Thermoplastic Polyurethane
Thermoplastic polyurethanes formulated with aliphatic dicarboxylic acids and specific diols address the blooming issue and maintain mechanical integrity, offering improved visual and performance characteristics.
Patent Information
- Application Number
- JP2022202354
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2017-06-26
- Filing Date
- 2022-12-19
- Publication Date
- 2024-12-04
- Estimated Expiration
- 2038-06-26
AI Technical Summary
Existing thermoplastic polyurethanes face issues with strong blooming, which leads to a white coating that makes them visually unacceptable for many applications, while also having insufficient mechanical properties.
The development of thermoplastic polyurethanes using a polyisocyanate composition, chain extender, and a polyol composition, where the polyol is derived from reacting aliphatic dicarboxylic acids with propane-1,3-diol and a further diol, such as butane-1,4-diol, to create a polyester polyol with reduced blooming and improved mechanical properties.
The resulting thermoplastic polyurethanes exhibit a significantly reduced tendency to bloom and maintain good mechanical properties, making them suitable for various applications without the visual defects of previous formulations.
Smart Images

Figure 0007594575000001 
Figure 0007594575000002 
Figure 0007594575000003
Abstract
Description
[Technical field]
[0001] The present invention relates to thermoplastic polyurethanes obtainable or obtainable by reacting at least one polyisocyanate composition comprising at least one polyisocyanate, at least one chain extender and at least one polyol composition, the polyol composition comprising at least one polyester polyol (P1) obtainable by reacting an aliphatic dicarboxylic acid having 2 to 12 carbon atoms with a mixture (M1) comprising propane-1,3-diol and a further diol (D1) having 2 to 12 carbon atoms, preferably butane-1,4-diol. The present invention also relates to a process for the preparation of such a thermoplastic polyurethane and to a process for the use of the thermoplastic polyurethanes of the present invention, or of the thermoplastic polyurethanes obtainable or obtainable by the process of the present invention, for producing extrusion products, films and mouldings or for producing polymer compositions. The polyurethanes according to the present invention show a low tendency to bloom. [Background technology]
[0002] Thermoplastic polyurethanes for various applications are in principle known from the prior art. By varying the feedstock, it is possible to obtain different property profiles. Due to their beneficial properties, polyester polyols are used in particular for high-quality polyurethane products.
[0003] For example, US5695884 discloses the use of polyester polyols based on sebacic acid for thermoplastic polyurethanes with high crystallinity. US 2006 / 0141883A1 and US2006 / 0121812 also describe the use of polyester polyols based on sebacic acid for polyurethanes for fibers with high melting points. WO00 / 51660A1 describes polyurethanes for cardiac catheters that can use polyester polyols based on sebacic acid. Here too, sufficient hardness is required.
[0004] However, the use of polyester polyols in the preparation of polyurethanes increasingly leads to a very strong bloom problem, i.e. the formation of a white coating on the processed polyurethane, which is no longer visually acceptable for many potential applications.
[0005] WO2010 / 107562A1 discloses thermoplastic polyurethanes obtained from the reaction product of propane-1,3-diol and dicarboxylic acid. This document states that the polyurethanes obtained or obtainable using homopolyesters based on adipic acid and propanediol have less bloom than the corresponding polyurethanes obtained or obtainable using homopolyesters based on adipic acid and butanediol.
[0006] However, for many applications the mechanical properties described in the above mentioned documents are insufficient. [Prior art documents] [Patent documents]
[0007] [Patent Document 1] US5695884 [Patent Document 2] US2006 / 0141883A1 [Patent Document 3] US2006 / 0121812 [Patent Document 4] WO00 / 51660A1 [Patent Document 5] WO2010 / 107562A1 Summary of the Invention [Problem to be solved by the invention]
[0008] It is an object of the present invention to provide a thermoplastic polyurethane which has good mechanical properties and further has a reduced tendency to bloom. [Means for solving the problem]
[0009] According to the invention, this object is achieved by providing at least components (i) to (iii): (i) a polyisocyanate composition comprising at least one polyisocyanate; (ii) at least one chain extender, and (iii) at least one polyol composition; wherein the polyol composition comprises at least one polyester polyol (P1) obtainable by reacting an aliphatic dicarboxylic acid having from 2 to 12 carbon atoms with a mixture (M1) comprising propane-1,3-diol and a further diol (D1) having from 2 to 12 carbon atoms.
[0010] Surprisingly, it has been found that the thermoplastic polyurethanes of the invention based on polyesters of polyol mixtures comprising propane-1,3-diol and a further diol (D1) having 2 to 12 carbon atoms have a significantly reduced tendency to bloom compared to those based on polyesters of pure diols, while at the same time having good mechanical properties comparable to commercially available thermoplastic polyurethanes.
[0011] According to the invention, at least components (i) to (iii) are reacted. For the preparation of the polyurethanes according to the invention, a polyol composition is used which comprises at least one polyester polyol (P1) obtainable by reacting an aliphatic dicarboxylic acid having 2 to 12 carbon atoms with a mixture (M1) comprising propane-1,3-diol and a further diol (D1) having 2 to 12 carbon atoms.
[0012] The mixture (M1) comprises propane-1,3-diol and a further diol (D1) having 2 to 12 carbon atoms. The diol (D1) is preferably selected from the group consisting of ethylene glycol, butane-1,4-diol and hexane-1,6-diol. According to the invention, butane-1,4-diol is particularly preferred. According to the invention, the mixture (M1) may also comprise, in addition to propane-1,3-diol, two or more diols having 2 to 12 carbon atoms.
[0013] Thus, in a further embodiment, the present invention relates to a thermoplastic polyurethane as described above, wherein the diol (D1) is selected from the group consisting of ethylene glycol, butane-1,4-diol and hexane-1,6-diol. In a further embodiment, the present invention relates to a thermoplastic polyurethane as described above, wherein the diol (D1) is butane-1,4-diol. Thus, the present invention relates to a thermoplastic polyurethane as described above, comprising at least components (i) to (iii): (i) a polyisocyanate composition comprising at least one polyisocyanate; (ii) at least one chain extender, and (iii) at least one polyol composition; wherein the polyol composition comprises at least one polyester polyol (P1) obtainable by reacting an aliphatic dicarboxylic acid having 2 to 12 carbon atoms with a mixture (M1) comprising propane-1,3-diol and butane-1,4-diol.
[0014] According to the invention, it is possible in principle to use any suitable polyesterol known to the skilled person. According to the invention, the polyester polyol used in this case preferably has an average functionality in the range of 1.8 to 2.3, preferably in the range of 1.9 to 2.2, in particular 2. The polyester polyol of the invention is preferably a polyester diol.
[0015] Suitable molecular weight ranges for the polyester polyols used according to the invention are known per se to the person skilled in the art. In a preferred embodiment, the molecular weight of the polyester polyols is in the range from 750 to 3000 g / mol, particularly preferably in the range from 800 to 2500 g / mol and very particularly preferably in the range from 1000 to 2000 g / mol.
[0016] In a further embodiment, the present invention therefore relates to a thermoplastic polyurethane as defined above, wherein the polyester polyol (P1) has a molecular weight Mw in the range from 750 to 3000 g / mol.
[0017] Particularly suitable polyester polyols according to the invention have OH numbers in the range from 25 to 230 mg KOH / g, particularly preferably in the range from 35 to 140 mg KOH / g and very particularly preferably in the range from 40 to 115 mg KOH / g.
[0018] According to the invention, the polyester polyols (P1) are obtainable or are obtained by reacting an aliphatic dicarboxylic acid having from 2 to 12 carbon atoms with a mixture (M1) comprising propane-1,3-diol and a further diol (D1) having from 2 to 12 carbon atoms, preferably butane-1,4-diol.
[0019] In the present invention, the mixing ratio of propane-1,3-diol and diol (D1) in the mixture (M1) can vary within wide limits. For example, the ratio of propane-1,3-diol and diol (D1) can range from 3:1 to 1:3. According to the present invention, the ratio of propane-1,3-diol and butane-1,4-diol can in particular range from 3:1 to 1:3.
