Additive-containing biopolymer composition

A composition of biopolymers and additives, including vinyl acetate polymers and organopolysiloxane pellets, addresses processing and mechanical challenges of biopolymers, enhancing their properties and performance.

JP7594128B2Active Publication Date: 2024-12-03WACKER CHEMIE AG
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
JP2023549672
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2021-02-17
Publication Date
2024-12-03
Estimated Expiration
2041-02-17

AI Technical Summary

Technical Problem

Biopolymers derived from renewable materials face challenges in processing conditions and mechanical properties, limiting their practical applications.

Method used

A composition comprising biopolymers like PLA, PBS, and additives such as vinyl acetate polymers and organopolysiloxane pellets, along with fillers and boric acid, enhances processing and mechanical properties through a synergistic effect.

Benefits of technology

The combination of additives significantly improves the processability, mechanical properties, and surface characteristics of biopolymers, resulting in improved bioplastics with reduced friction, enhanced transparency, and increased durability.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007594128000001
    Figure 0007594128000001
  • Figure 0007594128000002
    Figure 0007594128000002
  • Figure 0007594128000003
    Figure 0007594128000003
Patent Text Reader

Abstract

The present invention relates to a polymerizable composition comprising: (A) 65 to 99.4% by weight of a biopolymer selected from the group consisting of polylactic acid (PLA), polybutylene succinate (PBS), polybutylene succinate adipate (PBSA), thermoplastic starch (TPS), polyhydroxyalkanoate (PHA), polybutylene adipate terephthalate (PBAT), polybutylene sebacate terephthalate (PBST), polyhydroxybutyric acid (PHB), polycaprolactone (PCL), cellophane (CA), and mixtures thereof; (B) 0.5 to 30% by weight of a vinyl acetate-based homopolymer, copolymer, or terpolymer; and (C) (1) a polymerizable composition represented by the general formula R r SiO (4-r / 2) (I) 100 parts by weight of at least one polyorganosiloxane composed of units of the formula: (I) (wherein R is the same or different and represents a substituted or unsubstituted hydrocarbon residue, and r is 0, 1, 2 or 3, with the proviso that the average value of r is in the range of 1.9 to 2.1), (2) 1 to 200 parts by weight of a reinforcing or non-reinforcing filler or a mixture thereof, (3) 0.01 to 20 parts by weight of a boric acid-containing additive for producing a pellet material, and (4) optionally further auxiliaries selected from the group of processing aids, plasticizers, pigments and stabilizers, said organopolysiloxane pellets having a particle size of 1 to 100 mm.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a composition comprising a biopolymer and an additive. [Background technology]

[0002] Biopolymers are polymers made from wholly or partially renewable raw materials and / or are biodegradable. They are intended to replace petroleum-based plastics. In general, bioplastics have more difficult processing conditions and often have poorer mechanical properties.

[0003] US2017 / 313912A1 discloses a composition of polylactic acid (PLA), polyvinyl acetate and a plasticizer for film applications.

[0004] US 2005 / 0004296 A1 describes a method for producing an organopolysiloxane pellet material and the use of the organopolysiloxane pellet material as an additive for thermoplastics.

[0005] The aim was to optimise or improve the surface properties, mechanics and processing of biopolymers by the addition of additives.

[0006] This object is achieved by the present invention.

