Compatibilizer
A compatibilizer with a block polymer structure addresses the compatibility and mechanical strength issues in resin compositions, enhancing the properties of molded articles.
Patent Information
- Application Number
- JP2021034281
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2020-04-15
- Filing Date
- 2021-03-04
- Publication Date
- 2024-12-05
- Estimated Expiration
- 2041-03-04
AI Technical Summary
Existing resin compositions with different polarities have insufficient compatibility and mechanical strength, leading to unsatisfactory properties in molded articles.
A compatibilizer is developed using a block polymer with a hydrophobic polyolefin and a hydrophilic polymer, specifically designed to enhance the mechanical strength and compatibility of resin compositions.
The compatibilizer provides excellent mechanical strength and compatibility, resulting in improved appearance and performance of molded articles.
Smart Images

Figure 0007594942000001 
Figure 0007594942000002
Abstract
Description
[Technical field]
[0001] The present invention relates to a compatibilizer. [Background technology]
[0002] Resins with different polarities cannot be simply blended, and for this reason, attempts have been made to develop thermoplastic resins using compatibilizers (for example, Patent Document 1). [Prior art documents] [Patent documents]
[0003] [Patent Document 1] JP 2000-017120 A Summary of the Invention [Problem to be solved by the invention]
[0004] However, even with the technology of Patent Document 1, the compatibility of the resin composition is insufficient, and the mechanical strength of the molded article of the resin composition is not satisfactory. An object of the present invention is to provide a compatibilizer which imparts excellent mechanical strength to molded articles of resin compositions. [Means for solving the problem]
[0005] As a result of investigations aimed at achieving the above object, the present inventors have arrived at the present invention, which relates to a compatibilizer (X) for polyacetal resins, comprising a block polymer (A) having as its constituent units a block of a hydrophobic polymer (a) which is a polyolefin (a2) and a block of a hydrophilic polymer (b). Effect of the Invention
[0006] The compatibilizer (X) for polyacetal resin of the present invention has the following effects. (1) It gives excellent mechanical strength (tensile strength, impact strength) to articles molded from the resin composition. (2) Excellent compatibility, giving molded products an excellent appearance. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0007] <Polyolefin (a2)> The polyolefin (a2) in the present invention is a polyolefin which is a hydrophobic polymer (a). The hydrophobic polymer means a polymer having a water absorption rate (24 hours) of less than 0.1% by weight. The water absorption rate (24 hours) in the present invention can be measured by a known measurement method. That is, the water absorption rate can be measured according to the method for determining the water absorption rate described in JIS K7209 (2000).
[0008] Examples of polyolefin (a2) include polyolefin (a2-1) having carboxyl groups at both ends of the polymer, polyolefin (a2-2) having hydroxyl groups at both ends of the polymer, polyolefin (a2-3) having amino groups at both ends of the polymer, polyolefin (a2-4) having isocyanate groups at both ends of the polymer, polyolefin (a2-5) having carboxyl groups at one end of the polymer, polyolefin (a2-6) having hydroxyl groups at one end of the polymer, polyolefin (a2-7) having amino groups at one end of the polymer, and polyolefin (a2-8) having isocyanate groups at one end of the polymer, etc. Among these, (a2-1) and (a2-5) having carboxyl groups at the ends are preferred. In the present invention, the term "terminal" refers to the end where the repeating structure of the monomer units constituting the polymer is interrupted. In addition, "both terminals" refers to both terminals in the main chain of the polymer, and "one terminal" refers to either terminal in the main chain of the polymer.
[0009] As (a2-1), there can be used polyolefin (a2-01) having as its main component a polyolefin whose both ends are modifiable (preferably with a content of 50% by weight or more, more preferably 75% by weight or more, and particularly preferably 80 to 100% by weight) with carboxyl groups introduced at both ends; as (a2-2), there can be used (a2-01) with hydroxyl groups introduced at both ends; as (a2-3), there can be used (a2-01) with amino groups introduced at both ends; and as (a2-4), there can be used (a2-01) with isocyanate groups introduced at both ends.
[0010] As the polyolefins (a2-5) to (a2-8), instead of the polyolefins (a2-01), it is possible to use polyolefins (a2-02) which are mainly composed of polyolefins (preferably with a content of 50% by weight or more, more preferably 75% by weight or more, and particularly preferably 80 to 100% by weight) whose one end is modifiable, and which have a carboxyl group, a hydroxyl group, an amino group or an isocyanate group introduced at one end.
[0011] The polyolefin (a2-01) mainly composed of a polyolefin whose both ends can be modified includes polyolefins obtained by (co)polymerization (co)polymerization means polymerization or copolymerization. The same applies below) of one or a mixture of two or more olefins having 2 to 30 carbon atoms (preferably 2 to 12, more preferably 2 to 10) (polymerization method) and degraded polyolefins {those obtained by mechanically, thermally or chemically degrading high molecular weight polyolefins (preferably having a number average molecular weight (hereinafter abbreviated as Mn) of 50,000 to 150,000) (degradation method)}. Among these, from the viewpoints of ease of modification when introducing a carboxyl group, a hydroxyl group, an amino group, or an isocyanate group, and ease of availability, degraded polyolefins are preferred, and thermally degraded polyolefins are more preferred. By the thermal degradation, as described below, low molecular weight polyolefins having an average number of terminal double bonds of 1.5 to 2 per molecule can be easily obtained, and the low molecular weight polyolefins can be easily modified by introducing a carboxyl group, a hydroxyl group, an amino group, an isocyanate group, or the like.
[0012] In the present invention, Mn (number average molecular weight) and Mw (weight average molecular weight) can be measured by gel permeation chromatography (GPC) under the following conditions. Equipment (example): "HLC-8120" [Tosoh Corporation] Column (example): "TSKgelGMHXL" (2 pieces) "TSKgel Multipore HXL-M" (1 tube) Sample solution: 0.3% by weight orthodichlorobenzene solution Solution injection volume: 100μl Flow rate: 1ml / min Measurement temperature: 135℃ Detector: Refractive index detector Reference material: 12 standard polystyrenes (TSKstandard POLYSTYRENE) (molecular weight: 500, 1,050, 2,800, 5,970, 9,100, 18,100, 37,900, 96,400, 190,000, 355,000, 1,090,000, 2,890,000) [manufactured by Tosoh Corporation]
[0013] The thermally degraded polyolefin is not particularly limited, but examples thereof include those obtained by heating a high molecular weight polyolefin in an inert gas (at 300 to 450°C for 0.5 to 10 hours, for example, those obtained by the method described in JP-A-3-62804), and those thermally degraded by heating in air.
[0014] The high molecular weight polyolefin used in the thermal degradation method includes a (co)polymer of one or a mixture of two or more olefins having 2 to 30 carbon atoms (preferably 2 to 12, more preferably 2 to 10) [Mn is preferably 12,000 to 100,000, more preferably 15,000 to 70,000. Melt flow rate (hereinafter abbreviated as MFR, unit is g / 10 min) is preferably 0.5 to 150, more preferably 1 to 100.]. Here, MFR is a value that indicates the melt viscosity of a resin, and the larger the value, the lower the melt viscosity. For measuring MFR, an extrusion type plastometer specified in JIS K6760 is used, and the measuring method is in accordance with the method specified in JIS K7210 (1976). For example, in the case of polypropylene, it is measured under the conditions of 230°C and a load of 2.16 kgf. Examples of the olefin having 2 to 30 carbon atoms include α-olefins having 2 to 30 carbon atoms and dienes having 4 to 30 carbon atoms. Examples of the α-olefin having 2 to 30 carbon atoms include ethylene, propylene, 1-butene, 4-methyl-1-pentene, 1-pentene, 1-octene, 1-decene, 1-dodecene, 1-icosene, and 1-tetracosene. Examples of dienes having 4 to 30 carbon atoms include butadiene, isoprene, cyclopentadiene, and 1,11-dodecadiene. Among the olefins having 2 to 30 carbon atoms, from the viewpoint of molecular weight control, preferred are ethylene, propylene, α-olefins having 4 to 12 carbon atoms, butadiene, isoprene, and mixtures thereof, more preferred are ethylene, propylene, α-olefins having 4 to 10 carbon atoms, butadiene, and mixtures thereof, and particularly preferred are ethylene, propylene, butadiene, and mixtures thereof.