[0020] In a further embodiment, the present invention therefore relates to a thermoplastic polyurethane as defined above, wherein the mixture (M1) comprises propane-1,3-diol and diol (D1) in a ratio ranging from 3:1 to 1:3.In a further embodiment, the present invention also relates to a thermoplastic polyurethane as defined above, wherein the mixture (M1) comprises propane-1,3-diol and butane-1,4-diol in a ratio ranging from 3:1 to 1:3.
[0021] According to the invention, the ratio of propane-1,3-diol and diol (D1), in particular the ratio of propane-1,3-diol and butane-1,4-diol, may for example be in the range from 2.5:1 to 1:2.5, or in the range from 2:1 to 1:2, or in the range from 1.5:1 to 1:1.5, or 1:1.
[0022] The mixture (M1) may here comprise further components, such as solvents or further polyhydric alcohols. Suitable polyhydric alcohols are, for example, polyhydric aliphatic alcohols, for example aliphatic alcohols having 2, 3, 4 or more OH groups, for example 2 or 3 OH groups. Suitable aliphatic alcohols according to the invention are, for example, C2-C12 alcohols, preferably C2-C8 alcohols, and very particularly preferably C2-C6 alcohols. Suitable further aliphatic C2-C6 diols are, for example, diethylene glycol, 3-oxapentane-1,5-diol, propane-1,2-diol, dipropylene glycol, pentane-1,5-diol, 2-methylpropane-1,3-diol and 3-methylpentane-1,5-diol.
[0023] In a further embodiment, the present invention therefore relates to a thermoplastic polyurethane as described above, wherein mixture (M1) comprises a further diol.
[0024] Preferably, the mixture (M1) does not comprise any further alcohols other than propane-1,3-diol and diol (D1), in particular other than propane-1,3-diol and butane-1,4-diol. In a particularly preferred embodiment, the mixture (M1) does not comprise any further components other than propane-1,3-diol and diol (D1), in particular other than propane-1,3-diol and butane-1,4-diol.
[0025] According to the invention, it is also possible to use propanediol and / or further diols, such as butanediol, which are at least partially obtained from renewable raw materials. In this case, the polyhydric alcohols can be partially or completely obtained from renewable raw materials. According to the invention, at least one of the polyhydric alcohols used may be at least partially obtained from renewable raw materials.
[0026] The propane-1,3-diol may thus be a synthetically prepared propane-1,3-diol, but in particular a propane-1,3-diol from renewable raw materials ("biopropane-1,3-diol"). Biopropane-1,3-diol can be obtained, for example, from corn and / or sugar. A further possibility is the conversion of glycerol waste from biodiesel production. In a further preferred embodiment of the invention, the polyhydric alcohol is a propane-1,3-diol obtained at least in part from renewable raw materials.
[0027] In a further embodiment, the present invention also relates to the above polyurethanes, wherein the at least one polyhydric alcohol is propane-1,3-diol obtained at least in part from renewable raw materials.
[0028] According to the invention, aliphatic dicarboxylic acids having 2 to 12 carbon atoms are used to prepare the polyester polyols (P1).
[0029] According to the invention, the dicarboxylic acid used can be linear or branched. According to the invention, the dicarboxylic acid is preferably selected from dicarboxylic acids having 4 to 12 carbon atoms, particularly preferably from dicarboxylic acids having 6 to 10 carbon atoms. According to the invention, the dicarboxylic acid used is particularly preferably adipic acid. According to the invention, it is also possible to use a mixture of two or more of the mentioned dicarboxylic acids.
[0030] Thus, in a further embodiment, the present invention relates to the above thermoplastic polyurethanes, wherein the aliphatic dicarboxylic acid is adipic acid.
[0031] In a preferred embodiment of the present invention, no further components are used to prepare the polyester polyol (P1) other than the mixture (M1) and the aliphatic dicarboxylic acid having 2 to 12 carbon atoms. Thus, in a particularly preferred embodiment of the present invention, the polyester polyol (P1) is prepared using adipic acid and a mixture (M1) consisting of propane-1,3-diol and a diol (D1).
[0032] For the preparation of the thermoplastic polyurethanes of the present invention, at least one chain extender is used as component (ii).
[0033] Suitable chain extenders are known in principle to those skilled in the art. Examples of suitable compounds are those that have at least two isocyanate-reactive functional groups, such as hydroxyl, amino or thiol groups. Thus, in a further embodiment, the present invention relates to the above-mentioned thermoplastic polyurethanes, which use at least one chain extender selected from the group consisting of compounds that have at least two isocyanate-reactive functional groups.
[0034] Examples of suitable chain extenders are compounds selected from the group consisting of aliphatic and aromatic diols with a molecular weight of <500 g / mol, preferably <350 g / mol. In a further embodiment, the present invention also relates to the above-mentioned thermoplastic polyurethanes, which use at least one further chain extender (KV2) selected from the group consisting of aliphatic and aromatic diols with a molecular weight of <500 g / mol.
[0035] According to the invention, the further chain extenders (KV2) used are preferably diols. Here, aliphatic, araliphatic, aromatic and / or cycloaliphatic diols having a molecular weight of 50 g / mol to 220 g / mol can be preferably used. Preference is given to alkanediols having 2 to 10 carbon atoms in the alkylene radical, in particular di-, tri-, tetra-, penta-, hexa-, hepta-, octa-, nona- and / or decaalkylene glycols. Particular preference is given according to the invention to 1,2-ethylene glycol, butane-1,4-diol, hexane-1,6-diol and hydroquinone bis(2-hydroxyethyl) ether.
[0036] In the present invention, branched-chain compounds such as cyclohexane-1,4-dimethanol, 2-butyl-2-ethylpropanediol, neopentyl glycol, 2,2,4-trimethylpentane-1,3-diol, pinacol, 2-ethylhexane-1,3-diol, cyclohexane-1,4-diol or N-phenyldiethanolamine are also suitable as chain extenders. Also suitable are mixed compounds such as, for example, 4-aminobutanol.
[0037] In the present invention, the amounts of chain extender and polyol composition used may vary within wide limits, for example, components (iii) and (ii) are used in molar ratios of (iii) to (ii) of 1:0.7, 1:2.7 and 1:7.3.
[0038] According to the invention, the polyol composition comprises at least one polyester polyol (P1). According to the invention, the polyol composition may comprise further polyols. Suitable polyols are known in principle to the person skilled in the art and are described, for example, in "Kunststoffhandbuch [Plastics Handbook], Volume 7, Polyurethane [Polyurethane]", Carl Hanser Verlag, 3rd Edition 1993, Chapter 3.1. It is particularly preferred to use polyesterols or polyetherols as polyols. It is also possible to use polycarbonates. Copolymers may also be used in the present invention. The number-average molecular weight of the polyols used according to the invention is preferably 0.5x10 3 g / mol~8x10 3 g / mol, preferably between 0.6x10 3 g / mol~5x10 3 Between g / mol, specifically 0.8x10 3 g / mol~3x10 3 g / mol.
[0039] According to the invention, polyetherols are suitable, as well as polyesterols, block copolymers and hybrid polyols such as poly(ester / amides). Preferred polyetherols according to the invention are polyethylene glycols, polypropylene glycols, polyadipates, polycarbonates, polycarbonate diols and polycaprolactones.
[0040] In a further embodiment, the present invention also relates to the above thermoplastic polyurethane, wherein the polyol composition comprises a polyol selected from the group consisting of polyetherols, polyesterols, polycaprolactones, and polycarbonates.
[0041] Suitable block copolymers are, for example, those with ether and ester blocks, such as polycaprolactones with polyethylene oxide or polypropylene oxide end blocks, or polyethers with polycaprolactone end blocks. According to the invention, preferred polyetherols are polyethylene glycol and polypropylene glycol. Polycaprolactone is also preferred.
