Functionalized Acrylic Processing Aids for Gloss and Surface Finish Modification

Functionalized processing aids with reactive groups in PVC formulations effectively reduce surface gloss while preserving mechanical properties, addressing the limitations of existing matting agents.

JP7594562B2Active Publication Date: 2024-12-04ARKEMA INC
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
JP2022066536
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2016-03-25
Filing Date
2022-04-13
Publication Date
2024-12-04
Estimated Expiration
2037-03-23

AI Technical Summary

Technical Problem

Existing matting agents for polyvinyl chloride (PVC) and other thermoplastic polymers fail to substantially reduce surface gloss without adversely affecting mechanical properties.

Method used

Incorporation of functionalized processing aids, such as acrylic polymers or copolymers with reactive epoxy, hydroxyl, or carboxylic acid functionalities, into PVC formulations to reduce surface gloss while maintaining mechanical properties.

Benefits of technology

The functionalized processing aids achieve a significant reduction in surface gloss of at least 5 points at 85 degrees and up to 30 points at 60 degrees without compromising impact strength or other mechanical properties.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007594562000008
    Figure 0007594562000008
  • Figure 0007594562000009
    Figure 0007594562000009
  • Figure 0007594562000010
    Figure 0007594562000010
Patent Text Reader

Abstract

The present invention generally provides polyvinyl chloride (PVC) and other thermoplastic polymers and resins having reduced surface gloss, and methods for reducing the surface gloss thereof. A gloss reduction method results in a polyvinyl chloride (PVC) part exhibiting a reduced level of surface gloss, wherein the PVC or other thermoplastic part comprises PVC resin, one or more processing aids including at least one base polymer, and optionally one or more impact modifiers, the one or more processing aids being functionalized with reactive epoxy, hydroxyl, or carboxylic acid functional groups in an amount of from about 0.5% to about 35% by weight, based on the total weight of the processing aid. The PVC or other thermoplastic part exhibits at least a 5-point reduction in gloss measured at an angle of 85 degrees or less, compared to a similar PVC part except that the processing aid is not functionalized.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present disclosure relates generally to processing aids used in polyvinyl chloride (PVC) formulations as well as other thermoplastic polymers. More specifically, the present disclosure relates to processing aids that can reduce the specular gloss of PVC and other thermoplastic polymer parts without sacrificing mechanical properties. [Background technology]

[0002] The statements in this section are merely intended to provide background information regarding the present invention and may not constitute prior art.

[0003] Polyvinyl chloride (PVC) resins are generally chemically inert, resistant to water and environmental corrosion, provide good electrical and thermal insulation, and can maintain performance over a wide temperature range. Commercial polymerization and post-polymerization processing techniques (e.g., extrusion, injection molding, blow molding, etc.) used for polyvinyl chloride (PVC), or "vinyl" as it is commonly called, have matured over the past century. This manufacturing base, coupled with the fundamental properties exhibited by PVC, have led to an expansion of PVC-containing products. For example, within a decade, sales of vinyl windows (approximately 31 million per year) surpassed sales of both wood and aluminum-based windows. Vinyl products are durable, reusable, and easy to maintain. Vinyl products are resistant to fungal and mildew growth and are not susceptible to rotting, corrosion, cracking, flaking, or insect infestation. Vinyl products exhibit excellent fire resistance properties and meet most building codes for ignition, flaming flaming, heat release, burn rate, flame spread, and smoke development. Vinyl products are generally the same color throughout, so minor scratches do not require painting or repair, and the aesthetic features are easy to maintain by cleaning with soap and water. When properly installed and maintained, vinyl products provide long-lasting aesthetic features, reliable performance, and ongoing energy savings.

[0004] While the dispersion of pigments into PVC formulations can be used to impart color, the incorporation of matting agents into the formulation can alter the degree of surface gloss exhibited by the final PVC product. Matting agents typically fall into three areas: i) polymeric core / shell impact modifiers having a core of poly(butyl acrylate) and a shell of poly(methyl acrylate), such as Paraloid™ (the Dow Chemical Company, Midland, MI); ii) crosslinked poly(methyl methacrylate) particles having an average size of a few microns, such as Techpolymer® MBX K-8 (Sekisui Plastics Co. Ltd., Tokyo, Japan) or Altuglas® BS 100 particles (Arkema Inc., King of Prussia, PA); and iii) polymers such as methyl methacrylate / styrene copolymers, such as Acematt® OP 278 (Evonik Industries, Essen, Germany). However, many matting technologies directed at PVC and other thermoplastic polymers and resins may not substantially reduce surface gloss or may adversely affect other mechanical properties associated with the formed PVC part.

[0005] Other thermoplastic resins can also be used in a similar capacity as PVC resins to obtain final articles using similar post-polymerization processes. These resins can include acrylic polymers, styrenics, polyolefins, PVC blends, polycarbonates, polyurethanes, fluoropolymers / fluoropolymers and mixtures thereof.

[0006] US Patent No. 5,999,333 discloses thermoplastic polymer compositions that can be processed into capstocks with reduced gloss appearance, high impact strength, and excellent weatherability. The thermoplastic polymer compositions are alleged to comprise a core / shell polymer having a core derived from an alkyl acrylate monomer and a shell that is a copolymer derived from an alkyl methacrylate monomer and another copolymerizable monomer.

[0007] Patent Document 2 discloses a processing aid for polyvinyl chloride comprising a substantially linear copolymer obtained by polymerizing a mixture of 20 to 98.5% by weight of methyl methacrylate, 0.5 to 40% by weight of ethyl acrylate, and 1 to 40% by weight of glycidyl methacrylate so that at least 85% of the glycidyl methacrylate units have intact oxirane rings.

[0008] Patent Document 3 discloses a method for producing a methacrylate copolymer used as a processing aid for vinyl chloride resin. The method comprises the following steps: polymerizing a monomer mixture in the presence of a water-soluble initiator and an emulsifier to prepare a polymer latex; and solidifying the polymer latex. The monomer mixture comprises 60-85% by weight of methyl methacrylate, 15-30% by weight of an alkyl acrylate compound, and 1-10% by weight of an epoxide compound. [Prior art documents] [Patent documents]

[0009] [Patent Document 1] U.S. Pat. No. 7,557,158 [Patent Document 2] U.S. Pat. No. 3,301,919 [Patent Document 3] Korean Patent No. 10-1030513 Summary of the Invention

[0010] The present invention generally provides polyvinyl chloride (PVC) and other thermoplastic polymers and resins with reduced surface gloss and methods for reducing the surface gloss. The PVC or other thermoplastic polymer / resin comprises a polymer or resin such as PVC; one or more processing aids; and optionally at least one impact modifier. Parts made with the PVC or other thermoplastic polymer / resin exhibit at least a 5 point reduction in gloss measured at an angle of 85 degrees or less when compared to similar parts not functionalized with the processing aid. Parts made with the PVC or other thermoplastic polymer / resin may be used in packaging for automotive products, building materials, household or kitchen items, medical or office products, electronic products, clothing, or personal care products or other consumer products.

[0011] The processing aids comprise at least one base polymer, and one or more of the processing aids are functionalized with about 0.5% to about 35% by weight of reactive epoxy, hydroxyl, or carboxylic acid functional groups, based on the total weight of the processing aid. The processing aids are present in PVC formulations at about 0.1 to about 12 phr, or in other (non-PVC) thermoplastic parts at 0.1 to about 20 phr. If desired, the processing aids can be functionalized with at least 1% by weight of the reactive functional groups, based on the total weight of the processing aid. The reactive epoxy, hydroxyl, or carboxylic acid functional groups in the processing aids can be derived from hydroxyl-substituted alkyl esters of (meth)acrylic acid; vinyl esters of linear or branched carboxylic acids; unsaturated C3-C6 mono- and C4-C6 dicarboxylic acids; epoxy-group-containing monomers; or mixtures thereof.

[0012] According to one aspect of the present disclosure, the PVC or other thermoplastic part may exhibit at least a 10 point gloss reduction when measured at an angle of 60 degrees or less. In addition, the PVC or other thermoplastic part containing the functionalized processing aid may exhibit comparable impact properties to the similar PVC part containing the non-functionalized processing aid. The impact properties may be, but are not limited to, Izod impact or drop dart impact.

