A blend of TPU and polyamide
A blend of thermoplastic polyurethane and copolyamide addresses processing challenges by enhancing melt strength and range, offering improved mechanical properties and flame retardancy for industrial applications.
Patent Information
- Application Number
- JP2021564372
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2019-04-30
- Filing Date
- 2020-04-29
- Publication Date
- 2024-12-04
- Estimated Expiration
- 2040-04-29
AI Technical Summary
Thermoplastic polyurethanes (TPU) face challenges in processing due to re-dissociation of urethane bonds during high-temperature melting, leading to degradation and low melt strength, especially in extrusion processes for large shaped articles, while polyamides offer high melt strength but are difficult to process at high temperatures.
A composition comprising thermoplastic polyurethane (TPU) blended with a copolyamide (PA-1) prepared from C32-C40 dimer acid and C4-C12 diamine, enhancing melt strength and processing range, and allowing incorporation of flame retardants for improved mechanical properties and combustion performance.
The blend achieves high toughness, improved melt strength, and a wide processing range, enabling transparent materials with enhanced mechanical properties and flame retardancy, suitable for various industrial applications.
Smart Images

Figure 0007594547000001 
Figure 0007594547000002 
Figure 0007594547000003
Abstract
Description
[Technical field]
[0001] The present invention relates to a composition comprising at least one thermoplastic polyurethane (TPU-1) and a copolyamide (PA-1), which is prepared by polymerizing at least one lactam and a monomer mixture (M) comprising, as component (B1), at least one C32-C40 dimer acid and, as component (B2), at least one C4-C12 diamine. The present invention further relates to a process for producing such a composition and to the use of the composition of the present invention for the production of molded articles. [Background technology]
[0002] Thermoplastic polyurethanes are widely known and used as materials in many fields. Their properties can be adjusted within a wide range. Typically, thermoplastic polyurethanes can be processed within a certain temperature range. The problem in processing is the re-dissociation of urethane bonds, which leads to the degradation of thermoplastic polyurethanes during processing and very low melt strength, and therefore can cause problems during extrusion.
[0003] In particular, hard TPUs above about 40D are difficult to process. Firstly, the semi-crystalline material must be melted at high temperatures for processing, and secondly, the material is destroyed at these high temperatures. As a result, the material can only be processed in a very narrow temperature range. This is problematic when different temperatures occur at the nozzle, especially in processes for extruding large shaped articles. In this case, the material in the colder zone of the nozzle is not yet completely melted, but may already be destroyed in the hotter zone of the nozzle.
[0004] On the other hand, polyamides generally have high melt strength and a very wide processing range.Polyamides are characterized by very good mechanical properties, and are particularly important in industry, as they have high strength and toughness, good chemical stability and high abrasion resistance.Polyamides are used, for example, in fishing lines, climbing ropes and carpet linings.In addition, polyamides are also used to manufacture packaging films and packaging sheaths.
[0005] Copolyamides, which combine the advantages of different polyamides, are also frequently used for packaging films and packaging sheathing. A variety of copolyamides are described in the prior art.
[0006] EP 0352562 describes a film composed of a copolyamide, which is prepared from ε-caprolactam and preferably from 1 to 10 parts by weight of a dimer acid and a diamine. DE 2846596 describes a molded article composed of a copolyamide of caprolactam, a dimer fatty acid and hexamethylenediamine. Of particular interest in the industry are nylon-6 and nylon-6,6, which are used in many fields due to their excellent properties. However, nylon-6 and nylon-6,6 have very high melting temperatures.
[0007] WO 2018 / 050487 A1 describes copolyamides, which are prepared by polymerizing at least one lactam (A) with a monomer mixture (M), and further describes the production of a polymer film (P) comprising such a copolyamide. [Prior art documents] [Patent documents]
[0008] [Patent Document 1] EP0352562 [Patent Document 2] DE2846596 [Patent Document 3] WO2018 / 050487A1 Summary of the Invention [Problem to be solved by the invention]
[0009] It is an object of the present invention to go beyond the prior art and provide a material having improved melt strength and therefore a wide processing range, particularly in the hardness range of 40-90 D. It is a further object of the present invention to provide a material having improved melt strength and therefore a wide processing range, and which is transparent. [Means for solving the problem]
[0010] According to the invention, this object is at least (I) Thermoplastic polyurethane (TPU-1), and (II) Hereinafter: (A) at least one lactam; (B) a monomer mixture (M) comprising the following components: (B1) at least one C32-C40 dimer acid, and (B2) At least one C4-C12 diamine Copolyamide (PA-1), prepared by polymerization with This is achieved by the composition (Z-1) comprising:
[0011] Surprisingly, it has been found that the copolyamide (PA-1) can be blended with various thermoplastic polyurethanes. The blends have excellent mechanical properties, high toughness and high melt strength. It has also been found that it is possible to incorporate many flame retardants, including those with relatively low fracture temperatures, either directly into the corresponding blends or into the copolyamide (PA-1). The resulting materials have excellent mechanical properties, high toughness and good fire performance. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0012] The composition (Z-1) of the invention comprises at least one thermoplastic polyurethane (TPU-1) and a copolyamide (PA-1).
[0013] Thermoplastic polyurethanes are known in principle. They are typically produced by reacting isocyanates, isocyanate-reactive compounds and chain extenders, optionally in the presence of at least one catalyst and / or customary auxiliaries and / or additives. The isocyanates, isocyanate-reactive compounds and chain extenders, individually or collectively, are also called formation components.
[0014] In accordance with the invention, the isocyanates and isocyanate-reactive compounds customarily used are in principle suitable.
[0015] The isocyanate-reactive compound that can be used in principle includes any suitable compound known to those skilled in the art.According to the present invention, at least one diol is preferably used as the isocyanate-reactive compound.Here, in the present invention, it is possible to use any suitable diol, such as polyether diol or polyester diol, or a mixture of two or more of them.
[0016] According to the present invention, the thermoplastic polyurethane (TPU-1) is preferably prepared by using a polyol composition, typically comprising at least one polyol (P1), as the isocyanate-reactive compound. In the present invention, it is possible in principle to use any polyol that is suitable per se, for example polyesterols, polyetherols and / or polycarbonate diols. For example, the polyols used may have a molecular weight (Mn) in the range of 500 g / mol to 8000 g / mol and preferably an average functionality with respect to isocyanates of 1.8 to 2.3, preferably 1.9 to 2.2, in particular 2. Unless otherwise stated, the number average molecular weight is determined according to DIN 55672-1.
[0017] The polyol (P1) used preferably has a molecular weight in the range from 600 to 2000 daltons, more preferably in the range from 750 to 5000 daltons, in particular a molecular weight of about 1000 daltons.
[0018] The polyesters used may be polyesters based on diacids and diols. The diols used are preferably diols having from 2 to 10 carbon atoms, such as ethanediol, butanediol or hexanediol, in particular butane-1,4-diol, or mixtures thereof. The diacids used may be any known diacid, such as linear or branched diacids having from 4 to 12 carbon atoms, or mixtures thereof.
[0019] In addition, in the present invention, it is possible to use polyether polyols, such as those based on commonly known starting materials and conventional alkylene oxides, preferably ethylene oxide, propylene oxide and / or butylene oxide, more preferably 1,2-propylene oxide and ethylene oxide, and in particular polyoxytetramethylene glycol. One advantage of polyether polyols is that they have a relatively high hydrolytic stability.
[0020] Polyetherols with a low level of unsaturation are also suitable. In the present invention, polyols with a low level of unsaturation are understood to mean, in particular, polyether alcohols with a content of unsaturated compounds of less than 0.02 meq / g, preferably less than 0.01 meq / g. Such polyether alcohols are usually prepared by adding alkylene oxides, in particular ethylene oxide, propylene oxide and mixtures thereof, to the above-mentioned diols or triols in the presence of highly active catalysts.
[0021] Such highly active catalysts are preferably cesium hydroxide and polymetallic cyanide catalysts, also called DMC catalysts. A frequently and preferably used DMC catalyst is zinc hexacyanocobaltate. The DMC catalyst can be left in the polyether alcohol after the reaction, but is typically removed, for example, by settling or filtration.
[0022] Furthermore, in the present invention, it is possible to use polytetrahydrofuran, for example, polytetrahydrofuran having an average molecular weight Mn in the range of 400 to 1800 g / mol, preferably polytetrahydrofuran having an average molecular weight Mn in the range of 600 to 1500 g / mol, more preferably polytetrahydrofuran having an average molecular weight Mn in the range of 750 to 1250 g / mol, for example, polytetrahydrofuran having an average molecular weight Mn in the range of 900 to 1100 g / mol.
[0023] In particular, it has been found that when using polyols having an average molecular weight in the range of 900 to 1100 g / mol, compositions with a particularly advantageous property profile are obtained, for example the compositions according to the invention firstly have a low melting point and secondly have good low temperature properties.
[0024] Examples of suitable polycarbonate diols include polycarbonate diols based on alkane diols.Suitable polycarbonate diols are strictly difunctional OH-functional polycarbonate diols, preferably strictly difunctional OH-functional aliphatic polycarbonate diols.Suitable polycarbonate diols are, for example, based on butane-1,4-diol, pentane-1,5-diol or hexane-1,6-diol, in particular butane-1,4-diol, pentane-1,5-diol, hexane-1,6-diol, 3-methylpentane-1,5-diol or mixtures thereof, more preferably butane-1,4-diol, pentane-1,5-diol, hexane-1,6-diol or mixtures thereof. In the present invention, preferably, polycarbonate diols based on butane-1,4-diol and hexane-1,6-diol, polycarbonate diols based on pentane-1,5-diol and hexane-1,6-diol, polycarbonate diols based on hexane-1,6-diol, and mixtures of two or more of these polycarbonate diols are used. Suitable polycarbonate diols have an average molecular weight Mn in the range of, for example, 800 to 1200 g / mol.
[0025] It has been found that the use of polycarbonate diols provides compositions suitable for these applications with good hydrolytic stability and good aging resistance. For example, the compositions of the present invention have high hydrolytic resistance and good aging resistance as well as good low-temperature properties when polycarbonate diols are used as polyols.