[0042] The polyol composition preferably has an average functionality of 1.8 to 2.3, preferably 1.9 to 2.2, in particular 2. The polyols used according to the invention preferably have only primary hydroxyl groups.
[0043] According to the invention, the polyol composition may also comprise a solvent. Suitable solvents are known per se to those skilled in the art.
[0044] According to the present invention, component (i) used in the preparation of the thermoplastic polyurethane is a polyisocyanate composition comprising at least one polyisocyanate. The preferred polyisocyanates according to the present invention are diisocyanates, in particular aliphatic or aromatic diisocyanates, more preferably aromatic diisocyanates.
[0045] Thus, in a further embodiment, the present invention relates to a thermoplastic polyurethane as described above, wherein the polyisocyanate is an aliphatic or aromatic diisocyanate.
[0046] Furthermore, in the present invention, the pre-reaction product may be used as the isocyanate component, where a portion of the OH component is reacted with an isocyanate in a preceding reaction step, and the resulting product is reacted with the remaining OH component in a subsequent step, which is the actual polymer reaction, thereby forming a thermoplastic polyurethane.
[0047] The aliphatic diisocyanates used are the usual aliphatic and / or cycloaliphatic diisocyanates, such as tri-, tetra-, penta-, hexa-, hepta- and / or octamethylene diisocyanate, 2-methylpentamethylene 1,5-diisocyanate, 2-ethyltetramethylene 1,4-diisocyanate, hexamethylene 1,6-diisocyanate (HDI), pentamethylene 1,5-diisocyanate, butylene 1,4-diisocyanate, trimethylhexamethylene 1,6-diisocyanate, cyanate, 1-isocyanato-3,3,5-trimethyl-5-isocyanatomethylcyclohexane (isophorone diisocyanate, IPDI), 1,4- and / or 1,3-bis(isocyanatomethyl)cyclohexane (HXDI), cyclohexane 1,4-diisocyanate, 1-methyl-2,4- and / or 1-methylcyclohexane 2,6-diisocyanate, methylene dicyclohexyl 4,4'-, 2,4'- and / or 2,2'-diisocyanate (H12MDI).
[0048] Preferred aliphatic polyisocyanates are hexamethylene 1,6-diisocyanate (HDI), 1-isocyanato-3,3,5-trimethyl-5-isocyanatomethylcyclohexane and methylenedicyclohexyl 4,4'-, 2,4'- and / or 2,2'-diisocyanate (H12MDI).
[0049] Preferred aliphatic polyisocyanates are hexamethylene 1,6-diisocyanate (HDI), 1-isocyanato-3,3,5-trimethyl-5-isocyanatomethylcyclohexane and methylene dicyclohexyl 4,4'-, 2,4'- and / or 2,2'-diisocyanate (H12MDI), particularly preferred are methylene dicyclohexyl 4,4'-, 2,4'- and / or 2,2'-diisocyanate (H12MDI) and 1-isocyanato-3,3,5-trimethyl-5-isocyanatomethylcyclohexane or mixtures thereof.
[0050] Suitable aromatic diisocyanates are in particular naphthylene 1,5-diisocyanate (NDI), tolylene 2,4- and / or 2,6-diisocyanate (TDI), diphenylmethane 2,2'-, 2,4'- and / or 4,4'-diisocyanate (MDI), 3,3'-dimethyl-4,4'-diisocyanatodiphenyl (TODI), p-phenylene diisocyanate (PDI), diphenylethane 4,4'-diisocyanate (EDI), diphenylmethane diisocyanate, 3,3'-dimethyldiphenyl diisocyanate, diphenylethane 1,2-diisocyanate and / or phenylene diisocyanate.
[0051] Thus, in a further embodiment, the present invention relates to a thermoplastic polyurethane as described above, wherein the polyisocyanate is selected from the group consisting of methylene diphenyl diisocyanate (MDI), tolylene 2,4- and / or 2,6-diisocyanate (TDI), hexamethylene 1,6-diisocyanate (HDI), methylene dicyclohexyl 4,4'-, 2,4'- and / or 2,2'-diisocyanate (H12MDI) and isophorone diisocyanate (IPDI).
[0052] Preferred examples of isocyanates of higher functionality are triisocyanates, such as triphenylmethane 4,4',4"-triisocyanate, the cyanurates of the aforementioned diisocyanates, and oligomers obtainable by partial reaction of diisocyanates with water, such as biurets of the aforementioned diisocyanates, and also oligomers obtainable by specific reaction of semi-blocked diisocyanates with polyols having on average more than 2, preferably more than 3, hydroxyl groups.
[0053] According to the present invention, the polyisocyanate composition may also contain one or more solvents. Suitable solvents are known to those skilled in the art. Suitable examples are non-reactive solvents such as ethyl acetate, methyl ethyl ketone, and hydrocarbons.
[0054] Further usable in the present invention are crosslinking agents, such as the higher functionality polyisocyanates or polyols mentioned above, or other higher functionality molecules having multiple isocyanate-reactive functional groups. It is also possible in the present invention to achieve crosslinking of the product via the use of an excess of isocyanate groups in proportion to the hydroxyl groups.
[0055] According to the present invention, components (i) to (iii) are used in such a ratio that the molar ratio of the sum of the functionalities of the polyol composition and the chain extender used to the sum of the functionalities of the isocyanate composition used is in the range of 1:0.8 to 1:1.3. The ratio is preferably in the range of 1:0.9 to 1:1.2, more preferably in the range of 1:0.965 to 1:1.11, more preferably in the range of 1:0.97 to 1:1.11, more preferably in the range of 1:0.97 to 1:1.05, and particularly preferably in the range of 1:0.98 to 1:1.03.
[0056] In a further embodiment, the present invention relates to the above thermoplastic polyurethane, wherein the molar ratio of the sum of the functionalities of the polyol composition and the chain extender used to the sum of the functionality of the isocyanate composition used is in the range of 1:0.8 to 1:1.3.
[0057] A further parameter to be taken into account in the reaction of components (i) to (iii) is the isocyanate index. The index is in this case defined by the ratio of isocyanate-reactive groups, i.e. specifically groups of components (ii) and (iii), to the total isocyanate groups of component (i) used in the reaction. At an index of 1000 there is one active hydrogen atom for each isocyanate group of component (i). At an index of more than 1000 there are more isocyanate groups than isocyanate-reactive groups. The index in the reaction of components (i) to (iii) is preferably in the range of 965 to 1110, for example in the range of 970 to 1110, more preferably in the range of 970 to 1050, particularly preferably in the range of 980 to 1030.
[0058] In a further embodiment, the present invention relates to the above thermoplastic polyurethane, having a reaction index in the range of 965 to 1100.
[0059] According to the present invention, further additives, such as catalysts or auxiliaries and additives, may be added during the reaction of components (i) to (iii). Additives and auxiliaries are known per se to those skilled in the art. According to the present invention, it is also possible to use a combination of two or more additives.
[0060] In the context of the present invention, the term "additives" is understood to mean in particular catalysts, auxiliaries and additions, especially stabilizers, nucleating agents, release agents, release aids, fillers, flame retardants or crosslinking agents.
[0061] Suitable additives or additions are, for example, stabilizers, nucleating agents, fillers, such as silicates, or crosslinking agents, such as polyfunctional aluminosilicates.
[0062] Thus, in a further embodiment, the present invention relates to the above thermoplastic polyurethane, wherein the thermoplastic polyurethane comprises at least one additive.
[0063] Examples of auxiliaries and additives include surface-active substances, flame retardants, nucleating agents, oxidation stabilizers, antioxidants, lubricants and release aids, dyes and pigments, stabilizers (e.g. against hydrolysis, light, heat or discoloration), inorganic and / or organic fillers, reinforcing agents, plasticizers. Suitable auxiliaries and additives can be found, for example, in Kunststoffhandbuch [Plastics Handbook], Vol. VII, edited by Vieweg and Hoechtlen, Carl Hanser Verlag, Munich, 1966 (pages 103 to 113).