[0013] According to another aspect of the disclosure, the processing aids may exhibit an average molecular weight or weight average molar mass that is equal to or greater than about 50,000 g / mol. The base polymer in these processing aids may comprise an acrylic polymer or copolymer. The acrylic polymer or copolymer may be derived from vinyl-containing or (meth)acrylic-containing monomers; styrene or styrene derivatives; olefins; dienes; or mixtures thereof. These processing aids promote crosslinking in the PVC or other thermoplastic parts. These processing aids may also comprise between 0 and about 1 wt. % of a chain transfer agent or crosslinking agent.

[0014] The method for reducing the surface gloss of a polyvinyl chloride (PVC) or other thermoplastic part comprises the steps of: providing a PVC or other base thermoplastic resin; forming at least one base polymer as a processing aid; functionalizing the at least one base polymer to form a functionalized processing aid; optionally providing at least one impact modifier; producing a formulation from the base resin, the functionalized processing aid, and the optional impact modifier; and forming a PVC or other thermoplastic part from the formulation. The base polymer is functionalized with about 0.5% to about 35% by weight of reactive epoxy, hydroxyl, or carboxylic acid functional groups, based on the total weight of the processing aid. The resulting PVC part exhibits a gloss reduction of at least 5 points measured at an angle of 85 degrees or less when compared to a similar PVC part not functionalized with the processing aid. Alternatively, the PVC or other thermoplastic part exhibits a gloss reduction of at least 10 points measured at an angle of 60 degrees or less. Additionally, PVC or other thermoplastic parts containing the functionalized processing aids and similar PVC parts containing the non-functionalized processing aids may exhibit comparable impact properties, which may be measured, but are not limited to, Izod impact or drop dart impact.

[0015] The gloss reduction method may further include the processing aid being present at about 0.1 to about 12 phr in the PVC formulation or 0.1 to about 20 phr in the other thermoplastic formulation. If desired, the processing aids may be functionalized with at least 1 wt. % of the reactive functional group, based on the total weight of the processing aid. The reactive epoxy, hydroxyl, or carboxylic acid functional groups of the processing aids may be derived from hydroxyl-substituted alkyl esters of (meth)acrylic acid; vinyl esters of linear or branched carboxylic acids; unsaturated C3-C6 monocarboxylic acids and unsaturated C4-C6 dicarboxylic acids; epoxy group-containing monomers; or mixtures thereof. The base polymer of the processing aids may comprise an acrylic polymer or copolymer. The acrylic polymer or copolymer may be derived from vinyl-containing or (meth)acrylic-containing monomers; styrene or styrene derivatives; olefins; dienes; or mixtures thereof. The functionalized processing aids have a molecular weight (M) of about 50,000 g / mol or greater. w ).

[0016] Further scope of applicability will become apparent from the description provided herein. It should be understood that the description and specific examples are intended for purposes of illustration only and are not intended to limit the scope of the present disclosure.

[0017] The drawings described herein are for illustration purposes only and are not intended to limit the scope of the present disclosure in any way. [Brief description of the drawings]

[0018] [Figure 1] FIG. 1 is a schematic diagram of a method for forming a part from PVC or other thermoplastic polymer / resin in accordance with the teachings of the present disclosure. [Diagram 2] FIG. 2 is a graphical comparison of surface gloss (75°) and impact strength measured for PVC parts prepared from various PVC formulations of the present disclosure and conventional PVC formulations. [Diagram 3]FIG. 3 is another graphical comparison of surface gloss (60°) and impact strength measured for PVC parts prepared from various PVC formulations of the present disclosure and conventional PVC formulations. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0019] The following description is merely exemplary in nature and in no way limits the disclosure or its applications or uses. For example, polyvinyl chloride (PVC) formulations made and used according to the teachings contained herein are described throughout this disclosure in conjunction with "PVC" or "vinyl" windows and doors to more fully describe their composition and use. The incorporation and use of such PVC formulations in other applications or products is considered to be within the scope of this disclosure. Formulations made with other thermoplastic polymers / resins in other applications or products are also considered to be within the scope of this disclosure. Such applications may include, but are not limited to, packaging for automotive products, building materials, household or kitchen items, medical or office products, clothing, or personal care products or other consumer products. It should be understood that throughout the description, corresponding reference numerals indicate like or corresponding parts and features.

[0020] The present disclosure provides polyvinyl chloride (PVC) or other thermoplastic parts that exhibit reduced surface gloss without sacrificing mechanical properties overall. More specifically, the PVC or other thermoplastic parts comprise, consist essentially of, or consist of polyvinyl chloride (PVC) or other thermoplastic; one or more processing aids, at least one of which is functionalized with reactive epoxy, hydroxyl, or carboxylic acid functional groups in an amount of about 0.5% to about 35% by weight based on the total weight of the processing aids; and, optionally, at least one impact modifier. The PVC or other thermoplastic parts formed therefrom exhibit a gloss reduction of at least 5 points measured at an angle of 85 degrees or less when compared to a similar PVC part in which the processing aid (PA) is not functionalized. The functionalized processing aid (f-PA), used alone or in combination with the impact modifier, surprisingly reduces the surface gloss and maintains the mechanical properties of the PVC or other thermoplastic parts that are beneficial in many applications where aesthetic features are important. Mechanical properties that remain substantially unaffected or are improved upon functionalization of the processing aid with reactive functional groups include, but are not limited to, impact properties and density, as well as parameters related to processability (e.g., extrusion) of PVC or other thermoplastic compounds.

[0021] Alternatively, according to one embodiment of the present disclosure, the reduction in surface gloss of a PVC part comprising a functionalized processing aid (f-PA), compared to a similar PVC part using a conventional processing aid (PA), may be characterized as at least 10 points measured at an angle of 60 degrees or less; alternatively, at least 15 points measured at an angle of 20 degrees. Alternatively, the change in surface gloss (Δ) between a PVC part using an f-PA, compared to a similar PVC part using a conventional PA, is greater than about 5 points measured at any angle; alternatively, greater than about 10 points measured at any angle; alternatively, greater than 20 points measured at 85 degrees; alternatively, greater than 25 points measured at 60 degrees or less; alternatively, greater than 30 points measured at 60 degrees or less.

[0022] According to another aspect of the present disclosure, functionalized processing aids synthesized for polyvinyl chloride processing and modified with the above-mentioned functional groups, as further defined herein, achieve a differentiated effect in the polyvinyl chloride matrix when compared to conventional acrylic processing aids. These functionalized processing aids comprise acrylic polymers or copolymers synthesized with reactive epoxy, hydroxyl, or carboxylic acid functional groups that are capable of reacting during the process used to form PVC or other thermoplastic parts. Examples of methods by which PVC or other thermoplastic parts can be formed include, but are not limited to, extrusion methods. During the extrusion process, the reactive functional groups promote the occurrence of crosslinking in the presence or absence of optional chain extenders or crosslinkers. If desired, crosslinking during extrusion can occur between particles formed by the processing aids (e.g., crosslinking between the processing aids to be processed and / or between the processing aids and the PVC). Conventional processing aids used in polyvinyl chloride (PVC) formulations typically consist of acrylate and methacrylate monomers that do not react during such processing. The functionalized processing aids of the present disclosure may be made according to any method known in the art, including, but not limited to, emulsion polymerization.

[0023] The processing aids can be "acrylic" polymers or copolymers with a variety of different compositions and molecular weights. They can be of higher molecular weight than PVC resin or other thermoplastic resins. In PVC resins, in particular, they are highly compatible with PVC resins, so they aid in interparticle mixing of PVC particles in the early stages of melting. The processing aids of the present disclosure have a weight average molecular weight (molar mass (M)) of greater than about 50,000 g / mol. w or the weight average molecular weight of these processing aids is greater than about 100,000 g / mol; or the molecular weight of these processing aids (M w ) is about 250,000 g / mol or more; or the soluble fraction (M w ) is between about 50,000 g / mol and about 15,000,000 g / mol, alternatively between about 750,000 g / mol and about 12,000,000 g / mol. Molecular weight may be measured by any known method, including, but not limited to, gel permeation chromatography (GPC), the procedure of which is further described in Example 2. The upper limit of the molecular weight measurement may be affected by the occurrence of crosslinking between polymer processing aids.

