Method for producing copolyester

The method enhances PET resin transparency and color stability by using a titanium-based catalyst and phosphorus-based stabilizer, addressing yellowing issues and cobalt limitations, suitable for transparent products.

JP7594101B2Active Publication Date: 2024-12-03HANWHA SOLUTIONS CORP
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
JP2023519113
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2020-09-25
Filing Date
2021-08-11
Publication Date
2024-12-03
Estimated Expiration
2041-08-11

AI Technical Summary

Technical Problem

Polyethylene terephthalate (PET) resin exhibits low transparency and yellowing due to side reactions during polymerization, limiting its application in transparent products, and traditional cobalt-based coloring agents are not optimal for achieving desired color and transparency.

Method used

A method involving esterification of terephthalic acid, ethylene glycol, and 1,4-cyclohexanedimethanol using a titanium-based catalyst, followed by polycondensation with a phosphorus-based thermal stabilizer, specifically calcium bis[monoethyl(3,5-di-tert-butyl-4-hydroxylbenzyl)phosphonate] or triethyl phosphonoacetate, to minimize yellowing and enhance transparency.

Benefits of technology

The method produces a copolyester resin with improved transparency and color stability, suitable for transparent products like cosmetics and food containers, by reducing yellowing and minimizing cobalt-based coloring agent use.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007594101000001
    Figure 0007594101000001
  • Figure 0007594101000002
    Figure 0007594101000002
Patent Text Reader

Abstract

The present invention relates to a method for producing a copolyester, and more particularly to a method for producing a copolyester that minimizes yellowing while reducing the amount of cobalt-based colorants by using a specific heat stabilizer.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] Cross-reference to related application(s) This application claims the benefit of priority based on Korean Patent Application No. 10-2020-0124994 filed on September 25, 2020, and all contents disclosed in the documents of said Korean patent application are incorporated herein by reference.

[0002] The present invention relates to a method for producing a copolyester, and more particularly to a method for producing a copolyester in which yellowing is minimized while reducing the amount of a cobalt-based coloring agent by using a specific heat stabilizer. [Background technology]

[0003] Polyester resin has excellent mechanical and chemical properties and is used in a wide range of applications, for example, it has been used in fields such as drinking water containers, medical applications, food packaging materials, food containers, sheets, films, and automotive molded products.

[0004] A representative polyester resin is polyethylene terephthalate (PET), which is polymerized using terephthalic acid as a dicarboxylic acid component and ethylene glycol as a glycol component. PET is widely used due to its excellent physical and chemical properties and dimensional stability.

[0005] However, since polyethylene terephthalate resin is a crystalline resin and has low transparency, it has limitations in its application to products that require transparency, such as sheets, films, food wrapping paper, and cosmetic containers.

[0006] Meanwhile, copolyester resin copolymerized with terephthalic acid, ethylene glycol, and CHDM (1,4-cyclohexanedimethanol) as a glycol component comonomer is called glycol modified polyethylene terephthalate (PETG). PETG resin is a non-crystalline resin and has the advantage of being able to produce transparent, thick films and containers that are difficult to produce with existing PET resin. PETG resin can be used to produce transparent products of all moldable thicknesses without whitening due to crystallization, and it also has the advantages of having bright colors, excellent gloss, excellent printability, impact resistance, chemical resistance, and easy secondary processability.

[0007] However, PETG resin has a problem of yellowing caused by a side reaction due to the high activity of the catalyst during the polymerization process, and research to solve this problem is ongoing. Summary of the Invention [Problem to be solved by the invention]

[0008] In order to solve the above-mentioned problems of the conventional art, the present invention aims to provide a method for producing a copolyester resin having excellent color and transparency by minimizing yellowing while reducing the use of a cobalt-based coloring agent by using a specific heat stabilizer. [Means for solving the problem]

[0009] In order to achieve this object, the present invention comprises: Esterifying terephthalic acid, ethylene glycol, and 1,4-cyclohexanedimethanol (CHDM) in the presence of a titanium-based catalyst; and polycondensing the reactants of the esterification reaction in the presence of a phosphorus-based heat stabilizer, The phosphorus-based heat stabilizer is calcium bis[monoethyl(3,5-di-tert-butyl-4-hydroxylbenzyl)phosphonate] or triethyl phosphonoacetate. Effect of the Invention

[0010] According to the manufacturing method of the present invention, a specific heat stabilizer is used to reduce the amount of cobalt-based colorants used, while minimizing yellowing, to produce a copolyester resin having excellent color and transparency.

