Granulation method
The granulation method addresses the issues of brittle granules and skilled labor dependency by using a rotating bed granulator to produce strong, large-particle granules efficiently, enhancing productivity and reducing drying requirements.
Patent Information
- Application Number
- JP2021011169
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2021-01-27
- Publication Date
- 2024-12-03
- Estimated Expiration
- 2041-01-27
AI Technical Summary
Existing granulation methods using pan pelletizers or drum pelletizers result in brittle granules with high moisture content, requiring lengthy drying and curing times, and rely on skilled labor, leading to poor productivity and insufficient granule strength.
A granulation method using a kneading machine and a granulator with a rotating bed section to knead and granulate fine powder dust from stainless steel furnaces, adjusting water content and rotation speed to produce granules with a particle size of 4.75 mm or more and a strength of 3.0 kg/cm², eliminating the need for skilled labor and reducing drying time.
The method achieves granules with high strength and productivity, allowing 95% or more of particles to be 4.75 mm or larger, significantly improving handling properties and reducing production costs by eliminating the need for prolonged drying and curing.
Smart Images

Figure 0007593594000003 
Figure 0007593594000004 
Figure 0007593594000005
Abstract
Description
[Technical field]
[0001] The present invention relates to a granulation method using a raw material containing powder dust. [Background technology]
[0002] It has been known that powder dust is generated from electric furnaces used for melting / oxidation refining stainless steel. This powder dust is a fine powder with a particle size of 10 μm or less, so there is no application for which it can be used as is. In addition, it may contain elements that are harmful to the environment, such as Cr. For this reason, most of this dust is treated as industrial waste, and it has been pointed out that it cannot be easily disposed of in landfills, and disposal costs are required.
[0003] Furthermore, since Ni, Cr, Fe, etc. contained in the powder dust are valuable metals, it is important to find applications that can maximize the intrinsic value of these elements from the perspective of effective utilization of metal resources. However, in order to recover such valuable metals, it is preferable to granulate the powder dust into a granulated material that is easy to use. In order to solve the above problems, it has already been considered to collect the powder dust, granulate it into a larger particle size, and use it for new purposes other than disposal. For granulating such powder dust, the first thing that comes to mind is the use of a granulation method using a conventional pan pelletizer or drum pelletizer.
[0004] However, granulation methods using pan pelletizers or drum pelletizers require many operational variables, such as the angle of the granulator (which affects the growth of the granules), the position and amount of water added, and scraping off semi-granules that have adhered to unintended parts of the equipment. As a result, only experienced workers can perform satisfactory granulation, making them unsuitable for obtaining granules from powder dust. Therefore, techniques for granulation without using such general pan pelletizers or drum pelletizers have been developed as disclosed in Patent Documents 1 to 3.
[0005] For example, Patent Document 1 discloses a granulation method for sintering raw materials that uses a sintering raw material mainly composed of fine powder (raw material containing 60% by mass or more of particles with a particle size of under 500 μm), and that can granulate granules having a target particle size distribution at a higher yield than conventional methods. The granulation method of Patent Document 1 is a method that can carry out two steps, kneading and granulation, in a single device, and is defined as follows: the inner diameter of the horizontal vessel is D (m), the peripheral speed of the stirring blade is u (m / s), and the gravitational acceleration of the sintering raw material is G (m / s) 2 ), the stirring acceleration of the impeller is 2×u2 / D(m / s 2 ) to 2G (m / s 2 ) or more 10G(m / s 2 ) is set within the following range.
