Manufacturing method of aluminum alloy parts
The method improves high-temperature strength and rigidity of aluminum alloy parts by using specific alloy compositions and plastic working techniques, addressing the limitations of existing heat-resistant parts in high-speed, high-temperature environments.
Patent Information
- Application Number
- JP2020128343
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2020-07-29
- Publication Date
- 2024-12-04
- Estimated Expiration
- 2040-07-29
AI Technical Summary
Existing heat-resistant parts, such as compressor wheel impellers and rotor blades, face challenges in achieving high-temperature strength and rigidity due to increased operating speeds and temperatures, with forged alloy products lacking sufficient high-temperature properties.
A manufacturing method for aluminum alloy parts with specific alloy compositions (1.90 to 2.70% Cu, 1.30 to 1.80% Mg, 0.90 to 1.30% Fe, 0.90 to 1.20% Ni, 0.04 to 0.10% Ti, and limited amounts of Zn, Pb, Sn, and Bi) combined with homogenization and plastic working at an area reduction rate of 20.0 to 99.0%, followed by heat treatment.
The method produces aluminum alloy parts with enhanced high-temperature strength and rigidity, preventing creep deformation and maintaining strength in environments up to 280°C, suitable for high-speed applications.
Smart Images

Figure 0007594378000002 
Figure 0007594378000003 
Figure 0007594378000004
Abstract
Description
[Technical field]
[0001] The present invention relates to a method for manufacturing an aluminum alloy part, and more particularly to a method for manufacturing an aluminum alloy part by performing plastic working. [Background technology]
[0002] Heat-resistant parts such as compressor wheel impellers of turbochargers as internal combustion engines of transport equipment such as automobiles and ships, impellers of turbomolecular pumps which are mechanical vacuum pumps, and rotor blades of large blowers in thermal power plants are rotated at speeds of 100 to 10,000 rpm or more in high-temperature environments of 100 to 280°C. Therefore, materials used for these heat-resistant parts are required to have high strength and high rigidity under high temperatures. In addition, compressor wheel impellers are required to be lightweight in order to reduce energy loss, and are also required to have strength that can withstand high-speed rotation.
[0003] For example, conventionally, these heat-resistant parts were manufactured by cutting cast or forged products with the alloy composition of alloy 2618. However, in recent years, the speed and precision of cutting processes have increased, and cutting products are increasingly being made from aluminum extrusions, which has created a need for improved machinability and high-temperature strength.
[0004] For example, an Al-Cu-Mg aluminum alloy forging has been disclosed that has improved strength in a high-temperature environment of about 170° C. compared to conventional products (see Patent Document 1). [Prior art documents] [Patent documents]
[0005] [Patent Document 1] JP 2020-90726 A DISCLOSURE OF THEINVENTION [Problem to be solved by the invention]
[0006] From the viewpoint of reducing the environmental load, the above-mentioned heat-resistant parts are required to rotate at higher speeds than at present and to withstand further increases in operating temperature. However, the Al-Cu-Mg-based aluminum alloy forged product of Patent Document 1 has a problem in that it lacks high-temperature strength and rigidity at high temperatures.
[0007] The present invention has been made in consideration of the above-mentioned problems, and has an object to provide a technique capable of improving high-temperature strength and rigidity at high temperatures. [Means for solving the problem]
[0008] In order to achieve the above object, in a method for producing an aluminum alloy part of the present invention, a continuous cast material containing 1.90 to 2.70 mass% Cu, 1.30 to 1.80 mass% Mg, 0.90 to 1.30 mass% Fe, 0.90 to 1.20 mass% Ni, 0.04 to 0.10 mass% Ti, less than 0.25 mass% Si, less than 0.010 mass% Zn, less than 0.050 mass% Pb, less than 0.050 mass% Sn, less than 0.050 mass% Bi, with the balance being Al and unavoidable impurities, is subjected to a homogenization treatment and then subjected to a process for producing an aluminum alloy part having a cross-sectional area reduction rate of 20.0 to 99.0%. forging Processing is performed.
