 10 μm or more.
[0119] The prepreg can be produced by a known method such as a hot melt method or a solvent method.
[0120] The thickness of the prepreg may be in the same range as that of the resin composition layer in the adhesive film described above.
[0121] [Printed wiring boards and methods of manufacturing printed wiring boards] The printed wiring board of the present invention includes an insulating layer formed from a cured product of the resin composition of the present invention, a first conductor layer, and a second conductor layer. The insulating layer is provided between the first conductor layer and the second conductor layer, and insulates the first conductor layer from the second conductor layer (the conductor layer may be referred to as a wiring layer).
[0122] The thickness of the insulating layer between the first and second conductor layers is preferably 6 μm or less, more preferably 5.5 μm or less, and even more preferably 5 μm or less. The lower limit is not particularly limited, but may be 0.1 μm or more. The distance between the first conductor layer and the second conductor layer (thickness of the insulating layer between the first and second conductor layers) refers to the thickness t1 of the insulating layer 3 between the main surface 11 of the first conductor layer 1 and the main surface 21 of the second conductor layer 2, as shown in FIG. 1 as an example. The first and second conductor layers are adjacent conductor layers with an insulating layer interposed between them, and the main surface 11 and the main surface 21 face each other. The thickness of the insulating layer between the first and second conductor layers can be measured according to the method described in <Measurement of the distance between conductor layers (thickness of the insulating layer between conductor layers)> described later.
[0123] The thickness t2 of the entire insulating layer is preferably 30 μm or less, more preferably 20 μm or less, further preferably 15 μm or less, or 10 μm or less. There is no particular lower limit, but it can usually be 1 μm or more, 1.5 μm or more, 2 μm or more, etc.
[0124] A printed wiring board can be produced by using the above-mentioned adhesive film by a method including the following steps (I) and (II). (I) A step of laminating the adhesive film on the inner layer substrate so that the resin composition layer of the adhesive film is bonded to the inner layer substrate. (II) A step of thermally curing the resin composition layer to form an insulating layer
[0125] The "inner layer substrate" used in step (I) mainly refers to a substrate such as a glass epoxy substrate, a metal substrate, a polyester substrate, a polyimide substrate, a BT resin substrate, or a thermosetting polyphenylene ether substrate, or a circuit substrate having a patterned conductor layer (circuit) formed on one or both sides of the substrate. In addition, the "inner layer substrate" of the present invention also includes an inner layer circuit substrate of an intermediate product on which an insulating layer and / or a conductor layer is to be further formed during the manufacture of a printed wiring board. When the printed wiring board is a circuit board with built-in components, an inner layer substrate with built-in components can be used.
[0126] The lamination of the inner layer substrate and the adhesive film can be carried out, for example, by thermocompression bonding the adhesive film to the inner layer substrate from the support side. Examples of the member for thermocompression bonding the adhesive film to the inner layer substrate (hereinafter also referred to as the "thermocompression bonding member") include a heated metal plate (such as a SUS plate) or a metal roll (SUS roll). It is preferable to press the thermocompression member not directly onto the adhesive film but via an elastic material such as heat-resistant rubber so that the adhesive film can sufficiently follow the surface irregularities of the inner layer substrate.
[0127] The lamination of the inner layer substrate and the adhesive film may be performed by a vacuum lamination method. In the vacuum lamination method, the thermocompression temperature is preferably in the range of 60°C to 160°C, more preferably in the range of 80°C to 140°C, the thermocompression pressure is preferably in the range of 0.098MPa to 1.77MPa, more preferably in the range of 0.29MPa to 1.47MPa, and the thermocompression time is preferably in the range of 20 seconds to 400 seconds, more preferably in the range of 30 seconds to 300 seconds. The lamination is preferably performed under reduced pressure conditions of 26.7hPa or less.
[0128] The lamination can be performed by a commercially available vacuum laminator, such as a vacuum pressure laminator manufactured by Meiki Seisakusho Co., Ltd., a vacuum applicator manufactured by Nikko Materials Co., Ltd., or a batch type vacuum pressure laminator.
[0129] After lamination, the laminated adhesive film may be smoothed under normal pressure (atmospheric pressure), for example, by pressing a thermocompression member from the support side. The pressing conditions for the smoothing treatment may be the same as the thermocompression conditions for the lamination. The smoothing treatment may be performed using a commercially available laminator. The lamination and smoothing treatment may be performed consecutively using the commercially available vacuum laminator.