[0015] From the viewpoints of compatibility and reactivity with the hydrophilic polymer (b) described below, the Mn of the polyolefin (a2-01) is preferably 800 to 20,000, more preferably 1,000 to 10,000, and particularly preferably 1,200 to 6,000. The number of terminal double bonds in (a2-01) is preferably 1 to 40, more preferably 2 to 30, and particularly preferably 4 to 20 per 1,000 carbon atoms, from the viewpoint of controlling the molecular weight of the block polymer (A).
[0016] The average number of terminal double bonds per molecule of (a2-01) is preferably 1.1 to 5, more preferably 1.3 to 3, particularly preferably 1.5 to 2.5, and most preferably 1.8 to 2.2, from the viewpoints of ease of forming a repeating structure in the molecule and the thermoplasticity of the block polymer (A) described later.
[0017] By using a method for obtaining low molecular weight polyolefins by thermal degradation, it is easy to obtain (a2-01) with an average number of terminal double bonds of 1.5 to 2 per molecule in the range of Mn 800 to 6,000 [Murata Katsuhide, Makino Tadahiko, Journal of the Chemical Society of Japan, p. 192 (1975)].
[0018] Polyolefin (a2-02) mainly composed of a polyolefin whose one end can be modified can be obtained in the same manner as (a2-01). From the viewpoints of compatibility and mechanical strength (mechanical properties), Mn of (a2-02) is preferably 2,000 to 50,000, more preferably 2,500 to 30,000, and particularly preferably 3,000 to 20,000. The number of double bonds in (a2-02) per 1,000 carbon atoms is preferably 0.3 to 20, more preferably 0.5 to 15, and particularly preferably 0.7 to 10, from the viewpoint of controlling the molecular weight of the block polymer (A).
[0019] The average number of double bonds per molecule of (a2-02) is preferably 0.5 to 1.4, more preferably 0.6 to 1.3, particularly preferably 0.7 to 1.2, and most preferably 0.8 to 1.1, from the viewpoints of ease of forming a repeating structure in the molecule and the thermoplasticity of the block polymer (A) described later. Among (a2-02), from the viewpoint of ease of modification, low molecular weight polyolefins obtained by thermal degradation are preferred, and polyethylene and / or polypropylene having an Mn of 3,000 to 20,000 obtained by thermal degradation are more preferred. When a method for obtaining a low molecular weight polyolefin by thermal degradation is used, (a2-02) having Mn in the range of 6,000 to 30,000 and an average number of terminal double bonds per molecule of 1 to 1.5 is obtained. The low molecular weight polyolefin obtained by the thermal degradation method has the above-mentioned average number of terminal double bonds, and therefore can be easily modified by introducing a carboxyl group, a hydroxyl group, an amino group, an isocyanate group, or the like.
[0020] In addition, (a2-01) and (a2-02) are obtained, for example, as a mixture thereof, and the mixture may be used as it is or after purification and separation. Among these, the mixture is preferable from the viewpoint of production cost, etc.
[0021] Hereinafter, we will explain (a2-1) to (a2-4) which have a carboxyl group, a hydroxyl group, an amino group or an isocyanate group at both ends of the polyolefin (a2-01). However, (a2-5) to (a2-8) which have such a group at one end of the polyolefin (a2-02) can be obtained in the same manner as (a2-1) to (a2-4) by replacing (a2-01) with (a2-02).
[0022] Examples of the polyolefin (a2-1) having carboxyl groups at both polymer terminals include polyolefin (a2-1-1) having a structure in which the terminals of (a2-01) are modified with α,β-unsaturated carboxylic acid (anhydride) (meaning α,β-unsaturated carboxylic acid, its alkyl (having 1 to 4 carbon atoms) ester or its anhydride; the same applies below. Polyolefin (a2-1-2) having a structure in which (a2-1-1) is secondarily modified with lactam or aminocarboxylic acid; polyolefin (a2-1-3) having a structure in which (a2-01) is modified by oxidation or hydroformylation; polyolefin (a2-1-4) having a structure in which (a2-1-3) is secondarily modified with lactam or aminocarboxylic acid; and mixtures of two or more of these polyolefins.
[0023] (a2-1-1) can be obtained by modifying (a2-01) with an α,β-unsaturated carboxylic acid (anhydride). Examples of the α,β-unsaturated carboxylic acid (anhydride) used for modification include monocarboxylic acid, dicarboxylic acid, alkyl (carbon number 1 to 4) esters of mono- or dicarboxylic acid, and anhydrides of mono- or dicarboxylic acid, and specific examples thereof include (meth)acrylic acid ((meth)acrylic acid means acrylic acid or methacrylic acid, the same applies below), methyl (meth)acrylate, butyl (meth)acrylate, maleic acid (anhydride), dimethyl maleate, fumaric acid, itaconic acid (anhydride), diethyl itaconate, and citraconic acid (anhydride). Among these, from the viewpoint of ease of modification, preferred are dicarboxylic acids, alkyl esters of mono- or dicarboxylic acids, and anhydrides of mono- or dicarboxylic acids, more preferred are maleic acid (anhydride) and fumaric acid, and particularly preferred is maleic acid (anhydride).
[0024] The amount of α,β-unsaturated carboxylic acid (anhydride) used for modification is preferably 0.5 to 40% by weight, more preferably 1 to 30% by weight, and particularly preferably 2 to 20% by weight, based on the weight of polyolefin (a2-01), from the viewpoints of the ease of forming a repeating unit in the molecule and the thermoplasticity of the block polymer (A) described below. The modification with an α,β-unsaturated carboxylic acid (anhydride) can be carried out, for example, by subjecting the terminal double bond of (a2-01) to an addition reaction (ene reaction) with an α,β-unsaturated carboxylic acid (anhydride) by either a solution method or a melt method, and the reaction temperature is preferably 170 to 230°C.
[0025] (a2-1-1) can be obtained by secondarily modifying (a2-1) with a lactam or an aminocarboxylic acid. The lactam used for the secondary modification includes lactams having 6 to 12 carbon atoms (preferably 6 to 8, more preferably 6), and specific examples thereof include caprolactam, enantholactam, laurolactam, and undecanolactam. Examples of the aminocarboxylic acid include aminocarboxylic acids having 2 to 12 carbon atoms (preferably 4 to 12, and more preferably 6 to 12). Specific examples include amino acids (glycine, alanine, valine, leucine, isoleucine, phenylalanine, etc.), ω-aminocaproic acid, ω-aminoenanthic acid, ω-aminocaprylic acid, ω-aminopergonic acid, ω-aminocapric acid, 11-aminoundecanoic acid, and 12-aminododecanoic acid. Among the lactams and aminocarboxylic acids, preferred are caprolactam, laurolactam, glycine, leucine, ω-aminocaprylic acid, 11-aminoundecanoic acid and 12-aminododecanoic acid, more preferred are caprolactam, laurolactam, ω-aminocaprylic acid, 11-aminoundecanoic acid and 12-aminododecanoic acid, and particularly preferred are caprolactam and 12-aminododecanoic acid.
[0026] The amount of lactam or aminocarboxylic acid used for the secondary modification is preferably 0.5 to 200% by weight, more preferably 1 to 150% by weight, and particularly preferably 2 to 100% by weight, based on the weight of the modified substance (a2-1), from the viewpoints of the ease of forming a repeating unit in the molecule and the thermoplasticity of the block polymer (A).
[0027] (a2-3) can be obtained by oxidizing (a2-01) with oxygen and / or ozone (oxidation method), or by introducing a carboxyl group by hydroformylation using the oxo method. The introduction of a carbonyl group by oxidation can be carried out by known methods, for example, the method described in U.S. Patent No. 3,692,877. The introduction of a carbonyl group by hydroformylation can be carried out by various methods, including known methods, for example, the method described in Macromolecules, Vol. 31, p. 5943. (a2-4) can be obtained by secondarily modifying (a2-3) with a lactam or an aminocarboxylic acid. Examples of the lactam and aminocarboxylic acid include the same as those exemplified as the lactam and aminocarboxylic acid used in the secondary modification of (a2-1) above, and the preferred ranges and amounts used are also the same.
