Rubber composition and rubber product

A rubber composition with a specific copolymer and filler combination addresses heat generation issues in carbon black-reinforced rubber, enhancing fracture resistance and maintaining low heat properties for non-tire applications.

JP7594899B2Active Publication Date: 2024-12-05BRIDGESTONE CORP +1
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
JP2020207717
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2020-12-15
Publication Date
2024-12-05
Estimated Expiration
2040-12-15

AI Technical Summary

Technical Problem

Existing rubber compositions that incorporate carbon black for reinforcement face issues with heat generation due to carbon black rubbing, and existing solutions like modifying natural rubber complicate the manufacturing process and do not adequately address other mechanical properties.

Method used

A rubber composition containing a copolymer formed by polymerizing glycidyl (meth)acrylate, 2-hydroxyethyl (meth)acrylate, and optionally methyl (meth)acrylate, with specific molecular weight and proportion ratios, combined with carbon black and silica fillers, to enhance fracture resistance without worsening heat generation properties.

Benefits of technology

The rubber composition provides excellent fracture resistance and maintains low heat generation properties, suitable for non-tire rubber products, improving durability and mechanical properties.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007594899000001
    Figure 0007594899000001
Patent Text Reader

Abstract

To provide a rubber composition that is applied to a rubber product to give excellent fracture resistance without causing a deterioration of heat-generating properties, and a rubber product including the rubber composition.SOLUTION: A rubber composition contains a rubber component, and a copolymer that is prepared by polymerizing a monomer component containing glycidyl methacrylate and 2-hydroxyethyl methacrylate. The rubber composition is not applicable to tires.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a rubber composition used in the manufacture of rubber products (excluding tires), and to rubber products manufactured from the rubber composition. [Background technology]

[0002] Conventionally, fillers have been blended into rubber compositions for the purpose of reinforcing rubber products, imparting functions, etc. For example, blending carbon black into a rubber composition can improve properties that contribute to the durability of rubber products, such as tensile strength, hardness, and abrasion resistance, and can also impart electrical conductivity.

[0003] On the other hand, when carbon black is blended into a rubber composition, friction between the carbon black particles occurs, which leads to a problem of deterioration of heat generation. Therefore, attempts have been made to suppress the heat generation of rubber by improving the dispersibility of carbon black. For example, Patent Document 1 discloses a rubber composition that can suppress self-heat generation by mixing carbon black with modified natural rubber in which a polar group-containing monomer is graft-polymerized. [Prior art documents] [Patent documents]

[0004] [Patent Document 1] JP 2006-152212 A Summary of the Invention [Problem to be solved by the invention]

[0005] The technology of Patent Document 1 requires modification of natural rubber, which makes the manufacturing process complicated. In addition, Patent Document 1 considers improvement of wear resistance as a tread rubber for heavy-duty pneumatic tires, but does not consider other mechanical properties.

[0006] The present invention has been made in view of the above circumstances, and has an object to provide a rubber composition that, when used in rubber products other than tires, can provide excellent fracture resistance without deteriorating heat build-up, and also to provide a rubber product that uses the rubber composition and has excellent fracture resistance without deteriorating heat build-up. [Means for solving the problem]

[0007] In order to solve the above problems, the present invention provides the following [1] to

[12] . [1] A rubber composition (excluding tire applications) comprising a rubber component and a copolymer obtained by polymerizing a monomer component containing glycidyl (meth)acrylate and 2-hydroxyethyl (meth)acrylate. [2] The rubber composition according to [1], wherein the monomer components contain 9 to 79 mol % of the glycidyl (meth)acrylate and 21 to 91 mol % of the 2-hydroxyethyl (meth)acrylate. [3] The rubber composition according to [1] or [2], wherein the copolymer is obtained by polymerizing a monomer component further containing methyl (meth)acrylate. [4] The rubber composition according to [3], wherein, in the monomer components, the proportion of the glycidyl (meth)acrylate is 8 to 37 mol%, the proportion of the 2-hydroxyethyl (meth)acrylate is 27 to 85 mol%, and the proportion of the methyl (meth)acrylate is 6 to 47 mol%. [5] The rubber composition according to any one of [1] to [4], wherein the copolymer is solid at room temperature. [6] The rubber composition according to any one of [1] to [5], wherein the copolymer has a weight average molecular weight in terms of polystyrene of 2,000 to 20,000. [7] The rubber composition according to any one of [1] to [6], wherein the copolymer is contained in an amount of 0.1 to 20 parts by mass per 100 parts by mass of the rubber component. [8] The rubber composition according to any one of [1] to [7], further comprising carbon black as a filler. [9] The rubber composition according to any one of [1] to [8], further comprising silica as a filler.