[0064] Suitable catalysts are also known in principle from the prior art.Suitable catalysts are, for example, organometallic compounds selected from the group consisting of tin, titanium, zirconium, hafnium, bismuth, zinc, aluminum and iron organyls, such as tin organyl compounds, preferably dialkyltins, such as dimethyltin or diethyltin, or tin organyl compounds of aliphatic carboxylic acids, preferably tin diacetate, tin dilaurate, dibutyltin diacetate, dibutyltin dilaurate, bismuth compounds, such as bismuth alkyl compounds, or iron compounds, preferably iron(MI) acetylacetonate, or metal salts of carboxylic acids, such as tin(II) isooctate, tin dioctoate, titanate esters or bismuth(III) neodecanoate.
[0065] In a preferred embodiment, the catalyst is selected from tin and bismuth compounds, more preferably a tin or bismuth alkyl compound, with tin(II) isooctanoate and bismuth neodecanoate being particularly suitable.
[0066] The catalyst is usually used in an amount of 0 to 2000 ppm, preferably 1 ppm to 1000 ppm, more preferably 2 ppm to 500 ppm, and most preferably 5 ppm to 300 ppm.
[0067] The properties of the thermoplastic polyurethanes of the present invention may vary within wide limits depending on the application.
[0068] In a further aspect, the present invention provides a composition comprising at least components (i)-(iii): (i) a polyisocyanate composition comprising at least one polyisocyanate; (ii) at least one chain extender, and (iii) at least one polyol composition; The present invention relates to a method for preparing a thermoplastic polyurethane, comprising the reaction of The polyol composition here comprises at least one polyester polyol (P1) obtainable by reacting an aliphatic dicarboxylic acid having from 2 to 12 carbon atoms with a mixture (M1) comprising propane-1,3-diol and a further diol (D1) having from 2 to 12 carbon atoms.
[0069] Regarding preferred embodiments of the process, suitable feedstocks or mixing ratios, please refer to the corresponding remarks above.
[0070] The reaction of components (i) to (iii) can be carried out under reaction conditions known per se in principle. In this case, the reaction can be carried out batchwise or continuously, for example in a belt process or a reactive extrusion process. Suitable processes are described, for example, in EP 0922552 A1 or WO 2006 / 082183 A1.
[0071] The polyurethanes can be produced by known processes, discontinuously or continuously, for example using a reactive extruder, or a one-shot belt process or a prepolymer process, preferably by a one-shot process. In these processes, the components to be reacted are mixed with each other continuously or simultaneously and the reaction starts immediately. In the extruder process, the synthesis components and optionally chain extenders, catalysts and / or additives are introduced individually or as a mixture into an extruder and reacted at temperatures of, for example, 100 to 280° C., preferably 140 to 250° C., and the polyurethane obtained is extruded, cooled and pelletized.
[0072] In a preferred embodiment, the reaction of components (i)-(iii) is carried out at a temperature above room temperature.
[0073] According to the invention, heating may be carried out in any suitable manner known to the skilled artisan. The feedstock may be preferably heated before addition, for example using a heatable metering unit.
[0074] For example, in reactions using a reactive extrusion process, the reaction is carried out such that the zone temperatures are in the range of 170°C to 245°C, preferably in the range of 180°C to 235°C, and more preferably in the range of 190°C to 230°C.
[0075] According to the invention, it is also possible for the process to comprise further steps, for example for pre-treatment of the components or post-treatment of the resulting thermoplastic polyurethane.In a further embodiment, the invention thus also relates to a process for the preparation of a thermoplastic polyurethane as described above, in which the resulting thermoplastic polyurethane is heat-treated after the reaction.
[0076] The polyurethanes according to the invention are usually present in the form of granules or powders, from which the desired films, moldings, rolls, fibers, automotive trims, hoses, cable connectors, bellows, trailing cables, cable jackets, seals, belts or damping elements are obtained. The processing of the polyurethanes according to the invention is carried out by customary methods, such as injection molding, calendering, extrusion, etc.
[0077] The thermoplastic polyurethane of the present invention / thermoplastic polyurethane obtained or obtainable by the method of the present invention can be used in a wide variety of ways.The thermoplastic polyurethane of the present invention is particularly suitable for the manufacture of molded articles and films.Possible applications are, for example, seals, sealing rings, gaskets, sealing washers, sealing agents, sealing compositions, sealants or outer soles for shoes.Further applications are, for example, hoses, conveyor belts, films, packaging materials, cables, flooring applications, shock absorbers and sound absorbers, among others, for pneumatic applications.
[0078] In a further aspect, the present invention relates to the use of the above-mentioned thermoplastic polyurethanes or of the thermoplastic polyurethanes obtainable or obtainable by the process of the present invention for producing extrusion products, films and mouldings, in particular for producing cable jackets, hoses, seals.
[0079] Thus, the present invention provides: (a) At least components (i) to (iii): (i) a polyisocyanate composition comprising at least one polyisocyanate; (ii) at least one chain extender, and (iii) at least one polyol composition; A process for preparing a thermoplastic polyurethane comprising the reaction of preparing the polyol composition, which comprises at least one polyester polyol (P1) obtainable by reacting an aliphatic dicarboxylic acid having from 2 to 12 carbon atoms with a mixture (M1) comprising propane-1,3-diol and a further diol (D1) having from 2 to 12 carbon atoms, (b) a step of producing a molded body (SB) from a thermoplastic polyurethane; The present invention also relates to a method for producing the molded body (SB), comprising:
[0080] For preferred embodiments, see above. The commonly used methods for producing molded bodies (SB) from thermoplastic polyurethane as in step (b) are known per se to those skilled in the art. The method may also include further steps between steps (a) and (b), such as treatment or temperature treatment of the thermoplastic polyurethane.
[0081] In a further embodiment, the present invention also relates to the use of the thermoplastic polyurethanes described above or obtainable or obtainable by the process of the present invention for producing extruded products, films and mouldings, wherein the extruded products, films or sheets are reinforced with a filler.
[0082] Surprisingly, it has been found that the thermoplastic polyurethane of the present invention or the thermoplastic polyurethane obtained by the method of the present invention is well suited for the production of foamed materials.The thermoplastic polyurethane of the present invention can be processed into foamed materials in a manner known per se.Additives such as blowing agents, cell regulators, surface-active substances, nucleating agents, fillers, hollow microspheres and / or release agents are optionally used here.Suitable processing and additives are disclosed, for example, in WO2014 / 198779A1, WO2007 / 082838A1 or WO94 / 20568A1.
[0083] In a further aspect, the present invention therefore also relates to the use of the thermoplastic polyurethanes described above, or of the thermoplastic polyurethanes obtainable or obtainable by the process of the present invention, for producing foamed films, foamed moulded articles or foamed particles, or of particle foams obtainable therefrom.
[0084] In a further embodiment, the present invention also relates to the use of the above-mentioned thermoplastic polyurethanes or of the thermoplastic polyurethanes obtainable or obtainable by the process of the present invention for producing foamed films, foamed moulded articles or expanded beads or particle foams obtainable therefrom, wherein the foamed films, foamed moulded articles or expanded beads and particle foams obtainable therefrom are reinforced with a filler.
[0085] In the present invention, the thermoplastic polyurethane of the present invention or the thermoplastic polyurethane obtained or obtainable by the process of the present invention can also be used in a polymer composition or polymer blend. Such a polymer composition or polymer blend comprises the thermoplastic polyurethane of the present invention or the thermoplastic polyurethane obtained or obtainable by the process of the present invention and one or more further polymers. The present invention therefore also relates to the use of said thermoplastic polyurethane or the thermoplastic polyurethane obtainable or obtainable by the process of the present invention for the manufacture of a polymer composition.