[0006] Furthermore, Patent Document 2 discloses a method for granulating a sintering raw material mainly composed of fine powder (a raw material containing 60 mass% or more of particles with a particle size exceeding 0 μm and 250 μm or less), which can produce granulated products having a target particle size distribution at a higher yield than conventional methods. Furthermore, Patent Document 3 discloses a recycling method in which zinc-containing converter dust generated in the converter process during steel production is separated into dust with a low zinc content (dust with an average particle size in the range of 8 μm to 25 μm and a zinc content of 1 mass % or less) and dust with a high zinc content, and then efficiently recycled to a blast furnace, converter, or electric furnace. The recycling method of Patent Document 3 is said to make it possible to reduce the cost required for dezincing treatment. [Prior art documents] [Patent documents]
[0007] [Patent Document 1] JP 2009-242939 A [Patent Document 2] JP 2009-287122 A [Patent Document 3] Republished WO08 / 032638 Summary of the Invention [Problem to be solved by the invention]
[0008] However, granules produced using a pan pelletizer or drum pelletizer have the following problems. That is, granules produced using a pan pelletizer or drum pelletizer contain a large amount of water. Granules containing a lot of water are brittle, so in order to use the granules, it is necessary to remove the water and increase the strength of the granules. Specifically, when the strength of the granules is 3.0 kg / cm 2 In order to stably satisfy the above requirements, it is essential to remove moisture by drying or other methods to improve the strength of the granules. In other words, granulators such as pan pelletizers and drum pelletizers need to ensure a certain number of storage (curing) days until the moisture is removed and the strength is improved, and the productivity is reduced by the amount of storage required to remove the moisture.
[0009] In addition, since the working population is expected to decrease in the future, it is desirable to be able to granulate without relying on the skills of experienced workers. In this respect, pan pelletizers and drum pelletizers that rely on the skills of experienced workers are not preferable. On the other hand, the granulation method of Patent Document 1, which is a technology that does not use a general pan pelletizer or drum pelletizer, is said to be able to improve the yield of granulated material having a targeted particle size distribution by growing the granulated material until it reaches a targeted particle size, and for this reason, the stirring acceleration of the stirring blades, etc. are specified. However, since no consideration is given to the strength of the granulated material, it is not possible to realize high granulated material strength or good productivity.
[0010] Furthermore, even in the granulation method of Patent Document 2, the rotation speed of the granulator is low at about 20 rpm, and it is hard to imagine that granulated material with excellent strength can be obtained with such low-speed rotation. Furthermore, the recycling method of Patent Document 3 also uses fine dust with an average particle size of 8 μm or more and 25 μm or less as raw material, but does not consider the rotation speed of the granulator, and at least it cannot be considered that the strength of the granulated material is sufficient.
[0011] In other words, none of the methods in Patent Documents 1 to 3 can produce granulated materials with sufficient strength. Therefore, a semi-automatic device with few operating factors is used to produce granulated materials with a predetermined strength, i.e., 3.0 kg / cm that cannot be crushed by fingers. 2 There was a need to establish a technology that could produce granules with the above strength from fine dust generated in stainless steel smelting furnaces and other sources. The present invention has been made in view of the above problems, and is a method for producing a steel sheet having a strength of 3.0 kg / cm from fine dust. 2 The object of the present invention is to provide a granulation method capable of granulating the above granules with good productivity so that the proportion of granules having a particle size of 4.75 mm or more is 95% or more. [Means for solving the problem]
[0012] In order to solve the above problems, the delivery body of the present invention employs the following technical measures. That is, the granulation method of the present invention is Generated from electric furnaces that melt stainless steel or that oxidize and refine stainless steel Particle size 20μm or less The powder dust is used as the raw material. The raw materials are mixed with water in a mixer so that the water content is more than 10 mass% and less than 12 mass% of the total amount. The above Raw materials, every minute 60 ~ 90 The raw material is fed into a granulator equipped with a granulation chamber having a rotating bed and a fixed side wall, and the raw material is granulated while rotating the rotating bed in the granulation chamber for 2 minutes or more. The proportion of particles with a diameter of 4.75 mm or more among all particles is 95% or more. The method is characterized in that a granulated product is obtained.
[0013] N Preferably, the powdered raw material contains FeO: 0.1 to 10 mass%, Fe 2 O 3 :25~45mass%, CaO:2~15mass%, SiO2 : 5~15mass%, Al 2 O 3 :0.1~15mass%, MgO:0.1~5mass%, MnO:2~15mass%, Cr 2 O 3 It is preferable to use one containing 10 to 20 mass% of Cr, with the remainder being iron and unavoidable impurities, and having a particle size of 20 μm or less.
