Method and system for supplying liquid organic peroxide to polymer melt processing equipment - Patents.com

By transporting liquid organic peroxides undissolved in an inert aqueous medium, the method addresses safety and stability issues, ensuring safe delivery and improved polymer quality in melt processing.

JP7594665B2Active Publication Date: 2024-12-04LUMMUS NOVOLEN TECH
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
JP2023521135
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2020-10-06
Filing Date
2021-10-06
Publication Date
2024-12-04
Estimated Expiration
2041-10-06

AI Technical Summary

Technical Problem

The safe handling, transportation, and use of liquid organic peroxides in polymer melt processing are hindered by their instability and volatility, leading to safety risks and undesirable effects on polymer properties, and existing methods require complex and costly temperature-controlled enclosures.

Method used

Transporting liquid organic peroxides undissolved in an inert aqueous cooling medium at ambient temperature, allowing safe delivery using common pipes without specialized equipment, and volatilizing under melt processing conditions to minimize safety risks and maintain polymer quality.

Benefits of technology

This method enables safe and efficient transportation of liquid organic peroxides over any distance in industrial settings, reducing energy consumption and minimizing volatile organic compounds and odor in the final polymer product, while maintaining polymer properties.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007594665000001
    Figure 0007594665000001
Patent Text Reader

Abstract

The present disclosure relates to a method and system for supplying liquid organic peroxide to a polymer melt processing device, the method comprising transporting at least one liquid organic peroxide (13) in an undissolved and mixed state in an inert liquid cooling medium (4) from a controlled temperature section (3) to the polymer melt processing device.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present disclosure relates to a method for delivering at least one liquid organic peroxide to a polymer melt process, and to a corresponding system. [Background technology]

[0002] It is known to use organic peroxides (generally liquid organic peroxides) for the rheological modification of polyolefins (such as "visbreaking" and crosslinking). Traditionally, crosslinking has been applied to polyethylene and the like.

[0003] A known method for visbreaking polyolefins is extrusion in the presence of an organic peroxide compound at about 190° C. to 260° C. Such a method is described, for example, in Australian Patent Application Publication No. 5,141,785.

[0004] However, due to their organic nature, pure organic peroxides are extremely unstable, volatile, and dangerous substances with a high risk of combustion or explosion when the temperature rises uncontrollably, and therefore require strict handling precautions. This behavior makes the use of pure organic peroxides very costly and technically complex, as they are often incompatible with transport and storage regulations and / or require special efforts for safe handling and storage. Furthermore, the use of pure organic peroxides in polymer melt processes, such as extrusion processes, which are carried out at high temperatures, is even more dangerous.

[0005] Thus, safe handling and transportation of liquid organic peroxides is a significant concern and can be problematic when using pure liquid organic peroxides, or at least some diluted liquid organic peroxides, in polymer melt processing.

[0006] To overcome storage and transportation challenges, liquid organic peroxides have been diluted with mineral oil. Diluting the organic peroxides reduces the limitations of safety ratings for peroxide products. Diluting the organic peroxides with mineral oil also makes them easier to disperse in polymers such as polyolefins. However, mineral oil also causes undesirable side effects that affect the properties of the polymer. For example, currently available organic peroxides diluted with mineral oil do not pose safety issues and have a higher storage capacity than pure organic peroxides, but the solvent can migrate into the polymer, inhibiting the conversion of the polymer to the final polymer product and further decomposing by-products during the peroxidation reaction in the extruder. Such decomposition and by-products can easily generate high volatile organic compounds (VOCs) that can impart odor to the polymer and the final polymer product.

[0007] US 2018 / 0030163 describes a method for modifying the rheology of a polymer. The method includes extruding a molten polymer and an emulsion-like composition comprising at least one organic peroxide and water, and removing volatile compounds from the molten polymer. The volatile compounds include volatile organic compounds and water. However, US 2018 / 0030163 does not describe a method for handling the organic peroxide upstream of the extruder, specifically a method for transporting the organic peroxide from a storage of the organic peroxide to the extruder.

[0008] More generally, with respect to transporting liquid organic peroxides from a first location (such as a storage site for the organic peroxide) to a second location (such as a location where the organic peroxide is used), it is commonly known to transport these liquids in pipes equipped with temperature control means. For example, the entire length of the pipe may be placed within a temperature controlled enclosure. Such an enclosure must be designed to maintain the pipe at the desired controlled temperature from the first location to the second location, requiring additional equipment and associated costs. In addition to placing the entire pipe within a temperature controlled enclosure, other examples known in the art for transporting organic peroxides include the use of jacketed pipes. Still other examples include those comprising pipes with external heat tracing means. Regardless of the type of temperature control means known, in any case, they are not suitable for covering the long distances typical of industrial sites that use liquid organic peroxides as starting materials or additives in manufacturing processes.

[0009] In any of the above examples in the art, certain equipment must be arranged so that the pipes used to transport the liquid organic peroxides are kept within the limit temperatures required to safely transport the liquid.

