Semicrystalline copolyamides, molding materials containing them and their uses, as well as moldings produced therefrom - Patents.com
A semicrystalline copolyamide composition addresses the issue of dull surfaces in glass fiber reinforced polyamide molding compounds by optimizing crystallization behavior, achieving high gloss and rigidity with fast crystallization for efficient processing and improved surface quality.
Patent Information
- Application Number
- JP2020132942
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2019-08-09
- Filing Date
- 2020-08-05
- Publication Date
- 2024-12-05
- Estimated Expiration
- 2040-08-05
AI Technical Summary
Existing polyamide molding compounds, particularly glass fiber reinforced injection molded products, suffer from dull and rough surfaces due to unevenness and glass fiber effects, which are undesirable for visible molded parts requiring good visual properties and mechanical rigidity.
A semicrystalline copolyamide composition is developed, comprising specific monomers (1,6-hexanediamine, 1,3-bis(aminomethyl)cyclohexane, and dicarboxylic acids, with controlled molar ratios and additives, to achieve high rigidity and improved surface quality through optimized crystallization behavior.
The semicrystalline copolyamide enables the production of molded bodies with high gloss and smooth surfaces, along with excellent mechanical properties, including an elastic modulus of at least 5000 MPa, while maintaining fast crystallization rates for efficient processing.
Smart Images

Figure 0007594868000001 
Figure 0007594868000002 
Figure 0007594868000003
Abstract
Description
[Technical field]
[0001] The present invention relates to semi-crystalline copolyamides and to moulding compounds produced therefrom, which contain, in addition to the semi-crystalline copolyamide, at least one filler and, optionally, additives. The present invention also relates to mouldings produced therefrom.
[0002] A number of polyamide molding compounds are known from the prior art, and the composition of the molding compounds is adapted to their desired property profile. In particular for reinforced polyamide molding compounds, in addition to advantageous mechanical properties, a glossy and smooth surface in the moldings produced therefrom should be possible. The technical processing properties of the molding compounds should not be impaired in the process. However, in glass fiber reinforced injection molded products, the surface of the molded part is often dull and rough due to unevenness and glass fiber effects. However, for visible molded parts, which are often relevant for the design of the body, this effect is usually undesirable.
[0003] The surface quality of injection-molded parts is particularly influenced by the crystallization behavior of the copolyamide, where a high temperature of the injection-molding tool can clearly improve the surface quality, but also prolong the cooling time until the demoulding temperature is reached.
[0004] Polyamides or polyesteramides formed from at least 50 mol % of 1,3- or 1,4-bis(aminomethyl)cyclohexane are known from GB 922,677. They are used for the production of fibers, films or moldings.
[0005] Transparent polyamides are known from GB 1 433 144, from which moldings can be produced at relatively high temperatures without losing good mechanical properties. Here, they are amorphous polyamides formed from mixtures of 1,3-bis(aminomethyl)cyclohexane and aliphatic diamines and mixtures of aromatic and aliphatic dicarboxylic acids. The surface properties of the moldings produced from these molding compounds are not addressed here.
[0006] Fibres consisting of a blend of homopolyamide (PA6 or PA66) and a copolyamide formed from more than 80% by weight of the homopolyamide monomers and less than 20% by weight of 1,3-bis(aminomethyl)cyclohexane and 1,6-hexanediamine are known from GB 2 351 898. As carboxylic acids both aliphatic and aromatic dicarboxylic acids are used. These fibres are particularly suitable for the production of textile materials. Summary of the Invention [Problem to be solved by the invention]
[0007] The present invention has been made in view of these circumstances, and its object is to provide a copolyamide for the production of molding compounds which allows the production of moldings which, in addition to high rigidity, have very good visual properties. [Means for solving the problem]
[0008] This object is achieved by a semicrystalline copolyamide having the features of claim 1, a polyamide moulding compound having the features of claim 7 and a moulded body having the features of claim 10. The use according to the invention is described in claim 12.
[0009] According to the present invention, there is provided a semi-crystalline copolyamide formed from the following monomers (a1) to (a5): (a1) 23 to 37.5 mol% of 1,6-hexanediamine; (a2) 1,3-bis(aminomethyl)cyclohexane 12.5 to 22 mol%; (a3) 0-5 mol % of at least one diamine having 2 to 35 carbon atoms, different from the monomers (a1) and (a2); (a4) 1,6-hexanedioic acid 45 to 50 mol%; (a5) at least one dicarboxylic acid having 2 to 44 carbon atoms, different from monomer (a4), 0 to 5 mol %; The proportions of monomers (a1), (a2) and (a3) should be determined based on the total amount of diamines used. Equivalent The proportions of the monomers (a4) and (a5) are determined based on the total amount of dicarboxylic acids used. Equivalent The total amount of the monomers (a1) to (a5) is 50 mol %. The total amount of the monomers (a1) to (a5) is 100 mol %.
