Method for suppressing fatigue crack generation in welded parts and method for manufacturing welded joints

JP7593434B2Active Publication Date: 2024-12-03JFE STEEL CORP
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
JP2023067776
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2022-04-26
Filing Date
2023-04-18
Publication Date
2024-12-03
Estimated Expiration
2043-04-18

Smart Images

  • Figure 0007593434000002
    Figure 0007593434000002
  • Figure 0007593434000003
    Figure 0007593434000003
  • Figure 0007593434000004
    Figure 0007593434000004
Patent Text Reader

Abstract

To provide a method for suppressing fatigue crack initiation of a weld zone to improve fatigue strength of a thick material, by processing struck marks corresponding to two lanes in which no fatigue crack occurs, and a method for manufacturing a weld joint that is executed using the method.SOLUTION: In a method for suppressing fatigue crack initiation of a weld zone, a base material part near a weld toe is struck continuously along weld bead to form a first lane that is a belt-like struck mark and further the outside of the base material part is struck to form a second lane that is a belt-like struck mark. Further, it is preferable that when a distance between the weld toe and the struck mark that is the first lane is defined as L1 and a distance between the struck mark that is the first lane and the struck mark that is the second lane is defined as L2, a relational expression of 0.0 mm<L1≤1.0 mm, 0.0 mm≤L2≤2.0 mm is satisfied.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a method for suppressing fatigue crack generation in a welded portion and a method for manufacturing a welded joint. In particular, the present invention relates to a method for suppressing fatigue crack generation in a welded portion and improving fatigue strength in, for example, a monopile in the offshore wind power field by performing a two-lane hammer peening impact treatment on a base material portion to impart a large compressive residual stress. Furthermore, the present invention relates to a method for manufacturing a welded joint constructed using the method. [Background technology]

[0002] In recent years, the monopile type has been considered in the offshore wind power field to reduce construction costs. In addition, generators are becoming larger in size to reduce power generation costs and increase power generation efficiency, and the monopiles that support them are also becoming larger. The thickness of the steel plate used in this monopile is, for example, in the range of 30 to 100 mm. However, since there is a limit to the loading capacity of the laying ship that transports the monopile, there is an increasing demand for reducing the thickness by applying high-strength materials to the monopile. The application of high-strength materials makes it possible to design with higher stress than the current design stress, but in that case, there is a concern that the fatigue strength of the butt circumferential welds of the monopile will decrease.

[0003] As a technique for improving the fatigue strength of welds, Patent Document 1 discloses a hammer peening method for striking a base material. The hammer peening method described in Patent Document 1 specifies that the maximum depth of the impact indentation is 0.2 mm or more. However, the method of Patent Document 1 has a problem in that the width of the impact indentation is narrow, and the deeper the impact indentation, the more likely it is that a fatigue crack will occur due to the stress concentration caused by the formation of the impact indentation. [Prior art documents] [Patent documents]

[0004] [Patent Document 1] Patent No. 5955752 Summary of the Invention [Problem to be solved by the invention]

[0005] In the conventional impact hammer peening method for a base material, as the plate thickness of the target welded joint increases, the depth of the impact marks can be increased without limit, so there is a possibility that fatigue cracks may occur from the impact marks. Therefore, a method for constructing impact marks that improves fatigue strength without generating fatigue cracks was explored.

[0006] An object of the present invention is to solve the problems of the prior art and provide a method for improving the fatigue strength of thick members by treating impact marks that do not generate fatigue cracks for two lanes, and a method for manufacturing a welded joint constructed using this method.

Means for Solving the Problems

[0007] The inventors of the present invention conducted intensive studies to achieve the above object. Test pieces were collected from the butt welded joints of thick members, and fatigue tests were carried out using test pieces in which the base material impact for one lane was processed by hammer peening treatment and test pieces in which the treatment was carried out for two lanes. By comparing the results of these fatigue tests, it was newly found that the fatigue strength is improved by the base material impact hammer peening when the treatment is carried out for two lanes.

