High-strength eTPU
The combination of aliphatic diisocyanates with chain extenders and polyols in a polyisocyanate composition addresses the limitations of existing foamed pellets by enhancing stiffness, mechanical properties, and processability, resulting in improved molded bodies for footwear components.
Patent Information
- Application Number
- JP2021537998
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2018-12-28
- Filing Date
- 2019-12-27
- Publication Date
- 2024-12-04
- Estimated Expiration
- 2039-12-27
AI Technical Summary
Existing foamed pellets used in the production of molded bodies, such as shoe components, often lack sufficient stiffness, mechanical properties, and processability, particularly when fused at low temperatures, leading to weakened bonds and compromised mechanical performance.
A polyisocyanate composition comprising aliphatic diisocyanates with a molecular weight below 200 g/mol, combined with a chain extender and polyol composition, is used to create thermoplastic polyurethane foamed pellets that exhibit high elastic modulus, low softening points, and improved mechanical properties, enabling easy processing and better phase separation.
The resulting foamed pellets demonstrate enhanced elastic modulus, rebound resilience, and improved compression hardness, allowing for the production of molded bodies with superior mechanical properties and ease of processing, particularly suitable for footwear applications.
Smart Images

Figure 0007594531000001 
Figure 0007594531000002 
Figure 0007594531000003
Abstract
Description
[Technical field]
[0001] The present invention relates to foamed pellets comprising thermoplastic polyurethane obtainable or obtained by reacting a polyisocyanate composition (IC) comprising at least one aliphatic diisocyanate having a number average molecular weight of less than 200 g / mol, at least one chain extender (CE1), and a polyol composition (PC), and further relates to a process for producing such foamed pellets. The present invention also encompasses a process for using the foamed pellets of the present invention for producing a molded body. [Background technology]
[0002] Expanded pellets, also called expandable beads (or expandable particles), and thermoplastic polyurethane or other elastomer-based moldings produced therefrom are known (e.g. WO94 / 20568, WO2007 / 082838A1, WO2017030835, WO2013 / 153190A1, WO2010010010) and have a wide variety of viable uses.
[0003] Within the meaning of the present invention, "expanded pellets", also "expandable beads" or "expandable particles", refers to a foam in the form of beads, the average diameter of which is 0.2 to 20 mm, preferably 0.5 to 15 mm, in particular 1 to 12 mm. In the case of non-spherical, e.g. elongated or cylindrical, beads, the diameter means the longest dimension.
[0004] In principle, there is a need for foamed pellets or foamable beads that have improved processability, so that the corresponding moldings can be obtained at the lowest possible temperatures while maintaining advantageous mechanical properties. This is particularly relevant for the currently widely used fusion methods, in which the energy input for fusing the foamed pellets is introduced by an auxiliary medium, for example water vapor, since improved bonding is achieved here, so that damage to the material or foam structure is simultaneously reduced and at the same time sufficient bonding or fusion is obtained.
[0005] Sufficient bonding or fusion of the foam pellets is essential to obtain favorable mechanical properties of the moldings produced from the foam pellets. If the foam beads are insufficiently bonded or fused, these properties cannot be fully utilized, with a consequential negative effect on the overall mechanical properties of the resulting molding. Similar considerations apply if the molding is weakened. In such a case, the mechanical properties will be disadvantaged at the weakened points, with the same results as those mentioned above. Therefore, the properties of the polymers used must be efficiently adjustable.
[0006] Known materials often have a very low modulus at room temperature, so in order to achieve sufficient stiffness and stability for many applications, a high density must be achieved, while at the same time high resilience and good mechanical properties must be achieved for many applications, and the material should be easily fusible to produce moldings from the foamed pellets.
[0007] In the context of the present invention, "advantageous mechanical properties" shall be interpreted with respect to the intended application. The most prominent application for the subject matter of the present invention is in the footwear industry sector, where the foam pellets can be used for shoe components where damping and / or cushioning are relevant, such as moldings for insoles and inner soles. [Prior art documents] [Patent documents]
[0008] [Patent Document 1] WO94 / 20568 [Patent Document 2] WO2007 / 082838A1 [Patent Document 3] WO2017030835 [Patent Document 4] WO2013 / 153190A1 [Patent Document 5] WO2010010010 Summary of the Invention [Problem to be solved by the invention]
[0009] It was therefore an object of the present invention to provide polymer-based foamed pellets which have sufficient rigidity while at the same time having good mechanical properties and good processability. It was a further object of the present invention to provide a method for producing the corresponding foamed pellets. [Means for solving the problem]
[0010] According to the invention, this object is achieved by providing at least components (i) to (iii): (i) a polyisocyanate composition (IC); (ii) at least one chain extender (CE1); (iii) polyol composition (PC), wherein the isocyanate composition comprises at least one aliphatic diisocyanate having a number average molecular weight of less than 200 g / mol.
[0011] Surprisingly, it has been found that the components used according to the present invention, and in particular the use of a specific isocyanate composition (IC), make it possible to obtain foamed pellets with a high modulus and at the same time a low softening point, so that the foamed pellets can be easily processed into moldings.In addition, the foamed pellets of the present invention are characterized by good mechanical properties, such as high elasticity and good rebound.Surprisingly, the very good phase separation can be achieved according to the present invention, while at the same time having a better melting property of the hard phase, resulting in foamed pellets that are more rigid and at the same time easily processable.For example, in particular the compression hardness can be significantly improved over conventional materials.
[0012] In the context of the present invention, unless stated otherwise, the rebound is determined analogously to DIN 53512, April 2000. The deviation from the standard is the height of the test specimen, which should be 12 mm, but in this test 20 mm is used to avoid "penetration through" the specimen and measurement of the substrate.
[0013] The present invention relates to foamed pellets comprising thermoplastic polyurethane obtainable or obtained by reacting a polyisocyanate composition (IC), a chain extender (CE1) and a polyol composition (PC). The isocyanate composition (IC) here comprises at least one symmetrical diisocyanate having a number average molecular weight of less than 200 g / mol.
[0014] Surprisingly, it has been found that thermoplastic polyurethanes of this type can be easily processed to give foamed pellets which in turn can be easily processed to give moulded bodies having a particularly high elastic modulus and very good rebound.
[0015] According to the present invention, the isocyanate composition (IC) comprises an aliphatic diisocyanate having a number average molecular weight of less than 200 g / mol. Suitable isocyanates are known per se to those skilled in the art. According to the present invention, the isocyanate composition (IC) may also comprise further isocyanates.
[0016] In the context of the present invention, the aliphatic isocyanate is preferably a linear diisocyanate, in particular a linear diisocyanate having an even number of carbon atoms. Thus, in a further embodiment, the present invention relates to foamed pellets as previously described, in which the aliphatic diisocyanate is a linear diisocyanate having an even number of carbon atoms.
[0017] Within the context of the present invention, the aliphatic diisocyanates are more preferably isomerically pure.
[0018] An example of one suitable aliphatic diisocyanate having a number average molecular weight of less than 200 g / mole is hexamethylene diisocyanate (HDI).
[0019] Thus, in a further embodiment, the present invention relates to foamed pellets as previously described, wherein the aliphatic diisocyanate is hexamethylene diisocyanate (HDI).
[0020] Further isocyanates suitable within the context of the present invention are especially diisocyanates, in particular aliphatic or aromatic diisocyanates, more preferably aromatic diisocyanates.
[0021] In addition, within the context of the present invention, pre-reacted products can be used as isocyanate components, in which case part of the OH components are reacted with isocyanates in a preceding reaction step, and the resulting product is reacted with the remaining OH components in a subsequent step, the actual polymer reaction, thus forming the thermoplastic polyurethane.
[0022] The aliphatic diisocyanates used are customary aliphatic and / or cycloaliphatic diisocyanates, such as, for example, tri-, tetra-, penta-, hexa-, hepta- and / or octamethylene diisocyanate, 2-methylpentamethylene 1,5-diisocyanate, 2-ethyltetramethylene 1,4-diisocyanate, hexamethylene 1,6-diisocyanate (HDI), pentamethylene 1,5-diisocyanate, butylene 1,4-diisocyanate, trimethylhexamethylene 1,6-diisocyanate, These are 1-isocyanato-3,3,5-trimethyl-5-isocyanatomethylcyclohexane (isophorone diisocyanate, IPDI), 1,4- and / or 1,3-bis(isocyanatomethyl)cyclohexane (HXDI), cyclohexane 1,4-diisocyanate, 1-methylcyclohexane-2,4-diisocyanate and / or 1-methylcyclohexane 2,6-diisocyanate, methylene dicyclohexyl 4,4'-, 2,4'- and / or 2,2'-diisocyanate (H12MDI).