[0009] According to the manufacturing method of the aluminum alloy part configured as described above, it is possible to obtain an aluminum alloy part having excellent high-temperature strength and rigidity at high temperatures. [Brief description of the drawings]
[0010] [Figure 1] 1A to 1C are schematic diagrams showing examples of plastic processing of an aluminum alloy part. [Diagram 2] 1A to 1C are schematic diagrams showing examples of plastic processing of an aluminum alloy part. [Diagram 3] 1A to 1C are schematic diagrams showing examples of plastic processing of an aluminum alloy part. [Figure 4] 1 is a graph showing creep strength of examples and comparative examples. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0011] Hereinafter, an embodiment of the present invention will be described. <Alloy composition> The aluminum alloy part of the present invention has an alloy composition containing 1.90 to 2.70 mass% Cu, 1.30 to 1.80 mass% Mg, 0.90 to 1.30 mass% Fe, 0.90 to 1.20 mass% Ni, 0.04 to 0.10 mass% Ti, less than 0.25 mass% Si, less than 0.010 mass% Zn, less than 0.050 mass% Pb, less than 0.050 mass% Sn, less than 0.050 mass% Bi, with the balance being Al and unavoidable impurities.
[0012] In the alloy composition, Cu is an element that needs to be added to improve room temperature strength and high temperature strength. If the Cu content is less than 1.90 mass%, it is not preferable because it is not possible to obtain a sufficient effect of improving strength. Also, if the Cu content exceeds 2.70 mass%, it is not preferable because castability is deteriorated and cracks are likely to occur during solidification. Therefore, it is preferable that the Cu content is 1.90 to 2.70 mass%.
[0013] Like Cu, Mg is an element that needs to be added to improve room temperature strength and high temperature strength. If the Mg content is less than 1.30 mass%, it is not preferable because it is not possible to obtain a sufficient effect of improving strength. Also, if the Mg content exceeds 1.80 mass%, it is not preferable because the oxidation of the molten metal during casting becomes significant and it becomes difficult to control the Mg content. Therefore, the Mg content should be 1.30 to 1.80 mass%.
[0014] Fe is an element added to improve high-temperature strength. If the Fe content is less than 0.90 mass%, it is not preferable because it is not possible to obtain a sufficient effect of improving strength. Also, if the Fe content exceeds 1.30 mass%, it is not preferable because it combines with Cu to form crystallized products, which leads to a decrease in strength. Therefore, the Fe content should be 0.90 to 1.30 mass%.
[0015] Ni is an element added to improve high-temperature strength, similar to Fe. If the Ni content is less than 0.90 mass%, sufficient strength improvement effect cannot be obtained, which is not preferable. If the Ni content exceeds 1.20 mass%, Ni combines with Fe to generate giant crystals, which leads to a decrease in strength and cracks during plastic processing, which is not preferable. Therefore, the Ni content should be 0.90 to 1.20 mass%.
[0016] Ti is an element that refines the metal structure formed during casting and stabilizes mechanical properties. If the Ti content is less than 0.04 mass%, it is not preferable because it is not possible to obtain a sufficient effect of refining the metal structure. Also, if the Ti content exceeds 0.10 mass%, it is not preferable because it combines with Al to generate giant crystals, which leads to a decrease in strength and cracks during plastic processing. Therefore, the Ti content should be 0.04 to 0.10 mass%.
[0017] Incidentally, aluminum alloys obtained in actual operation contain various unavoidable impurities. The Al-Cu-Mg aluminum alloy based on the 2618 alloy according to the present invention also contains unavoidable impurities similar to those of other JISS2000 series aluminum alloys. Until now, it was believed that there would be no particular problem if the unavoidable impurities were less than 0.05% by mass individually and less than 0.15% by mass in total.