[0010] Definition of Terms Notations and abbreviations of polyamides and their monomers In the sense of the present invention, the term "polyamide" (abbreviation PA) is understood as a generic term; it includes homopolyamides and copolyamides. The notations and abbreviations selected for the polyamides and their monomers correspond to those set out in ISO standard 16396-1 (2015, (D)). The abbreviations used here are used below as synonyms of the IUPAC names of the monomers. In particular, the following abbreviations are used for the monomers in this application: 1,3-BAC stands for 1,3-bis(aminomethyl)cyclohexane (also called 1,3-cyclohexanedimethanamine, CAS number 2579-20-6); 1,4-BAC stands for 1,4-bis(aminomethyl)cyclohexane (also called 1,4-cyclohexanedimethanamine, CAS number 2549-93-1); IDP stands for isophoronediamine (also called 3-(aminomethyl)-3,5,5-trimethylcyclohexanamine, 1-amino-3-aminomethyl-3,5,5-trimethylcyclohexane, or cyclohexanemethanamine, 5-amino-1,3,5,5-trimethyl , CAS number 2855-13-2); MACM stands for bis(4-amino-3-methylcyclohexyl)methane (also called 3,3'-dimethyl-4,4'-diaminodicyclohexylmethane, CAS number 6854-37-5); PACM stands for bis(4-amino-cyclohexyl)methane (also called 4,4'-diamino-cyclohexyl)methane, CAS number 1761-71-3); 6 stands for 1,6-hexanediamine (CAS number 124-09-4); T stands for terephthalic acid (CAS number 100-21-0); I stands for isophthalic acid (CAS number 121-95-5), 6 stands for 1,6-hexanedioic acid (CAS number 124-04-9).
[0011] Semicrystalline copolyamide In the sense of the present invention, semicrystalline copolyamides are copolyamides which preferably have a melting point and / or a heat of fusion in differential scanning calorimetry (DSC) according to ISO 11357-3 (2013) of more than 4 J / g at a heating rate of 20 K / min.
[0012] General information on compounds The terms "containing" and "comprising" in the claims and the specification mean that further components are not excluded. Within the framework of the present invention, the term "consist of" is to be understood as a preferred embodiment of the terms "containing" or "comprising". When a group is defined as "contain" or "comprise" at least a certain number of components, this is also to be understood as preferably disclosing a group that "consists of" these components.
[0013] General discussion on indication of quantity The stated amounts of diamines and dicarboxylic acids in the copolyamide each add up to 50 mole %. All monomers in the copolyamide add up to 100 mole %. It should be understood that the stated ranges of amounts for the individual monomers allow any amount to be selected for each of the individual components within the specified ranges, provided that the strict requirement that all component monomers in the copolyamide add up to 100% by weight is met.
[0014] The sum of the molar amounts of all diamines is substantially equal to the sum of the molar amounts of all dicarboxylic acids, which applies to the indication of the amounts of dicarboxylic acids and diamines in the semicrystalline copolyamide. Substantially equal here means that the maximum excess of dicarboxylic acids or diamines is 3%, i.e. the molar ratio of dicarboxylic acids to diamines is 1.03:1 to 1:1.03. A maximum excess of dicarboxylic acids or diamines of 2% is preferred, i.e. the molar ratio of dicarboxylic acids to diamines is 1.02:1 to 1:1.02. The excess serves to balance the losses of monomers and / or to adjust the relative viscosity and therefore the molar mass of the polyamide.
[0015] Here, the indications of amounts relating to the monomers are to be understood such that the corresponding molar ratios of these monomers used in the polycondensation are also found again in the copolyamide produced by polycondensation.
[0016] The polyamide molding compound according to the invention comprises or consists of components (I) and (II) and optionally (III), with the provision that components (I), (II) and (III) add up to 100% by weight. The given ranges of amounts for each of the components (I), (II) and (III) are to be understood as meaning that any amount can be selected for each of the individual components within the specified ranges, provided that the strict provision that the sum of all components (I) to (III) adds up to 100% by weight is met.
[0017] Semicrystalline Copolyamide The proportion of monomer (a1) in the semicrystalline copolyamide is preferably in the range of 23 to 36 mol%, particularly preferably in the range of 25 to 34 mol%, more particularly preferably in the range of 27.5 to 32.5 mol%. The proportion of monomer (a2) in the semicrystalline copolyamide is preferably in the range of 14 to 22 mol%, particularly preferably in the range of 16 to 20 mol%, more particularly preferably in the range of 17.5 to 20 mol%. The proportion of monomer (a3) in the semicrystalline copolyamide is preferably in the range of 0 to 2.5 mol%. The proportions of monomers (a1), (a2) and (a3) relative to the total of the diamines used are Equivalent , totaling 50 mol %.
[0018] The proportion of monomer (a4) in the semi-crystalline copolyamide is preferably within the range of 47.5 to 50 mol %. The proportion of monomer (a5) in the copolyamide is preferably within the range of 0 to 2.5 mol %. The proportions of monomers (a4) and (a5) are determined by the amount of the monomers used. Dicarboxylic acids In total Equivalent , totaling 50 mol %.
[0019] The at least one monomer (a3) is preferably selected from the group consisting of ethylenediamine, butanediamine, pentanediamine, methylpentanediamine, 1,8-octanediamine, methyloctanediamine, 1,9-nonanediamine, 1,10-decanediamine, 1,11-undecanediamine, 1,12-dodecanediamine, trimethylhexamethylenediamine, 1,4-cyclohexanediamine, 1,3-cyclohexanediamine, bis-(4-amino-3-methyl-cyclohexyl)methane, bis-(4-amino-cyclohexyl)methane, isophoronediamine, 1,4-bis(aminomethyl)cyclohexane, m-xylylenediamine, p-xylylenediamine bis(aminocyclohexyl)propane and its alkyl derivatives, norbornanediamines, and bis(aminomethyl)norbornane.
[0020] A further preferred group from which the at least one monomer (a3) is selected consists of pentanediamine, methylpentanediamine, methyloctanediamine, 1,9-nonanediamine, 1,10-decanediamine, 1,12-dodecanediamine, trimethylhexamethylenediamine, bis-(4-amino-3-methyl-cyclohexyl)methane, bis-(4-amino-cyclohexyl)methane, isophoronediamine, 1,4-bis(aminomethyl)cyclohexane, m-xylylenediamine and p-xylylenediamine.