[0024] In one embodiment, the processing aids of the present invention are surprisingly insoluble in organic solvents. The soluble and insoluble fractions of these processing aids can be determined by use of extraction techniques (see Example 2) using solvents such as acetone, tetrahydrofuran (THF), or methyl ethyl ketone (MEK). The insoluble fraction of these processing aids ranges from 1% to about 90%, alternatively the insoluble fraction ranges from about 2% to about 70%; alternatively the insoluble fraction ranges from about 4% to about 55%, preferably about 10-50%, more preferably about 20-45%, and even more preferably about 25-40%.

[0025] These processing aids have a glass transition temperature (T g ) or the T of those processing aids g The T of these processing aids is in the range of about 60°C to about 85°C. gcan be measured either as a powder or as a pressed bar formed from the powder using any known method, including but not limited to analysis by differential scanning calorimetry (DSC), as further described in Example 3.

[0026] These processing aids comprise base polymers or copolymers derived from ethylenically unsaturated monomers, including, but not limited to, vinyl-containing and (meth)acrylic-containing monomers such as linear or branched alkyl esters of acrylic or methacrylic acid; styrene and styrene derivatives; olefins such as ethylene; dienes such as butadiene; and mixtures thereof, with linear or branched alkyl esters of acrylic or methacrylic acid being preferred. Some specific examples of vinyl-containing and (meth)acrylic-containing monomers include, but are not limited to, methyl (meth)acrylate, ethyl (meth)acrylate, n-butyl (meth)acrylate (BMA), 2-ethylhexyl (meth)acrylate, glycidyl (meth)acrylate, and mixtures thereof, with methyl (meth)acrylate, ethyl (meth)acrylate, and glycidyl (meth)acrylate being preferred. Alternatively, the base polymer or copolymer may be poly(methyl methacrylate), poly(butyl acrylate), poly(ethyl acrylate), poly(methyl methacrylate-styrene) copolymer, or mixtures thereof. Alternatively, the base polymer comprises poly(methyl methacrylate), which is preferred for its compatibility with the PVC matrix. If desired, the glass transition temperature (T g ) and other acrylates such as poly(butyl acrylate) or poly(ethyl acrylate) can be added at levels of 10-30 wt % to control melting properties.

[0027] At least one of the processing aids used in the PVC or other thermoplastic compound to form the PVC or other thermoplastic part is functionalized with about 0.5% to about 35% by weight of reactive epoxy, hydroxyl, or carboxylic acid functional groups, based on the total weight of the processing aid. Alternatively, the loading of functionalization with the reactive groups is between about 1% and about 25% by weight; or the one or more processing aids contain at least about 5% to about 20% by weight of reactive functional groups, based on the total weight of the processing aid. It is not necessary for all of the processing aids utilized in the compound to be functionalized. In other words, conventional processing aids (PA) and functionalized processing aids (f-PA) may be utilized in combination. The ratio of PA to f-PA may range from 0:100 to about 75:25; alternatively from about 0:100 to about 50:50; alternatively from about 0:100 to about 25:75.

[0028] These processing aids may be used in powder or particle form. The powder or particles may be solid particles comprising a base polymer substantially functionalized with reactive groups or they may be pseudo core-shell particles. Functionalized processing aids (f-PAs) may be prepared in a multi-stage polymerization process, where the functionalized processing aid resembles a pseudo core-shell particle comprising a core made of a non-functionalized base polymer, at least a portion of which is encapsulated with a shell containing reactive epoxy, hydroxyl, or carboxylic acid functional groups.

[0029] Reactive epoxy, hydroxyl, or carboxylic acid groups can be introduced by adding monomers containing epoxy, hydroxyl, or carboxylic acid to the base polymer. Examples of such monomers include, but are not limited to, hydroxyl-substituted alkyl esters of (meth)acrylic acid, such as 2-hydroxyethyl (meth)acrylate; vinyl esters of linear or branched carboxylic acids, such as vinyl valerate; unsaturated carboxylic acids, including unsaturated C3-C6 monocarboxylic acids, such as acrylic acid (AA), and unsaturated C4-C6 dicarboxylic acids, such as maleic acid and itaconic acid; and epoxy group-containing monomers, such as glycidyl acrylate or glycidyl methacrylate (GMA). Unsaturated C3-C6 monocarboxylic acids, such as acrylic acid (AA), and unsaturated C4-C6 dicarboxylic acids, such as maleic acid and itaconic acid; and epoxy group-containing monomers, such as glycidyl acrylate or glycidyl methacrylate (GMA), are preferred, and more preferred are acrylic acid, glycidyl acrylate, and glycidyl methacrylate (GMA). Alternatively, those functional groups may be incorporated into the base polymer of the processing aid by the addition of acrylic acid (AA), glycidyl methacrylate (GMA), or mixtures thereof, most preferably.

[0030] The amount of processing aid present in the PVC formulation may range from about 0.1 phr to about 12 phr in the PVC formulation, 0.1 to about 20 phr in the other thermoplastic resin part; or from about 0.1 phr to about 7 phr in the PVC formulation, 0.1 to about 10 phr in the other thermoplastic resin part; or 1 phr or more. In the context of this disclosure, the term "phr" means parts per hundred parts of the PVC or other thermoplastic base resin. The amount of processing aid present in the PVC or other thermoplastic resin formulation may also be expressed as a weight percentage based on the total weight of the PVC or other thermoplastic resin formulation. The use level of processing aid in the PVC formulation may vary depending on the type of PVC formulation selected and the written specifications for the application in which the PVC or other thermoplastic resin part is to be utilized. In other words, the amount of processing aid in the formulation may be predetermined based on the use level required to reduce the surface gloss to a level that meets the color requirements for a given application (i.e., siding, window profiles, pipes, or foam sheeting, among others).

[0031] Without being bound to a particular theory, it is believed that the processing aids may facilitate melting of the PVC resin by altering the melt rheology of the PVC compound during extrusion. The processing aids may also aid in facilitating mixing of the components as the melting of the PVC resin occurs, improving the strength of the molten polymer blend, controlling the volume increase or expansion (e.g., die swell) that occurs immediately after the molten polymer blend leaves the die opening, and reducing the occurrence of plate-out and crystallinity, as well as improving long-term impact strength and weatherability. In general, processing aids with higher molecular weights tend to provide higher levels of die swell. Higher levels of die swell may be beneficial when making foamed PVC parts.

[0032] The functionalized processing aid (f-PA) can also promote crosslinking during the process of forming a PVC part from the PVC compound. Such crosslinking can be carried out in the presence or absence of a chain transfer agent or crosslinking agent. If desired, an optional chain transfer agent or crosslinking agent can be incorporated into the processing aid in an amount of greater than 0% by weight up to about 1% by weight, based on the total weight of the processing aid. Some examples of such chain transfer agents or crosslinking agents include, but are not limited to, mercaptans, polymercaptans, alcohols, and halogen-containing compounds, with mercaptans and polymercaptans being preferred.

[0033] In other thermoplastics, the purpose of the processing aid is to reduce gloss.

[0034] PVC resins can be made in a number of different molecular weights using any method known in the art, including, but not limited to, solution polymerization, suspension polymerization, or emulsion polymerization. PVC resins can include, but are not limited to, rigid PVC resins, flexible PVC resins, PVC plastisols, and blends or combinations formed with one or more other thermoplastic and / or thermosetting resins. PVC resins can be characterized by their molecular weight, which is generally reported as intrinsic viscosity (IV) or K value. Generally, the higher the IV or K value of the PVC resin, the greater the impact strength of the PVC or other thermoplastic parts made therefrom. However, PVC resins with high molecular weights are also more difficult to achieve melting and polymer flow without the use of excessive heat or shear. The molecular weight of the PVC resin used in the formulation from which the PVC parts are made can be predetermined based on the mechanical properties desired for the final product and economic factors. Typically, resins in the K value range of about 56 to about 72; alternatively about 63 to about 67; alternatively about 65 are used to form PVC parts having rigid profiles, with lower molecular weights being used for foaming applications. The molecular weight of the PVC resin is generally less than the molecular weight of the processing aids with which it is used. The amount of PVC resin used in the formulation to form the PVC or other thermoplastic resin part can range between about 30% to about 85% by weight; alternatively about 50% to about 80% by weight of the total PVC formulation.

[0035] For example, other thermoplastics useful in the present invention as cap layers on a substrate include, but are not limited to, acrylic polymers, styrenic polymers, polyolefins, polyvinyl chloride (PVC), polycarbonate (PC), polyurethane (PU), polyvinylidine fluoride polymer (PVDF), polylactic acid (PLA), and the like, and mixtures thereof. Other thermoplastics such as those described herein can be combined with PVC or used in any combination thereof, with or without the presence of PVC, further comprising a processing aid of the present invention, to form parts with reduced surface gloss.

