Narrow gap gas shielded arc welding method for thick steel plate

JP7593427B2Active Publication Date: 2024-12-03JFE STEEL CORP
View PDF 8 Cites 0 Cited by

Patent Information

Application Number
JP2023025674
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2022-03-31
Filing Date
2023-02-22
Publication Date
2024-12-03
Estimated Expiration
2043-02-22

Smart Images

  • Figure 0007593427000005
    Figure 0007593427000005
  • Figure 0007593427000006
    Figure 0007593427000006
  • Figure 0007593427000007
    Figure 0007593427000007
Patent Text Reader

Abstract

To provide a narrow groove gas-shield arc-welding method for thick steel plates.SOLUTION: Thick steel plates with a plate thickness of 22 mm or more are joined by multi-layer narrow groove gas-shield arc welding with two or more electrodes. At that time, one of the first electrode and the second electrode is set to have a positive polarity and the other is set to a reverse polarity, and the first electrode and the second electrode are connected at a position along a predetermined parallel welding line, with a distance between the first electrode and the second electrode being in a range between 5 and 16 mm, and with an angle α of a straight line connecting the first electrode and the second electrode with respect to a direction perpendicular to the welding line being 60° or less, and the electrode that is set to have the positive polarity is supplied with a steel wire containing 0.015 to 0.100 mass% of a rare earth element (REM). Thereby, even in the case of applying low-cost groove processing by gas cutting or the like, a welding defect occurrence amount can be reduced without cleaning a groove surface, welding efficiency can be enhanced, and welding cost can be significantly reduced.SELECTED DRAWING: Figure 2
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a gas-shielded arc welding method, and in particular to a narrow-gap gas-shielded arc welding method for thick steel plates. Here, "narrow gap" means that the groove angle is 25° or less and the minimum groove width between the thick steel plates to be welded is 50% or less of the plate thickness of the steel materials. [Background technology]

[0002] Gas-shielded arc welding, which is used for welding steel materials, is widely used in the manufacturing fields of automobiles, buildings, bridges, electrical equipment, etc. In recent years, as steel structures have become larger and thicker, the amount of deposition during welding in the manufacturing process, especially in butt welding of steel materials, has increased, and welding work requires a lot of time, leading to increased construction costs. Therefore, the application of narrow-gap gas-shielded arc welding, which uses gas-shielded arc welding to multi-layer welds in gaps that are small compared to the plate thickness, is being considered. Narrow-gap gas-shielded arc welding reduces the amount of deposition compared to normal gas-shielded arc welding, achieving high efficiency and energy saving in welding, and is expected to reduce construction costs.

[0003] Furthermore, recently, a technology has been proposed for performing this narrow-gap gas-shielded arc welding method using multiple electrodes. With multi-electrode welding, the amount of deposited metal (metal that adheres to the inside of the gap after the welding wire melts) for filling the gap can be increased by the number of electrodes, making it possible to obtain higher welding efficiency than with single-electrode welding, and it is an effective means for increasing the efficiency of welding.

[0004] For example, Patent Document 1 describes a narrow-gap gas-shielded arc welding method for joining thick steel materials by multi-layer welding of narrow gaps. In the technology described in Patent Document 1, the first layer welding is performed by multi-electrode welding with two or more electrodes, one of the first and second electrodes is positive polarity and the other is reverse polarity, and the first and second electrodes are positioned along a predetermined parallel weld line. Furthermore, the distance between the welding wire tips of the first and second electrodes is set to a range of 5 mm to 16 mm, the angle of the straight line connecting the welding wire tips of the first and second electrodes with respect to the perpendicular direction of the weld line is set to a range of 45° or less, and the melting depth at the bottom of the thick steel material in the perpendicular direction to the weld line is set to 1.5 mm or more. As a result, even when groove processing such as gas cutting or plasma cutting is performed, there is no occurrence of defects and the effect of improving welding construction efficiency is obtained. [Prior art documents] [Patent documents]

[0005] [Patent Document 1] Patent No. 6137053 Summary of the Invention [Problem to be solved by the invention]

[0006] However, it is generally known that when gas shielded arc welding is performed with positive polarity, the arc becomes unstable and a large amount of spatter is generated. In the technology described in Patent Document 1, a large amount of spatter is generated from the electrode using positive polarity, and the spatter adheres to the inside of the groove or the welding torch, which may cause welding defects. Furthermore, it has been found that when multi-electrode welding with three or more electrodes is performed with the technology described in Patent Document 1, high-temperature cracks may occur in the center of the weld metal.