[0008] Based on such findings, the present invention was further studied and completed, and the gist of the present invention is as follows. 〔1〕A method for suppressing the occurrence of fatigue cracks in a welded part, characterized in that the base material part near the weld termination is continuously struck along the weld bead of the welded part to form a first lane which is a strip-shaped impact mark, and further the outside thereof is struck to form a second lane which is a strip-shaped impact mark. A method for suppressing the occurrence of fatigue cracks in a welded part. 〔2〕In the above 〔1〕, when the distance between the weld termination and the impact mark of the first lane is L1, and the distance between the impact mark of the first lane and the impact mark of the second lane is L2, 0.0 mm < L1 ≤ 1.0 mm, 0.0 mm ≤ L2 ≤ 2.0 mm. A method for suppressing the occurrence of fatigue cracks in a welded part. 〔3〕In the above 〔1〕 or 〔2〕, the maximum depth (D of the impact markP ) and width (W P ) product (D P ×W P ) is 3.0~5.0mm 2 A method for suppressing fatigue crack occurrence in a welded portion, comprising: [4] A method for suppressing the occurrence of fatigue cracks in a welded portion according to [1] or [2] above, characterized in that the base material portion of the welded portion is a butt welded joint having a plate thickness of 30 mm or more. [5] The method for suppressing fatigue crack occurrence in a welded portion according to [3] above, characterized in that the base material portion of the welded portion is a butt welded joint having a plate thickness of 30 mm or more. [6] A method for manufacturing a welded joint, characterized in that the method for suppressing fatigue crack occurrence in a welded joint described in [1] or [2] above is used. [7] A method for manufacturing a welded joint, characterized in that it is carried out using the method for suppressing fatigue crack occurrence in a welded portion described in [3] above. [8] A method for manufacturing a welded joint, characterized in that it is carried out using the method for suppressing fatigue crack occurrence in a welded portion described in [4] above. [9] A method for manufacturing a welded joint, characterized in that the method for suppressing fatigue crack occurrence in a welded portion described in [5] above is used. Effect of the Invention

[0009] According to the two-lane base material striking of the present invention, it is possible to improve the fatigue strength of thick-walled materials more than by one-lane base material striking, which is extremely effective in industry. [Brief description of the drawings]

[0010] [Figure 1] FIG. 2 is a schematic diagram showing a two-lane hammer peening method according to the present invention. [Diagram 2] FIG. 2 is a perspective view illustrating an example of a tip portion of a chipper used in a hammer peening process according to the present invention, illustrating X, Y, and Z directions. [Diagram 3] 1A and 1B are schematic diagrams illustrating the shape of an XZ cross section and a YZ cross section, respectively, of an example of a tip portion of a chipper used in a hammer peening process according to the present invention. [Figure 4]It is a schematic diagram explaining the four-point bending fatigue test method.

Mode for Carrying Out the Invention

[0011] The present invention is a method of continuously striking the base metal part in the vicinity of the welding termination part for two lanes with a chipper, introducing compressive residual stress into the welding termination part, and improving the fatigue strength of the welded joint more than the striking for one lane.

[0012] Hereinafter, embodiments of the present invention will be described.

[0013] [Two-lane Striking] As described above, in order to improve the fatigue strength of the welded joint, the present invention forms striking marks for two lanes and introduces compressive residual stress in the vicinity of the welding termination part. Specifically, the base metal part in the vicinity of the welding termination part is continuously struck along the welding bead of the welded part to form a first lane which is a band-shaped striking mark, and further the outside thereof is struck to form a second lane which is a band-shaped striking mark. Here, when the distance between the welding termination part and the striking mark of the first lane is L1, and the distance between the striking mark of the first lane and the striking mark of the second lane is L2, it is preferable that 0.0 mm < L1 ≤ 1.0 mm and 0.0 mm ≤ L2 ≤ 2.0 mm. Also, the product (D P ) of the maximum depth (D P ) and the width (W P ) of the striking mark (D P ) × W 2 ) is preferably 3.0 to 5.0 mm.

