Thermally conductive resin composition, heat dissipation structure, and method for producing thermally conductive resin composition

A thermally conductive resin composition with three types of alumina particles and optional fibers improves filling rates, achieving high thermal conductivity for efficient heat dissipation.

JP7594419B2Active Publication Date: 2024-12-04IBIDEN CO LTD
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
JP2020199622
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2020-12-01
Publication Date
2024-12-04
Estimated Expiration
2040-12-01

AI Technical Summary

Technical Problem

Existing thermally conductive resin compositions with two components of alumina particles of different average particle diameters struggle to achieve high thermal conductivity due to insufficient filling rates.

Method used

A thermally conductive resin composition comprising at least three types of alumina particles with different average particle diameters, where the content ratios satisfy R1≧(R2+R3), and optionally including alumina fibers, to enhance filling rates and thermal conductivity.

Benefits of technology

The composition achieves thermal conductivity of 3.5 W/m·K or more, effectively dissipating heat from semiconductor devices and other heat sources.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007594419000003
    Figure 0007594419000003
  • Figure 0007594419000004
    Figure 0007594419000004
  • Figure 0007594419000005
    Figure 0007594419000005
Patent Text Reader

Abstract

To provide a heat-conductive resin composition excellent in heat conductivity.SOLUTION: A heat-conductive resin composition includes a resin, and alumina particles included in the resin, where at least three kinds of alumina particles having different average particle diameters are included, the average particle diameter of any kind of alumina particles is 30 μm or less, at least the three kinds of alumina particles include a first alumina particle, a second alumina particle having an average particle diameter smaller than that of the first alumina particle, and a third alumina particle having an average particle diameter smaller than that of the second alumina particle, and when the content ratios of the first alumina particle, the second alumina particle, and the third alumina particle are R1, R2, and R3, respectively in terms of volume ratio, the relation R1≥(R2+R3) is satisfied.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a thermally conductive resin composition, a heat dissipation structure, and a method for producing the thermally conductive resin composition. [Background technology]

[0002] A semiconductor element is composed of a conductor for electrical conduction and an insulating material. In recent years, the amount of heat generated by semiconductor elements has increased due to the increase in output. Therefore, how to dissipate the heat generated by the semiconductor elements has become an important issue.

[0003] Patent Document 1 describes a highly thermally conductive resin composition. This composition contains 80-90 volume % of spherical aluminum oxide powder having an average particle size of 10-50 μm and an average sphericity of 0.85 or more, and aluminum oxide powder having an average particle size of 0.3-1 μm, in a volume ratio of 5:5-9.5:0.5. [Prior art documents] [Patent documents]

[0004] [Patent Document 1] Patent No. 5755977 Summary of the Invention [Problem to be solved by the invention]

[0005] The composition described in Patent Document 1 uses two alumina particles with different average particle sizes, but because it is a two-component composition, it is difficult to sufficiently increase the filling rate of the alumina particles in the composition, and therefore there is a problem that it is difficult to obtain high thermal conductivity with such a composition.

[0006] The present invention has been made in view of the above problems, and an object of the present invention is to provide a thermally conductive resin composition having excellent thermal conductivity. [Means for solving the problem]

[0007] That is, the thermally conductive resin composition of the present invention is a thermally conductive resin composition consisting of a resin and alumina particles contained in the resin, and contains at least three types of alumina particles having different average particle diameters, and the average particle diameter of each type of alumina particle is 30 μm or less, the at least three types of alumina particles include first alumina particles, second alumina particles having an average particle diameter smaller than that of the first alumina particles, and third alumina particles having an average particle diameter smaller than that of the second alumina particles, and is characterized in that, when the content ratios of the first alumina particles, the second alumina particles, and the third alumina particles are R1, R2, and R3, respectively, in volume ratio, the relationship R1≧(R2+R3) is satisfied.

[0008] The thermally conductive resin composition of the present invention contains at least three types of alumina particles having different average particle sizes, each of which has an average particle size of 30 μm or less, and further, the content ratios (volume %) of the first to third types of alumina particles satisfy the relationship R1≧(R2+R3), thereby improving the filling rate of the alumina particles in the thermally conductive resin composition, and thus making it possible to provide a thermally conductive resin composition having high thermal conductivity.

[0009] The thermally conductive resin composition of the present invention preferably further satisfies the relationship R1>R2>R3.