[0010] Thus, there remains a need for methods and systems for the safe transport of liquid organic peroxides in industrial sites, including those where the polymer melt process or equipment is intended to use the organic peroxides without affecting or changing the final properties of the polymer being melt processed. Summary of the Invention [Problem to be solved by the invention]

[0011] Applicants have surprisingly discovered that by transporting a liquid organic peroxide that is an aqueous liquid at ambient temperature and that is undissolved and mixed (i.e., a suspension) in an inert cooling medium that volatilizes under melt processing conditions, the organic peroxide can be safely delivered from any location, such as a temporary or long-term storage location, to a polymer melt processing device using ordinary pipes, tubing, or hollow bodies suitable for transporting liquids, without the use of equipment or devices specifically designed to control the temperature of the liquid organic peroxide.

[0012] This also allows the use of temperature control means (such as an enclosure, container, or the like suitable for this purpose) to be limited to only the reservoir of organic peroxide (such as a dedicated temperature controlled container), thereby reducing energy consumption.

[0013] In addition, transporting the liquid organic peroxide in an undissolved mixed state in the inert cooling medium defined above allows the liquid organic peroxide to be safely transported regardless of the distances that must be covered to reach the polymer melt processing equipment (e.g., in industrial plants where polymers are melt processed), resulting in easy, plant-size-compatible transport with low investment.

[0014] Applicants have discovered that the same technical effect can be achieved when multiple liquid organic peroxides are delivered to a polymer melt processing device. [Means for solving the problem]

[0015] According to a first aspect, the present disclosure relates to a method for supplying liquid organic peroxide to a polymer melt processing device, comprising mixing at least one liquid organic peroxide with an inert cooling medium in a mixing section located within a controlled temperature section, the mixing being carried out without dissolving the at least one liquid organic peroxide in the inert cooling medium. The method further comprises transporting the at least one liquid organic peroxide, in an undissolved mixed state in the inert cooling medium, from the controlled temperature section to a polymer melt processing device located outside the controlled temperature section. The inert cooling medium comprises an aqueous liquid at ambient temperature and volatilizes under melt processing conditions. For example, the controlled temperature section may have various containers of liquid organic peroxide, such as temporary or long-term liquid organic peroxide storage.

[0016] The inert cooling medium is not particularly limited as long as it is an aqueous medium that is inactive to the at least one organic peroxide, is liquid at ambient temperature and pressure, and can maintain the temperature of the at least one organic peroxide within the limit temperature required for safe transportation of the peroxide (e.g., 5°C to 40°C, depending on the liquid organic peroxide). For example, the inert cooling medium may be an aqueous liquid that is incompatible with the liquid organic peroxide, or may be an aqueous liquid that is incompatible with all liquid organic peroxides when liquid organic peroxides are used in combination. According to the present disclosure, the inert cooling medium does not act as a solvent. That is, the inert cooling medium does not dissolve the at least one liquid organic peroxide, but maintains the at least one liquid organic peroxide as a suspension. According to one or more embodiments, the at least one organic peroxide and the inert cooling medium may be transported to the polymer melt processing device in the state of an unstable mixture.

[0017] The process as defined in the first aspect of the present disclosure is effective for the safe transport of liquid organic peroxide and is suitable for integration of temperature controlled vessels or reservoirs with polymer melt processing equipment into one simplified plant without the need for specially designed enclosures, equipment or piping for the safe transport of liquid organic peroxide to the polymer melt processing equipment. Such integration can be effectively performed with reduced energy consumption compared to prior art processes, even in the case of high capacity polymer melt processing equipment or plants, such as high throughput extrusion plants.

[0018] According to one or more embodiments, the method includes transporting one or more liquid organic peroxides in an undissolved and mixed state in the inert cooling medium.

[0019] The liquid organic peroxide is not particularly limited as long as it is a liquid organic peroxide.

[0020] According to one or more embodiments, the at least one liquid organic peroxide may include at least one dialkyl peroxide, such as 2,5-dimethyl-2,5-di(t-butylperoxy)hexane, 2,5-dimethyl-2,5-di(tert-butylperoxy)hexane-3, di(tert-butylperoxy-isopropyl)-benzene, dicumyl peroxide, 3,6,9-triethyl-3,6,9-trimethyl-1,4,7-triperoxonane, 3,3,5,7,7-pentamethyl-1,2,4-trioxepane, and combinations thereof.

[0021] According to one or more embodiments, the inert cooling medium is volatilized at sub-atmospheric pressures, such as between 1000 mbar(a) and 800 mbar(a) or between 800 mbar(a) and 600 mbar(a), and at temperatures between 5°C and 80°C.

[0022] According to the present disclosure, the inert cooling medium includes an aqueous cooling medium. For example, the cooling medium may be water. The water may be distilled or deionized water (e.g., desalted water) containing less than 2%, less than 1%, less than 0.5%, less than 0.1%, or no dissolved compounds such as salts. If the water is distilled water, it may contain not only the amounts of salts mentioned above, but also less than 2%, less than 1%, less than 0.5%, or less than 0.1%, or no organic compounds.

[0023] Use of water as a medium allows for the aqueous medium to be readily removed after delivery of the undissolved mixture of liquid organic peroxide and aqueous medium to the polymer under melt processing conditions.