[0007] In view of the above-mentioned conventional techniques, an object of the present invention is to provide a narrow gap gas-shielded arc welding method for thick steel plates that can prevent the occurrence of welding defects and achieve high welding efficiency. [Means for solving the problem]

[0008] In order to achieve the above object, the present inventors have intensively studied factors that affect the arc stability of electrodes that adopt positive polarity. As a result, the multi-layer welding is performed as a multi-electrode welding with two or more electrodes, the first electrode and the second electrode are arranged along a predetermined parallel welding line, and one of the first electrode and the second electrode is made positive polarity and the other is made reverse polarity. Furthermore, the relative positions of the first electrode and the second electrode during welding are appropriately adjusted, and the welding wire supplied to the electrode that adopts positive polarity is made a steel wire containing 0.015 to 0.100 mass % of REM (rare earth element). As a result, the arc is stabilized, spatter generated during welding can be significantly reduced, and it has been found that multi-layer welding of thick steel plates is possible with high welding efficiency while ensuring a melting depth at the bottom of the groove (thick steel plate) of 1.5 mm or more. Furthermore, the causes of hot cracking in multi-electrode welding with three or more electrodes have been intensively studied. As a result, they discovered that if the distance between the second and subsequent electrodes is outside the appropriate range, a welding defect called hot cracking occurs in the center of the weld metal. They also discovered that if the distance between the second and subsequent electrodes is adjusted to within the range of 10 to 100 mm, a welded joint with a sound bead (weld metal) can be obtained.

[0009] The present invention has been completed based on these findings and through further investigation. [1] A method for narrow-gap gas-shielded arc welding of thick steel plates in which a thick steel plate having a plate thickness t of 22 mm or more is joined by multi-layer welding with a narrow groove having a groove angle θ of 25 ° or less and a bottom groove gap G of 7 to 18 mm, The multi-layer welding is performed by multi-electrode welding using two or more electrodes, Among the multiple electrodes, a first electrode and a second electrode are disposed at positions along a predetermined parallel welding line, and one of the first electrode and the second electrode is a wire negative (positive polarity) and the other is a wire positive (reverse polarity); Furthermore, the distance a between the tips of the welding wires supplied from the power feed tips at the tips of the welding torches of the first electrode and the second electrode is set in the range of 5 mm to 16 mm, and the angle α of a straight line connecting the tips of the welding wires of the first electrode and the second electrode with respect to a direction perpendicular to the welding line is set in the range of 60° or less, The welding wire to be supplied to the electrode having a positive polarity is a steel wire containing 0.015 to 0.100 mass% of REM (rare earth element), A narrow gap gas shielded arc welding method for thick steel plates, characterized in that the fusion depth p in the direction perpendicular to the weld line at the bottom of the thick steel plate is 1.5 mm or more. [2] A narrow gap gas-shielded arc welding method for thick steel plate as described in [1], characterized in that the feed angle φ of the welding wire of the first electrode and the second electrode to the bottom groove is between 0° and 15° with respect to the perpendicular. [3] A method for narrow gap gas-shielded arc welding of thick steel plates as described in [1] or [2], characterized in that the distance d between the side ends of the welding wire tips of the first electrode and the second electrode and the groove surface of the thick steel plate is 0.5 mm or more and 3.0 mm or less, respectively. [4] A method for narrow gap gas-shielded arc welding of thick steel plate as described in any one of [1] to [3], characterized in that the welding wire fed to the power feed tips of the first electrode and the second electrode is a welding wire curved with a radius of curvature in the range of 150 mm or more and 300 mm or less. [5] A method for narrow gap gas-shielded arc welding of thick steel plates as described in any one of [1] to [4], characterized in that a third electrode and subsequent electrodes are positioned in the center of the groove behind the first electrode and the second electrode, and the inter-electrode distance from the second electrode and subsequent electrodes is in the range of 10 mm to 100 mm. [6] A method for narrow gap gas-shielded arc welding of thick steel plates as described in any one of [1] to [5], characterized in that a mixed gas containing 60 volume % or more of CO2 gas is used as the shielding gas in the gas-shielded arc welding. Effect of the Invention