[0014] It is preferable that all of the primary particles of the powdery raw material have a diameter of 10 μm or less. Effect of the Invention
[0015] According to the granulation method of the present invention, the strength of the granulation can be increased from fine dust to 3.0 kg / cm 2 The above granulated material can be granulated with good productivity so that the ratio of particles having a particle size of 4.75 mm or more is 95% or more. Note that the raw material for the granulated material in the present invention is not limited to powder dust from a stainless steel manufacturing process, but can be widely applied to fine dust having a particle size of 20 μm or less, such as converter dust. [Brief description of the drawings]
[0016] [Figure 1] FIG. 1 is a diagram showing a granulation facility used in the granulation method of the present invention. [Diagram 2] FIG. 2 is a cross-sectional view showing the granulator of the present embodiment. [Diagram 3] 1 is a graph showing the relationship between the rotation speed of the rotating bed of the granulator and the proportion of granulated material having a particle size of 4.75 mm or more relative to the total granulated material. [Figure 4] 1 is a graph showing the relationship between the sieve opening and the proportion of granulated material captured on the sieve depending on the opening. [Diagram 5] FIG. 2 is a schematic diagram showing the forces acting on a granulated material during granulation. [Figure 6] FIG. 2 is a schematic diagram showing the trajectory of granulated material moving in the granulation chamber during granulation. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0017] Hereinafter, an embodiment of a granulation method according to the present invention will be described in detail with reference to the drawings. In the granulation method of the present embodiment, the powdered raw material M having a particle size of 20 μm or less and a strength of 3.0 kg / cm 2 The above granulated material is obtained. The powdered raw material M described above is generally called powder dust generated from an electric furnace for melting / oxidation refining stainless steel. This powder dust contains valuable metals such as Ni, Cr, and Fe, and in order to make effective use of metal resources, it is preferable to adjust the powder dust from its dust form, which is difficult to use, to a granulated material with a larger particle size. In the present invention, the composition of the powdered raw material M is not particularly limited, but for example, the powdered raw material may be a material having a composition of FeO: 0.1 to 10 mass%, Fe 2 O 3 :25~45mass%, CaO:2~15mass%, SiO 2 : 5~15mass%, Al 2 O 3 :0.1~15mass%, MgO:0.1~5mass%, MnO:2~15mass%, Cr 2 O 3 It is possible to use a powder containing 10 to 20 mass% of arsenic, with the remainder being iron and unavoidable impurities, and having a particle size of 20 μm or less. More preferably, it is possible to use a powder having a primary particle size of 10 μm or less. It is also preferable to use the powdered raw material M described above, which has a secondary particle size of 0.850 mm or less.
[0018] Fine powder (dust) with a particle size of 20 μm or less is too small to be used as is. In addition, since it contains elements (harmful elements) such as Cr mentioned above, it may not be easy to dispose of it in landfills as is. In the present invention, the powder dust is granulated into a granulated product that has a larger particle size than dust and is easier to use, thereby expanding the uses of the powder dust, which was previously difficult to reuse, and from the perspective of effective resource utilization, making it possible to maximize the intrinsic value of elements (valuable metals) such as Ni, Cr, Fe, etc. contained in the powder dust as metals or oxides.
[0019] Specifically, the granulation method of the present invention involves feeding water to a kneader 2 so that the total amount is greater than 10 mass% and less than or equal to 12 mass%, kneading the raw material M, feeding the kneaded raw material M into a granulator 3 equipped with a granulation chamber 6 having a rotating bed 4 rotating at 50 to 150 revolutions per minute and a fixed side wall 5, and granulating the raw material M while rotating the rotating bed 4 in the granulation chamber 6 for 2 minutes or more to obtain a granulated product. Preferably, when granulating in the granulation chamber 6, the raw material M is granulated while rotating the rotating bed 4 at 60 to 110 revolutions per minute.
