Resin composition and film

A resin composition of polyimide and ester resin with a bis(trimellitic anhydride) ester component addresses the challenge of achieving low birefringence and high mechanical strength in transparent films, resulting in films with improved transparency and strength for display applications.

JP7595032B2Active Publication Date: 2024-12-05KANEKA CORP
View PDF 10 Cites 0 Cited by

Patent Information

Application Number
JP2021567500
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2020-01-30
Filing Date
2020-12-22
Publication Date
2024-12-05
Estimated Expiration
2040-12-22

AI Technical Summary

Technical Problem

Conventional transparent polyimide resins face challenges in achieving both low birefringence and high mechanical strength, with rigid structures reducing solubility in organic solvents and transparency.

Method used

A resin composition comprising a specific polyimide resin and an ester resin, such as polycarbonate or polyarylate, with a compatible chemical structure that maintains transparency and mechanical strength, using a weight ratio of 98:2 to 2:98, and incorporating a bis(trimellitic anhydride) ester as an acid dianhydride component to enhance solubility and compatibility.

Benefits of technology

The composition results in a transparent film with low haze, reduced birefringence, and high tensile modulus, suitable for applications like display cover films, by balancing mechanical strength and optical properties.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007595032000001
    Figure 0007595032000001
  • Figure 0007595032000002
    Figure 0007595032000002
  • Figure 0007595032000003
    Figure 0007595032000003
Patent Text Reader

Abstract

A resin composition according to the present invention contains a polyimide resin and an ester resin. The ester resin is a polycarbonate or a polyarylate. The polyimide contains a structural unit represented by general formula (1). In general formula (1), X represents a divalent organic group shown in group (I); Y represents a divalent group that contains one or more moieties that are selected from the group consisting of a fluorine group, a trifluoromethyl group, a sulfonic group, a fluorene structure and an alicyclic structure; each of R1 and R2 represents a fluorine atom, an alkyl group having from 1 to 20 carbon atoms, or a fluoroalkyl group having from 1 to 20 carbon atoms; m represents an integer from 1 to 4; and n represents an integer from 0 to 4.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a resin composition and a film. [Background technology]

[0002] There is a demand for thinner, lighter, and more flexible electronic devices, such as liquid crystal, organic electroluminescence, and electronic paper displays, as well as solar cells and touch panels. By replacing the glass materials used in these devices with film materials, they can be made more flexible, thinner, and lighter. Transparent polyimide films have been developed as glass replacement materials and are used in display substrates, cover films, and other applications.

[0003] A typical polyimide film is obtained by applying a polyamic acid solution, which is a polyimide precursor, to a support in the form of a film, and subjecting the film to high-temperature treatment to remove the solvent and simultaneously perform thermal imidization. However, the heating temperature for thermal imidization is high (e.g., 300°C or higher), and coloring (increase in yellowness) due to heating is likely to occur, making it difficult to apply the film to applications requiring high transparency, such as display cover films. Patent documents 1 to 3 report polyimide resins that are soluble in organic solvents and do not require high-temperature imidization after film formation.

[0004] A polyimide film can be obtained by dissolving the soluble polyimide described in Patent Documents 1 to 3 in an organic solvent, applying the solution to a support, and then removing the organic solvent. Generally, films produced by solution casting have low birefringence, but polyimide molecules tend to be oriented in-plane due to their molecular structure, and even when a film is produced by solution casting, the birefringence in the thickness direction is large, and rainbow unevenness and color shifts are observed when viewed from an oblique direction.

