Manufacturing method for Zr-containing high Ni alloy ingot
A controlled ESR process with specific flux and electrode compositions stabilizes the slag-metal reaction, achieving uniform Zr distribution in large high-Ni alloy ingots, addressing efficiency and cost issues in existing methods.
Patent Information
- Application Number
- JP2020210527
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2020-12-18
- Publication Date
- 2024-12-05
- Estimated Expiration
- 2040-12-18
AI Technical Summary
Existing ESR processes face challenges in uniformly distributing Zr in large high-Ni alloy ingots due to Zr's high affinity for oxygen, leading to significant loss and low efficiency, especially with expensive slag materials like ZrO2.
A controlled ESR process is employed with specific flux and consumable electrode compositions, adjusting ZrO2 content to 0.01-2.0% and setting (A-Z) and (T-Z) within -1.0 to 1.0 and 0.5 to 2.5 ranges, respectively, to stabilize the slag-metal reaction and ensure uniform Zr distribution.
This method produces high-Ni alloy ingots with uniform Zr distribution, even in large sizes, by stabilizing the slag-metal reaction and reducing Zr addition, thereby enhancing efficiency and reducing costs.
Smart Images

Figure 0007594732000004 
Figure 0007594732000005 
Figure 0007594732000006
Abstract
Description
[Technical field]
[0001] The present invention relates to a method for producing a Zr-containing high Ni alloy ingot having uniformly distributed Zr by an ESR process, and more particularly to a method for producing a high Ni alloy ingot containing at least Al and Ti together with Zr. [Background technology]
[0002] In high-Ni alloys, which have excellent corrosion resistance and mechanical strength at high temperatures, the inclusion of Zr can further improve high-temperature strength. For such high-Ni alloys, the electroslag remelting (ESR) process can be used, in which an alloy ingot with a specified composition is obtained through refining by a metal-slag reaction between a consumable electrode and a slag made by melting flux. However, since Zr is an active element with high affinity for oxygen, it reacts with slag and is easily worn away, making it difficult to obtain a high-Ni alloy ingot with uniform Zr distribution.
[0003] Here, a method has been proposed for the ESR process of Zr-containing high-Ni alloys, in which ZrO2 is added to the flux to control the metal-slag reaction and produce a high-Ni alloy ingot with uniformly distributed Zr.
[0004] For example, Patent Document 1 discloses that in an ESR process for producing a relatively small Ni-based Cr-Mo-Fe alloy ingot containing Zr, with a diameter of about 100 mm, an appropriate amount of oxides of active components such as Si, Ti, and Al contained in the electrode components (target ingot components) together with ZrO2 is added to the flux composition (CaF2-CaO system) so that the electrode components and the flux composition are in equilibrium. By adding ZrO2 to the flux composition, Zr remains in the obtained alloy ingot even in an ESR process using an electrode that does not contain Zr. Specifically, it discloses selectively adding 10% by weight or less of SiO2, 5-25% by weight of TiO2, and 5-30% by weight of Al2O3 to a flux containing 5-25% by weight of ZrO2 in CaF2 and CaO. [Prior art documents] [Patent documents]
[0005] [Patent Document 1] Japanese Patent Application Publication No. 63-216935 Summary of the Invention [Problem to be solved by the invention]
[0006] It is difficult to obtain a high-Ni alloy ingot with uniformly distributed Zr by the ESR process, and Zr loss at the bottom tends to be large, especially in large alloy ingots with a diameter of 300 mm or more. In response to this, as mentioned above, a high-Ni alloy ingot with uniformly distributed Zr can be obtained by adding a large amount of ZrO2 to the flux in the ESR process. On the other hand, it has been pointed out that ZrO2 is expensive compared to the price of common slag materials such as CaF2 and CaO, and since most of the slag is removed, the utilization efficiency of the added Zr is low. Therefore, it was desired to optimize the amount of Zr added to the flux according to the composition of the desired alloy ingot.