[0020] Next, the granulation equipment 1 used in the granulation method of the present invention and the granulation conditions will be described in detail. As shown in FIG. 2, the granulation equipment 1 of this embodiment is composed of a raw material supplying machine 7, a kneading machine 2, and a granulator 3. The above-mentioned raw material supplying machine 7 includes a hopper 8 formed in a tapered shape so as to widen toward the top, and a shutter 9 provided at the bottom end of the hopper 8. The hopper 8 is formed in a tapered shape so as to widen toward the top, so that the raw material M can be collected without spilling. The raw material M supplied from the top of the hopper 8 is sent to the shutter 9 provided at the bottom of the hopper 8. The shutter 9 is capable of blocking the supplied raw material M at regular intervals, so that the raw material M can be supplied at a fixed amount. The material that passes through the shutter 9 is sent to the kneader 2 (one end side of the kneader 2).
[0021] The kneader 2 is a continuous kneader 2 having two kneading screws with their axes oriented horizontally. The raw material M is supplied between the two kneading screws, and a shearing force caused by kneading is applied to the raw material M, thereby kneading the raw material M. The kneader 2 is configured to supply the raw material M from one end connected to a hopper 8, knead the supplied raw material M while sending it to the other end, and discharge the kneaded raw material M from the other end connected to a granulator 3.
[0022] In addition, the other end side of the kneader 2 in this embodiment is arranged at the same height as the upper end of the granulator 3 or higher than the granulator 3, so that the kneaded raw material M can be supplied from above the granulator 3. As shown in Figures 2 and 3, the granulator 3 includes a granulation chamber 6 that granulates the raw material M mixed by the mixer 2. In this embodiment, the granulation chamber 6 is formed in a substantially cylindrical shape with its axis oriented in the vertical direction. The side wall 5 of the granulation chamber 6 is fixed, whereas the rotating bed 4 is rotatable, so that the raw material M supplied thereto can be granulated while rolling.
[0023] Specifically, the granulator 3 of this embodiment is provided with a cylindrical granulation chamber 6 with a bottom that opens upward. The side wall 5 of the granulation chamber 6 is formed as a vertical wall that stands up along the vertical direction, and the bottom wall 10 of the granulation chamber 6 is formed as a horizontal wall that extends along the horizontal direction. A through hole 11 that penetrates the bottom wall 10 in the vertical direction is formed in the center of the bottom wall 10. It is preferable that the side wall 5 formed in the granulation chamber 6 has a circular shape when observed from above the device, as shown in Figures 6 and 7, but this is not limited to this as long as the raw material M is processed as described below. For example, a polygonal shape is also acceptable.
[0024] A rotating bed 4 is provided above the bottom wall 10 of the granulation chamber 6. The rotating bed 4 is a separate member from the bottom wall 10 constituting the granulation chamber 6, and is formed in a disk shape that can be fitted into the granulation chamber 6 from above. The rotating bed 4 is provided above the bottom wall 10 of the granulation chamber 6, and is rotatable relative to the fixed bottom wall 10. A shaft 12 that protrudes downward is provided on the underside of the center of the rotating bed 4. This shaft 12 is rotatable integrally with the rotating bed 4, and is inserted from above into the through hole 11 of the bottom wall 10. The lower end of the shaft 12 is connected to a drive motor 13, and the rotational driving force of the drive motor 13 can be transmitted via a power transmission mechanism 14 such as a worm gear or a bevel gear.
[0025] Therefore, when the drive motor 13 is driven, the rotational driving force of the drive motor 13 is transmitted to the shaft 12 via the power transmission mechanism 14, and the disk-shaped rotating bed 4 rotates around an axis facing in the vertical direction. In other words, the above-mentioned granulation chamber 6 is structured so that the rotating bed 4 rotates around an axis facing in the vertical direction relative to the side wall 5 of the granulation chamber 6 which is fixed and does not rotate, and the raw material M supplied to the granulation chamber 6 can be granulated while rolling on the rotating rotating bed 4.