[0010] The thermally conductive resin composition of the present invention preferably further satisfies the relationship R1≧2×R3.

[0011] In the thermally conductive resin composition of the present invention, it is preferable that the first alumina particles have an average particle size of 10 to 30 μm, the second alumina particles have an average particle size of 1.5 to 5 μm, and the third alumina particles have an average particle size of 0.1 to 1 μm.

[0012] In the thermally conductive resin composition of the present invention, the filling rate of the at least three types of alumina particles is preferably 80 vol % or more and 95 vol % or less. By setting the filling rate of the alumina particles to 80 volume % or more, the effect of increasing the thermal conductivity is more suitably exhibited.

[0013] The thermally conductive resin composition of the present invention preferably has a thermal conductivity of at least 3.5 W / m K. When the thermal conductivity is at least 3.5 W / m K, the thermal conductivity is particularly excellent, and the composition can be more suitably used as a thermally conductive resin composition.

[0014] In the thermally conductive resin composition of the present invention, the at least three types of alumina particles are preferably surface-treated with a dispersing agent. Such particles have good compatibility with resins, particularly silicone resins, and can more effectively increase the filling rate of the alumina particles in the thermally conductive resin composition, resulting in a thermally conductive resin composition with higher thermal conductivity.

[0015] The thermally conductive resin composition of the present invention preferably further contains alumina fibers. Alumina fibers are generally longer than alumina particles and form an effective heat transfer path, so by further including alumina fibers, a thermally conductive resin composition having a higher thermal conductivity can be obtained.

[0016] The heat dissipation structure of the present invention is characterized by comprising a heat source, a heat dissipation member, and the thermally conductive resin composition of the present invention disposed between the heat source and the heat dissipation member. With this structure, heat from a heat source can be suitably conducted to the heat dissipation member via the thermally conductive resin composition.

[0017] The method for producing a thermally conductive resin composition of the present invention is a method for producing a thermally conductive resin composition comprising a resin and alumina particles contained in the resin, and includes a mixing step of mixing at least three types of alumina particles having different average particle diameters, each of which has an average particle diameter of 30 μm or less, with a resin material, wherein the at least three types of alumina particles include first alumina particles, second alumina particles having an average particle diameter smaller than that of the first alumina particles, and third alumina particles having an average particle diameter smaller than that of the second alumina particles, and the mixing ratios of the first alumina particles, the second alumina particles, and the third alumina particles are R1, R2, and R3, respectively, in volume ratio, and the relationship R1≧(R2+R3) is satisfied.

[0018] In the method for producing a thermally conductive resin composition of the present invention, at least three types of alumina particles having different average particle sizes, all of which are 30 μm or less, are mixed with a resin material, and the mixing ratio (volume %) of the first to third types of alumina particles is set to R1≧(R2+R3), thereby improving the filling rate of the alumina particles in the produced thermally conductive resin composition, and thus a thermally conductive resin composition having high thermal conductivity can be produced.

[0019] In the method for producing a thermally conductive resin composition of the present invention, it is further preferable that the relationship R1>R2>R3 is satisfied.

[0020] In the method for producing a thermally conductive resin composition of the present invention, it is preferable that the relationship R1≧2×R3 is further satisfied.

[0021] In the method for producing a thermally conductive resin composition of the present invention, it is preferable that the first alumina particles have an average particle size of 10 to 30 μm, the second alumina particles have an average particle size of 1.5 to 5 μm, and the third alumina particles have an average particle size of 0.1 to 1 μm.

[0022] In the method for producing a thermally conductive resin composition of the present invention, it is preferable that the filling rate of the at least three types of alumina particles in the thermally conductive resin composition containing the at least three types of alumina particles and the resin is 80 volume % or more and 95 volume % or less. By setting the filling rate of the alumina particles to 80 volume % or more, the effect of increasing the thermal conductivity is more suitably exhibited.

[0023] In the method for producing a thermally conductive resin composition of the present invention, the at least three types of alumina particles are preferably surface-treated with a dispersing agent. Such particles have good compatibility with resins, particularly silicone resins, and can more effectively increase the filling rate of the alumina particles in the thermally conductive resin composition, resulting in a thermally conductive resin composition having higher thermal conductivity.