[0010] According to the present invention, when multi-layer welding thick steel plates by narrow-gap gas-shielded arc welding is performed, defects such as incomplete fusion can be prevented without the need for groove surface preparation, even when low-cost groove preparation such as gas cutting is performed. Furthermore, the amount of spatter generated during welding can be reduced, the amount of welding defects can be reduced, the welding efficiency can be improved, and the welding cost can be significantly reduced compared to the manufacturing of conventional welded joints, providing a significant industrial effect. The present invention also has the effect of being extremely useful for welding general structures such as buildings, bridges, and ships. [Brief description of the drawings]

[0011] [Figure 1] FIG. 2 is an explanatory diagram illustrating a groove shape used in the present invention. [Diagram 2] This is a diagram showing the procedure for welding with four electrodes. (a) is a front view, and (b) is a top view. [Diagram 3] FIG. 2 is an explanatory diagram showing an example of a cross section of a welded joint after multi-layer welding with four electrodes. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0012] The present invention will be specifically described below.

[0013] The present invention is a narrow-gap gas-shielded arc welding method for joining thick steel plates having a plate thickness t of 22 mm or more by multi-layer welding with a narrow gap having a groove angle θ of 25° or less and a bottom groove gap G of 7 to 18 mm. Note that the term "thick steel plate" as used herein includes not only thick steel plates but also thick-walled materials, thick-plate steel materials, and the like.

[0014] The groove used in the present invention is a V-groove (including an I-groove (θ: 0°)), and the groove shape is shown in Fig. 1. In addition, 1 is a thick steel plate, and 2 is a groove surface.

[0015] [Thickness of steel plate 1: 22mm or more] The thickness t of the thick steel plate 1 is 22 mm or more, and preferably 200 mm or less. When the thickness t of the thick steel plate 1 is less than 22 mm, in a conventional R-shaped groove, by increasing the groove angle and reducing the groove gap, the groove cross-sectional area becomes smaller than that of the groove targeted by the present invention, and the R-shaped groove may result in highly efficient welding with a smaller amount of deposition.

[0016] In addition, since the plate thickness of steel structures, including special structures, is 200 mm or less, it is preferable that the upper limit of the plate thickness of the thick steel plate is 200 mm in the present invention. In addition, the present invention can be applied to various types of thick steel plates, from mild steel plates to 780 MPa-class high-tensile steel plates. Welding of 590 MPa-class high-tensile thick steel plates is also possible without preheating.

[0017] [Bevel angle θ: 25° or less] The groove used in the present invention is a V-groove including an I-groove.

[0018] The smaller the groove (groove angle θ), the more efficient the welding. However, if the groove angle θ of the groove is small, defects such as insufficient fusion are likely to occur. In a V groove, a groove angle θ of 0°, i.e., an I-groove, is the most efficient in terms of deposition amount, but the groove closes during welding due to welding heat distortion. Therefore, it is preferable to set the groove angle θ according to the plate thickness t, taking into account welding heat distortion.

[0019] Specifically, the groove angle θ is preferably in the range of (0.5×t / 20) to (2.0×t / 20)°, and more preferably in the range of (0.8×t / 20) to (1.2×t / 20)°. Note that when the plate thickness t exceeds 100 mm, the upper limit of the suitable range is 10°.

[0020] On the other hand, welding in which the groove angle θ exceeds 25° can be performed using conventional construction methods, and therefore, in the present invention, the upper limit of the groove angle θ is set to 25°.

[0021] [Bottom groove gap G: 7~18mm] If the bottom groove gap G is less than 7 mm, it is difficult to perform welding with multiple electrodes of two or more electrodes. On the other hand, welding with a bottom groove gap G of more than 18 mm can be performed using conventional welding methods. For this reason, in the present invention, the range of the bottom groove gap G is set to 7 mm or more and 18 mm or less, which is a range in which welding is difficult to perform using conventional welding methods and in which further high efficiency is expected. The range is preferably 8 mm or more and 12 mm or less.

[0022] In the present invention, the first layer and each of the layers after the second layer are welded and joined by multi-layer welding using two or more electrodes, using the narrow groove described above.

[0023] In the present invention, the groove processing of the thick steel plate is performed by gas cutting, plasma cutting, laser cutting, etc. However, mechanical processing is not excluded. The melting depth required for the groove surface in narrow-gap gas-shielded arc welding is mainly determined by the surface properties of the groove surface (particularly the recess depth and cleanliness). In the most common groove processing by gas cutting, except for special steels and stainless steels, the finish of the cut surface varies greatly depending on the gas flow rate and the nozzle selection during gas cutting. For example, when the gas flow rate and the nozzle are well adjusted, the recess depth on the groove surface is about 0.2 mm or less, but in special cases, such as when the flame flow rate is lower than usual due to wear of the nozzle, the recess depth may exceed 1 mm. However, even if such a recess occurs, it will be used for welding as it is without any maintenance in general structures, etc.