[0026] However, in the present invention, the polymer composition may comprise, in addition to the polyol (P1), one or more chain extenders (KV1) and optionally (KV2), and further isocyanate-reactive compounds. For example, the polyol composition may comprise a further polyol having an average molecular weight Mn in the range of 800 to 1200 g / mol.
[0027] According to the invention, it is also possible to use mixtures of different chain extenders. The chain extenders (KV1) and (KV2) used may be generally known aliphatic, araliphatic, aromatic and / or cycloaliphatic compounds, preferably bifunctional compounds, with a molecular weight, preferably an average molecular weight of 50 g / mol to 499 g / mol. Preference is given to, for example, alkanediols having 2 to 10 carbon atoms in the alkylene group, preferably butane-1,4-diol, hexane-1,6-diol, and / or di-, tri-, tetra-, penta-, hexa-, hepta-, octa-, nona- and / or decaalkylene glycols having 3 to 8 carbon atoms, more preferably unbranched alkanediols, in particular propane-1,3-diol, butane-1,4-diol and hexane-1,6-diol.
[0028] In a further embodiment, the present invention thus also relates to a composition as described above, wherein the chain extender (KV1) and / or the chain extender (KV2) is selected from the group consisting of ethane-1,2-diol, propane-1,3-diol, butane-1,4-diol and hexane-1,6-diol, diethylene glycol, triethylene glycol, hydroquinone bis(2-hydroxyethyl) ether and bis(2-hydroxyethyl) terephthalate.
[0029] The chain extender (KV1) according to the invention is more preferably selected from the group consisting of ethane-1,2-diol, propane-1,3-diol, butane-1,4-diol and hexane-1,6-diol. In a further embodiment, the invention thus also relates to the above composition, in which the chain extender (KV1) is butane-1,4-diol.
[0030] According to the present invention, it is also possible to use additional chain extenders in the polyol composition.
[0031] According to the invention, it is also possible to use polyhydric alcohols, such as propanediol and / or further diols, which are obtained, for example, at least in part, from renewable raw materials. Here, it is possible that the polyhydric alcohols are obtained in part or in full from renewable raw materials. According to the invention, at least one of the polyhydric alcohols used may be obtained, at least in part, from renewable raw materials.
[0032] What is called bio-propane-1,3-diol can be obtained, for example, from corn and / or sugar. A further option is the conversion of glycerol waste resulting from biodiesel production. In a further preferred embodiment of the invention, the polyhydric alcohol is propane-1,3-diol obtained at least in part from renewable raw materials.
[0033] In a further embodiment, the present invention thus relates to a composition as described above, wherein the thermoplastic polyurethane is based on renewable raw materials to an extent of at least 30%. One suitable determination method is, for example, the C14 method.
[0034] In principle, the organic isocyanates customarily used are suitable for the present invention. The organic isocyanates used are aliphatic, cycloaliphatic, araliphatic and / or aromatic isocyanates, more preferably tri-, tetra-, penta-, hexa-, hepta- and / or octamethylene diisocyanate, 2-methylpentamethylene 1,5-diisocyanate, 2-ethylbutylene 1,4-diisocyanate, pentamethylene 1,5-diisocyanate, butylene 1,4-diisocyanate, 1-isocyanato-3,3,5-trimethyl-5-isocyanatomethylcyclohexane (isophorone diisocyanate, IPDI), 1,4- and / or 1,3-bis(isocyanatomethyl)cyclohexane. Hexane (HXDI), cyclohexane 1,4-diisocyanate, 1-methylcyclohexane 2,4- and / or 2,6-diisocyanate and / or dicyclohexylmethane 4,4'-, 2,4'- and 2,2'-diisocyanate, diphenylmethane 2,2'-, 2,4'- and / or 4,4'-diisocyanate (MDI), naphthylene 1,5-diisocyanate (NDI), tolylene 2,4- and / or 2,6-diisocyanate (TDI), dimethyldiphenyl 3,3'-diisocyanate, 1,2-diphenylethane diisocyanate and / or phenylene diisocyanate. Particularly preferably, only 4,4'-MDI is used.
[0035] Thus, in a further embodiment, the present invention also relates to a composition as described above, in which the thermoplastic polyurethane (TPU-1) is based on an aromatic diisocyanate.
[0036] In an alternative embodiment, the present invention also relates to the above composition, wherein in a further embodiment, the thermoplastic polyurethane (TPU-1) is based on an aliphatic diisocyanate.
[0037] In a further embodiment, the present invention thus relates to a composition as described above, wherein the thermoplastic polyurethane is based on diphenylmethane 4,4'-diisocyanate.
[0038] Further suitable aliphatic isocyanates are, for example, hexamethylene diisocyanate (HDI) or 1-isocyanato-4-[(4-isocyanatocyclohexyl)methyl]cyclohexane (H12MDI).
[0039] According to the invention, particularly preferred isocyanates are hexamethylene diisocyanate (HDI), diphenylmethane 2,2'-, 2,4'- and / or 4,4'-diisocyanate (MDI) and tolylene 2,4- and / or 2,6-diisocyanate (TDI) or 1-isocyanato-4-[(4-isocyanatocyclohexyl)methyl]cyclohexane (H12MDI), particularly preferred are diphenylmethane 2,2'-, 2,4'- and / or 4,4'-diisocyanate (MDI), in particular diphenylmethane 4,4'-diisocyanate.
[0040] The thermoplastic polyurethane (TPU-1) may be prepared using, in addition to the isocyanate composition and the polyol composition, further components, such as suitable catalysts or coagents.
[0041] In a preferred embodiment, the catalysts which promote the reaction, in particular between the NCO groups of the diisocyanate and the hydroxyl groups of the isocyanate-reactive compound and the chain extender, are tertiary amines, in particular triethylamine, dimethylcyclohexylamine, N-methylmorpholine, N,N'-dimethylpiperazine, 2-(dimethylaminoethoxy)ethanol, diazabicyclo[2.2.2]octane, in another preferred embodiment they are organometallic compounds, for example titanate esters, iron compounds, preferably iron(III) acetylacetonate, tin compounds, preferably tin diacetate, tin dioctoate, tin dilaurate, or dialkyltin salts of aliphatic carboxylic acids, preferably dibutyltin diacetate, dibutyltin dilaurate, or bismuth salts, in which bismuth is preferably in the oxidation state 2 or 3, in particular 3. Salts of carboxylic acids are preferred. The carboxylic acids used are preferably carboxylic acids having from 6 to 14 carbon atoms, more preferably having from 8 to 12 carbon atoms. Examples of suitable bismuth salts are bismuth(III) neodecanoate, bismuth 2-ethylhexanoate and bismuth octanoate.
[0042] The catalyst is preferably used in an amount of 0.0001 to 0.1 parts by weight per 100 parts by weight of the isocyanate-reactive compound. It is preferred to use a tin catalyst, in particular tin dioctoate.
[0043] In addition to the catalyst, it is also possible to add conventional auxiliaries.For example, surface-active substances, fillers, additional flame retardants, nucleating agents, oxidation stabilizers, lubricants and demolding auxiliaries, dyes and pigments, and optionally, for example, stabilizers against hydrolysis, light, heat or discoloration, inorganic and / or organic fillers, reinforcing agents and plasticizers.Suitable auxiliaries and additives can be found, for example, in Kunststoffhandbuch, Volume VII, Vieweg and Hoechtlen (eds.), Carl Hanser Verlag, Munich, 1966 (pages 103-113).
[0044] Suitable processes for the preparation of thermoplastic polyurethanes are disclosed, for example, in EP 0922552 A1, DE 10103424 A1 or WO 2006 / 072461 A1. The preparation is typically carried out in a belt apparatus or a reactive extruder, but can also be carried out on a laboratory scale, for example by manual casting. Depending on the physical properties of the components, these are all mixed directly with each other, or the individual components are premixed and / or prereacted, for example to form a prepolymer, and only then are subjected to polyaddition. In a further embodiment, the thermoplastic polyurethane is first prepared from the building block components, optionally together with a catalyst, which may optionally incorporate auxiliaries. In this case, at least one filler is introduced into this material and homogeneously dispersed. The homogeneous dispersion is preferably carried out in an extruder, preferably a twin-screw extruder. According to the invention, it is preferable to add the filler in portions, for example in a portion at the extruder intake and in a further portion at a second input site, for example a side feeder. The hardness of the TPU can be set within a relatively wide molar ratio by varying the amounts of forming components used, with hardness typically increasing as chain extender content is increased.
[0045] According to the invention, the mixing ratio of the components used in the preparation of the thermoplastic polyurethane may vary within a wide range. For example, the chain extender and polyol used may be used in a molar mixing ratio ranging from 20:1 to 1:1, preferably from 18:1 to 2:1, more preferably from 17:1 to 3:1, and even more preferably from 15:1 to 4:1.
[0046] When a mixture of different chain extenders is used, the mixing ratio of the chain extenders used may vary within wide limits. For example, the chain extenders may be used in a molar mixing ratio KV1:KV2 in the range of 20:1 to 3:1, preferably in the range of 15:1 to 4:1, even more preferably in the range of 17:1 to 3:1, even more preferably in the range of 15:1 to 4:1.
[0047] The thermoplastic polyurethanes used according to the present invention preferably have a hardness, determined according to DIN ISO 7619-1 (Shore A hardness test (3s)), in the range of 70A to 90D, preferably in the range of 80A to 95A, determined according to DIN ISO 7619-1, more preferably in the range of 80A to 90A, determined according to DIN ISO 7619-1, and particularly preferably in the range of 85A to 90A, determined according to DIN ISO 7619-1.
[0048] In a further embodiment, the present invention thus also relates to a composition as described above, wherein the thermoplastic polyurethane (TPU-1) has a Shore hardness, determined according to DIN 53505, in the range of 70A to 90D.
[0049] For the preparation of the thermoplastic polyurethanes of the invention, the formers are preferably reacted in the presence of a catalyst and, optionally, auxiliaries and / or additives, in amounts such that the equivalent ratio of the NCO groups of the diisocyanate to the total sum of the hydroxyl groups of the further formers is 0.9 to 1.1:1, preferably 0.95 to 1.05:1, and in particular about 0.95 to 1.00:1.