[0005] Patent Document 4 reports that polyimides made from alicyclic tetracarboxylic dianhydrides can achieve both transparency and low birefringence. However, polyimides made from alicyclic tetracarboxylic dianhydrides have problems such as difficulty in increasing the molecular weight during polymerization and difficulty in producing a film with high mechanical strength. [Prior art documents] [Patent documents]

[0006] [Patent Document 1] JP 2012-144603 A [Patent Document 2] JP 2016-132686 A [Patent Document 3] WO2017 / 175869 International Publication Pamphlet [Patent Document 4] Patent No. 6174580 Summary of the Invention [Problem to be solved by the invention]

[0007] Although the introduction of a rigid structure into polyimide improves its mechanical strength, it also leads to a decrease in solubility in organic solvents and transparency, and to high birefringence, and it is not easy to achieve both low birefringence and high mechanical strength while maintaining transparency with conventional transparent polyimide resins. In view of such problems, the present invention aims to provide a transparent film having low birefringence and sufficient mechanical strength, and a resin composition used for producing the same. [Means for solving the problem]

[0008] The present inventors have discovered that a polyimide having a specific chemical structure and a specific ester-based resin are compatible with each other, and that a highly transparent film can be produced by mixing these in a resin composition, thereby solving the above-mentioned problems.

[0009] One aspect of the present invention relates to a film and a resin composition containing a polyimide resin and an ester resin. The resin composition may contain the polyimide resin and the ester resin in a weight ratio ranging from 98:2 to 2:98.

[0010] Polyimide contains a structural unit represented by the general formula (1).

[0011] [ka]

[0012] The structural unit of general formula (1) can be obtained by reacting an acid dianhydride represented by general formula (3) with a diamine represented by general formula (4).

[0013] [ka]

[0014] [ka]

[0015] In general formula (1) and general formula (3), X is a divalent organic group represented by group (I).

[0016] [ka]

[0017] R 1 and R 2 are each a fluorine atom, an alkyl group having 1 to 20 carbon atoms, or a fluoroalkyl group having 1 to 20 carbon atoms; m is an integer of 1 to 4; and n is an integer of 0 to 4.

[0018] In general formula (1) and general formula (4), Y is a divalent group containing one or more selected from the group consisting of a fluorine group, a trifluoromethyl group, a sulfone group, a fluorene structure, and an alicyclic structure.

[0019] The ratio of the tetracarboxylic acid dianhydride represented by general formula (3) to the total amount of the acid dianhydride components in the polyimide is preferably 30 mol% or more, and may be 40 mol% or more, 45 mol% or more, or 50 mol% or more, or may be 90 mol% or less.

[0020] The acid dianhydride component of the polyimide may contain an acid dianhydride represented by formula (6) as the acid dianhydride represented by general formula (3). The polyimide may contain 30 mol % or more, 40 mol % or more, 45 mol % or more, or 50 mol % or more of the acid dianhydride represented by formula (6) based on the total amount of the acid dianhydride component.

[0021] [ka]

[0022] The polyimide resin is preferably soluble in methylene chloride. The solubility parameter (SP value) of the polyimide is 8.10 to 9.10 (cal / cm 3 ) 1 / 2 The solubility parameter of the polyimide is the sum of the products of the solubility parameters and the molar ratios of the diamine and the acid dianhydride constituting the polyimide.

[0023] The ester resin is a polycarbonate or a polyarylate. The polycarbonate may contain a repeating unit of formula (8), and the polyarylate may contain a repeating unit of formula (10). When the ester resin is polycarbonate, the ratio of the tetracarboxylic dianhydride represented by general formula (3) to the total amount of the acid dianhydride components of the polyimide is preferably 60 mol % or more.When the ester resin is polyarylate, the ratio of the tetracarboxylic dianhydride represented by general formula (3) to the total amount of the acid dianhydride components of the polyimide is preferably 30 mol % or more.

[0024] [ka]

[0025] [ka]

[0026] A film according to one embodiment of the present invention has a thickness of 5 μm or more and 300 μm or less, a haze of 3.5% or less, a YI of 5.0 or less, a thickness retardation Rth of 3000 nm or less, and a tensile modulus of elasticity of 3.0 GPa or more. Effect of the Invention

[0027] Since the polyimide resin and the ester resin contained in the resin composition are compatible with each other, a transparent film with low haze can be obtained. In addition, since the polyimide resin and the ester resin are compatible with each other, birefringence can be reduced without significantly reducing the excellent mechanical strength of polyimide, so that a transparent film suitable for a cover film of a display can be produced. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0028] [Resin composition] One embodiment of the present invention is a compatible resin composition containing a polyimide resin and an ester-based resin. The polyimide contains a structural unit represented by the following general formula (1), and the ester-based polymer contains a structural unit represented by the following general formula (2).