[0018] However, as a result of investigations by the inventors of the present invention, it has become clear that, among the unavoidable impurities, Zn, Pb, Bi, and Sn have a significant effect on the high-temperature properties of Al-Cu-Mg aluminum alloys based on the 2618 alloy.
[0019] Zn is an element that is unevenly distributed in the grain boundaries of the metal structure, and reduces the strength in a high-temperature environment of 100°C or higher, significantly reducing the rigidity at high temperatures. Therefore, the Zn content must be limited to less than 0.010% by mass. More preferably, the Zn content is less than 0.005% by mass in order to more reliably obtain the above-mentioned effects.
[0020] Pb is an element that reacts with Al at 327°C or higher to produce a liquid phase, and significantly reduces the strength and rigidity of the material in a high-temperature environment of 100 to 280°C. Therefore, the Pb content is limited to less than 0.050% by mass, and preferably less than 0.010% by mass. More preferably, the Pb content is less than 0.005% by mass, in order to more reliably obtain the above-mentioned effects.
[0021] Sn is an element that reacts with Al at 228.3°C or higher to produce a liquid phase, and like Pb, it significantly reduces the strength and rigidity of the material in a high-temperature environment of 100 to 280°C. Therefore, the Sn content is limited to less than 0.050 mass%, and preferably less than 0.010 mass%. More preferably, the Sn content is less than 0.005 mass%, so that the above-mentioned effects can be obtained more reliably.
[0022] Bi is an element that reacts with Al at 271.4°C or higher to produce a liquid phase, and like Pb and Sn, it significantly reduces the strength and rigidity of the material in a high-temperature environment of 100 to 280°C. Therefore, the Bi content is limited to less than 0.050 mass%, and preferably less than 0.010 mass%. More preferably, when the Bi content is less than 0.005 mass%, the above effect can be obtained more reliably.
[0023] <Manufacturing method> In the present invention, for example, a continuous cast material (billet or slab) having the above alloy composition is produced by melting using a known method, and then homogenized, and then hot or a combination of hot and cold plastic working is performed so that the cross-sectional area reduction rate is 20.0 to 99.0%, preferably 80.0 to 95.0%, to obtain an aluminum alloy part. The shape of the continuous cast material can be, for example, a cylindrical shape.
[0024] In the present invention, the area reduction rate is a value calculated by the following formula (1). Area reduction rate (%)=((Aa) / A)×100 (1) In formula (1), a is the cross-sectional area of "a plane perpendicular to the central axis of an aluminum alloy part obtained by carrying out the manufacturing method of an aluminum alloy part of the present invention". A is the area of "the plane having the largest area among the cross sections of the continuous cast material before carrying out the manufacturing method of an aluminum alloy part of the present invention" corresponding to "the plane perpendicular to the central axis of an aluminum alloy part obtained by carrying out the manufacturing method of an aluminum alloy part of the present invention". Note that "the continuous cast material before carrying out the manufacturing method of an aluminum alloy part of the present invention" is the continuous cast material to be subjected to the manufacturing method of an aluminum alloy part of the present invention. In addition, in the manufacturing method of an aluminum alloy part of the present invention, when multiple plastic working processes are performed, the cross-sectional area reduction rate is defined as "a" for the cross-sectional area of the plastic worked material after the last plastic working process, and "A" for the cross-sectional area of the continuous cast material before the first plastic working process.
[0025] For example, as shown in the embodiment in Fig. 1, when a cylindrical forged round bar 20a is obtained by performing forging processing in which a cylindrical continuous cast material 10a is compressed in a central axis direction 11a at a hot temperature and expanded in a diametric direction, the cross-sectional area of the forged round bar 20a perpendicular to the central axis direction is "a", and the cross-sectional area of the cross-section when cut on a plane including the central axis of the continuous cast material 10a is "A". In the embodiment shown in Fig. 1, the shape of the cross-section of the forged round bar 20a perpendicular to the central axis direction is circular, and the shape of the cross-section when cut on a plane including the central axis of the continuous cast material 10a is rectangular. The central axis direction means the longitudinal direction of the continuous cast material 10a or the forged round bar 20a.