[0024] Therefore, in order to effectively prevent defects due to high-temperature cracking and incomplete fusion, it is necessary to melt the groove surface more deeply during welding, especially the bottom of the groove (thick steel plate) where the temperature during welding is low and the melting depth tends to be small. Also, since the cut surface is covered with a thick oxide film generated by processing heat, it is necessary to melt the groove surface more deeply during welding.

[0025] For this reason, in the present invention, the fusion depth at the bottom of the groove (thick steel plate) is limited to 1.5 mm or more. It is preferably 2.0 mm or more. However, if the fusion depth exceeds 4 mm, an undercut occurs at the top of the weld bead on the groove face, which can cause welding defects, so the fusion depth is preferably 4 mm or less.

[0026] In the present invention, the above-mentioned narrow groove is used to perform multi-layer welding of the first layer and each layer thereafter using multiple electrodes of two or more electrodes, and a welded joint is obtained by welding and joining while preventing defects such as insufficient fusion and welding defects under high welding efficiency. Note that in the present invention, the above-mentioned narrow groove is used and the welding conditions are appropriately adjusted so that the fusion depth p at the bottom of the groove (thick steel plate) is 1.5 mm or more.

[0027] [Multi-layer welding is defined as multi-electrode welding using two or more electrodes, with the first and second electrodes positioned along a predetermined parallel weld line] In the present invention, from the viewpoint of improving the efficiency of welding, multi-layer welding is performed using two or more electrodes, and preferably, from the viewpoint of hot cracking resistance, using four or less electrodes.

[0028] In narrow gap multi-pass welding, when one pass is performed per layer, with one electrode, the welding heat tends to concentrate at the center of the groove, which causes insufficient melting at the groove surface 2 of the thick steel plate 1, and defects due to poor fusion (cold lap) and spatter and slag inclusion on the groove surface are likely to occur. In particular, in the first layer welding, the temperature of the thick steel plate is low and the melting depth is small, so defects due to poor fusion are likely to occur. For this reason, in the present invention, among the multiple electrodes having two or more electrodes, the first and second electrodes are arranged at positions along a predetermined parallel welding line and welding is performed. The construction procedure for multi-pass welding with four electrodes is shown in Figure 2. Note that 7 is a backing material.

[0029] [One of the first and second electrodes is wire negative (positive polarity), and the other is wire positive (reverse polarity)] If the first and second electrodes are of the same polarity (for example, both the first and second electrodes are wire positive), the electromagnetic force of attraction will cause the arcs to be directed inward, and heat will be concentrated in the center of the groove. This will result in insufficient melting at the groove surface. On the other hand, if one of the first and second electrodes is wire negative (positive polarity) and the other is wire positive (reverse polarity), and the arrangement of the first and second electrodes is appropriately controlled, the magnetic fields due to the welding currents will generate strong outward electromagnetic forces, causing the arcs to repel each other. As a result, it will be possible to obtain sufficient melting depth at the groove surface.

[0030] For this reason, in the present invention, one of the first electrode and the second electrode is designated as a wire negative (positive polarity), and the other is designated as a wire positive (opposite polarity).

[0031] [Distance a between the tip of the welding wire supplied from the power feed tip at the tip of each welding torch of the first electrode and the second electrode: 5 mm or more and 16 mm or less] The distance a between the tips of the welding wires 3b, 4b supplied from the power feed tips 3a, 4a at the tip of each welding torch of the first electrode 3 and the second electrode 4 (hereinafter simply referred to as the "distance between the first and second electrodes"; see FIG. 2(b)) is adjusted to be in the range of 5 mm to 16 mm. Note that the "distance between the welding wire tips" here refers to the distance between the centers of the welding wire tips of each electrode.

[0032] If the distance a between the first and second electrodes is less than 5 mm, the heat of the arc itself is reduced by the current (electrons) flowing between the electrodes, and sufficient melting of the groove surface 2 is not achieved. On the other hand, if the distance a between the first and second electrodes exceeds 16 mm, the outward electromagnetic force between the electrodes decreases inversely proportional to the distance, and the arc repulsive force sufficient to overcome the inward electromagnetic force generated by the current flowing through the groove surface 2 is not obtained, so the arcs are directed inward and heat is concentrated at the center of the groove. As a result, sufficient melting of the groove surface 2 is not achieved.