[0029] [ka]

[0030] [ka]

[0031] In the general formula (1), Y is a diamine residue having one or more selected from the group consisting of a fluorine group, a trifluoromethyl group, a sulfone group, a fluorene structure, and an alicyclic structure, and X is a divalent organic group selected from the following group (I):

[0032] [ka]

[0033] R in group (I)1 and R 2 represents a fluorine atom, an alkyl group having 1 to 20 carbon atoms, or a fluoroalkyl group having 1 to 20 carbon atoms; m is an integer of 1 to 4; and n is an integer of 0 to 4.

[0034] In the general formula (2), Z is any divalent organic group, R 3 is a halogen, an alkyl group having 1 to 20 carbon atoms, or a halogenated alkyl group having 1 to 20 carbon atoms, and j is an integer of 0 to 4. Q is a direct bond or a divalent organic group selected from the following group (II):

[0035] [ka]

[0036] When Q is a direct bond, the polymer having the repeating unit of general formula (2) is a polycarbonate. When Q is a divalent organic group selected from group (II), the polymer having the repeating unit of general formula (2) is a polyarylate.

[0037] Polycarbonate is a carbonate ester of bisphenol, and polyarylate is an ester of bisphenol and phthalic acid, and both are common in that they are esters of bisphenol. Hereinafter, polycarbonate and polyarylate will be collectively referred to as "ester-based polymers," and polycarbonate resin and polyarylate resin will be collectively referred to as "ester-based resins."

[0038] <Polyimide resin> The polyimide in this embodiment contains a structural unit represented by the above general formula (1). The polyimide is obtained by dehydrating and cyclizing a polyamic acid obtained by condensing a tetracarboxylic dianhydride (hereinafter, sometimes referred to as an "acid dianhydride") with a diamine. That is, the polyimide has a structure derived from the acid dianhydride (acid dianhydride component) and a structure derived from the diamine (diamine component).

[0039] (acid dianhydride) The polyimide in this embodiment contains, as an acid dianhydride component, a bis(trimellitic anhydride) ester represented by the following general formula (3).

[0040] [ka]

[0041] X in the general formula (3) is the same as X in the general formula (1). That is, X is any one of the following (IA), (IB), (IC), and (ID).

[0042] [ka]

[0043] R in formula (IA) 1 is a fluorine atom, an alkyl group having 1 to 20 carbon atoms, or a fluoroalkyl group having 1 to 20 carbon atoms, and m is an integer from 1 to 4. The group represented by formula (1A) is a group obtained by removing two hydroxyl groups from a hydroquinone derivative having a substituent on the benzene ring. Examples of hydroquinone having a substituent on the benzene ring include tert-butylhydroquinone, 2,5-di-tert-butylhydroquinone, and 2,5-di-tert-amylhydroquinone.

[0044] R in formula (IB) 2 is a fluorine atom, an alkyl group having 1 to 20 carbon atoms, or a fluoroalkyl group having 1 to 20 carbon atoms, and n is an integer from 0 to 4. The group represented by formula (IB) is a group obtained by removing two hydroxyl groups from a biphenol which may have a substituent on the benzene ring. Examples of biphenol derivatives having a substituent on the benzene ring include 2,2'-dimethylbiphenyl-4,4'-diol, 3,3'-dimethylbiphenyl-4,4'-diol, 3,3',5,5'-tetramethylbiphenyl-4,4'-diol, and 2,2',3,3',5,5'-hexamethylbiphenyl-4,4'-diol.