[0050] According to the present invention, there is provided a thermoplastic polyurethane having an average molecular weight (M W It is preferable to use a thermoplastic polyurethane having an average molecular weight (M W The upper limit of the average molecular weight (M) is generally determined by processability and the desired property spectrum. More preferably, the thermoplastic polyurethane has an average molecular weight (M) in the range of 50,000 to 250,000 Da, particularly preferably in the range of 50,000 to 150,000 Da. W ).
[0051] According to the invention, it is also possible for the composition to comprise two or more thermoplastic polyurethanes, which differ, for example, in their average molecular weight or in their chemical composition. For example, the composition of the invention may comprise a first thermoplastic polyurethane TPU-1 and a second thermoplastic polyurethane TPU-2, for example a thermoplastic polyurethane TPU-1 based on an aliphatic diisocyanate and a further TPU-2 based on an aromatic diisocyanate.
[0052] Here, TPU-1 is prepared with an aliphatic isocyanate and TPU-2 with an aromatic isocyanate.
[0053] The organic isocyanate used in the preparation of TPU-1 is preferably an aliphatic or cycloaliphatic isocyanate, more preferably tri-, tetra-, penta-, hexa-, hepta- and / or octamethylene diisocyanate, 2-methylpentamethylene 1,5-diisocyanate, 2-ethylbutylene 1,4-diisocyanate, pentamethylene 1,5-diisocyanate, butylene 1,4-diisocyanate, 1-isocyanato 3,3,5-trimethyl-5-isocyanatomethylcyclohexane (isophorone diisocyanate, IPDI), 1,4- and / or 1,3-bis(isocyanatomethyl)cyclohexane (HXDI), cyclohexane 1,4-diisocyanate, 1-methylcyclohexane 2,4- and / or 2,6-diisocyanate, and / or dicyclohexylmethane 4,4'-, 2,4'- and 2,2'-diisocyanate.
[0054] In a further embodiment, the present invention therefore relates to a composition as described above, wherein the thermoplastic polyurethane TPU-1 is based on at least one aliphatic diisocyanate selected from the group consisting of hexamethylene diisocyanate and di(isocyanatocyclohexyl)methane.
[0055] The organic isocyanates (a) used in the preparation of TPU-2 are preferably araliphatic and / or aromatic isocyanates, more preferably diphenylmethane 2,2'-, 2,4'- and / or 4,4'-diisocyanate (MDI), naphthylene 1,5-diisocyanate (NDI), tolylene 2,4- and / or 2,6-diisocyanate (TDI), dimethyldiphenyl 3,3'-diisocyanate, 1,2-diphenylethane diisocyanate, and / or phenylene diisocyanate. It is particularly preferred to use 4,4'-MDI.
[0056] Therefore, in a further embodiment, the present invention relates to a composition as described above, wherein the thermoplastic polyurethane TPU-2 is based on diphenylmethane diisocyanate (MDI).
[0057] The isocyanate-reactive compound preferably used for TPU-1 and TPU-2 is polycarbonate diol or polytetrahydrofuran polyol. Suitable polytetrahydrofuran polyol has a molecular weight in the range of, for example, 500 to 5,000, preferably 500 to 2,000, more preferably 800 to 1,200.
[0058] According to the present invention, TPU-1 and TPU-2 are preferably prepared with at least one polycarbonate diol, preferably an aliphatic polycarbonate diol. Examples of suitable polycarbonate diols include polycarbonate diols based on alkanediols. Suitable polycarbonate diols are strictly difunctional OH-functional polycarbonate diols, preferably strictly difunctional OH-functional aliphatic polycarbonate diols. Suitable polycarbonate diols are, for example, based on butanediol, pentanediol or hexanediol, in particular butane-1,4-diol, pentane-1,5-diol, hexane-1,6-diol, 3-methylpentane-1,5-diol or mixtures thereof, more preferably butane-1,4-diol, pentane-1,5-diol, hexane-1,6-diol or mixtures thereof. In the present invention, it is preferable to use polycarbonate diols based on butanediol and hexanediol, polycarbonate diols based on pentanediol and hexanediol, polycarbonate diols based on hexanediol, and mixtures of two or more of these polycarbonate diols.
[0059] The polycarbonate diol used in preparing TPU-1 and TPU-2 preferably has a number average molecular weight Mn in the range of 500 to 4000 as determined by GPC, preferably in the range of 650 to 3500 as determined by GPC, and more preferably in the range of 800 to 3000 as determined by GPC.
[0060] Chain extenders which may be used for the preparation of TPU-1 and TPU-2 preferably comprise aliphatic, araliphatic, aromatic and / or cycloaliphatic compounds having a molecular weight of 0.05 kg / mol to 0.499 kg / mol, preferably difunctional compounds, such as diamines and / or alkanediols having 2 to 10 carbon atoms in the alkylene group, di-, tri-, tetra-, penta-, hexa-, hepta-, octa-, nona- and / or decaalkylene glycols having 3 to 8 carbon atoms, in particular 1,2-ethylene glycol, propane-1,3-diol, butane-1,4-diol, hexane-1,6-diol, preferably the corresponding oligo- and / or polypropylene glycols, and it is also possible to use mixtures of chain extenders. Compound (c) preferably has only primary hydroxyl groups, and very particular preference is given to using a mixture of butane-1,4-diol and a further chain extender selected from the abovementioned compounds, for example a mixture comprising butane-1,4-diol and a second chain extender in a molar ratio in the range from 100:1 to 1:1, preferably in the range from 95:1 to 5:1 and more preferably in the range from 90:1 to 10:1.
[0061] Therefore, in a further embodiment, the present invention relates to a composition as described above, wherein the thermoplastic polyurethane is prepared using, as chain extender, a mixture of butane-1,4-diol and a further chain extender.
[0062] According to the present invention, TPU-1 preferably has a hardness in the range of 85A to 70D, determined according to DIN ISO 7619-1, preferably in the range of 95A to 70D, determined according to DIN ISO 7619-1, more preferably in the range of 55D to 65D, determined according to DIN ISO 7619-1.
[0063] According to the present invention, TPU-2 preferably has a hardness in the range of 70A to 70D, determined according to DIN ISO 7619-1, more preferably in the range of 80A to 60D, determined according to DIN ISO 7619-1, more preferably in the range of 80A to 90A, determined according to DIN ISO 7619-1.
[0064] In a further embodiment, the present invention therefore relates to a composition as described above, in which the thermoplastic polyurethane TPU-1 has a Shore hardness, determined according to DIN ISO 7619-1, in the range from 85A to 65D. In a further embodiment, the present invention therefore relates to a composition as described above, in which the thermoplastic polyurethane TPU-2 has a Shore hardness, determined according to DIN ISO 7619-1, in the range from 70A to 65D.
[0065] TPU-1 preferably has a molecular weight above 100,000 Da and TPU-2 preferably has a molecular weight in the range of 150,000 to 300,000 Da. The upper limit of the number average molecular weight of the thermoplastic polyurethanes is generally determined by processability and the spectrum of desired properties.
[0066] In a further embodiment, the present invention therefore relates to a composition as described above, in which the thermoplastic polyurethane TPU-1 has a molecular weight in the range of 100000 Da to 400000 Da.In a further embodiment, the present invention therefore relates to a composition as described above, in which the thermoplastic polyurethane TPU-2 has a molecular weight in the range of 150000 Da to 300000 Da.
[0067] The composition of the present invention comprises, for example, at least one thermoplastic polyurethane TPU-1 and at least one thermoplastic polyurethane TPU-2 in a total combined amount in the range from 5% to 95% by weight, based on the total composition, in particular in the range from 20% to 80% by weight, preferably in the range from 25% to 75% by weight and more preferably in the range from 30% to 70% by weight, based on the total composition, in each case based on the total sum of components (I) and (II).
[0068] Thermoplastic polyurethanes may be prepared batchwise or continuously by known methods, for example using a reactive extruder or belt process, by the "one-shot" process or the prepolymer process, preferably by the "one-shot" process. In these processes, the components to be reacted may be mixed with each other successively or simultaneously, and the reaction begins immediately. In the extruder process, the forming components are introduced individually or as a mixture into an extruder and reacted, for example, preferably at a temperature of 100°C to 280°C, more preferably 140°C to 250°C, and then the resulting polyurethane is extruded, cooled and pelletized.
[0069] The composition of the present invention comprises at least one thermoplastic polyurethane (TPU1) in an amount in the range from 5% to 95% by weight, based on the entire composition, in particular in the range from 20% to 80% by weight, preferably in the range from 25% to 75% by weight, based on the entire composition, in each case based on the total sum of components (I) and (II).
[0070] Thus, in a further embodiment, the present invention also relates to a composition as described above, in which the proportion of thermoplastic polyurethane (TPU-1) in the composition ranges from 5% by weight to 95% by weight, based on the total weight of components (I) and (II).
[0071] The sum of components (I) and (II) here in each case adds up to 100% by weight.
[0072] Furthermore, the composition (Z-1) of the invention comprises at least one copolyamide (PA-1), the proportion of which in the composition may vary within wide limits, for example in the range from 5% to 95% by weight, based on the entire composition, in particular in the range from 20% to 80% by weight, preferably in the range from 25% to 75% by weight, based on the entire composition, in each case based on the total sum of components (I) and (II).
[0073] Thus, in a further embodiment, the present invention also relates to a composition as described above, in which the proportion of copolyamide (PA-1) in the composition ranges from 5% by weight to 95% by weight, based on the total sum of components (I) and (II).
[0074] In the context of the present invention, "at least one copolyamide" is understood to mean either exactly one copolyamide or a mixture of two or more copolyamides.
[0075] According to the present invention, the copolyamide (PA-1) can be obtained by polymerizing component (A), at least one lactam, and component (B), which is a monomer mixture (M) comprising component (B1), at least one C32-C40 dimer acid, and component (B2), at least one C4-C12 diamine.