[0024] In the method for producing a thermally conductive resin composition of the present invention, in the mixing step, alumina fibers are preferably further mixed in addition to the at least three types of alumina particles and the resin. Alumina fibers are generally longer than alumina particles and form an effective heat transfer path, so by further mixing alumina fibers, a thermally conductive resin composition with higher thermal conductivity can be produced. [Brief description of the drawings]

[0025] [Figure 1] FIG. 1 is a cross-sectional view that illustrates a schematic diagram of one embodiment of the thermally conductive resin composition of the present invention. [Diagram 2] FIG. 2 is a cross-sectional view that illustrates a schematic diagram of another embodiment of the thermally conductive resin composition of the present invention. [Diagram 3] FIG. 3 is a cross-sectional view that illustrates a schematic diagram of another embodiment of the thermally conductive resin composition of the present invention. [Figure 4] FIG. 4 is a cross-sectional view that illustrates a schematic diagram of an embodiment of a heat dissipation structure.

[0026] Detailed Description of the Invention The thermally conductive resin composition and the heat dissipation structure of the present invention will be described in detail below. The thermally conductive resin composition of the present invention is a thermally conductive resin composition comprising a resin and alumina particles contained in the resin, At least three types of alumina particles having different average particle sizes are included, and the average particle size of each type of alumina particle is 30 μm or less; the at least three types of alumina particles include first alumina particles, second alumina particles having an average particle size smaller than that of the first alumina particles, and third alumina particles having an average particle size smaller than that of the second alumina particles; When the content ratios of the first alumina particles, the second alumina particles and the third alumina particles are R1, R2 and R3, respectively, in terms of volume ratio, the composition is characterized in that it satisfies the relationship R1≧(R2+R3).

[0027] FIG. 1 is a cross-sectional view that illustrates a schematic diagram of one embodiment of the thermally conductive resin composition of the present invention. The thermally conductive resin composition 10 shown in FIG. 1 is composed of a resin 20 and three types of alumina particles contained in the resin 20. The resin 20 matrix contains three types of alumina particles, namely, first alumina particles 31, second alumina particles 32, and third alumina particles 33. FIG. 1 shows a form in which the first alumina particles 31 and the second alumina particles 32 are spherical, and the third alumina particles are shapeless.

[0028] The resin is preferably at least one selected from the group consisting of epoxy resin, silicone resin, acrylic resin, polyimide resin, melamine resin, polycarbonate resin, polypropylene resin, and polyethylene resin. Of these, epoxy resins and silicone resins are preferred. Epoxy resins and silicone resins are preferred because they have high insulating properties and therefore can ensure insulating properties when the thermally conductive resin composition is used in contact with a semiconductor element or the like.

[0029] The second alumina particles have a smaller average particle size than the first alumina particles, and the third alumina particles have a smaller average particle size than the second alumina particles. Moreover, the average particle size of all types of alumina particles is 30 μm or less. That is, it is preferable that the thermally conductive resin composition does not contain any type of alumina particles having an average particle size exceeding 30 μm.

[0030] In the thermally conductive resin composition of the present invention, when the content ratios of the first alumina particles, the second alumina particles and the third alumina particles are R1, R2 and R3, respectively, in volume ratio, the relationship R1≧(R2+R3) is satisfied. Since the ratio of the first alumina particles having a large average particle size is high, the volume of the alumina particles in the thermal conductive resin composition is large, and the thermal conductivity is high. The spaces between the first alumina particles are filled with the second alumina particles having a medium average particle size. Furthermore, the spaces between the second alumina particles are filled with the third alumina particles having a small average particle size. By using three types of particles with different average particle sizes, the spaces between the alumina particles are filled with smaller alumina particles, improving the filling rate of the alumina particles in the thermal conductive resin composition, resulting in a thermal conductive resin composition with high thermal conductivity.

[0031] When an attempt is made to increase the filling rate of the alumina particles by blending a large amount of alumina particles with a small average particle size into a thermally conductive resin composition, a large number of interfaces between the alumina particles are generated, resulting in a decrease in thermal conductivity due to the presence of interfaces between the particles. However, by increasing the proportion of the first alumina particles with a large average particle size, the interfaces between the particles can be reduced, resulting in a thermally conductive resin composition with high thermal conductivity.