[0086] Further embodiments of the invention can be found in the claims and the examples. It will be understood that the features of the subject matter / method / use according to the invention mentioned above and described below can in each case be used not only in the specified combination but also in other combinations without departing from the scope of the invention. For example, combinations of preferred features with particularly preferred features or combinations of features not further characterized as particularly preferred features etc. are implicitly encompassed even if this combination is not explicitly mentioned as such. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0087] Exemplary embodiments of the present invention are listed below without, however, limiting the present invention. In particular, the present invention also encompasses embodiments resulting from the combinations specified below by reference to dependencies.
[0088] 1. At least components (i) to (iii): (i) a polyisocyanate composition comprising at least one polyisocyanate; (ii) at least one chain extender, and (iii) at least one polyol composition; wherein the polyol composition comprises at least one polyester polyol (P1) obtainable by reacting an aliphatic dicarboxylic acid having from 2 to 12 carbon atoms with a mixture (M1) comprising propane-1,3-diol and a further diol (D1) having from 2 to 12 carbon atoms.
[0089] 2. The thermoplastic polyurethane of embodiment 1, wherein the diol (D1) is selected from the group consisting of ethylene glycol, butane-1,4-diol and hexane-1,6-diol.
[0090] 3. The thermoplastic polyurethane according to any one of the preceding embodiments, wherein the diol (D1) is butane-1,4-diol.
[0091] 4. A thermoplastic polyurethane described in any one of embodiments 1 to 3, wherein the aliphatic dicarboxylic acid is adipic acid.
[0092] 5. A thermoplastic polyurethane according to any one of the preceding embodiments, wherein the mixture (M1) comprises propane-1,3-diol and the diol (D1) in a ratio ranging from 3:1 to 1:3.
[0093] 6. A thermoplastic polyurethane according to any one of the preceding embodiments, wherein the mixture (M1) comprises a further diol.
[0094] 7. The thermoplastic polyurethane according to any one of the preceding embodiments, wherein the polyester polyol (P1) has a molecular weight Mw in the range of 750 to 3000 g / mol.
[0095] 8. A thermoplastic polyurethane according to any one of the preceding embodiments, wherein the chain extender used in (ii) is selected from the group consisting of aliphatic and aromatic diols having a molecular weight of <500 g / mol.
[0096] 9. The thermoplastic polyurethane of any one of embodiments 1 to 8, wherein the polyisocyanate is an aliphatic or aromatic diisocyanate.
[0097] 10. The thermoplastic polyurethane of any one of the preceding claims, wherein the polyisocyanate is selected from the group consisting of methylene diphenyl diisocyanate (MDI), tolylene 2,4- and / or 2,6-diisocyanate (TDI), hexamethylene 1,6-diisocyanate (HDI), methylene dicyclohexyl 4,4'-, 2,4'- and / or 2,2'-diisocyanate (H12MDI) and isophorone diisocyanate (IPDI).
[0098] 11. At least components (i) to (iii): (i) a polyisocyanate composition comprising at least one polyisocyanate; (ii) at least one chain extender, and (iii) at least one polyol composition; wherein the polyol composition comprises at least one polyester polyol (P1) obtainable by reacting an aliphatic dicarboxylic acid having from 2 to 12 carbon atoms with a mixture (M1) comprising propane-1,3-diol and a further diol (D1) having from 2 to 12 carbon atoms.
[0099] 12. The method of embodiment 11, wherein the diol (D1) is selected from the group consisting of ethylene glycol, butane-1,4-diol and hexane-1,6-diol.
[0100] 13. The method of embodiment 11, wherein the diol (D1) is butane-1,4-diol.
[0101] 14. The method of any one of embodiments 11 to 13, wherein the aliphatic dicarboxylic acid is adipic acid.
[0102] 15. The method according to any one of embodiments 11 to 14, wherein the mixture (M1) comprises propane-1,3-diol and the diol (D1) in a ratio ranging from 3:1 to 1:3.
[0103] 16. The method of any one of embodiments 11 to 15, wherein the mixture (M1) comprises a further diol.
[0104] 17. The method according to any one of embodiments 11 to 16, wherein the polyester polyol (P1) has a molecular weight Mw in the range of 750 to 3000 g / mol.
[0105] 18. The method according to any one of embodiments 11 to 17, wherein the chain extender used in (ii) is selected from the group consisting of aliphatic and aromatic diols having a molecular weight of <500 g / mol.
[0106] 19. The method of any one of embodiments 11 to 18, wherein the polyisocyanate is an aliphatic or aromatic diisocyanate.
[0107] 20. The method of any one of embodiments 11 to 19, wherein the polyisocyanate is selected from the group consisting of methylene diphenyl diisocyanate (MDI), tolylene 2,4- and / or 2,6-diisocyanate (TDI), hexamethylene 1,6-diisocyanate (HDI), methylene dicyclohexyl 4,4'-, 2,4'- and / or 2,2'-diisocyanate (H12MDI) and isophorone diisocyanate (IPDI).
[0108] twenty one. (a) At least components (i) to (iii): (i) a polyisocyanate composition comprising at least one polyisocyanate; (ii) at least one chain extender, and (iii) at least one polyol composition; A process for preparing a thermoplastic polyurethane comprising the reaction of preparing the polyol composition, which comprises at least one polyester polyol (P1) obtainable by reacting an aliphatic dicarboxylic acid having from 2 to 12 carbon atoms with a mixture (M1) comprising propane-1,3-diol and a further diol (D1) having from 2 to 12 carbon atoms, (b) producing a molded body (SB) from the thermoplastic polyurethane; A method for producing a molded body (SB), comprising:
[0109] 22. The method of embodiment 21, wherein the diol (D1) is selected from the group consisting of ethylene glycol, butane-1,4-diol, and hexane-1,6-diol.
[0110] 23. The method of embodiment 21, wherein the diol (D1) is butane-1,4-diol.
[0111] 24. The method of any one of embodiments 21 to 23, wherein the aliphatic dicarboxylic acid is adipic acid.
[0112] 25. The method of any one of embodiments 21 to 24, wherein the mixture (M1) comprises propane-1,3-diol and the diol (D1) in a ratio ranging from 3:1 to 1:3.
[0113] 26. The method of any one of embodiments 21 to 25, wherein the mixture (M1) comprises a further diol.
[0114] 27. The method according to any one of embodiments 21 to 26, wherein the polyester polyol (P1) has a molecular weight Mw in the range of 750 to 3000 g / mol.
[0115] 28. The method according to any one of embodiments 21 to 27, wherein the chain extender used in (ii) is selected from the group consisting of aliphatic and aromatic diols having a molecular weight of <500 g / mol.
[0116] 29. The method of any one of embodiments 21 to 28, wherein the polyisocyanate is an aliphatic or aromatic diisocyanate.
[0117] 30. The method of any one of embodiments 21 to 29, wherein the polyisocyanate is selected from the group consisting of methylene diphenyl diisocyanate (MDI), tolylene 2,4- and / or 2,6-diisocyanate (TDI), hexamethylene 1,6-diisocyanate (HDI), methylene dicyclohexyl 4,4'-, 2,4'- and / or 2,2'-diisocyanate (H12MDI) and isophorone diisocyanate (IPDI).
[0118] 31. Use of the thermoplastic polyurethane according to any one of embodiments 1 to 10, or of the thermoplastic polyurethane obtainable or obtainable by the method according to any one of embodiments 11 to 20, for producing extrusion products, films and mouldings.
[0119] 32. The use of embodiment 31, wherein the extruded product, film or sheet is reinforced with a filler.
[0120] 33. Use of a thermoplastic polyurethane according to any one of embodiments 1 to 10, or of a thermoplastic polyurethane obtainable or obtainable by the method according to any one of embodiments 11 to 20, for the manufacture of a polymer composition.
[0121] 34. At least components (i) to (iii): (i) a polyisocyanate composition comprising at least one polyisocyanate; (ii) at least one chain extender, and (iii) at least one polyol composition; A thermoplastic polyurethane obtainable or obtainable by reacting The polyol composition comprises at least one polyester polyol (P1) obtainable by reacting an aliphatic dicarboxylic acid having 2 to 12 carbon atoms with a mixture (M1) comprising propane-1,3-diol and butane-1,4-diol.