[0023] Suitable aromatic diisocyanates are in particular naphthylene 1,5-diisocyanate (NDI), tolylene 2,4- and / or 2,6-diisocyanate (TDI), 3,3'-dimethyl-4,4'-diisocyanatobiphenyl (TODI), p-phenylene diisocyanate (PDI), diphenylethane 4,4'-diisocyanate (EDI), methylene diphenyl diisocyanate (MDI), the term MDI being taken to mean diphenylmethane 2,2', 2,4'- and / or 4,4'-diisocyanate, dimethyldiphenyl 3,3'-diisocyanate, diphenylethane 1,2-diisocyanate and / or phenylene diisocyanate or H12MDI (methylenedicyclohexyl 4,4'-diisocyanate).
[0024] Mixtures can also be used in principle. An example of a mixture is a mixture that contains, in addition to methylene diphenyl 4,4'-diisocyanate, at least one further methylene diphenyl diisocyanate. The term "methylene diphenyl diisocyanate" here means diphenylmethane 2,2'-, 2,4'- and / or 4,4'-diisocyanate or a mixture of two or three isomers. It is therefore possible to use further isocyanates, for example diphenylmethane 2,2'- or 2,4'-diisocyanate or a mixture of two or three isomers. In this embodiment, the polyisocyanate composition can also contain other above-mentioned polyisocyanates.
[0025] If further isocyanates are used, these are present in the isocyanate composition (IC) preferably in an amount in the range from 0.1% to 20% by weight, more preferably in an amount in the range from 0.1% to 10% by weight and particularly preferably in an amount in the range from 0.5% to 5% by weight.
[0026] Preferred examples of higher functional isocyanates are triisocyanates, such as triphenylmethane 4,4',4''-triisocyanate, as well as the cyanurates of the abovementioned diisocyanates and oligomers obtainable by partial reaction of diisocyanates with water, such as biurets of the abovementioned diisocyanates, as well as oligomers obtainable by controlled reaction of semiblocked diisocyanates with polyols having an average of more than two, preferably three or more, hydroxyl groups.
[0027] The organic isocyanates which can be used are aliphatic, cycloaliphatic, araliphatic and / or aromatic isocyanates.
[0028] Crosslinkers can also be used, for example the previously described higher functional polyisocyanates or polyols, but also other higher functional molecules having multiple isocyanate-reactive functional groups. It is also possible in the context of the present invention to achieve crosslinking of the product via an excess of isocyanate groups used in proportion to the hydroxyl groups. Examples of higher functional isocyanates are triisocyanates, for example triphenylmethane 4,4',4''-triisocyanate and isocyanurates, as well as the cyanurates of the abovementioned diisocyanates, and oligomers obtainable by partial reaction of diisocyanates with water, for example biurets of the abovementioned diisocyanates, and also oligomers obtainable by controlled reaction of semiblocked diisocyanates with polyols having an average of more than two, preferably three or more, hydroxyl groups.
[0029] Here, in the context of the present invention, the amount of crosslinker, i.e. the amount of higher functional isocyanate and higher functional polyol or higher functional chain extender, is less than 3% by weight, preferably less than 1% by weight, more preferably less than 0.5% by weight, based on the mixture of all components.
[0030] The polyisocyanate composition may also include one or more solvents. Suitable solvents are known to those skilled in the art. Suitable examples are non-reactive solvents such as ethyl acetate, methyl ethyl ketone, and hydrocarbons.
[0031] A polyol composition (PC) is used according to the invention. According to the invention, the polyol composition (PC) comprises at least one polyol. Suitable polyols are known in principle to the skilled artisan and are described, for example, in "Kunststoffhandbuch [Plastics Handbook], Volume 7, Polyurethane [Polyurethanes]", Carl Hanser Verlag, 3rd Edition, 1993, Chapter 3.1. As polyol (P1), it is particularly preferred to use polyesterols or polyetherols as polyols. It is likewise possible to use polycarbonates. Copolymers may also be used in the context of the invention. Polyether polyols are particularly preferred. The number-average molecular weight of the polyols used according to the invention is preferably in the range from 500 to 5000 g / mol, for example in the range from 550 g / mol to 2000 g / mol, preferably in the range from 600 g / mol to 1500 g / mol, in particular between 650 g / mol and 1000 g / mol.
[0032] Polyetherols, as well as polyesterols, block copolymers and hybrid polyols, such as poly(ester / amides), are suitable according to the invention. Preferred polyetherols according to the invention are polyethylene glycols, polypropylene glycols, polyadipates, polycarbonates, polycarbonate diols and polycaprolactones.
[0033] Thus, in a further embodiment, the present invention relates to the foamed pellets previously described, wherein the polyol composition comprises a polyol selected from the group consisting of polyetherol, polyesterol, polycaprolactone polyol and polycarbonate polyol.
[0034] Suitable polyols are, for example, those with ether and ester blocks, such as polycaprolactones with polyethylene oxide or polypropylene oxide end blocks, and also polyethers with polycaprolactone end blocks. In accordance with the invention, preferred polyetherols are polyethylene glycol and polypropylene glycol. Polycaprolactone is also preferred.
[0035] According to the invention it is also possible to use mixtures of different polyols. The polyols / polyol compositions used preferably have an average functionality between 1.8 and 2.3, preferably between 1.9 and 2.2, in particular 2. The polyols used according to the invention preferably have only primary hydroxyl groups.
[0036] In one embodiment of the present invention, a polyol composition (PC) is used that comprises at least polytetrahydrofuran. According to the present invention, the polyol composition may also comprise further polyols in addition to polytetrahydrofuran.
[0037] Further polyols suitable according to the invention are, for example, polyethers, also polyesters, block copolymers, and also hybrid polyols, such as poly(ester / amide).Suitable block copolymers are, for example, block copolymers with ether and ester blocks, such as polycaprolactone with polyethylene oxide or polypropylene oxide end blocks, and also polyethers with polycaprolactone end blocks.Preferred polyetherols according to the invention are polyethylene glycol and polypropylene glycol.Polycaprolactone is also preferred as further polyol.
[0038] In a particularly preferred embodiment, the polytetrahydrofuran has a number average molecular weight Mn in the range of 500 g / mol to 5000 g / mol, more preferably in the range of 550 to 2500 g / mol, and particularly preferably in the range of 650 to 2000 g / mol.
[0039] Within the context of the present invention, the composition of the polyol composition (PC) may vary within wide limits. The polyol composition may also contain a mixture of different polyols.
[0040] According to the invention, the polyol composition may also contain a solvent. Suitable solvents are known per se to those skilled in the art.
[0041] When polytetrahydrofuran is used, the number average molecular weight Mn of polytetrahydrofuran is preferably in the range of 500 to 5000 g / mol, more preferably in the range of 500 to 1400 g / mol.
[0042] In a further embodiment, the present invention also relates to the foamed pellets as previously described, wherein the polyol composition comprises a polyol selected from the group consisting of polytetrahydrofurans having a number average molecular weight Mn in the range of 500 g / mol to 5000 g / mol.
[0043] Thus, in a further embodiment, the present invention relates to foamed pellets as previously described, wherein the polyol composition comprises a polyol selected from the group consisting of polytetrahydrofurans having a number average molecular weight Mn in the range of 500 g / mol to 2000 g / mol.
[0044] Mixtures of various polytetrahydrofurans can also be used in accordance with the present invention, ie, the mixture of polytetrahydrofurans has different molecular weights.
[0045] Preferred polyetherols according to the invention are polyethylene glycol, polypropylene glycol and polytetrahydrofuran, as well as mixed polyetherols thereof. Mixtures of various polytetrahydrofurans of different molecular weights can also be used according to the invention, for example.
[0046] According to the present invention, at least one chain extender (CE1) is also used. Suitable chain extenders are known per se to those skilled in the art. By way of example, the chain extender is a compound having two groups reactive towards isocyanate groups, in particular one having a molecular weight of less than 500 g / mol. Suitable chain extenders are, for example, diamines or diols. According to the present invention, diols are more preferred.
[0047] Within the scope of the present invention, mixtures of two or more chain extenders may also be used.