[0033] In addition, in narrow gap welding, suppressing welding defects caused by spatter adhesion to the groove surface is an issue. However, the first electrode 3 and the second electrode 4 are arranged along the predetermined parallel welding lines 8, 8, one of which is wire negative (positive polarity) and the other is wire positive (reverse polarity), and the distance a between the first and second electrodes is adjusted to a range of 5 mm to 16 mm. This allows the spatter to be absorbed by the molten metals, suppressing the adhesion of spatter to the groove surface, making it possible to obtain a sound weld.

[0034] For this reason, the distance a between the tips of the welding wires supplied from the power feed tips at the tips of the welding torches of the first electrode 3 and the second electrode 4 is adjusted to a range of 5 mm to 16 mm. Note that in order to obtain deeper and more stable melting of the groove face by stronger repulsion of the arc, it is preferable to set the distance a between the first and second electrodes to a range of 5 mm to 8 mm.

[0035] [Angle α of the straight line connecting the tips of the welding wires of the first and second electrodes with respect to the perpendicular direction of the weld line: 60° or less] In the present invention, the repulsion of the arc is utilized to ensure melting of the groove surface. However, if the angle α of the straight line connecting the welding wire tips of the first electrode 3 and the second electrode 4 with respect to the perpendicular direction of the welding line exceeds 60°, a sufficient repulsive force of the arc cannot be obtained, and sufficient melting cannot be obtained at the groove surface. Therefore, the angle α of the straight line connecting the welding wire tips of the first electrode and the second electrode with respect to the perpendicular direction of the welding line (hereinafter, also simply referred to as the "first-second electrode arrangement angle", see FIG. 2(b)) is limited to 60° or less. It is preferably 45° or less. The first-second electrode arrangement angle α may be 0°.

[0036] [Welding wire supplied to the electrode with positive polarity: Steel wire containing 0.015 to 0.100 mass% REM (rare earth element)] REM (rare earth elements) are effective elements for refining inclusions during steelmaking and casting, and for improving the toughness of weld metal during welding. In addition, when welding is performed by supplying a welding wire containing REM to a positive electrode, it is possible to refine droplets and stabilize transfer. This refinement of droplet transfer suppresses the generation of spatter, and enables stable gas shielded arc welding even with positive polarity. For this reason, in the present invention, a steel wire containing 0.015 to 0.100 mass% of REM (rare earth elements) is supplied to the positive electrode. Note that elements other than REM (rare earth elements) are included in the appropriate amounts that are usually contained according to the grade (steel type) of the welding wire, as specified in JIS Z 3312.

[0037] If the REM (rare earth element) content is less than 0.015% by mass, the droplets cannot be made fine and the transfer cannot be stabilized. On the other hand, if the REM (rare earth element) content exceeds 0.100%, cracks occur during the wire manufacturing process, making it difficult to manufacture the welding wire. For this reason, the REM (rare earth element) content is limited to the range of 0.015 to 0.100% by mass. The REM content is preferably 0.025 to 0.050% by mass.

[0038] Welding wire for gas shielded arc welding is generally manufactured with a diameter in the range of 0.6 mm to 2.0 mm, but when welding with the same current, the thinner the wire diameter, the higher the deposition rate due to Joule heat. Therefore, it is preferable to select a relatively thin wire diameter to achieve highly efficient welding work. On the other hand, if the wire diameter is too thin, the wire will soften due to Joule heat, making the welding unstable. For this reason, it is preferable to use a diameter of the welding wire in the range of 1.0 mm to 1.6 mm.

[0039] The above-mentioned welding conditions are the basic welding conditions in the present invention, and by performing welding under such conditions, it is possible to obtain a welded joint having a weld metal portion capable of ensuring a fusion depth p of 1.5 mm or more from the groove face in the direction perpendicular to the weld line at the bottom of the groove.

[0040] In addition, in the present invention, by further satisfying the welding conditions shown below in addition to the basic welding conditions described above, it is possible to obtain a deeper and more stable fusion depth p from the groove face at the bottom of the thick steel plate in the narrow groove.