[0024] In addition, volatile compounds may be removed from the molten polymer. Whenever desired, the rheology of the polymer may be modified in the melt processing equipment. Removal of volatile compounds reduces the concentration of decomposition products and by-products in the polymer, which results in less VOCs, lower odor concentration, and less color in the polymer. Also, the aqueous cooling medium or water as a medium can inactivate the active catalytic sites remaining in the polymer. Therefore, the polymer can be inactivated in the melt processing equipment without the need for special inactivation equipment. Also, thorough mixing in the melt processing equipment allows for uniform and efficient inactivation.

[0025] According to one or more embodiments, the method includes providing the aqueous cooling medium or water at a predetermined temperature for mixing with the at least one liquid organic peroxide, for example, water may be provided at a temperature between 5°C and 40°C.

[0026] According to one or more embodiments, the melt processing equipment comprises an extruder or kneader. The melt processing equipment may comprise, for example, a single screw or twin screw extruder, either separately or in combination. Regardless of the type of extruder, according to one or more embodiments, the method may comprise feeding a mixture of liquid organic peroxide and water to a feed hopper of the extruder. Alternatively, the mixture of peroxide and cooling medium may be injected into a processing unit of the plastic processing equipment immediately downstream of the feed hopper of the processing equipment, i.e., where the polymer fed in the feed hopper can be assumed to still be in solid form.

[0027] According to one or more embodiments, the method may further comprise storing the at least one liquid organic peroxide in the controlled temperature section, thus allowing the method to supply the at least one liquid organic peroxide directly from a location where the at least one liquid organic peroxide is stored.

[0028] In accordance with the present disclosure, the method further comprises mixing, e.g., mechanically mixing, the at least one liquid organic peroxide with the inert cooling medium in a mixing section disposed within the controlled temperature section. In accordance with one or more embodiments, a single controlled temperature section is sufficient to control the temperature of storage and mixing. For example, a typical controlled temperature section can safely accommodate a vessel or reservoir for storing the at least one liquid organic peroxide and a mixing section for mixing the at least one liquid organic peroxide with the inert cooling medium.

[0029] According to one or more embodiments, the method further comprises the step of feeding the inert cooling medium to the mixing section, e.g., continuously. According to one or more embodiments, the method further comprises the step of feeding the inert cooling medium to the mixing section at a predetermined flow rate, which may be constant or variable. Such a predetermined flow rate may be, for example, 1000 ppm to 5000 ppm, 1200 ppm to 4000 ppm, 1500 ppm to 3000 ppm, 2000 ppm to 3000 ppm relative to the throughput of the plastic processing equipment (ppm throughout this disclosure and the claims below refers to mg / kg, and thus ppm wt). For example, the flow rate of the inert cooling medium may be at least twice the flow rate of the liquid organic peroxide. For example, the flow rate of the inert cooling medium may be three times greater than the flow rate of the liquid organic peroxide. The method may further comprise the step of adjusting the flow rate of the inert cooling medium, either constant or variable, as required, depending on the flow rate of the liquid organic peroxide. The method may optionally further comprise adjusting the flow rate of the liquid organic peroxide and the constant flow rate of the inert cooling medium depending, for example, on the method of melt processing the polymer and the rate at which the polymer is fed.

[0030] According to one or more embodiments, the method further comprises pumping the at least one liquid organic peroxide from a reservoir to the mixing section at a predetermined flow rate, which may be constant or variable. For example, such a predetermined flow rate may be 10 ppm to 6000 ppm, 30 ppm to 6000 ppm, 50 ppm to 6000 ppm, 50 ppm to 5000 ppm, 100 ppm to 4000 ppm, 200 ppm to 2000 ppm, 300 ppm to 800 ppm relative to the throughput of the plastics processing equipment. If necessary, the method may further comprise adjusting the predetermined flow rate of the at least one liquid organic peroxide, e.g., depending on the method of melt processing the polymer and the flow rate at which the polymer is fed.

[0031] According to one or more embodiments, the polymer comprises or consists of a polyolefin.

[0032] According to one or more embodiments, the polyolefin may be selected from, for example, olefin homopolymers and copolymers, where the olefin monomers may have, for example, from 2 to 8 carbon atoms.

[0033] According to one or more embodiments, the polyolefin may be selected from the group including polypropylene homopolymer, polyethylene homopolymer, copolymers containing propylene, copolymers containing ethylene, and combinations thereof. For example, the polyolefin may be selected from the group consisting of polypropylene homopolymer, propylene copolymer, polyethylene homopolymer, and ethylene copolymer.

[0034] According to one or more embodiments, polyethylenes such as linear low density polyethylene (LLDPE), low density polyethylene (LDPE), high density polyethylene (HDPE), ethyl vinyl acetate copolymer (EVA) and polyolefin elastomers (POE) may be used. For example, polyethylenes with a density of 0.88 g / cm3 may be used according to one or more embodiments. 3 ~0.96g / cm 3 Polyethylene homopolymers and copolymers ranging from 0.1 to 1.0 mm may be used. The polyethylene homopolymers and copolymers may be produced by known processes.