[0014] In addition, the compressive residual stress is measured based on the ASTM E837 standard (hole drilling method). This measurement of residual stress by the hole drilling method is a measurement method for obtaining the residual stress by evaluating the amount of deformation before and after the stress is released by making a hole in the test piece.

[0015] Here, as the residual stress, -400 to -200 MPa is a preferable range for suppressing the occurrence of fatigue cracks.

[0016] Hereinafter, it will be described based on FIG. 1.

[0017] First, it is preferable that the distance (L1) between the welding stop end 3 and the impact mark 4 in the first lane is greater than 0.0 mm and equal to or less than 1.0 mm. That is, the distance (L1) from the welding stop end 3, which is the boundary between the weld metal 2 and the base material 1 of the welded joint formed by butt-welding the base materials (hereinafter also referred to as "base material parts") 1, to the position where the tip of the chipper, which is an impact pin, contacts the base material 1 is preferably equal to or less than 1.0 mm. If the distance (L1) exceeds 1.0 mm, the impact mark 4 in the first lane will be separated from the welding stop end 3, making it difficult to introduce the compressive residual stress in the vicinity of the welding stop end 3, and thus the fatigue strength of the welded joint cannot be improved. Also, since the impact of the chipper should not hit the welding stop end 3 and it is preferable that the distance (L1) is greater than 0.0 mm, it is preferable that the distance (L1) satisfies 0.0 mm < L1 ≤ 1.0 mm.

[0018] In addition, when manually performing the hammer peening process, it is preferable to pre-draw a grid with a marker.

[0019] Next, the outside of the impact mark 4 in the first lane is struck to form a strip-shaped impact mark 5 in the second lane. At this time, the distance (L2) between the impact mark 4 in the first lane and the impact mark 5 in the second lane is preferably 0.0 - 2.0 mm. In the case of the distance (L2), it is acceptable even if it hits the impact mark 4 in the first lane, so it may be 0.0 mm or more. Also, if it exceeds 2.0 mm, the impact mark 5 in the second lane will be separated from the welding stop end 3, making it difficult to introduce the compressive residual stress in the vicinity of the welding stop end 3, and thus the fatigue strength of the welded joint cannot be improved.

[0020] Next, for both the impact mark 4 and the impact mark 5, the product (D P ) of the maximum depth (D P ) of the impact mark, which is the cross-sectional area in the depth direction of each impact mark, and the width (W P ) of the impact mark (D P ) is preferably 3.0 - 5.0 mm 2 . The product (D P ) of the maximum depth (D P ) and the width (W P ) of the impact mark (DP ) is 3.0 mm 2 If it is less than 5.0 mm, sufficient compressive residual stress cannot be imparted. 2 If the product (D P ×W P ) is 3.0~4.0mm 2 It is.

[0021] [Welded joint manufacturing method, welding method] Next, a specific example of the manufacturing method and welding method for a welded joint according to the present invention will be described.

[0022] The type of steel for the steel plate that becomes the base material 1 is, for example, SM490, and the tensile strength is preferably in the range of 400 MPa to 600 MPa.

[0023] The plate thickness is intended to be a thick steel plate suitable for monopiles, which is the object of the present invention, and specifically, is preferably 30 mm or more, and more preferably 50 to 100 mm.

[0024] The base material is double-sided multi-layer welded by gas-shielded arc welding using carbon dioxide gas under welding conditions of a heat input of 0.6 to 1.0 kJ / mm to produce a butt welded joint.

[0025] [Hammer peening method] The obtained butt welded joint is subjected to a hammer peening treatment to impart compressive residual stress to the base material 1 in the vicinity of the weld toe.