[0021] It is particularly preferred that the at least one monomer (a3) is selected from the group consisting of pentanediamine, methylpentanediamine, methyloctanediamine, 1,9-nonanediamine, 1,10-decanediamine, 1,12-dodecanediamine, trimethylhexamethylenediamine, bis-(4-amino-3-methyl-cyclohexyl)methane, bis-(4-amino-cyclohexyl)methane and isophoronediamine.
[0022] As monomer (a3) bis-(4-amino-3-methyl-cyclohexyl)methane, bis-(4-amino-cyclohexyl)methane and / or isophoronediamine are more particularly preferably used.
[0023] The at least one monomer (a5) is preferably selected from the group consisting of isophthalic acid, terephthalic acid, naphthalenedicarboxylic acid, 1,9-nonanedioic acid, 1,10-decanedioic acid, 1,11-undecanedioic acid, 1,12-dodecanedioic acid, 1,13-tridecanoic acid, 1,14-tetradecanedioic acid, 1,15-pentadecanoic acid, 1,16-hexadecanedioic acid, 1,17-heptadecanedioic acid, 1,18-octadecanedioic acid, arachidic acid, Nippon acid, behenic acid, cyclohexanedioic acid, phenylindanedicarboxylic acid, phenylenediooxydiacetic acid, and dimeric fatty acids having 36 or 44 carbon atoms.
[0024] A further preferred group from which the at least one monomer (a5) is selected consists of isophthalic acid, terephthalic acid, 1,10-decanedioic acid, 1,12-dodecanedioic acid, 1,14-tetradecanedioic acid and 1,16-hexadecanedioic acid.
[0025] It is particularly preferred that the at least one monomer (a5) is selected from the group consisting of isophthalic acid, terephthalic acid, 1,10-decanedioic acid and 1,12-dodecanedioic acid.
[0026] As the monomer (a5), isophthalic acid and / or terephthalic acid are more particularly preferably used.
[0027] The semi-crystalline copolyamide (component A) preferably contains neither lactams nor amino acids.
[0028] The semi-crystalline copolyamide preferably has a relative viscosity, measured at 20° C. using 0.5 g in 100 ml of m-cresol, of 1.45 to 2.10, particularly preferably 1.50 to 2.05, and more particularly preferably 1.55 to 1.98.
[0029] The glass transition temperature of the semicrystalline copolyamide is preferably within the range of 50 to 200°C, more preferably within the range of 60 to 190°C, and particularly preferably within the range of 65 to 90°C.
[0030] The melting point of the semi-crystalline copolyamide is preferably within the range of 180 to 260°C, more preferably within the range of 205 to 245°C, and particularly preferably within the range of 210 to 235°C.
[0031] The crystallization temperature of the semi-crystalline copolyamide is preferably within the range of 130 to 200°C, more preferably within the range of 140 to 200°C.
[0032] In a further preferred embodiment, the crystallization rate of the semicrystalline copolyamide is preferably in the range from 12 to 50 J / g min, particularly preferably in the range from 15 to 47 J / g min and more particularly preferably in the range from 23 to 45 J / g min.
[0033] The copolyamides according to the invention can preferably have one or more, particularly preferably all, of the properties named above (relative viscosity, glass transition temperature, melting point, crystallization temperature, crystallization rate).
[0034] Polyamide Molding Compound The polyamide moulding compound according to the invention comprises a semi-crystalline copolyamide as defined above. In this specification, the polyamide molding compound can be rephrased as a polyamide molding material.
[0035] The polyamide moulding compound according to the invention preferably comprises or consists of: I) 22 to 70% by weight of at least one copolyamide as defined above II) 30 to 70% by weight of at least one filler, and III) 0-8% by weight of at least one additive.
[0036] Here, component (III) is different from component (II), and the total amount of components (I) to (III) is 100% by weight.
[0037] The proportion of component (I) in the polyamide molding compound is preferably within the range of 29 to 64.9% by weight, particularly preferably within the range of 36 to 59.8% by weight, relative to the total weight of the polyamide molding compound.
[0038] The proportion of component (II) in the polyamide molding compound is preferably within the range of 35 to 65% by weight, particularly preferably within the range of 40 to 60% by weight, relative to the total weight of the polyamide molding compound.
[0039] The proportion of component (III) in the molding compound is preferably in the range from 0.1 to 6% by weight, particularly preferably in the range from 0.2 to 4% by weight, relative to the total weight of the polyamide molding compound.
[0040] The behavior of polyamide molding compounds in thermoplastic processing into molded parts by injection molding or extrusion is influenced by a range of thermal properties of the molding compound.
[0041] Cycle time has a significant impact on the economics of the injection molding process. The cooling time of the molding compound in the tool is limited until the molded part is stable enough to be demolded without deformation or ejector marks. Ideally, the molding compound should also be fully crystallized during the cooling time in the tool. Delay in crystallization after demolding results in shrinkage and deformation. Fast crystallizing molding compounds are characterized by fast crystallization rates and short cycle times.
[0042] A lower melting point allows for lower mass temperatures, thus saving energy, while at the same time preventing the associated thermal degradation and discoloration of the molding compound.
[0043] At the same time, however, the temperature and rate of crystallization do not have to be so high that the molding compound solidifies immediately upon contact with the surface of the cold tool. An effective holding pressure without premature solidification of the molding compound is necessary for accurate release of the surface. The molding compound according to the invention achieves a very good surface with good crystallinity within the minimum cooling time dictated by the thermal conductivity of polyamide molding compounds with normal wall thicknesses.