[0007] The present invention has been made in view of the above circumstances, and an object of the present invention is to provide a method for producing a high Ni alloy ingot in which Zr is uniformly distributed by controlling the metal-slag reaction while suppressing the amount of ZrO2 added to the flux in the ESR process of a Zr-containing high Ni alloy. [Means for solving the problem]
[0008] The present invention has discovered that, in a high-Ni alloy ingot containing at least Al and Ti in addition to Zr, Zr can be uniformly distributed even in a large alloy ingot by controlling the amount of ZrO2 added to the flux in the ESR process while suppressing the amount of ZrO2 added.
[0009] The manufacturing method according to the present invention is a method for manufacturing a high Ni alloy ingot containing at least Al and Ti together with Zr by utilizing an electroslag remelting (ESR) process, characterized in that the flux has a composition, in mass%, of CaO: 10-40%, ZrO2: 0.01-2.0%, Al2O3: 10-40%, TiO2: 0.1-10%, MgO: 5% or less, SiO2: 3% or less, and the balance being CaF2, and the composition of the flux and the consumable electrode are adjusted so that Z, A, and T defined in the following formulas 1, 2, and 3 satisfy -1.0≦AZ≦1.0 and 0.5≦TZ≦2.5.
[0010]
number
[0011] According to this feature, it is possible to produce a high Ni alloy ingot in which Zr is uniformly distributed while suppressing the amount of ZrO2 added to the flux.
[0012] In the above-mentioned invention, the composition of the high Ni alloy ingot may be characterized in that it is mainly a Ni alloy containing 10 to 25% of Cr and 5% or less of Fe. With such a feature, it is possible to suppress iron oxide in the slag, stabilize the slag-metal reaction, and produce a high Ni alloy ingot with uniformly distributed Zr.
[0013] In the above invention, the consumable electrode may have a composition, in mass%, of Cr: 10-25%, Al: 1-5%, Ti: 1-4%, Zr: 0.01-0.1%, and the balance Ni. With this feature, the slag-metal reaction can be stabilized, and a high Ni alloy ingot with uniformly distributed Zr can be produced.
[0014] In the above-mentioned invention, the composition of the consumable electrode may be characterized in that it contains Co: 25% or less, Mo: 5% or less, W: 3% or less, Fe: 5% or less, Nb: 3% or less, Mg: 0.1% or less, and B: 0.1% or less. According to this characteristic, it is possible to produce a high Ni alloy ingot in which Zr is uniformly distributed without significantly affecting the slag-metal reaction.
[0015] In the above-mentioned invention, the electrode may have a diameter of 300 mm or more. With this feature, even if the alloy ingot is large, a high Ni alloy ingot with uniformly distributed Zr can be produced. [Brief description of the drawings]
[0016] [Figure 1] 1 is a table showing the component composition of a consumable electrode used in a production test. [Diagram 2] 1 is a detailed view of some of the components of the consumable electrode. [Diagram 3] 1 is a table showing the composition of the flux in (a) mass % and (b) mole fraction. [Figure 4] 1 is a table showing the Z value, A value, T value, and Zr analysis results of the obtained alloy ingot. [Diagram 5] This is a balance diagram between Z and A values. [Figure 6] This is a balance diagram between Z and T values. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0017] A method for producing a high Ni alloy ingot as one embodiment of the present invention will be described.
[0018] The high Ni alloy ingot to be obtained has a composition containing at least Al and Ti together with Zr, and is produced by utilizing an electroslag remelting (ESR) process. The flux used in the ESR process has a composition, in mass%, of CaO: 10-40%, ZrO2: 0.01-2.0%, Al2O3: 10-40%, TiO2: 0.1-10%, MgO: 5% or less, SiO2: 3% or less, and the balance CaF2.