[0028] From the viewpoints of heat resistance and reactivity with the hydrophilic polymer (b) described below, Mn of (a2-1) is preferably 800 to 25,000, more preferably 1,000 to 20,000, and particularly preferably 2,500 to 10,000. In addition, from the viewpoints of reactivity with (b) and thermoplasticity of the block polymer (A), the acid value of (a2-1) is preferably 4 to 280 mgKOH / g, more preferably 4 to 100 mgKOH / g, and particularly preferably 5 to 50 mgKOH / g.
[0029] As the polyolefin (a2-2) having hydroxyl groups at both polymer terminals, a polyolefin having hydroxyl groups obtained by modifying the polyolefin (a2-1) having carboxyl groups at both polymer terminals with an amine having a hydroxyl group, or a mixture of two or more of these can be used. Examples of amines having a hydroxyl group that can be used for modification include amines having a hydroxyl group and having 2 to 10 carbon atoms, and specific examples thereof include 2-aminoethanol, 3-aminopropanol, 1-amino-2-propanol, 4-aminobutanol, 5-aminopentanol, 6-aminohexanol, and 3-aminomethyl-3,5,5-trimethylcyclohexanol. Among these, from the viewpoint of ease of modification, preferred are amines having a hydroxyl group having 2 to 6 carbon atoms (2-aminoethanol, 3-aminopropanol, 4-aminobutanol, 5-aminopentanol, 6-aminohexanol, etc.), more preferred are 2-aminoethanol and 4-aminobutanol, and particularly preferred is 2-aminoethanol.
[0030] The amount of the amine having a hydroxyl group used for modification is preferably 0.5 to 50% by weight, more preferably 1 to 40% by weight, and particularly preferably 2 to 30% by weight, based on the weight of the modified substance (a2-1), from the viewpoints of the ease of forming a repeating unit in the molecule and the thermoplasticity of the block polymer (A) described below. From the viewpoints of heat resistance and reactivity with the hydrophilic polymer (b) described below, Mn of (a2-2) is preferably 800 to 25,000, more preferably 1,000 to 20,000, and particularly preferably 2,500 to 10,000. From the viewpoints of reactivity with (b) and thermoplasticity of the block polymer (A), the hydroxyl value of (a2-2) is preferably 4 to 280 mgKOH / g, more preferably 4 to 100 mgKOH / g, and particularly preferably 5 to 50 mgKOH / g.
[0031] As the polyolefin (a2-3) having amino groups at both polymer terminals, a polyolefin having amino groups obtained by modifying the polyolefin (a2-1) having carboxyl groups at both polymer terminals with a diamine (Q1), or a mixture of two or more of these can be used. As the diamine (Q1), diamines having 2 to 12 carbon atoms can be used, and specific examples thereof include ethylenediamine, hexamethylenediamine, heptamethylenediamine, octamethylenediamine, and decamethylenediamine. Among these, from the viewpoint of ease of modification, diamines having 2 to 8 carbon atoms (such as ethylenediamine, hexamethylenediamine, heptamethylenediamine, and octamethylenediamine) are preferred, ethylenediamine and hexamethylenediamine are more preferred, and ethylenediamine is particularly preferred.
[0032] The amount of (Q1) used to modify (a2-1) is preferably 0.5 to 50% by weight, more preferably 1 to 40% by weight, and particularly preferably 2 to 30% by weight, based on the weight of (a2-1), from the viewpoint of the ease of forming a repeating structure in the molecule and the thermoplasticity of the block polymer (A) described later. In addition, the modification of (a2-1) with (Q1) is preferably performed by using preferably 0.5 to 1,000% by weight, more preferably 1 to 500% by weight, and particularly preferably 2 to 300% by weight, based on the weight of (a2-1), and then removing unreacted (Q1) under reduced pressure at 120 to 230° C., from the viewpoint of preventing polyamide (imide) formation.
[0033] From the viewpoints of heat resistance and reactivity with the hydrophilic polymer (b) described below, Mn of (a2-3) is preferably 800 to 25,000, more preferably 1,000 to 20,000, and particularly preferably 2,500 to 10,000. The amine value of (a2-3) is preferably 4 to 280 mgKOH / g, more preferably 4 to 100 mgKOH / g, and particularly preferably 5 to 50 mgKOH / g, from the viewpoints of reactivity with (b) and thermoplasticity of the block polymer (A).
[0034] Examples of the polyolefin (a2-4) having isocyanate groups at both ends include polyolefins having isocyanate groups obtained by modifying (a2-2) with poly(2 to 3 or more) isocyanate (hereinafter abbreviated as PI), and mixtures of two or more of these. Examples of PI include aromatic PIs having 6 to 20 carbon atoms (excluding carbon atoms in NCO groups, the same applies below), aliphatic PIs having 2 to 18 carbon atoms, alicyclic PIs having 4 to 15 carbon atoms, aromatic aliphatic PIs having 8 to 15 carbon atoms, modified versions of these PIs, and mixtures of two or more of these.
[0035] Examples of aromatic PI include 1,3- or 1,4-phenylene diisocyanate, 2,4- or 2,6-tolylene diisocyanate (TDI), crude TDI, 2,4'- or 4,4'-diphenylmethane diisocyanate (MDI), 4,4'-diisocyanatobiphenyl, 3,3'-dimethyl-4,4'-diisocyanatobiphenyl, 3,3'-dimethyl-4,4'-diisocyanatodiphenylmethane, and 1,5-naphthylene diisocyanate.
[0036] Examples of aliphatic PIs include ethylene diisocyanate, tetramethylene diisocyanate, hexamethylene diisocyanate (HDI), dodecamethylene diisocyanate, 2,2,4-trimethylhexamethylene diisocyanate, lysine diisocyanate, 2,6-diisocyanatomethyl caproate, bis(2-isocyanatoethyl) fumarate, bis(2-isocyanatoethyl) carbonate, and 2-isocyanatoethyl-2,6-diisocyanatohexanoate.
[0037] Examples of alicyclic PIs include isophorone diisocyanate (IPDI), dicyclohexylmethane-4,4'-diisocyanate (hydrogenated MDI), cyclohexylene diisocyanate, methylcyclohexylene diisocyanate (hydrogenated TDI), bis(2-isocyanatoethyl)-4-cyclohexene-1,2-dicarboxylate, and 2,5- or 2,6-norbornane diisocyanate.
[0038] Examples of the aromatic aliphatic PI include m- or p-xylylene diisocyanate (XDI) and α,α,α',α'-tetramethylxylylene diisocyanate (TMXDI).
[0039] Examples of modified PI include urethane modified PI, urea modified PI, carbodiimide modified PI, and uretdione modified PI. Among the PIs, TDI, MDI and HDI are preferred, and HDI is more preferred.
[0040] The reaction of PI with (a2-2) can be carried out, for example, in the same manner as in the urethanization reaction. The molar equivalent ratio (NCO / OH) of PI to (a2-2) is preferably 1.8 / 1 to 3 / 1, and more preferably 2 / 1. In order to promote the urethanization reaction, a known catalyst used in the urethanization reaction may be used as necessary. Examples of the catalyst include metal catalysts {tin catalysts [dibutyltin dilaurate and stannous octoate, etc.], lead catalysts [lead 2-ethylhexanoate and lead octenate, etc.], other metal catalysts [metal naphthenate (cobalt naphthenate, etc.) and phenylmercury propionate, etc.]}; amine catalysts {triethylenediamine, diazabicycloalkene [1,8-diazabicyclo[5,4,0]undecene-7, etc.], dialkylaminoalkylamines (dimethylaminoethylamine and dimethylaminooctylamine, etc.), carbonates or organic acid (formic acid, etc.) salts of heterocyclic aminoalkylamines [2-(1-aziridinyl)ethylamine and 4-(1-piperidinyl)-2-hexylamine, etc.], N-methyl or ethylmorpholine, triethylamine and diethyl- or dimethylethanolamine, etc.}; and combinations of two or more of these. The amount of the catalyst used is preferably 3% by weight or less, and more preferably 0.001 to 2% by weight, based on the total weight of PI and (a2-2).