[0026] After forming the above-mentioned welded joint, as shown in Fig. 1, the base metal portion 1 in the vicinity of the weld toe 3 is struck (peened) to form a band-shaped first lane impact mark 4, and a band-shaped second lane impact mark 5 is formed outside of it. As described above, the range is preferably such that the distance (L1) between the weld toe 3 and the first lane impact mark 4 is greater than 0.0 mm and not more than 1.0 mm, and the distance (L2) between the first lane impact mark 4 and the second lane impact mark 5 is 0.0 to 2.0 mm. In addition, the maximum depth (D P ) and width (WP ) product (D P ×W P ) is 3.0~5.0mm 2 If the stress is outside this range, the range in which compressive residual stress is introduced is small, and it is not possible to exert the effect of preventing fatigue cracks from occurring from the weld toe 3. Here, the treatment is performed so that the residual stress is in the range of -400 to -200 MPa.

[0027] [Chipper] The chipper, which is an impact tool, is preferably a square prism with a semicircular curved surface at the bottom end, and the area of ​​the impact mark is preferably impacted with the semicircular curved surface. The tip of the chipper may be spherical, rectangular, or of a similar shape. The thickness (width) of the tip is preferably in the range of 1.0 to 10.0 mm.

[0028] An example of the tip shape of the chipper is shown in Fig. 2 and Fig. 3. Fig. 2 is a perspective view for explaining the X, Y and Z directions when the X direction is defined as a direction perpendicular to the direction of advance of the impact (direction perpendicular to the weld line direction) and the Y direction is defined as the direction of advance of the impact (direction parallel to the weld line direction). Fig. 3(a) is a diagram of a cross section (XZ cross section) of the tip of the chipper perpendicular to the chipper advance direction (Y direction), and Fig. 3(b) is a diagram of a cross section (YZ cross section) parallel to the chipper advance direction (Y direction). In the example of the chipper shown here, the thickness (width) of the tip of the XZ cross section is a (mm), has an arc-shaped outer periphery with a curvature radius of r (mm), and the tip of the YZ cross section has a kamaboko shape with a length of b (mm). The length a of the XZ cross section and the length b of the YZ cross section are both preferably in the range of 1.0 to 10.0 mm. More preferably, they are in the range of 5.0 to 9.5 mm. The above-mentioned radius of curvature r is preferably 1.0 to 10.0 mm. If it is less than 1.0 mm, deformation that easily causes stress concentration at the weld toe is likely to be formed, and if it exceeds 10.0 mm, the contact area between the chipper and the weld toe during impact becomes too large, making it difficult to introduce sufficient compressive residual stress into the weld toe.

[0029] This chipper is connected to an impact device, which is driven by air pressure, high-frequency current, ultrasonic waves, etc. For example, a method is preferred in which the tip of the semi-cylindrical shape is operated by air pressure to impact the aforementioned area. Here, the impact frequency is preferably a low frequency of 100 Hz or less.

[0030] In addition, the maximum depth of the impact mark (D P ) and width (W P ) product (D P ×W P ) is 3.0~5.0mm 2 It is preferable to control the temperature so as to be within the range.

[0031] Furthermore, the inclination angle (θ) of the impact direction of the chipper is permissible if it is about 80 to 100° with respect to the base material surface, but it is preferable that it is approximately perpendicular, that is, 90°. EXAMPLES

[0032] The test material used was SM490B. The plate thickness was 50 mm. The test material was double-sided welded by gas shielded arc welding under the following welding conditions (heat input 0.8 kJ / mm) to produce a butt welded joint. Young's modulus E and Poisson's ratio v were measured as properties of the welded joint. Test pieces were taken from the butt welded joint, and one was subjected to one lane of hammer peening and one was subjected to two lanes of hammer peening. A four-point bending fatigue test was conducted on each test piece.