[0007] According to the present invention, (A) Polylactic acid (PLA), Polybutylene succinate (PBS), Polybutylene succinate adipate (PBSA), Thermoplastic starch (TPS), Polyhydroxyalkanoates (PHAs), Polybutylene adipate terephthalate (PBAT), Polybutylene sebacate terephthalate (PBST), Polyhydroxybutyrate (PHB), Polycaprolactone (PCL), and Cellophane (CA) 65 to 99.4% by weight, preferably 85 to 90% by weight, of a biopolymer selected from the group consisting of (B) 0.5 to 30% by weight, preferably 10 to 15% by weight, of a vinyl acetate homopolymer, copolymer, or terpolymer, and (C)(1) General formula R r SiO (4-r / 2) [In the general formula, R is the same or different and is a substituted or unsubstituted hydrocarbon group, and r is 0, 1, 2 or 3, with the proviso that the average value of r is within the range of 1.9 to 2.1.] 100 parts by weight of at least one polyorganosiloxane composed of units (2) 1 to 200 parts by weight of a reinforcing or non-reinforcing filler or a mixture thereof, (3) 0.01 to 20 parts by weight of a boric acid-containing additive for producing a pellet material, and (4) Optionally, further auxiliaries selected from the group of processing aids, plasticizers, pigments and stabilizers. The organopolysiloxane pellets having a particle size of 1 to 100 mm are added in an amount of 0.1 to 5% by weight, preferably 1 to 2% by weight. A composition comprising: The composition is provided, wherein the contents of components (A), (B) and (C) in weight percent are each based on the total weight of the composition.

[0008] According to the present invention, there is provided a method for producing the composition, comprising the steps of: (A) Polylactic acid (PLA), Polybutylene succinate (PBS), Polybutylene succinate adipate (PBSA), Thermoplastic starch (TPS), Polyhydroxyalkanoates (PHAs), Polybutylene adipate terephthalate (PBAT), Polybutylene sebacate terephthalate (PBST), Polyhydroxybutyrate (PHB), Polycaprolactone (PCL) and Cellophane (CA), 65 to 99.4% by weight, preferably 85 to 90% by weight, of a biopolymer selected from the group consisting of (B) 0.5 to 30% by weight, preferably 10 to 15% by weight, of a vinyl acetate homopolymer, copolymer, or terpolymer, and (C)(5) General formula R r SiO (4-r / 2) [In the general formula, R is the same or different and is a substituted or unsubstituted hydrocarbon group, and r is 0, 1, 2 or 3, with the proviso that the average value of r is within the range of 1.9 to 2.1.] 100 parts by weight of at least one polyorganosiloxane composed of units (6) 1 to 200 parts by weight of a reinforcing or non-reinforcing filler or a mixture thereof, (7) 0.01 to 20 parts by weight of a boric acid-containing additive for producing a pellet material, and (8) Optionally, further auxiliaries selected from the group of processing aids, plasticizers, pigments and stabilizers. The organopolysiloxane pellets have a particle size of 1 to 100 mm, and the amount of the organopolysiloxane pellets is 0.1 to 5% by weight, preferably 1 to 2% by weight. mixing the mixture; The method is also provided, wherein the weight percent contents of components (A), (B) and (C) are each based on the total weight of the composition.

[0009] Biopolymers (A) are commercially available and can be prepared, for example, Polylactic acid (PLA) from Nature Works and Total-Corbion; Polybutylene succinate (PBS) from MCPP-Europe; MCPP-Europe Polybutylene Succinate Adipate (PBSA), Thermoplastic starch (TPS) from Rodenburg Biopolymers; Polyhydroxyalkanoates (PHAs) from Biomer and Danimer Scientific; Polybutylene adipate terephthalate (PBAT) from BASF, BASF's polybutylene sebacate terephthalate (PBST), Polyhydroxybutyrate (PHB) from Biomer and Danimer Scientific; Polycaprolactone (PCL) from Dow-DuPont and Perstorp; FKuR Cellophane (CA) Examples include:

[0010] The biopolymers used are preferably polylactic acid (PLA) and polybutylene succinate (PBS).

[0011] The vinyl acetate homopolymer, copolymer or terpolymer used as additive (B) is preferably Vinyl acetate homopolymer, Copolymers of vinyl acetate and ethylene, Copolymers of vinyl acetate and vinyl laurate, Terpolymer of vinyl acetate, ethylene and versatic ester, Terpolymers of vinyl acetate, ethylene and acrylates; Terpolymers of vinyl acetate, vinyl laurate and vinyl acrylate, and A mixture of them is selected from the group consisting of:

[0012] Vinyl acetate-based homopolymers, copolymers and terpolymers are commercially available, for example vinyl acetate homopolymers and copolymers sold under the trade name Vinnex® by Wacker Chemie AG.