[0048] Suitable diols are known in principle to those skilled in the art. According to the invention, the diol preferably has a molecular weight of <500 g / mol. According to the invention, aliphatic, araliphatic, aromatic and / or cycloaliphatic diols having a molecular weight of 50 g / mol to 220 g / mol can be used here, for example, as chain extenders. Preference is given to alkanediols having 2 to 10 carbon atoms in the alkylene group, in particular di-, tri-, tetra-, penta-, hexa-, hepta-, octa-, nona- and / or decaalkylene glycols. Particular preference is given to 1,2-ethylene glycol, propane-1,3-diol, butane-1,4-diol, hexane-1,6-diol for the present invention.
[0049] Suitable chain extenders (CE1) within the context of the present invention are also branched compounds, such as 1,4-cyclohexanedimethanol, 2-butyl-2-ethylpropanediol, neopentyl glycol, 2,2,4-trimethylpentane-1,3-diol, pinacol, 2-ethylhexane-1,3-diol or cyclohexane-1,4-diol.
[0050] Thus, in a further embodiment, the present invention relates to the foamed pellets previously described, wherein the chain extender (CE1) is selected from the group consisting of propane-1,3-diol, ethane-1,2-diol, butane-1,4-diol, hexane-1,6-diol and HQEE.
[0051] The quantitative ratio of the components used, here as in step (b), is preferably selected so as to obtain a hard segment content in the range of 10% to 40%.
[0052] Unless otherwise stated, the weight average molecular weight Mw of thermoplastic block copolymers is determined in the context of the present invention using GPC dissolved in HFIP (hexafluoroisopropanol). Molecular weight is determined using two GPC columns (PSS-Gel; 100A; 5μ; 300×8mm, Jordi-Gel DVB; mixed bed; 5μ; 250×10mm; column temperature 60° C.; flow rate 1 ml / min; RI detector) arranged in series. Calibration is performed here with polymethylmethacrylate (EasyCal; PSS, Mainz), HFIP is used as eluent.
[0053] In a further aspect, the present invention also relates to a method for producing foamed pellets, in which the present invention relates to a method for producing foamed pellets, comprising the steps of: (i) A step of preparing a composition (C1) containing a thermoplastic polyurethane, the thermoplastic polyurethane comprising at least components (a) to (c): (a) a polyisocyanate composition (IC), (b) at least one chain extender (CE1); (c) polyol composition (PC), wherein the isocyanate composition comprises at least one aliphatic diisocyanate having a number average molecular weight of less than 200 g / mole; (ii) impregnating composition (C1) with a blowing agent under pressure; (iii) Expanding composition (C1) using a pressure reduction The present invention relates to a method comprising the steps of:
[0054] Within the context of the present invention, composition (C1) can be used here in the form of a melt or in the form of pellets.
[0055] With regard to preferred embodiments of the process, suitable feedstocks or mixing ratios, reference is made to the statements made above which apply accordingly.
[0056] The method of the invention may include further steps, such as adjusting the temperature.
[0057] The non-expanded polymer mixture of composition (C1) required for the production of the foamed pellets is produced in a known manner from the individual components and also from any further components, such as, for example, processing aids, stabilizers, compatibilizers or pigments. Examples of suitable methods are conventional mixing methods, in continuous or batch mode, with the assistance of a kneader or with the assistance of an extruder, for example a co-rotating twin screw extruder.
[0058] In the case of compatibilizers or auxiliaries, such as stabilizers, these may already be incorporated into the components during their production. The individual components are usually combined or metered into the device in which the mixing is carried out prior to the mixing process. In the case of an extruder, the components are all metered into the inlet and fed together into the extruder, or the individual components are added via a side feed.
[0059] The processing is carried out at a temperature at which the components are in a plasticized state. The temperature depends on the softening or melting range of the components, but must be below the decomposition temperature of each component. Additives, such as pigments or fillers or other of the conventional auxiliaries mentioned above, are also not melted, but rather incorporated as solids.
[0060] Further embodiments using predefined methods are also possible here, where the methods used for the production of the starting materials can be integrated into the direct production.
[0061] For example, in the case of a belt process, it is possible to introduce the styrene polymer, the reinforcing agent and also the fillers or colorants directly at the end of the belt where the material is fed into an extruder to obtain lenticular granules.
[0062] Some of the above conventional auxiliaries may be added to the mixture at this stage.
[0063] The foamed pellets according to the invention generally have a bulk density of 50 g / l to 200 g / l, preferably 60 g / l to 180 g / l, particularly preferably 80 g / l to 150 g / l. The bulk density is measured in accordance with DIN ISO 697 as opposed to the standard, and the determination of said values involves the use of a container with a volume of 10 l instead of a container with a volume of 0.5 l, since a measurement using only a volume of 0.5 l is too inaccurate, especially for foamed beads with low density and high mass.
[0064] As stated above, the diameter of the foam pellets is 0.5 to 30 mm, preferably 1 to 15 mm, in particular 3 to 12 mm. For non-spherical, e.g. elongated or cylindrical, foam pellets, the diameter refers to the longest dimension.
[0065] The foam pellets are prepared by known and well-established methods in the prior art. (i) preparing a composition (C) of the present invention; (ii) impregnating the composition with a blowing agent under pressure; (iii) expanding the composition using a pressure reduction. It can be generated using:
[0066] The amount of the foaming agent is preferably 0.1 to 40 parts by mass, particularly preferably 0.5 to 35 parts by mass, and particularly preferably 1 to 30 parts by mass, per 100 parts by mass of the composition (C) used.
[0067] One embodiment of the above method comprises: (i) providing the composition (C) of the present invention in the form of pellets; (ii) impregnating the pellets with a blowing agent under pressure; (iii) Expanding the pellets using a pressure reduction. Includes.
[0068] A further embodiment of the above method further comprises the steps of: (i) providing the composition (C) of the present invention in the form of pellets; (ii) impregnating the pellets with a blowing agent under pressure; (iii-a) reducing the pressure to standard pressure, optionally with a prior reduction in temperature, without expanding the pellets; (iii-b) Expanding the pellets using an increase in temperature Includes.
[0069] The non-expanded pellets here preferably have an average minimum diameter of 0.2 to 10 mm (determined via 3D evaluation of the pellets, for example via dynamic image analysis using a PartAn 3D optical measuring device from Microtrac).
[0070] The individual pellets generally have an average mass in the range of 0.1 to 50 mg, preferably in the range of 4 to 40 mg, particularly preferably in the range of 7 to 32 mg. This average mass of the pellets (particle mass) is determined as the arithmetic mean using three weighing operations of in each case 10 pellet particles.
[0071] One embodiment of the above method comprises impregnating the pellets with a blowing agent under pressure, followed by steps (I) and (II): (I) impregnating the pellets in a suitable closed reaction vessel (e.g., an autoclave) in the presence of a blowing agent under pressure and at elevated temperature; (II) Rapidly reducing pressure without cooling The method includes expanding the pellets with
[0072] The impregnation of step (I) here can be carried out in the presence of water and optionally a suspending aid, or simply in the presence of a blowing agent and in the absence of water.
[0073] Suitable suspension aids are, for example, water-insoluble inorganic stabilizers such as tricalcium phosphate, magnesium pyrophosphate, metal carbonates, as well as polyvinyl alcohol and surfactants such as sodium dodecylarylsulfonate, which are usually used in an amount of 0.05 to 10% by weight based on the composition of the present invention.
[0074] Depending on the pressure selected, the impregnation temperature is in the range from 100° C. to 200° C., the pressure in the reaction vessel is between 2 and 150 bar, preferably between 5 and 100 bar, particularly preferably between 20 and 60 bar, and the impregnation time is generally between 0.5 and 10 hours.
[0075] Carrying out this process in suspension is known to those skilled in the art and is described extensively in, for example, WO2007 / 082838.
[0076] When carrying out this process in the absence of a blowing agent, care must be taken to avoid agglomeration of the polymer pellets.
[0077] Suitable blowing agents for carrying out the process in a suitable closed reaction vessel are, by way of example, organic liquids and gases which are in the gaseous state under the process conditions, such as hydrocarbons or inorganic gases, or mixtures of organic liquids or gases with inorganic gases, which can also be combined.
[0078] Examples of suitable hydrocarbons are halogenated or non-halogenated, saturated or unsaturated aliphatic hydrocarbons, preferably non-halogenated, saturated or unsaturated aliphatic hydrocarbons.
[0079] Preferred organic blowing agents are saturated aliphatic hydrocarbons, especially those having 3 to 8 carbon atoms, such as butane or pentane.
[0080] Suitable inorganic gases are nitrogen, air, ammonia or carbon dioxide, preferably nitrogen or carbon dioxide, or a mixture of the abovementioned gases.