[0011] Therefore, the copolyester resin obtained by the method for producing a copolyester of the present invention has excellent physical properties such as transparency and color, and can be usefully applied to, but is not limited to, cosmetic, beverage, and food-related containers that require transparency, as well as shrink films, sheets, and various molded products. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0012] The terms used in this specification are merely used to describe exemplary embodiments and are not intended to limit the present invention. A singular expression includes a plural expression unless otherwise clearly indicated in the context.

[0013] In addition, in the present invention, when it is said that each component is formed "on" each other, it means that each component is formed directly on each component, or that other components may be additionally formed between each layer, on the object, or on the substrate.

[0014] The present invention can be modified in various ways and can have various forms, and the specific embodiments are described in detail below. However, it is not intended to limit the present invention to the specific disclosed forms, but it should be understood that the present invention includes all modifications, equivalents, and alternatives falling within the spirit and technical scope of the present invention.

[0015] The process for producing the copolyester of the present invention will now be described in more detail.

[0016] A method for producing a copolyester according to an embodiment of the present invention includes the steps of: esterifying terephthalic acid, ethylene glycol, and 1,4-cyclohexanedimethanol (CHDM) in the presence of a titanium-based catalyst; and polycondensing the esterification reactant in the presence of a phosphorus-based thermal stabilizer, wherein the phosphorus-based thermal stabilizer is calcium bis[monoethyl(3,5-di-tert-butyl-4-hydroxylbenzyl)phosphonate] or triethyl phosphonoacetate.

[0017] More specifically, terephthalic acid, ethylene glycol, and cyclohexanedimethanol (1,4-cyclohexanedimethanol, CHDM) are first subjected to an esterification reaction.

[0018] In general, polyester resin is a polymer synthesized through esterification and polycondensation reactions of dicarboxylic acid and glycol monomers. Polyethylene terephthalate (PET), one of such polyesters, is a resin polymerized using terephthalic acid as a dicarboxylic acid component and ethylene glycol as a glycol component, and is a representative crystalline resin that has been widely used in the past.

[0019] However, since polyethylene terephthalate resin is a crystalline resin and has low transparency, it has limitations in its application to products that require transparency, such as sheets, films, food wrapping paper, and cosmetic containers.

[0020] Meanwhile, copolyester resin copolymerized with terephthalic acid, ethylene glycol, and CHDM (1,4-cyclohexanedimethanol) as a glycol component comonomer is called glycol modified polyethylene terephthalate (PETG). PETG resin is a non-crystalline resin and has the advantage of being able to produce transparent, thick films and containers that are difficult to produce with existing PET resin. PETG resin can be used to produce transparent products of all moldable thicknesses without whitening caused by crystallization, and it also has the advantages of having bright colors, excellent gloss, excellent printability, impact resistance, chemical resistance, and easy secondary processability.

[0021] The manufacturing method of the present invention is for producing a copolyester resin, more specifically, a glycol-modified polyethylene terephthalate (PETG) resin polymerized using terephthalic acid, ethylene glycol, and 1,4-cyclohexanedimethanol (CHDM) as a comonomer of the glycol component.

[0022] According to one embodiment of the present invention, in addition to the terephthalic acid, other dicarboxylic acids may be additionally used as the dicarboxylic acid component within a range that does not impair the object of the present invention.

[0023] According to one embodiment of the present invention, as the glycol component, for example, other glycols than ethylene glycol and cyclohexanedimethanol can be used within a range that does not impair the object of the present invention.

[0024] The molar ratio of the dicarboxylic acid component including terephthalic acid to the glycol component including ethylene glycol and cyclohexanedimethanol may be about 1: 1 to about 1: 2. Theoretically, the esterification reaction is a reaction between the dicarboxylic acid component and the glycol component in a molar ratio of 1: 1, but when the dicarboxylic acid component and the glycol component have the above molar ratio, the esterification reaction can occur more efficiently.