[0013] The additives (B) used are preferably homopolymers of vinyl acetate and copolymers of vinyl acetate and ethylene.

[0014] The additive (B) is a fine powder (preferably with a diameter of about 100 μm). 50 The pharmaceutical composition may be in the form of a tablet, a spherical pill (preferably having a maximum diameter of 2 mm), a broken flake (irregular shape), or a pellet (preferably having a maximum diameter of about 4 mm).

[0015] The additive (C) used is an organopolysiloxane pellet as described in US 2005 / 0004296 A1 (incorporated by reference), more particularly in paragraphs

[0009] to

[0054] .

[0016] Examples of the hydrocarbon group R are alkyl groups, for example methyl, ethyl, n-propyl, isopropyl, n-butyl, isobutyl, tert-butyl, n-pentyl, isopentyl, neopentyl or tert-pentyl groups, hexyl groups such as n-hexyl, heptyl groups such as n-heptyl, octyl groups such as n-octyl, isooctyl groups such as 2,2,4-trimethylpentyl, nonyl groups such as n-nonyl, decyl groups such as n-decyl, dodecyl groups such as n-dodecyl, cycloalkyl groups, for example, cyclopentyl, cyclohexyl, cycloheptyl and methylcyclohexyl groups; aryl groups, for example, phenyl, biphenyl, naphthyl, anthryl and phenanthryl groups; alkaryl groups, for example, o-tolyl, m-tolyl and p-tolyl, xylyl and ethylphenyl groups; aralkyl groups, for example, benzyl, α-phenylethyl and β-phenylethyl groups.

[0017] Examples of substituted hydrocarbon groups R are halogenated alkyl groups such as 3-chloropropyl, 3,3,3-trifluoropropyl and perfluorohexylethyl groups, and halogenated aryl groups such as p-chlorophenyl and p-chlorobenzyl groups.

[0018] The group R is preferably a hydrogen atom group or a hydrocarbon group having 1 to 8 carbon atoms, more preferably a methyl group.

[0019] Further examples of radicals R are the vinyl, allyl, methallyl, 1-propenyl, 1-butenyl and 1-pentenyl, 5-hexenyl, butadienyl, hexadienyl, cyclopentenyl, cyclopentadienyl, cyclohexenyl, ethynyl, propargyl and 1-propynyl radicals.

[0020] In a further preferred embodiment of the invention, the group R is an alkenyl group having 2 to 8 carbon atoms, more preferably a vinyl group.

[0021] The polyorganosiloxane (1) is preferably a high viscosity substance. Preferably, the polyorganosiloxane (1) has a viscosity of 1,000,000 to 100,000,000 mm at 25° C. 2 / s (measured in accordance with DIN 1342-2, version 2003-11).

[0022] The polyorganosiloxane (1) is preferably a diorganopolysiloxane having a trialkylsiloxy group, a trimethylsiloxy group, a dimethylhydroxysiloxy group or a dimethylvinylsiloxy group as a terminal group.

[0023] The polyorganosiloxane (1) is preferably a diorganopolysiloxane that is end-capped with trialkylsiloxy groups, preferably trimethylsiloxy groups, and is composed of approximately 70 to 100%, preferably 90 to 100%, dimethylsiloxane units and approximately 0 to 30%, preferably 0 to 10%, alkenylmethylsiloxane units, preferably vinylmethylsiloxane units.

[0024] It is possible to use one type of polyorganosiloxane (1), or a mixture of at least two different types of polyorganosiloxanes (1).

[0025] An example of the reinforcing filler (2) is at least 50 m 2 The silica is a fumed or precipitated silica having a BET surface area of ​​100 / g.

[0026] The above-mentioned silica fillers may be hydrophilic in nature or may be hydrophobized by known methods. They are preferably used.