[0041] From the viewpoints of heat resistance and reactivity with the hydrophilic polymer (b) described below, Mn of (a2-4) is preferably 800 to 25,000, more preferably 1,000 to 20,000, and particularly preferably 2,500 to 10,000.
[0042] From the viewpoints of compatibility and mechanical strength, the Mn of the polyolefin (a2) is preferably from 200 to 25,000, more preferably from 500 to 20,000, and particularly preferably from 1,000 to 15,000.
[0043] <Hydrophilic polymer (b)> The hydrophilic polymer (b) in the present invention means a polymer having a water absorption rate (24 hours) of 0.1% by weight or more.
[0044] Examples of the hydrophilic polymer (b) include hydrophilic polymers described in Japanese Patent No. 3488163, and specific examples thereof include polyether (b1), polyether-containing hydrophilic polymer (b2), cationic polymer (b3), and anionic polymer (b4). Of the above hydrophilic polymers (b), from the viewpoints of mechanical strength (mechanical properties) and compatibility, (b1) and (b2) are preferred.
[0045] Examples of the polyether (b1) include polyether diols (b1-1), polyether diamines (b1-2) and modified products thereof (b1-3). The polyether diol (b1-1) may be one obtained by subjecting the diol (b0) to an addition reaction with an alkylene oxide (hereinafter abbreviated as AO), and specifically may be one represented by the general formula (1). H-(OR 1 ) m -OE 1 -O-(R 2 O) n -H (1)
[0046] E in general formula (1) 1 is the residue obtained by removing all hydroxyl groups from diol (b0). Examples of the diol (b0) include aliphatic dihydric alcohols having 2 to 12 carbon atoms, alicyclic dihydric alcohols having 5 to 12 carbon atoms, aromatic dihydric alcohols having 6 to 18 carbon atoms, and tertiary amino group-containing diols. Examples of the aliphatic dihydric alcohol having 2 to 12 carbon atoms include ethylene glycol (hereinafter abbreviated as EG), 1,2-propylene glycol (hereinafter abbreviated as PG), 1,4-butanediol (hereinafter abbreviated as 1,4-BD), 1,6-hexanediol (hereinafter abbreviated as 1,6-HD), neopentyl glycol (hereinafter abbreviated as NPG), and 1,12-dodecanediol.
[0047] Examples of the alicyclic dihydric alcohols having 5 to 12 carbon atoms include 1,4-di(hydroxymethyl)cyclohexane and 1,5-di(hydroxymethyl)cycloheptane. Examples of aromatic dihydric alcohols having 6 to 18 carbon atoms include monocyclic aromatic dihydric alcohols (xylylenediol, hydroquinone, catechol, resorcin, urushiol, bisphenol A, bisphenol F, bisphenol S, 4,4'-dihydroxydiphenyl-2,2-butane, dihydroxybiphenyl, etc.) and polycyclic aromatic dihydric alcohols (dihydroxynaphthalene, binaphthol, etc.). Examples of the tertiary amino group-containing diol include bishydroxyalkylated products of aliphatic or alicyclic primary amines having 1 to 12 carbon atoms (methylamine, ethylamine, cyclopropylamine, 1-propylamine, 2-propylamine, pentylamine, isopentylamine, cyclopentylamine, hexylamine, cyclohexylamine, heptylamine, nonylamine, decylamine, undecylamine, dodecylamine, etc.) and bishydroxyalkylated products of aromatic primary amines having 6 to 12 carbon atoms (aniline, benzylamine, etc.). Among these, from the viewpoint of reactivity with bishydroxyalkylated products, aliphatic dihydric alcohols having 2 to 12 carbon atoms and aromatic dihydric alcohols having 6 to 18 carbon atoms are preferred, and EG and bisphenol A are more preferred.
[0048] R in general formula (1) 1 and R 2are each independently an alkylene group having 2 to 4 carbon atoms. Examples of the alkylene group having 2 to 4 carbon atoms include an ethylene group, a 1,2- or 1,3-propylene group, and a 1,2-, 1,3-, 1,4- or 2,3-butylene group. In the general formula (1), m and n each independently represent a number from 1 to 300, preferably from 2 to 250, and more preferably from 10 to 100. R in the case where m and n in the general formula (1) are each 2 or more 1 , R 2 may be the same or different, (OR 1 )m, (R 2 O) The n portion may be a random bond or a block bond.
[0049] The polyether diol (b1-1) can be produced by subjecting the diol (b0) to an addition reaction with AO. As the AO, AO having 2 to 4 carbon atoms [ethylene oxide (hereinafter abbreviated as EO), 1,2- or 1,3-propylene oxide (hereinafter abbreviated as PO), 1,2-, 1,3-, 1,4-, 2,3- or butylene oxide (hereinafter abbreviated as BO), and a combination of two or more of these are used, but if necessary, other AO [α-olefin oxide having 5 to 12 carbon atoms, styrene oxide, epihalohydrin (epichlorohydrin, etc.), etc.] can also be used in combination in a small proportion (30% by weight or less based on the total weight of the AO). When two or more kinds of AO are used in combination, the bonding form may be either random bonding or block bonding. Preferred as AO is EO alone or a combination of EO and another AO.
[0050] The addition reaction of AO can be carried out by a known method, for example, in the presence of an alkali catalyst at a temperature of 100 to 200°C. (OR 1 )m and (R 2 The content of O)n is preferably 5 to 99.8% by weight, more preferably 8 to 99.6% by weight, and particularly preferably 10 to 98% by weight. In general formula (1), (OR 1 )m and (R 2 The content of oxyethylene groups based on the weight of O)n is preferably 5 to 100% by weight, more preferably 10 to 100% by weight, particularly preferably 50 to 100% by weight, and most preferably 60 to 100% by weight.
[0051] The polyether diamine (b1-2) may be one represented by the general formula (2). H2N-R 3 -(OR 4 ) p -OE 2 -O-(R 5 O) q -R 6 -NH2(2) E in general formula (2) 2 is a residue obtained by removing all hydroxyl groups from diol (b0). Examples of diol (b0) include the same ones as those mentioned above, and the preferred ranges are also the same. R in general formula (2) 3 , R 4 , R 5 and R 6 are each independently an alkylene group having 2 to 4 carbon atoms. Examples of the alkylene group having 2 to 4 carbon atoms include R 1 and R 2 The same as those exemplified above can be mentioned, and the preferred ranges are also the same. In the general formula (2), p and q each independently represent a number from 1 to 300, preferably from 2 to 250, and more preferably from 10 to 100. R in the case where p and q in the general formula (2) are each 2 or more 4 , R 5 may be the same or different, (OR 4 )p, (R 5 O) The q portion may be a random bond or a block bond.
[0052] Polyetherdiamine (b1-2) can be obtained by converting all hydroxyl groups of polyetherdiol (b1-1) to amino groups. For example, it can be produced by reacting (b1-1) with acrylonitrile and hydrogenating the resulting cyanoethylated product.
[0053] Examples of the modified product (b1-3) include amino carboxylic acid modified products (terminal amino group), isocyanate modified products (terminal isocyanate group) and epoxy modified products (terminal epoxy group) of (b1-1) or (b1-2). The aminocarboxylic acid modified product can be obtained by reacting (b1-1) or (b1-2) with an aminocarboxylic acid or a lactam. The isocyanate-modified product can be obtained by reacting (b1-1) or (b1-2) with a polyisocyanate, or by reacting (b1-2) with phosgene. The epoxy modified product can be obtained by reacting (b1-1) or (b1-2) with a diepoxide (an epoxy resin such as a diglycidyl ether, a diglycidyl ester, or an alicyclic diepoxide: epoxy equivalent of 85 to 600) or by reacting (b1-1) with an epihalohydrin (epichlorohydrin, etc.).
