Alumina ceramics and method for producing alumina ceramics

By using sodium carbonate and silicon dioxide as sintering aids with controlled Na and Si content, alumina ceramics achieve desired resistivity and density, addressing electrical issues in plasma generation devices without transition metals, ensuring mechanical strength and device performance.

JP7594995B2Active Publication Date: 2024-12-05COORSTEK GK
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
JP2021192366
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2021-11-26
Publication Date
2024-12-05
Estimated Expiration
2041-11-26

AI Technical Summary

Technical Problem

Existing alumina ceramics used in plasma generation devices face issues with electrical charging and conductive phenomena due to high or low resistivity, which can lead to particle adhesion and device malfunction, and adding transition metals like Ti to lower resistivity often inhibits sintering and reduces mechanical strength.

Method used

Alumina ceramics with controlled surface resistivity are produced using sodium carbonate and silicon dioxide as sintering aids, maintaining high purity and density without adding transition metals, with specific Na and Si content ratios within a 500 μm depth from the surface.

Benefits of technology

The solution achieves alumina ceramics with surface resistivity in a desired range, suitable for plasma generation devices, while ensuring high purity and density, thus preventing electrical issues and maintaining mechanical integrity.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007594995000003
    Figure 0007594995000003
  • Figure 0007594995000001
    Figure 0007594995000001
  • Figure 0007594995000002
    Figure 0007594995000002
Patent Text Reader

Abstract

To provide alumina ceramics having surface resistivity in a desired range while satisfying high purity and high densification, and to provide a method for producing the same.SOLUTION: The alumina ceramics of the present invention includes Al2O3 as a main crystal and Na and Si as a sintering assistant, wherein in at least a range from a surface layer to a depth of 500 μm, an Na content is 1,000 ppm or less, an Si content is 10 ppm or more and 2,000 ppm or less, and an Na / Si value is 0.1 or more and 2 or less. Furthermore, the alumina ceramics of the present invention have: a purity of Al2O3 of 99% or more; and a surface resistivity of 5×1012 Ω / sq. or more and 5×1014 Ω / sq. or less.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to an alumina ceramic having a surface resistivity in a desired range and a method for producing the same. [Background technology]

[0002] For example, if the resistivity of alumina ceramics used in plasma generating devices is high, they may be easily charged and attract reaction products. This may lead to particles adhering to the surface. On the other hand, if the resistivity of alumina ceramics is low, they may be prone to weak conductive phenomena, which may adversely affect the control of the entire device. Therefore, alumina ceramics with a resistivity that can suppress charging and conductive phenomena are required for plasma generating devices.

[0003] Furthermore, alumina ceramics is the most well-known ceramic material, and has excellent properties such as high hardness, high wear resistance, corrosion resistance, and chemical resistance. It is also highly versatile and is used in a variety of fields.

[0004] For example, Non-Patent Document 1 describes that alumina ceramics are suitable as a material for use in electrostatic chucking devices. Specifically, the volume resistivity of high-purity alumina ceramics is approximately 10 14 The resistivity of the material is about Ωcm, and the Coulomb force generated by this resistivity is used in electrostatic adsorption devices. The volume resistivity suitable for generating electrostatic adsorption force according to the Johnsen-Rahbek method is 10 9 ~10 12 The volume resistivity is Ωcm. Therefore, additives (such as titanium oxide) are used to reduce the volume resistivity. Specifically, the additives are mixed with the raw material alumina powder at a rate of several percent and sintered to adjust the volume resistivity to the required level. In this way, Non-Patent Document 1 describes how the volume resistivity of alumina ceramics is adjusted to the desired volume resistivity.