[0032] In addition, when the content ratios of the first alumina particles, the second alumina particles, and the third alumina particles in the thermally conductive resin composition are R1, R2, and R3, respectively, in terms of volume ratio, it is preferable that the relationship R1>R2>R3 is satisfied. When R2 is compared with R3, if R2 is larger than R3, the interface between particles can be reduced, and therefore the thermal conductivity of the thermally conductive resin composition can be further improved.

[0033] In addition, when the content ratios of the first alumina particles and the third alumina particles in the thermally conductive resin composition are R1 and R3, respectively, in terms of volume ratio, it is preferable that the relationship R1 ≥ 2 × R3 is satisfied. R1 being greater than twice R3 means that R3 is relatively small, and when R3 is small, the interface between particles can be reduced, so that the thermal conductivity of the thermally conductive resin composition can be further improved.

[0034] With respect to the content ratio of each alumina particle in the thermally conductive resin composition, on the premise that the relationship R1≧(R2+R3) is satisfied, the content ratio of the first alumina particles (R1) is preferably 50 to 65 volume % of all the alumina particles, the content ratio of the second alumina particles (R2) is preferably 26 to 30 volume % of all the alumina particles, and the content ratio of the third alumina particles (R3) is preferably 5 to 24 volume % of all the alumina particles.

[0035] The preferred average particle size of each alumina particle is as follows: The first alumina particles preferably have an average particle size of 10 to 30 μm. The second alumina particles preferably have an average particle size of 1.5 to 5 μm. The third alumina particles preferably have an average particle size of 0.1 to 1 μm. When the average particle size of each alumina particle falls within the above range, the thermal conductivity of the thermally conductive resin composition can be further improved.

[0036] The average particle size of the alumina particles in the thermally conductive resin composition can be measured by observation with a SEM (scanning electron microscope). The measurement conditions are preferably an acceleration voltage of 2 kV and a magnification of about 10,000 times.

[0037] The shape of each of the first alumina particles, the second alumina particles, and the third alumina particles is not particularly limited, and may be spherical, roundish, irregular, or the like. The concept of "spherical" includes so-called perfect spheres and nearly perfect spheres, and refers to particles with a sphericity of 0.85 or more. The term "rounded" refers to a shape that is rounded, and includes particles that are not as highly spherical as spherical particles. The sphericity of the particles is less than 0.85. The irregular shape may include angular parts and the length of the short axis and the long axis may be different. Since irregular particles can be obtained by crushing a lump of alumina, they are also called crushed particles.

[0038] The first alumina particles are preferably spherical or rounded in shape, the second alumina particles are preferably spherical or irregular in shape, and the third alumina particles are preferably irregular in shape.

[0039] The sphericity of alumina particles can be measured as follows by taking particle images using a stereomicroscope, such as the Model SMZ-10 (Nikon Corporation) or a scanning electron microscope, and importing them into an image analyzer, such as (Nippon Avionics Corporation). That is, the projected area (A) and perimeter (PM) of the particle are measured from the photograph. If the area of ​​a perfect circle corresponding to the perimeter (PM) is (B), then the sphericity of the particle can be expressed as A / B. Therefore, assuming a perfect circle with the same perimeter as the perimeter (PM) of the sample particle, PM=2πr and B=πr 2 Therefore, B = π × (PM / 2π) 2 The sphericity of each particle is given by: Sphericity = A / B = A × 4π / (PM) 2The sphericity of 200 randomly selected particles thus obtained is calculated, and the average value is taken as the average sphericity.

[0040] The first alumina particles, the second alumina particles and the third alumina particles are preferably alumina particles whose α-alumina content is 90% by weight or more.

[0041] In the thermally conductive resin composition of the present invention, the filling rate of the at least three types of alumina particles is preferably 80 volume % or more and 95 volume % or less. The filling rate of the alumina particles in the thermally conductive resin composition is the ratio (percentage) of the volume of all types of alumina particles contained in the thermally conductive resin composition to the volume of the entire thermally conductive resin composition. By setting the filling rate of the alumina particles to 80 volume % or more, the effect of increasing the thermal conductivity is more suitably exhibited. It is difficult to increase the filling rate of the alumina particles beyond 95% from the viewpoint of maintaining the shape of the thermally conductive resin composition. When using two alumina particles having different average particle sizes as described in Patent Document 1, it is difficult to sufficiently improve the packing rate.