[0035] According to one or more embodiments, polypropylenes may be used, including homopolymers, random copolymers, block copolymers, and terpolymers of propylene. Copolymers of propylene may include copolymers of propylene with other olefins, such as ethylene, 1-butene, 2-butene, and pentene isomers, for example, copolymers of propylene and ethylene. Terpolymers of propylene may include copolymers of propylene with ethylene and one other olefin. Random copolymers (also known as statistical copolymers) are polymers in which propylene and comonomer are randomly distributed throughout the polymer chain, with the ratio depending on the feed ratio of propylene and comonomer. Block copolymers are composed of chain segments composed of propylene homopolymer and chain segments composed of random copolymers, for example, of propylene and ethylene. Homopolymers, random copolymers, and block copolymers may be produced by known processes.

[0036] According to a second aspect of the present disclosure, the present disclosure comprises a method for melt processing a molten polymer, comprising providing at least one liquid organic peroxide as defined in any one of the embodiments disclosed herein to a polymer melt processing device. The method for melt processing a molten polymer further comprises melt processing the molten polymer in the presence of the at least one organic peroxide and the inert cooling medium in the polymer melt processing device, and removing the inert cooling medium from the molten polymer. The melt processing step may include an extrusion step, and may optionally rheologically modify the polymer, for example, by decomposing and / or crosslinking the polymer. The method for melt processing may also include removing other volatile compounds from the molten polymer in addition to removing the inert cooling medium.

[0037] According to one or more embodiments, the polymer melt processing equipment can include an extruder.

[0038] For example, the volatile compounds removed may include volatile organic compounds in addition to the aqueous cooling medium or water.

[0039] According to one or more embodiments, the above-mentioned step of melt processing the molten polymer in the presence of the at least one organic peroxide and the inert cooling medium in the polymer melt processing device may include a step of extruding the molten polymer and the non-dissolved mixture of the at least one organic peroxide and the inert cooling medium. According to one or more embodiments, the step of extruding the molten polymer and the non-dissolved mixture may be performed by extruding the polymer, which may be in the form of, for example, a primary powder or pellets, adding the above-mentioned mixture to the polymer, and melt extruding the polymer in the presence of the mixture. The step of adding the mixture to the polymer may be performed, for example, before or during the extrusion of the polymer. According to one or more embodiments, the mixture may be added to the polymer such that the amount of the at least one organic peroxide relative to the amount of the polymer is a predetermined value. For example, the mixture may be added to the polymer such that the amount of the at least one peroxide added to the polymer is in the range of 100 ppm to 6000 ppm, 200 ppm to 5000 ppm, or 300 ppm to 4000 ppm relative to the amount of the polymer. According to one or more embodiments, the mixture may be added to the polymer such that the amount of the at least one peroxide added to the polymer ranges from 100 ppm to 3000 ppm relative to the amount of the polymer.

[0040] The extrusion step may be carried out in an extruder or any other melt processing equipment. In either case, the extrusion step is carried out under extrusion conditions. The inert cooling medium may be vaporous under extrusion conditions, and may be one that, once removed, for example by venting the extruder, easily extracts undesirable inert species and decomposition products from the molten polymer. Removal of the vapor under extrusion conditions facilitates degassing of undesirable decomposition products and by-products, further reducing both VOC and odor concentrations. As a result, the polymer is further degassed during melt processing of the polymer. Thus, the method according to one or more embodiments of the present disclosure not only allows safe and easy transport of at least one liquid organic peroxide and contacting the at least one organic peroxide with the molten polymer under extrusion conditions to melt process the polymer, but also allows for effective extraction of the inert cooling medium and the inert species and decomposition products from the molten polymer.

[0041] In accordance with one or more embodiments, the extrusion process may be carried out in the presence of one or more polymer additives, such as, for example, fillers, antioxidants, fungicides, bactericides, reinforcing agents, antistatic agents, heat stabilizers, UV stabilizers, flow enhancers, colorants, and other processing aids known to those of skill in the art.

[0042] According to one or more embodiments, the extrusion step may be carried out in an extruder under predetermined extrusion conditions suitable for extruding the polymer, such as a predetermined extrusion temperature and a predetermined extrusion throughput. For the extruder, unless otherwise indicated, the extrusion temperatures and extrusion pressures exemplified in this specification and the claims below are intended to refer to barrel temperatures and barrel pressures.

[0043] For example, the extrusion step may be carried out at an extrusion temperature of 180°C to 260°C, such as 190°C to 250°C, for example 190°C to 240°C.

[0044] According to one or more embodiments, the extrusion conditions may vary along the length of the extruder, for example, the extrusion temperature may be increased or decreased along at least a portion of the extrusion path, which may be across different zones of the extruder.

[0045] Independently of or in combination with the temperature which may vary along the length of the extruder, the extrusion pressure may also vary along the length of the extruder. For example, the extrusion conditions may be such that the pressure in the feed zone is between 10 mbar and 50 mbar, and the pressure in the melt compression zone is between 30 bar and 120 bar. For other zones, the pressure may be between the pressures exemplified for the feed zone and the melt compression zone.

[0046] The extrusion conditions may further include intensive mixing in the extruder. According to one or more embodiments, sufficient mixing may be achieved by varying the screw speed of the extruder in the range of 2 m / s to 6 m / s based on the peripheral speed.