[0026] Also, for example, as in the embodiment shown in Fig. 2, when a cylindrical forged round bar 20b is obtained by performing a forging process in which a cylindrical continuous cast material 10b is compressed in a diameter direction 11b by hot working and expanded in a central axis direction, the cross-sectional area of the forged round bar 20b perpendicular to the central axis direction is "a", and the cross-sectional area of the continuous cast material 10b perpendicular to the central axis direction is "A". In the embodiment shown in Fig. 2, the shape of the cross-section perpendicular to the central axis direction of the forged round bar 20b is circular, and the shape of the cross-section perpendicular to the central axis direction of the continuous cast material 10b is also circular. The central axis direction means the longitudinal direction of the continuous cast material 10b or the forged round bar 20b.
[0027] Also, for example, as in the embodiment shown in Fig. 3, when a cylindrical forged round bar 20c is obtained by hot extrusion of a cylindrical continuous cast material 10c in a central axis direction 11c, the cross-sectional area of the forged round bar 20c perpendicular to the central axis direction is "a", and the cross-sectional area of the continuous cast material 10c perpendicular to the central axis direction is "A". In the embodiment shown in Fig. 3, the shape of the cross-section perpendicular to the central axis direction of the forged round bar 20c is circular, and the shape of the cross-section perpendicular to the central axis direction of the continuous cast material 10c is also circular. The central axis direction means the longitudinal direction of the continuous cast material 10c or the forged round bar 20c.
[0028] In the method for producing an aluminum alloy part of the present invention, the continuous cast material may be subjected to only one type of hot plastic working after the homogenization treatment.
[0029] In addition, in the manufacturing method of the aluminum alloy part of the present invention, two or more kinds of hot plastic processing can be combined. For example, after homogenization treatment of the continuous cast material, first, a first forging process is performed in which the cylindrical continuous cast material is compressed in the central axis direction and expanded in the diametric direction, and then, a second forging process is performed in which the obtained cylindrical first forged material is compressed in the diametric direction and expanded in the central axis direction to obtain a plastically processed material (forged round bar). In this case, the cross-sectional area of the cross section when cut along a plane including the central axis of the cylindrical continuous cast material before the first casting process is "A", and the cross-sectional area of the cross section perpendicular to the central axis direction of the plastically processed material (forged round bar) after the second forging process is "a".
[0030] In the method for producing an aluminum alloy part of the present invention, the continuous cast material may be subjected to a homogenization treatment, followed by hot plastic working, and then further plastic working into a forged round bar.
[0031] The shape of the plastically worked product obtained by subjecting the continuous cast material to plastic working may be, for example, a round bar shape.
[0032] By subjecting the plastically worked product obtained by subjecting the continuous cast material to plastic working, strength and rigidity in a high-temperature environment can be obtained more reliably. For example, the heat treatment may be performed in the order of solution treatment, quenching treatment, and aging treatment. In the solution treatment, the heating temperature is preferably 500 to 540°C, and the treatment time is preferably 1 to 15 hours. In the quenching treatment, cooling with water at 15 to 90°C is preferably performed. In the aging treatment, the heating temperature is preferably 170 to 230°C, and the treatment time is preferably 1 to 24 hours.
[0033] The heat-treated plastically worked product is then cut to be shaped according to the intended use, to obtain heat-resistant parts such as compressor wheel impellers for turbochargers in internal combustion engines for transport equipment, impellers for turbomolecular pumps, rotor blades for large-scale blowers, etc. This cutting process may be performed before or after the heat treatment.