[0025] According to one embodiment of the present invention, cyclohexanedimethanol may be contained in an amount of about 10 mol% or more, about 20 mol% or more, or about 30 mol% or more, and 90 mol% or less, about 80 mol% or less, about 70 mol% or less, or about 50 mol% or less, based on 100 mol% of the total glycol component. If the molar ratio of cyclohexanedimethanol is too low, the properties of the polymerized glycol-modified PET resin may not be well expressed, and if the cyclohexanedimethanol is contained in an excessive amount, crystallization of the polymer may occur. In this respect, it is preferable that the cyclohexanedimethanol is contained in the above-mentioned range.

[0026] In the method for preparing the copolyester of the present invention, the step of esterifying terephthalic acid, ethylene glycol, and cyclohexanedimethanol is carried out in the presence of a titanium-based catalyst, which may be, for example, tetraethyl titanate, acetyltripropyl titanate, tetrapropyl titanate, tetrabutyl titanate, polybutyl titanate, 2-ethylhexyl titanate, octylene glycol titanate, lactate titanate, triethanolamine titanate, acetylacetonate titanate, ethylacetoester titanate, isostearyl titanate, or titanium dioxide, but is not limited thereto.

[0027] The titanium catalyst may be added so that the total titanium content of the titanium catalyst is about 5 ppm or more, about 10 ppm or more, or about 15 ppm or more, and about 200 ppm or less, about 150 ppm or less, or about 100 ppm or less, based on the weight of the copolyester finally produced. If the total titanium content is too low, it is difficult to exhibit sufficient catalytic activity, which causes a problem of long polymerization time, and conversely, if it is too high, it causes a problem of yellowing due to side reactions and high catalyst costs.

[0028] According to one embodiment of the present invention, the esterification reaction of terephthalic acid, ethylene glycol, and cyclohexanedimethanol can be carried out at a temperature of about 220 to about 270° C., preferably about 240 to about 260° C., for about 1 to about 10 hours, preferably about 2 to about 5 hours. If the esterification reaction is carried out at a temperature below 220° C., the reaction time becomes long, and the polyester resin produced due to the long reaction time may be more likely to yellow. On the other hand, if the esterification reaction is carried out at a temperature exceeding 270° C., there may be a problem of yellowing due to the high reaction temperature.

[0029] The esterification reaction may be carried out in a batch or continuous manner, and the terephthalic acid, ethylene glycol, and cyclohexanedimethanol may be added separately or in combination.

[0030] Next, a step of polycondensing the reactants of the esterification reaction is carried out in the presence of a phosphorus-based heat stabilizer.

[0031] According to the manufacturing method of the present invention, in order to reduce the thermal decomposition of the copolyester, a phosphorus-based heat stabilizer is added to the polycondensation reaction step, and calcium bis[monoethyl(3,5-di-tert-butyl-4-hydroxylbenzyl)phosphonate] or triethyl phosphonoacetate is used as the phosphorus-based heat stabilizer.

[0032] Heat stabilizers suppress the production of color bodies generated by heat during ester exchange reactions and polycondensation reactions, control the activity of catalysts to suppress unintended addition reactions, and prevent thermal decomposition during timed solid-state polymerization to suppress yellowing of the final polyester, making the color transparent and nearly colorless.

[0033] According to the manufacturing method of the present invention, in manufacturing a copolyester resin, a phosphorus-based heat stabilizer having a specific structure is used to compensate for the disadvantage of titanium-based catalysts, which are susceptible to discoloration, and thus the yellowing of the final copolyester can be suppressed and the color and transparency can be improved.

[0034] Conventionally, triethyl phosphate (TEP) has been mainly used as a phosphorus-based heat stabilizer, but when triethyl phosphate is used as a heat stabilizer in the production of glycol modified PET resin, the color properties cannot be sufficiently improved.

[0035] Therefore, the present invention has been made based on the finding that when calcium bis[monoethyl(3,5-di-tert-butyl-4-hydroxylbenzyl)phosphonate] or triethyl phosphonoacetate is used among phosphorus-based heat stabilizers, excellent color properties can be obtained during the production of glycol-modified PET resin.