[0047] According to one or more embodiments, the polymer powder or pellets and the mixture may be fed separately or together into an extruder, which may be single or twin screw.

[0048] When they are supplied together, the polymer powder or pellets and the mixture may be premixed, for example, at 30°C to 40°C, as necessary.

[0049] The polymer powder or pellets and the mixture may be fed separately to the extruder at a predetermined feed rate. For example, the polymer feed rate may be set in the range of 2 to 500 kg / h for a laboratory extruder and in the range of 5 tons / h to 100 tons / h for an industrial extruder, and the feed rate of the mixture may be adjusted to obtain final pellets with a desired MFR.

[0050] According to one or more embodiments, the non-molten mixture, if fed separately from the polymer, may be added continuously to the extruder or may be added discontinuously in a single step or in small increments.

[0051] According to one or more embodiments, the temperature of each zone of the extruder may be set at a predetermined temperature range known in the art at steady state, or may be set to a lower value before the mixture is added. For example, the temperature of each zone of the extruder may be set at a temperature range at least 10°C to 20°C lower than the corresponding extrusion temperature at steady state. On the other hand, the mixture may be added after the temperature of each zone of the extruder reaches the temperature range at steady state.

[0052] According to one or more embodiments, the rate at which the mixture is fed into the extruder may be gradually increased to a predetermined value, which may vary depending on the desired final MFR of the pellets, which may be measured, for example, using an online rheometer located in the die zone of the extruder.

[0053] Before the rate at which the mixture is fed to the extruder is increased to a steady state value, the barrel and die zone temperatures are held at the same temperatures set before the mixture was added or may be reduced by an additional 5°C to 10°C, for example.

[0054] According to one or more embodiments, the removing step is performed by venting the polymer melt processing equipment. To this end, the polymer melt processing equipment may have, for example, a reduced pressure zone, including a vent zone.

[0055] In accordance with one or more embodiments, the polymer melt processing apparatus includes an extruder having at least one reduced pressure zone, e.g., a vent zone having at least one vent port or multiple vent ports. The at least one reduced pressure zone may be located, e.g., about 2 / 3 of the way down the extruder screw. The reduced pressure zone allows gases, such as water vapor and volatiles, including an inert cooling medium, to escape from the molten polymer through the vent zone, e.g., through one or more vent ports in the vent zone.

[0056] A vented extruder having at least one vent port may be used to release pressure in at least one reduced pressure zone and aspirate off trapped gas. Such an extruder provides additional benefits to the method according to one or more embodiments of the present disclosure, such as a positive impact on the properties of polymers such as polyolefins. These benefits include inactivation of active catalyst sites and better degassing of the polymer than would be expected from water and organic peroxides separately. Inactivation of active catalyst sites and better degassing of the polymer results in a polymer that contains fewer and purer reaction by-products and volatiles, improved organoleptic properties such as taste and aroma, and reduced color. Additionally, when removed from at least one vent port, the water of the composition extracts undesirable inert species and decomposition products from the molten polymer.

[0057] According to one or more embodiments, the removing step is accomplished by, for example, venting the extruder during the extrusion step. Venting may be accomplished, for example, through at least one vent or suction port in a vent zone of the extruder. According to one or more embodiments, a plurality of vent ports may be defined circumferentially around the barrel and / or longitudinally along a portion of the barrel.

[0058] The vent port may provide a vacuum (ie, subatmospheric pressure) to remove water of reaction and undesirable inert species, thereby preventing water from remaining in the polymer.

[0059] According to one or more embodiments, the removing step is performed by applying a vacuum in a vent zone or vent zones of the extruder. In the case of multiple vent zones, each vent zone may be located in a corresponding one of the reduced pressure zones of an extruder having multiple reduced pressure zones. However, according to one or more embodiments, multiple vent zones may be located in each reduced pressure zone of the extruder.

[0060] According to one or more embodiments, the predetermined vacuum level is set to 0 mbar to 800 mbar, for example, 200 mbar to 800 mbar, for example, 300 mbar to 600 mbar, for example, 350 mbar to 550 mbar. According to one or more embodiments, the removal step may be performed by setting a predetermined vacuum pressure in a reduced pressure zone of an extruder having a vent zone. For example, the vacuum pressure in the reduced pressure zone may be 0 mbar to 800 mbar.

[0061] For example, the pressure in the vent zone can be maintained below atmospheric pressure by installing at least one vent port in piping leading to a vacuum generating device such as a vacuum pump.

[0062] According to one or more embodiments, the polymer melt processed in the above method may include any of the exemplary polymers defined above.

[0063] For example, the polymer to be melt processed may be a propylene homopolymer or copolymer. According to one or more embodiments, the propylene homopolymer or copolymer may have an initial MFR before melt processing, measured according to ISO 1133 at 230°C under a load of 2.16 kg, of about 0.2 g / 10 min to about 100 g / 10 min, e.g., 0.2 g / 10 min to 50 g / 10 min, e.g., 0.2 g / 10 min to 20 g / 10 min.

[0064] In this specification and claims, MFR is measured at 230° C. under a load of 2.16 kg according to ISO 1133, unless otherwise indicated.