[0027] Examples of non-reinforcing fillers (2) are quartz powder, diatomaceous earth, calcium silicate, zirconium silicate, zeolites, metal oxide powders, such as aluminum powder, titanium powder, iron powder or zinc oxide, barium silicate, barium sulfate, calcium carbonate, gypsum, polytetrafluoroethylene powder. It is also possible to use fibrous components, such as glass fibers or plastic fibers, as fillers. The BET surface area of ​​these fillers is preferably greater than 50 m. 2 / g.

[0028] The organopolysiloxane pellets of the present invention contain the filler (2) in an amount of preferably 1 to 200 parts by weight, more preferably 30 to 100 parts by weight, per 100 parts by weight of the polyorganosiloxane (1).

[0029] The boric acid-containing additive (3) is described in EP 1028140 A1, the relevant disclosure of which is intended to form part of the present application, and enables the production of a completely free-flowing organopolysiloxane pellet material. The additive (3) preferably consists essentially of boric acid, water, preferably deionized or high purity water, and optionally a fatty acid salt, and is added to the polyorganosiloxane (1) in an amount of preferably 0.01 to 20 parts by weight, preferably 0.1 to 4 parts by weight, more preferably 0.1 to 2 parts by weight, based on 100 parts by weight of the polyorganosiloxane (1).

[0030] The water functions as a solvent for the boric acid and is preferably removed prior to pelletizing.

[0031] The fatty acid salt optionally present in the boric acid additive (3) is preferably a salt of metals Al, Ba, Ca, Cd, Co, Cr, Cu, Fe, Li, Mg, Mn, Ni, Pb, Sn, Sr, Zn with higher fatty acids, resin acids and naphthenic acids, such as stearates, palmitates, oleates, linoleates, resin acids, laurates, octanoates, ricinoleates, 12-hydroxystearates, naphthenates, tolates and the like. Fatty acids having more than 12 and up to 30 carbon atoms are preferred, and fatty acids having more than 16 and up to 26 carbon atoms are particularly preferred, with stearates, particularly calcium stearate being particularly preferred. The fatty acid salt is present in the boric acid additive composition in an amount of preferably 0.1 to 10% by weight, preferably 0.2 to 6% by weight, more preferably 0.3 to 4% by weight.

[0032] Examples of plasticizers that can be used as component (4) in the organopolysiloxane pellet material are trimethylsiloxy or hydroxyl terminated plasticizers having a maximum viscosity of 5000 mm at 25° C. 2 / s, or diphenylsilanediol. The dipolyorganosiloxane is preferably formed from dimethylsiloxane units and / or vinylmethylsiloxane units.

[0033] After mixing the individual components (1)-(4), preferably in a kneader, at a temperature of preferably 100-250°C, preferably 120-200°C, the composition is pelletized using conventional pelletizing means such as perforated plates and rotary knives to obtain a completely free-flowing pellet material. The particle size of the resulting organopolysiloxane pellets is 1-100 μm, preferably 2-50 μm. The organopolysiloxane pellets of the present invention preferably have a typical cylindrical pellet structure with a diameter of preferably 3-10 mm, more preferably 4-8 mm, and a height of preferably 2-10 mm, more preferably 3-8 mm.

[0034] The particle size of the organopolysiloxane pellets is determined by the diameter of the perforated plate used.

[0035] Organopolysiloxane pellets used as additive (C) are commercially available, for example, under the trade name Genioplast® from Wacker Chemie AG.

[0036] In addition to components (A) to (C), the composition of the present invention may contain further components (D) such as fillers, pigments, stabilizers and antioxidants.

[0037] The fillers used may be reinforcing or non-reinforcing fillers.

[0038] Reinforcing filler, i.e. at least 50m 2 An example of a packing material having a BET surface area of ​​50 m 2 The fillers are fumed silica, precipitated silica or silicon-aluminum mixed oxides having a BET surface area of ​​more than 1000 nm / g. The abovementioned fillers may be hydrophobized, for example by treatment with organosilanes, silazanes or siloxanes, or by etherifying the hydroxyl groups to alkoxy groups.