[0005] Patent Document 1 also describes the use of Ti and Ti oxides to reduce the resistance of alumina ceramics. The alumina ceramics described in this document are mainly composed of alumina with Ti and other elements dispersed therein, and the surface resistance is 10 4 ~10 11 In addition, Non-Patent Document 2 discloses that the measured surface resistivity of alumina ceramic samples manufactured by each company is 10 15 ~10 18 It has been disclosed that the distribution is between Ω / □. [Prior art documents] [Patent documents]

[0006] [Patent Document 1] JP 2004-352572 A [Non-patent literature]

[0007] [Non-Patent Document 1] Tadashi Iguchi, Toshihiro Tachikawa, Takashi Kayamoto, "Materials and Methods of Electrostatic Adsorption Devices", Vacuum Society of Japan, Vol. 45, No. 8, 2002, pp. 633-636 [Non-Patent Document 2] Y.Yamamoto, S.Michizono, “CERAMIC STUDY ON RF WINDOWS FOR POWER COUPLER, WAVEGUIDE, AND KLYSTRON IN PARTICLE ACCELERATOR” Retrieved September 27, 2021, Internet,<https: / / accelconf.web.cern.ch / srf2019 / papers / mop077.pdf> Summary of the Invention [Problem to be solved by the invention]

[0008] As disclosed in the above-mentioned prior art documents, the electrical resistance can be reduced by adding a conductive material such as a transition metal element, typically Ti, to alumina ceramics. However, adding a conductive material to alumina ceramics tends to hinder sintering, leading to problems such as a deterioration in thermal conductivity and a decrease in mechanical strength due to the generation of pores. For example, when alumina ceramics to which Ti has been added for the purpose of reducing electrical resistance is used in a plasma generating device, there may be cases where the denseness is not satisfied.

[0009] One way to avoid these problems would be to produce high-purity alumina ceramics with a surface resistivity in the desired range without adding transition metal elements such as Ti, but little progress has been made in improving the alumina ceramics themselves.

[0010] The present invention has been made to solve the above problems, and an object of the present invention is to provide an alumina ceramic having a surface resistivity within a desired range while satisfying high purity and high density, and a method for producing the same. [Means for solving the problem]

[0011] The alumina ceramic according to the present invention has Al2O3 as the main crystal, and uses Na and Si as sintering aids. At least in the range from the surface to a depth of 500 μm, the Na content is 1000 ppm or less, the Si content is 10 ppm or more and 2000 ppm or less, and Na / Si value is 0.1 or more and 0.23 or less Furthermore, the purity of Al2O3 is 99% or more and the Ti content is 0.3 ppm or more and 28 ppm or less and the surface resistivity is 3.2×10 13 Ω / □ or more 6.5×10 13 Ω / □ or less The present invention is characterized in that:

[0012] According to the present invention, it is possible to provide an alumina ceramic having a surface resistivity within a desired range while satisfying the requirements of high purity and high density.

[0013] The alumina ceramics according to the present invention can be used in plasma generating devices including CVD devices, ion plating devices, etching devices, and electrostatic chucks. Either It is advisable to use it in such a case.

[0014] The method for producing alumina ceramics according to the present invention further comprises the steps of: As described above, A method for producing an alumina ceramic having Al2O3 as the main crystal, the method comprising the steps of: (a) producing an alumina ceramic having a main crystal structure of Al2O3, the method comprising the steps of: (a) producing an alumina ceramic having a main crystal structure of Al2O3; Between 0.1 and 0.23. The content of Ti contained as an impurity is 0.3 ppm or more and 28 ppm or less The method includes the steps of: adding Na and Si to the alumina powder to prepare a raw material powder; adding a binder to the raw material powder to prepare a granulated powder; preparing a molded body from the granulated powder; and sintering the molded body to obtain an alumina sintered body.

[0015] In addition, in the method for producing alumina ceramics according to the present invention, the purity of Al2O3 in the alumina powder is set to 99% or more. Toga desirable.

[0016] In addition, in the method for producing alumina ceramics according to the present invention, sodium carbonate and silicon dioxide are added to the alumina powder to set the Na content to 1000 ppm or less and the Si content to 400 ppm or more and 2000 ppm or less, and the Na / Si value is 0.1 or more and 0.23 or less Let us assume that. Effect of the Invention

[0017] According to the present invention, it is possible to provide an alumina ceramic having a surface resistivity within a desired range while satisfying high purity and high density, and a method for producing the same. [Brief description of the drawings]

[0018] [Figure 1]FIG. 1 is a flow chart showing an example of a method for producing alumina ceramics according to the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0019] Hereinafter, an embodiment of the alumina ceramic and its manufacturing method according to the present invention will be described in detail, however, the present invention is not limited to the embodiment.