[0076] According to the invention, the ratio of components (A) and (B) used may vary within wide limits. Suitable copolyamides are described, for example, in WO 2018 / 050487 A1. The copolyamide (PA-1) preferably comprises the following components: (A) 15% to 84% by weight of at least one lactam; (B) 16% by mass to 85% by mass of a monomer mixture (M) containing the following components: (B1) at least one C32-C40 dimer acid, and (B2) At least one C4-C12 diamine and The weight percent of components (A) and (B) is based on the total weight percent of components (A) and (B), respectively.
[0077] In the present invention, the terms "component (A)" and "at least one lactam" are used synonymously and therefore have the same meaning.
[0078] The same applies to the terms "component (B)" and "monomer mixture (M)", which terms are likewise used synonymously in the present invention and therefore have the same meaning.
[0079] In the present invention, "at least one lactam" means either exactly one lactam or a mixture of two or more lactams. Exactly one lactam is preferred.
[0080] According to the invention, at least one copolyamide is preferably prepared by polymerizing 15% to 84% by weight of component (A) and 16% to 85% by weight of component (B), the copolyamide is preferably prepared by polymerizing 40% to 83% by weight of component (A) and 17% to 60% by weight of component (B), and the at least one copolyamide is particularly preferably prepared by polymerizing 60% to 80% by weight of component (A) and 20% to 40% by weight of component (B), where the weight percentages of components (A) and (B), respectively, are based on the total weight percentages of components (A) and (B).
[0081] Preferably, the total weight percent of components (A) and (B) add up to 100 weight percent.
[0082] In the present invention, the weight percentages of components (A) and (B) are based on the weight percentages of components (A) and (B) before polymerization, i.e., when components (A) and (B) have not yet reacted with each other. During the polymerization, the weight ratio of components (A) and (B) may be varied, if appropriate.
[0083] According to the invention, the copolyamide is prepared by polymerizing components (A) and (B). The polymerization of components (A) and (B) is known per se to the person skilled in the art. Typically, the polymerization of components (A) and (B) is a condensation reaction. During the condensation reaction, component (A) reacts with components (B1) and (B2) present in component (B) and, if appropriate, with component (B3), which may also be present in component (B), as described further below. This results in the formation of amide bonds between the individual components. Typically, component (A) is at least partially in open-chain form during the polymerization, i.e. as an amino acid.
[0084] The polymerization of components (A) and (B) can be carried out in the presence of a catalyst. Suitable catalysts are any catalysts known to those skilled in the art that catalyze the polymerization of components (A) and (B). Such catalysts are known to those skilled in the art. Preferred catalysts are phosphorus compounds, such as sodium hypophosphite, phosphorous acid, triphenylphosphine or triphenylphosphite.
[0085] The polymerization of components (A) and (B) forms a copolyamide, thus resulting in structural units derived from component (A) and structural units derived from component (B). The structural units derived from component (B) include structural units derived from components (B1) and (B2) and, optionally, structural units derived from component (B3).
[0086] The polymerization of components (A) and (B) forms the copolyamide as a copolymer, which may be a random copolymer, but also a block copolymer.
[0087] In a block copolymer, a block of units derived from component (B) and a block of units derived from component (A) are formed. These alternate. In a random copolymer, structural units derived from component (A) and structural units derived from component (B) alternate. This alternates randomly, for example, two structural units derived from component (B) are followed by one structural unit derived from component (A), which is then followed by one structural unit derived from component (B), which is then followed by a structural unit consisting of three structural units derived from component (A).
[0088] The at least one copolyamide (PA-1) is preferably a random copolymer.
[0089] The present invention therefore also provides a polymer film, wherein at least one copolyamide is a random copolymer.
[0090] The preparation of at least one copolyamide preferably comprises the following steps: a) polymerizing components (A) and (B) to obtain at least one first copolyamide; b) pelletizing the at least one first copolyamide obtained in step a) to obtain at least one pelletized copolyamide; c) extracting the at least one pelletized copolyamide obtained in step b) with water to obtain at least one extracted copolyamide; d) drying the at least one extracted copolyamide obtained in step c) at a temperature (Tr) to obtain at least one copolyamide.
[0091] Suitable reaction conditions are described, for example, in WO2018 / 050487A1.
[0092] The polymerization in step a) may be carried out in any reactor known to those skilled in the art. Stirred tank reactors are preferred. It is also possible to use auxiliaries known to those skilled in the art to improve reaction management, for example antifoaming agents such as polydimethylsiloxane (PDMS).
[0093] In step b), the at least one first copolyamide obtained in step a) may be pelletized by any method known to the person skilled in the art, such as strand pelletizing or underwater pelletizing.
[0094] The extraction in step c) may be carried out by any method known to the person skilled in the art.
[0095] During the extraction in step c), by-products formed during the polymerization of components (A) and (B) in step a) are typically extracted from the at least one pelletized copolyamide.
[0096] In step d), the at least one extracted copolyamide obtained in step c) is dried. Methods for drying are known to the person skilled in the art. According to the invention, the at least one extracted copolyamide is dried at a temperature (Tr), which is preferably less than the glass transition temperature (TG C ) and the melting temperature (TM C ) or less.
[0097] Drying in step d) is typically carried out for a period in the range of from 1 to 100 hours, preferably in the range of from 2 to 50 hours and particularly preferably in the range of from 3 to 40 hours.
[0098] The at least one copolyamide typically has a glass transition temperature (TG C ) Glass transition temperature (TG C ) is, for example, in the range of 20 to 50°C, preferably in the range of 23 to 47°C, and particularly preferably in the range of 25 to 45°C, as determined in accordance with ISO11357-2:2014.
[0099] Component (A) according to the invention is at least one lactam. Lactams are known per se to those skilled in the art. According to the invention, lactams having 4 to 12 carbon atoms are preferred.
[0100] In the present invention, "lactam" is understood to mean a cyclic amide having preferably 4 to 12 carbon atoms in the ring, more preferably 5 to 8 carbon atoms. Suitable lactams are, for example, 3-aminopropanolactam (propio-3-lactam; β-lactam; β-propiolactam), 4-aminobutanolactam (butyro-4-lactam; γ-lactam; γ-butyrolactam), 5-aminopentanolactam (2-piperidinone; δ-lactam; δ-valerolactam), 6-aminohexanolactam (hexano-6-lactam; ε-lactam; ε-caprolactam), 7-aminoheptanolactam (heptano-7-lactam; ζ-lactam; ζ-heptanolactam). lactam), 8-aminooctanolactam (octano-8-lactam; eta-lactam; eta-octanolactam), 9-aminononanolactam (nonano-9-lactam; θ-lactam; θ-nonanolactam), 10-aminodecanolactam (decano-10-lactam; ω-decanolactam), 11-aminoundecanolactam (undecano-11-lactam; ω-undecanolactam) and 12-aminododecanolactam (dodecano-12-lactam; ω-dodecanolactam).
[0101] According to the invention, the lactam is unsubstituted or at least monosubstituted. If an at least monosubstituted lactam is used, its nitrogen atom and / or ring carbon atoms may bear one, two or more substituents independently selected from the group consisting of C5- to C10-alkyl, C5- to C6-cycloalkyl and C5- to C10-aryl.
[0102] Suitable C5- to C10-alkyl substituents are, for example, methyl, ethyl, propyl, isopropyl, n-butyl, sec-butyl and tert-butyl. Suitable C5- to C6-cycloalkyl substituents are, for example, cyclohexyl. Preferred C5- to C10-aryl substituents are phenyl and anthranyl.
[0103] It is preferred to use unsubstituted lactams, with γ-lactam (γ-butyrolactam), δ-lactam (δ-valerolactam) and ε-lactam (ε-caprolactam) being preferred, δ-lactam (δ-valerolactam) and ε-lactam (ε-caprolactam) being particularly preferred, with ε-caprolactam being especially preferred.
[0104] According to the present invention, component (B) is a monomer mixture (M). The monomer mixture (M) comprises components (B1), at least one C32-C40 dimer acid, and (B2), at least one C4-C12 diamine.
[0105] In the context of the present invention, monomer mixture (M) is understood to mean a mixture of two or more monomers, at least components (B1) and (B2) being present in the monomer mixture (M).
[0106] In the present invention, the terms "component (B1)" and "at least one C32-C40 dimer acid" are used synonymously and therefore have the same meaning. The same applies to the terms "component (B2)" and "at least one C4-C12 diamine".
[0107] These terms are also used synonymously in the present invention and therefore have the same meaning.
[0108] The monomer mixture (M) comprises, for example, from 45 to 55 mol % of component (B1) and from 45 to 55 mol % of component (B2), in each case based on the total sum of the molar percentages of components (B1) and (B2), preferably based on the total molar amount of component (B).
[0109] Preferably, component (B) comprises in the range of 47 to 53 mol % of component (B1), and in the range of 47 to 53 mol % of component (B2), in each case based on the total sum of the molar percentages of components (B1) and (B2), preferably based on the total molar amount of component (B).
[0110] More preferably, component (B) comprises in the range of 49 to 51 mol % of component (B1), and in the range of 49 to 51 mol % of component (B2), in each case based on the total sum of the molar percentages of components (B1) and (B2), preferably based on the total molar amount of component (B).
[0111] The total mole percentages of components (B1) and (B2) present in component (B) typically add up to 100 mole %.
[0112] Component (B) may further comprise at least one C4-C20 diacid, which is component (B3). In the present invention, the terms "component (B3)" and "at least one C4-C20 diacid" are used synonymously and therefore have the same meaning.
[0113] When component (B) further comprises component (B3), component (B) preferably comprises 25 to 54.9 mol % of component (B1), 45 to 55 mol % of component (B2), and 0.1 to 25 mol % of component (B3), in each case based on the total molar amount of component (B).
[0114] More preferably, component (B) in this case comprises in the range of 13 to 52.9 mol % of component (B1), in the range of 47 to 53 mol % of component (B2), and in the range of 0.1 to 13 mol % of component (B3), in each case based on the total molar amount of component (B).
[0115] More preferably, component (B) in this case comprises in the range of 7 to 50.9 mol % of component (B1), in the range of 49 to 51 mol % of component (B2), and in the range of 0.1 to 7 mol % of component (B3), in each case based on the total molar amount of component (B).