[0065] According to one or more embodiments, the propylene homopolymer or copolymer, after melt processing with one or more embodiments of the blend, may have a final MFR up to 5000% higher than the initial MFR. According to one or more embodiments, the final MFR may be from 50g / 10min to 2000g / 10min, such as from 20g / 10min to 100g / 10min, such as from 5g / 10min to 20g / 10min.

[0066] According to yet another aspect, the present disclosure relates to a polymer composition obtained by one or more embodiments of the process defined above.

[0067] The polymer compositions can be used to make products for a variety of applications, such as molding applications, membrane applications, and fiber applications. Product applications include injection molded and blow molded articles used in packaging and automotive applications. Spunbond nonwoven and meltblown fiber applications, such as hygiene, medical, automotive, and geotextile applications, are also examples of applications for the polymer compositions.

[0068] According to yet another aspect, the present disclosure relates to the use of distilled or deionized water as an inert cooling medium for at least one organic peroxide for polymer melt processing equipment.

[0069] According to one or more embodiments, the water may have one or more of the properties set out in any one of the embodiments discussed above in relation to any of the methods above.

[0070] According to yet another aspect, the present disclosure relates to a system for supplying liquid organic peroxide to a polymer melt processing device. The system includes a temperature control section, which includes a storage section for at least one organic peroxide and a mixing section for mixing the at least one liquid organic peroxide with an inert liquid cooling medium without dissolving the at least one liquid organic peroxide. The system also includes a pipe configured to fluidly connect the mixing section to a polymer processing device located outside the temperature control section. The pipe does not include a cooling means such as a cooling jacket, a double wall for circulating a cooling medium, or other external cooling device. Furthermore, according to one or more embodiments, the inert liquid cooling medium can achieve the cooling function in a satisfactory, effective, and convenient manner. Thus, the system may include a conventional pipe that can easily and safely transport the at least one liquid organic peroxide mixed with the inert liquid cooling medium from the controlled temperature section to the polymer melt processing device.

[0071] According to one or more embodiments, the pipe may be between 5m and 200m in length, for example between 10m and 100m.

[0072] According to one or more embodiments, the pipe comprises a single-walled pipe.

[0073] According to one or more embodiments, the pipe may have multiple sections of different lengths and / or oriented in different directions, for example, the multiple sections may be connected to one another with straight or curved connectors, joints, elbows, and similar connecting means.

[0074] According to one or more embodiments, the mixing section may include or be, for example, a static mixer for continuous mixing of fluids.

[0075] According to one or more embodiments, the temperature management section further comprises an injection section for injecting an inert liquid cooling medium into the mixing section at a predetermined temperature, for example, between 5° C. and 25° C. For example, the injection section may be configured to inject the inert liquid cooling medium fluid within lower and upper temperature limits such that the at least one liquid organic peroxide is not frozen and heated. To this end, the injection section may be equipped with a temperature regulator.

[0076] According to one or more embodiments, the injection section may be configured to inject the inert liquid cooling medium into the mixing section at a rate that is adjustable to a predetermined rate relative to the polymer throughput of the processing equipment, e.g., between 1000 ppm and 5000 ppm.

[0077] According to one or more embodiments, the temperature control section further comprises a pump for pumping at least one organic peroxide to the mixing section at a predetermined flow rate relative to the throughput of the polymer processing device, e.g., 10 ppm to 6000 ppm, 10 ppm to 5000 ppm, etc. The pump may be, for example, a liquid metering pump suitable for injecting a metered amount of liquid into another liquid.

[0078] The polymer melt processing equipment may include an extruder and may have any of the features exemplified above in connection with the polymer melt processing equipment that may be used in the method embodiments described above. [Brief description of the drawings]

[0079] [Figure 1] FIG. 1 is a schematic diagram of a system for altering the rheology of a polymer according to an embodiment of the present disclosure. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0080] The following exemplary methods and systems for supplying at least one liquid organic peroxide to a polymer melt processing apparatus and melt processing a polymer are intended to be illustrative and not limiting.

[0081] A system for melt processing a polymer according to one embodiment of the present disclosure is shown diagrammatically in Figure 1 and generally designated by the reference numeral 12. Melt processing a polymer includes degrading and / or crosslinking a polymer, which may be, for example, polypropylene.

[0082] System 12 includes a system for supplying liquid organic peroxide to a polymer melt processing apparatus (this system is described in more detail below) and a melt processing apparatus including a vent zone 10 .

[0083] 1, the melt processing equipment is an extruder 9 located outside the temperature controlled section and is generally designated by the reference numeral 3. However, the system may include any type of melt processing equipment located outside the temperature controlled section 3.

[0084] Extruder 9 has a feed hopper 8, a melt compression zone (not shown), and a pressure reduction zone with a vent zone 10 located downstream of feed hopper 8. Vent zone 10 may include at least one vent port (not shown). Extruder 9 may be a twin screw extruder, such as a co-rotating closely intermeshed twin screw extruder.

[0085] The temperature control section 3 may be, for example, an enclosure maintained at a predetermined temperature, for example, 10° C. to 20° C., by HVAC.