[0130] The support may be removed between step (I) and step (II) or after step (II).
[0131] In step (II), the resin composition layer is thermally cured to form an insulating layer.
[0132] The conditions for thermally curing the resin composition layer are not particularly limited, and conditions that are usually employed when forming an insulating layer for a printed wiring board may be used.
[0133] For example, the thermal curing conditions for the resin composition layer will vary depending on the type of resin composition, etc., but the curing temperature can be in the range of 120°C to 240°C (preferably in the range of 150°C to 220°C, more preferably in the range of 170°C to 200°C), and the curing time can be in the range of 5 minutes to 120 minutes (preferably in the range of 10 minutes to 100 minutes, more preferably in the range of 15 minutes to 90 minutes).
[0134] Before the resin composition layer is thermally cured, the resin composition layer may be preheated at a temperature lower than the curing temperature. For example, prior to thermally curing the resin composition layer, the resin composition layer may be preheated for 5 minutes or more (preferably 5 minutes to 150 minutes, more preferably 15 minutes to 120 minutes) at a temperature of 50°C or more and less than 120°C (preferably 60°C or more and 110°C or less, more preferably 70°C or more and 100°C or less).
[0135] In manufacturing a printed wiring board, the steps of (III) drilling holes in the insulating layer, (IV) roughening the insulating layer, and (V) forming a conductor layer may be further carried out. These steps (III) to (V) may be carried out according to various methods known to those skilled in the art for use in manufacturing printed wiring boards. When the support is removed after step (II), the support may be removed between steps (II) and (III), between steps (III) and (IV), or between steps (IV) and (V). If necessary, the steps (II) to (V) of forming the insulating layer and the conductor layer may be repeated to form a multilayer wiring board. In this case, the thickness of the insulating layer between each conductor layer (t1 in FIG. 1) is preferably within the above range.
[0136] Step (III) is a step of drilling holes in the insulating layer, which allows holes such as via holes and through holes to be formed in the insulating layer. Step (III) may be performed using, for example, a drill, a laser, plasma, etc., depending on the composition of the resin composition used to form the insulating layer. The dimensions and shape of the holes may be appropriately determined depending on the design of the printed wiring board.
[0137] Step (IV) is a step of roughening the insulating layer. The procedure and conditions of the roughening treatment are not particularly limited, and known procedures and conditions that are usually used when forming an insulating layer of a printed wiring board can be adopted. For example, the insulating layer can be roughened by performing a swelling treatment with a swelling liquid, a roughening treatment with an oxidizing agent, and a neutralization treatment with a neutralizing liquid in this order. The swelling liquid used for the roughening treatment is not particularly limited, but includes an alkaline solution, a surfactant solution, and the like, and is preferably an alkaline solution, and as the alkaline solution, a sodium hydroxide solution and a potassium hydroxide solution are more preferable. Examples of commercially available swelling liquids include "Swelling Dip Securigans P" and "Swelling Dip Securigans SBU" manufactured by Atotech Japan. The swelling treatment with a swelling liquid is not particularly limited, but can be performed, for example, by immersing the insulating layer in a swelling liquid at 30°C to 90°C for 1 minute to 20 minutes. From the viewpoint of suppressing the swelling of the resin of the insulating layer to an appropriate level, it is preferable to immerse the insulating layer in a swelling liquid at 40°C to 80°C for 5 to 15 minutes. The oxidizing agent used in the roughening treatment is not particularly limited, but for example, an alkaline permanganate solution in which potassium permanganate or sodium permanganate is dissolved in an aqueous solution of sodium hydroxide can be mentioned. The roughening treatment using an oxidizing agent such as an alkaline permanganate solution is preferably performed by immersing the insulating layer in an oxidizing agent solution heated to 60°C to 80°C for 10 to 30 minutes. In addition, the concentration of the permanganate in the alkaline permanganate solution is preferably 5% by mass to 10% by mass. Examples of commercially available oxidizing agents include alkaline permanganate solutions such as "Concentrate Compact CP" and "Dosing Solution Securigans P" manufactured by Atotech Japan. The neutralizing solution used in the roughening treatment is preferably an acidic aqueous solution, and a commercially available product is, for example, "Reduction Solution Securigant P" manufactured by Atotech Japan. Treatment with a neutralizing solution can be performed by immersing the surface that has been roughened with an oxidizing agent in a neutralizing solution at 30°C to 80°C for 5 to 30 minutes. From the viewpoint of workability, etc., a method in which the object that has been roughened with an oxidizing agent is immersed in a neutralizing solution at 40°C to 70°C for 5 to 20 minutes is preferred.