[0081] In a further embodiment, the impregnation of the pellets with the blowing agent under pressure comprises subjecting the pellets to steps (α) and (β): (α) impregnating the pellets in an extruder under pressure and at elevated temperature in the presence of a blowing agent; (β) pelletizing the composition emerging from the extruder under conditions which prevent uncontrolled foaming. and subsequent expansion.
[0082] Suitable blowing agents in this process version are volatile organic compounds having a boiling point of -25°C to 150°C, in particular -10°C to 125°C, at standard pressure, 1013 mbar. Good suitability is provided by hydrocarbons (preferably halogen-free), in particular C4-10-alkanes, such as butane, pentane, hexane, heptane and the isomers of octane, particularly preferably isobutane. Further possible blowing agents are more sterically demanding compounds, such as alcohols, ketones, esters, ethers and organic carbonates.
[0083] In this case, the composition is mixed in an extruder in step (ii) while molten and under pressure with a blowing agent fed to the extruder. The mixture including the blowing agent is extruded and pelletized under pressure, preferably using a controlled back pressure at a moderate level (e.g. underwater pelletization). The melt strand foam in this process and pelletization results in foamed pellets.
[0084] Carrying out this process via extrusion is known to the person skilled in the art and has been described extensively, for example in WO2007 / 082838 and also in WO2013 / 153190A1.
[0085] Extruders which can be used are, for example, any of the conventional screw-based equipment, in particular single-screw and twin-screw extruders (for example ZSK type from Werner & Pfleiderer), co-kneaders, Kombiplast equipment, MPC kneading mixers, FCM mixers, KEX kneading screw extruders and shear roll extruders, as described in chapters 3.2.1 and 3.2.4 of Saechtling (ed.), Kunststoff-Taschenbuch [Plastics Handbook], 27th edition, Hanser-Verlag, Munich, 1998. The extruder is usually operated at a temperature at which the composition (C1) is present as a melt, for example 120°C to 250°C, in particular 150 to 210°C, and at a pressure of 40 to 200 bar, preferably 60 to 150 bar, particularly preferably 80 to 120 bar, after the addition of the blowing agent, thereby ensuring that the blowing agent is homogenous with the melt.
[0086] The process here can be carried out in an extruder or in an arrangement consisting of one or more extruders. Thus, by way of example, the components can be melted and blended in a first extruder and the blowing agent injected. In a second extruder, the impregnated melt is homogenized and the temperature and / or pressure is adjusted. By way of example, when three extruders are combined with each other, the mixing of the components and the injection of the blowing agent can also be divided between two different processing sections. When only one extruder is used, as is preferred, all the process steps, i.e. melting, mixing, injection of the blowing agent, homogenization and temperature and / or pressure adjustment, are carried out in a single extruder.
[0087] Alternatively and according to the methods described in WO2014 / 150122 or WO2014 / 150124A1, the corresponding foamed pellets, optionally already colored, can be saturated with a supercritical liquid, removed from the supercritical liquid, and subsequently (i') Immersing the article in a heated fluid; or (ii') exposing the article to energetic radiation (e.g., infrared or microwave radiation); This allows it to be produced directly from pellets.
[0088] Suitable supercritical liquids are those described in WO2014150122 or for example carbon dioxide, nitrogen dioxide, ethane, ethylene, oxygen or nitrogen, preferably carbon dioxide or nitrogen.
[0089] The supercritical liquid here is 9 MPa. -1 / 2 Polar liquids having Hildebrand solubility parameters equal to or greater than 100 nm may also be included.
[0090] The supercritical or heated fluid herein may also contain a colorant, resulting in a colored foamed article.
[0091] The present invention further provides a molded body produced from the foamed pellets of the present invention.
[0092] The corresponding shaped bodies can be produced by methods known to those skilled in the art.
[0093] A preferred method for the production of foam mouldings herein comprises the following steps: (A) introducing the foamed pellets of the invention into a suitable mold; (B) Fusing the foamed pellets of the present invention from step (i). Includes.
[0094] The fusion in step (B) is preferably carried out in a closed mould and the fusion can be carried out using water vapour, hot air (for example as described in EP1979401B1) or energetic radiation (microwaves or radio waves).
[0095] The temperature during fusion of the foam pellets is preferably below or near the melting temperature of the polymer from which the bead foam is produced. Thus, for commonly used polymers, the temperature of fusion of the foam pellets is between 100°C and 180°C, preferably between 120°C and 150°C.
[0096] The temperature profile / residence time can be determined individually here, for example, similarly to the methods described in US20150337102 or EP2872309B1.
[0097] Fusion by energetic radiation is generally carried out in the microwave or radio frequency range, optionally in the presence of water or other polar liquids, such as microwave absorbing hydrocarbons with polar groups (e.g. esters of carboxylic acids with diols or triols, or glycols and liquid polyethylene glycols), and can be carried out similarly to the methods described in EP 3053732A or WO 16146537.
[0098] As mentioned above, the foamed pellets may also include a colorant, which may be added in a variety of ways.
[0099] In one embodiment, the foamed pellets produced can be colored after production. In this case, the corresponding foamed pellets are contacted with a carrier liquid containing a colorant, the carrier liquid (CL) having a suitable polarity for adsorption of the carrier liquid onto the foamed pellets to occur. This can be done similarly to the method described in the EP application with application number 17198591.4.
[0100] Examples of suitable colorants are inorganic or organic pigments. Examples of suitable natural or synthetic inorganic pigments are carbon black, graphite, titanium oxide, iron oxide, zirconium oxide, cobalt oxide compounds, chromium oxide compounds, copper oxide compounds. Examples of suitable organic pigments are azo pigments and polycyclic pigments.
[0101] In a further embodiment, the color can be added during the production of the foam pellets. By way of example, the colorant can be added to the extruder via extrusion during the production of the foam pellets.
[0102] Alternatively, already pigmented material can be used as the starting material for the production of foamed pellets, which are extruded or expanded in a closed container by the processes described above.
[0103] Additionally, in the process described in WO2014150122, the supercritical liquid or heated liquid may contain a colorant.
[0104] As stated above, the mouldings of the invention have advantageous properties for the above mentioned applications in the requirements of the footwear and sports footwear industry sector.
[0105] In this case, the tensile and compressive properties of the mouldings produced from the foamed pellets are distinguished by the fact that the tensile strength exceeds 600 kPa (DIN EN ISO 1798, April 2008), the elongation at break exceeds 100% (DIN EN ISO 1798, April 2008) and the compressive stress exceeds 15 kPa at 10% compression (similar to DIN EN ISO 844, November 2014; the deviation from the standard, the specimen height, is 20 mm instead of 50 mm and the test speed is therefore adjusted to 2 mm / min).
[0106] The resilience of the mouldings resulting from the foamed pellets is greater than 55% (similar to DIN 53512, April 2000; the deviation from the standard is the height of the test specimen, which should be 12 mm, but in this test 20 mm is used to avoid "penetration through" the specimen and measurement of the substrate).
[0107] As mentioned above, there is a relationship between the density and the compression properties of the resulting compact. The density of the resulting compact is advantageously between 75 and 375 kg / m 3 , preferably 100 to 300 kg / m3 , particularly preferably 150 to 200 kg / m 3 (DIN EN ISO845, October 2009).
[0108] The ratio of the density of the mouldings to the bulk density of the foamed pellets according to the invention is here generally between 1.5 and 2.5, preferably between 1.8 and 2.0.
[0109] The invention further provides a method of using the foamed pellets of the invention for producing moldings for shoe insoles, shoe insoles, shoe combi-soles, bicycle saddles, bicycle tires, damping elements, cushioning, mattresses, underlays, grips, protective films, in components in automotive interiors and exteriors, in balls and sports equipment or as floor coverings, in particular for sports surfaces, athletics surfaces, sports halls, children's parks and walkways.
[0110] It is preferred to use the foamed pellets according to the invention to produce moldings for shoe insoles, shoe insoles, shoe combi-soles or cushioning elements for shoes.
[0111] Here, the shoes are preferably outdoor shoes, sports shoes, sandals, boots or safety shoes, particularly preferably sports shoes.
[0112] The invention therefore further provides a molding which is a shoe combi-sole for a shoe, preferably for an outdoor shoe, a sports shoe, a sandal, a boot or a safety shoe, particularly preferably for a sports shoe.
[0113] The invention therefore further provides a moulded body which is an insole for shoes, preferably for outdoor shoes, sports shoes, sandals, boots or safety shoes, particularly preferably for sports shoes.