[0116] When component (B) further comprises component (B3), the mole percentages of components (B1), (B2) and (B3) typically add up to 100 mole %.
[0117] The monomer mixture (M) may further comprise water.
[0118] Components (B1), (B2) and optional (B3) of component (B) can be reacted with each other to obtain amides. This reaction is known per se to those skilled in the art. Thus, component (B) may contain components (B1), (B2) and optional (B3) in fully reacted form, partially reacted form or unreacted form. Preferably, component (B) contains components (B1), (B2) and optional (B3) in unreacted form.
[0119] Thus, in the present invention, "in unreacted form" means that component (B1) is present as at least one C32-C40 dimer acid, component (B2) as at least one C4-C12 diamine, and component (B3), if present, as at least one C4-C20 diacid.
[0120] If components (B1), (B2) and, optionally, (B3) present have at least partially reacted with one another, then components (B1), (B2) and, optionally, (B3) present are at least partially in the form of amides.
[0121] According to the present invention, component (B1) is at least one C32-C40 dimer acid. In the present invention, "at least one C32-C40 dimer acid" means exactly one C32-C40 dimer acid or a mixture of two or more C32-C40 dimer acids.
[0122] Dimer acids are also called dimer fatty acids. C32-C40 dimer acids are known per se to those skilled in the art and are typically prepared by dimerizing unsaturated fatty acids. This dimerization may be catalyzed, for example, by alumina. Unsaturated fatty acids suitable for preparing at least one C32-C40 dimer acid are known to those skilled in the art and are, for example, unsaturated C16 fatty acids, unsaturated C16 fatty acids and unsaturated C20 fatty acids.
[0123] Component (B1) is therefore preferably prepared proceeding from unsaturated fatty acids selected from the group consisting of unsaturated C16 fatty acids, unsaturated C18 fatty acids and unsaturated C20 fatty acids, with unsaturated C18 fatty acids being particularly preferred. An example of a suitable unsaturated C16-fatty acid is palmitoleic acid ((9Z)-hexadec-9-enoic acid).
[0124] Suitable unsaturated C18 fatty acids are, for example, petroselinic acid ((6Z)-octadec-6-enoic acid), oleic acid ((9Z)-octadec-9-enoic acid), elaidic acid ((9E)-octadec-9-enoic acid), vaccenic acid ((11E)-octadec-11-enoic acid), linoleic acid ((9Z,12Z)-octadeca-9,12-dienoic acid), alpha-linoleic acid ((11E)-octadec-11-eno ... linolenic acid ((9Z,12Z,15Z)-octadeca-9,12,15-trienoic acid), gamma-linolenic acid ((6Z,9Z,12Z)-octadeca-6,9,12-trienoic acid), calendula acid ((8E,10E,12Z)-octadeca-8,10,12-trienoic acid), punicic acid ((9Z,11E,13Z)-octadeca-9,11,13-trienoic acid), The unsaturated cis-fatty acids are selected from the group consisting of alpha-eleostearic acid ((9Z,11E,13E)-octadeca-9,11,13-trienoic acid) and beta-eleostearic acid ((9E,11E,13E)-octadeca-9,11,13-trienoic acid). Particularly preferred are unsaturated cis-fatty acids selected from the group consisting of petroselinic acid ((6Z)-octadec-6-enoic acid), oleic acid ((9Z)-octadec-9-enoic acid), elaidic acid ((9E)-octadec-9-enoic acid), vaccenic acid ((11E)-octadec-11-enoic acid), and linoleic acid ((9Z,12Z)-octadeca-9,12-dienoic acid).
[0125] Suitable unsaturated C20 fatty acids are, for example, selected from the group consisting of gadoleic acid ((9Z)-eicosa-9-enoic acid), icosenoic acid ((11Z)-eicosa-11-enoic acid), arachidonic acid ((5Z,8Z,11Z,14Z)-eicosa-5,8,11,14-tetraenoic acid), and timnodonic acid ((5Z,8Z,11Z,14Z,17Z)-eicosa-5,8,11,14,17-pentaenoic acid).
[0126] Component (B1) is particularly preferably at least one C36 dimer acid.
[0127] At least one C36 dimer acid is preferably prepared from an unsaturated cis fatty acid. The C36 dimer acid is more preferably petroselinic acid ((6Z)-octadec-6-enoic acid), oleic acid ((9Z)-octadec-9-enoic acid), elaidic acid ((9E)-octadec-9-enoic acid), It is prepared proceeding from a cis fatty acid selected from the group consisting of vaccenic acid ((11E)-octadec-11-enoic acid) and linoleic acid ((9Z,12Z)-octadeca-9,12-dienoic acid).
[0128] Preparation of component (B1) from unsaturated fatty acids can further lead to the formation of trimer acid and may also leave residues of unreacted unsaturated fatty acids.
[0129] The formation of trimer acid is known to those skilled in the art.
[0130] Preferably, according to the invention, component (B1) comprises at most 0.5% by weight of unreacted unsaturated fatty acid and at most 0.5% by weight of trimer acid, more preferably at most 0.2% by weight of unreacted unsaturated fatty acid and at most 0.2% by weight of trimer acid, in each case based on the total weight of component (B1).
[0131] Thus, dimer acids (also known as dimerized fatty acids or dimer fatty acids) generally, and in particular in the present invention, refer to mixtures produced by oligomerization of unsaturated fatty acids. They can be prepared, for example, by catalytic dimerization of unsaturated fatty acids of vegetable origin, in particular using unsaturated C16- to C20-fatty acids as starting materials. The bond formation proceeds mainly by the Diels-Alder mechanism, resulting in a mixture of mainly dimer products with alicyclic, linear aliphatic, branched aliphatic and C6 aromatic hydrocarbon groups between the carboxyl groups, depending on the number and position of the double bonds in the fatty acids used to prepare the dimer acids. Depending on the mechanism and / or any subsequent hydrogenation, the aliphatic radicals may be saturated or unsaturated and the proportion of aromatic groups may also vary. And the radical between the carboxylic acid groups contains, for example, 32 to 40 carbon atoms. For the preparation, it is preferable to use fatty acids with 18 carbon atoms, so that the dimer product has 36 carbon atoms. The radicals linking the carboxyl groups of the dimer fatty acids preferably contain no unsaturated bonds or aromatic hydrocarbon radicals.
[0132] Therefore, according to the invention, it is preferred to use Cie fatty acids in the preparation, and it is particularly preferred to use linoleic acid, linoleic acid and / or oleic acid.
[0133] Depending on the reaction regime, the oligomerization results in a mixture containing mainly dimeric molecules, but also trimeric and monomeric molecules and other by-products. Purification by distillation is customary. Commercially available dimer acids generally contain at least 80% by weight of dimeric molecules, up to 19% by weight of trimeric molecules, and up to 1% by weight of monomeric molecules and other by-products.
[0134] It is preferred to use dimer acids which are composed to the extent of at least 90%, preferably to the extent of at least 95%, most preferably to the extent of at least 98% by weight of dimeric fatty acid molecules.
[0135] The proportions of monomeric, dimeric and trimeric molecules in the dimer acid, as well as the proportions of other by-products, may be determined, for example, by gas chromatography (GC). Prior to GC analysis, the dimer acid is converted to the corresponding methyl esters by the boron trifluoride method (see DIN EN ISO 5509) and then analyzed by GC.
[0136] Thus, in the present invention, the essential feature of "dimer acid" is that its preparation involves the oligomerization of unsaturated fatty acids. This oligomerization mainly forms dimer products, in other words, preferably to the extent of at least 80% by weight, more preferably to the extent of at least 90%, even more preferably to the extent of at least 95% by weight, and in particular to the extent of at least 98% by weight. Thus, the fact that the oligomerization mainly forms dimer products containing exactly two fatty acid molecules justifies this designation, which is in any case general. Thus, an alternative expression of the related term "dimer acid" is "mixtures containing dimerized fatty acids".
[0137] The dimer acids for use can be obtained commercially, for example Radiacid 0970, Radiacid 0971, Radiacid 0972, Radiacid 0975, Radiacid 0976 and Radiacid 0977 from Oleon, Pripol 1006, Pripol 1009, Pripol 1012 and Pripol 1013 from Croda, Empol 1008, Empol 1012, Empol 1061 and Empol 1062 from BASF SE, and Unidyme 10 and Unidyme Tl from Arizona Chemical.
[0138] The component (B1) has an acid value in the range of, for example, 190 to 200 mgKOH / g.
[0139] According to the invention, component (B2) is at least one C4-C12 diamine. In the present invention, "at least one C4-C12 diamine" means exactly one C4-C12 diamine or a mixture of two or more C4-C12 diamines. In the present compound, "C4-C12 diamine" is understood to mean an aliphatic and / or aromatic compound having 4 to 12 carbon atoms and two amino groups (-NH2 groups). The aliphatic and / or aromatic compounds may be unsubstituted or further at least monosubstituted. If the aliphatic and / or aromatic compounds are further at least monosubstituted, they may have one, two or more substituents that do not participate in the polymerization of components (A) and (B). Such substituents are, for example, alkyl or cycloalkyl substituents. These are known per se to the person skilled in the art. The at least one C4-C12 diamine is preferably unsubstituted.
[0140] Examples of suitable components (B2) are selected from the group consisting of 1,4-diaminobutane (butane-1,4-diamine; tetramethylenediamine; putrescine), 1,5-diaminopentane (pentamethylenediamine; pentane-1,5-diamine; cadaverine), 1,6-diaminohexane (hexamethylenediamine; hexane-1,6-diamine), 1-diaminoheptane, 1,8-diaminooctane, 1,9-diaminononane, 1,10-diaminodecane (decamethylenediamine), 1,11-diaminoundecane (undecamethylenediamine) and 1,12-diaminododecane (dodecamethylenediamine).
[0141] Preferably, component (B2) is selected from the group consisting of tetramethylenediamine, pentamethylenediamine, hexamethylenediamine, decamethylenediamine and dodecamethylenediamine.
[0142] According to the present invention, the optional component (B3) present in component (B) is at least one C4-C20 diacid. In the present invention, "at least one C4-C20 diacid" means either exactly one C4-C20 diacid or a mixture of two or more C4-C20 diacids.