[0044] Furthermore, a molded article having high rigidity, which is represented by a high elastic modulus, is desired.
[0045] For a high gloss surface, the tool temperature should usually be higher than the glass transition temperature, but if the tool temperature is too high, the cooling time will be unnecessarily long and may cause sticking or removal marks on the molded part surface.
[0046] It must also be noted that in the case of tool temperatures of 190-200 °C, water must be replaced by heat transfer oil as a heat carrier. In that case, additional expensive construction measures are required. Both the additional costs for tool temperature control and the long cycle times are disadvantageous for the molding compound, since they increase the cost of the parts produced from it.
[0047] The molded article produced according to the present invention preferably has an elastic modulus, measured in accordance with ISO 527, of at least 5000 MPa, more preferably at least 8000 MPa, and particularly preferably at least 12000 MPa.
[0048] The molded body produced according to the present invention preferably has a surface gloss value, measured in the dry state at 60° in accordance with DIN EN 2813 (2015), of 70 to 100 GU.
[0049] The molded body produced according to the present invention preferably has a surface gloss value of 60 to 100 GU, measured in a conditioned state at 60° according to DIN EN 2813 (2015).
[0050] The moulded bodies produced according to the invention can preferably have one or more, particularly preferably all, of the above-named properties (elastic modulus and gloss value).
[0051] Component (II) The term filler (ingredient (II)) includes fibrous or acicular fillers, particulate fillers, and mixtures thereof.
[0052] The fillers can preferably be coated or surface treated, i.e. they can be provided with a suitable finishing or binder system or can be otherwise surface activated. Systems based on urethanes, silanes, epoxides, polyamides, polyhydroxyethers, acrylates, their respective combinations or mixtures thereof can be used for this purpose, for example. The leveling or binder system can also contain other auxiliaries such as antistatic agents or mold lubricants (mold release agents).
[0053] The fibrous or acicular fillers are preferably selected from the group consisting of glass fibers, carbon fibers, basalt fibers, slag fibers, metal fibers, whiskers, mineral fibers, wollastonite, ground glass fibers, ground carbon fibers, ground mineral fibers, and mixtures thereof. The fibrous or acicular fillers are particularly preferably selected from the group consisting of glass fibers, carbon fibers, basalt fibers, and mixtures thereof. It is more particularly preferred to use only glass fibers as the fibrous or acicular fillers.
[0054] The glass or carbon fibers can be used as stable fibers (staple fibers) or as continuous fibers (rovings).
[0055] The glass or carbon fibers may have a round, oval, elliptical, angular or rectangular cross section. Fibers with non-circular cross sections ("flat fibers") may also be used, in particular fibers with an oval, elliptical, angular or rectangular cross section.
[0056] The appearance of the glass fibers can be stretched or spiral.
[0057] Glass fibres from all glass types such as A-, C-, D-, E-, E-CR-, L-, LD-, M-, NE-, S-, R-, AR-glass or any desired mixtures thereof can be used. Glass fibres from E-glass or mixtures with E-glass fibres or mixtures with E-glass fibres are preferred.
[0058] The fiber length of the short glass fibers (staple glass fibers) is preferably 1 to 25 mm, more preferably 1.5 to 20 mm, particularly preferably 2 to 12 mm, and even more particularly preferably 2 to 8 mm.
[0059] The diameter of the glass fiber is preferably 5 to 20 μm, more preferably 5 to 15 μm, and particularly preferably 6 to 12 μm.
[0060] When the glass fibers are used as continuous fibers (rovings) in the pultrusion process, the diameter is preferably 20 μm or less (maximum 20 μm), more preferably 18 μm or less, and particularly preferably 10 to 17 μm.
[0061] The diameter of the carbon fibers is preferably from 3 to 12 μm, more preferably from 4 to 10 μm, and particularly preferably from 4 to 9 μm.
[0062] In the case of flat fibers, the aspect ratio, ie the ratio of the main cross-sectional axis to the secondary cross-sectional axis, is 1.5-8, preferably 2-6, and particularly preferably 3-5.
[0063] Of the flat fibers, flat glass fibers are particularly preferred.
[0064] The length of the cross-sectional axis of the flat glass fiber is 3 to 30 μm. The length of the minor cross-sectional axis is preferably 3 to 20 μm, particularly preferably 4 to 10 μm, and the length of the main cross-sectional axis is preferably 6 to 40 μm, particularly preferably 12 to 30 μm.
[0065] The particulate filler is preferably selected from the group consisting of dolomite, silicates, quartz, talc, mica, kaolin, perlite, silica, precipitated or pyrogenic silicon dioxide, diatomaceous earth, titanium dioxide, magnesium carbonate, magnesium hydroxide, aluminum hydroxide, ground or precipitated calcium carbonate, chalk, calcium, limestone dust, slate powder, feldspar, barium carbonate, barium sulfate, synthetic sheet silicate, natural sheet silicate, permanently magnetic or magnetizable metals or alloys, glass flakes, glass spheres, hollow glass spheres, hollow spherical silicate fillers, and mixtures thereof. Particularly preferably, the particulate filler is selected from the group consisting of silicates, quartz, talc, mica, kaolin, perlite, silica, precipitated or pyrogenic silicon dioxide, diatomaceous earth, titanium dioxide, magnesium carbonate, magnesium hydroxide, aluminum hydroxide, ground or precipitated calcium carbonate, chalk, calcium, limestone dust, slate powder, feldspar, barium carbonate, barium sulfate, synthetic silicate sheets, natural silicate sheets, glass flakes, glass spheres, hollow glass spheres, hollow spherical silicate fillers, and mixtures thereof. Particulate fillers are more particularly preferably selected from the group consisting of silicates, talc, mica, kaolin, titanium dioxide, ground or precipitated calcium carbonate, chalk, limestone dust, slate powder, synthetic silicate sheets, natural silicate sheets, glass flakes, glass spheres, hollow glass spheres, and mixtures thereof.