[0114] The invention therefore further provides a moulding which is an insole for a shoe, preferably for an outdoor shoe, a sports shoe, a sandal, a boot or a safety shoe, particularly preferably for a sports shoe.
[0115] The invention therefore further provides a moulded article, wherein the moulded object is a cushioning element for shoes, preferably for outdoor shoes, sports shoes, sandals, boots or safety shoes, particularly preferably for sports shoes.
[0116] The cushioning element may be used in the heel region or the forefoot region, here by way of example.
[0117] The present invention therefore further provides a shoe in which the inventive molding is used as a midsole, insole or cushioning, for example in the heel region or forefoot region, which shoe is preferably an outdoor shoe, a sports shoe, a sandal, a boot or a safety shoe, particularly preferably a sports shoe.
[0118] In a further aspect, the present invention also relates to foamed pellets obtainable or obtainable by the process of the present invention.
[0119] The block copolymers used according to the present invention usually have a hard phase, which is composed of aromatic polyester, and a soft phase. Due to these predefined block structures, such as polytetrahydrofuran building blocks and polybutylene terephthalate building blocks, which are themselves already polymers and therefore result from the construction of molecules that are long chains, the block copolymers used according to the present invention have good phase separation between the elastic soft phase and the rigid hard phase. This good phase separation is manifested as a property called high "snapback", which can be very difficult to characterize using only physical methods, and this leads to the particularly advantageous properties of the foamed pellets of the present invention.
[0120] Due to the good mechanical properties and good temperature behavior, the polymer foams of the invention are particularly suitable for the production of moldings, which can be produced from the foam pellets of the invention, for example by fusion or bonding.
[0121] In a further aspect, the present invention also relates to a method of using the foamed pellets of the present invention or the foamed pellets obtainable or obtainable by the method of the present invention for producing a molded body. Thus, in a further embodiment, the present invention also relates to a method of using the foamed pellets of the present invention or the foamed pellets obtainable or obtainable by the method of the present invention for producing a molded body, wherein the molded body is produced by means of fusion or bonding of the beads to each other.
[0122] The mouldings obtainable according to the invention are suitable, for example, for the production of shoe soles, parts of shoe soles, bicycle saddles, cushioning, mattresses, underlays, grips, protective films, components in automobile interiors and exteriors, components in balls and sports equipment or as floor coverings, and also for wall panels, in particular sports surfaces, athletics surfaces, sports halls, children's parks and walkways.
[0123] Therefore, in a further embodiment, the present invention also relates to a method of using the foamed pellets of the present invention or the foamed pellets obtained or obtainable by the method of the present invention for producing a molded body, which is a shoe sole, a part of a shoe sole, a bicycle saddle, a cushioning material, a mattress, an underlay, a grip, a protective film, a component in an automobile interior and exterior.
[0124] In a further aspect, the present invention also relates to the use of the foam pellets or foam beads of the present invention in balls and sports equipment or as floor coverings and wall panels, in particular for sports surfaces, athletics surfaces, sports halls, children's parks and walkways.
[0125] In a further aspect, the present invention also relates to a hybrid material comprising a matrix made of a polymer (PM) and foamed pellets according to the present invention. A material comprising foamed pellets and a matrix material is called a hybrid material in the context of the present invention. Here, the matrix material may be made of a compression molded material or also a foamed material.
[0126] Polymers (PM) suitable as matrix materials are known per se to those skilled in the art. For example, ethylene-vinyl acetate copolymers, epoxy-based binders, and also polyurethanes, are suitable in the context of the present invention. In this case, polyurethane foams, and also polyurethane compression moldings, such as thermoplastic polyurethanes, are suitable according to the present invention.
[0127] According to the invention, the polymer (PM) is selected here such that there is sufficient adhesion between the foamed pellets and the matrix to obtain a mechanically stable hybrid material.
[0128] The matrix here may be completely or partially surrounded by the foamed pellets. According to the invention, the hybrid material may contain further components, for example further fillers or also pellets. According to the invention, the hybrid material may also contain a mixture of different polymers (PM). The hybrid material may also contain a mixture of foamed pellets.
[0129] Foam pellets which can be used in addition to the foam pellets according to the invention are known per se to the person skilled in the art. Foam pellets composed of thermoplastic polyurethanes are particularly suitable within the context of the present invention.
[0130] Thus, in one embodiment, the present invention also relates to a hybrid material comprising a matrix made of a polymer (PM), expanded pellets according to the invention and further expanded pellets made of a thermoplastic polyurethane.
[0131] In the context of the present invention, the matrix consists of a polymer (PM). Examples of suitable matrix materials in the context of the present invention are elastomers or foams, in particular polyurethane-based foams, such as elastomers, for example ethylene-vinyl acetate copolymers or else thermoplastic polyurethanes.
[0132] The present invention therefore also relates to a hybrid material as previously described, in which the polymer (PM) is an elastomer. The present invention further relates to a hybrid material as previously described, in which the polymer (PM) is selected from the group consisting of ethylene-vinyl acetate copolymers and thermoplastic polyurethanes.
[0133] In one embodiment, the present invention also relates to a hybrid material comprising a matrix composed of an ethylene-vinyl acetate copolymer and the foamed pellets according to the present invention.
[0134] In a further embodiment, the present invention relates to a hybrid material comprising a matrix composed of an ethylene-vinyl acetate copolymer, foamed pellets according to the invention and further foamed pellets composed, for example, of a thermoplastic polyurethane.
[0135] In one embodiment, the present invention relates to a hybrid material comprising a matrix composed of thermoplastic polyurethane and foamed pellets according to the present invention.
[0136] In a further embodiment, the present invention relates to a hybrid material comprising a matrix composed of a thermoplastic polyurethane, expanded pellets according to the invention and further expanded pellets, for example composed of a thermoplastic polyurethane.
[0137] Suitable thermoplastic polyurethanes are known per se to those skilled in the art. They are described, for example, in "Kunststoffhandbuch [Plastics Handbook], Volume 7, Polyurethane [Polyurethanes]", Carl Hanser Verlag, 3rd Edition, 1993, Chapter 3.
[0138] In the context of the present invention, the polymer (PM) is preferably a polyurethane. Within the meaning of the present invention, "polyurethane" encompasses all known elastic polyisocyanate polyaddition products. These include, in particular, compression molded products of polyisocyanate polyaddition products, such as viscoelastic gels or thermoplastic polyurethanes, and elastic foams based on polyisocyanate polyaddition products, such as flexible foams, semi-rigid foams or monolithic foams. Within the meaning of the present invention, "polyurethane" is also considered to mean elastic polymer blends comprising polyurethane and further polymers, as well as foams of these polymer blends. The matrix is preferably a compression molded product of a cured polyurethane binder, an elastic polyurethane foam foam or a viscoelastic gel.
[0139] In the context of the present invention, "polyurethane binder" is taken here to mean a mixture which constitutes to the extent of at least 50% by weight, preferably to the extent of at least 80% by weight, in particular to the extent of at least 95% by weight, of prepolymers containing isocyanate groups (hereinafter referred to as isocyanate prepolymers). The viscosity of the polyurethane binder according to the invention is preferably here in the range from 500 to 4000 mPa.s, particularly preferably in the range from 1000 to 3000 mPa.s, measured at 25° C. according to DIN 53 018.
[0140] In the context of the present invention, "polyurethane foam" is taken to mean a foam according to DIN 7726.
[0141] The density of the matrix material is preferably 1.2 to 0.01 g / cm 3 The matrix material is particularly preferably in the range of 0.8 to 0.1 g / cm 3 In particular, the range of 0.6 to 0.3 g / cm 3 The preferred foams are resilient or monolithic foams having densities in the range of 0.1 to 1.0 mm, or compression molded materials such as cured polyurethane binders.
[0142] Foams are particularly suitable matrix materials. Hybrid materials that include a matrix material comprised of polyurethane foam foam preferably exhibit good adhesion between the matrix material and the foam pellets.
[0143] In one embodiment, the present invention also relates to a hybrid material comprising a matrix composed of polyurethane foam foam and foamed pellets according to the present invention.
[0144] In a further embodiment, the present invention relates to a hybrid material comprising a matrix composed of a polyurethane foam foam, foam pellets according to the invention, and further foam pellets composed, for example, of a thermoplastic polyurethane.
[0145] In one embodiment, the present invention relates to a hybrid material comprising a matrix composed of polyurethane integral foam and foamed pellets according to the present invention.