[0138] In one embodiment, the arithmetic mean roughness Ra of the insulating layer surface after the roughening treatment is preferably 400 nm or less, more preferably 350 nm or less, and even more preferably 300 nm or less. The lower limit is not particularly limited, but is preferably 0.5 nm or more, and more preferably 1 nm or more. The root mean square roughness Rq of the insulating layer surface after the roughening treatment is preferably 400 nm or less, more preferably 350 nm or less, and even more preferably 300 nm or less. The lower limit is not particularly limited, but is preferably 0.5 nm or more, and more preferably 1 nm or more. The arithmetic mean roughness (Ra) and root mean square roughness (Rq) of the insulating layer surface can be measured using a non-contact surface roughness meter.
[0139] Step (V) is a step of forming a conductor layer. When no conductor layer is formed on the inner layer substrate, step (V) is a step of forming a first conductor layer, and when a conductor layer is formed on the inner layer substrate, the conductor layer is the first conductor layer and step (V) is a step of forming a second conductor layer.
[0140] The conductor material used for the conductor layer is not particularly limited. In a preferred embodiment, the conductor layer contains one or more metals selected from the group consisting of gold, platinum, palladium, silver, copper, aluminum, cobalt, chromium, zinc, nickel, titanium, tungsten, iron, tin and indium. The conductor layer may be a single metal layer or an alloy layer, and examples of the alloy layer include layers formed from alloys of two or more metals selected from the above group (e.g., nickel-chromium alloy, copper-nickel alloy and copper-titanium alloy). Among them, from the viewpoints of versatility, cost, ease of patterning, etc. of the conductor layer formation, a single metal layer of chromium, nickel, titanium, aluminum, zinc, gold, palladium, silver or copper, or an alloy layer of a nickel-chromium alloy, a copper-nickel alloy or a copper-titanium alloy is preferred, a single metal layer of chromium, nickel, titanium, aluminum, zinc, gold, palladium, silver or copper, or an alloy layer of a nickel-chromium alloy is more preferred, and a single metal layer of copper is even more preferred.
[0141] The conductor layer may be a single-layer structure or a multi-layer structure in which two or more single metal layers or alloy layers made of different kinds of metals or alloys are laminated. When the conductor layer has a multi-layer structure, the layer in contact with the insulating layer is preferably a single metal layer of chromium, zinc or titanium, or an alloy layer of a nickel-chromium alloy.
[0142] The thickness of the conductor layer depends on the desired design of the printed wiring board, but is generally 3 μm to 35 μm, and preferably 5 μm to 30 μm.
[0143] In one embodiment, the conductor layer may be formed by plating. For example, a conductor layer having a desired wiring pattern can be formed by plating the surface of the insulating layer by a conventionally known technique such as a semi-additive method or a full-additive method. An example of forming the conductor layer by a semi-additive method is shown below.
[0144] First, a plating seed layer is formed on the surface of an insulating layer by electroless plating. Next, a mask pattern is formed on the formed plating seed layer to expose a part of the plating seed layer corresponding to a desired wiring pattern. After a metal layer is formed on the exposed plating seed layer by electrolytic plating, the mask pattern is removed. Thereafter, unnecessary plating seed layer is removed by etching or the like to form a conductor layer having a desired wiring pattern.
[0145] The adhesive film of the present invention provides an insulating layer with good component embedding properties, and therefore can be suitably used when the printed wiring board is a circuit board with built-in components. The circuit board with built-in components can be produced by a known production method.
[0146] A printed wiring board produced using the adhesive film of the present invention may be in an embodiment including an insulating layer that is a cured product of the resin composition layer of the adhesive film, and an embedded wiring layer embedded in the insulating layer.
[0147] In another embodiment, a printed wiring board can be manufactured using the above-mentioned prepreg. The manufacturing method is basically the same as when an adhesive film is used.