[0026] An outlet 15 is formed on the lower side of the side wall 5 of the granulation chamber 6 to take out the granulated material outside the chamber after granulation in the granulation chamber 6. The outlet 15 is formed so as to penetrate the side wall 5 of the granulation chamber 6 from the inside to the outside, and is formed at a position where the lower edge of the opening is flush (same height) with the upper surface of the rotating bed 4, so that the granulated material that rolls on the rotating rotating bed 4 and rolls to the outer periphery by centrifugal force can be taken out of the chamber.
[0027] The outlet 15 is provided with a granulation size adjusting plate 16 for adjusting the size of the granulation material taken out from the outlet 15 to the outside of the room. The granulation size adjusting plate 16 is a plate member capable of closing the lower part of the opening of the outlet 15. That is, the supplied raw material M is processed in the granulation chamber 6 formed in a cylindrical shape, and remains in the granulation chamber 6 for a predetermined processing time. In the granulation chamber 6, the particle size of the granulated material rolling on the surface of the rotating bed 4 increases as the rolling time increases, and the granulated material gradually grows into a larger size. Eventually, the granulated material that has reached a target particle size or larger is automatically discharged by climbing over the granulation size adjustment plate 16. For example, if the above-mentioned granulation size adjustment plate 16 is present, granulated material with a small particle size cannot climb over the granulation size adjustment plate 16 and is not taken out of the chamber. However, if the particle size has grown to a large size, the granulated material can climb over the granulation size adjustment plate 16, and only granulated material that has grown to a certain size is taken out of the chamber.
[0028] In other words, the granule size adjusting plate 16 functions as a regulating plate (baffle plate) that regulates the discharge of granules that do not meet a predetermined particle size, and allows only granules with a particle size equal to or larger than the predetermined size to be taken out. The granulation chamber 6 has a function of adjusting the size of the discharged granulated material by adjusting the length of time the granulated material is retained in the granulation chamber 6. Therefore, when granulating a granulated material with a large particle size, it is advisable to lengthen the processing time the granulated material is retained in the granulation chamber 6 and to increase the vertical width of the granulated material size adjusting plate 16, in other words, the height of the granulated material size adjusting plate 16. When granulating a granulated material with a small particle size, it is advisable to shorten the processing time the granulated material is retained in the granulation chamber 6 and to decrease the vertical width of the granulated material size adjusting plate 16, in other words, the height of the granulated material size adjusting plate 16.
[0029] When granulation is performed using the granulation equipment 1 having the above-mentioned configuration, the strength of the granulated material is such that it cannot be crushed even when pinched with fingers, specifically, 3.0 kg / cm 2 The strength must be 3.0kg / cm or more. 2 If the strength does not satisfy the above requirements, the granules will easily crumble and become difficult to use. In addition, in order to further increase the strength of the granules, additional curing and drying will be required, which will increase the cost of granulation and reduce productivity.
[0030] On the other hand, when it is used as a granulated product, it is necessary to granulate the granulated product to a size that is easy to use. In this regard, in the granulation method of the present invention, it is preferable to granulate the granulated product to a size (particle size distribution) such that the ratio of particles having a particle size of 4.75 mm or more to the total particles of the granulated product is 95% or more. Furthermore, when producing granules having the above-mentioned strength and size, it is also necessary to perform granulation with good productivity.
[0031] In order to satisfy all of the above-mentioned strength, particle size distribution, and productivity of the granulated product, the granulation method of the present invention rotates the rotating bed 4 at a rotation speed of 50 to 150 rpm, preferably 60 to 110 rpm, for 2 minutes or more to perform granulation. Note that this processing time refers to the time from when the raw material M such as powder dust is completely charged from the hopper 8 to the granulated product is discharged from the discharge port 15.
[0032] When granulation is performed at the above-mentioned rotation speed and processing time, the granulated material is compacted as it rolls on the surface of the rotating bed 4, and at the same time, moisture is removed from the granulated material, improving its strength. 2 It is possible to efficiently produce granulated material having the above strength. Moreover, the longer the processing time for granulation in the granulation chamber 6, the larger the particle size of the granulated material becomes. When granulation is performed for 2 minutes, the particles grow until the majority of the particles have a particle size of 4.75 mm or more. Therefore, by providing a granulation size adjusting plate 16 with a height of, for example, 50 mm, and adjusting the size of the granulated material to be taken out, it is possible to obtain granulated material with a particle size distribution in which the proportion of particles having a particle size of 4.75 mm or more is 95% or more.