[10] The rubber composition according to any one of [1] to [9], wherein the rubber component includes natural rubber, polybutadiene rubber, and styrene-butadiene rubber.

[11] The rubber composition according to

[10] , wherein the proportion of the natural rubber is 20 to 60% by mass, the proportion of the polybutadiene rubber is 20 to 60% by mass, and the proportion of the styrene-butadiene rubber is 10 to 40% by mass.

[0008]

[12] A rubber product (excluding tires) using a vulcanizate of the rubber composition according to any one of [1] to

[11] .

Advantages of the Invention

[0009] According to the present invention, when used for rubber products other than tires, a rubber composition can be provided that exhibits excellent fracture resistance without deteriorating heat generation characteristics. Further, by using the rubber composition, a rubber product with excellent fracture resistance can be provided without deteriorating heat generation characteristics.

Embodiments for Carrying Out the Invention

[0010] Hereinafter, the present invention will be exemplified and described in detail based on its embodiments. In the following description, the description of "A to B" indicating a numerical range represents a numerical range including the endpoints A and B, and represents "A or more and B or less" (when A < B), or "A or less and B or more" (when A > B). Also, parts by mass and mass% are synonymous with parts by weight and weight%, respectively.

[0011] [Rubber Composition] The rubber composition of the present invention includes a rubber component and a copolymer obtained by polymerizing a monomer component including glycidyl (meth) acrylate and 2-hydroxyethyl (meth) acrylate. The rubber composition of the present invention contains a copolymer obtained by polymerizing monomer components including glycidyl (meth)acrylate and 2-hydroxyethyl (meth)acrylate, and therefore when made into a rubber product, it is possible to obtain a rubber product having excellent fracture resistance without deteriorating heat buildup.

[0012] The rubber composition and the rubber product of the present invention will be described in detail below. <Rubber component> In the rubber composition of the present invention, the type of rubber is not particularly limited. For example, natural rubber (NR), polyisoprene rubber (IR), polybutadiene rubber (BR), styrene-butadiene copolymer rubber (SBR), butyl rubber (IIR), ethylene-propylene-diene copolymer (EPDM), acrylonitrile-butadiene copolymer (NBR), and rubbers made by combining these may be mentioned.

[0013] In the present invention, the rubber component preferably contains natural rubber, polybutadiene rubber, and styrene-butadiene copolymer rubber. Among them, it is particularly preferable that the rubber component contains 20 to 60 mass% of natural rubber, 20 to 60 mass% of polybutadiene rubber, and 10 to 40 mass% of styrene-butadiene rubber. The polybutadiene rubber may be modified butadiene rubber or unmodified butadiene rubber, but is more preferably modified butadiene rubber. The styrene-butadiene copolymer rubber may be modified styrene-butadiene copolymer rubber or unmodified styrene-butadiene copolymer rubber, but is more preferably modified styrene-butadiene copolymer rubber. For example, the modified conjugated diene polymer described in WO 2019 / 146323 can be applied.

[0014] <Copolymer> The copolymer added to the rubber composition of the present invention is obtained by polymerizing monomer components including glycidyl (meth)acrylate and 2-hydroxyethyl (meth)acrylate as monomer components. In the present invention, glycidyl (meth)acrylate refers to glycidyl methacrylate or glycidyl acrylate. In the present invention, the copolymer includes not only the case where glycidyl methacrylate or glycidyl acrylate is contained alone, but also the case where a mixture of glycidyl methacrylate and glycidyl acrylate is contained. In the present invention, 2-hydroxyethyl (meth)acrylate refers to 2-hydroxyethyl methacrylate or 2-hydroxyethyl acrylate. In the present invention, the copolymer includes not only the case where 2-hydroxyethyl methacrylate or 2-hydroxyethyl acrylate is contained alone, but also the case where a mixture of 2-hydroxyethyl methacrylate and 2-hydroxyethyl acrylate is contained. An example of such a copolymer is a binary copolymer obtained by polymerizing glycidyl methacrylate (GMA) and 2-hydroxyethyl methacrylate (HEMA) as monomer components.