[0036] When calcium bis[monoethyl(3,5-di-tert-butyl-4-hydroxylbenzyl)phosphonate] is used as the phosphorus-based compound, the content of the phosphorus-based compound may be added so that the phosphorus content of calcium bis[monoethyl(3,5-di-tert-butyl-4-hydroxylbenzyl)phosphonate] is about 50 ppm or more, about 100 ppm or more, or about 300 ppm or more, and about 1,000 ppm or less, about 900 ppm or less, or about 850 ppm or less, based on the weight of the finally produced copolyester. Adding calcium bis[monoethyl(3,5-di-tert-butyl-4-hydroxylbenzyl)phosphonate] within the above range is preferable in terms of preventing viscosity increase and thermal decomposition during polyester polymerization.

[0037] In addition, when triethyl phosphonoacetate is used as the phosphorus-based compound, the content of the phosphorus-based compound may be added so that the phosphorus content contained in the triethyl phosphonoacetate is about 5 ppm or more, about 10 ppm or more, or about 15 ppm or more, and about 100 ppm or less, about 80 ppm or less, or about 50 ppm or less, based on the weight of the finally produced copolyester. Adding triethyl phosphonoacetate in the above range is preferable in terms of preventing viscosity increase and thermal decomposition during polyester polymerization.

[0038] Furthermore, according to an embodiment of the present invention, a cobalt-based color developer may be added to improve color. Examples of the cobalt-based coloring agent include cobalt acetate, cobalt acetylacetonate, cobalt benzoylacetonate, cobalt hydroxide, cobalt bromide, cobalt chloride, cobalt iodide, cobalt fluoride, cobalt cyanide, cobalt nitrate, cobalt sulfate, cobalt selenide, cobalt phosphate, cobalt oxide, and cobalt thiocyanate. Examples of suitable cobalt compounds include, but are not limited to, cobalt-based compounds such as cobalt thiocyanate or cobalt propionate.

[0039] The content of the cobalt-based color developer may be about 3 ppm or more, about 5 ppm or more, or about 7 ppm or more, and about 100 ppm or less, about 90 ppm or less, or about 70 ppm or less, based on the weight of the final copolyester. When the cobalt compound is added in the above range, coloring can be inhibited without causing a decrease in brightness or thermal stability of the copolyester.

[0040] In addition, the step of adding the cobalt compound in the present invention is not limited to the step of esterification reaction during polymerization reaction or the step of polycondensing the reactant of the esterification reaction, but can be added at any step.

[0041] The step of polycondensing the reactants of the esterification reaction can be carried out at a temperature of about 250 to about 300° C., preferably about 260 to about 290° C., for about 30 minutes to about 6 hours, preferably about 1 to about 4 hours. If the polycondensation reaction is carried out at a temperature of less than 250° C., the reaction time becomes long, and a copolyester having low molecular weight is produced, and the polyester resin produced due to the long reaction time may be more likely to yellow, and if the temperature is more than 300° C., there may be a problem of yellowing due to the high reaction temperature.

[0042] In addition, the step of polycondensing the esterification reaction product can be carried out under reduced pressure conditions of about 760 to about 1 mmHg, preferably about 760 to about 0.01 mmHg. When the polycondensation reaction is carried out under such reduced pressure conditions, by-products generated during the polycondensation reaction can be sufficiently removed from the reaction system.

[0043] The copolyester resin obtained by the production method of the present invention can exhibit an intrinsic viscosity (IV) in the range of about 0.5 to about 1.0 dl / g.

[0044] The copolyester obtained by the production method of the present invention has an intrinsic viscosity (IV) of 0.65 to 0.74 dl / g and has a color b value of 0 or less, for example, 0 or less, or -0.3 or less, or -0.5 or less, and may be -3.5 or more, or -3.2 or more, or -3 or more.

[0045] In addition, when the copolyester obtained by the production method of the present invention has an intrinsic viscosity (IV) of 0.75 to 0.80 dl / g, the color b value may be 5 or less, for example, 5 or less, or 4.5 or less, or 0 or less, and may be -8.0 or more, or -7.5 or more, or -7.0 or more.

[0046] Thus, the copolyester obtained by the production method of the present invention exhibits the property of suppressing yellowing and exhibiting a high degree of blue discoloration, which is desirable for products.

[0047] The L, a, and b color system is used internationally as a standard for the color evaluation of polyester. These color numbers are one of the color systems for standardizing color measurement and describe the perceptible color and color difference. In this system, L is the lightness factor, and a and b are color measurement numbers. Generally, the b value, which indicates the yellow / blue balance, is the important number in the production of drinking water containers and food packaging materials. A positive b value means yellow discoloration and a negative value means blue discoloration. And a positive a value means red discoloration and a negative value means green discoloration. The L value also means a numerical factor indicating brightness and is very important like the b value in the production of drinking water containers and food packaging materials.