[0066] As filler (component (II)) in the polyamide molding compound according to the invention, it is preferable to use at least one fibrous or acicular filler or a mixture of at least one fibrous or acicular filler and at least one particulate filler.
[0067] When a mixture of at least one fibrous or acicular filler and at least one particulate filler is used, the proportion of the particulate filler accounts for no more than half (maximum half) of the total amount of filler, preferably no more than one third, particularly preferably no more than one quarter.
[0068] It is particularly preferable to use exclusively fibrous or acicular fillers as fillers in the polyamide moulding compounds according to the invention.
[0069] Ingredient (III) According to a preferred embodiment of the present invention, the at least one additive (component (III)) is selected from the group consisting of inorganic and organic stabilizers, in particular antioxidants, antiozonants, light stabilizers, in particular UV stabilizers, UV absorbers or UV blockers, mould lubricants, dyes, marking agents, pigments, black carbon, graphite, graphene, polyamide oligomers, carbon nanotubes, photochromic agents, antistatic agents, mould release means, antiblocking agents, chain extension additives, chain shortening additives, optical brighteners, IR absorbers, NIR absorbers, non-halogen flame retardants, metal pigments, metal flakes, metal coated particles and mixtures thereof.
[0070] The number-average molar mass of the polyamide oligomer is preferably 1000 to 6000 g / mol, particularly preferably 2500 to 4500 g / mol, determined by gel permeation chromatography (GPC) with triple detector.
[0071] The at least one additive can also be added in the form of a masterbatch. As the base polymer of the masterbatch, it is preferred to use a polyamide, which is preferably selected from the group consisting of PA6, PA66, PA12, PA1012, PA1212, PA6 / 12, PA6 / 66, PA6 / 69 and mixtures thereof, or consists of the copolyamide (A) itself.
[0072] Molded body The invention likewise provides moldings which can be produced from the copolyamides or molding compounds described above. The moldings according to the invention can be produced from the copolyamides or polyamide molding compounds according to the invention by conventional processing techniques, such as injection molding.
[0073] A preferred embodiment provides that the moulding is selected from the group consisting of non-lacquered visible parts with or without a function, in the passenger compartment or trunk of a motor vehicle, in the home, in mechanical engineering, in electrical devices, electronic devices, household appliances, furniture, in particular fan blades, gear sticks, rocker switches, buttons, rotary controls, straps, operating elements for seat adjustment, operating elements on steering columns, operating levers, operating elements, drawers, holders for accessories, drink holders, luggage hooks, covers, light switches, razor heads, scissor parts, threaded rods, in particular insulin pumps, housings and decorative elements.
[0074] use The invention further relates to the use of the above-mentioned polyamide moulding compounds according to the invention for producing functional or non-functional, unlacquered visible parts in the passenger compartment or trunk of a motor vehicle, in the household, in mechanical engineering, for electrical equipment, electronic devices, household appliances, furniture, in particular fan blades, gear sticks, rocker switches, buttons, rotary controls, straps, operating elements for seat adjustment, operating elements on steering columns, operating levers, operating elements, drawers, holders for accessories, drink holders, luggage hooks, covers, light switches, razor heads, scissor parts, threaded rods, in particular insulin pumps, housings and decorative elements.
[0075] The subject matter according to the invention will be explained in more detail with reference to the following examples, without being limited to the particular embodiments shown herein.
[0076] Examples and Comparative Examples Measurement method
[0077] Relative Viscosity The relative viscosity was measured at 20 °C according to ISO 307 (2007). For this purpose, 0.5 g of polymer pellets were weighed into 100 ml of m-cresol; the calculation of the relative viscosity (RV) according to RV = t / t0 was performed based on section 11 of the standard.
[0078] Glass transition temperature (Tg), heat of crystallization, heat of fusion, and melting point Measurements were performed on pellets according to SO11357-3(2013). Differential scanning calorimetry (DSC) was performed at each of the three heating steps with a heating rate of 20 K / min. Cooling was performed at 20 K / min after the first heat. The samples were quenched in dry ice after the second heat. The glass transition temperature (Tg) was measured at the third heat and the melting point at the second heat. The crystallization temperature and crystallization rate were measured on cooling after the first heat. The peak maximum temperature is defined as the melting point. The center of the glass transition range, defined herein as the glass transition temperature (Tg), was measured using the "half height" method.
[0079] Gloss value at 60° The gloss values at a measuring angle of 60° were measured according to DIN EN ISO 2813 (2015) at 23° C. with a plate of dimensions 60×60×2 mm using a glossmeter (ATP Messtechnik GmbH, Germany) and are reported in gloss units (GU).
[0080] Elasticity The elastic modulus measurements were performed according to ISO 527 (2012) at 23 °C and a tensile speed of 1 mm / min using ISO tensile rods (type A1, mass 170 × 20 / 10 × 4) manufactured according to the standard: ISO / CD3167 (2003).