[0039] Non-reinforcing filler, i.e. 50m 2 Examples of fillers having a BET surface area of ​​less than 1 / g are calcium carbonate, powdered quartz, cristobalite, diatomaceous earth, calcium silicate, zirconium silicate, montmorillonites such as bentonite, zeolites including molecular sieves such as sodium aluminum silicate, metal oxides such as aluminum oxide or zinc oxide or mixed oxides thereof, metal hydroxides such as aluminum hydroxide, barium sulfate, gypsum, silicon nitride, silicon carbide and boron nitride.

[0040] The composition of the present invention preferably comprises a filler in an amount of 5-40% by weight, preferably 10-15% by weight.

[0041] Suitable for compounding the compositions of the present invention are twin screw extruders, preferably commercial co-rotating twin screw extruders, where the screw length / diameter ratio (L / D ratio) is preferably >30, more preferably >40.

[0042] The temperature at which additives (B) and (C) are compounded into the biopolymer depends on the melting of the biopolymer. Here, it is necessary not to exceed the recommended temperature. When compounding additives (B) and (C) into the biopolymer, a temperature of 170-220°C, preferably 175-210°C, is preferred. After compounding at elevated temperature in suitable processing equipment, the resulting compound can be further processed by conventional techniques, such as injection molding, blow molding, compression molding or vacuum molding, to produce the corresponding plastics.

[0043] The addition of additive (B) has the advantage of being highly compatible with biopolymers, especially polylactic acid (PLA). Moreover, additive (B) allows the production of high-performance polymer blends combining polylactic acid (PLA), other biopolyesters and starch with organic and inorganic fillers. The use of additive (B) in combination with PLA is particularly suitable for blown-film extrusion and injection molding applications.

[0044] By adding additive (B) to polybutylene succinate (PBS), the recrystallization rate of PBS can be significantly reduced and its properties can be kept constant. Depending on the proportion of additive (B) selected and the addition of polylactic acid (PLA), the flexibility or stiffness can be adjusted as required. It is also possible to use a higher proportion of organic or inorganic fillers without adversely affecting the physical properties.

[0045] However, only when additive (B) is combined with additive (C) can a biopolymer be obtained with significantly better processability. Moreover, bioplastics treated with the combination of additive (B) and additive (C) have significantly improved surface properties and mechanical parameters compared to bioplastics treated with additive (B) alone or with additive (C) alone. Here, the combination of the two additives (B) and (C) produces a synergistic effect.

[0046] The use of a combination of the two additives (B) and (C) in the bioplastics according to the invention makes it possible to produce molded parts and films which have better mechanical properties and better surface properties than molded parts and films made from bioplastics produced with only one additive (B) or (C). EXAMPLES

[0047] 1. Preparation of Compositions 1 to 18 The 18 compounds were mixed at a temperature of 185° C., a screw speed of 250 rpm, and a throughput of 10 kg / h using a KraussMaffei Berstorff ZE-25 twin screw extruder with a length / diameter ratio of 47 and a screw diameter of 25 mm. The 18 compositions are as listed in Table 1 below. The compounding conditions of the relevant compounds are as listed in Table 2. For this, all the components of the pellet material were mixed to form a dry mix, which was weighed gravimetrically into the feed zone of the extruder. Similarly, all the powder components were mixed to form a dry mix, which was also weighed gravimetrically into the feed zone of the extruder. The resulting extrudate was pelletized in a UWG and cooled.

[0048] [Table 1]

[0049] [Table 2]

[0050] The use of both additives in the processing process resulted in the greatest reduction in torque and power consumption during the compounding process.