[0036] Styrenic polymers used herein include, but are not limited to, polystyrene, high impact polystyrene (HIPS), acrylonitrile-butadiene-styrene (ABS) copolymers, acrylonitrile-styrene-acrylate (ASA) copolymers, styrene-acrylonitrile (SAN) copolymers, methacrylate-acrylonitrile-butadiene-styrene (MABS) copolymers, styrene-butadiene copolymers (SB), styrene-butadiene-styrene block (SBS) copolymers and their partially or fully hydrogenated derivatives, styrene-isoprene copolymers, styrene-isoprene-styrene (SIS) block copolymers and their partially or fully hydrogenated derivatives, styrene-(meth)acrylate copolymers such as styrene-methyl methacrylate copolymer (S / MMA), and mixtures thereof. A preferred styrenic polymer is ASA. The styrenic copolymers of the present invention have a styrene monomer content of at least 10% by weight, preferably at least 25% by weight.

[0037] These styrenic polymers can also be blended with other polymers to form compatible blends. Examples include ASA blended with PVC, and SAN blended with PMMA.

[0038] As used herein, acrylic polymers include, but are not limited to, homopolymers, copolymers and terpolymers comprising alkyl (meth)acrylates.

[0039] The alkyl methacrylate monomer is preferably methyl methacrylate, which may comprise 60-100% of the monomer mixture. 0-40% of other acrylates, methacrylates, and / or other vinyl monomers may also be present in the monomer mixture. Other methacrylates, acrylates, and other vinyl monomers useful in the monomer mixture include, but are not limited to, methyl acrylate, ethyl acrylate and methacrylate, butyl acrylate and methacrylate, isooctyl methacrylate and acrylate, lauryl acrylate and methacrylate, stearyl acrylate and methacrylate, isobornyl acrylate and methacrylate, methoxyethyl acrylate and methacrylate, 2-ethoxyethyl acrylate and methacrylate, dimethylaminoethyl acrylate and methacrylate monomers, styrene and its derivatives. Alkyl (meth)acrylic acids such as (meth)acrylic acid and acrylic acid may be useful in the monomer mixture. Small amounts of multifunctional monomers as crosslinkers may also be used. The preferred acrylic polymer is methyl methacrylate and 2-16% of one or more C 1-4 It is a copolymer with acrylate.

[0040] The thermoplastic polymers of the present invention can be produced by any means known in the art, including emulsion polymerization, solution polymerization, and suspension polymerization. In one embodiment, the thermoplastic matrix has a weight average molecular weight between 50,000 and 500,000 g / mol, preferably 75,000 to 150,000 g / mol, as measured by gel permeation chromatography (GPC). The molecular weight distribution of the thermoplastic matrix can be unimodal or multimodal with a polydispersity index greater than 1.5.

[0041] Particularly preferred thermoplastics for the matrix polymer are styrenic polymers (including SAN, ABS, MABS, ASA, HIPS), acrylic polymers, and PVDF polymers.

[0042] If desired, the PVC formulations used to form the PVC or other thermoplastic parts may optionally include at least one impact modifier. The impact modifier increases the toughness and resistance of the final product to cracking or shattering during any subsequent manufacturing operations performed on the PVC or other thermoplastic parts, such as cutting or drilling in the part's profile. Impact modifiers typically function by absorbing energy and / or dissipating the energy of a propagating crack. These impact modifiers may include any compatible polymer particles, including block copolymers and "core-shell particulate" polymers having a soft rubbery core (Tg<0°C) or hard core (Tg>0°C) that is barely compatible with the PVC resin, and a grafted, compatible, outer polymer shell. The polymer particles or compatible outer polymer shells may comprise methacrylate / butadiene / styrene (MBS), acrylic polymers (e.g., known as acrylic impact modifiers [AIMs]), or acrylate / butadiene / methacrylate, and acrylonitrile / butadiene / styrene (ABS); semi-compatible polymers such as chlorinated polyethylene (CPE) and ethylene-vinyl acetate (EVA) polymers; and other polymers such as ethylene / vinyl acetate / carbon monoxide, ethylene / propylene / carbon monoxide terpolymers, polymers of olefins and acrylates, various copolymers of butadiene with acrylonitrile, methacrylates or other rubbers, as well as polysiloxane toughening materials. A preferred shell comprises polymethyl methacrylate (PMMA).

[0043] The PVC or other thermoplastic resin formulation may also optionally comprise one or more inorganic fillers or particles, pigments, lubricants, stabilizers, or other desired additives. For example, ultrafine CaCO3 particles may be used as a filler to enhance low temperature impact resistance and improve UV stability of rigid PVC products. Synthetic amorphous silica particles may also be incorporated into the PVC formulation to enhance impact resistance and provide improved flow properties. Other solid fillers, including but not limited to kaolin clay, talc, mica, wollastonite, calcium metasilicate, may also be incorporated into the formulation simply to reduce the cost of the formulation without substantially affecting the properties exhibited by the PVC or other thermoplastic resin part.

[0044] A variety of pigments can be included to impart color to PVC or other thermoplastic parts. These pigments are generally stable at high temperatures and in the presence of hydrogen chloride. These pigments can include, but are not limited to, a variety of organic or ceramic pigments, such as titanium dioxide and other metal oxides, with or without silica or alumina surface treatments.

[0045] Various lubricants can be included in the PVC formulation in relatively small amounts to reduce the flow resistance of the polymer chains and other components present. These lubricants can act as external lubricants or metal release (slip) agents to enhance the flow of the "hot" material through the processing equipment or as internal lubricants to reduce the melt viscosity of the material being processed. Lubricants are the main additional components that can be added to the formulation that can help promote or drive the melting of the PVC resin. Some examples of lubricants include, but are not limited to, paraffin wax and long chain carboxylic acids or their esters, amides, and salts. The amount of lubricant utilized is typically at a level that does not cause "plate out." Plate out occurs when the lubricant present in the formulation is locked out of the hot bulk material as the extrudate leaves the die or passes through a vacuum calibrator, thereby causing either a plug or a buildup of material.

[0046] To name a few, various stabilizers can be included in PVC or other thermoplastic formulations to enhance resistance to heat or UV light. Heat stabilizers can include, but are not limited to, lead-based or organotin compounds, mixed metal stabilizers, or organic stabilizers such as epoxides. UV stabilizers can include, but are not limited to, hindered amines or phenols.

[0047] According to another aspect of the present disclosure, a method (10) for reducing the specular gloss of a polyvinyl chloride (PVC) or other thermoplastic part is provided. Referring to FIG. 1, the method (10) generally comprises the steps of providing a PVC or other thermoplastic base resin (15), forming at least one base polymer as a processing aid (20); functionalizing the base polymer with reactive functional groups to form a functionalized processing aid (25); producing a PVC or other thermoplastic formulation from the base resin and the functionalized processing aid (30); and forming a PVC or other thermoplastic part from the PVC or other thermoplastic formulation (35). More specific information regarding the PVC formulation and its composition has been previously discussed above and is further defined herein. The base polymer is functionalized with between about 0.5% and 35% by weight of reactive epoxy, hydroxyl, or carboxylic acid functional groups. Optionally, at least one impact modifier can also be provided (40) and incorporated into the PVC or other thermoplastic formulation (30). The resulting PVC or other thermoplastic part exhibits at least a 5 point reduction in surface gloss measured at an angle of 85° or less.