[0081] Molar mass measurement Molar mass measurements were performed using gel permeation chromatography (GPC) equipped with a triple detector of refractive index, viscosity and light scattering (7° and 90°). Samples are dissolved in hexafluoroisopropanol (HFIP) (approximately 5 mg of polymer in 1 ml) for measurement and filtered through disposable syringe filters before loading into vials. Unit: Malvern OMNISEC GPC-System Software: Malvern OMNISEC version 10.41 Column: Malvern HFIP3000+HFIP6000M 300×7.8mm, particle size 10μm Eluent: HFIP containing 0.1M potassium trifluoroacetate Column temperature: 40℃ Detector temperature: 40℃ Flow rate 1.0ml / min
[0082] Molecular weights (number average Mn and weight average Mw) are determined using the triple detection method. Calibration of the GPC system is performed using monodisperse PMMA standards. Three measurements are each performed. The arithmetic average of the molecular weights is shown.
[0083] The solvent HFIP was obtained in HPLC quality from Fluorochem, Germany, and potassium trifluoroacetate was obtained from Sigma-Aldrich, Switzerland.
[0084] Disposable filters are available from Chemie Brunschwig, Switzerland under the designation SFPTFE0250022NBC (PTFE membrane, pore size 0.45 μm, filter diameter 25 mm).
[0085] Disposal filters are available from VWR International GmbH, Germany.
[0086] Preparation of test specimens Test specimens were prepared using pellets with a moisture content of less than 0.1% by weight.
[0087] The test specimens were produced on an Arburg injection molding machine, model Allrounder 420 C 1000-250. The process used an increasing and decreasing cylinder temperature from the feed to the nozzle.
[0088] ISO Tensile Rod Cylinder temperature: 260 / 265 / 270 / 275 / 280 / 275℃ Tool temperature: 110℃
[0089] Plate 60×60×2mm Cylinder temperature: 270 / 275 / 280 / 285 / 290 / 285℃ Tool temperature: 110℃
[0090] Abrasive tools were used in the preparation of the plates. Unless otherwise stated, the test specimens were used in dry condition; for this purpose, they were stored in a dry environment, i.e. on silica gel, at room temperature for at least 48 hours after injection molding.
[0091] The 60x60x2mm plates for surface gloss measurements in the conditioned state were stored at 70°C and 62% relative humidity for 7 days according to ISO1110.
[0092] Starting materials The monomers used in the examples and comparative examples are given in Table 1, and the components (II) and (III) of the polyamide molding compounds used are given in Table 2.
[0093] [Table 1]
[0094] [Table 2]
[0095] General rules for the production of copolyamides The preparation of the copolyamide according to the invention is carried out in a manner known per se in known stirred pressure autoclaves having a presentation vessel and a reaction vessel.
[0096] Deionized water is presented in the presentation vessel, monomers and possible additives are added. Inertization is carried out several times with nitrogen gas. Heating is performed to 180-230 ° C, with stirring at the pressure employed to obtain a homogeneous solution. The solution is pumped through a screen into the reaction vessel and heated to the desired reaction temperature of 250-300 ° C, at a pressure of up to 30 bar. The preparation is maintained at the reaction temperature for 2-4 hours in the pressure phase. In the following expansion phase, the pressure can be reduced to atmospheric pressure within 1-2 hours and the temperature reduced slightly. In the following degassing phase, the preparation is maintained at a temperature of 250-300 ° C and atmospheric pressure for 0.5-6 hours. The molten polymer is discharged in the form of strands, cooled to 10-80 ° C in a water bath and pelletized. The pellets are dried at 60-120 ° C under nitrogen or in vacuum to a moisture content of less than 0.1% by weight.
[0097] A suitable catalyst for accelerating the polycondensation reaction is H 3 PO 2 , H 3 PO 3 , H 3 PO 4 The catalyst is preferably mixed in an amount of 0.01 to 0.5% by weight, particularly preferably 0.03 to 0.1% by weight, based on the polyamide.
[0098] Suitable antifoaming agents to avoid foam formation during degassing include silicones or silicone derivatives and are preferably aqueous 10% emulsions used in an amount of 0.01 to 1.0% by weight, particularly preferably 0.01 to 0.10% by weight, based on the polyamide.
[0099] The setting of the relative viscosity and therefore the molar mass can be carried out in a manner known per se, for example via monofunctional amines or carboxylic acids and / or difunctional diamines or dicarboxylic acids as chain regulators. Preferred monofunctional chain regulators for the copolyamides according to the invention are benzoic acid, acetic acid, propionic acid, butylic acid, valeric acid, capric acid, lauric acid, stearic acid, 2-ethylhexanoic acid, cyclohexanoic acid, propylamine, butylamine, pentylamine, hexylamine, 2-ethylhexylamine, n-octylamine, n-nonylamine, n-dodecylamine, n-tetradecylamine, n-hexadidcylamine, stearylamine, cyclohexylamine, 3-(cyclohexylamino)propylamine, methylcyclohexylamine, dimethylcyclohexylamine, benzylamine, 2-phenylethylamine, aniline or triacetonediamine. The chain regulators can be used alone or in combination. Other monofunctional compounds can also be used as chain regulators capable of reacting with amino or acid groups, such as anhydrides, isocyanates, acid halides, amides, or esters, etc. Typical amounts of monofunctional chain regulators used are 10-200 mmol per kg of copolyamide.
[0100] Preparation of the copolyamide according to Example 2 The preparation of the copolyamide PA66 / 1,3-BAC6 according to the invention of Example 2 is described below:
[0101] 1.80 kg of deionized water was placed in the proposed vessel of a 20 liter pressure autoclave and 3.68 kg of 1,6-hexanedioic acid were stirred in. 1.63 kg of 1,3-bis(aminomethyl)cyclohexane, 1.63 kg of 1,6-hexanediamine, 1.2 g of Antifoam RD 10% by weight emulsion as antifoaming agent and finally 15 g of benzoic acid as chain controller were added. The procedure was then carried out as follows: Heating to 210°C was performed after 10x inerting. The homogenous solution was pumped through a screen into the reaction vessel at 210°C. The preparation was heated to 290°C with stirring and held at a pressure of 20 bar for 2 hours. The pressure was relieved to atmospheric pressure within 1.5 hours and then degassed at 290°C for 1 hour. The molten polymer was discharged, cooled in a water bath (20°C) and pelletized. The pellets were dried in vacuum (30 mbar) at 100°C to a moisture content of less than 0.1 wt%. The relative viscosity of the product was 1.74; the glass transition temperature was 72°C and the melting point was 220°C.