[0020] The alumina ceramic of this embodiment has a high purity of 99% or more for the Al2O3, which is the main crystal. In addition, the alumina ceramic of this embodiment has the above-mentioned high purity and does not contain any transition metal element such as Ti. 3.2×10 13 Ω / □ or more 6.5×10 13 Ω / □ or less This surface resistivity is measured, for example, in accordance with JIS C2141 (Testing methods for ceramic materials for electrical insulation) and JIS C2139 (Dielectric and resistive properties of solid electrical insulating materials).

[0021] In order to control the surface resistivity of the alumina ceramics without adding a transition metal element such as Ti, the alumina ceramics of this embodiment uses sodium carbonate (Na2CO3) as a first sintering aid and silicon dioxide (SiO2) as a second sintering aid. Here, the Na content in the alumina ceramics is preferably 1000 ppm or less, and the Si content is preferably 10 ppm or more and 2000 ppm or less. If either Na or Si is extremely high, the surface resistivity of the alumina ceramics cannot be controlled, so the ratio of Na to Si contained in the alumina ceramics (the Na / Si value when each metal content is expressed in ppm) is set to 0.1 or more. 0.23 It is preferable that:

[0022] The above Na and Si contents must be satisfied at least in the range of 500 μm deep from the surface layer of the alumina ceramic to be manufactured. This is because this range affects the surface resistivity. Also, if the Na content exceeds 1000 ppm, alumina crystals containing sodium, called β-alumina, are likely to be formed in the alumina ceramic, and when a β-alumina structure is formed, the surface resistance is significantly reduced even in the above Si range due to the ionic conductivity of Na, which is not preferable. Also, if the Si content is less than 10 ppm, it is not preferable because it may deteriorate the sinterability of the alumina ceramic and leave pores. On the other hand, if the Si content exceeds 2000 ppm, an amorphous structure is likely to be formed at the grain boundary, and it is difficult to change the amorphous structure to a crystalline structure even if the above Na is used, so it is not preferable.

[0023] In addition, the above Na / Si value (0.1 or more 0.23 The above-mentioned condition (below) must be satisfied within a range of 500 μm deep from the surface layer of the alumina ceramics, as described above. This is because this range affects the surface resistivity. The above Na / Si value can be obtained, for example, by determining the content of each element by ICP emission analysis. The Na / Si value outside the range of 500 μm deep must be 0.1 or more. 0.23 It is desirable that the following:

[0024] For example, when the Na / Si value is less than 0.1, the effect of Si is large, and amorphous material is easily formed, making it difficult to control the surface resistance, which is not preferable.On the other hand, when the Na / Si value exceeds 2, the effect of Na is large, and β-alumina is formed, which significantly reduces the surface resistance due to the ionic conductivity of Na, which is also not preferable.

[0025] In this manner, in this embodiment, by appropriately mixing Na and Si, the surface resistivity is controlled without including a transition metal such as Ti.

[0026] In addition, the alumina ceramic of this embodiment is intended to be used in plasma generating devices including, for example, CVD devices, ion plating devices, etching devices, and electrostatic chucks, and therefore its surface characteristics are important. For example, the surface resistivity of alumina ceramics is affected by the particles, grain boundaries (boundaries of crystal grains), and impurities that make up the alumina ceramics. Specifically, the surface resistivity of alumina ceramics is related to the amorphous portion, and is greatly affected by the texture and impurities (Na, Si, etc.) in the range from the surface to a depth of 500 μm. In some cases, it may be dominated by the texture and impurities in the range from the surface to a depth of 200 μm.

[0027] In particular, impurities that exist at grain boundaries and triple junctions (points where three grain boundaries meet) that occur at the contact points between particles are more mobile than impurities that are dissolved in the particles.In addition, impurities tend to segregate non-stoichiometrically at grain boundaries and triple junctions, and amorphous material tends to form, especially when the material contains 10 ppm or more of Si, which tends to form glass, which has the effect of lowering the electrical resistance of alumina ceramics.

[0028] On the other hand, alkali metals, especially Na, are elements that easily change amorphous material to crystalline material, and in alumina ceramics, Na, like Si, tends to segregate at grain boundaries and triple junctions. Therefore, whether or not an amorphous material forms is determined by the ratio of Na to Si (Na / Si value).