[0015] In the monomer components, the proportion of glycidyl (meth)acrylate is preferably 9 to 79 mol % and the proportion of 2-hydroxyethyl (meth)acrylate is preferably 21 to 91 mol %, and more preferably the proportion of glycidyl (meth)acrylate is 9 to 68 mol % and the proportion of 2-hydroxyethyl (meth)acrylate is 32 to 91 mol %.

[0016] The copolymer is preferably obtained by further polymerizing a monomer component containing methyl (meth)acrylate. In the present invention, methyl (meth)acrylate refers to methyl methacrylate or methyl acrylate. In the present invention, the copolymer includes not only the case where methyl methacrylate or methyl acrylate is contained alone, but also the case where a mixture of methyl methacrylate and methyl acrylate is contained. The copolymer is obtained by polymerizing a monomer component containing methyl (meth)acrylate, so that the melting point of the copolymer can be increased. As a result of being able to increase the melting point of the copolymer, it is easy to handle since it is weighed as a solid in the production stage as described below. Among them, it is more preferable that the copolymer is obtained by polymerizing a monomer component containing methyl methacrylate (MMA). In the present invention, it is more preferable that the copolymer is obtained by polymerizing a monomer component containing glycidyl methacrylate (GMA), 2-hydroxyethyl methacrylate (HEMA), and methyl methacrylate (MMA). An example of such a copolymer is a ternary copolymer obtained by polymerizing glycidyl methacrylate (GMA), 2-hydroxyethyl methacrylate (HEMA), and methyl methacrylate (MMA) as monomer components.

[0017] When the copolymer is obtained by polymerizing a monomer component containing methyl (meth)acrylate, the monomer components preferably contain glycidyl (meth)acrylate at a ratio of 8 to 37 mol%, 2-hydroxyethyl (meth)acrylate at a ratio of 27 to 85 mol%, and methyl (meth)acrylate at a ratio of 6 to 47 mol%, more preferably glycidyl (meth)acrylate at a ratio of 9 to 30 mol%, 2-hydroxyethyl (meth)acrylate at a ratio of 30 to 75 mol%, and methyl (meth)acrylate at a ratio of 10 to 45 mol%, and even more preferably glycidyl (meth)acrylate at a ratio of 20 to 30 mol%, 2-hydroxyethyl (meth)acrylate at a ratio of 40 to 60 mol%, and methyl (meth)acrylate at a ratio of 20 to 30 mol%.

[0018] The copolymer may be in any form such as a random copolymer, a block copolymer, an alternating copolymer, etc. In particular, a random copolymer is preferred.

[0019] In the present invention, the copolymer is preferably solid at room temperature. Such a copolymer makes it easy to weigh the copolymer in the manufacturing stage of the rubber composition. In addition, the copolymer is easy to put into a mixer in the kneading stage of the rubber composition. Furthermore, since the variation in the amount of copolymer put into the rubber composition between batches can be suppressed, there is also the advantage that the composition variation between batches can be suppressed. As long as it is in a solid state, there is no particular restriction on the form of the copolymer, and it can be used in the kneading of the rubber composition in the form of granules, powder, etc. In addition, in the present invention, "room temperature" refers to 25±5°C.

[0020] In the present invention, the polystyrene-equivalent weight average molecular weight of the copolymer is preferably 2000 to 20000. When the polystyrene-equivalent weight average molecular weight is 2000 or more, the copolymer becomes solid at room temperature. In addition, when the copolymer is mixed with a rubber component to form a rubber composition, it is possible to obtain a rubber product having excellent fracture resistance without deteriorating heat buildup. The polystyrene-equivalent weight average molecular weight of the copolymer is more preferably 2300 or more, and even more preferably 2500 or more. On the other hand, in consideration of the mixability with the rubber component, the polystyrene-equivalent weight average molecular weight of the copolymer is preferably 20000 or less, more preferably 18000 or less, and even more preferably 15000 or less.