[0102] General rules for the manufacture of the polyamide molding compounds according to the invention To produce the polyamide molding compounds according to the invention, components (I), (II) and, optionally, (III) are mixed in conventional compounders, such as single- or twin-screw extruders or screw kneaders, where the components are either metered individually or fed in the form of a dry blend via gravimetric or volumetric trolleys into a feed or side feeder, respectively.
[0103] If additives (component (III)) are used, they can be introduced directly or in the form of a masterbatch. The carrier material of the masterbatch is preferably a polyamide or a polyolefin. Among the polyamides, the copolyamides (I) are particularly suitable for this.
[0104] The dry pellets of the copolyamide and, optionally, the additive (III) are mixed in a closed container to prepare a dry blend. The mixture is homogenized for 10 to 40 minutes using a wobble mixer, a tumble mixer, or a tumble dryer. Homogenization can be carried out under a dry protective gas to avoid moisture absorption.
[0105] Compounding is carried out with a cylinder temperature set at 250-310°C, the temperature of the first cylinder can be set below 90°C. Degassing can be carried out before the nozzle. This can be done by vacuum or air. The melt is discharged in strands and cooled to 10-80°C in a water bath before pelletizing. Alternatively, the melt can be forced into a water bath through a perforated plate with a cutting device, and the cut pellets can be separated in a post-processing path (underwater pelletizing). The pellets are dried at 60-120°C under nitrogen or in vacuum to a moisture content of less than 0.1% by weight.
[0106] Production of polyamide molding compound according to Example 18 Dry pellets of the copolyamide of Example 2 were mixed with additive (IIIM) to form a dry blend, in effect in the ratio shown in Example 18 of Table 6. The mixture was homogenized using a tumble mixer for approximately 20 minutes.
[0107] The polyamide molding compound was produced in a twin-screw extruder of the Werner & Pfleiderer type ZSK25, where the dry blend was metered into the feed via a metering scale. The glass fibers (II-1) were conveyed into the melt before the nozzle by a metering scale and a side feeder 6 housing zones.
[0108] The temperature of the first housing was set at 50°C; the temperature of the remaining housings was set at 260-280°C. The speed was 250 rpm and the throughput was 15 kg / h. No degassing was performed. The molten strand was cooled in a water bath, cut and the resulting pellets were dried in vacuum (30 mbar) at 100°C for 24 hours to a moisture content of less than 0.1% by weight.
[0109] Experimental Results The relative viscosity (RV), glass transition temperature, melting point, crystallization temperature, and crystallization rate of the copolyamides according to the invention were measured, and the corresponding values are shown in Table 3 for Examples 1 to 5 according to the invention, in Table 4 for Examples 6 to 12 according to the invention, and in Table 5 for Comparative Examples 13 to 16.
[0110] All copolymers prepared or used in the examples and comparative examples contain Antifoam RD 10% by weight emulsion (silicone emulsion, manufacturer: Dow Corning SA, Belgium) as antifoam agent and benzoic acid as chain regulator.
[0111] The molding compounds according to the invention of Examples 17 to 32 were tested for surface gloss and modulus of elasticity. The results of these tests are shown in Tables 6 and 7.
[0112] The molding compounds not according to the invention of Comparative Examples 33 to 37 were identically tested for surface gloss and modulus of elasticity under the same measurement conditions. The results of the Comparative Examples are shown in Table 8.
[0113] [Table 3]
[0114] [Table 4]
[0115] [Table 5]
[0116] [Table 6]
[0117] [Table 7]
[0118] [Table 8]
[0119] Discussion of results When the copolyamides according to the present invention in Examples 1 to 12 are compared with the copolyamides not according to the present invention in Comparative Examples 13 to 16, it is found that the copolyamides according to the present invention have lower melting points and crystallization temperatures.
[0120] The plates of the polyamide moulding compounds according to the invention of Examples 17 to 23 and 26 to 32 made from the copolyamides according to the invention filled with glass fibres of Examples 1 to 12 in fact show consistently better gloss values than the plates of the comparative materials of Comparative Examples 33, 34 and 36 in both the dry and conditioned state.
[0121] Plates from the polyamide molding compounds of Examples 24 and 25, filled with mineral only or with a mixture of glass fibre and mineral, show the best gloss results.
[0122] In the case of the glass fiber filled PA1,3-BAC6 of Comparative Example 35, the gloss test plates could only be ejected at a tool temperature of 80° C., because a high tool temperature would result in noticeable ejection marks and too long a cycle time. In the dry state, the gloss indeed reaches high values, but this is significantly reduced by conditioning, due to post-crystallization occurring during this process.
[0123] The plate from comparative example 36 PA66 filled with glass fibres shows an insufficient surface quality and is therefore not suitable for visible parts.
[0124] In order to be able to achieve a modulus of elasticity of at least 5000 MPa, the polyamide moulding compounds according to the invention must contain a filler, as can be seen from the polyamide moulding compound of Comparative Example 37.