[0148] [Semiconductor Devices] The semiconductor device of the present invention includes the printed wiring board of the present invention. The semiconductor device of the present invention can be manufactured by using the printed wiring board of the present invention.
[0149] Examples of the semiconductor device include various semiconductor devices used in electric appliances (for example, computers, mobile phones, digital cameras, and televisions) and vehicles (for example, motorcycles, automobiles, trains, ships, and aircraft).
[0150] The semiconductor device of the present invention can be manufactured by mounting a component (semiconductor chip) on a conductive portion of a printed wiring board. The "conductive portion" refers to a portion of a printed wiring board that transmits an electric signal, and the portion may be either on the surface or embedded. The semiconductor chip is not particularly limited as long as it is an electric circuit element made of semiconductor material.
[0151] The method of mounting a semiconductor chip when manufacturing a semiconductor device is not particularly limited as long as the semiconductor chip functions effectively, but specific examples include a wire bonding mounting method, a flip chip mounting method, a bumpless buildup layer (BBUL) mounting method, an anisotropic conductive film (ACF) mounting method, a non-conductive film (NCF) mounting method, etc. Here, the "bumpless buildup layer (BBUL) mounting method" refers to "a mounting method in which a semiconductor chip is directly embedded in a recess in a printed wiring board and the semiconductor chip is connected to the wiring on the printed wiring board." EXAMPLES
[0152] The present invention will be specifically described below with reference to examples. The present invention is not limited to these examples. In the following, "parts" and "%" mean "parts by mass" and "% by mass", respectively, unless otherwise specified.
[0153] <Example 1> 40 parts of bixylenol type epoxy resin ("YX4000HK" manufactured by Mitsubishi Chemical Corporation, epoxy equivalent weight approximately 185) was heated and dissolved in 30 parts of solvent naphtha while stirring, and then cooled to room temperature. Inorganic filler ("SO-C2" manufactured by Admatechs Co., Ltd., average particle size 0.5 μm, carbon amount per unit surface area 0.38 mg / m 2 ) 330 parts were mixed and kneaded and dispersed with a three-roll mill. 92.3 parts of an active ester curing agent (DIC Corporation "HPC-8000-65T", a toluene solution with a non-volatile content of 65% and an active group equivalent of about 223), 15 parts of a compound having a cyclic ether structure of 5 or more members (Shin-Nakamura Chemical Co., Ltd. "A-DOG"), 5 parts of indene coumarone resin (Nippon Paint Chemical Co., Ltd. "H-100"), 2 parts of a 5% MEK solution of 4-dimethylaminopyridine (DMAP) as a curing accelerator, and 0.13 parts of dicumyl peroxide (NOF Corp. "Percumyl D") were mixed and uniformly dispersed with a rotary mixer to prepare resin varnish 1.
[0154] Resin varnish 1 was uniformly applied to the release surface of an alkyd-based release-treated polyethylene terephthalate film (PET film, "AL-5" manufactured by Lintec Corporation, thickness 38 μm) using a die coater so that the thickness of the resin composition layer after drying would be 40 μm, and the film was dried at 80 to 110°C (average 95°C) for 5 minutes to produce adhesive film 1.
[0155] <Example 2> In Example 1, the amount of bixylenol-type epoxy resin ("YX4000HK" manufactured by Mitsubishi Chemical Corporation, epoxy equivalent weight: about 185) was changed from 40 parts to 25 parts, and the inorganic filler ("SO-C2" manufactured by Admatechs Co., Ltd., average particle size: 0.5 μm, carbon amount per unit surface area: 0.38 mg / m) was changed to 0.5 parts. 2) was changed from 330 parts to 320 parts, the active ester curing agent (DIC Corporation's "HPC-8000-65T", a toluene solution with a non-volatile content of 65% and an active group equivalent of about 223) was changed from 92.3 parts to 61.5 parts, and the compound having a cyclic ether structure of 5 or more members (Shin-Nakamura Chemical Co., Ltd.'s "A-DOG") was changed from 15 parts to 40 parts. A resin varnish 2 and an adhesive film 2 were produced in the same manner as in Example 1, except for the above points.