[0045] The group represented by formula (IC) is a group obtained by removing two hydroxyl groups from 4,4'-isopropylidenediphenol (bisphenol A). The group represented by formula (1D) is a group obtained by removing two hydroxyl groups from resorcinol.

[0046] Among the above, from the viewpoint of compatibility with ester resins, X is preferably (IB), (IC) or (ID), and among these, formula (IB) is more preferred, and in particular, it is preferred that n=3 and that the biphenyl has substituents at the 2,2', 3,3', 5,5' positions. If the biphenyl has substituents at these positions, the bonds between the benzene rings of the biphenyl skeleton are twisted due to steric hindrance of the substituents, and the solubility of the polyimide in organic solvents is improved, and the compatibility with ester resins tends to be enhanced.

[0047] A specific example of the divalent organic group represented by formula (IB) and having substituents at the 2,2',3,3',5,5'-positions of biphenyl is 2,2',3,3',5,5'-hexamethylbiphenyl-4,4'-diyl represented by the following formula (5). The acid dianhydride in which X in formula (3) is 2,2',3,3',5,5'-hexamethylbiphenyl-4,4'-diyl is represented by formula (6).

[0048] [ka]

[0049] [ka]

[0050] That is, in one embodiment, the polyimide contains, as an acid dianhydride, a compound represented by formula (6): bis(1,3-dioxo-1,3-dihydroisobenzofuran-5-carboxylic acid)-2,2',3,3',5,5'-hexamethylbiphenyl-4,4'diyl (abbreviation: TAHMBP).

[0051] The amount of the acid dianhydride of general formula (3) relative to the total amount of the acid dianhydride components constituting the polyimide (100 mol%) is preferably 30 mol% or more. The higher the ratio of the acid dianhydride of general formula (3), the more the compatibility between the polyimide and the ester polymer improves, and the film tends to have less haze and more transparency. The amount of the acid dianhydride of general formula (3) relative to the total amount of the acid dianhydride components (100 mol%) is preferably 40 mol% or more, more preferably 45 mol% or more, more preferably 50 mol% or more, and may be 55 mol% or more, 60 mol% or more, 65 mol% or more, or 70 mol% or more.

[0052] From the viewpoint of improving compatibility with ester-based polymers, the amount of the acid dianhydride of formula (6) relative to the total amount of the acid dianhydride components constituting the polyimide (100 mol%) is preferably 30 mol% or more. The amount of the acid dianhydride of formula (6) relative to the total amount of the acid dianhydride components (100 mol%) is preferably 40 mol% or more, more preferably 45 mol% or more, more preferably 50 mol% or more, and may be 55 mol% or more, 60 mol% or more, 65 mol% or more, or 70 mol% or more. The polyimide may contain, in addition to TAHMBP, an acid dianhydride represented by general formula (3) other than TAHMBP as an acid dianhydride component.

[0053] If the ratio of the acid dianhydride of general formula (3) is too high, the birefringence of the film may become large. The amount of the acid dianhydride of general formula (3) relative to the total amount of the acid dianhydride components (100 mol%) is preferably 90 mol% or less, and may be 85 mol% or less, 80 mol% or less, or 75 mol% or less.

[0054] As described above, among the acid dianhydride components of the polyimide, the amount of the acid dianhydride of general formula (3) is preferably 90 mol % or less, and it is preferable that 10 mol % or more of the acid dianhydride components are acid dianhydrides other than those of general formula (3).