[0054] From the viewpoints of heat resistance and reactivity with the hydrophobic polymer (a), the Mn of the polyether (b1) is preferably 150 to 20,000, more preferably 300 to 18,000, particularly preferably 1,000 to 15,000, and most preferably 1,200 to 8,000.
[0055] Examples of the polyether-containing hydrophilic polymer (b2) include polyetheresteramide (b2-1) having a polyetherdiol (b1-1) segment, polyetheramideimide (b2-2) having a (b1-1) segment, polyetherester (b2-3) having a (b1-1) segment, polyetheramide (b2-4) having a polyetherdiamine (b1-2) segment, and polyetherurethane (b2-5) having a (b1-1) or (b1-2) segment.
[0056] The content of the polyether (b1) segment in the polyether-containing hydrophilic polymer (b2) is preferably 30 to 80% by weight, more preferably 40 to 70% by weight, based on the weight of (b2), from the viewpoints of compatibility and mechanical strength. The content of oxyethylene groups in (b2) is preferably 30 to 80% by weight, and more preferably 40 to 70% by weight, based on the weight of (b2), from the viewpoints of compatibility and mechanical strength. The lower limit of Mn of (b2) is preferably 800 from the viewpoint of heat resistance, and more preferably 1,000. The upper limit of Mn of (b2) is preferably 50,000, and more preferably 30,000 from the viewpoint of reactivity with the hydrophobic polymer (a).
[0057] The cationic polymer (b3) may be a polymer having cationic groups separated by nonionic molecular chains within the molecule. Examples of the nonionic molecular chain include divalent hydrocarbon groups, divalent hydrocarbon groups having one or more groups selected from the group consisting of ether bonds, thioether bonds, carbonyl bonds, ester bonds, imino bonds, amide bonds, imide bonds, urethane bonds, urea bonds, carbonate bonds, and siloxy bonds, and hydrocarbon groups having a heterocyclic structure containing a nitrogen atom or an oxygen atom. Of the nonionic molecular chains, a divalent hydrocarbon group and a divalent hydrocarbon group having an ether bond are preferred. The cationic group may be a group having a quaternary ammonium salt or a phosphonium salt. Examples of the counter anion that forms the quaternary ammonium salt or the phosphonium salt include a super strong acid anion and other anions. Examples of superacid anions include anions of superacids derived from a combination of a protonic acid and a Lewis acid (such as tetrafluoroboric acid and hexafluorophosphoric acid) and anions of trifluoromethanesulfonic acid. Other anions include halogen ions (F - , Cl - , Br - and I - etc.), OH - , PO4 - , CH3OSO4 - , C2H5OSO4 - , and ClO4 - etc. The protonic acid which induces the superacid includes hydrogen fluoride, hydrogen chloride, hydrogen bromide, hydrogen iodide, and the like. Examples of Lewis acids include boron trifluoride, phosphorus pentafluoride, antimony pentafluoride, arsenic pentafluoride, and tantalum pentafluoride. (b3) The number of cationic groups in one molecule is preferably 2 to 80, and more preferably 3 to 60.
[0058] Specific examples of (b3) include the cationic polymers described in JP-A-2001-278985.
[0059] From the viewpoints of compatibility and reactivity with the hydrophobic polymer (a), Mn of (b3) is preferably from 500 to 20,000, more preferably from 1,000 to 15,000, and particularly preferably from 1,200 to 8,000.
[0060] The anionic polymer (b4) is a polymer having a dicarboxylic acid (γ') having a sulfonyl group and a diol (b0) or a polyether (b1) as essential constituent units, and having 2 to 80, preferably 3 to 60, sulfonyl groups in the molecule. Examples of (γ') include those in which a sulfonyl group has been introduced into the dicarboxylic acid (γ), such as an aromatic dicarboxylic acid having a sulfonyl group, an aliphatic dicarboxylic acid having a sulfonyl group, and an aromatic dicarboxylic acid or aliphatic dicarboxylic acid having a sulfonyl group in which only the sulfonyl group is in the form of a salt.
[0061] Examples of aromatic dicarboxylic acids having a sulfonyl group include 5-sulfoisophthalic acid, 2-sulfoisophthalic acid, 4-sulfoisophthalic acid, 4-sulfo-2,6-naphthalenedicarboxylic acid, and ester-forming derivatives thereof [alkyl (having 1 to 4 carbon atoms) esters (e.g., methyl esters and ethyl esters) and acid anhydrides]. Examples of the aliphatic dicarboxylic acid having a sulfonyl group include sulfosuccinic acid and its ester-forming derivatives [alkyl (having 1 to 4 carbon atoms) esters (such as methyl ester and ethyl ester) and acid anhydrides]. Examples of salts forming aromatic dicarboxylic acids or aliphatic dicarboxylic acids having a sulfonyl group in which only the sulfonyl group is a salt include alkali metal (lithium, sodium, potassium, etc.) salts, alkaline earth metal (magnesium, calcium, etc.) salts, ammonium salts, amine salts such as mono-, di-, or triamines having a hydroxyalkyl group (having 2 to 4 carbon atoms) (mono-, di-, or triethylamine, mono-, di-, or triethanolamine, diethylethanolamine, etc.), and quaternary ammonium salts of the above amines. Of these, aromatic dicarboxylic acids having a sulfonyl group are preferred, 5-sulfoisophthalic acid salts are more preferred, and 5-sulfoisophthalic acid sodium salt and 5-sulfoisophthalic acid potassium salt are particularly preferred.
[0062] Of the (b0) or (b1) constituting (b4), preferred are alkanediols having 2 to 10 carbon atoms, EG, polyethylene glycol (hereinafter abbreviated as PEG) (degree of polymerization 2 to 20), EO adducts of bisphenols (such as bisphenol A) (number of moles added: 2 to 60 moles), and mixtures of two or more of these. As the method for producing (b4), a known method for producing polyesters can be applied as it is. The polyesterification reaction is carried out at a temperature range of 150 to 240°C under reduced pressure, and the reaction time is preferably 0.5 to 20 hours. If necessary, a catalyst used in a known esterification reaction may be used. Examples of the esterification catalyst include antimony catalysts (antimony trioxide, etc.), tin catalysts (monobutyltin oxide, dibutyltin oxide, etc.), titanium catalysts (tetrabutyl titanate, etc.), zirconium catalysts (tetrabutyl zirconate, etc.), and metal acetate catalysts (zinc acetate, etc.).
[0063] From the viewpoints of compatibility and reactivity with the hydrophobic polymer (a), Mn of (b4) is preferably from 500 to 20,000, more preferably from 1,000 to 15,000, and particularly preferably from 1,200 to 8,000.
[0064] <Block polymer (A)> The block polymer (A) in the present invention has as its constituent units a block of a hydrophobic polymer (a), which is the polyolefin (a2), and a block of a hydrophilic polymer (b). A preferred embodiment of the block polymer is a block polymer having a structure in which a block of (a2) and a block of hydrophilic polymer (b) are bonded via at least one bond selected from the group consisting of an ester bond, an amide bond, an ether bond, an imide bond, a urethane bond, and a urea bond. In the present invention, the polyolefin (a2) may be referred to as a hydrophobic polymer (a) for convenience. The weight ratio of the block (a) and the block (b) constituting (A) is preferably 10 / 90 to 80 / 20, more preferably 20 / 80 to 75 / 25, from the viewpoints of compatibility and mechanical strength.
[0065] The structure in which block (a) and block (b) constituting (A) are bonded includes the (a2)-(b) type, the (a)-(b)-(a) type, the (b)-(a)-(b) type, and the [(a)-(b)] type (n represents the average number of repetitions). From the viewpoints of compatibility and mechanical strength, the structure of the block polymer (A) is preferably an [(a)-(b)]n type in which (a) and (b) are repeatedly and alternately bonded. In the [(a)-(b)]n type structure, n is preferably 2 to 50, more preferably 2.3 to 30, particularly preferably 2.7 to 20, and most preferably 3 to 10, from the viewpoints of compatibility and mechanical strength. n is the Mn and 1 It can be determined by H-NMR analysis.
[0066] From the viewpoint of mechanical strength, Mn of (A) is preferably from 2,000 to 1,000,000, more preferably from 4,000 to 500,000, and particularly preferably from 6,000 to 100,000.