[0021] In the rubber composition of the present invention, the content of the copolymer is preferably 1 to 20 parts by mass per 100 parts by mass of the rubber component. By having the content of the copolymer of 1 part by mass or more, it is possible to obtain a rubber product having excellent fracture resistance. On the other hand, from the viewpoint of abrasion resistance, the content of the copolymer is preferably 20 parts by mass or less per 100 parts by mass of the rubber component.

[0022] <Filling agent> The rubber composition of the present invention contains a filler that reinforces the rubber composition. When the rubber composition contains a filler, the strength, such as the fracture resistance, of the rubber product can be increased. The rubber composition of the present invention preferably contains carbon black as a filler. The rubber composition of the present invention may contain silica and an inorganic filler other than carbon black. Examples of the inorganic filler include clay, talc, calcium carbonate, and aluminum hydroxide.

[0023] <<Carbon black>> The carbon black is not particularly limited, and examples thereof include GPF, FEF, HAF, ISAF, and SAF grade carbon black. These carbon blacks may be used alone or in combination of two or more.

[0024] From the viewpoint of wear resistance, the content of carbon black in the rubber composition is preferably 5 parts by mass or more and more preferably 10 parts by mass or more per 100 parts by mass of the rubber component. Also, from the viewpoint of suppressing deterioration of heat buildup, the content of carbon black in the rubber composition is preferably 70 parts by mass or less and more preferably 50 parts by mass or less per 100 parts by mass of the rubber component.

[0025] <<Silica>> In the present invention, the type of silica is not particularly limited, and examples thereof include wet silica (hydrated silicic acid), dry silica (anhydrous silicic acid), calcium silicate, aluminum silicate, etc., and among these, wet silica is preferred. These silicas may be used alone or in combination of two or more kinds. The cetyltrimethylammonium bromide specific surface area (CTAB) of the silica used in the present invention is not particularly limited. For example, the cetyltrimethylammonium bromide specific surface area (CTAB) of the silica is preferably 40 to 350 m 2 / g, more preferably 100 to 250 m 2The CTAB specific surface area of ​​silica is a value measured according to the method of ASTM-D3765-80.

[0026] The content of silica in the rubber composition is not particularly limited and can be appropriately selected depending on the required performance. However, from the viewpoint of improving the fracture resistance while suppressing the deterioration of the low heat generation property, the content of silica is preferably 5 to 120 parts by mass, more preferably 15 to 100 parts by mass, per 100 parts by mass of the rubber component.

[0027] The total content of silica and carbon black is preferably 25 to 130 parts by mass, and more preferably 50 to 90 parts by mass, per 100 parts by mass of the rubber component.

[0028] <Various ingredients> In addition to the components already described, the rubber composition of the present invention may contain, as necessary, various components commonly used in the rubber industry, such as stearic acid, antioxidants, silane coupling agents, zinc oxide, vulcanization accelerators, vulcanizing agents, workability improvers, resins, waxes, oils, and the like, which are appropriately selected within ranges that do not impair the object of the present invention.

[0029] [Preparation of Rubber Composition] The rubber composition of the present invention can be produced by blending the above-mentioned components and kneading them using a kneading machine such as a Banbury mixer, a roll, an internal mixer, etc. The blending amount of each component is the same as the amount already described as the content in the rubber composition. The components may be kneaded in one step, but it is preferable to knead the components in two or more steps. When kneading is performed in two or more steps, at least the rubber component, the copolymer, and silica are kneaded in the first step of kneading.

[0030] [Use of rubber composition (method of use)] The rubber composition of the present invention is preferably used in applications where excellent fracture resistance can be obtained without deteriorating heat buildup when a rubber product is made using the rubber composition. Specifically, the rubber composition is particularly preferably used in applications where rubber products other than tires that contain a rubber component and a filler do not require large deformation resistance or high durability as in tires, but require reduced heat buildup and fracture resistance under a usage environment. Specific examples of the rubber products include conveyor belts, crawlers, anti-vibration rubber, seismic control rubber, seismic isolation rubber, hoses and tubes, piping, cables, sealing materials, caps, packing, gaskets, sound absorbing materials, soles, etc.