[0051] The efficacy was evaluated for the biopolymers containing both additives (B) and (C), i.e., 10% or 15% by weight of Vinnex® and 1% by weight of Genioplast® (compositions 3 and 6, and compositions 10 and 13), and - by comparing pure biopolymers without additives, both with unfilled biopolymers (PLA, composition 1) and with filled biopolymers (PBS+CaCO3, composition 8); - Additive (B) to the biopolymer alone, for example 10% or 15% by weight of Vinnex® (Compositions 2 and 5, and Compositions 9 and 12) This was determined and implemented by comparing the

[0052] 2. Further processing 2.1 Injection molded plate The compounds in Table 1 were processed using an Engel ES 600 / 125 injection molding machine at 170-200°C, injection speeds of 30-80 mm / s, and dynamic pressure of 5.4 bar into injection molded plates with smooth surfaces and dimensions of 8 cm x 12 cm.

[0053] 2.2 Flow Spiral A 1.6 mm deep flow spiral was also fabricated from the compound using the same system at 160-190 °C, injection speed of 50 mm / s, and back pressure of 2 bar.

[0054] 2.3 Blown film Further, an inflation film was produced to obtain a test specimen.

[0055] 3. Preparation of press plate-shaped test specimens Each compound was subjected to a 180°C and 10 N / mm2 The mixture was processed at a pressure of 100 psi for 10 minutes into press plates of various thicknesses.

[0056] 4. Testing and evaluation of specimens The injection molded plate obtained in 2.1 and the press plate obtained in 3 were stored for 2 days under standard climatic conditions of 23° C. and 50% relative humidity.

[0057] 4.1 COF: Slip properties COF in accordance with ISO8295 - Plastics - Films and sheets - Determination of coefficient of friction The COF is expressed unitless and was measured using a press plate.

[0058] [Table 3]

[0059] By combining two types of additives (B) and (C), it became possible to reduce the sliding friction resistance and significantly improve the sliding characteristics. The coefficient of friction (CoF value) was reduced. A synergistic effect was clearly observed by adding additives (B) and (C).

[0060] 4.2 Flow Spiral The flow spiral was constructed according to 2.2.

[0061] [Table 4]

[0062] Very good results were obtained with the flow spiral: additive (B) Vinnex® significantly extended the flow path, and additive (C) Genioplast® provided an additional boost effect.

[0063] 4.3 MFR: Melt Mass Flow Rate The values ​​were determined on pellet material in accordance with DIN EN ISO1133.

[0064] [Table 5]

[0065] The melt mass flow rate profile was improved by adding both additives (B) and (C) in PBS.

[0066] 4.4 Transparency Clarity was assessed visually using injection molded plates.

[0067] The clarity of the cast plates was affected by Vinnex®; further addition of Genioplast® virtually eliminated any further turbidity.

[0068] 4.5 Ball Drop The ball drop test complies with the DIN EN ISO6272-2 standard.

[0069] [Table 6]

[0070] [Table 7]

[0071] Ball drop tests carried out showed that there was less surface damage when both additives were used in combination.

[0072] 4.6 Abrasion test The abrasion tests were carried out according to DIN 53516 - Tests on rubber and elastomers: Determination of abrasion -.

[0073] [Table 8]

[0074] Depending on the type of Vnnex® additive (B) used, wear was either reduced or worsened by more wear. Addition of additive (C) Genioplast® not only reduced wear, but also counteracted the negative effect of additive (B) on wear. A synergistic effect of adding additives (B) and (C) was clearly seen.

[0075] 4.7 Elixir Scratch Test: Scratch Resistance The Elixens scratch test was carried out according to PV3974-Scratch resistance test-.

[0076] Using an Elixin scratch hardness tester (Model 430 PI), scratches were made on the smooth injection molded plate obtained in 2.1 with a force of 10 N at a speed of 1000 mm / min.

[0077] Scratches were assessed by confocal microscopy using optical microscopy.

[0078] [Table 9]

[0079] The addition of additive (B) Vinnex® to PLA and PBS had a negative effect on the scratch depth. This was not only counterbalanced but also significantly improved by the addition of additive (C) Genioplast®, i.e., the scratch resistance was improved. A synergistic effect by adding additives (B) and (C) was clearly seen. In this case, a dosage of 2 wt.% of Genioplast® is recommended.