[0033] [Gas shielded arc welding conditions] Shielding gas: CO2 Welding heat input: 0.8kJ / mm, welding current: 310A, welding voltage: 40V Welding speed: 29.5cm / min Welding wire composition: C: 0.07wt%, Si: 0.37wt%, Mn: 1.11wt%, P: 0.013wt%, S: 0.009wt%, Mo: 0.37wt% Welding wire diameter: 1.2mm

[0034] [Method of measuring Young's modulus and Poisson's ratio] The Young's modulus and Poisson's ratio were measured in accordance with ASTM E8M "Method of tensile testing for metallic materials."

[0035] [Four-point bending fatigue test] The four-point bending fatigue test method used a fatigue testing device 10 as shown in Fig. 4, in which stress was repeatedly applied to a fatigue test piece 11, and a fatigue test was performed by bending the fatigue test piece 11 at four points (two upper supports 12 on the upper side and two lower supports 13 on the lower side). That is, an impact was applied from above the fatigue testing device 10, and the number of loading cycles until the fatigue test piece 11 broke was determined. The nominal stress range (MPa) is the difference between the maximum stress and the minimum stress.

[0036] The measurement and test results are shown in Table 1.

[0037] [Table 1]

[0038] Nos. 1 and 2 are test results when one lane was subjected to hammer peening as a comparative example, and Nos. 3 to 6 are test results when two lanes were subjected to hammer peening according to the present invention. The test results when two lanes were subjected to hammer peening showed that the fatigue life was more than twice as long (improvement by one grade on the fatigue design curve) compared to the test results when one lane was subjected to hammer peening.

[0039] On the other hand, the maximum depth and width product is 6.0 mm 2 In No. 7, which was the conventional method of striking the base material, a fatigue crack occurred from the impact mark.

[0040] Furthermore, No. 8 is a comparative example in which the product of the depth and width of the impact mark is small.

[0041] No.9: The product of the depth and width of the impact mark is 6.0 mm 2In this large example, impact treatment for two lanes created compressive residual stress, improving fatigue strength slightly.

[0042] As described above, by forming two lanes of impact indentations along the weld bead, the present invention prevents fatigue cracks from occurring from the impact indentations and exhibits a greater fatigue strength improvement effect than that achieved by one lane of impact indentations. [Explanation of symbols]

[0043] 1 Base metal (base metal part) 2. Weld metal 3 Weld Toe 4 Impact marks on lane 1 5 Impact marks on the second lane 10. Fatigue Testing Equipment 11 Fatigue test specimen 12 Upper Support Point 13 Lower fulcrum 14 Loading fixture 15 Receiving jig L1 Distance between the weld toe and the impact mark in the first lane L2 Distance between the first lane impact mark and the second lane impact mark

Claims

1. A method for suppressing the occurrence of fatigue cracks in a welded portion, comprising the steps of: striking a base material portion near a weld toe of the welded portion continuously along a weld bead of the welded portion to form a first lane which is a band-shaped impact mark; and striking the outside of the first lane to form a second lane which is a band-shaped impact mark. a distance between the weld toe and the impact mark of the first lane is L1, and a distance between the impact mark of the first lane and the impact mark of the second lane is L2, 0.0 mm<L1≦1.0 mm and 0.0 mm≦L2≦2.0 mm; The maximum depth of the impact mark (D P ) and width (W P ) product (D P ×W P ) is 3.0 to 5.0 mm 2 A method for suppressing fatigue crack occurrence in a welded portion, comprising:

2. 2. The method for suppressing fatigue crack occurrence in a welded portion according to claim 1, wherein the base material portion of the welded portion is a butt welded joint having a plate thickness of 30 mm or more.

3. A method for manufacturing a welded joint, comprising the method for suppressing fatigue crack initiation in a welded portion according to claim 1 or 2.

Citation Information

Patent Citations

  • Control system of printing press

    JP1984055752A

  • Mitigating method of welding residual stress

    JP1995328788A

  • Straightening method of distortion and welded structure using it

    JP2006175511A

  • Welded structure of thick steel plate

    JP2009113080A

  • Peening construction method and weld joint using the same

    JP2011167693A