[0031] [Rubber products] The rubber product of the present invention is a vulcanized rubber obtained by vulcanizing the rubber composition of the present invention, and exhibits excellent fracture resistance and low heat build-up. The rubber product of the present invention is a rubber product other than a tire. Specific examples include conveyor belts, crawlers, anti-vibration rubber, vibration-damping rubber, seismic isolation rubber, hoses and tubes, piping, cables, sealing materials, caps, packing, gaskets, sound-absorbing materials, soles, etc. EXAMPLES

[0032] [Preparation of Rubber Composition] The rubber compositions were prepared by kneading the components in two stages according to the compounding composition (the values ​​in the table are parts by mass) shown in Table 1 below. The details of the components in the table are as follows.

[0033] 1. Rubber component NR: Natural rubber (RSS♯3) BR: Modified polybutadiene rubber obtained by the following method SBR: Modified styrene-butadiene copolymer rubber obtained by the following method 2.Copolymer Copolymer 1: Methacrylic acid-based random copolymer obtained by polymerizing monomer components of 25 mol% GMA, 50 mol% HEMA, and 25 mol% MMA, weight average molecular weight in polystyrene equivalent: 3,800, granular (room temperature) Copolymer 2: Methacrylic acid-based random copolymer obtained by polymerizing monomer components of 25 mol% GMA, 50 mol% HEMA, and 25 mol% MMA, weight average molecular weight in polystyrene equivalent: 7,300, granular (room temperature) The weight average molecular weight was measured by gel permeation chromatography (GPC: HLC-8121GPC / HT manufactured by Tosoh Corporation, column: GMH manufactured by Tosoh Corporation). HR The measurements were performed using two -H(S)HT tubes, detector: differential refractometer (RI) at a measurement temperature of 40°C, and the values ​​were calculated using monodisperse polystyrene as the standard. 3. Fillers Silica: Cetyltrimethylammonium bromide specific surface area (CTAB) 191m 2 / g Silica Carbon black: SAF grade carbon 4. Silane coupling agents Bis-(triethoxysilylpropyl)-polysulfide 5. Resin C5 Aliphatic Hydrocarbon Resin 6. Vulcanization accelerator A mixture of sulfenamide and thiazole vulcanization accelerators

[0034] <Method of manufacturing modified polybutadiene rubber> A glass bottle with a rubber stopper and a volume of about 1 liter was dried and purged with nitrogen. A cyclohexane solution of dried and purified butadiene and dry cyclohexane were put into the glass bottle, so that 330 g of a cyclohexane solution containing 15.0 mass % butadiene was put into the bottle. 0.513 mmol of hexamethyleneimine (HMI) was put into the bottle. Next, 0.36 mL of tert-butyllithium (1.57 M) and 0.057 mL of 2,2-di(2-tetrahydrofuryl)propane (0.2 N) were added, and polymerization was carried out for 4.5 hours in a water bath at 50 ° C. Then, 0.10 mmol of tin tetrachloride (SnCl4) was added, and the reaction was carried out at 50 ° C. for 1 hour. After that, the mixture was reprecipitated in isopropanol containing a trace amount of 2,2'-methylene-bis(4-ethyl-6-t-butylphenol) (NS-5), and then dried in a drum to obtain a modified butadiene rubber. The yield was nearly 100%.

[0035] <Method of manufacturing modified styrene-butadiene copolymer rubber> A cyclohexane solution of 1,3-butadiene and a cyclohexane solution of styrene were added to a dried, nitrogen-substituted 800 mL pressure-resistant glass vessel so that the resulting mixture was 67.5 g of 1,3-butadiene and 7.5 g of styrene. 0.6 mmol of 2,2-ditetrahydrofurylpropane was added, and 0.8 mmol of n-butyllithium was added, followed by polymerization at 50°C for 1.5 hours. The polymerization conversion rate at this time was almost 100%. 0.72 mmol of [N,N-bis(trimethylsilyl)-(3-amino-1-propyl)](methyl)(diethoxy)silane was added to this polymerization reaction system, and a modification reaction was carried out at 50°C for 30 minutes. Thereafter, 2 mL of a 5% by mass solution of 2,6-di-t-butyl-p-cresol (BHT) in isopropanol was added to stop the reaction, and the mixture was dried according to a conventional method to obtain a modified styrene-butadiene copolymer rubber. The microstructure of the obtained modified styrene-butadiene copolymer rubber was measured, and the bound styrene content was 10% by mass, the vinyl content of the butadiene portion was 40%, and the peak molecular weight in terms of polystyrene obtained by gel permeation chromatography was 200,000.