[0048] The copolyester produced by the production method of the present invention is not particularly limited in its application, but can be widely used in food packaging materials, bottles, films, or fibrous plastics that require excellent transparency, brightness, and color conditions. More specifically, it can be used in cosmetic, beverage, and food-related containers that require transparency, as well as shrink films, sheets, and various molded products.

[0049] The present invention will be described in more detail with reference to the following examples, however, these examples are merely presented as examples of the invention and do not limit the scope of the invention. EXAMPLES

[0050] <Example> Example 1 1162g of terephthalic acid, 412g of ethylene glycol, 302g of 1,4-cyclohexanedimethanol, and a titanium-based catalyst were placed in a reactor, the reactor was replaced with a nitrogen atmosphere, and the mixture was stirred and heated to gradually increase the temperature to 250°C, and reacted at 1 barg for 2 hours.

[0051] During the reaction, the temperature at the top of the column was maintained below 125° C., and when the water discharge did not proceed any further, the pressure was gradually reduced to allow all the water produced in the reactor to flow out of the system.

[0052] Irganox 1425 (830 ppm based on the final copolyester) and cobalt acetate (20 ppm based on the final copolyester) were then charged to the reactor.

[0053] After stirring for an additional 30 minutes, the mixture was transferred to a reactor equipped with a heating system, stirrer, and pressure reduction system, and the pressure inside the reactor was gradually reduced from 760 mmHg to 5 mmHg over 80 minutes while stirring, and the temperature was gradually increased until the temperature of the final polymerization water reached 267°C, during which the reaction was continued.

[0054] The vacuum was then increased to a maximum of 0.5 mmHg, and the reaction temperature was increased to 270°C to continue the reaction. The reaction was terminated when the target viscosity was reached. The resulting copolyester polymer was discharged, cooled, and cut into pellets, and the viscosity, color, molecular weight, etc. were analyzed.

[0055] In Example 1, Examples 2 to 4 and Comparative Examples 1 and 2 were carried out by varying the content of cobalt acetate, the type and content of the phosphorus-based heat stabilizer, the polymerization time, the viscosity, and the like.

[0056] The process conditions for Examples 1 to 4 and Comparative Examples 1 and 2 are summarized in Table 1 below.

[0057] [Table 1]

[0058] 1) In Table 1, the contents of titanium catalyst, cobalt acetate, and phosphorus-based heat stabilizer all refer to the contents of each element (Ti, Co, P) based on the final copolyester produced. 2) Irganox 1425 stands for calcium bis[monoethyl(3,5-di-tert-butyl-4-hydroxylbenzyl)phosphonate], TEP stands for triethyl phosphate, and TEPa stands for triethyl phosphonoacetate. 3) Polymerization time means the polycondensation reaction time under full vacuum of 0.5 mmHg or less.

[0059] <Experimental Example> Measurement method 1) Intrinsic Viscosity (IV) 0.4g of the resin to be measured is added to 100mL of a reagent mixture of phenol and 1,1,2,2-tetrachloroethanol in a weight ratio of 6:4, and after dissolving for 90 minutes, it is transferred to an Ubbelohde viscometer and kept in a 30℃ thermostatic bath for 10 minutes, and the time it takes for the solution to fall can be calculated using the viscometer and aspirator. The time it takes for the solvent to fall can also be calculated in the same way, and the RV and IV values ​​are calculated using the following formulas 1 and 2. In the formula below, C represents the concentration of the sample.

[0060] [Formula 1] RV = sample drop time / solvent drop time [Formula 2] IV = 1 / 4(RV-1) / C+3 / 4(ln RV / C)

[0061] 2) Resin color (Color=L, a, b) After removing moisture from 50 g of the resin to be measured in air, the resin was placed in a Colorimeter Model SA-2000 and the color was measured 10 times to obtain an average value.

[0062] 3) Weight average molecular weight (M w ) and number average molecular weight (Mn) Gel permeation chromatography (GPC) was used to measure the weight average molecular weight (Mw) and number average molecular weight (Mn), respectively.