[0146] In a further embodiment, the present invention relates to a hybrid material comprising a matrix composed of a polyurethane integral foam, foam pellets according to the invention, and further foam pellets composed, for example, of a thermoplastic polyurethane.
[0147] The hybrid material of the present invention comprising a polymer (PM) as a matrix and the foamed pellets of the present invention can be produced, for example, by mixing the components used to produce the polymer (PM) and the foamed pellets, optionally further components, and reacting them to obtain the hybrid material, the reaction being preferably carried out under conditions in which the foamed pellets are essentially stable.
[0148] Suitable processes and reaction conditions for producing polymers (PM), in particular ethylene-vinyl acetate copolymers or polyurethanes, are known per se to those skilled in the art.
[0149] In a preferred embodiment, the hybrid material of the invention is an integral foam, in particular an integral foam based on polyurethane. Suitable methods for producing integral foams are known per se to those skilled in the art. The integral foams are preferably produced in a one-shot process using low-pressure or high-pressure techniques in a closed, advantageously temperature-controlled mould. The mould is preferably made of metal, for example aluminium or steel. These procedures are described, for example, by Piechota and Roehr in "Integralschaumstoff" [Integral Foam], Carl-Hanser-Verlag, Munich, Vienna, 1975, or in "Kunststoff-Handbuch" [Plastics Handbook], Vol. 7, "Polyurethane" [Polyurethanes], 3rd edition, 1993, Chapter 7.
[0150] When the hybrid material of the present invention includes an integral foam, the amount of reaction mixture introduced into the mold is such that the resulting molded article composed of the integral foam is 0.08 to 0.70 g / cm 3 , especially 0.12 to 0.60 g / cm 3 The degree of compression molding to produce a molding having a compression molded surface zone and a cellular core is in the range of 1.1 to 8.5, preferably 2.1 to 7.0.
[0151] Therefore, it is possible to produce a hybrid material with a matrix composed of polymer (PM) and the foamed pellets of the present invention contained therein, in which there is a homogeneous distribution of foamed beads.The foamed pellets of the present invention can be easily used in the method for producing a hybrid material, since due to their small size, the individual beads are free-flowing and do not impose any special requirements on processing.Techniques for homogeneous distribution of foamed pellets, such as slow-rolling type, can be used here.
[0152] Further auxiliaries and / or additives may be optionally added to the reaction mixture to produce the hybrid material of the present invention, examples of which include surface active substances, foam stabilizers, cell regulators, release agents, fillers, dyes, pigments, hydrolysis stabilizers, odor absorbing substances and fungistatic and bacteriostatic substances.
[0153] The surface-active substances that can be used are compounds that serve to support the homogenization of starting materials and are suitable for adjusting cell structure.Examples include emulsifiers, such as castor oil sulfate or the sodium salt of fatty acid, as well as the salts of fatty acids with amines, such as diethylamine oleate, diethanolamine stearate, diethanolamine ricinoleate, salts of sulfonic acids, such as the alkali metal or ammonium salts of dodecylbenzene disulfonic acid or dinaphthylmethane disulfonic acid and ricinoleic acid, foam stabilizers, such as siloxane-oxyalkylene copolymers and other organopolysiloxanes, ethoxylated alkylphenols, ethoxylated fatty alcohols, paraffin oil, castor oil esters or ricinoleic acid esters, turmeric oil and peanut oil, and cell regulators, such as paraffin, fatty alcohols and dimethylpolysiloxane. Oligomeric acrylates having polyoxyalkylene and fluoroalkane groups as pendant groups are also suitable for improving the emulsification, cell structure and / or foam stabilization.
[0154] For example, suitable release agents include reaction products of fatty acid esters with polyisocyanates, salts of amino-group-containing polysiloxanes with fatty acids, salts of saturated or unsaturated (cyclo)aliphatic carboxylic acids having at least 8 carbon atoms and tertiary amines, and more particularly internal release agents, such as mixtures of montanic acid and at least one aliphatic carboxylic acid having at least 10 carbon atoms with at least bifunctional alkanolamines, polyols and / or polyamines having a molecular weight of 60 to 400, mixtures of organic amines, mixtures of stearic acid and metal salts of organic mono- and / or dicarboxylic acids or their anhydrides, or mixtures of imino compounds, metal salts of carboxylic acids, and carboxylic acid esters and / or carboxylamides, optionally produced by esterifying or amidating carboxylic acids.
[0155] Fillers, especially reinforcing fillers, are taken to mean conventional organic and inorganic fillers, reinforcing materials, extenders, agents for improving the wear behavior of paints, coating compositions, etc., which are known per se. Specific examples which may be mentioned are inorganic fillers, such as siliceous minerals, such as sheet silicates, for example antigorite, bentonite, serpentine, hornblende, amphibole, chrysotile, talc; metal oxides, such as kaolin, aluminum oxide, titanium oxide, zinc oxide and iron oxide, metal salts, for example chalk, barytes, and inorganic pigments, such as cadmium sulfide, zinc sulfide, and also glass. It is preferred to use kaolin (china clay), aluminum silicate and coprecipitates of barium sulfate and aluminum silicate, and also natural and synthetic fibrous minerals, such as wollastonite, metal fibers, and in particular glass fibers of various lengths, which can be sized arbitrarily. Examples of organic fillers which can be used are carbon black, melamine, colophony, cyclopentadienyl resins and graft polymers, also cellulose fibres, polyamide fibres, polyacrylonitrile fibres, polyurethane fibres, polyester fibres based on aromatic and / or aliphatic dicarboxyl esters, and especially carbon fibres.
[0156] The inorganic and organic fillers can be used individually or as a mixture.
[0157] In the hybrid material of the present invention, the proportion by volume of the foamed pellets is preferably at least 20 volume percent, particularly preferably at least 50 volume percent, more preferably at least 80 volume percent, in particular at least 90 volume percent, in each case relative to the volume of the hybrid system of the present invention.
[0158] The hybrid materials of the present invention, in particular those having a matrix composed of cellular polyurethane, are characterized by a very good adhesion of the matrix material to the foamed pellets of the present invention, so that the hybrid materials of the present invention preferably do not tear at the interface between the matrix material and the foamed pellets, which allows the hybrid materials to have improved mechanical properties, such as tear propagation resistance and elasticity, for a given density, compared to conventional polymer materials, in particular compared to conventional polyurethane materials.
[0159] According to DIN 53512, the elasticity of the hybrid material according to the invention in the form of an integral foam is preferably more than 40%, particularly preferably more than 50%.
[0160] The hybrid material of the present invention, especially one based on a one-piece foam, further exhibits high resilience at low density. Therefore, the one-piece foam based on the hybrid material of the present invention is particularly suitable as a shoe sole material. A light, comfortable sole with good durability properties is obtained as a result. Such a material is particularly suitable as an insole for sports shoes.
[0161] The hybrid material of the present invention having a cellular matrix is suitable for cushioning in furniture and mattresses, for example.
[0162] Hybrid materials with a matrix composed of viscoelastic gels are particularly characterized by the properties of increased viscoelasticity and improved elasticity, and are therefore also suitable as materials of cushioning, for example for seats, in particular for saddles, for example bicycle saddles or motorcycle saddles.
[0163] Hybrid materials with a compression moulded matrix are suitable, for example, as floor coverings, in particular as coverings for playgrounds, athletics surfaces, sports fields and sports halls.
[0164] The properties of the hybrid materials of the present invention can vary within wide limits depending on the polymer (PM) used, in particular by variation of the size, shape and properties of the expanded pellets, but also within wide boundaries by the addition of further additives, for example also additional non-expanded pellets, for example plastic pellets, for example rubber pellets.
[0165] The hybrid material of the present invention has high durability and toughness, which is manifested in particular by high tensile strength and elongation at break. In addition, the hybrid material of the present invention has low density.
[0166] Further embodiments of the invention can be found in the claims and examples. It should be recognized that the features of the subject matter / method / method of use according to the invention described above and hereinafter can be used not only in the combination specified in each case, but also in other combinations without departing from the scope of the invention. Thus, for example, combinations of preferred features with particularly preferred features, or combinations of preferred features with features not further characterized as particularly preferred features, etc., are implicitly encompassed even if this combination is not explicitly described.