[0048] Other embodiments of the present invention 1. A polyvinyl chloride (PVC) part having reduced surface gloss, one or more processing aids comprising at least one base polymer, one or more of the processing aids being functionalized with from about 0.5% to about 35% by weight of reactive epoxy, hydroxyl, or carboxylic acid functional groups, based on the total weight of the processing aid; optionally, at least one impact modifier; comprising wherein the PVC part exhibits at least a 5 point gloss reduction measured at an angle of 85 degrees or less when compared to a similar PVC part that is not functionalized with the processing aid. 2. The PVC part of claim 1, wherein the processing aid is present at about 0.1 to about 12 phr. 3. The PVC part of any one of claims 1 or 2, wherein the one or more processing aids are functionalized with at least 5 wt.% of the reactive functional group, based on the total weight of the processing aids, and the PVC part exhibits a gloss reduction of at least 10 points when measured at an angle of 60 degrees or less. 4. The PVC part of any one of claims 1 to 3, wherein the PVC part containing the functionalized processing aid and the similar PVC part containing the non-functionalized processing aid exhibit comparable impact properties; the impact properties being measured as Izod impact or drop dart impact. 5. The PVC part according to any one of claims 1 to 4, wherein the reactive epoxy, hydroxyl, or carboxylic acid functional groups are derived from hydroxyl-substituted alkyl esters of (meth)acrylic acid; vinyl esters of linear or branched carboxylic acids; unsaturated C3-C6 monocarboxylic acids and unsaturated C4-C6 dicarboxylic acids; epoxy group-containing monomers; or mixtures thereof. 6. The base polymer of the one or more processing aids comprises an acrylic polymer or copolymer, and the molecular weight (M w 6. The PVC part according to claim 1, wherein the molecular weight of the PVC part is about 50,000 g / mol or more. 7. The PVC part according to any one of claims 1 to 6, wherein the acrylic polymer or copolymer is derived from vinyl-containing or (meth)acrylic-containing monomers; styrene or styrene derivatives; olefins; dienes; or mixtures thereof. 8. The PVC part of any one of claims 1-7, wherein the one or more functionalized processing aids promote crosslinking in the PVC part, and the functionalized processing aid further comprises between 0 and about 1 weight percent of a chain transfer agent or crosslinking agent. 9. Use of the PVC part according to any one of claims 1 to 8 in packaging for automotive products, building materials, household or kitchen items, medical or office products, clothing, or personal care products or other consumer products. 10. A method for reducing the surface gloss of a polyvinyl chloride (PVC) part, comprising: providing a PVC resin; forming at least one base polymer as a processing aid; functionalizing the at least one base polymer to form a functionalized processing aid, the base polymer being functionalized with about 0.5% to about 35% by weight of reactive epoxy, hydroxyl, or carboxylic acid functional groups, based on the total weight of the processing aid; Optionally, providing at least one impact modifier; producing a PVC formulation from said PVC resin, said functionalized processing aid, and said optional impact modifier; forming the PVC part from the PVC formulation; comprising wherein the PVC part exhibits at least a 5 point gloss reduction measured at an angle of 85 degrees or less when compared to a similar PVC part that is not functionalized with said processing aid. 11. The method of claim 11, wherein said processing aid is present at about 0.1 to about 12 phr. 12. The method of any one of claims 10 or 11, wherein the one or more processing aids are functionalized with at least 5 wt.% of the reactive functional group, based on the total weight of the processing aids, and the PVC part exhibits a gloss reduction of at least 10 points when measured at an angle of 60 degrees or less. 13. The method of any one of claims 10-12, wherein the PVC part containing the functionalized processing aid and the similar PVC part containing the non-functionalized processing aid exhibit comparable impact properties; the impact properties being measured as Izod impact or drop dart impact. 14. The method of any one of claims 10-13, wherein the reactive epoxy, hydroxyl, or carboxylic acid functional groups are derived from hydroxyl-substituted alkyl esters of (meth)acrylic acid; vinyl esters of linear or branched carboxylic acids; unsaturated C3-C6 mono- and C4-C6 dicarboxylic acids; epoxy group-containing monomers; or mixtures thereof, and the base polymer of the one or more processing aids comprises an acrylic polymer or copolymer, which is derived from vinyl- and (meth)acrylic-containing monomers; styrene and styrene derivatives; olefins; dienes; or mixtures thereof. 15. The one or more functionalized processing aids promote crosslinking in the PVC part, and the one or more functionalized processing aids have a molecular weight (M) of about 50,000 g / mol or greater. w 15. The method of any one of claims 10-14, wherein the functionalized processing aid further comprises between 0 and about 1 weight percent of a chain transfer agent or crosslinking agent. EXAMPLES

[0049] Example 1 - General Experimental Conditions and Test Protocol Both functionalized and conventional processing aids were evaluated in PVC formulations to observe and compare mechanical properties including processability, and gloss levels. Polymer processing was performed using a Brabender rheometer to measure melt torque, melt time, melt temperature, and equilibrium torque using blended PVC formulations (powders) containing either control acrylic processing aids or those functionalized with reactive species. The methodology for measuring melting of PVC compounds using a torque rheometer is standard practice performed according to ASTM D2538-02 (2010, ASTM International, West Conshohocken, PA).

[0050] Pellets made from the PVC formulations are then used in an injection molding machine to prepare injection molded test bars and plaques or sheets. After the bars and plaques are made, they are tested for impact strength and gloss with a gloss meter, and the ability of the surface of each sample to reflect light is recorded. Izod impact is defined as the kinetic energy required to initiate and continue a fracture until the specimen breaks. Izod specimens are notched and measured according to the methodology defined in ASTM D256-10e1 (ASTM International, West Conshohocken, PA). The impact strength or toughness of plastics may also be determined using the falling dart (i.e., Gardner impact) methodology defined according to ASTM D4226 and ASTM D5420 (ASTM International, West Conshohocken, PA).

[0051] Gloss is related to the ability of a surface to reflect more light in a more specular direction. The specular gloss of the bars and plaques was measured at various angles according to the standard test methodology described in ASTM D523 (2014, ASTM International, West Conshohocken, PA). The measured gloss rating was obtained by comparing the specular reflectance of the test bar or plaque to that of a black glass standard.

[0052] The amount of each processing aid that forms a soluble fraction or remains as an insoluble fraction can be measured using extractions performed with solvents such as acetone, THF, or MEK. A predetermined total amount of powder is added to a flask along with about 35 grams of solvent. This powder / solvent mixture is stirred or shaken for 22 hours, at which point another about 30 grams of solvent is added to the flask, which is then stirred or shaken for an additional 1.5 hours. About 30 grams of the mixed solution is then placed in a centrifuge tube and centrifuged at 16,500 rpm at a temperature of 5°C for 3 to 5 hours. The top of the separated mixed solution is added to another tube, which is then centrifuged once more under similar conditions. The clear supernatant present in the centrifuge tube is collected and 10 mL of this supernatant is placed in an aluminum pan using a serological pipette. The supernatant in the aluminum pan is exposed to heat to dryness, and the percentage of the insoluble fraction can be determined according to Equation 1, where W f is the final weight of the aluminum pan, and W i is the initial weight of the aluminum pan, W(powder) is the weight of the predetermined amount of powder placed in the flask, V(solvent) is the total volume of solvent placed in the flask, and V(supernatant) is the volume of supernatant pipetted into the aluminum pan.

[0053] Insoluble fraction (%) = [1-{(W f -W i ) / W(powder)×V(solvent) / V(supernatant)}]×100 (Formula 1)

[0054] Example 2 - Determination of molecular weight of processing aids Molecular weights for processing aids may be determined by various known methods and procedures using gel permeation chromatography (GPC). One such method utilizes a differential refractometer equipped with two PL gel mixed A columns and a guard column. An injection volume of 150 microliters (μL) of the soluble portion of the processing aid as a THF solution having a concentration of 1.5 mg / mL is injected into the column at a temperature of 35° C. Elution of the processing aid through the column is performed using THF solvent (HPLC grade) at a flow rate of 1.0 mL / min. Each sample of processing aid may be tested in either a filtered or unfiltered state. Chromatograms of each sample tested are obtained and the molar mass values ​​are calculated against a poly(methyl methacrylate), PMMA, calibration curve and analyzed. Further information regarding GPC methodology can be found in ASTM D4001-13 (ASTM International, West Conshohocken, PA).

[0055] The molar mass averages of filtered and unfiltered samples may differ slightly from each other. In other words, filtration of a sample with a 1.0 μm PTFE film may affect the measured molecular weight distribution. Filtration of a sample may remove very high molar mass species, thereby lowering the upper limit of the molar mass distribution. Filtration of a sample may also cause decomposition of high molar mass species, thereby increasing the amount of lower molar mass species, resulting in higher values ​​of number-averaged and / or weight-averaged molar mass averages. The molar mass average is a weighted average based on the number of molecules in each slice, therefore, an increase or decrease in the amount of molecules of a given molar mass may affect the molar mass average and distribution.