[0042] The filling rate of the alumina particles contained in the thermally conductive resin composition can be calculated as follows. When the resin is an organic resin such as an epoxy resin, the organic components are removed by heating to leave only the alumina particles, and the filling rate can be calculated from the volume of the alumina particles and the volume of the original thermally conductive resin composition. When the resin contains an inorganic component such as a silicone resin, it is difficult to remove the resin by heating. In this case, the weight ratio of the alumina particles is calculated from the weight of the thermally conductive resin composition, the specific gravity of the resin, and the specific gravity of the alumina particles, and the volume ratio of the alumina particles contained in the thermally conductive resin composition is calculated based on the weight ratio of the alumina particles, thereby obtaining the filling rate.

[0043] In the thermally conductive resin composition of the present invention, it is preferable that at least three types of alumina particles are surface-treated with a dispersing agent. The dispersant is preferably a silane compound, and more preferably a methoxy type, an ethoxy type, a silazane, a siloxane, etc. Also, a compound used as a general silane coupling agent may be used. When the alumina particles are surface-treated with a dispersant, they are more compatible with resins, particularly silicone resins, and the filling rate of the alumina particles in the thermally conductive resin composition can be more effectively improved, resulting in a thermally conductive resin composition with higher thermal conductivity. The dispersant is not particularly limited, and any dispersant that is used for the surface treatment of inorganic fillers can be used.

[0044] FIG. 2 is a cross-sectional view that illustrates a schematic diagram of another embodiment of the thermally conductive resin composition of the present invention. The shapes of the alumina particles are different in the thermally conductive resin composition 11 shown in Fig. 2. Fig. 2 shows an example in which the first alumina particles 41 have a rounded shape, the second alumina particles 42 have an irregular shape, and the third alumina particles 33 have an irregular shape.

[0045] FIG. 3 is a cross-sectional view that illustrates a schematic diagram of another embodiment of the thermally conductive resin composition of the present invention. The thermally conductive resin composition 12 shown in FIG. 3 contains first alumina particles 31, second alumina particles 32, and third alumina particles 33 similar to the thermally conductive resin composition 10 shown in FIG. 1, and further contains alumina fibers 51. The thermally conductive resin composition of the present invention preferably contains alumina fibers. Alumina fibers are generally longer than alumina particles and form an effective heat transfer path, so by further including alumina fibers, a thermally conductive resin composition having a higher thermal conductivity can be obtained. When the alumina fibers are contained, the average fiber length of the alumina fibers is preferably 10 to 50 μm, and the average fiber diameter is preferably 2 to 8 μm. The alumina fibers may or may not be surface-treated with a dispersant, but if the alumina fibers are surface-treated with a dispersant, they will have good compatibility with resins, particularly silicone resins, and the filling rate of the alumina particles in the thermally conductive resin composition can be more effectively improved.

[0046] When the thermally conductive resin composition contains alumina fibers, the content of the alumina fibers in the thermally conductive resin composition is preferably 1 to 20% by weight, and more preferably 3 to 20% by weight.

[0047] The thermally conductive resin composition of the present invention may contain other types of inorganic fibers together with or instead of the alumina fibers, such as silica-alumina fibers, silica fibers, zirconia fibers, titania fibers, and biosoluble fibers.

[0048] The thickness of the thermally conductive resin composition is preferably 50 μm or more and 10 mm or less. Moreover, it is more preferable that the thickness is 100 μm or more, and more preferably 5 mm or less. In addition, since the thermal conductivity of a thermally conductive resin composition is low compared to that of a metal material, if the thickness of the thermally conductive resin composition is too large (for example, exceeding 10 mm), the use of the thermally conductive resin composition may result in a decrease in the overall thermal conductivity. The thermally conductive resin composition may be a thermally conductive sheet formed into a sheet shape, or a thermally conductive film formed into a film shape. It may also be a resin material formed or processed into other shapes, a paste-like resin material having fluidity, a putty-like resin material having high viscosity, etc. Furthermore, a layer having adhesiveness or tackiness may be disposed on the surface of the sheet-like or film-like thermally conductive resin composition.

[0049] The thermal conductivity of the thermally conductive resin composition is preferably 3.5 W / m·K or more, more preferably 4.0 W / m·K or more, and even more preferably 5.0 W / m·K or more. The thermal conductivity of the thermally conductive resin composition can be measured by a laser flash method.