[0055] Examples of acid dianhydrides other than those of general formula (3) include ethylene tetracarboxylic dianhydride, butane tetracarboxylic dianhydride, 1,2,3,4-cyclobutane tetracarboxylic dianhydride, 1,2,3,4-cyclopentane tetracarboxylic dianhydride, 1,2,4,5-cyclohexane tetracarboxylic dianhydride, 1,1'-bicyclohexane 53,3',4,4' tetracarboxylic acid-3,4,3',4'-dianhydride, 3,3',4,4'-benzophenone tetracarboxylic dianhydride, 2,2',3,3'-benzophenone tetracarboxylic dianhydride, 2,2', 3,3'-Biphenyltetracarboxylic dianhydride, pyromellitic dianhydride, 3,3',4,4'-biphenyltetracarboxylic dianhydride, 2,2-bis(3,4-dicarboxyphenyl)propane dianhydride, 2,2-bis(2,3-dicarboxyphenyl)propane dianhydride, bis(3,4-dicarboxyphenyl)ether dianhydride, bis(3,4-dicarboxyphenyl)sulfone dianhydride, 1,1-bis(2,3-dicarboxyphenyl)ethane dianhydride, bis(2,3-dicarboxyphenyl)methane dianhydride, bis(3,4-dicarboxyphenyl) 2,2-bis(3,4-dicarboxyphenyl)-1,1,1,3,3,3-hexafluoropropane dianhydride, 2,2-bis(2,3-dicarboxyphenyl)-1,1,1,3,3,3-hexafluoropropane dianhydride, 2,2-bis{4-[4-(1,2-dicarboxy)phenoxy]phenyl}-1,1,1,3,3,3-hexafluoropropane dianhydride, 1,3-bis[(3,4-dicarboxy)benzoyl]benzene dianhydride, 1,4-bis[(3,4-dicarboxy)benzoyl]benzene dianhydride, 2,2 -Bis{4-[4-(1,2-dicarboxy)phenoxy]phenyl}propane dianhydride, 2,2-bis{4-[3-(1,2-dicarboxy)phenoxy]phenyl}propane dianhydride, bis{4-[4-(1,2-dicarboxy)phenoxy]phenyl}ketone dianhydride, bis{4-[3-(1,2-dicarboxy)phenoxy]phenyl}ketone dianhydride, 4,4'-bis[4-(1,2-dicarboxy)phenoxy]biphenyl dianhydride, 4,4'-bis[3-(1,2-dicarboxy)phenoxy]biphenyl dianhydride, bis{4-[4-(1,2-dicarboxy)phenoxy]phenyl}ketone dianhydride, bis{4-[3-(1,2-dicarboxy)phenoxy]phenyl}ketone dianhydride, bis{4-[4-(1,2-dicarboxy)phenoxy]phenyl}sulfone dianhydride, bis{4-[3-(1,2-dicarboxy)phenoxy]phenyl}sulfone dianhydride, bis{4-[4-(1,2-dicarboxy)phenoxy]phenyl}sulfide dianhydride, bis{4-[3-(1,2-dicarboxy)phenoxy]phenyl}sulfide dianhydride, 2,2-bis{4-[4-(1,2-dicarboxy)phenoxy]phenyl}-1,1,1,3,3,3-hexafluoropropane dianhydride, 2,2- Examples of the dianhydride include bis{4-[3-(1,2-dicarboxy)phenoxy]phenyl}-1,1,1,3,3,3-propane dianhydride, 2,3,6,7-naphthalene tetracarboxylic dianhydride, 1,4,5,8-naphthalene tetracarboxylic dianhydride, 1,2,5,6-naphthalene tetracarboxylic dianhydride, 1,2,3,4-benzene tetracarboxylic dianhydride, 3,4,9,10-perylene tetracarboxylic dianhydride, 2,3,6,7-anthracene tetracarboxylic dianhydride, 1,2,7,8-phenanthrene tetracarboxylic dianhydride, and bis(1,3-dihydro-1,3-dioxo-5-isobenzofuran carboxylic acid)-1,4-phenylene ester.

[0056] Among the above, from the viewpoints of improving the transparency and solubility in organic solvents of the polyimide and reducing birefringence, it is preferable to contain an acid dianhydride represented by X-1, X-2, or X-3 below, or an acid dianhydride having an alicyclic structure, where M in X-3 is O, S, or SO2.

[0057] [ka]

[0058] Specific examples of the alicyclic acid dianhydride include the acid dianhydrides of group (III) below.