[0067] When (A) has a structure in which the block (a) and the block (b) are bonded via an ester bond, an amide bond, an ether bond, or an imide bond, it can be produced by the following method. One example of such a method is to charge (a) and (b) into a reaction vessel and react them for 1 to 50 hours under stirring at a reaction temperature of 100 to 250°C and a pressure of 0.003 to 0.1 MPa while removing water generated in the amidation reaction, esterification reaction, or imidization reaction (hereinafter abbreviated as generated water) from the reaction system. From the viewpoints of compatibility and mechanical strength, the weight ratio of (a) and (b) is 10 / 90 to 80 / 20, and more preferably 20 / 80 to 75 / 25.
[0068] In the case of the esterification reaction, it is preferable to use 0.05 to 0.5% by weight of a catalyst based on the weight of (a) and (b) in order to promote the reaction. Examples of the catalyst include inorganic acids (sulfuric acid, hydrochloric acid, etc.), organic sulfonic acids (methanesulfonic acid, paratoluenesulfonic acid, xylenesulfonic acid, naphthalenesulfonic acid, etc.), antimony catalysts (antimony trioxide, etc.), tin catalysts (monobutyltin oxide, dibutyltin oxide, etc.), titanium catalysts (tetrabutyl titanate, bistriethanolamine titanate, potassium oxalate titanate, etc.), zirconium catalysts (tetrabutyl zirconate, zirconyl acetate, etc.), and zinc catalysts (zinc acetate, etc.). When a catalyst is used, the catalyst can be neutralized as necessary after the esterification reaction is completed, and the catalyst can be removed and purified by treating with an adsorbent. The following methods can be used to remove the generated water from the reaction system. (1) A method in which an organic solvent that is not miscible with water (e.g., toluene, xylene, cyclohexane, etc.) is used, and the organic solvent and the generated water are subjected to azeotropic distillation under reflux, thereby removing only the generated water from the reaction system. (2) A carrier gas (e.g., air, nitrogen, helium, argon, and carbon dioxide) is introduced into the reaction system. etc.) and remove the generated water from the reaction system together with the carrier gas. (3) A method in which the reaction system is depressurized to remove the generated water from the reaction system.
[0069] When (A) has a structure in which a block (a) and a block (b) are bonded via a urethane bond or a urea bond, it can be produced by the following method. One method is to charge (a) into a reaction vessel, heat with stirring to 30 to 100°C, then charge (b) and react at the same temperature for 1 to 20 hours. From the viewpoints of compatibility and mechanical strength, the weight ratio of (a) to (b) is 10 / 90 to 80 / 20, and more preferably 20 / 80 to 75 / 25. In order to promote the reaction, it is preferable to use 0.001 to 5% by weight of a catalyst based on the weight of (a) and (b). Examples of the catalyst include organometallic compounds (dibutyltin dilaurate, dioctyltin dilaurate, lead octanoate, bismuth octanoate, etc.), tertiary amines {triethylenediamine, trialkylamines having an alkyl group with 1 to 8 carbon atoms (trimethylamine, tributylamine, trioctylamine, etc.), diazabicycloalkenes [1,8-diazabicyclo[5,4,0]undecene-7], etc.}, and combinations of two or more of these.
[0070] <Compatibilizer for polyacetal resin (X)> The polyacetal resin compatibilizer (X) of the present invention contains the block polymer (A). The resin compatibilizer (X) is suitable as a compatibilizer for compatibilizing a polyacetal resin with a resin having a different polarity, and is particularly suitable for compatibilizing a polyacetal resin (E) and a polyolefin resin (D) described below.
[0071] <Polyolefin resin (D)> The polyolefin resin (D) in the present invention includes one or more (co)polymers of olefins, as well as copolymers of one or more olefins with one or more other monomers. The olefins include alkenes having 2 to 30 carbon atoms (hereinafter sometimes abbreviated as C), such as ethylene, propylene, 1- and 2-butene, and isobutene, as well as C5 to C30 α-olefins (1-hexene, 1-decene, 1-dodecene, etc.); other monomers include C4 to C30 unsaturated monomers copolymerizable with olefins, such as vinyl acetate, etc.
[0072] Specific examples of (D) include ethylene unit-containing (propylene unit-free) (co)polymers, such as high-, medium-, and low-density polyethylenes, and copolymers of ethylene and C4-30 unsaturated monomers [butene (1-butene, etc.), C5-30 α-olefins (1-hexene, 1-dodecene, etc.), vinyl acetate, etc.] (weight ratios are preferably 30 / 70 to 99 / 1, more preferably 50 / 50 to 95 / 5); propylene unit-containing (ethylene unit-free) (co)polymers, such as polypropylene, and copolymers of propylene and C4-30 unsaturated monomers (same as above) (weight ratios are the same as above); ethylene / propylene copolymers (weight ratios are preferably 0.5 / 99.5 to 30 / 70, more preferably 2 / 98 to 20 / 80); and (co)polymers of C4 or higher olefins, such as polybutene. Among these, from the viewpoints of mechanical strength and compatibility, preferred are polyethylene, polypropylene, ethylene / propylene copolymer, and propylene / C4-30 unsaturated monomer copolymer, and more preferred are ethylene / propylene copolymer and propylene / C4-30 unsaturated monomer copolymer. From the viewpoints of mechanical strength and compatibility, (D) has a number average molecular weight (Mn) of preferably 10,000 to 500,000, and more preferably 20,000 to 400,000.
[0073] <Polyacetal resin (E)> The polyacetal resin (E) in the present invention may be a known one, or a polymer containing oxymethylene and, if necessary, oxyethylene as unit structures. Commercially available products of (E) include, for example, Delrin (registered trademark, manufactured by DuPont) and Duracon (registered trademark, manufactured by Polyplastics Co., Ltd.). The polyacetal resin (E) may be used either alone or in combination of two or more kinds.
[0074] <Resin composition (Y)> The resin composition (Y) of the present invention contains the above-mentioned compatible solvent for polyacetal resin (X), a polyolefin resin (D), and a polyacetal resin (E). The weight ratio of (D) to (E) [(D) / (E)] is preferably 10 / 90 to 90 / 10, more preferably 15 / 85 to 50 / 50, or 20 / 80 to 40 / 60, from the viewpoints of mechanical strength and compatibility. The weight ratio of the total weight of (D) and (E) to (X), {[(D)+(E)] / (X)}, is preferably 80 / 20 to 99 / 1, and more preferably 90 / 10 to 97 / 3, from the viewpoints of mechanical strength and compatibility.
[0075] The composition may further contain, if necessary, at least one other additive (F) selected from the group consisting of colorants, release agents, antioxidants, flame retardants, UV absorbers, antibacterial agents, fillers, and transesterification inhibitors other than the above-mentioned (A), (D), and (E), as long as the effect of the present invention is not impaired. Each of the (F) may be used alone or in combination of two or more.