[0143] In the present invention, "C4-C20 diacid" is understood to mean an aliphatic and / or aromatic compound having 2 to 18 carbon atoms and two carboxyl groups (-COOH groups). The aliphatic and / or aromatic compounds may be unsubstituted or further at least monosubstituted. If the aliphatic and / or aromatic compounds are further at least monosubstituted, they may have one, two or more substituents that do not participate in the polymerization of components (A) and (B). Such substituents are, for example, alkyl or cycloalkyl substituents. These are known to the person skilled in the art. The at least one C4-C20 diacid is preferably unsubstituted.
[0144] Suitable components (B3) are, for example, selected from the group consisting of butanedioic acid (succinic acid), pentanedioic acid (glutaric acid), hexanedioic acid (adipic acid), heptanedioic acid (pimelic acid), octanedioic acid (suberic acid), nonanedioic acid (azelaic acid), decanedioic acid (sebacic acid), undecanedioic acid, dodecanedioic acid, tridecanedioic acid, tetradecanedioic acid and hexadecanedioic acid.
[0145] Preferably, component (B3) is selected from the group consisting of pentanedioic acid (glutaric acid), hexanedioic acid (adipic acid), decanedioic acid (sebacic acid) and dodecanedioic acid.
[0146] According to the invention, composition (Z1) can be prepared, for example, by mixing the individual components, for example thermoplastic polyurethane (TPU1) and polyamide (PA1), in a suitable device, such as an extruder or kneader, where composition (Z1) can be prepared under conditions known per se.
[0147] According to the invention, it is also possible to use further additives, such as flame retardants or fillers. Suitable fillers, plasticizers or flame retardants are known per se to the person skilled in the art.
[0148] In a further embodiment, the present invention thus relates to composition (Z1) as defined above, wherein the composition comprises at least one flame retardant.
[0149] In a further embodiment, the present invention also relates to composition (Z1) as defined above, wherein the composition comprises at least one filler.
[0150] In the present invention, it is preferable to use a flame retardant selected from the group consisting of metal hydroxides, nitrogen-containing flame retardants, and phosphorus-containing flame retardants. According to the present invention, a flame retardant selected from the group consisting of melamine cyanurate, magnesium hydroxide, and phosphorus-containing flame retardants is preferred.
[0151] In a further embodiment, the present invention also relates to the above composition (Z1), wherein the flame retardant is selected from the group consisting of metal hydroxides, nitrogen-containing flame retardants and phosphorus-containing flame retardants.
[0152] In a further embodiment, the present invention further relates to the above composition, wherein the composition comprises at least one flame retardant selected from the group consisting of melamine cyanurate, magnesium hydroxide, and phosphorus-containing flame retardants.
[0153] In the present invention, for example, mixtures of different flame retardants are also suitable, for example mixtures comprising one or more phosphorus-containing flame retardants.
[0154] Thus, in a further embodiment, the present invention relates to a composition as described above, wherein the composition comprises at least one first phosphorus-containing flame retardant (F1) selected from the group consisting of derivatives of phosphoric acid and derivatives of phosphonic acid, and at least one further phosphorus-containing flame retardant (F2) selected from the group consisting of derivatives of phosphinic acid.
[0155] Suitable flame retardants are, for example, metal hydroxides. In the event of fire, metal hydroxides release only water, so they do not form any toxic or corrosive smoke gas products. Furthermore, these hydroxides can reduce the density of smoke gas in the event of fire. However, the disadvantage of these substances is that they sometimes promote the hydrolysis of thermoplastic polyurethane and also affect the oxidative aging of polyurethane.
[0156] The hydroxides suitable in the present invention are preferably magnesium, calcium, zinc and / or aluminum hydroxides, or mixtures thereof. More preferably, the metal hydroxide is selected from the group consisting of aluminum hydroxide, aluminum oxide hydroxide, magnesium hydroxide and mixtures of two or more of these hydroxides.
[0157] The composition of the present invention may comprise a phosphorus-containing flame retardant. According to the present invention, it is possible in principle to use any known phosphorus-containing flame retardant for thermoplastic polyurethanes.
[0158] In the present invention, it is preferred to use a derivative of phosphoric acid, a derivative of phosphonic acid or a derivative of phosphinic acid, or a mixture of two or more of these derivatives. In a further preferred embodiment, the phosphorus-containing flame retardant is liquid at 21°C.
[0159] Preferably, the derivatives of phosphoric, phosphonic or phosphinic acids are salts with organic or inorganic cations or organic esters. Organic esters are derivatives of phosphorus-containing acids in which at least one oxygen atom directly attached to phosphorus is esterified with an organic radical. In a preferred embodiment, the organic esters are alkyl esters, and in another preferred embodiment, aryl esters. More preferably, all hydroxyl groups of the corresponding phosphorus-containing acids are esterified.
[0160] Suitable organic phosphate esters are, for example, triesters of phosphoric acid, such as the trialkyl phosphates, and especially the triaryl phosphates, such as resorcinol bis(diphenyl phosphate).
[0161] Particularly preferred according to the invention are the salts of phosphoric, phosphonic or phosphinic acid derivatives, respectively, more preferably the phosphinate salts. Preferred examples in the present invention are melamine polyphosphate or diethylaluminum phosphinate.
[0162] Furthermore, it is also possible to use nitrogen-containing flame retardants in the present invention. In principle, it is possible to use all known nitrogen-containing flame retardants for thermoplastic polyurethanes according to the present invention.
[0163] Flame retardants suitable in the present invention are also melamine derivatives, such as, in particular, melamine polyphosphate or melamine cyanurate.
[0164] In the present invention, it is also possible that the composition comprises, in addition to the thermoplastic polyurethane, a mixture of various flame retardants, for example melamine derivatives and derivatives of phosphoric acid, or melamine derivatives and derivatives of phosphinic acid, or melamine derivatives and derivatives of phosphoric acid and derivatives of phosphinic acid.
[0165] The melamine derivative may preferably be melamine cyanurate. Thus, in a further embodiment, the present invention also relates to a composition comprising, in addition to a thermoplastic polyurethane, for example, melamine cyanurate and a derivative of phosphoric acid, or melamine cyanurate and a derivative of phosphinic acid, or melamine cyanurate and a derivative of phosphoric acid and a derivative of phosphinic acid. For example, the composition of the present invention comprises at least one thermoplastic polyurethane, at least melamine cyanurate, at least one first phosphorus-containing flame retardant (F1) selected from the group consisting of derivatives of phosphoric acid and derivatives of phosphonic acid, and at least one further phosphorus-containing flame retardant (F2) selected from the group consisting of derivatives of phosphinic acid.
[0166] Preferably, the composition does not comprise any further flame retardants apart from melamine cyanurate, the at least one phosphorus-containing flame retardant (F1) and the at least one phosphorus-containing flame retardant (F2).More preferably, the composition of the present invention comprises melamine cyanurate, exactly one phosphorus-containing flame retardant (F1) selected from the group consisting of derivatives of phosphoric acid and derivatives of phosphonic acid, and exactly one phosphorus-containing flame retardant (F2) selected from the group consisting of derivatives of phosphinic acid.
[0167] Thus, in a further embodiment, the present invention also relates to a composition as described above, in which the phosphorus-containing flame retardant (F1) is a phosphinate.
[0168] In a further embodiment, the present invention further relates to the above composition, wherein the phosphinate is selected from the group consisting of aluminum phosphinate or zinc phosphinate.
[0169] Furthermore, in a further embodiment, the present invention also relates to the above composition, wherein the phosphorus-containing flame retardant (F2) is a phosphoric acid ester.
[0170] In a further embodiment, the present invention also relates to the above composition, wherein the flame retardant (F1) is selected from the group consisting of resorcinol bis(diphenyl phosphate) (RDP), bisphenol A bis(diphenyl phosphate) (BDP) and diphenylcresyl phosphate (DPK).
[0171] The proportion of the flame retardant (F) in the composition is, for example, in the range of 2.5% by mass to 40% by mass based on the entire composition, preferably in the range of 5% by mass to 30% by mass based on the entire composition, and more preferably in the range of 10% by mass to 20% by mass based on the entire composition.
[0172] In a further embodiment, the present invention thus also relates to a composition as described above, wherein the flame retardant (F) is present in an amount ranging from 2.5% to 40% by weight, based on the total composition.
[0173] In one embodiment, for the preparation of the composition of the present invention, thermoplastic polyurethane and flame retardant are processed in one step.In another preferred embodiment, for the preparation of the composition of the present invention, a reactive extruder, a belt system or other suitable equipment is first used to prepare the thermoplastic polyurethane, preferably in pellet form, and then at least one additional flame retardant is introduced therein in at least one additional step or in two or more steps.
[0174] The mixing of the thermoplastic polyurethane with the at least one flame retardant is carried out, for example, in a mixing unit, which is preferably an internal kneader or an extruder, preferably a twin-screw extruder. In another preferred embodiment using an extruder, the flame retardant introduced is liquid at the temperature present downstream of the addition to the extruder in the flow direction.
[0175] The composition of the invention may further comprise a filler (FS1). According to the invention, the chemical nature and morphology of the filler (FS1) may vary within wide limits, provided that it is sufficiently compatible with the composition (Z1). The filler (FS1) should here be selected such that the morphology and particle size of the filler allow sufficient miscibility and homogeneous distribution in the composition.
[0176] Suitable fillers are, for example, glass fibers, glass beads, carbon fibers, aramid fibers, potassium titanate fibers, fibers of liquid crystal polymers, organic fibrous fillers or inorganic reinforcing materials. Organic fibrous fillers are, for example, cellulose fibers, hemp fibers, sisal or kenaf. Inorganic reinforcing materials are, for example, ceramic fillers, such as aluminum nitride and boron nitride, or mineral fillers, such as asbestos, talc, wollastonite, microbite, silicates, chalk, calcined kaolin, mica and quartz flour. Preferably, according to the present invention, the filler (F1) is selected from the group consisting of glass fibers, carbon fibers, aramid fibers, potassium titanate fibers, fibers of liquid crystal polymers, metal fibers, polyester fibers, polyamide fibers, organic fibrous fillers and inorganic fibrous fillers.