Claims
1. A semi-crystalline copolyamide formed from the following monomers (a1) to (a5): (a1) 23 to 37.5 mol% of 1,6-hexanediamine; (a2) 1,3-bis(aminomethyl)cyclohexane 12.5 to 22 mol%; (a3) 0 to 5 mol % of at least one diamine having 2 to 35 carbon atoms, different from the monomers (a1) and (a2); (a4) 45 to 50 mol % of 1,6-hexanedioic acid; and (a5) 0 to 5 mol % of at least one dicarboxylic acid having 2 to 44 carbon atoms, different from the monomers (a4); provided that the proportions of monomers (a1), (a2) and (a3) correspond to the sum of the diamines used, totalling 50 mol %; and the proportion of monomers (a4) and (a5) corresponds to the sum of the dicarboxylic acids used, totalling 50 mol %; and The total amount of the monomers (a1) to (a5) is 100 mol %.
2. the proportion of monomers (a1) in the copolyamide is in the range from 23 to 35 mol %; and / or the proportion of monomers (a2) in the copolyamide is in the range from 14 to 22 mol %; and / or the proportion of monomer (a3) in the copolyamide is in the range from 0 to 2.5 mol %, provided that the proportions of the monomers (a1), (a2) and (a3) correspond to the sum of the diamines used, and total 50 mol %.
2. The copolyamide of claim 1 .
3. the proportion of monomers (a4) in the copolyamide is in the range from 47.5 to 50 mol %; and / or the proportion of monomer (a5) in the copolyamide is in the range from 0 to 2.5 mol %, provided that the proportions of monomers (a4) and (a5) correspond to the sum of the dicarboxylic acids used, totalling 50 mol %; 3. Copolyamide according to claim 1 or 2.
4. at least one monomer (a3) is selected from the group consisting of ethylenediamine, butanediamine, pentanediamine, methylpentanediamine, 1,8-octanediamine, methyloctanediamine, 1,9-nonanediamine, 1,10-decanediamine, 1,11-undecanediamine, 1,12-dodecaneamine, trimethylhexamethylenediamine, 1,4-cyclohexanediamine, 1,3-cyclohexanediamine, bis-4-amino-3-methyl-cyclohexyl)methane, bis-(4-amino-cyclohexyl)methane, isophoronediamine, 1,4-bis(aminomethyl)cyclohexane, m-xylylenediamine, p-xylylenediamine bis(aminocyclohexyl)propane and its alkyl derivatives, norbornanediamines and bis(aminomethyl)norbornane; and / or at least one monomer (a5) is selected from the group consisting of isophthalic acid, terephthalic acid, naphthalenedicarboxylic acid, 1,9-nonanedioic acid, 1,10-decanedioic acid, 1,11-undecanedioic acid, 1,12-dodecanedioic acid, 1,13-tridecanedioic acid, 1,14-tetradecanedioic acid, 1,15-pentadecanoic acid, 1,16-hexadecanedioic acid, 1,17-heptadecanedioic acid, 1,18-octadecanedioic acid, arachidic acid, Nippon acid, behenic acid, cyclohexanedioic acid, phenylindanedioic acid, phenylenediooxydiacetic acid, and dimeric fatty acids having 35 or 44 carbon atoms; Copolyamide according to any one of claims 1 to 3.
5. The copolyamide has a relative viscosity, measured at 20° C. using 0.5 g in 100 ml of m-cresol, of 1.45 to 2.
10. Copolyamide according to any one of claims 1 to 4.
6. Copolyamide according to any one of claims 1 to 5, characterized in that the copolyamide has at least one of the following properties: a glass transition temperature in the range of 50 to 200°C; and / or - a melting point in the range of 180-260°C; and / or the crystallization temperature is in the range of 130 to 200°C; and / or The crystallization rate is in the range of 12 to 50 J / g min.
7. Polyamide moulding material comprising at least one copolyamide according to any one of claims 1 to 6.
8. 8. The polyamide molding material according to claim 7, which comprises: I) 22 to 70% by weight of at least one copolyamide according to any one of claims 1 to 6; II) 30 to 70% by weight of at least one filler; and III) 0 to 8 wt. % of at least one additive; However, component (III) differs from component (II) in that the total proportions of components (I) to (III) are 100% by weight.
9. 9. The polyamide molding material according to claim 7, characterized in that the moldings produced from the polyamide molding material have at least one of the following properties: - has an elastic modulus, measured according to ISO 527, of at least 5000 MPa; and / or a gloss value, measured in dry conditions at 60° according to DIN EN 2813 (2015), of 70 to 100 GU; and / or The gloss value, measured at 60° conditioning according to DIN EN 2813 (2015), is 60 to 100 GU.
10. Moulded bodies which can be produced from the copolyamides according to any one of claims 1 to 6 or from the polyamide moulding materials according to any one of claims 7 to 9.
11. the molding is selected from the group consisting of non-lacquered visible parts with or without a function in the passenger compartment or trunk of a motor vehicle, in household and mechanical engineering, in electrical equipment, electronic equipment, household appliances, furniture, The molded article according to claim 10 .
12. Use of the copolyamides according to any one of claims 1 to 6 or the polyamide moulding compositions according to any one of claims 7 to 9 for producing functional or non-functional, unlacquered visible parts in the passenger compartment or trunk of a motor vehicle, in the household, in mechanical engineering, in electrical equipment, electronics, household appliances, furniture.
Citation Information
Patent Citations
JP1974055796A
Glass filler-reinforced polyamide molding compounds based on amorphous copolyamides
JP2018062651A
Polyamide molding material and molded article thereof
JP2018178117A
Polyamides derived from cyclohexanebis
US3012994A