[0056] The molecular weight of the soluble portion of a total of 13 different processing aid samples prepared according to the teachings of the present disclosure was measured. A total of three injections were averaged for each sample, and the average molecular weight (M w The molecular weights of each different processing aid sample were obtained unfiltered and filtered as well. The average molecular weights (M w) ranged from 50,000 g / mol to about 15,000,000 g / mol in both the unfiltered and filtered states. The ratio of weight average to number average molecular weight (M w / M n The polydispersity, defined as the weight average molecular weight (M), was measured to be between about 10 and about 60. For example, one particular processing aid sample had a weight average molecular weight (M w ) 2,690,000 g / mol and polydispersity 54.2, and the M w The molecular weight was 2,110,000 g / mol and the polydispersity was 15.5.

[0057] Example 3 - Determination of Glass Transition Temperature of Processing Aids The glass transition temperature (T g Differential scanning calorimetry (DSC) is utilized to determine the thermal conductivity (Tc) of the polymer. Each DSC measurement is obtained over a temperature range of -75°C to 160°C using a heating rate of 20°C / min and a cooling rate of 10°C / min. T g DSC is determined as the average of at least two measurements taken for each sample formulation. Further description of DSC methodology can be found in ASTM E1356-08(2014) (ASTM International, West Conshohocken, PA).

[0058] The glass transition temperature (T g ) can be determined as a powder or as a bar formed from the powder. The powder can be pressed into a bar when exposed to high pressure (e.g., 25 tons) and high temperature (e.g., 215°C). A total of 10 different processing aid samples were analyzed, and the average T for each sample was g The glass transition temperatures ranged from 0°C to approximately 150°C. No significant differences were observed in the glass transition temperatures measured for the bars and powders. For example, one particular processing aid sample exhibited a glass transition temperature of 85.0°C in bar form and 83.4°C in powder form.

[0059] Example 4 - PVC Formulations and Parts Prepared and Tested with Glycidyl Methacrylate (GMA) Functionalized Processing Aids 24,948 grams (100 phr) of PVC resin (PVC-5385, Axiall Corp., formerly Georgia Gulf, Atlanta, GA), 249.48 grams (1.0 phr) of tin stabilizer (T-161, PMC Organometallix, Inc., Carrollton, KY), 299.38 grams (1.2 phr) of calcium stearate, 249.48 grams (1.0 phr) of lubricant (Rheolub® RL-165, Honeywell International Inc., NJ), 24.95 grams (0.1 phr) of a second polyethylene lubricant (AC629A, Honeywell International A masterbatch of 29,014.52 grams (116.3 phr) of polyvinyl chloride (PVC) formulation was prepared comprising calcium carbonate (Arkema Inc., NJ), 748.44 grams (3.0 phr), and 2,494.8 grams (10 phr) of titanium dioxide. This PVC masterbatch was then utilized to prepare PVC formulations containing various combinations of conventional processing aids (c-PA) and functionalized processing aids (f-PA) with conventional impact modifiers (c-IM) or functionalized impact modifiers (f-IM). The conventional impact modifier (c-IM) utilized in this experiment was an acrylic polymer (Durastrength® D-350, Arkema Inc., King of Prussia, PA), and the conventional processing aid (c-PA) utilized in this experiment was an acrylic polymer (Plastistrength® 550, Arkema Inc., King of Prussia, PA). The functionalized impact modifier (f-IM) and functionalized processing aid (f-PA) utilized in this study were prepared by functionalizing conventional IM and PA with approximately 16 wt % glycidyl methacrylate (GMA).

[0060] A summary of the processing aids and impact modifiers present in the four comparative samples (Test Nos. C1-C4) and two test samples (Test Nos. R1 and R2) that were prepared and tested is provided below in Table 1. The amount of impact modifier utilized in each of the comparative and test samples was 4 phr. The amount of processing aid utilized in each of the comparative and test samples was either 1 phr or 3 phr. Thus, the total amount of impact modifier and processing aid added to the PVC masterbatch was on the order of 5 phr or 7 phr.

[0061] [Table 1]

[0062] The PVC formulations containing the impact modifiers and processing aids were then evaluated using a Brabender rheometer and injection molded bars or plaques formed therefrom were tested for density, Izod impact, and surface gloss at various angles. A summary of the test results is provided in Table 2 below. The test samples (Test Nos. R1 and R2) were observed to exhibit similar properties with respect to density, melt time, melt torque, melt temperature, and equilibrium torque.

[0063] [Table 2]

[0064] It was observed that the comparative samples (C2 and C4) comprising the functionalized impact modifier exhibited gloss levels at all angles similar to the comparative samples (C1 and C3) comprising the conventional impact modifier. However, a shift in gloss was observed at all angles for the test samples (R1 and R2) when compared to the comparative samples (C1-C4). More specifically, the test sample (R1) comprising 1 phr of the functionalized processing aid exhibited a reduction in gloss in the range of about 38-46 points at an angle of 20°, about 16-18 points at an angle of 60°, and about 7-9 points at an angle of 85° when compared to the comparative samples (C1 and C2). Similarly, the test sample (R2) comprising 3 phr of the functionalized processing aid exhibited a reduction in gloss in the range of about 50-56 points at an angle of 20°, about 68-70 points at an angle of 60°, and about 33 points at an angle of 85° when compared to the comparative samples (C3 and C4). In addition, the test samples (R1 and R2) exhibited Izod impact resistance that was as good, if not better, than the comparative samples (C1-C4).

[0065] This example demonstrates that PVC formulations incorporating functionalized processing aids can be formed into PVC parts that exhibit reduced gloss at angles of 20°, 60°, and 85° when compared to similar PVC parts containing only conventional non-functionalized processing aids. This example also demonstrates that similar functionalization of impact modifiers does not provide the beneficial effect of gloss reduction observed for the use of functionalized processing aids. In addition, the use of functionalized impact modifiers reduces the impact properties of PVC or other thermoplastic parts (see comparison of C1 / C3 to C2 / C4). On the other hand, the use of functionalized processing aids maintains the mechanical properties of the PVC formulation during processing and after formation of the PVC parts at similar levels as observed for PVC formulations and parts formed with conventional processing aids.

[0066] Example 5 - Preparation of processing aids functionalized with acrylic acid (AA) or glycidyl methacrylate (GMA) f-PA via GMA functionalization- A 5 liter polymerization heating mantle reactor equipped with stirrer and reflux condenser was charged with 848.7 g of distilled water, 31.34 g of sodium dodecylbenzenesulfonate, and 0.48 g of sodium carbonate. A monomer mixture of 320.0 grams of methyl methacrylate (MMA), 100.0 grams of butyl acrylate (BA), and 80.0 grams of glycidyl methacrylate (GMA) having a MMA / BA / GMA weight percent ratio of 64 / 20 / 16 was prepared and then added to the reactor. The reaction temperature was set at 45°C while the reactor was sparged with nitrogen for 20 minutes. The reaction was initiated under a nitrogen atmosphere by adding 20.45 g of a 4% solution of potassium persulfate in distilled water and 12.12 g of a 5% solution of sodium metabisulfite in distilled water. A peak temperature of 86°C was observed after 12 minutes. The reactor temperature was set to 80°C and 1.25g of a 4% solution of potassium persulfate in distilled water was added to the reactor. The batch was held at 80°C for 30 minutes and then cooled to room temperature. The average latex particle size Dv was measured to be about 100nm using a Nicomp Modle 380 ZLS. The solids content was about 36%. The latex particles of GMA-functionalized f-PA were isolated using a spray drying method.

[0067] f-PA via AA functionalization The same procedure as described above for GMA functionalization of the processing aid was followed to produce an acrylic acid (AA) functionalized processing aid, except that the -GMA comonomer was replaced with acrylic acid. Thus, the monomer mixture utilized comprised 324.6 grams of methyl methacrylate (MMA), 100.0 grams of butyl acrylate (BA), 75.0 grams of acrylic acid (AA), and 0.375 grams of tert-dodecyl mercaptan (t-DDM), with a MMA / BA / AA / t-DDM weight percent ratio of 64.925 / 20 / 15 / 0.075. A peak temperature of 79.5°C was observed 18 minutes after the addition of the initiator. The average latex particle size was measured to be about 165 nm. The solids content was about 35.7%. The latex particles of AA functionalized f-PA were isolated using a spray drying method.