[0059] [ka]

[0060] The polyimide preferably contains the above-mentioned X-1, X-2, X-3 and group (III) acid dianhydrides in a total amount of 10 mol % or more as the acid dianhydride component, and may contain a total amount of 15 mol % or more, 20 mol % or more, or 25 mol % or more.

[0061] (Diamine) The polyimide in this embodiment contains, as a diamine component, a diamine represented by the following general formula (4).

[0062] [ka]

[0063] Y in general formula (4) is the same as Y in general formula (1). That is, Y is a diamine residue having one or more selected from the group consisting of a fluorine group, a trifluoromethyl group, a sulfone group, a fluorene structure, and an alicyclic structure. By including a diamine component having these functional groups, the polyimide exhibits transparency and excellent solubility in organic solvents.

[0064] Examples of the diamine represented by the general formula (4), that is, the diamine having one or more selected from the group consisting of a fluorine group, a trifluoromethyl group, a sulfone group, a fluorene structure, and an alicyclic structure, include 3,3'-diaminodiphenyl sulfone, 3,4'-diaminodiphenyl sulfone, 4,4'-diaminodiphenyl sulfone, bis[4-(3-aminophenoxy)phenyl]sulfone, bis[4-(4-aminophenoxy)phenyl]sulfone, 4,4'-bis[4-(4-amino-α,α-dimethylbenzyl)phenoxy]diphenyl sulfone, 4, 4'-Bis[4-(4-aminophenoxy)phenoxy]diphenyl sulfone 1,4-diamino-2-fluorobenzene, 1,4-diamino-2,3-difluorobenzene, 1,4-diamino-2,5-difluorobenzene, 1,4-diamino-2,6-difluorobenzene, 1,4-diamino-2,3,5-trifluorobenzene, 1,4-diamino-2,3,5,6-tetrafluorobenzene, 1,4-diamino-2-(trifluoromethyl)benzene, 1,4-diamino-2,3-bis(trifluoromethyl)benzene, 1,4-diamino-2 ,5-Bis(trifluoromethyl)benzene, 1,4-diamino-2,6-bis(trifluoromethyl)benzene, 1,4-diamino-2,3,5-tris(trifluoromethyl)benzene, 1,4-diamino-2,3,5,6-tetrakis(trifluoromethyl)benzene, 2-fluorobenzidine, 3-fluorobenzidine, 2,3-difluorobenzidine, 2,5-difluorobenzidine, 2,6-difluorobenzidine, 2,3,5-trifluorobenzidine, 2,3,6-trifluorobenzidine, 2,3,5,6-tetrafluorobenzidine , 2,2'-difluorobenzidine, 3,3'-difluorobenzidine, 2,3'-difluorobenzidine, 2,2',3-trifluorobenzidine, 