[0050] Next, the heat dissipation structure of the present invention will be described. The heat dissipation structure of the present invention is characterized by comprising a heat source, a heat dissipation member, and the thermally conductive resin composition of the present invention disposed between the heat source and the heat dissipation member.

[0051] FIG. 4 is a cross-sectional view that illustrates a schematic diagram of an embodiment of a heat dissipation structure. FIG. 4 shows a heat dissipation structure 100 in which a thermally conductive resin composition 10 is disposed between a semiconductor element 110 as a heat source and a heat sink 200 as a heat dissipation member. In this embodiment, the heat generated from the semiconductor element 110 can be conducted to the heat sink 200 via the thermally conductive resin composition 10 .

[0052] FIG. 4 shows a state in which thermally conductive grease 115 is disposed between the semiconductor element 110 and the thermally conductive resin composition 10, and between the thermally conductive resin composition 10 and the heat sink 200. The thermally conductive grease is placed to fill the space between the semiconductor element and the thermally conductive resin composition, and between the thermally conductive resin composition and the heat sink, thereby improving contact and thereby improving thermal conductivity; however, the use of thermally conductive grease is not essential, and the semiconductor element 110 and the thermally conductive resin composition 10 may be in direct contact, or the thermally conductive resin composition 10 and the heat sink 200 may be in direct contact.

[0053] Examples of heat sources for the heat dissipation structure include semiconductor elements, as well as light-emitting elements (such as LED elements), capacitors, resistor elements, batteries, motors, and the like. Moreover, the heat dissipation member may be a heat sink, a heat dissipation block, a heat dissipation fin, a heat diffusion sheet, a heat pipe, or the like.

[0054] Next, a method for producing the thermally conductive resin composition of the present invention will be described. The method for producing a thermally conductive resin composition of the present invention is a method for producing a thermally conductive resin composition comprising a resin and alumina particles contained in the resin, and includes a mixing step of mixing at least three types of alumina particles having different average particle diameters, each of which has an average particle diameter of 30 μm or less, with a resin material, wherein the at least three types of alumina particles include first alumina particles, second alumina particles having an average particle diameter smaller than that of the first alumina particles, and third alumina particles having an average particle diameter smaller than that of the second alumina particles, and the mixing ratios of the first alumina particles, the second alumina particles, and the third alumina particles are R1, R2, and R3, respectively, in volume ratio, and the relationship R1≧(R2+R3) is satisfied.

[0055] According to the above-described method for producing a thermally conductive resin composition of the present invention, the thermally conductive resin composition of the present invention can be suitably produced.

[0056] Prior to the mixing step, at least three types of alumina particles are prepared. The details of the first alumina particles, the second alumina particles, and the third alumina particles are as described above. The alumina particles are prepared so that their blending ratio by volume satisfies the relationship R1≧(R2+R3). It is also preferable to prepare and use alumina particles whose surfaces have been treated with a dispersing agent.

[0057] In the mixing step, at least three types of alumina particles and a resin material are mixed to prepare a thermally conductive resin composition. As the resin material, a precursor resin composition containing the precursors of the resins described above can be used. In addition to the precursors of each resin, additives such as a solvent, a curing agent, and a plasticizer may be added to the precursor resin composition. Furthermore, alumina fibers and / or other inorganic fibers may be mixed as necessary.

[0058] The thermally conductive resin composition is obtained by molding the thermally conductive resin composition mixed in the mixing step. The molding method can be arbitrarily set depending on the shape of the thermally conductive resin composition, and methods such as press molding, doctor blade method, extrusion molding, injection molding, sheet molding, and film molding can be used. In addition, after molding into a predetermined shape, machining such as cutting and polishing may be performed to obtain the desired shape. When the resin constituting the thermally conductive resin composition is a curable resin such as a thermosetting resin or a photocurable resin, the resin material and alumina particles are mixed, molded, and the obtained resin precursor is subjected to a thermal curing or photocuring process.

[0059] In the method for producing a thermally conductive resin composition of the present invention, at least three types of alumina particles having different average particle sizes, all of which are 30 μm or less, are mixed with a resin material, and the mixing ratio (volume %) of the first to third types of alumina particles is set to R1≧(R2+R3), thereby improving the filling rate of the alumina particles in the produced thermally conductive resin composition, and thus a thermally conductive resin composition having high thermal conductivity can be produced.