[0019] The consumable electrode used in the ESR process and the above-mentioned flux have a composition in which the contents of Al, Ti, and Zr are adjusted as follows in order to control the slag-metal reaction. That is, in Z, A, and T defined in the following formulas 1, 2, and 3, The A value minus the Z value (AZ) is within the range of -1.0 to 1.0, and the T value minus the Z value (TZ) is within the range of 0.5 to 2.5. In other words, -1.0≦(AZ)≦1.0 and 0.5≦(TZ)≦2.5.
[0020]
number
[0021] Setting (AZ) and (TZ) within the above-mentioned ranges is intended to stabilize the following slag-metal reaction of Al and Ti with respect to Zr. 4Al+3ZrO2=2Al2O3+3Zr Ti+ZrO2=TiO2+Zr
[0022] That is, by setting the values of (AZ) and (TZ) within a predetermined range, the slag-metal reaction is stabilized to maintain the equilibrium state for Zr, and the ESR process proceeds. As a result, Zr can be stably present in both the metal and the slag, and a high-Ni alloy ingot containing a stable amount of Zr can be obtained. This makes it possible to distribute Zr uniformly, particularly in large alloy ingots, while suppressing the amount of ZrO2 added to the flux.
[0023] Generally, only a part of Zr contained in the flux can be transferred to the alloy ingot, and the utilization efficiency is low. Therefore, when Zr is to be contained in the alloy ingot, the content of ZrO2 in the flux is generally increased. For example, the above-mentioned Patent Document 1 specifies that the content of ZrO2 in the flux is 5 to 25% by weight. In contrast, according to the above-mentioned method, even if the amount of ZrO2 added is suppressed to 0.01 to 2.0% by mass, the equilibrium state in the slag-metal reaction can be stabilized, and Zr can be uniformly contained in the obtained alloy ingot.
[0024] It is also preferable that the alloy ingot obtained has a composition mainly containing 10 to 25 mass% of Cr and 5 mass% or less of Fe. By reducing the Fe content, the content of iron oxide in the slag can be suppressed and the ESR process can be advanced. This makes it possible to stabilize the slag-metal reaction so as not to affect the equilibrium state regarding Zr, and to obtain an alloy ingot in which Zr is uniformly distributed.
[0025] Furthermore, it is also preferable that the consumable electrode used in the ESR process has a composition of Cr: 10-25%, Al: 1-5%, Ti: 1-4%, Zr: 0.01-0.1%, and the balance Ni, in mass %. This can also stabilize the metal-slag reaction. In addition, the consumable electrode can have a composition that does not significantly affect the above-mentioned slag-metal reaction, which is Co: 25% or less, Mo: 5% or less, W: 3% or less, Fe: 5% or less, Nb: 3% or less, Mg: 0.1% or less, and B: 0.1% or less. Although Si, C, and N can be unavoidably contained, it is preferable to reduce the content of these elements.
[0026] The above-mentioned manufacturing method of high Ni alloy ingot can be used to obtain a large alloy ingot as mentioned above. For example, even if the electrode diameter of the consumable electrode is 300 mm or more, it is possible to manufacture an alloy ingot with uniformly distributed Zr.
[0027] [Manufacturing test] Next, the results of a test carried out to produce a high Ni alloy ingot using the above-mentioned method will be described.
[0028] First, five consumable electrodes were prepared using a high Ni alloy with a composition containing each component in the range shown in Figure 1. All of the electrodes used were large, with an electrode diameter of 300 mm or more.
[0029] In particular, in FIG. 2, the five consumable electrodes are divided into Comparative Example and Examples 1 to 4, and the analytical values of the Al, Ti, Si, and Zr contents for each are shown.
[0030] Fluxes were prepared so as to have the component compositions ((a) mass %, (b) molar fraction) shown in the comparative example and examples 1 to 4 in FIG.
[0031] Here, the above-mentioned "Z", "A", and "T" values, as well as "AZ" and "TZ" values, regarding the relationship between Al2O3, TiO2, and ZrO2 in the flux and Al, Ti, and Zr in the consumable electrode are shown in Figure 4. Then, ESR was performed using these consumable electrodes and fluxes, and alloy ingots were obtained for each of the comparative example and examples 1 to 4.