[0167] Exemplary embodiments of the invention are listed below without, however, limiting the invention. In particular, the invention also encompasses those embodiments resulting from recitation in the dependent claims and therefore the combinations specified herein below. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0168] 1. At least components (i) to (iii): (i) a polyisocyanate composition (IC); (ii) at least one chain extender (CE1); (iii) polyol composition (PC), 1. Foamed pellets comprising a thermoplastic polyurethane obtainable or obtainable by reacting
[0169] 2. The foamed pellets according to embodiment 2, wherein the aliphatic diisocyanate is a linear diisocyanate having an even number of carbon atoms.
[0170] 3. The foamed pellets of embodiment 1 or 2, wherein the aliphatic diisocyanate is hexamethylene diisocyanate (HDI).
[0171] 4. The expanded pellets according to any of the preceding embodiments, wherein the chain extender (CE1) is selected from the group consisting of propane-1,3-diol, ethane-1,2-diol, butane-1,4-diol, hexane-1,6-diol and HQEE.
[0172] 5. The foamed pellets according to any one of the preceding embodiments, wherein the polyol composition comprises a polyol selected from the group consisting of polyetherols, polyesterols, polycaprolactone polyols and polycarbonate polyols.
[0173] 6. The foamed pellets according to any one of the preceding embodiments, wherein the polyol composition comprises a polyol selected from the group consisting of polytetrahydrofurans having a number average molecular weight Mn in the range of 500 g / mol to 2000 g / mol.
[0174] 7. A method for producing foamed pellets, comprising: (i) A step of preparing a composition (C1) containing a thermoplastic polyurethane, the thermoplastic polyurethane comprising at least components (a) to (c): (a) a polyisocyanate composition (IC), (b) at least one chain extender (CE1); (c) polyol composition (PC), wherein the isocyanate composition comprises at least one aliphatic diisocyanate having a number average molecular weight of less than 200 g / mole; (ii) impregnating composition (C1) with a blowing agent under pressure; (iii) Expanding composition (C1) using a pressure reduction A method comprising:
[0175] 8. The method of embodiment 2, wherein the aliphatic diisocyanate is a linear diisocyanate having an even number of carbon atoms.
[0176] 9. The method of embodiment 1 or 2, wherein the aliphatic diisocyanate is hexamethylene diisocyanate (HDI).
[0177] 10. The method according to any of the preceding claims, wherein the chain extender (CE1) is selected from the group consisting of propane-1,3-diol, ethane-1,2-diol, butane-1,4-diol, hexane-1,6-diol and HQEE.
[0178] 11. The method of any of the preceding claims, wherein the polyol composition comprises a polyol selected from the group consisting of polyetherols, polyesterols, polycaprolactone polyols and polycarbonate polyols.
[0179] 12. The method of any of the preceding embodiments, wherein the polyol composition comprises a polyol selected from the group consisting of polytetrahydrofurans having a number average molecular weight Mn in the range of 500 g / mol to 2000 g / mol.
[0180] 13. Expanded pellets obtained or obtainable by the method according to any of embodiments 7 to 12.
[0181] 14. A method of using the foamed pellets according to any of embodiments 1 to 6 or 13 for producing a molded body.
[0182] 15. The method of embodiment 14, wherein the shaped body is produced by fusing or bonding beads together.
[0183] 16. The method according to embodiment 14 or 15, wherein the shaped article is a shoe sole, a part of a shoe sole, a bicycle saddle, a cushioning material, a mattress, an underlay, a grip, a protective film, or a component in an automobile interior or exterior.
[0184] 17. Use of the foamed pellets according to any of embodiments 1 to 6 or 13 in balls and sports equipment or as floor coverings and wall panels, in particular for sports surfaces, athletics surfaces, sports halls, children's parks and walkways.
[0185] 18. A hybrid material comprising a matrix composed of a polymer (PM) and expanded pellets according to any of embodiments 1 to 6 or 13 or obtainable or obtainable by the method according to any of embodiments 7 to 12.
[0186] 19. The hybrid material of embodiment 18, wherein the polymer (PM) is EVA.
[0187] 20. The hybrid material according to embodiment 18, wherein the polymer (PM) is a thermoplastic polyurethane.
[0188] 21. The hybrid material of embodiment 18, wherein the polymer (PM) is a polyurethane foam.
[0189] 22. The hybrid material of embodiment 18, wherein the polymer (PM) is a polyurethane monolithic foam.
[0190] The following examples serve to illustrate the invention and are in no way limiting with respect to the subject matter thereof. EXAMPLES
[0191] 1. The following feedstocks were used: Polyol 1: polyether polyol with an OH number of 112.2 and exclusively primary OH groups (based on tetramethylene oxide, functionality: 2) Chain extender 1: Butane-1,4-diol Isocyanate 1: Aliphatic isocyanate (hexamethylene 1,6-diisocyanate) Isocyanate 2: Aromatic isocyanate (methylenediphenyl 4,4'-diisocyanate) Catalyst 1: Tin(II) dioctoate (50% in DOA) Catalyst 2: Tin(II) dioctoate (10% in DOA) Antioxidants 1: sterically hindered phenols Antioxidants 2: sterically hindered phenols TPU Crosslinker 1: Thermoplastic polyurethane with NCO content of 8.5% and functionality of 2.05 by addition of oligomeric MDI
[0192] 2. Generate TPU The following examples TPU1-4, identified hereafter, were produced in a ZSK58 MC twin screw extruder (manufactured by Coperion) with a processing length of 48D (12 barrels). A gear pump was used to discharge the melt from the extruder. After filtration of the melt, underwater pelletization was used to process the polymer melt into pellets, which were continuously dried in a heated fluidized bed at 40-90°C.
[0193] The polyol, chain extender and diisocyanate, plus any optional catalyst, were metered into the first zone. The feeding of further additives as described above is carried out in zone 8.
[0194] The barrel temperature is in the range of 150-230°C. Melt discharge and underwater pelletization are carried out at a melt temperature of 210-230°C. The feed rate is 180-240 min -1 The throughput is in the range of 180-220 kg / hour.
[0195] Doses are summarized in Table 1.
[0196] [Table 1]
[0197] 3. Creating eTPU 3.1 A twin-screw extruder with a screw diameter of 44 mm and a length to diameter ratio of 42, equipped with a connected melt pump, starter valve with screen changer, die plate and underwater pelletizer, was used to produce expanded beads made of thermoplastic polyurethane (Table 1). The thermoplastic polyurethane was dried and then processed at 80° C. for 3 hours to obtain a residual water content of less than 0.02% by weight. In addition to the thermoplastic polyurethane, TPU that had been blended with diphenylmethane 4,4′-diisocyanate having an average functionality of 2.05 was added in a separate extrusion process.
[0198] Each thermoplastic polyurethane used, as well as TPU crosslinker 1, were each weighed separately into the inlet of a twin-screw extruder via a gravimetric metering device.
[0199] After the materials were metered into the inlet of the twin-screw extruder, they were melted and mixed. The blowing agents CO2 and N2 were added subsequently through one injector each. The remaining length of the extruder was used for uniform incorporation of the blowing agent into the polymer melt. After the extruder, the polymer / blowing agent mixture was forced using a gear pump (GP) through an actuation valve with a screen changer (SV) to a die plate (DP), where it was split into strands, which were cut into pellets in the pressurized cutting chamber of the underwater pelletizer (UWP) with a temperature-controlled liquid flow, conveyed out of the water, and expanded in the process.
[0200] A centrifugal dryer was used to ensure that the expanded beads were separated from the process water.
[0201] The total throughput of the extruder, polymer and blowing agent was 40 kg / h. Table 2 lists the amounts of polymer and blowing agent used, where the polymer always constitutes 100 parts and the blowing agent is additionally counted so that the total of the resulting composition is greater than 100 parts.
[0202] [Table 2]
[0203] The temperatures used for the extruder and downstream devices as well as the pressure in the cutting chamber of the UWP are listed in Table 3.
[0204] [Table 3]
[0205] After separating the water from the swollen pellets using a centrifugal dryer, the swollen pellets are dried at 60° C. for 3 hours to remove any remaining surface water and any moisture that may be present in the beads, preventing them from interfering with further analysis of the beads.
[0206] Table 4 lists the resulting bulk densities for each expanded thermoplastic polyurethane after drying.
[0207] [Table 4]
[0208] 3.2 In addition to processing in the extruder, expanded beads were also produced in an impregnation tank. For this purpose, the tank was filled with solid / liquid phase to a filling level of 80%, with a phase ratio of 0.32.