[0080] 4.8 Tensile Test Tensile tests were carried out using DIN EN ISO 5271B.

[0081] [Table 10]

[0082] Tensile tests showed that the elongation at break was significantly improved in the filled systems, where the combination of additives (B) and (C), Vinnex® and Genioplast®, proved to be effective.

[0083] 4.9 Tear propagation test Tear propagation tests were carried out on blown films using angle specimens according to DIN 53515 version 01 / 1990 and according to Graves with incision.

[0084] [Table 11]

[0085] In summary, by adding additives (B) and (C) to the biopolymer of the present invention, the following advantageous results were achieved:

[0086] The use of both additives in the processing process resulted in the greatest reduction in torque and power consumption during the compounding process.

[0087] Sliding properties: The coefficient of friction value is measured using a CoF measuring device. The combination of the two additives makes it possible to improve the sliding properties. The combination of the two additives (B) and (C) produces a synergistic effect.

[0088] Flow Path: Upon further processing using an injection molding machine, it was found that additive (B) significantly extended the flow path, and additive (C) provided an additional boost effect.

[0089] Melt Mass Flow Rate (MFR) The melt mass-flow rate profile was improved by adding additives (B) and (C) in PBS.

[0090] Transparency: The clarity of the molded plates was found to be affected by additive (B): further addition of additive (C) resulted in virtually no further turbidity.

[0091] Ball Drop Test: Ball drop tests were carried out and it was found that the combination of both additives (B) and (C) caused less surface damage, more specifically the addition of additive (C) enhanced this effect.

[0092] Abrasion resistance: The wear resistance is measured by a friction wheel test. Depending on the type of additive (B), wear was either reduced or increased. The addition of additive (C) almost completely counteracted this effect, reducing wear. This applies equally to both types of plastic. The combination of the two additives (B) and (C) resulted in a synergistic effect.

[0093] Scratch Depth: The addition of additive (B) to PLA and PBS had a negative effect on the scratch depth. Not only could this be counteracted by the addition of additive (C), but a significant improvement was achieved, especially at higher doses of additive (C), i.e., the scratch resistance was improved. The combination of the two additives (B) and (C) resulted in a synergistic effect.

[0094] Tensile test: Tensile tests showed that the elongation at break was significantly improved in the filled systems, where the combination of additives (B) and (C) proved to be effective.

[0095] The addition of additives (B) and (C) according to the invention improves, as a result of a synergistic effect, the surface properties, such as scratch and abrasion resistance, the mechanical properties and the processability of bioplastics.

Claims

1. (A) polylactic acid (PLA), Polybutylene succinate (PBS), Polybutylene succinate adipate (PBSA), Thermoplastic starch (TPS), Polyhydroxyalkanoates (PHAs), Polybutylene adipate terephthalate (PBAT), Polybutylene sebacate terephthalate (PBST), Polyhydroxybutyric acid (PHB), Polycaprolactone (PCL) and Cellophane (CA), and A mixture of them 65 to 99.4% by weight of a biopolymer selected from the group consisting of: (B) 0.5 to 30% by weight of a vinyl acetate homopolymer, copolymer, or terpolymer; and (C) (1) General formula R r SiO (4-r/2) (I) [In the general formula, R is the same or different and is a substituted or unsubstituted hydrocarbon group, and r is 0, 1, 2 or 3, with the proviso that the average value of r is in the range of 1.9 to 2.1.] 100 parts by weight of at least one polyorganosiloxane composed of units (2) 1 to 200 parts by weight of a reinforcing or non-reinforcing filler or a mixture thereof, (3) 0.01 to 20 parts by weight of a boric acid-containing additive for producing a pellet material; and (4) Optionally, further auxiliaries selected from the group of processing aids, plasticizers, pigments and stabilizers. Organopolysiloxane pellets having a particle size of 1 to 100 mm are contained in an amount of 0.1 to 5% by weight. A composition comprising: The composition, wherein the weight percent contents of components (A), (B) and (C) are each based on the total weight of the composition.