[0177] In a further embodiment, the present invention thus also relates to a composition as defined above, in which the filler (FS1) is selected from the group consisting of glass fibres, carbon fibres, aramid fibres, potassium titanate fibres, fibres of liquid crystal polymers, metal fibres, polyester fibres, polyamide fibres, organic fibrous fillers and inorganic fibrous fillers.
[0178] In the context of the present invention, fibrous fillers are preferred. In a further embodiment, the present invention thus also relates to a composition as described above, in which the filler (F1) is fibrous.
[0179] The dimensions of the fillers used may vary within customary limits. The fillers used preferably have a length in the range of 3 mm to 4 mm and a diameter in the range of 1 μm to 20 μm, in each case determined according to ASTM D578-98. In a further embodiment, the invention thus also relates to the above composition, in which the filler (FS1) has a length in the range of 3 mm to 4 mm and a diameter in the range of 1 μm to 20 μm, in each case determined according to ASTM D578-98.
[0180] Fillers, such as fibrous fillers, may be pretreated, for example with silane compounds, to improve compatibility with thermoplastics.
[0181] It is preferable to use an inorganic fibrous filler, since a greater reinforcing effect and higher heat resistance are observed when an inorganic fibrous filler is used.
[0182] According to the invention, the composition may contain two or more fillers.
[0183] The proportion of the filler (FS1) in the composition is, for example, in the range of 40% by mass to 60% by mass based on the entire composition, preferably in the range of 45% by mass to 55% by mass based on the entire composition, and more preferably in the range of 48% by mass to 52% by mass based on the entire composition.
[0184] In a further embodiment, the present invention thus also relates to a composition as described above, wherein the filler (FS1) is present in an amount ranging from 40% to 60% by weight, based on the total composition.
[0185] According to the invention, the composition may also contain further ingredients such as demolding aids, UV protection, antioxidants or colour pigments.
[0186] In a further aspect, the present invention also relates to a method for producing the composition (Z-1), comprising the following steps: (a) (I) Thermoplastic polyurethane (TPU-1), and (II) a copolyamide (PA-1) prepared by polymerizing at least one lactam with a monomer mixture (M) comprising components (B1) at least one C32-C40 dimer acid and (B2) at least one C4-C12 diamine; and (b) mixing components (I) and (II); The present invention relates to a method for producing the composition (Z-1), comprising:
[0187] This method of the present invention comprises at least steps (a) and (b). The method may comprise further steps, such as a drying step or temperature adjustment. According to the present invention, it is also possible to add further components, such as the above-mentioned auxiliaries and additives.
[0188] In a further aspect, the present invention thus relates to a method as described above, wherein the components used are dried, for example at a temperature in the range of 80-100° C. For example, drying can be carried out at a temperature in the range of 80-100° C. for 2-4 hours.
[0189] According to the invention, in step (b) the copolyamide (PA-1) and the thermoplastic polyurethane (TPU-1) are mixed. This can be carried out in equipment known per se to the skilled person, for example in an extruder. Suitable extruders and process conditions are known per se to the skilled person. For example, the mixing in the extruder can be carried out at a temperature in the range of 180-240°C, preferably at a temperature in the range of 190°C-230°C, more preferably at a temperature in the range of 200°C-225°C.
[0190] A suitable residence time in the extruder is, for example, in the range of 5 to 20 minutes, preferably 10 to 15 minutes.
[0191] Regarding the preferred embodiment, please see above details of the components preferably used.
[0192] Suitable methods for preparing the compositions are known per se to those skilled in the art. In the present invention, methods known per se are typically used for the formulation.
[0193] For example, the composition can be produced in an extruder in a manner known per se, for example in a twin-screw extruder. According to the invention, it is preferred to add the filler in portions, for example in a portion at the extruder intake and in a further portion at a second input site, for example a side feeder. The temperature here is preferably in the range of 160-230° C. In the present invention, the extruder can be operated, for example, at a speed in the range of 150-300 revolutions per minute.
[0194] The present invention further relates to compositions obtained or obtainable by the process of the present invention.
[0195] The present invention also relates to the use of the composition (Z1) according to the invention or of a composition obtained or obtainable by the process according to the invention, for the manufacture of shaped articles.
[0196] In a further aspect, the present invention further relates to a shaped article comprising the inventive composition according to the present invention or the composition obtained or obtainable by the inventive process.
[0197] The present invention also relates to the use of the inventive composition comprising at least one flame-retardant thermoplastic polyurethane as defined above for the manufacture of coatings, damping elements, bellows, films or fibers, molded articles, building and transport floors, random laid webs, preferably seals, rollers, shoe soles, hoses, cables, cable connectors, cable sheaths, cushions, laminates, profiles, belts, saddles, foams, plug connectors, trailing cables, solar cell modules, automotive trim. The use for the manufacture of cable sheaths is preferred. The manufacture is preferably carried out by injection molding, calendering, powder sintering or extrusion and / or additional foaming of the inventive composition from pellet material.
[0198] Due to the good mechanical and thermal properties, the thermoplastic polyurethanes according to the invention and the compositions according to the invention are particularly suitable for the production of films, moulded articles, wheels / rollers, fibres, automotive trim, hoses, cable plugs, bellows, trailing cables, cable sheaths, seals, belts or damping elements.
[0199] The present invention thus also provides a film, a moulded article, a wheel / roller, a fibre, an automotive trim, a hose, a cable plug, a bellows, a trailing cable, a cable sheath, a seal, a belt or a damping element comprising said thermoplastic polyurethane or said composition.
[0200] Further embodiments of the invention are found in the claims and examples.It will be understood that the features of the subject matter / method of the invention or the features of the use of the invention described above and elucidated below in this specification can be used not only in the combinations specified in each case but also in other combinations without departing from the scope of the invention.Thus, for example, combinations of preferred features with particularly preferred features, or of features not further characterized with particularly preferred features, etc. are implicitly included even if this combination is not explicitly mentioned.
[0201] Exemplary embodiments of the invention are detailed below, but are not intended to limit the invention, and in particular the invention also encompasses those embodiments resulting from the dependent references and combinations thereof specified below in this specification.
[0202] 1. At least the following: (I) Thermoplastic polyurethane (TPU-1), and (II) Hereinafter: (A) at least one lactam; (B) a monomer mixture (M) comprising the following components: (B1) at least one C32-C40 dimer acid, and (B2) At least one C4-C12 diamine Copolyamide (PA-1), prepared by polymerization with A composition comprising:
[0203] 2. The composition of embodiment 1, wherein the thermoplastic polyurethane (TPU-1) is based on an aromatic diisocyanate.
[0204] 3. The composition of embodiment 2, wherein the thermoplastic polyurethane (TPU-1) has a Shore hardness, determined according to DIN 53505, in the range of 70A to 85D.
[0205] 4. The composition of embodiment 1, wherein the thermoplastic polyurethane (TPU-1) is based on an aliphatic diisocyanate.
[0206] 5. The composition according to any one of the preceding claims, wherein the proportion of thermoplastic polyurethane (TPU-1) in the composition is in the range of 5% by weight to 95% by weight, based on the total sum of components (I) and (II).
[0207] 6. The composition according to any one of the preceding claims, wherein the proportion of copolyamide (PA-1) in the composition ranges from 5% by weight to 95% by weight, based on the total sum of components (I) and (II).
[0208] 7. The composition of any one of the preceding claims, wherein the composition comprises at least one flame retardant selected from the group consisting of melamine cyanurate, magnesium hydroxide, and phosphorus-containing flame retardants.
[0209] 8. The composition according to any one of the preceding claims, wherein the composition comprises at least one first phosphorus-containing flame retardant (F1) selected from the group consisting of derivatives of phosphoric acid and derivatives of phosphonic acid, and at least one further phosphorus-containing flame retardant (F2) selected from the group consisting of derivatives of phosphinic acid.
[0210] 9. The composition of embodiment 8, wherein the phosphorus-containing flame retardant (F1) is a phosphinate.
[0211] 10. The composition of embodiment 9, wherein the phosphinate is selected from the group consisting of aluminum phosphinate or zinc phosphinate.
[0212] 11. The composition of any one of embodiments 8 to 10, wherein the phosphorus-containing flame retardant (F2) is a phosphate ester.
[0213] 12. The composition according to any one of embodiments 8 to 11, wherein the flame retardant (F1) is selected from the group consisting of resorcinol bis(diphenyl phosphate) (RDP), bisphenol A bis(diphenyl phosphate) (BDP), and diphenylcresyl phosphate (DPK).
[0214] 13. The following steps: (a) (I) Thermoplastic polyurethane (TPU-1), and (II) a copolyamide (PA-1) prepared by polymerizing at least one lactam with a monomer mixture (M) comprising components (B1) at least one C32-C40 dimer acid and (B2) at least one C4-C12 diamine; and (b) mixing components (I) and (II); A method for producing the composition (Z-1), comprising:
[0215] 14. Use of a composition according to any one of embodiments 1 to 12 for the manufacture of a shaped article.
[0216] 15. A shaped article comprising the composition of any one of embodiments 1 to 12.
[0217] 16. A shaped article comprising the composition of any one of embodiments 14 to 20.
[0218] 17. A shaped article comprising the composition of any one of embodiments 22-23.
[0219] The following examples illustrate the invention but do not in any way limit the subject matter. EXAMPLES
[0220] 1. Starting Materials Ultramid RX2298®: A copolymer of nylon-6 and nylon-6,36 (PA6 / 6.36) sold under the trade name Ultramid RX2298® by BASF SE®, with a viscosity of 28 ml / g according to DIN 53727 (0.005 g / ml H2SO4) and an MVR (230°C / 10 kg) of 115 cm 3 / 10 min, melting temperature 201℃, and density 1.054g / cm 3 It is.
[0221] Elastollan 1180A10: TPU with a Shore hardness of 80A from BASF Polyurethanes GmbH, Elastogranstrasse 60, 49448 Lemfoerde, based on polytetrahydrofuran polyol (PTHF) with a molecular weight of 1000 g / mol, butane-1,4-diol, diphenylmethane 4,4'-diisocyanate.