[0156] <Example 3> In Example 1, the amount of the compound having a cyclic ether structure of 5 or more members ("A-DOG" manufactured by Shin-Nakamura Chemical Co., Ltd.) was changed from 15 parts to 1.5 parts, the amount of the bixylenol type epoxy resin ("YX4000HK" manufactured by Mitsubishi Chemical Co., Ltd., epoxy equivalent of about 185) was changed from 40 parts to 45 parts, the amount of the active ester type curing agent ("HPC-8000-65T" manufactured by DIC Corporation, a toluene solution of 65% non-volatile content with an active group equivalent of about 223) was changed from 92.3 parts to 84.6 parts, and 22.5 parts of a thermoplastic resin ("OPE-2St 1200" manufactured by Mitsubishi Gas Chemical Co., Ltd., a toluene solution of 60% non-volatile content) were mixed. A resin varnish 3 and an adhesive film 3 were produced in the same manner as in Example 1 except for the above items.
[0157] <Example 4> In Example 1, the amount of bixylenol-type epoxy resin ("YX4000HK" manufactured by Mitsubishi Chemical Corporation, epoxy equivalent weight: about 185) was changed from 40 parts to 20 parts, and the inorganic filler ("SO-C2" manufactured by Admatechs Co., Ltd., average particle size: 0.5 μm, carbon amount per unit surface area: 0.38 mg / m) was changed to 0.5 parts. 2 ) was changed from 330 parts to 310 parts, the active ester curing agent (DIC Corporation's "HPC-8000-65T", a toluene solution with a non-volatile content of 65% and an active group equivalent of about 223) was changed from 92.3 parts to 46.2 parts, and the compound having a cyclic ether structure of 5 or more members (Shin-Nakamura Chemical Co., Ltd.'s "A-DOG") was changed from 15 parts to 50 parts. Resin varnish 4 and adhesive film 4 were produced in the same manner as in Example 1 except for the above points.
[0158] <Comparative Example 1> In Example 1, the amount of bixylenol-type epoxy resin ("YX4000HK" manufactured by Mitsubishi Chemical Corporation, epoxy equivalent weight: about 185) was changed from 40 parts to 20 parts, and the inorganic filler ("SO-C2" manufactured by Admatechs Co., Ltd., average particle size: 0.5 μm, carbon amount per unit surface area: 0.38 mg / m) was changed to 0.5 parts. 2 ) was changed from 330 parts to 310 parts, the active ester curing agent (DIC Corporation's "HPC-8000-65T", a toluene solution with a non-volatile content of 65% and an active group equivalent of about 223) was changed from 92.3 parts to 46.2 parts, and the compound having a cyclic ether structure of 5 or more members (Shin-Nakamura Chemical Co., Ltd.'s "A-DOG") was changed from 15 parts to 60 parts. A resin varnish 5 and an adhesive film 5 were produced in the same manner as in Example 1 except for the above points.
[0159] <Comparative Example 2> In Example 3, the compound having a cyclic ether structure of 5 or more members ("A-DOG" manufactured by Shin-Nakamura Chemical Co., Ltd.) was changed from 1.5 parts to 0.5 parts, and the thermoplastic resin ("OPE-2St 1200" manufactured by Mitsubishi Gas Chemical Co., Ltd., a toluene solution with a non-volatile content of 60%) was changed from 22.5 parts to 24.2 parts. A resin varnish 6 and an adhesive film 6 were produced in the same manner as in Example 3 except for the above.
[0160] <Comparative Example 3> In Example 1, 15 parts of a compound having a cyclic ether structure of 5 or more members ("A-DOG" manufactured by Shin-Nakamura Chemical Co., Ltd.) was changed to 15 parts of a resin having a vinyl group ("23G" manufactured by Shin-Nakamura Chemical Co., Ltd.). Resin varnish 7 and adhesive film 7 were produced in the same manner as in Example 1 except for the above points.
[0161] <Comparative Example 4> In Example 1, 15 parts of a compound having a cyclic ether structure of 5 or more members ("A-DOG" manufactured by Shin-Nakamura Chemical Co., Ltd.) was changed to 15 parts of a resin having a vinyl group ("A-DCP" manufactured by Shin-Nakamura Chemical Co., Ltd.). A resin varnish 8 and an adhesive film 8 were produced in the same manner as in Example 1 except for the above.