[0041] [The feed angle φ of the welding wire of the first electrode and the second electrode to the bottom groove: 0° to 15° with respect to the perpendicular] Arcs have a directivity and tend to point in the direction that the tip of the electrode (welding wire) points. To effectively utilize the directivity of the arc in melting the groove surface, it is advantageous to point the direction of the electrode tip toward the groove surface, and the direction of the electrode tip changes significantly depending on the feed angle φ of the welding wire supplied from the power feed tip at the tip of the welding torch. The feed angle φ of the welding wire supplied from the power feed tip at the tip of the welding torch to the bottom groove is shown in Figure 2(a). If the feed angle φ of the welding wires 3b and 4b supplied from the power feed tips 3a and 4a at the tip of the welding torch to the bottom groove is less than 0° with respect to the perpendicular line, the current flows through a path with less resistance. As a result, the arc creeps up the wire, which is the electrode (crawling up of the arc), making it difficult to maintain the targeted melting at the groove surface 2, especially at the bottom. On the other hand, if the feed angle φ of the welding wire supplied from the power feed tip to the bottom groove exceeds 15° with respect to the perpendicular line, the arc faces the groove surface 2 too much, so the shape of the weld bead becomes convex, and melting by the arc in the welding after the first layer becomes insufficient, which makes it easy to cause welding defects. For this reason, the feed angle φ of the welding wires 3b and 4b of the first electrode 3 and the second electrode 4 to each bottom groove is preferably in the range of 0° to 15° with respect to the perpendicular line. More preferably, it is 5° to 12°. The feed angle φ of the welding wires of the first electrode 3 and the second electrode 4 to each bottom groove is the same as the inclination of the power feed tips 3a and 4a, particularly the tip of the power feed tip, so that the feed angle φ of the welding wire can be controlled by the inclination of the tip of the power feed tip. The feed angle φ is defined as + in the direction facing the groove surface. The perpendicular line here refers to the perpendicular line to the bottom groove.

[0042] [Distance d between the side end of the welding wire tip of the first electrode and the second electrode and the groove surface of the thick steel plate: 0.5 mm or more and 3.0 mm or less] The distance d between the side end of the tip of the welding wire of the first electrode 3 and the second electrode 4 and the groove surface 2 of the thick steel plate is shown in FIG. 2(a). If the distance d between the side end of the tip of the welding wire 3b and 4b at the bottom groove and the groove surface 2 of the thick steel plate is less than 0.5 mm, an arc is generated between the upper part of the wire and the groove surface 2, and the groove surface 2 at the bottom of the thick steel plate cannot be efficiently melted. On the other hand, if it exceeds 3.0 mm, the arc is separated from the groove surface 2, and the groove surface 2 cannot be efficiently melted. For this reason, the distance d between the side end of the tip of the welding wire and the groove surface 2 of the thick steel plate is preferably 0.5 mm or more and 3.0 mm or less. More preferably, it is 0.5 to 2.0 mm, and even more preferably, it is 0.5 to 1.0 mm. The "side end of the tip of the welding wire" referred to here refers to the side end on the side close to the groove surface 2 of the thick steel plate to be melted by each electrode.

[0043] [Curvature radius of the welding wire fed to the power feed tips of the first electrode and the second electrode: 150 mm or more and 300 mm or less] In the present invention, a power feed tip with a bent tip is used to control the feed angle φ of the welding wires 3b and 4b fed from the power feed tips 3a and 4a at the tips of the welding torches of the first electrode 3 and the second electrode 4. At this time, the welding wire passes through the power feed tip with a bent tip, and in order to pass through it more smoothly, it is preferable to bend the welding wire in advance using a so-called three-point roller or the like.

[0044] If the radius of curvature of the welding wire is less than 150 mm, the wire feed resistance increases, the welding wire cannot be fed stably, and it becomes difficult to maintain the arc. On the other hand, if the radius of curvature of the welding wire exceeds 300 mm, the wire feed resistance is not effectively reduced when the tip of the power feed tip is bent, so the welding wire cannot be fed stably and it becomes difficult to maintain the arc. For this reason, the radius of curvature of the welding wires 3b and 4b fed to the power feed tips 3a and 4a of the first electrode 3 and the second electrode 4 is preferably 150 mm or more and 300 mm or less. More preferably, it is 175 mm or more and 275 mm or less.