[0029] As described above, the Na and Si contents specified in the alumina ceramic of this embodiment may be those that are filled within a range of 500 μm deep from the surface, but are not limited to this. For example, they may be filled both within a range of 500 μm deep from the surface and inside outside that range.

[0030] In addition, the alumina ceramic of this embodiment has a Ti content of 100 ppm or less as an impurity. Note that this Ti is contained as an impurity and is not actively used to reduce the resistivity of the alumina ceramic.

[0031] In this way, the alumina ceramic of this embodiment has Al2O3 as the main crystal, and Na and Si are used as sintering aids. At least in the range from the surface to a depth of 500 μm, the Na content is 1000 ppm or less, the Si content is 10 ppm or more and 2000 ppm or less, and the Na / Si value is 0.1 or more. 0.23 Furthermore, the alumina ceramic of this embodiment has an Al2O3 purity of 99% or more and a surface resistivity of 3.2×10 13 Ω / □ or more 6.5×10 13 Ω / □ or less That is, according to this embodiment, it is possible to obtain an alumina ceramic having a surface resistivity in a desired range while satisfying high purity and high density. As a result, the alumina ceramic of this embodiment can be suitably used in plasma generating devices including CVD devices, ion plating devices, etching devices, electrostatic chucks, etc.

[0032] Next, a method for producing the alumina ceramic according to the present embodiment will be described with reference to the drawings. Fig. 1 is a flow chart showing an example of the method for producing the alumina ceramic.

[0033] First, an alumina powder having an Al2O3 purity of 99% or more and an average particle size of 1 to 2 μm is prepared as a raw material (step S1). This alumina powder is preferably of high purity, but may contain 100 ppm or less of Ti as an impurity. Note that in this embodiment, the content of Ti as an impurity is specified, but Ti is not actively added to the alumina powder. This is to avoid an increase in pore size due to the active addition of Ti.

[0034] Next, the prepared alumina powder was subjected to a test in which the Na content was 1000 ppm or less, the Si content was 10 ppm or more and 2000 ppm or less, and the Na / Si value was 0.1 or more in a range of 500 μm from the surface layer (the surface layer of the alumina sintered body described later). 0.23Sodium carbonate (Na2CO3) and silicon dioxide (SiO2) are added as follows to prepare raw material powder (step S2). Polyvinyl alcohol is added as a binder to the raw material powder to prepare granulated powder (step S3).

[0035] Next, the granulated powder is filled into a mold and a molded body is produced by cold isostatic pressing (CIP) at a pressure in the range of 80 to 200 MPa (step S4). The molded body is then fired in an air atmosphere or a reducing atmosphere at a maximum temperature of, for example, 1600°C to obtain an alumina sintered body (step S5).

[0036] Then, the alumina sintered body is ground and polished to a desired shape to obtain a final surface condition (step S6). After the CIP molding in step S4, a degreasing process may be performed, and in step S5, the body may be fired in a hydrogen atmosphere at, for example, 1800°C.

[0037] As described above, in this embodiment, when producing an alumina ceramic having Al2O3 as a main crystal, at least in the range of 500 μm deep from the surface layer of the alumina sintered body, the Na content is 1000 ppm or less, the Si content is 10 ppm or more and 2000 ppm or less, and the Na / Si value is 0.1 or more. 0.23 As shown below, raw material powder is prepared by adding Na and Si to alumina powder. After that, a binder is added to the raw material powder to prepare granulated powder, a compact is made from the granulated powder, and the compact is fired to prepare an alumina sintered body (alumina ceramics). This allows the alumina to be sintered without the need to actively add transition metal elements such as Ti in order to reduce the surface resistivity. 3.2×10 13 Ω / □ or more 6.5×10 13 Ω / □ or less It is possible to obtain an alumina ceramic having a surface resistivity of 0.1 to 1.0 μm. EXAMPLES

[0038] The alumina ceramics and the manufacturing method thereof according to the present invention will be further described with reference to examples.

[0039] [Experimental Method] In this experiment, alumina ceramics were produced using Na and Si as sintering aids, and the preferred ranges of the Na and Si contents and ratios were verified.