2,3,3'-trifluorobenzidine, 2,2',5-trifluorobenzidine, 2,2',6-trifluorobenzidine, 2,3',5-trifluorobenzidine, 2,3',6-trifluorobenzidine, 2,2',3,3'-tetrafluorobenzidine, 2,2',5,5'-tetrafluorobenzidine, 2,2',6,6'-tetrafluorobenzidine, 2,2',3,3',6,6'-Hexafluorobenzidine, 2,2',3,3',5,5',6,6'-Octafluorobenzidine, 2-(trifluoromethyl)benzidine, 3-(trifluoromethyl)benzidine, 2,3-Bis(trifluoromethyl)benzidine, 2,5-Bis(trifluoromethyl)benzidine, 2,6-Bis(trifluoromethyl)benzidine, 2,3,5-Tris(trifluoromethyl)benzidine, 2,3,6-Tris(trifluoromethyl)benzidine, 2,3,5,6-Tetrakis(trifluoromethyl)benzidine, 2,2'-Bis(trifluoromethyl)benzidine, trifluoromethyl)benzidine, 3,3'-bis(trifluoromethyl)benzidine, 2,3'-bis(trifluoromethyl)benzidine, 2,2',3-bis(trifluoromethyl)benzidine, 2,3,3'-tris(trifluoromethyl)benzidine, 2,2',5-tris(trifluoromethyl)benzidine, 2,2',6-tris(trifluoromethyl)benzidine, 2,3',5-tris(trifluoromethyl)benzidine, 2,3',6-tris(trifluoromethyl)benzidine, 2,2',3,3'-tetrakis(trifluoromethyl)benzidine 2,2',5,5'-tetrakis(trifluoromethyl)benzidine, 2,2',6,6'-tetrakis(trifluoromethyl)benzidine 2,2-di(3-aminophenyl)-1,1,1,3,3,3-hexafluoropropane, 2,2-di(4-aminophenyl)-1,1,1,3,3,3-hexafluoropropane, 2-(3-aminophenyl)-2-(4-aminophenyl)-1,1,1,3,3,3-hexafluoropropane, 1,3-bis(3-amino-α,α-ditrifluoromethylbenzyl)benzene, 1,3-bis bis(4-amino-α,α-ditrifluoromethylbenzyl)benzene, 1,4-bis(3-amino-α,α-ditrifluoromethylbenzyl)benzene, 1,4-bis(4-amino-α,α-ditrifluoromethylbenzyl)benzene, bis[4-(3-aminophenoxy)phenyl]sulfone, bis[4-(4-aminophenoxy)phenyl]sulfone, 2,2-bis[3-(3-aminophenoxy)phenyl]-1,1,1,3,3,3-hexafluoropropane, 2,2-bis[4-(4-aminophenoxy)phenyl]-1,1,1,3,3,3-Hexafluoropropane, 4,4'-bis[4-(4-amino-α,α-dimethylbenzyl)phenoxy]diphenyl sulfone, 4,4'-bis[4-(4-aminophenoxy)phenoxy]diphenyl sulfone, 1,2-diaminocyclohexane, 1,3-diaminocyclohexane, 1,4-diaminocyclohexane, 1,2-di(2-aminoethyl)cyclohexane, 1,3-di(2-aminoethyl)cyclohexane, 1,4-di(2-aminoethyl)cyclohexane, bis(4-aminocyclohexyl)methane, 2,6-bis(aminomethyl)bicyclo[2.2.1]heptane, 2,5-bis(aminomethyl)bicyclo[2.2.1]heptane, 9,9'-bis(4-aminophenyl)fluorene (FDA), 9,9'-bis(4-amino-3-fluorophenyl)fluorene (FFDA).