[0034] The plastic processing according to the present invention is preferably a forging process for compressing in the axial direction (the longitudinal direction of the member before processing) or an extrusion process for extruding in the axial direction (the longitudinal direction of the member before processing), and may be performed in combination, or one of these processes may be performed multiple times. The plastic processing according to the present invention may be only hot plastic processing, or may be a combination of hot and cold plastic processing, for example, a plastic processing in which hot plastic processing is performed once or multiple times, and then cold finishing plastic processing is performed. The reduction in area in the plastic processing is preferably set to 20.0 to 99.0%, preferably 80.0 to 95.0%. By setting this reduction in area within the above-mentioned specified range, sufficient room temperature strength, high temperature strength, and rigidity at high temperatures can be reliably obtained.
[0035] In the aluminum alloy parts manufactured by the manufacturing method of the present invention described above, normal temperature strength, high temperature strength, and rigidity at high temperature are increased. In particular, creep resistance, which is one of the rigidity characteristics at high temperature, is increased. And, since creep resistance is high, high strength is maintained even at high temperature. Therefore, by using the aluminum alloy parts manufactured by the present invention as the heat-resistant parts used in a high temperature environment of 100 to 280 ° C, it is possible to suppress aging deformation (creep deformation) under load in a high temperature environment. Furthermore, it is possible to stabilize the performance of the entire system in which the heat-resistant parts are incorporated (for example, fuel efficiency performance in the case of a compressor wheel of a turbocharger), and to extend the product life.
[0036] In this way, according to the manufacturing method of the present invention, it is possible to manufacture aluminum alloy parts, forged preforms, extruded blank rods, and heat-resistant parts such as compressor wheel impellers of turbochargers, impellers of turbomolecular pumps, and rotor blades of large-sized blowers as internal combustion engines of transportation equipment, all of which have the above-mentioned excellent performance. EXAMPLES
[0037] Examples related to the present invention and comparative examples for comparison with the examples will be described in detail below.
[0038] <Alloy composition> As shown in Table 1, three types of alloys A, B, and C with different alloy compositions were prepared. Alloy A is an alloy (embodiment) defined in the present invention. Alloys B and C are comparative materials (comparative examples), and have a higher Zn content than the composition of alloy A. Alloys with a content below the lower measurement limit are indicated in Table 1 as "not detected."
[0039] [Table 1]
[0040] <Casting and homogenization treatment> Alloys A, B, and C were cast into cylindrical billets with a diameter of 600 mm and a length of 1000 mm, and then homogenized at 495°C for 14 hours.
[0041] <Plastic processing (hot forging)> As shown in FIG. 1, the continuous cast material 10a obtained by the homogenization treatment was subjected to hot upset forging in the axial direction, and further stretched in the radial direction of the continuous cast material 10a by hot forging to produce a cylindrical forged round bar (plastic processed product) 20a with a diameter of 271 mm and a length of 4550 mm. When the cross-sectional area of the forged round bar 20a is a and the cross-sectional area of the raw continuous cast material 10a is A, the cross-sectional area reduction rate defined as "Cross-sectional area reduction rate (%) = ((Aa) / A) x 100" was 90.3%. In FIG. 1, the cross-sectional area A of the continuous cast material 10a is the area of a rectangular cross section obtained by cutting the continuous cast material 10a on a plane including the central axis. The cross-sectional area a of the forged round bar 20a is the area of a circular cross section obtained by cutting the forged round bar 20a on a plane perpendicular to the central axis in FIG. 1.
[0042] By subjecting the forged round bar 20a of alloy A produced in the manner described above to the heat treatment and cutting process described above, heat-resistant parts such as compressor wheel impellers of turbochargers for internal combustion engines of transportation equipment, impellers of turbomolecular pumps, and rotor blades of large blowers can be manufactured.
[0043] <Creep test> A cylinder with a diameter of 271 mm and a length of 255 mm was cut out from the forged round bar 20a described above, and then cut in the radial direction to obtain a plate with a length of about 271 mm, a width of 255 mm, and a thickness of 95 mm. The plate was subjected to the same heat treatment as that used in manufacturing the heat-resistant part. Specifically, the plate was subjected to a solution treatment at 530°C for 7 hours, a quenching treatment in which the plate was immersed in water at 90°C, and an aging treatment at 200°C for 12 hours in that order.