[0033] By using the above-mentioned granulation equipment 1 and rotating the rotating bed 4 for 2 minutes or more at a rotation speed of 50 to 150 rpm, preferably 60 to 110 rpm, it is possible to obtain granules excellent in strength, particle size distribution, and productivity. As a result, even if the powdery raw material M has a particle size of 20 μm or less, such as fine powder dust, it is possible to obtain granules having a strength of 3.0 kg / cm. 2It is possible to granulate the above granules with a particle size distribution such that 95% or more of the granules have a particle size of 4.75 mm or more.
[0034] In addition, with the above-mentioned granulation method, moisture is sufficiently removed from the granulated material through granulation, so that storage (curing) and drying to remove moisture as in conventional granulation methods are not an expense, and the number of days required for these processes can be omitted from the production process, thereby dramatically increasing the productivity of granulation. EXAMPLES
[0035] Next, the effects of the granulation method of the present invention will be described in detail using comparative examples and examples. In the examples and comparative examples, powdery raw materials with a particle size of 20 μm or less were granulated using the granulator 3 of the present invention, a pan pelletizer, and a drum pelletizer under the conditions shown in Tables 1 and 2, and the strength, moisture content, and particle size distribution of the granulated products were measured.
[0036] The strength is the crushing strength measured using a sample compression / destruction type crushing strength tester, and is rated at 3.0 kg / cm, which is the strength that cannot be crushed by fingers. 2 As mentioned above, the granulated material was judged to be "3 kg / cm or more". 2 If the strength is "or more," it can be determined that "the handleability of the pellets can be improved." In addition, if the above-mentioned strength can be achieved immediately after granulation, the moisture will be removed after granulation and the strength will be improved. Since the number of storage (curing) days until the product is ready can be eliminated, it can be expected that "production costs will be reduced and productivity will be improved."
[0037] The strength was measured immediately after granulation, 3 days after granulation, and 7 days after granulation. The moisture content was measured by measuring the moisture content of the granules immediately after granulation using an infrared heating type dry mass meter. Furthermore, the particle size distribution is "the percentage by weight of granulated material with a particle size of 4.75 mm or more to the total particles."
[0038] The results of the above-mentioned Examples and Comparative Examples are shown in Table 1.
[0039] [Table 1]
[0040] Looking at the crushing strengths of Comparative Example 1 and Comparative Example 2 in Table 1, in Comparative Example 1 where a pan pelletizer was used for the granulator 3, and in Comparative Example 2 where a drum pelletizer was used, the crushing strength was 0.5 kg / cm 2 or 1kg / cm 2 The crush strength of the example is very low at 4.9 kg / cm 2 ~7.2kg / cm 2 It can be seen that the granules are more easily crushed than the pelletizers in Comparative Examples 1 and 2. This is thought to be because, in the case of a pan pelletizer or drum pelletizer in which the stationary side wall 5 and the rotating rotary bed 4 are not provided in the granulation chamber 6, the granules do not roll, or even if they do, the rolling speed is slow. In other words, in Comparative Examples 1 and 2 in which the rolling is insufficient, no significant strain is imparted to the granules, and the granules are weak, so that the target pressure of "≧3 kg / cm 2 In contrast, the granulator 3 of the embodiment, in which the bottom surface rotates with respect to the stationary side wall portion 5, has a large difference in relative speed between the side wall portion 5 and the bottom surface, and the granulated material can be rolled strongly. Therefore, a large strain can be imparted to the granulated material, and the granulated material becomes stronger, and does not meet the target crushing strength of "≧3 kg / cm 2 It is judged that the crushing strength of the material is satisfactory.
[0041] In addition, in Comparative Example 1 and Comparative Example 2, workers who are skilled in actually operating the equipment are in charge of the work. Such work includes the introduction of raw material M, the supply of moisture (the water is introduced so as to be sprinkled evenly), and the supply of new raw material M (the raw material M is introduced so as to be sprinkled evenly in the same way as the water), and the finished state of the granulated product is good due to the skilled skills of the workers.