[0222] Elastollan 1160D 10 Based on TPU with a Shore hardness of 60D from BASF Polyurethanes GmbH (Elastogranstrasse 60, 49448 Lemfoerde), polytetrahydrofuran polyol (PTHF) with a molecular weight of 1000, butane-1,4-diol and MDI.
[0223] Elastollan 1178 D11U: TPU with a Shore hardness of 78D from BASF Polyurethanes GmbH, Elastogranstrasse 60, 49448 Lemfoerde, based on polytetrahydrofuran polyol (PTHF) with a molecular weight of 1000, butane-1,4-diol and MDI.
[0224] Elastollan 1183D11U: TPU with a Shore hardness of 83D from BASF Polyurethanes GmbH, Elastogranstrasse 60, 49448 Lemfoerde, based on polytetrahydrofuran polyol (PTHF) with a molecular weight of 1000, butane-1,4-diol and MDI.
[0225] Elastollan 685A10: TPU with a Shore hardness of 85A from BASF Polyurethanes GmbH, Elastogranstrasse 60, 49448 Lemfoerde, based on butanediol adipate ester, butane-1,4-diol, MDI.
[0226] Elastollan B60D11: TPU with a Shore hardness of 85A from BASF Polyurethanes GmbH, Elastogranstrasse 60, 49448 Lemfoerde, based on butanediol adipate ester, butane-1,4-diol, MDI.
[0227] Elastollan AC85A12: TPU with a Shore hardness of 60A from BASF Polyurethanes GmbH, Elastogranstrasse 60, 49448 Lemfoerde, based on polyester polyol with a molecular weight of 2000 (adipic acid, butane-1,4-diol and hexane-1,6-diol), butane-1,4-diol, hexamethylene diisocyanate.
[0228] Elastollan L1160D 12 : TPU with a Shore hardness of 60D from BASF Polyurethanes GmbH, Elastogranstrasse 60, 49448 Lemfoerde, based on polytetrahydrofuran polyol (PTHF) with a molecular weight of 1000 g / mol, 1,4-butanediol and 4,4'-diisocyanatodicyclohexylmethane.
[0229] Exolit OP1230: Aluminum diethylphosphinate, CAS number: 225789-38-8, from Clariant Produkte (Deutschland) GmbH, Chemiepark Knapsack, 50351 Huerth, moisture content % (w / w) <0.2, average particle size (D50) 20-40 μm.
[0230] Fyrolflex RDP: Resorcinol bis(diphenyl phosphate), CAS number: 125997-21-9, from Supresta Netherlands BV, Office Park De Hoef, Hoefseweg 1, 3821 AE Amersfoort, The Netherlands, viscosity at 25°C = 700 mPas, acid number < 0.1 mg KOH / g, water content % (w / w) < 0.1.
[0231] Melapur MC15ED: Melamine cyanurate (1,3,5-triazine-2,4,6(1H,3H,5H)-trione, compound with 1,3,5-triazine-2,4,6-triamine (1:1)), CAS number: 37640-57-6, manufactured by BASF SE, 67056 Ludwigshafen, Germany, particle size D99%≦50 μm, D50%≦4.5 μm, moisture content (w / w)<0.2.
[0232] Melapur MC200 / 70: Melamine polyphosphate (nitrogen content 42-44% by mass, phosphorus content 12-14% by mass), CAS number: 218768-84-4, manufactured by BASF SE, 67056 Ludwigshafen, Germany, particle size D99%≦70 μm, average particle diameter D50%≦10 μm, moisture content (w / w)<0.3.
[0233] Chopvantage HP3550 EC10-3,8: Glass fiber from PPG Industries Fiber Glass, Energieweg 3, 9608PC Westerbroek, The Netherlands. E-glass, filament diameter 10 μm, length 3.8 mm.
[0234] 2. Manufacturing Examples The following table lists the compositions with the individual components listed in parts by weight (PW). Each blend was produced using a Berstorff ZE40A twin screw extruder with a screw length of 35D, divided into 10 barrel sections. Pelletization was performed using a standard underwater pelletizer (UWG) from Gala.
[0235] The density, Shore hardness, tensile strength, tear propagation resistance, abrasion and elongation at break were determined for 1.6 mm thick films. The films were extruded using an Arenz single screw extruder (screw ratio 1:3) with a 3-zone screw equipped with a mixing section. The films were evaluated for their appearance.
[0236] UL94V and HB flame retardancy tests were performed using 1.6 mm films or 2 mm injection molded plaques.
[0237] The elastic modulus, impact resistance and notched impact resistance were determined on injection-molded test specimens. For this purpose, test specimens were produced on an Arburg 520S with a thread diameter of 30 mm.
[0238] The burst pressure of a hose with an outer diameter of 8.0 mm and an inner diameter of 5.5 mm was determined. The hose was extruded using a Kuhne single screw extruder with a 3-zone screw (screw ratio 1:3) equipped with a mixing section.
[0239] The results are summarized in the table below.
[0240] 2.1 Example 1 A blend made from Elastollan 1180A10 and Ultramid RX2298.
[0241] [Table 1]
[0242] 2.2 Example 2 A blend made from Elastollan 1160D10 and Ultramid RX2298.
[0243] [Table 2]
[0244] 2.3 Example 3 A blend made from Elastollan 1178D11U and Ultramid RX2298.
[0245] [Table 3]
[0246] 2.4 Example 4 A blend made from Elastollan 1183D11U and Ultramid RX2298.
[0247] For one mixture it was possible to obtain only films, in which case the Shore hardness was determined on injection moulded parts.
[0248] [Table 4]
[0249] 2.5 Example 5 A blend made from Elastollan 685A10 and Ultramid RX2298.
[0250] [Table 5]
[0251] 2.6 Example 6 A blend made from Elastollan B60D11 and Ultramid RX2298.
[0252] [Table 6]
[0253] 2.7 Example 7 A blend made from Elastollan AC85A12 and Ultramid RX2298.
[0254] [Table 7]
[0255] 2.8 Example 8 A blend made from Elastollan L1160D12 and Ultramid RX2298.
[0256] [Table 8]
[0257] 2.9 Example 9 A mixture made from Ultramid RX2298, Exolit OP1230 and Melamine Cyanurate 15ED.
[0258] [Table 9]
[0259] 2.10 Example 10 Various exemplary mixtures made from Ultramid RX2298, AC85A12, 1160D10, Exolit OP1230, Fyrolflex RDP, melamine polyphosphate MC200 / 70 and melamine cyanurate MC15ED.
[0260] [Table 10]
[0261] 2.11 Example 11 Various exemplary mixtures made from Ultramid RX2298, AC85A12, 1160D10, Exolit OP1230, Fyrolflex RDP, melamine polyphosphate MC200 / 70 and melamine cyanurate MC15ED.
[0262] [Table 11]
[0263] References EP0352562A1 DE2846596A1 WO2018 / 050487A1 EP0922552A1 DE10103424A1 WO2006 / 072461A1
Claims
1. At least the following: (I) Thermoplastic polyurethane (TPU-1), and (II) Below, (A) at least one lactam; (B) A monomer mixture (M) containing the following components: (B1) at least one C32-C40 dimer acid, and (B2) at least one C4 to C12 diamine Copolyamide (PA-1), prepared by polymerization with A composition comprising the above (but excluding any composition which is a hot melt adhesive).
2. The composition of claim 1, wherein said thermoplastic polyurethane (TPU-1) is based on an aromatic diisocyanate.
3. 3. The composition of claim 2, wherein the thermoplastic polyurethane (TPU-1) has a Shore hardness, determined according to DIN 53505, in the range of 70A to 85D.
4. The composition of claim 1, wherein said thermoplastic polyurethane (TPU-1) is based on an aliphatic diisocyanate.
5. The composition according to any one of claims 1 to 4, wherein the proportion of said thermoplastic polyurethane (TPU-1) in said composition is in the range of 5% by weight to 95% by weight based on the total of components (I) and (II).
6. 6. Composition according to claim 1, wherein the proportion of said copolyamide (PA-1) in said composition ranges from 5% to 95% by weight, based on the total sum of components (I) and (II).
7. 7. The composition of claim 1, wherein the composition comprises at least one flame retardant selected from the group consisting of melamine cyanurate, magnesium hydroxide, and phosphorus-containing flame retardants.
8. 8. The composition according to claim 1, wherein the composition comprises at least one first phosphorus-containing flame retardant (F1) selected from the group consisting of derivatives of phosphoric acid and derivatives of phosphonic acid, and at least one further phosphorus-containing flame retardant (F2) selected from the group consisting of derivatives of phosphinic acid.
9. 9. The composition of claim 8, wherein the phosphorus-containing flame retardant (F2) is a phosphinate.
10. 10. The composition of claim 9, wherein the phosphinate is selected from the group consisting of aluminum phosphinate or zinc phosphinate.
11. 11. The composition according to claim 8, wherein the phosphorus-containing flame retardant (F1) is a phosphate ester.
12. 9. The composition of claim 8, wherein the flame retardant (F1) is selected from the group consisting of resorcinol bis(diphenyl phosphate) (RDP), bisphenol A bis(diphenyl phosphate) (BDP) and diphenyl cresyl phosphate (DPK).
13. The following steps: (a) (I) Thermoplastic polyurethane (TPU-1), and (II) a copolyamide (PA-1) prepared by polymerizing at least one lactam with a monomer mixture (M) comprising components (B1) at least one C32-C40 dimer acid and (B2) at least one C4-C12 diamine; and (b) mixing components (I) and (II); A method for producing a composition (Z-1) (excluding those which are hot melt adhesives), comprising:
14. Use of a composition according to any one of claims 1 to 12 for the manufacture of a moulded article.
Citation Information
Patent Citations
Novel hot melt adhesive and preparation method thereof
CN105733494A
Process for the production of elastic copolyamides
DE2846596A1
Process for the preparation of polyamide sheets
EP0352562A2
Molding compositions based on semihard polyamide derived fr-om fatty acid dimer and elastomer and optionally normal polyamide, manufacture, method of carrying out same and products
JP1984059745A
Flame retardant-stabiliser combination for thermoplastic polymers
JP2018154842A