[0060] [Example] The present invention will be further described below with reference to examples, but the present invention is not limited to the following examples. [Preparation of ingredients] The dispersant was mixed with ethanol according to the formula shown in Table 1, and the mixture was added dropwise to the raw material alumina powder while stirring. After that, it was dried in a dryer at 100°C for 10 hours to obtain alumina particles surface-treated with the dispersant. The raw material alumina powder and dispersant shown in Table 1 were as follows.

[0061] Raw material Alumina powder: Average particle size (d50) 39μm, rounded Average particle size (d50) 18μm, rounded Average particle size (d50) 22μm, rounded Average particle diameter (d50) 16μm, spherical Average particle size (d50) 2.0μm, spherical Average particle size (d50) 2.2μm, irregular shape Average particle size (d50) 4.0μm, amorphous Average particle size (d50) 0.26μm, amorphous Dispersant: Silane-based ethoxy dispersant

[0062] Alumina particles 1-1, 1-2, and 1-3 shown in Table 1 are alumina particles having average particle sizes intended to be used as first alumina particles, alumina particles 2-1 and 2-2 as second alumina particles, and alumina particles 3-1 as third alumina particles. Alumina particles 4-1 have an average particle diameter exceeding 30 μm, and are therefore particles that do not fall under any of the first alumina particles, second alumina particles, or third alumina particles used in the production of a thermally conductive resin composition (classified as “other alumina particles” in Table 2).

[0063] [Table 1]

[0064] Additionally, alumina fibers (manufactured by Safil Corporation) were treated at 1500° C. to increase the α-alumina ratio to 80% or more, and to prepare alumina fibers with an average fiber length of 30 μm and an average fiber diameter of 3.5 μm.

[0065] As the resin, an addition reaction type liquid silicone resin (manufactured by Shin-Etsu Chemical Co., Ltd., product name "KE-109E-A / B") was prepared.

[0066] (Examples 1 to 6, Comparative Examples 1 to 5) The resin prepared as described above and alumina particles were added in the ratio (volume %) shown in Table 2, and mixed for 10 minutes at a rotation speed of 1700 rpm using a planetary centrifugal mixer "Awatori Rentaro" manufactured by Shinky Corporation, to produce a thermally conductive resin composition. Alumina fibers were used in Example 6. The blending ratio of each alumina particle and alumina fiber is shown with the total of the alumina particles and alumina fiber being 10. The resin was blended in an amount that could be molded by hot pressing under the following conditions and maximized the filling rate of the thermally conductive resin composition. This thermally conductive resin composition was placed on a jig and pressed for 15 minutes at 150°C under a pressure of 5 MPa to produce a precursor of the thermally conductive resin composition with a thickness of 1 mm.Then, the precursor was heated at 150°C for 4 hours to obtain a thermally conductive resin composition. This thermally conductive resin composition was processed into a size of 200 mm×200 mm, and the thermal conductivity was measured using a laser flash thermal constant measuring device (TC-1200RH, manufactured by ULVAC-RIKO, Inc.). The thermal conductivity of the thermally conductive resin composition obtained above was measured, and the results are shown in Table 2. The filling rate of the alumina particles in the thermally conductive resin composition was also shown.

[0067] [Table 2]

[0068] As can be seen from the results shown in Table 2, in Examples 1 to 6, the packing rate could be made 80 volume % or more, and the packing rate of the alumina particles was high, so the thermal conductivity was high, at 3.5 W / m·K or more. Example 6, in which alumina fibers were added, had a higher thermal conductivity than Example 1, which had a similar alumina particle structure.