[0042] In other words, in Comparative Examples 1 and 2, because the work was performed by workers with skilled techniques, the percentage of granulated material with a particle size of 4.75 mm or more, which is the target particle size, i.e., the yield, was high at 99.1% and 99.3%. However, the inventors have confirmed that when the work is performed by a worker with ordinary skills or a worker with a low level of proficiency, the proportion of particles with a particle size of 4.75 mm or more will be lower than the above-mentioned value, and it will be difficult to achieve a stable yield. Therefore, it can be determined that the result of the embodiment, where "the proportion of particles with a particle size of 4.75 mm or more will be stably 95% or more," is highly likely to be unsatisfactory.
[0043] Next, using the granulator 3 of this embodiment, in other words, "a granulator 3 in which the rotating bed 4 rotates with the side wall 5 fixed," we analyzed how the "crushing strength immediately after granulation" and the "proportion of granulated material with a particle size of 4.75 mm or more in the total amount of granulated material (+4.75 mm ratio)" change when the granulation conditions, "the rotation speed of the rotating bed 4 (the rotation speed of the device)" and "the blending amount of water in the raw material M (the blending set value)," are changed, and the results are shown in Table 2 and Figure 4.
[0044] [Table 2]
[0045] From the results in Table 2 and Figure 4, it can be seen that the "ratio of granulated material with a particle size of 4.75 mm or more to the total amount of granulated material" gradually decreases when the rotation speed of the granulating chamber 6 of the granulator 3 (the rotation speed of the rotating bed 4) is increased. This is thought to be because when the rotation speed of the rotating bed 4 becomes too high, the granulated material collides with the side wall 5, damaging the granulated material that has been granulated with great care, and instead increasing the amount of granulated material with a small particle size.
[0046] That is, as shown in Fig. 5, during granulation, in other words, the granulated material rolling on the rotating rotating bed 4 is naturally subjected to not only the circumferential force accompanying the rotation, but also the centrifugal force. Therefore, the resultant force of these forces acts on the granulated material as shown by the arrow in the figure. Since this resultant force acts in a direction that causes the granulated material to collide with the side wall 5, the granulated material repeats the action of colliding with the side wall 5, being separated from the side wall 5 by the reaction force of the collision, and then colliding again as the granulated material rotates.
[0047] As a result, as shown in Fig. 6, the granulated material rotates in a spiral shape, repeatedly colliding and separating, and moves in circles around the rotation axis of the rotating bed 4. Therefore, when the rotation speed of the rotating bed 4 is high, the frequency of collisions with the side wall 5 increases, and it is considered that there is a high possibility that the granulated material will be damaged, resulting in a smaller particle size. Also, looking at the results in Table 2 and Figure 4, when the "content of water in raw material M (set value)" is 10%, the "proportion of granulated material with a particle size of 4.75 mm or more in the total amount of granulated material" is remarkably low at 19% or 29%. In contrast, when the "content of water in raw material M (set value)" is 11% or 12%, it is possible to increase the "proportion of granulated material with a particle size of 4.75 mm or more in the total amount of granulated material" to above the target value of 95%, depending on the rotation speed of the rotating bed 4.
[0048] On the other hand, with regard to the rotation speed of the rotating bed 4, in experimental examples in which the "moisture content in the raw material M (set value)" is 11% or 12%, by setting the rotation speed to 50 rpm to 150 rpm, preferably 60 rpm to 110 rpm, the "proportion of granulated material with a particle size of 4.75 mm or more in the total amount of granulated material" can be made to be equal to or greater than the target value of 95%. Furthermore, FIG. 5 shows the weight percent of the granulated material collected on sieves having mesh sizes of 1.0 mm, 1.75 mm, 4.75 mm, 6.75 mm, 9.5 mm, and 19 mm in order of the largest mesh size, for Examples 1 to 11 in Table 2.