[0086] In the embodiment shown in FIG. 1, the temperature control section 3 comprises a storage 1 (e.g., a storage tank) of liquid organic peroxide 13 (which may be, for example, 2,5-dimethyl-2,5-di(tert-butylperoxy)hexane) and a mixing section 5 for mixing the liquid organic peroxide 13 with an inert aqueous cooling medium 4 (which may be, for example, demineralized water). The demineralized water may, for example, have less than 2%, less than 1%, less than 0.5%, less than 0.1% or no dissolved compounds such as salts. The storage tank may be any storage tank known in the art for safely storing liquid organic peroxides and in compliance with established safety regulations for these types of materials. The mixing section 5 may be a static mixer for continuous mixing of the liquids.

[0087] The temperature management section 3 further comprises an injection section (not shown in detail) for injecting the inert aqueous cooling medium 4 into the mixing section 5. The injection section may inject the inert aqueous cooling medium 4 at a predetermined flow rate, for example 1000 ppm to 5000 ppm, relative to the throughput of the polymer processing device. For example, the flow rate of the inert aqueous cooling medium 4 may be at least twice the flow rate of the liquid organic peroxide 1, and may be, for example, three times greater than the flow rate of the liquid organic peroxide 1. The injection section may inject the inert aqueous cooling medium 4 at a predetermined temperature, for example 5 to 25°C, depending on the liquid organic peroxide 13. For this purpose, the injection section may comprise a temperature control device. The temperature of the inert aqueous cooling medium 4 may be selected and / or adjusted within lower and upper temperature limits such that the liquid organic peroxide 13 is not frozen and heated. For example, when the liquid organic peroxide 13 is 2,5-dimethyl-2,5-di(tert-butylperoxy)hexane, the temperature may be in the range of 10°C to 40°C.

[0088] The temperature control section 3 further includes a pump 2 for pumping the liquid organic peroxide 13 to the mixing section 5 at a predetermined flow rate, for example, 50 ppm to 6000 ppm, relative to the throughput of the polymer processing device. The pump 2 is not particularly limited as long as it is, for example, a liquid metering pump suitable for injecting a metered liquid into another liquid.

[0089] The system for feeding the liquid organic peroxide to the extruder 9 comprises a temperature controlled section 3 and a pipe 6 arranged to fluidly connect the mixing section 5 with the extruder 9 located outside the temperature controlled section 3. The pipe 6 does not have any external temperature control means such as a cooling jacket or a double wall for circulating a cooling medium. In fact, the function of cooling the liquid organic peroxide 13 is performed by an inert aqueous cooling medium 4. The pipe 6 may therefore be a conventional single-wall pipe that does not need to be equipped with any specific cooling means. The pipe 6 may have a length of 5 m to 200 m, but may vary depending on the size of the system 12 for melt processing the polymer and the layout of the equipment.

[0090] According to an embodiment of the present disclosure, an example of a method for melt processing a polymer, comprising decomposing and / or crosslinking polypropylene with at least one organic peroxide, such as 2,5-dimethyl-2,5-di(tert-butylperoxy)hexane, may be as follows: The example of a method for melt processing a polymer comprises transporting liquid organic peroxide 13, which is in an undissolved and mixed state in an inert aqueous cooling medium 4 (such as demineralized water), from a controlled temperature section 3 to a hopper of an extruder 9, extruding the molten polymer in the presence of the liquid organic peroxide 13 and the inert aqueous cooling medium 4 in the extruder 9, and removing the inert aqueous cooling medium 4 and other volatile compounds from the molten polymer. To produce a mixture of liquid organic peroxide 13 and inert aqueous cooling medium 4, the method may include storing liquid organic peroxide 13 in a storage section 1 located within a controlled temperature section 3, pumping the liquid organic peroxide 13 from the storage section 1 to a mixing section 5 at a predetermined rate relative to the throughput of the polymer processing equipment, e.g., 500 ppm, providing the inert aqueous cooling medium 4 to the mixing section 5 at a predetermined rate relative to the throughput of the polymer processing equipment, e.g., 2500 ppm, and mixing the liquid organic peroxide 13 and the inert aqueous cooling medium 4 in the mixing section 5.

[0091] Liquid organic peroxide 13, which is not dissolved but mixed in the inert aqueous cooling medium 4, is fed, for example under a nitrogen blanket, through pipe 6 to extruder feed hopper 8 along with polypropylene powder or pellets 7. Along with the liquid organic peroxide 13, the inert aqueous cooling medium 4, polymer powder or pellets 7, stabilizers, and / or other additives may also be fed from feed hopper 8 to extruder 9. Extruder 9 may incorporate the components using a rotating screw at an extrusion temperature in the range of, for example, 190° C. to 260° C. The screw of extruder 9 mixes the polymer, liquid organic peroxide 13, and inert aqueous cooling medium 4.

[0092] The pressure and temperature of the extrusion process may be varied along the length of the extruder 9. For example, the melt pressure in the melt compression zone may be about 100 bar at a temperature of about 230° C. During the reactive extrusion process, the liquid organic peroxide 13 rheologically modifies the molten polymer.