[0069] Comparative Examples 1 and 2 contain only one or two types of alumina particles, and therefore have a low packing rate and low thermal conductivity. In Comparative Example 3, the average particle size of the largest alumina particles exceeds 30 μm, so that the filling rate is low and the thermal conductivity is low. In Comparative Examples 4 and 5, the content ratios (volume %) of the first to third types of alumina particles do not satisfy the relationship R1≧(R2+R3). Since the ratio of relatively small particles is large, the influence of the decrease in thermal conductivity due to the existence of interfaces between particles becomes large, resulting in low thermal conductivity. [Explanation of symbols]

[0070] 10, 11, 12 Thermally conductive resin composition 20 Resin 31, 41 First alumina particles 32, 42 Second alumina particles 33 Third Alumina Particles 51 Alumina Fiber 100 Heat dissipation structure 110 Semiconductor elements 115 Thermal grease 200 Heatsink

Claims

1. A thermally conductive resin composition comprising a resin and alumina particles contained in the resin, At least three types of alumina particles having different average particle sizes are included, and the average particle size of each type of alumina particle is 30 μm or less, the at least three types of alumina particles include first alumina particles, second alumina particles having an average particle size smaller than that of the first alumina particles, and third alumina particles having an average particle size smaller than that of the second alumina particles; The first alumina particles have an average particle size of 10 to 30 μm; The second alumina particles have an average particle size of 1.5 to 5 μm; The third alumina particles have an average particle size of 0.1 to 1 μm; The first alumina particles have a spherical or rounded shape; The second alumina particles have an irregular shape, The third alumina particles have an irregular shape, When the content ratios of the first alumina particles, the second alumina particles and the third alumina particles are R1, R2 and R3, respectively, in terms of volume ratio, the following relationships are all satisfied: R1 ≧ (R2 + R3), R1 > R2 > R3, and R1 ≧ 2 × R3; A thermally conductive resin composition, wherein R1 is 50 to 65 volume %, R2 is 26 to 30 volume %, and R3 is 5 to 24 volume %.

2. 2. The thermally conductive resin composition according to claim 1, wherein the filling rate of the at least three types of alumina particles is 80 volume % or more and 95 volume % or less.

3. 3. The thermally conductive resin composition according to claim 1, which has a thermal conductivity of 3.5 W / m·K or more.

4. 4. The thermally conductive resin composition according to claim 1, wherein the at least three types of alumina particles are surface-treated with a dispersing agent.

5. The thermally conductive resin composition according to any one of claims 1 to 4, further comprising alumina fibers.

6. A heat dissipation structure comprising: a heat source; a heat dissipation member; and the thermally conductive resin composition according to any one of claims 1 to 5, disposed between the heat source and the heat dissipation member.

7. A method for producing a thermally conductive resin composition comprising a resin and alumina particles contained in the resin, comprising the steps of: The method includes a mixing step of mixing at least three types of alumina particles, each having a different average particle size, and each type of alumina particle having an average particle size of 30 μm or less, with a resin material; the at least three types of alumina particles include first alumina particles, second alumina particles having an average particle size smaller than that of the first alumina particles, and third alumina particles having an average particle size smaller than that of the second alumina particles; The first alumina particles have an average particle size of 10 to 30 μm; The second alumina particles have an average particle size of 1.5 to 5 μm; The third alumina particles have an average particle size of 0.1 to 1 μm; The first alumina particles have a spherical or rounded shape; The second alumina particles have an irregular shape, The third alumina particles have an irregular shape, When the blending ratios of the first alumina particles, the second alumina particles, and the third alumina particles are R1, R2, and R3, respectively, in terms of volume ratio, the relationships R1 ≧ (R2 + R3), R1 > R2 > R3, and R1 ≧ 2 × R3 are all satisfied, A method for producing a thermally conductive resin composition, wherein R1 is 50 to 65 volume %, R2 is 26 to 30 volume %, and R3 is 5 to 24 volume %.

8. 8. The method for producing a thermally conductive resin composition according to claim 7, wherein a filling rate of the at least three types of alumina particles in the thermally conductive resin composition containing the at least three types of alumina particles and the resin is 80 volume % or more and 95 volume % or less.

9. The method for producing a thermally conductive resin composition according to claim 7 or 8, wherein the at least three types of alumina particles are surface-treated with a dispersing agent.

10. The method for producing a thermally conductive resin composition according to any one of claims 7 to 9, wherein in the mixing step, alumina fibers are further mixed in addition to the at least three types of alumina particles and the resin.

Citation Information

Patent Citations

  • Water-erasable lead for solid charlk and pencil

    JP1982055977A

  • Epoxy resin composition and epoxy resin cured product

    JP2008013759A

  • Thermoconductive silicone composition

    JP2010006923A

  • Heat-conductive epoxy resin sheet material

    JP2010229269A

  • Thermally conductive silicone grease composition

    JP2012007057A