[0076] Examples of the colorant (F1) include inorganic pigments [white pigments, cobalt compounds, iron compounds, sulfides, etc.], organic pigments [azo pigments, polycyclic pigments, etc.], dyes [azo-based, indigoid-based, sulfide-based, alizarin-based, acridine-based, thiazole-based, nitro-based, aniline-based, etc.], etc.;
[0077] Examples of the release agent (F2) include lower (C1-4) alcohol esters (butyl stearate, etc.) of higher fatty acids (as mentioned above), polyhydric (dihydric to tetrahydric or higher) alcohol esters (hydrogenated castor oil, etc.) of fatty acids (C2-18), glycol (C2-8) esters (ethylene glycol monostearate, etc.) of fatty acids (C2-18), liquid paraffin, etc.;
[0078] Examples of the antioxidant (F3) include phenol compounds [monocyclic phenols (2,6-di-t-butyl-p-cresol, etc.), bisphenols [2,2'-methylenebis(4-methyl-6-t-butylphenol), etc.], polycyclic phenols [1,3,5-trimethyl-2,4,6-tris(3,5-di-t-butyl-4-hydroxybenzyl)benzene, etc.], sulfur compounds (dilauryl 3,3'-thiodipropionate, etc.), phosphorus compounds (triphenyl phosphite, etc.), amine compounds (octylated diphenylamine, etc.), etc.;
[0079] Examples of the flame retardant (F4) include halogen-containing flame retardants, nitrogen-containing flame retardants, sulfur-containing flame retardants, silicon-containing flame retardants, phosphorus-containing flame retardants, etc.;
[0080] Examples of ultraviolet absorbers (F5) include benzotriazoles [2-(2'-hydroxy-5'-methylphenyl)benzotriazole, etc.], benzophenones [2-hydroxy-4-methoxybenzophenone, etc.], salicylates [phenyl salicylate, etc.], acrylates [2-ethylhexyl-2-cyano-3,3'1-diphenylacrylate, etc.], and the like;
[0081] Antibacterial agents (F6) include benzoic acid, sorbic acid, halogenated phenols, organic iodines, nitriles (e.g., 2,4,5,6-tetrachloroisophthalonitrile), thiocyano (methylenebisthiocyanate), N-haloalkylthioimides, copper agents (e.g., 8-oxyquinoline copper), benzimidazole, benzothiazole, trihaloallyl, triazole, organic nitrogen-sulfur compounds (e.g., Slaof 39), quaternary ammonium compounds, pyridine compounds, and the like;
[0082] Examples of the filler (F8) include inorganic fillers (calcium carbonate, talc, clay, etc.) and organic fillers (urea, calcium stearate, etc.);
[0083] Examples of the transesterification inhibitor (F9) include phosphate esters [bisphenol A bis(diphenyl phosphate), monooctadecyl phosphate, dioctadecyl phosphate, etc.], and phosphite esters [tris(2,4-di-t-butylphenyl)phosphite, etc.].
[0084] The total content of (F) based on the total weight of (D) and (E) is, for example, 45% or less, and from the viewpoints of the effect of each additive and the mechanical strength (mechanical properties) of the molded product, it is preferably 0.001 to 40%, more preferably 0.01 to 35%; from the same viewpoints, the content of each (E) is, (F1) is preferably 0.1 to 3%, more preferably 0.2 to 2%; (F2) is preferably 0.01 to 3%, more preferably 0.05 to 1%; and (F3) is preferably 0.01 to 3%. (F4) is preferably 0.5 to 20%, and more preferably 1 to 10%; (F5) is preferably 0.01 to 3%, and more preferably 0.05 to 1%; (F6) is preferably 0.5 to 20%, and more preferably 1 to 10%; (F8) is preferably 0.5 to 10%, and more preferably 1 to 5%; (F9) is 0.01 to 3%, and more preferably 0.05 to 1%.
[0085] The resin composition of the present invention can be obtained by melt-mixing the resin compatibilizer (X) of the present invention, the polyolefin resin (D), the resin (E), and, if necessary, other additives (F). As a method for melt mixing, generally, each component in a pellet or powder form is mixed in an appropriate mixer (such as a Henschel mixer), and then melt mixed in an extruder to form pellets. The order of addition of each component during melt mixing is not particularly limited. For example, [1] (X), (D), (E), and (F) (if necessary) are all charged at once and melt mixed; [2] A method in which a portion of (X), (D) and / or (E) are melt-mixed in advance to prepare a high-concentration composition of (X) (masterbatch resin composition), and then the remaining (D) and / or (E) and, if necessary, (F) are melt-mixed (masterbatch method or master pellet method); etc. In the method [2], the concentration of (X) in the masterbatch resin composition is preferably 40 to 80% by weight, and more preferably 50 to 70% by weight. Of the methods [1] and [2], the method [2] is preferred from the viewpoint of facilitating efficient dispersion of (X) in the resin composition.
[0086] <Molded products> The molded article of the present invention can be obtained by molding the resin composition (Y) of the present invention. Examples of the molding method include injection molding, compression molding, calendar molding, slush molding, rotational molding, extrusion molding, blow molding, film molding (casting method, tenter method, inflation method, etc.), and any method incorporating means such as single-layer molding, multi-layer molding, or foam molding can be used depending on the purpose.
[0087] The molded article of the present invention has excellent mechanical properties and an excellent appearance, and also has good paintability and printability, and a molded article can be obtained by painting and / or printing the molded article. Methods for painting the molded article include, but are not limited to, air spray painting, airless spray painting, electrostatic spray painting, dip coating, roller coating, and brush coating. As the paint, paints generally used for painting plastics can be used, and specific examples thereof include polyester melamine resin paint, epoxy melamine resin paint, acrylic melamine resin paint, and acrylic urethane resin paint. The coating film thickness (dry film thickness) can be appropriately selected depending on the purpose, and is, for example, 10 to 50 μm.
[0088] As a method for printing on a molded article or a painted surface of a molded article, any printing method generally used for printing on plastics can be used, including gravure printing, flexographic printing, screen printing, pad printing, dry offset printing, and offset printing. As the printing ink, any known ink used in printing on plastics can be used, such as gravure ink, flexographic ink, screen ink, pad ink, dry offset ink, and offset ink.
[0089] The polyacetal resin compatibilizer (X) has excellent compatibility, and therefore provides molded products of the resin composition with excellent mechanical strength and excellent appearance. Therefore, it is suitable as a material for housing products (for home appliances, OA equipment, game equipment, office equipment, etc.) molded by various molding methods [injection molding, compression molding, calendar molding, slush molding, rotational molding, extrusion molding, blow molding, foam molding, and film molding (cast method, tenter method, and inflation method), etc.], plastic container materials [trays (IC trays, etc.) and other containers used in clean rooms, etc.], various cushioning materials, covering materials (packaging films and protective films, etc.), flooring sheets, artificial turf, mats, tape base materials (for semiconductor manufacturing processes, etc.), and various molded products (automobile parts, etc.). EXAMPLES
[0090] Examples of the present invention will be described below, but the present invention is not limited to these. In the following, parts are parts by weight. In the following, Examples 23, 24, and 25 are Reference Examples 1, 2, and 3, respectively.
[0091] <Production Example 1> [Production of polyolefin (a2-1-1α) having carboxyl groups at both ends] Into a stainless steel pressure-resistant reactor equipped with a stirrer, a thermometer, a heating / cooling device, a nitrogen inlet tube, and a pressure reducing device, 90 parts of low molecular weight polypropylene obtained by thermal degradation [obtained by thermally degrading polypropylene (MFR: 10g / 10min) at 410±0.1°C for 16 minutes under nitrogen aeration (80mL / min), Mn: 3,400, number of double bonds per 1,000 carbon atoms: 7.0, average number of double bonds per molecule: 1.8, content of polyolefins that can be modified at both ends: 90% by weight], 10 parts of maleic anhydride, and 30 parts of xylene were added, mixed uniformly, replaced with nitrogen, and heated to 200°C while stirring under a sealed condition to melt, and reacted at the same temperature for 10 hours. Next, excess maleic anhydride and xylene were distilled off under reduced pressure (0.013 MPa or less) at 200°C for 3 hours to obtain 95 parts of polyolefin (a2-1-1α) having carboxyl groups at both ends of the polymer. (a2-1-1α) had an acid value of 27.5 and Mn of 3,600.
[0092] <Production Example 2> [Production of polyolefin (a2-1-2) obtained by secondary modification of (a2-1-1α)] In a pressure-resistant reactor similar to that of Production Example 1, 88 parts of (a2-1-1α) and 12 parts of 12-aminododecanoic acid were added and mixed uniformly, and then the mixture was heated to 200°C under stirring in a nitrogen gas atmosphere, and reacted at the same temperature under reduced pressure (0.013 MPa or less) for 3 hours to obtain 96 parts of polyolefin (a2-1-2) obtained by secondary modification of (a2-1-1α). The acid value of (a2-1-2) was 24.8, and Mn was 4,000.