[0122] 35. The thermoplastic polyurethane of embodiment 34, wherein the aliphatic dicarboxylic acid is adipic acid.
[0123] 36. The thermoplastic polyurethane according to embodiment 34 or 35, wherein the mixture (M1) comprises propane-1,3-diol and butane-1,4-diol in a ratio ranging from 3:1 to 1:3.
[0124] 37. The thermoplastic polyurethane of any one of embodiments 34 to 36, wherein the mixture (M1) comprises hexane-1,6-diol.
[0125] 38. The thermoplastic polyurethane of any one of embodiments 34 to 37, wherein the mixture (M1) consists of propane-1,3-diol and butane-1,4-diol.
[0126] 39. The thermoplastic polyurethane according to any one of embodiments 34 to 38, wherein the polyester polyol (P1) has a molecular weight Mw in the range of 750 to 3000 g / mol.
[0127] 40. A thermoplastic polyurethane according to any one of embodiments 34 to 39, wherein the chain extender used in (ii) is selected from the group consisting of aliphatic and aromatic diols having a molecular weight of <500 g / mol.
[0128] 41. The thermoplastic polyurethane of any one of embodiments 34 to 40, wherein the polyisocyanate is an aliphatic or aromatic diisocyanate.
[0129] 42. The thermoplastic polyurethane of any one of embodiments 34 to 41, wherein the polyisocyanate is selected from the group consisting of methylene diphenyl diisocyanate (MDI), tolylene 2,4- and / or 2,6-diisocyanate (TDI), hexamethylene 1,6-diisocyanate (HDI), methylene dicyclohexyl 4,4'-, 2,4'- and / or 2,2'-diisocyanate (H12MDI), and isophorone diisocyanate (IPDI).
[0130] 43. At least components (i) to (iii): (i) a polyisocyanate composition comprising at least one polyisocyanate; (ii) at least one chain extender, and (iii) at least one polyol composition; A thermoplastic polyurethane obtainable or obtainable by reacting The polyol composition comprises at least one polyester polyol (P1) obtainable by reacting an aliphatic dicarboxylic acid having 2 to 12 carbon atoms with a mixture (M1) comprising propane-1,3-diol and butane-1,4-diol, The aliphatic dicarboxylic acid is adipic acid, and the mixture (M1) consists of propane-1,3-diol and butane-1,4-diol.
[0131] 44. At least components (i) to (iii): (i) a polyisocyanate composition comprising at least one polyisocyanate; (ii) at least one chain extender, and (iii) at least one polyol composition; A thermoplastic polyurethane obtainable or obtainable by reacting The polyol composition comprises at least one polyester polyol (P1) obtainable by reacting an aliphatic dicarboxylic acid having 2 to 12 carbon atoms with a mixture (M1) comprising propane-1,3-diol and butane-1,4-diol, The mixture (M1) comprises propane-1,3-diol and butane-1,4-diol in a ratio ranging from 3:1 to 1:3.
[0132] 45. At least components (i) to (iii): (i) a polyisocyanate composition comprising at least one polyisocyanate; (ii) at least one chain extender, and (iii) at least one polyol composition; A thermoplastic polyurethane obtainable or obtainable by reacting The polyol composition comprises at least one polyester polyol (P1) obtainable by reacting an aliphatic dicarboxylic acid having 2 to 12 carbon atoms with a mixture (M1) comprising propane-1,3-diol and butane-1,4-diol, The aliphatic dicarboxylic acid is adipic acid, The mixture (M1) comprises propane-1,3-diol and butane-1,4-diol in a ratio ranging from 3:1 to 1:3.
[0133] 46. At least components (i) to (iii): (i) a polyisocyanate composition comprising at least one polyisocyanate; (ii) at least one chain extender, and (iii) at least one polyol composition; A thermoplastic polyurethane obtainable or obtainable by reacting The polyol composition comprises at least one polyester polyol (P1) obtainable by reacting an aliphatic dicarboxylic acid having 2 to 12 carbon atoms with a mixture (M1) comprising propane-1,3-diol and butane-1,4-diol, The aliphatic dicarboxylic acid is adipic acid, The mixture (M1) contains propane-1,3-diol and butane-1,4-diol in a ratio ranging from 3:1 to 1:3; The polyester polyol (P1) has a molecular weight Mw in the range of 750 to 3000 g / mol, the chain extender used in (ii) is selected from the group consisting of aliphatic and aromatic diols having a molecular weight of <500 g / mol; 1. A thermoplastic polyurethane, wherein the polyisocyanate is selected from the group consisting of methylene diphenyl diisocyanate (MDI), tolylene 2,4- and / or 2,6-diisocyanate (TDI), hexamethylene 1,6-diisocyanate (HDI), methylene dicyclohexyl 4,4'-, 2,4'- and / or 2,2'-diisocyanate (H12MDI) and isophorone diisocyanate (IPDI).
[0134] 47. At least components (i) to (iii): (i) a polyisocyanate composition comprising at least one polyisocyanate; (ii) at least one chain extender, and (iii) at least one polyol composition; A thermoplastic polyurethane obtainable or obtainable by reacting The polyol composition comprises at least one polyester polyol (P1) obtainable by reacting an aliphatic dicarboxylic acid having 2 to 12 carbon atoms with a mixture (M1) comprising propane-1,3-diol and butane-1,4-diol, The aliphatic dicarboxylic acid is adipic acid, The mixture (M1) contains hexane-1,6-diol, The polyester polyol (P1) has a molecular weight Mw in the range of 750 to 3000 g / mol, the chain extender used in (ii) is selected from the group consisting of aliphatic and aromatic diols having a molecular weight of <500 g / mol; 1. A thermoplastic polyurethane, wherein the polyisocyanate is selected from the group consisting of methylene diphenyl diisocyanate (MDI), tolylene 2,4- and / or 2,6-diisocyanate (TDI), hexamethylene 1,6-diisocyanate (HDI), methylene dicyclohexyl 4,4'-, 2,4'- and / or 2,2'-diisocyanate (H12MDI) and isophorone diisocyanate (IPDI).
[0135] 48. At least components (i) to (iii): (i) a polyisocyanate composition comprising at least one polyisocyanate; (ii) at least one chain extender, and (iii) at least one polyol composition; 1. A method for preparing a thermoplastic polyurethane comprising the reaction of 1. A process for preparing a polyol composition comprising at least one polyester polyol (P1) obtainable by reacting an aliphatic dicarboxylic acid having 2 to 12 carbon atoms with a mixture (M1) comprising propane-1,3-diol and butane-1,4-diol.
[0136] 49. (a) At least components (i) to (iii): (i) a polyisocyanate composition comprising at least one polyisocyanate; (ii) at least one chain extender, and (iii) at least one polyol composition; A process for preparing a thermoplastic polyurethane comprising the reaction of preparing the polyol composition, the polyol composition comprising at least one polyester polyol (P1) obtainable by reacting an aliphatic dicarboxylic acid having 2 to 12 carbon atoms with a mixture (M1) comprising propane-1,3-diol and butane-1,4-diol; (b) producing a molded body (SB) from the thermoplastic polyurethane; A method for producing a molded body (SB), comprising:
[0137] 50. The method of embodiment 48 or 49, wherein the aliphatic dicarboxylic acid is adipic acid.
[0138] 51. The method of any one of embodiments 48 to 50, wherein the mixture (M1) comprises propane-1,3-diol and butane-1,4-diol in a ratio ranging from 3:1 to 1:3.
[0139] 52. The method of any one of embodiments 48 to 51, wherein the mixture (M1) comprises hexane-1,6-diol.
[0140] 53. The method according to any one of embodiments 48 to 52, wherein the polyester polyol (P1) has a molecular weight Mw in the range of 750 to 3000 g / mol.
[0141] 54. The method according to any one of embodiments 48 to 53, wherein the chain extender used in (ii) is selected from the group consisting of aliphatic and aromatic diols having a molecular weight of <500 g / mol.