[0093] The extruder 9 has a vent zone 10 downstream of the extruder's feed hopper 8, so that the demineralized water, which has finished acting as an inert aqueous cooling medium 4 for the liquid organic peroxide 13 along the pipe 6, can be extracted as steam 11 from the polymer melt. In addition, other volatile compounds and reaction products of the peroxide decomposition reaction may be removed together with the water. The vacuum pressure required to completely extract the inert cooling medium consisting of the demineralized water and other volatile compounds may be selected from subatmospheric pressures in the vent zone, for example from 1000 mbar(a) to 800 mbar(a), for example from 800 mbar(a) to 600 mbar(a). The subatmospheric pressure in the vent zone can be maintained at a desired level, for example by providing at least one vent port in the piping leading to a known device for generating a vacuum, such as a vacuum pump. The vented polymer is discharged from the extruder 9 as pellets through a pelletizer (not shown).

[0094] Finally, VOCs can be further reduced, odor can be easily reduced, and the color of the final polymer pellets can be improved.

[0095] The above embodiment includes 2,5-dimethyl-2,5-di(tert-butylperoxy)hexane as a liquid organic peroxide for modifying the rheology of polymers such as polypropylene under extrusion conditions. However, other polymers may be rheologically modified by other organic peroxides according to embodiments of the method of the present disclosure. Also, the above embodiment is based on the use of a single organic peroxide. However, multiple organic peroxides may be used according to one or more embodiments of the method of the present disclosure. Furthermore, stabilizers and / or other additives may be used according to one or more embodiments of the method of the present disclosure.

[0096] While the present invention has been described with respect to only a limited number of embodiments, those skilled in the art having the benefit of this disclosure will appreciate that other embodiments are possible that do not depart from the scope of the invention disclosed herein, the scope of which should therefore be limited only by the scope of the appended claims.

Claims

1. 1. A method for supplying a liquid organic peroxide to a polymer melt processing apparatus, comprising: The method comprises the steps of storing at least one liquid organic peroxide (13) in a reservoir (1) located within a controlled temperature section (3); mixing said at least one liquid organic peroxide (13) with an inert cooling medium (4) in a mixing section arranged in said controlled temperature section (3), said mixing step being carried out without dissolving said at least one liquid organic peroxide (13) in said inert cooling medium (4); transporting said at least one liquid organic peroxide (13), in an undissolved and mixed state in said inert cooling medium (4), from said controlled temperature section (3) to a polymer melt processing device located outside said controlled temperature section; having The inert cooling medium (4) comprises an aqueous liquid that volatilizes under melt processing conditions; method.

2. 2. The method according to claim 1, wherein the inert cooling medium (4) consists of demineralized water.

3. 3. The method according to claim 1 or 2, wherein the polymer melt processing device comprises an extruder (9).

4. The method according to any one of claims 1 to 3, wherein the mixing is mechanical mixing.

5. 2. The method of claim 1, further comprising the step of supplying the inert cooling medium (4) to the mixing section at a predetermined flow rate.

6. 2. The method of claim 1, further comprising the step of pumping the at least one liquid organic peroxide (13) from the storage (1) to the mixing section at a predetermined flow rate.

7. The method of any one of claims 1 to 6, wherein the polymer is a polyolefin.

8. A method for melt processing a molten polymer, comprising feeding at least one liquid organic peroxide (13) as defined in any one of claims 1 to 7 to a polymer melt processing device, comprising the steps of: The method for melt processing the molten polymer comprises the steps of melt processing the molten polymer in the presence of the at least one organic peroxide (13) and the inert cooling medium (4) in the polymer melt processing apparatus; removing said inert cooling medium (4) from said molten polymer; The method further comprises:

9. The method of claim 8 , wherein the melt processing step comprises an extrusion step.

10. 10. The method of claim 8 or 9, wherein the removing step is performed by venting the polymer melt processing apparatus.

11. 1. A system for supplying liquid organic peroxide to a polymer melt processing apparatus, comprising: The system comprises a temperature control section (3), the temperature control section (3) comprising: A reservoir (1) of at least one liquid organic peroxide (13); a mixing section (5) for mixing the at least one liquid organic peroxide (13) with an inert liquid cooling medium (4) without dissolving the at least one liquid organic peroxide (13); and a pipe (6) arranged to fluidly connect said mixing section (5) with a polymer processing device arranged outside said temperature control section (3), said pipe (6) being not provided with cooling means; A system having

12. The system of claim 11 , wherein the mixing section is a static mixer.

13. 13. The system according to claim 11 or 12, wherein the thermal management section (3) further comprises an injection section for injecting the inert liquid cooling medium (4) into the mixing section (5) at a predetermined flow rate.

14. The system according to any one of claims 11 to 13, wherein the temperature control section (3) further comprises a pump (2) for pumping the at least one liquid organic peroxide (13) to the mixing section (5) at a predetermined flow rate.

Citation Information

Patent Citations

  • Proper quantity discharge device

    JP1980065509A

  • Production of modified propylene polymer composition

    JP1992348148A

  • Method and apparatus for continuously introducing liquid phase material into plastic particles

    JP2002533238A

  • Improved feed assembly

    JP2003534151A

  • Methods for modifying rheology of polymers

    JP2018505293A