[0032] The results of the analysis of the Zr content in the alloy flakes cut from a position 100 mm from the bottom side of the obtained alloy ingot are also shown in mass% in the "ESR ingot Bot. [Zr]" column in the figure. The "change rate" is the ratio of the difference between the analytical value of the Zr content in the alloy flakes and the analytical value of the Zr content in the consumable electrode, expressed as a percentage. The absolute value of the change rate is 10% or less and is evaluated as good, with a "◎", while that between over 10% and 30% or less and is evaluated as acceptable, with a "◯", and that over 30% and is evaluated as unacceptable, with a "×".
[0033] As a result, the comparative example was rated as "not good", while Examples 1 to 4 were rated as "good" or "fair". In other words, in Examples 1 to 4, the change in the Zr content of the obtained alloy ingot relative to the consumable electrode was small, and it is considered that the equilibrium state in the slag-metal reaction was stabilized. As a result, it is presumed that Zr was uniformly contained in the obtained alloy ingot.
[0034] Here, FIG. 5 shows a balance diagram of Z value and A value. In the figure, the straight line sloping upward to the right indicates AZ=1.0 at the top and AZ=-1.0 at the bottom. The values of Z and A in Examples 1 to 4 are plotted between these straight lines. In other words, (AZ) was set within the range of -1.0 to 1.0.
[0035] FIG. 6 shows the equilibrium diagram of Z value and T value. The straight line in the figure sloping upwards to the right indicates TZ=2.5 at the top and TZ=0.5 at the bottom. The Z and T values of Examples 1 to 4 are plotted between these straight lines. In other words, (TZ) was set within the range of 0.5 to 2.5.
[0036] In Examples 1 to 4, alloy ingots with uniformly distributed Zr could be produced, because the equilibrium state in the slag-metal reaction was stabilized. Based on Examples 1 to 4, the straight lines on the equilibrium diagram were determined as the range in which the metal-slag reaction can be stabilized. In other words, an alloy ingot with uniformly distributed Zr can be produced by setting the Z value, A value, and T value within the range between the straight lines.
[0037] Although the representative embodiments of the present invention and modified examples based thereon have been described above, the present invention is not necessarily limited to these, and a person skilled in the art will be able to find various alternative embodiments and modified examples without departing from the spirit of the present invention or the scope of the appended claims.
Claims
1. A method for producing a high Ni alloy ingot containing at least Al and Ti together with Zr by using an electroslag remelting (ESR) process to pass an electric current between a consumable electrode and a slag obtained by melting a flux, comprising: The consumable electrode has an electrode diameter of 300 mm or more, In mass percent, Cr: 10-25%, Al: 1 to 5%, Ti: 1 to 4%, Zr: 0.01 to 0.1%, Co: 25% or less, Mo: 5% or less, W: 3% or less, Fe: 5% or less, Nb: 3% or less, Mg: 0.1% or less, B: 0.1% or less The remainder of the composition is Ni and unavoidable impurities. The flux comprises, in mass %, CaO: 10-40%, ZrO 2 : 0.01 to 2.0%, A 2 O 3 : 10-40%, TiO 2 : 0.1 to 10%, MgO: 5% or less, SiO 2 : 3% or less, The remainder is CaF 2 The composition is as follows: In the following formulas 1, 2, and 3, Z, A, and T are defined as follows: A method for producing a Zr-containing high Ni alloy ingot, comprising adjusting the composition of the flux and the consumable electrode so as to satisfy -1.0≦A-Z≦0 and 0.5≦T-Z≦2.
5. [0010]
Citation Information
Patent Citations
High-temperature alloy ingot blank, preparation method thereof and high-temperature alloy part
CN111155021A
Manufacture of zr-containing ni-base alloy
JP1988216935A
Ni-based welding material for electroslag welding
WO2017145854A1