[0093] <Production Example 3> [Production of polyether ester (b2α)] Into a reaction vessel equipped with a stirrer, a thermometer, and a heating / cooling device, 79 parts of polyether diol [PEG (Mn: 600)], 21 parts of dodecanedioic acid, and 0.1 parts of zirconyl acetate were added, and the mixture was heated to 240°C with stirring. Polymerization was carried out at the same temperature for 6 hours under reduced pressure (0.13 kPa or less) to obtain a viscous polyether ester (b2α) (hydroxyl value: 36.2, acid value: 0.4).
[0094] <Example 1> Into a reaction vessel equipped with a stirrer, a thermometer, and a heating / cooling device, 67.1 parts of (a2-1-1α), 32.9 parts of polyetherdiamine (b1-2) [α,ω-diamino PEG (Mn: 2,000)], 0.3 parts of antioxidant "Irganox 1010", and 0.5 parts of zirconyl acetate were added, and the mixture was heated to 220°C with stirring, and polymerized at the same temperature for 6 hours under reduced pressure (0.013 MPa or less), to obtain a polyacetal resin compatibilizer (X-1) containing a block polymer (A2-1). The Mn of (A2-1) was 50,000.
[0095] <Example 2> A compatibilizer (X-2) containing a block polymer (A2-2) was obtained in the same manner as in Example 1, except that 67.1 parts of (a2-1-1α) and 32.9 parts of (b1-2) were replaced with 60.1 parts of (a2-1-2) and 39.9 parts of polyether diol (b1-1α) [PEG (Mn: 3,000)] in Example 1. The Mn of (A2-2) was 30,000.
[0096] <Example 3> In Example 1, 67.1 parts of (a2-1-1α) and 32.9 parts of (b1-2) were changed to 71.5 parts of (a2-1-2) and 28.5 parts of polyether diol (b1-1β) [polytetramethylene glycol (Mn: 1,800)], and the same procedure as in Example 1 was repeated to obtain a compatibilizer (X-3) containing a block polymer (A2-3). The Mn of (A2-3) was 40,000.
[0097] <Example 4> In Example 1, 67.1 parts of (a2-1-1α) and 32.9 parts of (b1-2) were changed to 62.5 parts of (a2-2), 34.5 parts of polyether ester (b2α), and 3 parts of dodecanedioic acid, and the procedure was repeated to obtain a compatibilizer (X-4) containing a block polymer (A2-4). The Mn of (A2-4) was 24,000.
[0098] <Example 5> Into a reaction vessel equipped with a stirrer, a thermometer, and a heating / cooling device, 60.1 parts of (a2-1-1α), 39.8 parts of polyether diol (b1-1α) [PEG (Mn: 3,000)], 0.3 parts of antioxidant "Irganox 1010", and 0.8 parts of zirconyl acetate were added, and the mixture was heated to 220°C with stirring, and polymerized at the same temperature for 10 hours under reduced pressure (0.013 MPa or less) to obtain a compatibilizer (X-5) containing a block polymer (A2-5). The Mn of (A2-5) was 85,000.
[0099] <Comparative Example 1> The polyolefin (a2-1-1α) obtained in Production Example 1 was used as it was as a resin compatibilizer (Comparative X-1) for comparison.
[0100] <Examples 11 to 27, Comparative Example 11> According to the composition (parts by weight) shown in Tables 1 and 2, the ingredients were mixed for 3 minutes in a Henschel mixer, and then melt-kneaded in a vented twin-screw extruder at 100 rpm, a residence time of 5 minutes, and a cylinder temperature of 190°C to obtain each resin composition (Y).
[0101] The symbols in Tables 1 and 2 have the following meanings: (D-1): Propylene-ethylene copolymer ["PM771M", manufactured by SunAllomer Co., Ltd.] (D-2): Polypropylene resin ["PM600A", manufactured by SunAllomer Co., Ltd.] (D-3): Ethylene-α-olefin copolymer ["Tafmer DF640", manufactured by Mitsui Chemicals, Inc.]
[0102] (E-1): Polyacetal resin, [Duracon M90S, manufactured by Polyplastics Co., Ltd.] (E-2): Polyacetal resin, [Delrin 500, manufactured by DuPont] (G3-1): Antioxidants ["Irganox 1010", tetrakis [Methylene-3-(3',5'-di-t-butyl-4'-hydroxyphenyl) propionate]methane, manufactured by BASF]
[0103] The obtained resin composition was used to prepare test pieces using an injection molding machine "PS40E5ASE" (manufactured by Nissei Plastic Industrial Co., Ltd.) at a cylinder temperature of 190° C. and a mold temperature of 80° C., and the test pieces were evaluated by the following performance tests. The results are shown in Tables 1 and 2.
[0104] <Performance test> (1) Number average particle size of the dispersed phase in the resin composition (Y) (unit: μm) Using a scanning electron microscope [model number "S4800", manufactured by Hitachi, Ltd.], a test piece with a platinum-vapor-deposited surface was observed in an area of 25 μm × 35 μm, and the number average particle size (unit: μm) of the dispersed phase was measured to evaluate compatibility. The number average particle size is the number average value in an area of 25 μm × 35 μm. The smaller the number average particle size, the better the compatibility of the resin composition.
[0105] (2) Tensile strength (unit: MPa), tensile elongation (%) Marked lines were placed at 50 mm intervals in the center of the ASTM D638 tensile test piece Type I. This was attached to an autograph and pulled at a rate of 50 mm / min to determine the maximum strength and maximum elongation until the test piece broke.
[0106] (3) Izod impact strength (unit: kJ / m 2 ) Measurement was performed in accordance with ASTM D256 Method A (notched, 3.2 mm thickness).
[0107] (4) Appearance The surface appearance of the test piece (100×100×2 mm) was visually observed and evaluated according to the following criteria. <Evaluation criteria> ◎: Appearance is good with absolutely no abnormalities (color stripes, flow marks, etc.) ○: Almost no abnormality in appearance △: There is a slight abnormality in the appearance. ×: There is something wrong with the appearance
[0108] [Table 1]
[0109] [Table 2]
[0110] From the results in Tables 1 and 2, the compatibilizer (X) for polyacetal resin of the present invention imparts superior mechanical strength to molded articles of resin compositions compared to the comparative ones, and also has excellent compatibility and imparts superior appearance to molded articles. [Industrial Applicability]
[0111] The polyacetal resin compatibilizer (X) of the present invention imparts excellent mechanical strength and excellent appearance to molded articles of the resin composition. Therefore, it is suitable as a material for housing products (for home appliances, OA equipment, game equipment, office equipment, etc.) molded by various molding methods [injection molding, compression molding, calendar molding, slush molding, rotational molding, extrusion molding, blow molding, foam molding, and film molding (cast method, tenter method, and inflation method), etc.], plastic container materials [trays (IC trays, etc.) and other containers used in clean rooms, etc.], various cushioning materials, covering materials (packaging films and protective films, etc.), flooring sheets, artificial turf, mats, tape substrates (for semiconductor manufacturing processes, etc.), and various molded articles (automobile parts, etc.).
Claims
1. The resin composition (Y) comprises a polyacetal resin compatibilizer (X) containing a block polymer (A) whose constituent units are a block of a hydrophobic polymer (a) which is a polyolefin (a2) and a block of a hydrophilic polymer (b) which is a polyether (b1) and / or a polyether-containing hydrophilic polymer (b2), a polyolefin resin (D), and a polyacetal resin (E), wherein the weight ratio of (D) to (E) [(D) / (E)] is 15 / 85 to 50 / 50, and the weight ratio of the total weight of (D) and (E) to (X) {[(D)+(E)] / (X)} is 80 / 20 to 99 / 1.
2. The resin composition (Y) according to claim 1, wherein the block polymer (A) has an [(a)-(b)] n-type (n=2 to 50) structure in which (a) and (b) are alternately bonded.
3. A molded article obtained by molding the resin composition (Y) described in claim 1 or 2.
4. A molded article obtained by painting and / or printing the molded article described in claim 3.
Citation Information
Patent Citations
Polyacetal resin composition
JP1996291247A
Thermoplastic resin composition
JP2000017120A
Block polymer and antistatic agent from the same
JP2001278985A
Polyoxymethylene resin composition and its molded product
JP2007224247A
Antistatic agent and antistatic resin composition
JP2012031395A