[0068] Example 6 - PVC formulations and parts prepared and tested with processing aids prepared in Run 2. Two masterbatches were prepared comprising 3,090 grams (123.6 phr) of a polyvinyl chloride (PVC) formulation and pigmented with either a white or a beige pigment. Each batch comprised 2,500.0 grams (100 phr) of PVC resin (SE-950, Shintech Inc., Houston, TX), 25.0 grams (1.0 phr) of tin stabilizer (Thermolite® 161, PMC Group Inc., Mount Laurel, NJ), 25.0 grams (1.2 phr) of calcium stearate, 2.5 grams (0.1 phr) of lubricant (Epoline E-14, Westlake Chemical Corp., Houston, TX), 112.5 grams (4.5 phr) of impact modifier (Durastrength® D-350, Arkema Inc., King of Prussia, PA), 125.0 grams (5.0 phr) of calcium carbonate, 250.0 grams (10.0 phr) of titanium dioxide, and 25.0 grams (1.0 phr) of white or beige pigment. These PVC masterbatches were then utilized to prepare various PVC formulations containing various combinations of the functionalized processing aids prepared in Experiment 2 (Test Nos. R3-R7), as well as a control sample comprising conventional non-functionalized processing aids (Control No. C5).

[0069] A summary of the processing aid composition added to the masterbatches to form the PVC formulations is shown in Table 3. Each test sample (Test Nos. R3-R7) and control sample (Control No. C5) contained a total of 25.0 grams (1.0 phr) of processing aid. The processing aid in the control sample (C5) was a conventional acrylic polymer (Plastistrength® 550, Arkema Inc., King of Prussia, PA). The f-PA used in Test No. R3 consisted entirely of processing aids functionalized with acrylic acid (AA) in Run 2. Similarly, the f-PA used in Test No. R7 consisted entirely of processing aids functionalized with glycidyl methacrylate (GMA) in Run 2. The f-PA used in Test Nos. R4-R6 consisted of a mixture of AA-functionalized and GMA-functionalized processing aids in Run 2. The ratios of AA / GMA processing aids utilized in Test Nos. 4, 5, and 6 were 1 / 3, 2 / 2, and 3 / 1, respectively. Each test sample (Test Nos. R3-R7) and control sample (Control No. C5) contained two tests, i.e., one test with a white pigment and one test with a beige pigment.

[0070] [Table 3]

[0071] The PVC formulations containing the functionalized processing aids (Test Nos. R3-R7) and the PVC formulation containing the conventional processing aid (Control No. C5) were then formed into sheets (0.040" x 4.5") using a Brabender conical twin screw extruder and the surface gloss of the sheets was measured at various angles. No differences were noted in the processing of the sheets. A summary of the average gloss measurements obtained for each test sample is provided below in Table 4. The reported average gloss represents the average of 60 measurements obtained from the top, bottom, left and right sides of the sheet.

[0072] All of the test sheets (Test Nos. R3-R7) containing functionalized processing aids, either white or beige, showed substantial reductions in gloss at all angles when compared to the gloss measured for a comparative sheet (Control No. C5) containing a conventional non-functionalized processing aid. The white pigmented test sheets (R3-R7) showed reductions in gloss on the order of about 34-39 points at a 20° angle, about 34-55 points at a 60° angle, about 13-20 points at a 75° angle, and about 20-27 points at an 85° angle, compared to the comparative sheet (Control No. C5). Similarly, the beige-pigmented test sheets (Test Nos. R3-R7) exhibited gloss reductions on the order of about 23-30 points at an angle of 20°, about 27-46 points at an angle of 60°, about 12-19 points at an angle of 75°, and about 11-20 points at an angle of 85°, compared to the comparison sheet (Control No. C5).

[0073] [Table 4]

[0074] In addition, it is observed that the amount of GMA-functionalized f-PA or AA-functionalized f-PA affects the level of gloss reduction. In general, it is observed that as the GMA / AA ratio increases, the gloss reduction measured on the test sheets or parts increases. For example, the test sheet completely composed of GMA-functionalized f-PA (Test No. R7) showed a greater gloss reduction than the test sheet completely composed of AA-functionalized f-PA (Test No. R3) when measured at angles between 20° and 75° on both the white and beige parts.

[0075] Referring now to Figures 2 and 3, the gloss values ​​measured at angles of 60° and 75° for the test sheets or parts (Test Nos. R3-R7), respectively, are graphically compared to the gloss values ​​measured for the comparative sheet (Control No. C5). In addition, the Dart Drop test impact results for each sheet are also compared. It has been found that the incorporation of f-PA into PVC or other thermoplastic parts reduces the gloss and does not affect the impact strength of the parts when compared to the impact performance of PVC parts having only conventional non-functionalized processing aids.

[0076] This example also demonstrates that PVC formulations incorporating functionalized processing aids can be formed into PVC parts that exhibit reduced gloss at angles of 20°, 60°, and 85° when compared to similar PVC parts containing only conventional non-functionalized processing aids. This example further demonstrates that functionalization of the processing aids can be performed with GMA, AA, or mixtures thereof. A comparison between the gloss reduction exhibited by test parts containing f-PA functionalized with GMA and test parts containing f-PA functionalized with AA indicates that GMA functionalization can be more effective at reducing the gloss of parts than AA functionalization. This example also demonstrates that gloss reduction resulting from the incorporation of functionalized processing aids can be observed in differently colored PVC parts.

[0077] Example 7 - Additional PVC formulations and parts prepared and tested with the processing aids prepared in Run 2. 2,000 grams (100 phr) of PVC resin (SE-950, Shintech Inc., Houston, TX), 20.0 grams (1.0 phr) of tin stabilizer (Thermolite® 161, PMC Group Inc., Mount Laurel, NJ), 24.0 grams (1.2 phr) of calcium stearate, 20.0 grams (0.1 phr) of lubricant (Rheolub® RL-165 Honeywell International Inc., NJ), 2.0 grams (0.1 phr) of a second polyethylene lubricant (AC629A, Honeywell International Inc., NJ), 90.0 grams (4.5 phr) of impact modifier (Durastrength® D-350, Arkema A 2,526.0 gram (126.3 phr) polyvinyl chloride (PVC) formulation masterbatch was prepared comprising 100.0 grams (5.0 phr) calcium carbonate, 200.0 grams (10.0 phr) titanium dioxide, and 70.0 grams (3.5 phr) beige pigment (Chemical Polymers, Inc., King of Prussia, PA). This PVC masterbatch was then utilized to prepare various PVC formulations containing various combinations of the functionalized processing aids prepared in Experiment 2 (Test Nos. R8-R12), as well as control formulations comprising non-functionalized processing aids and / or impact modifiers (Control Nos. C6-C14).

[0078] A summary of the processing aid compositions added to the masterbatches to form the PVC formulations is provided in Table 5. Each test sample (Test Nos. R8-R11) and control formulation (Control Nos. C6-C14) contained a total of 20.1 grams (1.0 phr) of processing aid. The processing aid in Control Nos. C6-C9 and C11-C13 was a conventional acrylic polymer (Plastistrength® 550, Arkema Inc., King of Prussia, PA). Control Nos. C7-C10 utilized an impact modifier (Paraloid™ EXL-5136, Dow Chemical Co., Midland, MI). The impact modifier is a polymeric core / shell impact modifier having a core of poly(butyl acrylate) and a shell of poly(methyl acrylate). Controls C11-C14 utilized a different impact modifier (Altuglas® BS-130, Arkema Inc., King of Prussia, PA). This impact modifier is a crosslinked poly(methyl methacrylate) particle having an average size of a few microns. The f-PA used in Test No. R8 consisted entirely of a processing aid functionalized with acrylic acid (AA) in Run 2. Similarly, the f-PA used in Test No. R9 consisted entirely of a processing aid functionalized with glycidyl methacrylate (GMA) in Run 2. The f-PA used in Test No. R10 consisted of a 50:50 mixture of AA-functionalized and GMA-functionalized processing aids in Run 2. Finally, the f-PA used in Run No. R11 consisted of a 50:50 mixture of the processing aid functionalized with AA in Run 2 and a conventional acrylic polymer (Plastistrength® 550, Arkema Inc., King of Prussia, PA).