2. The vinyl acetate homopolymer, copolymer or terpolymer used is Vinyl acetate homopolymer, Copolymers of vinyl acetate and ethylene, Copolymers of vinyl acetate and vinyl laurate, Terpolymer of vinyl acetate, ethylene and versatic ester, Terpolymers of vinyl acetate, ethylene and acrylates; Terpolymers of vinyl acetate, vinyl laurate and vinyl acrylate, and A mixture of them The composition of claim 1 selected from the group consisting of:

3. The composition according to claim 1 or 2, wherein the polyorganosiloxane (1) is a diorganopolysiloxane having a trialkylsiloxy group, a trimethylsiloxy group, a dimethylhydroxysiloxy group, or a dimethylvinylsiloxy group as a terminal group.

4. The polyorganosiloxane (1) has a viscosity of 1,000,000 to 100,000,000 mm at 25° C. 2 4. The composition according to claim 1, 2 or 3, having a viscosity of 0.1 g / s (measured according to DIN 1342-2, version 2003-11).

5. 13. A method for producing the composition of claim 1, comprising: (A) polylactic acid (PLA), Polybutylene succinate (PBS), Polybutylene succinate adipate (PBSA), Thermoplastic starch (TPS), Polyhydroxyalkanoates (PHAs), Polybutylene adipate terephthalate (PBAT), Polybutylene sebacate terephthalate (PBST), Polyhydroxybutyric acid (PHB), Polycaprolactone (PCL) and Cellophane (CA), and A mixture of them 65 to 99.4% by weight of a biopolymer selected from the group consisting of: (B) 0.5 to 30% by weight of a vinyl acetate homopolymer, copolymer, or terpolymer; and (C) (1) General formula R r SiO (4-r/2) (I) [In the general formula, R is the same or different and is a substituted or unsubstituted hydrocarbon group, and r is 0, 1, 2 or 3, with the proviso that the average value of r is in the range of 1.9 to 2.1.] 100 parts by weight of at least one polyorganosiloxane composed of units (2) 1 to 200 parts by weight of a reinforcing or non-reinforcing filler or a mixture thereof, (3) 0.01 to 20 parts by weight of a boric acid-containing additive for producing a pellet material; and (4) Optionally, further auxiliaries selected from the group of processing aids, plasticizers, pigments and stabilizers. Organopolysiloxane pellets having a particle size of 1 to 100 mm are contained in an amount of 0.1 to 5% by weight. mixing the mixture; The method, wherein the weight percent contents of components (A), (B) and (C) are each based on the total weight of the composition.

6. The vinyl acetate homopolymer, copolymer or terpolymer used is Vinyl acetate homopolymer, Copolymers of vinyl acetate and ethylene, Copolymers of vinyl acetate and vinyl laurate, Terpolymer of vinyl acetate, ethylene and versatic ester, Terpolymers of vinyl acetate, ethylene and acrylates; Terpolymers of vinyl acetate, vinyl laurate and vinyl acrylate, and A mixture of them The method of claim 5, wherein the compound is selected from the group consisting of:

7. The method according to claim 5 or 6, wherein the polyorganosiloxane (1) is a diorganopolysiloxane having a trialkylsiloxy group, a trimethylsiloxy group, a dimethylhydroxysiloxy group or a dimethylvinylsiloxy group as a terminal group.

8. The polyorganosiloxane (1) has a viscosity of 1,000,000 to 100,000,000 mm at 25° C. 2 8. The method according to claim 5, 6 or 7, wherein the composition has a viscosity of 0.15 g / s (measured according to DIN 1342-2, version 2003-11).

Citation Information

Patent Citations

  • Organopolysiloxane granule, its producing method, and its application

    JP2005029792A

  • Composition and film containing polylactic acid polymer, polyvinyl acetate polymer and plasticizer

    JP2018502957A

  • Scratch resistant polymer composition

    US20210032447A1