[0162] <Comparative Example 5> In Example 1, 15 parts of a compound having a cyclic ether structure of 5 or more members ("A-DOG" manufactured by Shin-Nakamura Chemical Co., Ltd.) was changed to 25 parts of a thermoplastic resin ("OPE-2St 1200" manufactured by Mitsubishi Gas Chemical Co., Ltd., a toluene solution with a non-volatile content of 60%). A resin varnish 9 and an adhesive film 9 were produced in the same manner as in Example 1 except for the above.
[0163] [Evaluation method] <Preparation of samples for evaluation of cured properties> The adhesive films obtained in the Examples and Comparative Examples were thermally cured at 190° C. for 90 minutes, and the PET film support was peeled off to prepare sheet-like cured product samples for evaluation.
[0164] <Measurement of dielectric tangent> A test piece 2 mm wide and 80 mm long was cut out from the sample for evaluation of the cured product. The dielectric tangent of the cut test piece was measured at a measurement frequency of 5.8 GHz and a measurement temperature of 23°C by the cavity resonance perturbation method using a measuring device "HP8362B" manufactured by Agilent Technologies, and was evaluated according to the following criteria.
[0165] <Evaluation of compatibility> The resin composition layer side of the adhesive film produced in the Examples and Comparative Examples was subjected to a 1 cm 2 The presence or absence of coarse particles was confirmed and evaluated according to the following criteria. Good: No precipitation of coarse particles of 50 μm or more and no oil droplets were observed in the resin composition layer. Poor: Precipitation of coarse particles of 50 μm or more and oil droplets are observed in the resin composition layer.
[0166] <Preparation of evaluation board> (1) Substrate preparation A glass cloth-based epoxy resin double-sided copper-clad laminate (copper foil thickness 18 μm, substrate thickness 0.4 mm, Panasonic "R1515A") with an inner layer circuit formed was prepared. This laminate has copper foil as a first conductor layer on its surface. Both sides of this laminate were immersed in MEC's "CZ8101" and etched 1 μm to roughen the copper surface, producing an inner layer circuit board.
[0167] (2) Lamination of adhesive film The adhesive films prepared in the examples and comparative examples were laminated on both sides of the inner layer circuit board using a batch type vacuum pressure laminator ("MVLP-500" manufactured by Meiki Co., Ltd.) so that the resin composition layer was bonded to the inner layer circuit board. The lamination was performed by reducing the pressure for 30 seconds to 13 hPa or less, and then pressing at 100°C and a pressure of 0.74 MPa for 30 seconds. The resin composition layer was then cured by heating in an oven at 190°C for 90 minutes to obtain an insulating layer.
[0168] (3) Via hole formation Using a CO2 laser processing machine (LC-2E21B / 1C) manufactured by Hitachi Via Mechanics, a part of the insulating layer was irradiated with a laser under the following conditions: mask diameter 1.60 mm, focus offset value 0.050, pulse width 25 μs, power 0.66 W, aperture 13, shot number 2, burst mode, and a hole was drilled in the part of the insulating layer. The top diameter of the hole (via hole) formed by the drilling process was 50 μm. The PET film supporting the layer was then peeled off.
[0169] (4) Roughening treatment The interior circuit board on which the insulating layer was formed was subjected to wet roughening treatment using a kit of surface treatment agents consisting of swelling liquid, oxidizing agent, and neutralizing liquid. Specifically, the interior circuit board on which the insulating layer was formed was immersed in swelling dip Securigant P (aqueous solution of glycol ethers and sodium hydroxide) containing diethylene glycol monobutyl ether manufactured by Atotech Japan, which was the swelling liquid, at 60°C for 10 minutes, then immersed in Concentrate Compact P (aqueous solution of KMnO4: 60g / L, NaOH: 40g / L) manufactured by Atotech Japan, which was the oxidizing agent, at 80°C for 20 minutes, and finally immersed in Reduction Showreusin Securigant P (aqueous solution of sulfuric acid) manufactured by Atotech Japan, which was the neutralizing liquid, at 40°C for 5 minutes, and then dried at 80°C for 30 minutes. The obtained substrate was designated as evaluation substrate A.