[0040] Example 1 In Example 1, an alumina powder with a purity of 99% or more and an average particle size of 1 to 2 μm was used as a raw material. Sodium carbonate (Na2CO3) was added to this alumina powder in a range of 500 μm deep from the surface layer (the surface layer of the alumina sintered body) so that the Na content was 90 ppm, and silicon dioxide (SiO2) was added so that the Si content was 900 ppm. At this time, the Na / Si value was 0.1. The Ti content in the raw material powder was 28 ppm.

[0041] In addition, polyvinyl alcohol was added as a binder to the raw material powder containing the above additives to produce granulated powder.

[0042] Next, the granulated powder was filled into a mold and molded at a pressure of 80 to 200 MPa by cold isostatic pressing (CIP). This molded body was then sintered in air at a maximum temperature of 1600°C to obtain an alumina sintered body (alumina ceramics).

[0043] The purity of the obtained sintered body was determined by ICP emission analysis, and the contents of Na, Si, and Ti are shown in Table 1. Furthermore, after processing into a sample shape, the surface resistivity was measured according to JIS C2141 (Testing methods for ceramic materials for electrical insulation) and JIS C2139 (Dielectric and resistive properties of solid electrical insulating materials), and the measurement results are shown in Table 2.

[0044] Example 2 In Example 2, sodium carbonate (Na2CO3) was added to the alumina powder so that the Na content was 360 ppm in the range of 500 μm deep from the surface layer, and silicon dioxide (SiO2) was added so that the Si content was 1600 ppm. At this time, the Na / Si value was 0.23. The Ti content in the raw material powder was 26 ppm. The other implementation conditions were the same as in Example 1.

[0045] Example 3 In Example 3, sodium carbonate (Na2CO3) was added to the alumina powder so that the Na content was 75 ppm in the range of 500 μm deep from the surface layer, and silicon dioxide (SiO2) was added so that the Si content was 450 ppm. At this time, the Na / Si value was 0.17. The Ti content in the raw material powder was 5 ppm. The other implementation conditions were the same as in Example 1.

[0046] ( Reference example 1 ) Reference example 1 In this example, sodium carbonate (Na2CO3) was added to the alumina powder so that the Na content was 490 ppm in the range of 500 μm deep from the surface layer, and silicon dioxide (SiO2) was added so that the Si content was 300 ppm. At this time, the Na / Si value was 1.6. The Ti content in the raw material powder was 73 ppm. The other implementation conditions were the same as in Example 1.

[0047] ( Reference example 2 ) Reference example 2 In this example, sodium carbonate (Na2CO3) was added to the alumina powder so that the Na content was 820 ppm in the range of 500 μm deep from the surface layer, and silicon dioxide (SiO2) was added so that the Si content was 500 ppm. At this time, the Na / Si value was 1.6. The Ti content in the raw material powder was 34 ppm. The other implementation conditions were the same as in Example 1.

[0048] ( Example 4 ) Example 4 In this study, sodium carbonate (Na2CO3) was added to the alumina powder so that the Na content was 3 ppm in the range of 500 μm deep from the surface layer, and silicon dioxide (SiO2) was added so that the Si content was 15 ppm. At this time, the Na / Si value was 0.2. The Ti content in the raw material powder was 0.3 ppm.

[0049] The granulated powder was filled into a mold, and a molded body was produced by cold isostatic pressing (CIP) at a pressure in the range of 80 to 200 MPa, after which a degreasing treatment was carried out and the body was fired at 1800°C in a hydrogen atmosphere to obtain an alumina sintered body (alumina ceramics). The other implementation conditions were the same as those in Example 1.

[0050] ( Example 5 ) Example 5 In this experiment, sodium carbonate (Na2CO3) was added to the alumina powder so that the Na content was 20 ppm in the range of 500 μm deep from the surface layer, and silicon dioxide (SiO2) was added so that the Si content was 150 ppm. At this time, the Na / Si value was 0.13. The Ti content in the raw material powder was 13 ppm. Other experimental conditions were Example 4 It was deemed to be the same as above.