[0063] The intrinsic viscosity, color value (L, b), weight average molecular weight (M w ) and number average molecular weight (Mn) were measured and are shown in Table 2 below.

[0064] [Table 2]

[0065] Referring to Tables 1 and 2, the copolyester resins of the examples prepared using a specific phosphorus-based heat stabilizer according to the manufacturing method of the present invention showed better color properties in the same viscosity range than the comparative example in which triethyl phosphate was used as a heat stabilizer according to the conventional method.

Claims

1. Esterification of terephthalic acid, ethylene glycol, and 1,4-cyclohexanedimethanol (CHDM) in the presence of a titanium-based catalyst; and polycondensing the reactants of the esterification reaction in the presence of a phosphorus-based heat stabilizer, The phosphorus-based heat stabilizer is calcium bis[monoethyl(3,5-di-tert-butyl-4-hydroxylbenzyl)phosphonate] or triethyl phosphonoacetate; When the intrinsic viscosity (IV) is 0.65 to 0.74 dl / g, the color b value is -3.5 or more and 0 or less; A method for producing a copolyester, wherein the color b value is -8.0 or more and 0 or less when the intrinsic viscosity (IV) is 0.75 to 0.80 dl / g.

2. 2. The method for producing a copolyester according to claim 1, wherein the titanium-based catalyst comprises at least one selected from the group consisting of tetraethyl titanate, acetyl tripropyl titanate, tetrapropyl titanate, tetrabutyl titanate, polybutyl titanate, 2-ethylhexyl titanate, octylene glycol titanate, lactate titanate, triethanolamine titanate, acetylacetonate titanate, ethyl acetoacetic ester titanate, isostearyl titanate, and titanium dioxide.

3. The method for producing a copolyester according to claim 1, wherein the content of titanium contained in the titanium-based catalyst is 5 ppm or more and 200 ppm or less based on the weight of the finally produced copolyester.

4. 2. The method for producing a copolyester according to claim 1, wherein the esterification reaction of terephthalic acid, ethylene glycol, and cyclohexanedimethanol is carried out at a temperature of 200 to 270° C. for 1 to 10 hours.

5. 2. The method for producing a copolyester according to claim 1, wherein when calcium bis[monoethyl(3,5-di-tert-butyl-4-hydroxylbenzyl)phosphonate] is used as the phosphorus-based heat stabilizer, the content of the phosphorus-based heat stabilizer is from 50 ppm to 1,000 ppm based on the weight of the final copolyester.

6. 2. The method for producing a copolyester according to claim 1, wherein when triethyl phosphonoacetate is used as the phosphorus-based thermal stabilizer, the content of the phosphorus element contained in the phosphorus-based thermal stabilizer is 5 ppm to 100 ppm based on the weight of the final copolyester.

7. In the polycondensation step, a cobalt-based color developer is further included. A method for producing the copolyester of claim 1.

8. The cobalt-based color developer includes cobalt acetate, cobalt acetylacetonate, cobalt benzoylacetonate, cobalt hydroxide, cobalt bromide, cobalt chloride, cobalt iodide, cobalt fluoride, cobalt cyanide, cobalt nitrate, and cobalt sulfate.

8. The method for producing the copolyester according to claim 7, wherein the cobalt sulfate, the cobalt selenide, the cobalt phosphate, the cobalt oxide, the cobalt thiocyanate and the cobalt propionate are selected from the group consisting of cobalt propionate.

9. 8. The method for producing a copolyester according to claim 7, wherein the content of the cobalt-based color developer is 3 ppm or more and 100 ppm or less based on the weight of the finally produced copolyester.

10. The method for preparing a copolyester according to claim 1, wherein the step of polycondensing the esterification reaction product is carried out at a temperature of 250 to 300° C. and a reduced pressure of 760 to 0.01 mmHg for 30 minutes to 6 hours.

Citation Information

Patent Citations

  • Method for producing polyester resin copolymerized with 1,4-cyclohexanedimethanol

    JP2001323054A

  • Aromatic polyester, method for producing the same and aromatic polyester film

    JP2011026470A

  • Copolyesters with improved thermal stability and methods for producing the same

    JP2012525466A

  • Preparation method of polyester resin

    KR1020160059287A

  • Film Containing Transparent Metal Oxide, Method for the Production Thereof, and Thereof

    US20070248803A1