[0209] The solid phase is identified here as TPU1 or TPU2, and the liquid phase as a mixture of water with calcium carbonate and surfactant. The blowing agent (butane) was injected into this mixture in a tight gas tank (previously purged with nitrogen) in the amount for the solid phase (TPU1 or TPU2) indicated in Table 5. The tank was heated while stirring the solid / liquid phase and nitrogen was injected in a defined manner at a pressure up to 8 bar and a temperature of 50° C. Heating was subsequently continued until the desired impregnation temperature (IMT) was reached. Once the impregnation temperature and impregnation pressure were reached, after a given hold time, the tank was depressurized via a valve. The exact production parameters of the experiment as well as the achieved bulk density are listed in Table 5.
[0210] [Table 5]
[0211] 4. Fusion and Mechanical Properties 4.1 Formation of green bodies by steam fusion The expanded pellets were subsequently fused to obtain square planks with a side length of 200 mm and a thickness of 10 mm or 20 mm by contacting them with water steam in a molding machine from Kurtz ersa GmbH (Energy Foamer). For the plank thickness, the fusion parameters differ only with respect to cooling. The fusion parameters for the different materials were selected so that the plank side of the final molding facing the movable side of the mold (MII) had the minimum number of collapsed eTPU beads. Gap steaming was also optionally performed through the movable side of the mold. Regardless of the experiment, a cooling time of 120 seconds for plank thickness 20 mm and 100 seconds for plank thickness 10 mm from the fixed side (MI) and the movable side of the mold was always established at the end. Table 6 lists the respective steaming conditions in steam pressure. The planks are stored in an oven at 70 °C for 4 hours.
[0212] [Table 6]
[0213] [Table 7]
[0214] 4.2 Comparative experiment of rebound resilience To demonstrate the better resilience of the claimed material, two TPUs (TPU3 and TPU4) with a hard phase of MDI but with the same Shore hardness as TPU1 and TPU2 were also foamed in the impregnation process as described above.
[0215] For this purpose, the tank was filled with solid / liquid phase to a filling level of 80%, the phase ratio being 0.32.
[0216] The solid phase can now be seen as TPU3 or TPU4, and the liquid phase as a mixture of water with calcium carbonate and surfactant. The blowing agent (butane) was injected into a tight gas tank (previously purged with nitrogen) and onto this mixture in the amount shown in Table 8 for the solid phase (TPU3 or TPU4). The tank was heated while stirring the solid / liquid phase and nitrogen was injected in a defined manner at a pressure up to 8 bar and a temperature of 50° C. Heating was continued until the desired impregnation temperature (IMT). Once the impregnation temperature and pressure were reached, the tank was depressurized via a valve after a given hold time.
[0217] [Table 8]
[0218] The expanded pellets were subsequently fused to obtain square planks with a side length of 200 mm and a thickness of 20 mm by contacting them with steam in a molding machine from Kurtz ersa GmbH (Energy Foamer). The fusion parameters for the different materials were selected so that the plank side of the final molding facing the movable side of the mold (MII) had the minimum number of collapsed eTPU beads. Regardless of the experiment, a cooling time of 40 seconds from the fixed side (MI) and the movable side of the mold was always established at the end. Table 9 lists the respective steaming conditions. The planks are then stored in an oven at 70° C. for 4 hours.
[0219] [Table 9]
[0220] The rebound resilience was subsequently determined for all samples according to DIN EN ISO 8307:2008-03 (Table 10).
[0221] [Table 10]
[0222] 5.Measurement method: Measurement methods that can be used for material characterization include: DSC, DMA, TMA, NMR, FT-IR, GPC Mechanical properties (eTPU) Foam density DIN EN ISO845:2009-10 Tear propagation resistance DIN EN ISO8067:2009-06 Dimensional stability test ISO 2796:1986-08 Tensile Test ASTM D5035:2011 Resilience DIN 53512:2000-4 (Table 7) DIN EN ISO8307:2008-03 (Table 10)
[0223] References WO 94 / 20568 A1 WO 2007 / 082838 A1 WO 2017 / 030835 A1 WO 2013 / 153190 A1 WO 2010 / 010010 “Kunststoffhandbuch Band 7, Polyurethane” [Plastics Handbook, volume 7, Polyurethane], Carl Hanser Verlag, 3rd edition, 1993, chapter 3.1. WO 2007 / 082838 A1 WO 2013 / 153190 A1 Saechtling (Ed.), Kunststoff-Taschenbuch [Plastics Handbook], 27th edition, Hanser-Verlag, Munich 1998, chapters 3.2.1 and 3.2.4 WO 2014 / 150122 A1 WO 2014 / 150124 A1 EP 1 979 401B1 US 2015 / 0337102 A1 EP 2 872 309B1 EP 3 053 732 A1 WO 2016 / 146537 A1
Claims
1. At least components (i) to (iii): (i) a polyisocyanate composition (IC), (ii) at least one chain extender (CE1); (iii) polyol composition (PC); 1. Foamed pellets comprising a thermoplastic polyurethane obtainable or obtainable by reacting the polyisocyanate composition comprises at least one linear, aliphatic diisocyanate having a number average molecular weight of less than 200 g / mol, and if further isocyanates are used, they are present in the polyisocyanate composition (IC) in an amount ranging from 0.1% to 20% by weight, said chain extender (CE1) being a diamine or diol having a molecular weight of less than 500 g / mol; The average diameter of the beads of the foamed pellets is 0.2 to 20 mm; the further isocyanate is an aromatic diisocyanate, the polyol composition comprises a polyol selected from the group consisting of polyetherols, polyesterols, polycaprolactone polyols, and polycarbonate polyols; The foamed pellets, wherein the polyol composition has an average functionality between 1.8 and 2.
3.
2. 2. The foamed pellets of claim 1, wherein the aliphatic diisocyanate is a linear diisocyanate having an even number of carbon atoms.
3. 3. The foamed pellets according to claim 1 or 2, wherein the aliphatic diisocyanate is hexamethylene diisocyanate (HDI).
4. The foamed pellets according to any one of claims 1 to 3, wherein the chain extender (CE1) is selected from the group consisting of propane-1,3-diol, ethane-1,2-diol, butane-1,4-diol, hexane-1,6-diol and HQEE.
5. The foamed pellets according to any one of claims 1 to 4, wherein the polyol composition comprises a polyol selected from the group consisting of polytetrahydrofurans having a number average molecular weight Mn in the range of 500 g / mol to 2000 g / mol.
6. 1. A method for producing foamed pellets, comprising: (i) preparing a composition (C1) comprising a thermoplastic polyurethane, the thermoplastic polyurethane comprising at least components (a)-(c): (a) a polyisocyanate composition (IC), (b) at least one chain extender (CE1); (c) a polyol composition (PC); wherein the polyisocyanate composition comprises at least one linear, aliphatic diisocyanate having a number average molecular weight of less than 200 g / mol, and if further isocyanates are used, they are present in the polyisocyanate composition (IC) in an amount ranging from 0.1% to 20% by weight, wherein said chain extender (CE1) is a diamine or diol having a molecular weight of less than 500 g / mol; (ii) impregnating the composition (C1) with a blowing agent under pressure; (iii) Expanding said composition (C1) using a pressure reduction The foamed pellets have an average bead diameter of 0.2 to 20 mm; the further isocyanate is an aromatic diisocyanate, the polyol composition comprises a polyol selected from the group consisting of polyetherols, polyesterols, polycaprolactone polyols, and polycarbonate polyols; The method wherein the polyol composition has an average functionality between 1.8 and 2.
3.
7. 6. Use of the foamed pellets according to any one of claims 1 to 5 for producing a moulded body.
8. The method of claim 7 , wherein the shaped body is produced by fusing or bonding the beads together.
9. 9. The method according to claim 7 or 8, wherein the molded article is a shoe sole, a part of a shoe sole, a bicycle saddle, a cushioning material, a mattress, an underlay, a grip, a protective film, or a component in the interior or exterior of an automobile.
10. 6. Use of the foamed pellets according to any one of claims 1 to 5 in balls or sports equipment or as floor coverings or wall panels.
11. A hybrid material comprising a matrix composed of a polymer (PM) and the foamed pellets according to any one of claims 1 to 5.
Citation Information
Patent Citations
Light-weighted polyurethane foam material with high physical properties and preparation method of light-weighted polyurethane foam material
CN105273394A
Novel composite foaming material and preparation method thereof
CN108559057A
Method for producing effervescent polylactic acid-containing granules
JP2013517340A
Method for producing expanded polyester foam beads
JP2016537450A
Expanded thermoplastic polyurethane beads, their manufacturing method and method for manufacturing molded parts
JP2019535873A