[0045] [Third and subsequent electrodes: placed in the center of the groove behind the first and second electrodes, and distances b and c from adjacent preceding electrodes: 10 mm to 100 mm] If the weld build-up height H exceeds the bottom groove gap G in the first layer welding, the risk of hot cracking increases. To avoid this, it is effective to position the third electrode 5 and subsequent electrodes (third electrode 5 and fourth electrode 6 in the example of Figure 2) in the center of the groove behind the first electrode 3 and second electrode 4. This also makes it possible to further reduce the number of layers, greatly reducing the risk of stacking defects in multi-layer welding. Note that the "groove center" is allowed to be within a range of ±10% of the groove gap G from the center of the groove.

[0046] From the viewpoint of hot cracking resistance, it is preferable to arrange the third electrode 5 and subsequent electrodes at a distance of 10 mm to 100 mm from the adjacent preceding electrodes. Here, the distance between the adjacent preceding electrodes refers to the distance b between the tip of the welding wire 4b of the second electrode 4 and the tip of the welding wire 5b of the third electrode 5, and the distance c between the tip of the welding wire 5b of the third electrode 5 and the tip of the welding wire 6b of the fourth electrode 6, as shown in Fig. 2(b). The polarity of the third electrode 5 and subsequent electrodes is not particularly limited, and may be either wire negative (positive polarity) or wire positive (reverse polarity).

[0047] [Shielding gas: mixed gas containing 60% or more CO2 gas by volume] Since the amount of oxygen in the weld metal is also greatly affected by the shielding gas composition, the shielding gas used in the gas-shielded arc welding of the present invention is preferably a mixed gas containing 60 volume % or more CO2 gas and the remainder an inert gas such as Ar. More preferably, it is 100 volume % CO2 gas. In the present invention, it is preferable to increase the oxygen concentration in the weld metal, which controls the flow of the weld metal, and direct the convection of the weld metal from the center outward to stably deepen the molten depth at the bottom of the thick steel plate in the groove.

[0048] The other conditions are not particularly limited and may be in accordance with established standards, such as welding current: 280-360 A, welding voltage: 32-37 V (increases with current), welding speed: 30-90 cm / min, wire extension length: 15-30 mm, and welding heat input per pass: 10-50 kJ / cm.

[0049] The present invention will be further described below with reference to examples. EXAMPLES

[0050] For various steel plates of the steel types (grades) shown in Table 1, grooves were processed by gas cutting so as to have the groove shapes shown in Figure 1 and Table 2. Note that no preparation such as grinding was performed on the groove surface 2. For the processed groove surface 2, a laser displacement meter was used to measure the surface quality of the groove surface 2, and the maximum recess depth was determined, which is shown in Table 2.

[0051] For a thick steel plate (length: 500 mm) with a groove shape shown in Table 2, narrow-gap gas-shielded arc welding was performed as the first layer welding under the welding conditions shown in Tables 3 and 4 using welding wire (steel wire) of the steel type (grade) shown in Table 1. Multi-layer welding was then performed from the second layer onwards to obtain a narrow-gap gas-shielded arc-welded joint (welding length: 500 mm). The welding conditions for the second layer onwards were the same as those for the first layer. The electrode with positive polarity was supplied with REM-containing welding wire as shown in Table 3. The third and fourth electrodes were both placed in the center of the groove behind the first and second electrodes, and were set so that the distance between them and the adjacent leading electrodes was in the range of 10 to 100 mm.

[0052] The obtained welded joint was cut into five cross sections in the longitudinal direction, and the bottom fusion width wi (w1 to w5) was measured for each cross section (cross section 1 to cross section 5) as shown in Figure 3. For each cross section, the length of the bottom groove gap G was subtracted from the fusion width wi obtained for each cross section, and the obtained value was divided by 2 to determine the fusion depth pi (p1 to p5) for that cross section. The average value for the five cross sections was calculated, and this average value was determined as the bottom fusion depth p of the welded joint. The results are shown in Table 4.

[0053] The welded joints obtained were subjected to ultrasonic inspection to evaluate the presence or absence of weld defects. The cases where no defects were detected were marked with a ◎, the cases where only passable defects with a length of 3 mm or less were detected were marked with a 〇, and the cases where defects with a length of more than 3 mm were detected were marked with an ×. The results are shown in Table 4.