[0049] Looking at the results in Figure 5, the moisture content of raw material M (mixture setting value) is 10%. In Examples 10 and 11, the powder is captured on sieves with mesh sizes of 1.0 mm, 1.75 mm, 4.75 mm, and 6.75 mm, but is hardly captured on sieves with mesh sizes of 9.5 mm and 19 mm. This shows that when the "water content in raw material M (mixture set value)" is less than 10%, the particle size of the granulated product becomes small, and it is not possible to granulate granulated products with a particle size of 4.75 mm or more.
[0050] However, in Examples 1 to 9 in which the "content of water in raw material M (set value)" is 11% or 12%, almost no granulated material is captured on sieves with openings of 1.0 mm or 1.75 mm, and most of the granulated material is captured on sieves with openings of 4.75 mm to 19 mm. From this, it is judged that if the "content of water in raw material M (set value)" is set to 11% or 12%, the granulated material grows to a sufficient particle size, and granulated material with a particle size of 4.75 mm or more can be granulated at a high yield.
[0051] In view of the above, the powdery raw material M having a particle size of 20 μm or less is mixed with water in an amount of more than 10 mass% and not more than 12 mass% of the total amount, and the mixed raw material M is kneaded in the above-mentioned configuration (having a granulation chamber 6 in which only the rotating bed portion 4 rotates). It is believed that by granulating using a granulator 3 of the above configuration under granulation conditions with a rotation speed of 50 rpm to 150 rpm, preferably 60 rpm to 110 rpm, the result that "the proportion of particles with a particle size of 4.75 mm or more will stably be 95% or more" can be obtained.
[0052] It should be noted that the embodiments disclosed herein are illustrative in all respects and should not be considered as limiting. In particular, in the embodiments disclosed herein, matters not expressly disclosed, such as operating conditions, operating conditions, various parameters, dimensions, weights, volumes of components, etc., do not deviate from the scope of ordinary practice by a person skilled in the art, and values that can be easily assumed by a person skilled in the art are adopted. [Explanation of symbols]
[0053] 1 Granulation equipment 2. Mixing machine 3 Granulator 4 Rotating bed 5 Side wall 6 Granulation chamber 7 Raw material feeder 8 Hopper 9. Shutter 10 Bottom wall 11 Through hole 12 Shaft 13 Drive motor 14 Power transmission mechanism 15 Outlet 16 Granulation size adjustment plate M Raw material
Claims
1. A method for producing a stainless steel product by kneading powder dust having a particle size of 20 μm or less, which is generated from an electric furnace for melting stainless steel or an electric furnace for oxidatively refining stainless steel, by feeding water and the raw material into a kneading machine so that the water content is greater than 10 mass% and less than 12 mass% of the total amount of the raw material; The mixed raw materials are introduced into a granulator equipped with a granulation chamber having a rotating bed portion rotating at 60 to 90 revolutions per minute and a fixed side wall portion, The raw material is granulated while rotating the rotating bed in the granulation chamber for 2 minutes or more, thereby obtaining a granulated product in which particles having a particle diameter of 4.75 mm or more account for 95% or more of the total particles. A granulation method comprising the steps of:
2. The powdered raw material includes FeO: 0.1 to 10 mass%, Fe 2 O 3 :25~45mass%, CaO:2~15mass%, SiO 2 : 5 to 15 mass%, Al 2 O 3 : 0.1~15mass%, MgO: 0.1~5mass%, MnO: 2~15mass%, Cr 2 O 3 : Contains 10-20 mass% of iron, with the remainder being iron and unavoidable impurities, and has a particle size of 20 μm or less. The granulation method according to claim 1 .
3. 3. The granulation method according to claim 2, wherein all of the powdery raw materials used have a primary particle size of 10 μm or less.
Citation Information
Patent Citations
Treatment of dust
JP1977156769A
Treating method for stainless steel refining dust
JP1978116214A
Granulation of sintered raw material
JP1991213138A
Method for pelletizing coarse and fine particulate substance mixture and production of sintered ore
JP1993247547A
Continuous centrifugal granulation method and device therefor
JP1994007663A