[0036] [evaluation] 1.Low heat generation evaluation The rubber compositions of the examples and comparative examples were vulcanized at 145°C for 33 minutes to obtain vulcanized rubber. Test pieces were obtained from the obtained vulcanized rubber, and the loss tangent (tan δ) of the vulcanized rubber was measured using a viscoelasticity measuring device under the conditions of dynamic strain: 10%, frequency: 15Hz, and measurement temperature: 30°C. The tan δ of the vulcanized rubber of Comparative Example 1 was set to 100, and the measured values ​​of each Example and Comparative Example were expressed as an index. The results are shown in Table 1. A larger index indicates that the rubber product has better low heat build-up properties.

[0037] 2. Destruction resistance performance evaluation For each vulcanized rubber, a tensile test was carried out at room temperature in accordance with JIS K6301-1995 to measure the tensile strength (TB). The tensile strength of the test piece of Comparative Example 1 was set as 100, and the tensile strength was expressed as an index according to the following formula. Fracture resistance index = (tensile strength of test piece other than Comparative Example 1 / tensile strength of test piece of Comparative Example 1) × 100 A higher fracture property index indicates that the rubber product has better fracture properties.

[0038] [Table 1]

[0039] The rubber products using the rubber compositions of the Examples containing the above-mentioned methacrylic acid-based copolymers all had significantly improved fracture resistance compared to the Comparative Examples. In addition, the rubber products obtained from the rubber compositions of the Examples had low heat build-up properties comparable to those of the Comparative Examples.

Claims

1. A rubber component, A vulcanized rubber product (excluding tires) which is a product of vulcanized rubber obtained by vulcanizing a rubber composition containing a copolymer obtained by polymerizing a monomer component containing glycidyl (meth)acrylate, 2-hydroxyethyl (meth)acrylate, and methyl (meth)acrylate, In the monomer components, the ratio of the glycidyl (meth)acrylate is 8 to 37 mol %, the ratio of the 2-hydroxyethyl (meth)acrylate is 27 to 85 mol %, and the ratio of the methyl (meth)acrylate is 6 to 47 mol %, The copolymer is contained in an amount of 0.1 to 20 parts by mass based on 100 parts by mass of the rubber component. Vulcanized rubber products (excluding tyres).

2. 10. The vulcanized rubber article (excluding tires) of claim 1, wherein said copolymer is a solid at room temperature.

3. 3. The vulcanized rubber product (excluding tires) according to claim 1 or 2, wherein the copolymer has a weight average molecular weight in terms of polystyrene of 2,000 to 20,000.

4. The vulcanized rubber product (excluding tires) according to any one of claims 1 to 3, which contains carbon black as a filler.

5. The vulcanized rubber product (excluding tires) according to any one of claims 1 to 4, further comprising silica as a filler.

6. The vulcanized rubber product (excluding tires) according to any one of claims 1 to 5, wherein the rubber component comprises natural rubber, polybutadiene rubber, and styrene-butadiene rubber.

7. The vulcanized rubber product (excluding tires) according to claim 6, wherein the proportion of the natural rubber is 20 to 60% by mass, the proportion of the polybutadiene rubber is 20 to 60% by mass, and the proportion of the styrene-butadiene rubber is 10 to 40% by mass.

Citation Information

Patent Citations

  • Backing composition

    JP1987078273A

  • Pneumatic tire for heavy loading use

    JP2006152212A

  • Rubber composition and pneumatic tire using the same

    JP2006274049A

  • Rubber composition and pneumatic tire