[0054] [Table 1]

[0055] [Table 2]

[0056] [Table 3]

[0057] [Table 4]

[0058] In all of the examples of the present invention, even when narrow-gap multi-layer welding was performed using multi-electrode welding with two or more electrodes, the bottom fusion length was 1.5 mm or more. In addition, even without groove surface preparation, no welding defects were detected, resulting in a sound narrow-gap gas-shielded arc-welded joint, and it can be seen that the welding construction efficiency was improved. On the other hand, in the comparative examples outside the scope of the present invention, the bottom fusion length was less than 1.5 mm, or welding defects were detected, and a sound narrow-gap gas-shielded arc-welded joint was not obtained. [Explanation of symbols]

[0059] 1 thick steel plate 2 Bevel surface 3 1st electrode 4 Second electrode 5 Third electrode 6 4th electrode 3a, 4a, 5a, 6a Power supply chip 3b, 4b, 5b, 6b welding wire 7 Backing material 8 Welding seam 9 First layer weld bead 10 Molten pool (second layer) 11 Weld bead during welding (second layer)

Claims

1. A narrow-gap gas-shielded arc welding method for thick steel plates, in which a thick steel plate having a plate thickness t of 22 mm or more is joined by multi-layer welding with a narrow groove having a groove angle θ of 25° or less and a bottom groove gap G of 7 to 18 mm, The multi-layer welding is performed by multi-electrode welding using two or more electrodes, Among the multiple electrodes, a first electrode and a second electrode are disposed at positions along a predetermined parallel welding line, and one of the first electrode and the second electrode is a wire negative (positive polarity) and the other is a wire positive (reverse polarity); Furthermore, the distance a between the tips of the welding wires supplied from the power feed tips at the tips of the welding torches of the first electrode and the second electrode is set in the range of 5 mm to 16 mm, and the angle α of a straight line connecting the tips of the welding wires of the first electrode and the second electrode with respect to a direction perpendicular to the welding line is set in the range of 60° or less, The welding wire to be supplied to the electrode having a positive polarity is a steel wire containing 0.015 to 0.100 mass% of REM (rare earth element), The fusion depth p in the direction perpendicular to the weld line at the bottom of the thick steel plate is 1.5 mm or more, The third electrode and subsequent electrodes are disposed in the center of the groove behind the first electrode and the second electrode, and the inter-electrode distance from the second electrode and subsequent electrodes is set in the range of 10 mm to 100 mm. A narrow gap gas shielded arc welding method for thick steel plates.

2. 2. The narrow gap gas-shielded arc welding method for thick steel plate according to claim 1, wherein each feed angle φ of the welding wire of the first electrode and the second electrode with respect to the bottom groove is set to be 0° or more and 15° or less with respect to the perpendicular line.

3. 3. The narrow gap gas-shielded arc welding method for thick steel plate according to claim 1, wherein the distance d between the side end of the welding wire tip of the first electrode and the groove surface of the thick steel plate is set to 0.5 mm or more and 3.0 mm or less, respectively.

4. 3. The narrow gap gas-shielded arc welding method for thick steel plate according to claim 1, wherein the welding wire fed to the power feed tips of the first electrode and the second electrode is curved with a radius of curvature in the range of 150 mm to 300 mm.

5. 4. The narrow gap gas-shielded arc welding method for thick steel plate according to claim 3, wherein the welding wire fed to the power feed tips of the first electrode and the second electrode is curved with a radius of curvature in the range of 150 mm to 300 mm.

6. The shielding gas in the gas-shielded arc welding process is 60% or more by volume of CO. 2 3. The narrow gap gas shielded arc welding method for thick steel plates according to claim 1, wherein a mixed gas containing a gas is used.

7. The shielding gas in the gas-shielded arc welding process is 60% or more by volume of CO. 2 4. The narrow gap gas shielded arc welding method for thick steel plates according to claim 3, characterized in that a mixed gas containing a gas is used.

8. The shielding gas in the gas-shielded arc welding process is 60% or more by volume of CO. 2 5. The method for narrow gap gas-shielded arc welding of thick steel plates according to claim 4, characterized in that a mixed gas containing a gas is used.

9. The shielding gas in the gas-shielded arc welding process is 60% or more by volume of CO. 2 6. The method for narrow gap gas-shielded arc welding of thick steel plates according to claim 5, characterized in that a mixed gas containing a gas is used.

Citation Information

Patent Citations

  • Process for the submerged arc welding of metallic materials in a narrow gap

    DE3136526A1

  • JP1972003881U

  • Atsuenkyohiatsuentaiannaibuzai

    JP1976023461A

  • Tadenkyoku mig jidoyosetsuho

    JP1976106658A

  • Preparation of cake

    JP1986037053A