[0170] (5) Semi-additive plating Evaluation substrate A was immersed in an electroless plating solution containing PdCl2 at 40°C for 5 minutes, and then immersed in an electroless copper plating solution at 25°C for 20 minutes. The immersed evaluation substrate A was heated at 150°C for 30 minutes for annealing, and then subjected to copper sulfate electroplating to form a second conductor layer with a thickness of 30 μm. Evaluation substrate A with the resulting second conductor layer was annealed at 190°C for 60 minutes, and the resulting substrate was designated evaluation substrate B.
[0171] <Measurement of plating adhesion> A 10 mm wide and 100 mm long cut was made in the second conductor layer of evaluation board B, and one end of this was peeled off and held with a gripper (TSE Corporation, Autocom type testing machine AC-50C-SL). 35 mm was peeled off vertically at a speed of 50 mm / min at room temperature (25°C), and the load (kgf / cm) was measured and evaluated according to the following criteria.
[0172] <Evaluation of smear removal at the bottom of via holes> The periphery of the bottom of the via hole of evaluation substrate A was observed with a scanning electron microscope (SEM), and the maximum smear length from the wall side of the bottom of the via hole was measured from the obtained image. Here, the "maximum smear length" means the maximum length of the smear from the circumference of the bottom of the via to the center of the circle. The evaluation is as follows. Good: Maximum smear length is less than 3 μm Defective: Maximum smear length is 3μm or more
[0173] <Measurement of substrate adhesion> (1) Copper foil preparation The shiny side of Mitsui Mining & Smelting's "3EC-III" (electrolytic copper foil, 35μm) was immersed in MEC's MEC Etch Bond "CZ-8101" to roughen the copper surface (Ra value = 1μm) and to apply anti-rust treatment (CL8300). This copper foil is called CZ copper foil. It was then heated in an oven at 130℃ for 30 minutes.
[0174] (2) Laminating copper foil and forming an insulating layer The adhesive films prepared in the examples and comparative examples were laminated on both sides of the inner layer circuit board using a batch type vacuum pressure laminator ("MVLP-500" manufactured by Meiki Co., Ltd.) so that the resin composition layer was bonded to the inner layer circuit board. The lamination was performed by reducing the pressure for 30 seconds to 13 hPa or less, and then pressing at 100°C and a pressure of 0.74 MPa for 30 seconds. The PET film, which was the support, was peeled off from the laminated adhesive film. The treated side of the CZ copper foil of "3EC-III" was laminated on the resin composition layer from which the support was peeled off under the same conditions as above. Then, the resin composition layer was cured under the curing conditions of 190°C and 90 minutes to form an insulating layer, thereby preparing a sample.
[0175] (3) Measurement of copper foil peel strength (adhesion) The prepared sample was cut into small pieces of 150 x 30 mm. A cutter was used to make a 10 mm wide and 100 mm long cut in the copper foil part of the small piece, and one end of the copper foil was peeled off and held with a gripper (TSE Corporation, Autocom type testing machine, "AC-50C-SL"), and the load at which 35 mm was peeled off vertically at room temperature at a speed of 50 mm / min was measured in accordance with JIS C6481 using an Instron universal testing machine, and the results were evaluated according to the following criteria.
[0176] The results of the above-mentioned Examples and Comparative Examples are shown in the following table. In the table, the meanings of the abbreviations are as follows. YX4000HK: Bixylenol type epoxy resin ("YX4000HK" manufactured by Mitsubishi Chemical Corporation) HPC-8000-65T: Active ester curing agent (DIC "HPC-8000-65T") A-DOG: Dioxane acrylic monomer ("A-DOG" manufactured by Shin-Nakamura Chemical Co., Ltd.) A-DCP: Dicyclopentane acrylic monomer ("A-DCP" manufactured by Shin-Nakamura Chemical Co., Ltd.) 23G: Ethylene oxide acrylic monomer ("23G" manufactured by Shin-Nakamura Chemical Co., Ltd.) OPE-2St 1200: Thermoplastic resin (“OPE-2St 1200” manufactured by Mitsubishi Gas Chemical Co., Ltd.) H-100: Indene coumarone resin ("H-100" manufactured by Nippon Paint Chemical Co., Ltd.) SO-C2: Spherical silica ("SO-C2" manufactured by Admatechs) Percumyl D: Dicumyl peroxide (manufactured by NOF Corporation) DMAP: 4-dimethylaminopyridine In the table, the blend amounts are calculated as solid contents, and "Content of component (A) (mass%)", "Content of component (B) (mass%)", and "Content of component (C) (mass%)" represent the contents when the resin component is taken as 100 mass%.