[0044] Test pieces specified in "JIS Z 2271: Test methods for creep and creep rupture testing of metallic materials" were cut out from the heat-treated plate material so that the radial direction of the forged round bar 20a was the longitudinal direction, and creep tests were carried out at 120°C in accordance with the same standard.
[0045] FIG. 4 shows the results of the creep test. The vertical axis of FIG. 4 shows creep strain (amount of creep deformation), and the horizontal axis shows time. As is clear from FIG. 4, the alloys A (A-1, A-2) of the examples have sufficiently suppressed creep strain at the time of 500 hr retention, and exhibit excellent rigidity at 120°C, compared with the alloys B and C (C-1, C-2) of the comparative examples. In contrast, the creep strain of the comparative alloys B and C is not sufficiently suppressed, and it was found that the rigidity at 120°C is low.
[0046] As described above, the aluminum alloy parts of the examples manufactured by the manufacturing method of the present invention have excellent rigidity, particularly at high temperatures, and are therefore suitable for heat-resistant parts such as compressor wheel impellers of turbochargers in internal combustion engines of transportation equipment, impellers of turbomolecular pumps, and rotor blades of large-sized blowers. [Explanation of symbols]
[0047] 10 Continuous casting material 11a, 11c Center axis direction 11b Diameter direction 20 Forged round bars (plastic processed products)
Claims
1. A continuous cast material containing 1.90 to 2.70 mass% Cu, 1.30 to 1.80 mass% Mg, 0.90 to 1.30 mass% Fe, 0.90 to 1.20 mass% Ni, 0.04 to 0.10 mass% Ti, less than 0.25 mass% Si, less than 0.010 mass% Zn, less than 0.050 mass% Pb, less than 0.050 mass% Sn, less than 0.050 mass% Bi, with the balance being Al and unavoidable impurities, is subjected to a homogenization treatment and then forged to a cross-sectional area reduction rate of 20.0 to 99.0%. Manufacturing method of aluminum alloy parts.
2. A continuous cast material containing 1.90 to 2.70 mass% Cu, 1.30 to 1.80 mass% Mg, 0.90 to 1.30 mass% Fe, 0.90 to 1.20 mass% Ni, 0.04 to 0.10 mass% Ti, less than 0.25 mass% Si, less than 0.010 mass% Zn, less than 0.010 mass% Pb, less than 0.010 mass% Sn, less than 0.010 mass% Bi, with the balance being Al and unavoidable impurities, is subjected to a homogenization treatment and then forged to a cross-sectional area reduction rate of 20.0 to 99.0%. Manufacturing method of aluminum alloy parts.
3. The forged product obtained by the forging process is subjected to a heat treatment. The method for producing an aluminum alloy part according to claim 1 or 2.
4. The heat treatment includes a solution treatment, a quenching treatment, and an aging treatment, in that order. In the solution treatment, the solution is heated at a temperature of 500 to 540° C. for 1 to 15 hours, In the quenching treatment, the quenching is performed by cooling with water at 15 to 90°C. In the aging treatment, heating is performed at a temperature of 170 to 230° C. for 1 to 24 hours. The method for producing an aluminum alloy part according to claim 3.
5. A cutting process is performed on the forged product before the heat treatment. The method for producing an aluminum alloy part according to claim 3 or 4.
6. The forged product after the heat treatment is subjected to a cutting process. The method for producing an aluminum alloy part according to claim 3 or 4.
Citation Information
Patent Citations
Manufacturing technique of high-heat-resistance 2618 alloy extrusion bar
CN107236916A
Aluminum alloy material for engine member
JP1989152237A
Heat-resistant aluminum-alloy extruded material and heat treatment method therefor
JP2008101264A
Spool valve
JP2010276088A
Cold forging material for impeller, and manufacturing method therefor
JP2020012182A