[0142] 55. The method of any one of embodiments 48 to 54, wherein the polyisocyanate is an aliphatic or aromatic diisocyanate.
[0143] 56. The method of any one of embodiments 48 to 55, wherein the polyisocyanate is selected from the group consisting of methylene diphenyl diisocyanate (MDI), tolylene 2,4- and / or 2,6-diisocyanate (TDI), hexamethylene 1,6-diisocyanate (HDI), methylene dicyclohexyl 4,4'-, 2,4'- and / or 2,2'-diisocyanate (H12MDI) and isophorone diisocyanate (IPDI).
[0144] 57. Use of the thermoplastic polyurethane according to any one of embodiments 1 to 14, or of the thermoplastic polyurethane obtainable or obtainable by the method according to any one of embodiments 48 or 50 to 56, for producing extrusion products, films and moldings.
[0145] 58. The use of embodiment 57, wherein the extruded product, film or sheet is reinforced with a filler.
[0146] 59. Use of a thermoplastic polyurethane according to any one of embodiments 34 to 47, or of a thermoplastic polyurethane obtainable or obtainable by the method according to any one of embodiments 48 or 50 to 56, for the manufacture of a polymer composition.
[0147] The following examples serve to illustrate the invention but are in no way limiting with respect to the subject matter thereof. EXAMPLES
[0148] 1.Feed material The following feedstocks were used:
[0149] Polyol 1: polyester polyol with an OH number of 45.4 and only primary OH groups (based on propane-1,3-diol and butane-1,4-diol (ratio 1:1) and adipic acid, functionality: 2) Polyol 2: polyester polyol with an OH number of 56.6 and only primary OH groups (based on propane-1,3-diol and butane-1,4-diol (ratio 1:3) and adipic acid, functionality: 2) Polyol 3: polyester polyol with an OH number of 44.0 and only primary OH groups (based on propane-1,3-diol and butane-1,4-diol (ratio 3:1) and adipic acid, functionality: 2) Polyol 4: polyester polyol with an OH number of 45.1 and only primary OH groups (based on propane-1,3-diol and hexane-1,6-diol (ratio 1:1) and adipic acid, functionality: 2) Polyol 5: polyester polyol with an OH number of 43.3 and only primary OH groups (based on propane-1,3-diol and adipic acid, functionality: 2) Polyol 6: polyester polyol with an OH number of 45.2 and only primary OH groups (based on butane-1,4-diol and adipic acid, functionality: 2) Diisocyanate 1: Aromatic isocyanate (methylenediphenyl 4,4'-diisocyanate) CE1: Butane-1,4-diol Stabilizer 1: Polymeric carbodiimide Catalyst: Titanium(IV) butoxide (TTB), CAS: 5593-70-4 Tin(II) 2-ethylhexanoate (SDO), CAS: 301-10-0
[0150] 2. Methodology: 2.1 Determination of viscosity: Unless otherwise stated, the viscosity of the polyols was determined according to DIN EN ISO 3219 (1994) at 25 °C with a Rheotec RC20 rotational viscometer using a CC25 DIN spindle (spindle diameter: 12.5 mm, internal diameter of the graduated cylinder: 13.56 mm) at a shear rate of 50 1 / s.
[0151] 2.2 Hydroxyl number determination: Hydroxyl number was determined by the phthalic anhydride method DIN 53240 (1971-12) and is reported in mg KOH / g.
[0152] 2.3 Determination of Acid Number: Acid numbers are determined according to DIN EN 1241 (1998-05) and are reported in mg KOH / g.
[0153] 3. Preparation of polyols 3.1 Example 1 (ADA / P1,3 / B1,4 (1:1), Mw: 2500) - Polyol 1 A 4 L round neck flask equipped with a thermometer, nitrogen inlet, heating mantle, distillation column and stirrer was initially charged with 1828.09 g of adipic acid, 608.72 g of butane-1,4-diol, 514.02 g of propane-1,3-diol, 5 ppm of SDO and 1 ppm of TTB, which was heated to 120° C. After the mixture became clear, the temperature was first increased to 150° C., then in stages to 240° C., and water was distilled off at 240° C. for several hours. After removing 90% of the calculated condensed water, the pressure in the apparatus was reduced to 60 mbar. The formed condensed water was continuously distilled off until an acid number of less than 1 mg KOH / g was reached. The reaction time was about 18 hours in total.
[0154] A polyester polyol was obtained having a hydroxyl number of 45.4 mg KOH / g, an acid number of 0.79 mg KOH / g, and a viscosity of 1423 mPas at 75°C.
[0155] 3.2 Example 2 (ADA / P1,3 / B1,4 (1:3), Mw: 2000) - Polyol 2 A 4 L round neck flask equipped with a thermometer, nitrogen inlet, heating mantle, distillation column and stirrer was initially charged with 1792.91 g of adipic acid, 914.48 g of butane-1,4-diol, 257.4 g of propane-1,3-diol, 5 ppm of SDO and 1 ppm of TTB, which was heated to 120° C. After the mixture became clear, the temperature was first increased to 150° C., then in stages to 240° C., and water was distilled off at 240° C. for several hours. After removing 90% of the calculated condensed water, the pressure in the apparatus was reduced to 60 mbar. The formed condensed water was continuously distilled off until an acid number of less than 1 mg KOH / g was reached. The reaction time was about 20 hours in total.
[0156] A polyester polyol was obtained having a hydroxyl number of 56.6 mg KOH / g, an acid number of 0.4 mg KOH / g and a viscosity of 882 mPas at 75°C.
[0157] 3.3 Example 3 (ADA / P1,3 / B1,4 (3:1), Mw: 2500) - Polyol 3 A 4 L round neck flask equipped with a thermometer, nitrogen inlet, heating mantle, distillation column and stirrer was initially charged with 1864.56 g adipic acid, 309.98 g butane-1,4-diol, 785.28 g propane-1,3-diol, 5 ppm SDO and 1 ppm TTB, which was heated to 120° C. After the mixture became clear, the temperature was first increased to 150° C., then in stages to 240° C., and water was distilled off at 240° C. for several hours. After removing 90% of the calculated condensed water, the pressure in the apparatus was reduced to 60 mbar. The formed condensed water was continuously distilled off until an acid number of less than 1 mg KOH / g was reached. The reaction time was about 17 hours in total.
[0158] A polyester polyol was obtained having a hydroxyl number of 44.0 mg KOH / g, an acid number of 0.86 mg KOH / g, and a viscosity of 1325 mPas at 75°C.
[0159] 3.4 Example 4 (ADA / P13 / H16 (1:1), Mw 2500) - Polyol 4 A 4 L round neck flask equipped with a thermometer, nitrogen inlet, heating mantle, distillation column and stirrer was initially charged with 1694.43 g adipic acid, 744.21 g hexane-1,6-diol, 479.22 g propane-1,3-diol, 5 ppm SDO and 1 ppm TTB, which was heated to 120° C. After the mixture became clear, the temperature was first increased to 150° C., then in stages to 240° C., and water was distilled off at 240° C. for several hours. After removing 90% of the calculated condensed water, the pressure in the apparatus was reduced to 60 mbar. The formed condensed water was continuously distilled off until an acid number of less than 1 mg KOH / g was reached. The reaction time was about 21 hours in total.
[0160] A polyester polyol was obtained having a hydroxyl number of 45.1 mg KOH / g, an acid number of 0.61 mg KOH / g, and a viscosity of 1065 mPas at 75°C.
[0161] 3.5 Example 5 (ADA / P1,3, Mw: 2500) - Polyol 5 (Comparative Example) A 4 L round neck flask equipped with a thermometer, nitrogen inlet, heating mantle, distillation column and stirrer was initially charged with 1902.45 g of adipic acid and 1066.75 g of propane-1,3-diol and heated to 120° C. After the acids had completely dissolved, the temperature was first increased to 150° C. and then increased stepwise to 240° C., at which point water was distilled off for several hours. After removing 90% of the calculated condensed water, the mixture was cooled to 180° C. and 5 ppm of SDO and 1 ppm of TTB were added. The mixture was then heated again to 240° C. and the pressure in the apparatus was reduced to 60 mbar. The condensed water formed was continuously distilled off until an acid number of less than 1 mg KOH / g was reached. The reaction time was about 22 hours in total.