[0051] Comparative Example 1 In Comparative Example 1, sodium carbonate (Na2CO3) was added to the alumina powder so that the Na content was 250 ppm in the range of 500 μm deep from the surface layer, and silicon dioxide (SiO2) was added so that the Si content was 2100 ppm. At this time, the Na / Si value was 0.12. The Ti content in the raw material powder was 55 ppm. The other implementation conditions were the same as in Example 1.

[0052] Comparative Example 2 In Comparative Example 2, sodium carbonate (Na2CO3) was added to the alumina powder so that the Na content was 30 ppm in the range of 500 μm deep from the surface layer, and silicon dioxide (SiO2) was added so that the Si content was 1800 ppm. At this time, the Na / Si value was 0.02. The Ti content in the raw material powder was 88 ppm. Other implementation conditions were Example 4 It was deemed to be the same as above.

[0053] Comparative Example 3 In Comparative Example 3, sodium carbonate (Na2CO3) was added to the alumina powder so that the Na content was 5 ppm in the range of 500 μm deep from the surface layer, and silicon dioxide (SiO2) was added so that the Si content was 66 ppm. At this time, the Na / Si value was 0.08. The Ti content in the raw material powder was 8 ppm. Other implementation conditions were Example 4 It was deemed to be the same as above.

[0054] (evaluation) Example 1 ~4, Reference examples 1 and 2 The conditions for Comparative Examples 1 to 3 are shown in Table 1, and the surface resistivities obtained as evaluation results are shown in Table 2.

[0055] [Table 1]

[0056] [Table 2]

[0057] As a result of the experiment, when the above-mentioned manufacturing method is performed within the specified range (preferable range of Na and Si contents and ratios), the surface resistivity can be reduced without actively adding a transition metal element such as Ti. 3.2×10 13 Ω / □ or more 6.5×10 13 Ω / □ or lessIt was confirmed that an alumina ceramic having a surface resistivity of 100% or more could be obtained. On the other hand, when the alumina ceramic was produced under conditions outside the above-mentioned range, it was not possible to obtain an alumina ceramic having a desired surface resistivity.

Claims

1. A 2 O 3 is used as the main crystal, and Na and Si are used as sintering aids. The Na content is 1000 ppm or less in at least the range of 500 μm deep from the surface layer, The Si content is 10 ppm or more and 2000 ppm or less, and the Na / Si value is 0.1 or more and 0.23 or less, Furthermore, Al 2 O 3 1. An alumina ceramic having a purity of 99% or more, a Ti content of 0.3 ppm or more and 28 ppm or less, and a surface resistivity of 3.2×10 13 Ω / □ or more and 6.5×10 13 Ω / □ or less.

2. For use in any of CVD apparatus, ion plating apparatus, etching apparatus, and plasma generating apparatus including electrostatic chucks; 2. The alumina ceramic according to claim 1 .

3. The Al according to claim 1. 2 O 3 A method for producing an alumina ceramic having a main crystal structure comprising the steps of: preparing a raw material powder by adding Na and Si to an alumina powder having a Ti content of 0.3 ppm or more and 28 ppm or less, so that the Na content is 1000 ppm or less, the Si content is 10 ppm or more and 2000 ppm or less, and the Na / Si value is 0.1 or more and 0.23 or less, at least in a range of 500 μm deep from the surface layer; Adding a binder to the raw material powder to prepare a granulated powder; Producing a compact from the granulated powder; sintering the compact to obtain an alumina sintered body; A method for producing alumina ceramics, comprising:

4. The alumina powder is Al 2 O 3 The purity of is 99% or more. The method for producing alumina ceramics according to claim 3 .

5. By adding sodium carbonate and silicon dioxide to the alumina powder, the Na content is set to 1000 ppm or less, the Si content is set to 400 ppm or more and 2000 ppm or less, and the Na / Si value is set to 0.1 or more and 0.23 or less. The method for producing alumina ceramics according to claim 3 or 4.

Citation Information

Patent Citations

  • Electrostatic chuck

    JP1999312729A

  • Alumina sintered compact and its production

    JP2000044330A

  • Alumina sintered compact, and production method therefor

    JP2003112963A

  • Alumina ceramics and method for producing the same

    JP2004352572A

  • Alumina ceramics

    JP2012046365A