[0177] [Table 1]
[0178] The results in Table 1 show that Examples 1 to 4, which contain components (A) to (C) and a specified amount of component (C), are all excellent in dielectric tangent, compatibility, plating adhesion, adhesion to base, and smear removability.
[0179] On the other hand, Comparative Example 1, which contains components (A) to (C) but in which the content of component (C) exceeds 50 mass% when the resin component is taken as 100 mass%, is found to have inferior plating adhesion and substrate adhesion compared to Examples 1 to 4. It is clear that Comparative Example 2, which contains components (A) to (C) but in which the content of component (C) is less than 1 mass % relative to 100 mass % of the resin component, has inferior smear removability compared to Examples 1 to 4. It is clear that Comparative Example 3, which does not contain component (C), is inferior in dielectric tangent to Examples 1 to 4. In addition, in Comparative Examples 4 and 5 which did not contain the component (C), the dielectric loss tangent, plating adhesion, adhesion to the base, and smear removability could not be measured due to poor compatibility.
[0180] It should be noted that, in Examples 1 to 4, even when components (D) to (G) are not contained, it has been confirmed that the same results as those of the above-mentioned Examples are obtained, although to a lesser extent. [Explanation of symbols]
[0181] 1 First Conductor Layer 11: Main surface of first conductor layer 2 Second conductor layer 21 Main surface of second conductor layer 3. Insulation layer t1: Distance between the first and second conductor layers (thickness of the insulating layer between the first and second conductor layers) t2 Total thickness of the insulating layer
Claims
1. A resin composition comprising (A) an epoxy resin, (B) a curing agent, (C) a compound having a cyclic ether structure with five or more members, and (D) an inorganic filler, The component (B) is an active ester curing agent, the component (C) has one or more functional groups selected from the group consisting of a vinyl group and a methacryl group, the vinyl group being a group contained in one or more functional groups selected from the group consisting of an acryl group, an allyl group, and a styryl group; The component (D) is silica, The content of the (A) component is 5% by mass to 40% by mass, relative to 100% by mass of the non-volatile components constituting the resin composition excluding the (D) component, the content of the (C) component is 1% by mass to 50% by mass, relative to 100% by mass of the non-volatile components constituting the resin composition excluding the (D) component; The content of the (B) component is 5% by mass or more and 60% by mass or less, when the total amount of the non-volatile components constituting the resin composition excluding the (D) component is taken as 100% by mass, A resin composition, wherein when the resin composition is thermally cured at 190°C for 90 minutes, the resulting cured product has a dielectric tangent of 0.005 or less.
2. The resin composition according to claim 1, wherein the content of the component (D) is 50% by mass or more, based on 100% by mass of non-volatile components of the resin composition.
3. The resin composition according to claim 1 or 2, wherein the component (C) contains a dioxane structure.
4. The resin composition according to any one of claims 1 to 3, wherein the component (C) has a vinyl group.
5. The resin composition according to any one of claims 1 to 4, wherein the component (C) is the following compound: [Formula 1]
6. The resin composition according to any one of claims 1 to 5, which is used for forming an insulating layer of a printed wiring board.
7. The resin composition according to any one of claims 1 to 5, which is used for forming an interlayer insulating layer of a printed wiring board.
8. A sheet-like substrate comprising the resin composition according to any one of claims 1 to 7.
9. An adhesive film comprising a support and a resin composition layer formed from the resin composition according to any one of claims 1 to 7 provided on the support.
10. A printed wiring board including a first conductor layer, a second conductor layer, and an insulating layer formed between the first conductor layer and the second conductor layer, A printed wiring board, wherein the insulating layer is a cured product of the resin composition according to any one of claims 1 to 7.
11. A semiconductor device comprising the printed wiring board according to claim 10.
Citation Information
Patent Citations
Resin composition, solder resist resin composition and cured product thereof
JP2002226529A
Thermosetting liquid sealing resin composition and semiconductor device using the same
JP2005200444A
Epoxy resin composition and laminate using the same
JP2006063256A
Resin composition
JP2014034580A
Resin composition
JP2015145498A