[0162] A polyester polyol was obtained having a hydroxyl number of 43.3 mg KOH / g, an acid number of 0.86 mg KOH / g, and a viscosity of 1465 mPas at 75°C.
[0163] 3.6 Example 6 (ADA / B14, Mw: 2500) - Polyol 6 (Comparative Example) A 4 L round neck flask equipped with a thermometer, nitrogen inlet, heating mantle, distillation column and stirrer was initially charged with 1758.1 g of adipic acid, 1210.8 g of butane-1,4-diol, 1 ppm of TTB and 5 ppm of SDO and heated to 120° C. After the acids had completely dissolved, the temperature was first increased to 150° C. and then in stages to 240° C., at which point water was distilled off for several hours. After removing 90% of the calculated condensed water, the pressure in the apparatus was reduced to 60 mbar. The formed condensed water was continuously distilled off until an acid number of less than 1 mg KOH / g was reached. The reaction time was about 15 hours in total.
[0164] A polyester polyol was obtained having a hydroxyl number of 45.2 mg KOH / g, an acid number of 0.6 mg KOH / g and a viscosity of 1080 mPas at 75°C.
[0165] 4. Preparation example of TPU synthesis: Thermoplastic polyurethane (TPU) was synthesized in a reaction vessel with stirring from diisocyanate, chain extender (CE), stabilizer, and polyol according to the formulation in Table 1. The starting temperature was 80° C. After reaching a reaction temperature of 110° C., the solution was poured out onto a heating plate heated to 125° C., and the resulting TPU slab was pelletized after heat treatment (15 h, 80° C.).
[0166] [Table 1]
[0167] 5. Mechanical properties The mechanical property values of the resulting thermoplastic polyurethanes are listed in Table 2, where the mechanical properties were determined at room temperature on injection molded sheets heat treated at 100° C. for 20 hours according to the following procedure.
[0168] Shore hardness DIN ISO7619-1:2012, determined after an indentation time of 3 seconds Tensile strength: measured using DIN53504, S2 test specimen Elongation at break DIN53504 Tear propagation resistance DIN53515 Abrasion DIN53516.
[0169] [Table 2]
[0170] 6. Bloom characteristics The bloom properties were analyzed on non-heat-treated injection-molded sheets stored under standard temperature and humidity conditions using an alternating climate test, in which specimens were stored alternately between -18°C and room temperature for 12 hours in each case over a period of two weeks. The results are summarized in Table 3.
[0171] [Table 3]
[0172] Legend: 0=no bloom, 1=bloom, 2=strong bloom References: US5695884 US2006 / 0141883A1 US2006 / 0121812A1 WO00 / 51660A1 WO2010 / 107562A1 Kunststoffhandbuch [Plastics Handbook], Volume VII, edited by Vieweg and Hoechtlen, Carl Hanser Verlag, Munich 1966 (pp. 103-113) EP0922552A1 WO2006 / 082183A1 WO2014 / 198779A1 WO2007 / 082838A1 WO94 / 20568A1
Claims
1. At least components (i) to (iii): (i) a polyisocyanate composition comprising at least one polyisocyanate; (ii) at least one chain extender, and (iii) at least one polyol composition; A thermoplastic polyurethane obtainable or obtainable by reacting the polyol composition comprises at least one polyester polyol (P1) obtainable by reacting an aliphatic dicarboxylic acid having from 2 to 12 carbon atoms, with the exception of succinic acid, with a mixture (M1) comprising propane-1,3-diol and a further diol (D1) having from 2 to 12 carbon atoms, the diol (D1) is selected from the group consisting of ethylene glycol, butane-1,4-diol and hexane-1,6-diol; A thermoplastic polyurethane in which the chain extender used in (ii) does not contain 4,4'-alkylidene dicyclohexyldiamine.
2. The thermoplastic polyurethane of claim 1, wherein the diol (D1) is butane-1,4-diol.
3. 3. The thermoplastic polyurethane of claim 1 or 2, wherein the aliphatic dicarboxylic acid is adipic acid.
4. 4. Thermoplastic polyurethane according to claim 1, wherein the mixture (M1) comprises propane-1,3-diol and the diol (D1) in a ratio ranging from 3:1 to 1:
3.
5. The thermoplastic polyurethane according to claim 1 , wherein the mixture (M1) comprises a further diol.
6. The thermoplastic polyurethane according to any one of claims 1 to 5, wherein the polyester polyol (P1) has a molecular weight Mw in the range from 750 to 3000 g / mol.
7. 7. A thermoplastic polyurethane according to any one of claims 1 to 6, wherein the chain extender used in (ii) is selected from the group consisting of aliphatic and aromatic diols with a molecular weight of <500 g / mol.
8. 8. The thermoplastic polyurethane of claim 1, wherein the polyisocyanate is an aliphatic or aromatic diisocyanate.
9. 9. The thermoplastic polyurethane of any one of claims 1 to 8, wherein the polyisocyanate is selected from the group consisting of methylene diphenyl diisocyanate (MDI), tolylene 2,4- and 2,6-diisocyanate (TDI), hexamethylene 1,6-diisocyanate (HDI), methylene dicyclohexyl 4,4'-, 2,4'- and 2,2'-diisocyanate (H12MDI) and isophorone diisocyanate (IPDI).
10. At least components (i) to (iii): (i) a polyisocyanate composition comprising at least one polyisocyanate; (ii) at least one chain extender, and (iii) at least one polyol composition; 1. A method for preparing a thermoplastic polyurethane comprising the reaction of the polyol composition comprises at least one polyester polyol (P1) obtainable by reacting an aliphatic dicarboxylic acid having from 2 to 12 carbon atoms, with the exception of succinic acid, with a mixture (M1) comprising propane-1,3-diol and a further diol (D1) having from 2 to 12 carbon atoms, the diol (D1) is selected from the group consisting of ethylene glycol, butane-1,4-diol and hexane-1,6-diol; The preparation method, wherein the chain extender used in (ii) does not include 4,4'-alkylidene dicyclohexyldiamine.
11. (a) at least components (i)-(iii): (i) a polyisocyanate composition comprising at least one polyisocyanate; (ii) at least one chain extender, and (iii) at least one polyol composition; A process for preparing a thermoplastic polyurethane comprising the reaction of the polyol composition comprises at least one polyester polyol (P1) obtainable by reacting an aliphatic dicarboxylic acid having from 2 to 12 carbon atoms, with the exception of succinic acid, with a mixture (M1) comprising propane-1,3-diol and a further diol (D1) having from 2 to 12 carbon atoms, the diol (D1) is selected from the group consisting of ethylene glycol, butane-1,4-diol and hexane-1,6-diol; (ii) a chain extender used does not comprise 4,4'-alkylidene dicyclohexyldiamine; (b) a step of producing a molded body (SB) from the thermoplastic polyurethane; A method for producing a molded body (SB), comprising the steps of:
12. 11. Use of a thermoplastic polyurethane according to any one of claims 1 to 9, or of a thermoplastic polyurethane obtainable or obtainable by the process according to claim 10, for producing an extruded product, a film or a moulded body.
13. 13. The use of claim 12, wherein the extruded product, film or sheet is reinforced with a filler.
14. Use of a thermoplastic polyurethane according to any one of claims 1 to 9, or of a thermoplastic polyurethane obtainable or obtainable by the process according to claim 10, for the manufacture of a polymer composition.
Citation Information
Patent Citations
JP1969026673Y1
Polyurethane elastomer composition and squeegee for screen printing
JP2011173310A
Polyurethane urea dispersion
JP2014516367A
Polyurethane made mainly from renewable raw materials
JP2016524017A
Urethane resin composition and leather-like sheet
JP2017002145A