[0079] [Table 5]

[0080] The PVC formulations containing the impact modifiers and / or processing aids were then evaluated using a Brabender rheometer and injection molded bars or plaques formed therefrom were tested for density, Gardner impact, and surface gloss at various angles. A summary of bulk density, melt time, melt torque, melt temperature, and equilibrium torque is provided in Table 6. The test samples (Test Nos. R8-R11) and comparative samples (Control Nos. C6-C14) were observed to exhibit similar properties with respect to density, melt time, melt torque, and melt temperature. However, the test samples (Test Nos. R8-R11) were found to exhibit a substantial enhancement in equilibrium torque versus the comparative samples (Control Nos. C6-C14). Thus, PVC formulations containing functionalized processing aids (Test Nos. R8-R10) or mixtures of functionalized and non-functionalized processing aids (Test No. R11) exhibit better mechanical properties than PVC formulations containing non-functionalized processing aids (Control No. C6) or mixtures of conventional, non-functionalized processing aids and impact modifiers (Control Nos. C7-C9 and C11-C13), or impact modifiers alone (Control Nos. C10 and C14).

[0081] [Table 6]

[0082] The PVC formulations containing functionalized processing aids (Test Nos. R8-R11) and PVC formulations containing conventional processing aids and / or impact modifiers (Control Nos. C5-C14) were then formed into sheets (0.040 in. x 6 ft.) using a Brabender conical twin screw extruder and the surface gloss of the sheets was measured at a 60° angle. A summary of the average gloss measurements obtained for each test sample is provided below in Table 7. The reported average gloss represents the average of 20 measurements taken from the top and bottom of the sheet.

[0083] All of the test sheets containing functionalized processing aids (Test Nos. R8-R11) exhibited either reduced gloss or improved impact properties when compared to the gloss measured for the comparative sheets (Control Nos. C6-C14) containing non-functionalized processing aids, conventional impact modifiers, or mixtures thereof. The test sheets (Test Nos. R3-R7) exhibited improved Gardner impact versus the control sheets containing only conventional impact modifiers (Control Nos. C10 and C14) or mixtures of impact modifiers and conventional processing aids (Control Nos. C7-C9 and C11-C13). In addition, the test sheets (Test Nos. R3-R7) exhibited a reduction in gloss measured on the top of the sheet on the order of about 10 points or more at a 60° angle compared to the comparative sheets (Control Nos. C6-C14). Similarly, the test sheets (Test Nos. R3-R7) exhibited the same or lower level of gloss measured on the bottom of the sheet when compared to the comparison sheets (Control Nos. C6-C14) at a 60° angle.

[0084] [Table 7]

[0085] This example demonstrates that PVC formulations incorporating functionalized processing aids can be formed into PVC parts that exhibit reduced gloss or improved impact properties at a 60° angle when compared to similar PVC parts containing a conventional non-functionalized processing aid alone, a mixture of a conventional processing aid and an impact modifier, or an impact modifier alone. This example further demonstrates that functionalization of the processing aid can be accomplished with GMA, AA, or a mixture thereof. Finally, this example demonstrates the improved performance of PVC parts comprising functionalized processing aids when compared to current matting technology (Control Nos. C7-C14) currently commercially utilized in the PVC window, door, and siding capstock industry.

[0086] Although the embodiments have been described herein in a manner that enables a clear and concise specification to be written, it is intended and understood that the embodiments may be variously combined or separated without departing from the invention, For example, it will be understood that all preferred features described herein are applicable to all aspects of the invention described herein.

[0087] The foregoing description of various forms of the invention has been presented for purposes of illustration and description. It is not intended to be exhaustive or to limit the invention to the precise form disclosed. Numerous modifications or variations are possible in light of the above teachings. The forms discussed have been chosen and described to provide the best illustration of the principles of the invention and its practical application, thereby enabling those skilled in the art to utilize the invention in various forms and with various modifications suited to the particular uses contemplated. All such modifications and variations are within the scope of the invention, as determined by the appended claims, when interpreted in accordance with the breadth to which they are fairly, legally and equitably entitled.

[0088] Example 8 (Prophetic Example) - PVC-acrylic formulation prepared and tested using the processing aids prepared in Run 2. A 1,262 gram (63.1 phr) masterbatch of polyvinyl chloride (PVC) formulation is prepared comprising 1,000 grams (50 phr) PVC resin (SE-950, Shintech Inc., Houston, TX), 24 grams (1.2 phr) tin stabilizer (Thermolite® 172, PMC Group Inc., Mount Laurel, NJ), 24 grams (1.2 phr) lubricant (Rheolub® RL-165 Honeywell International Inc., NJ), 12 grams (0.6 phr) calcium stearate, 2 grams (0.1 phr) of a second polyethylene lubricant (AC629A, Honeywell International Inc., NJ), and 200 grams (10 phr) titanium dioxide.

[0089] In addition to the PVC masterbatch, 1,000 grams (50 phr) of acrylic resin (Solarkote® PB, Arkema Inc., King of Prussia, PA) and 100 grams (5 phr) of the processing aid from that prepared in Example 2 are added and blended together to form a PVC-acrylic formulation.

[0090] Example 9 (Prophetic Example) - An acrylic formulation prepared and tested using the processing aids prepared in Run 2. To prepare the acrylic formulation, add 100 grams (5 phr) of the processing aid from that prepared in Example 2 to 2,000 grams (100 phr) of acrylic resin (Solarkote® P600, Arkema Inc., King of Prussia, PA).

Claims

1. 1. A polyvinyl chloride (PVC) part having reduced surface gloss comprising a PVC resin, one or more processing aids comprising at least one base polymer, and optionally one or more impact modifiers, comprising: the one or more processing aids are functionalized with reactive epoxy or hydroxyl functional groups, the reactive epoxy or hydroxyl functional groups being from 0.5 to 35 weight percent based on the total weight of the functionalized processing aid monomer mixture; the base polymer of the one or more processing aids comprises an acrylic or (meth)acrylic polymer or copolymer; the one or more processing aids have a molecular weight (M) greater than 50,000 g / mol; a portion of the one or more processing aids is insoluble in acetone, THF, and MEK, the insoluble fraction being in the range of 1% to 90%; The PVC part exhibits at least a 5 point reduction in gloss when measured at an angle of 85 degrees or less compared to an otherwise similar PVC part in which the processing aid is not functionalized.

2. 10. The PVC part of claim 1, further comprising one or more inorganic fillers or particles.

3. 3. The PVC part of claim 2, wherein the one or more inorganic fillers or particles are selected from the group consisting of calcium carbonate, kaolin clay, talc, mica, wollastonite, and calcium metasilicate.

4. 3. The PVC part of claim 2, wherein the one or more inorganic fillers or particles are calcium carbonate.

5. 10. The PVC part of claim 1, wherein the processing aid is present at 0.1 to 12 phr.

6. 2. The PVC part of claim 1, wherein said one or more processing aids are functionalized with at least 5% by weight of said reactive epoxy or hydroxyl functional groups, based on the total weight of the functionalized processing aid monomer mix.

7. 10. The PVC part of claim 1, wherein the processing aid exhibits at least a 10 point reduction in gloss when measured at an angle of 60 degrees or less compared to an otherwise similar PVC part that is not functionalized.

8. 2. The PVC part of claim 1, wherein the reactive epoxy or hydroxyl functionality is derived from a hydroxyl-substituted alkyl ester of (meth)acrylic acid, or an epoxy group-containing monomer.

9. 10. The PVC part of claim 1, wherein the base polymer of the one or more processing aids comprises an acrylic polymer or copolymer.

10. The one or more processing aids have a molecular weight (M w 2. The PVC part of claim 1, having a thickness of 100 mm.

11. The PVC part of claim 9, wherein the base polymer of the one or more processing aids comprises an acrylic copolymer, the acrylic copolymer being derived from a (meth)acrylic-containing monomer and a vinyl-containing monomer; styrene or a styrene derivative; an olefin; a diene; or mixtures thereof.

12. 13. Packaging for an automotive product, a building material, a household or kitchen item, a medical or office product, an article of clothing, or a personal care product or other consumer product comprising the PVC part of claim 1.

Citation Information

Patent Citations

  • Vinyl chloride based resin composition

    JP1987138546A

  • Crosslinkable plastisol

    JP1992300939A

  • Gloss-reducing polymer composition

    JP2006089740A

  • Methacrylate Copolymer for Processing Aids of Vinylchloride Resin and Method for Production Thereof

    KR101030513B1

  • Blend of particulated polyvinyl chloride, and a terpolymer of methyl methacrylate, ethyl acrylate, and glycidyl acrylate

    US3301919A