[0065] Among the above, the diamines represented by Y-1 to Y-5 are preferred from the viewpoint of reducing the birefringence of the polyimide, and the diamine represented by Y-6 is preferred from the viewpoint of transparency. 9 is a methyl group or hydrogen. The polyimide may contain, as diamine components, both Y-6 and one or more selected from Y-1 to Y-5.

[0066] [ka]

[0067] The amount of the above diamines relative to the total amount of the diamine components (100 mol%) is preferably 5 mol% or more, more preferably 10 mol% or more, and even more preferably 15 mol% or more, and may be 20 mol% or more, 30 mol% or more, 40 mol% or more, 50 mol% or more, 60 mol% or more, 70 mol% or more, 80 mol% or more, 90 mol% or more, or 100%. The total of Y-1 to Y-6 may be within this range.

[0068] From the viewpoint of transparency and solubility of the polyimide, the amount of 2,2'-bis(trifluoromethyl)benzidine (Y-6 above) relative to the total amount of the diamine components is preferably 5 mol % or more, and may be 10 to 99 mol %, 20 to 98 mol %, 30 to 97 mol %, 35 to 96 mol %, or 40 to 95 mol %.

[0069] A diamine that does not contain any of a fluorine group, a trifluoromethyl group, a sulfone group, a fluorene structure, and an alicyclic structure may be used within a range that does not excessively decrease the transparency and solubility in an organic solvent of the polyimide. Specific examples thereof include 1,4-phenylenediamine, 1,3-phenylenediamine, 3,3'-diaminodiphenyl ether, 3,4'-diaminodiphenyl ether, 4,4'-diaminodiphenyl ether, 3,3'-diaminodiphenyl sulfide, 3,4'-diaminodiphenyl sulfide, 4,4'-diaminodiphenyl sulfide, 3,3'-diaminobenzophenone, 4,4'-diaminobenzophenone, and 3,4'-diaminobenzof. phenylene, 3,3'-diaminodiphenylmethane, 4,4'-diaminodiphenylmethane, 3,4'-diaminodiphenylmethane, 2,2-di(3-aminophenyl)propane, 2,2-di(4-aminophenyl)propane, 2-(3-aminophenyl)-2-(4-aminophenyl)propane, 1,1-di(3-aminophenyl)-1-phenylethane, 1,1-di(4-aminophenyl)-1-phenylethane, 1-(3-aminophenyl)-1-( 1,3-bis(3-aminophenoxy)benzene, 1,3-bis(4-aminophenoxy)benzene, 1,4-bis(3-aminophenoxy)benzene, 1,4-bis(4-aminophenoxy)benzene, 1,3-bis(3-aminobenzoyl)benzene, 1,3-bis(4-aminobenzoyl)benzene, 1,4-bis(3-aminobenzoyl)benzene, 1,4-bis(4-aminobenzoyl)benzene Zene, 1,3-bis(3-amino-α,α-dimethylbenzyl)benzene, 1,3-bis(4-amino-α,α-dimethylbenzyl)benzene, 1,4-bis(3-amino-α,α-dimethylbenzyl)benzene, 1,4-bis(4-amino-α,α-dimethylbenzyl)benzene, 2,6-bis(3-aminophenoxy)benzonitrile, 2,6-bis(3-aminophenoxy)pyridine, 4,4'-bis(3-aminophenoxy)biphenyl, 4,4'-Bis(4-aminophenoxy)biphenyl, bis[4-(3-aminophenoxy)phenyl]ketone, bis[4-(4-aminophenoxy)phenyl]ketone, bis[4-(3-aminophenoxy)phenyl]sulfide, bis[4-(4-aminophenoxy)phenyl]sulfide, bis[4-(3-aminophenoxy)phenyl]ether, bis[4-(4-aminophenoxy)phenyl]ether, 2,2-bis[4-(3-aminophenoxy)phenyl]propane, 2,2-bis[4-(4-aminophenoxy)phenyl]propane, 1,3-bis[4-(3-aminophenoxy)phenyl]propane, 1,3-bis[4-(4-aminophenoxy)benzoyl]benzene, 1,3-bis[4-(4-aminophenoxy)benzoyl]benzene, 1,4-bis[4-(3-aminophenoxy)benzoyl]benzene, 1,4-bis[4-(4-aminophenoxy)benzoyl]benzene, 1,3-bis[4-(3-aminophenoxy)-α,α-dimethylbenzyl]benzene, 1,3-bis[4-(4-aminophenoxy)-α,α-dimethylbenzyl]benzene, 1,4- Bis[4-(3-aminophenoxy)-α,α-dimethylbenzyl]benzene, 1,4-bis[4-(4-aminophenoxy)-α,α-dimethylbenzyl]benzene, 4,4'-bis[4-(4-aminophenoxy)benzoyl]diphenyl ether, 4,4'-bis[4-(4-amino-α,α-dimethylbenzyl)phenoxy]benzophenone, 3,3'-diamino-4,4'-diphenoxybenzophenone, 3,3'-diamino-4,4'-dibiphenoxybenzophenone, 3,3'-diamino-4-fu Phenoxybenzophenone, 3,3'-diamino-4-biphenoxybenzophenone, 6,6'-bis(3-aminophenoxy)-3,3,3',3'-tetramethyl-1,1'-spirobiindane, 6,6'-bis(4-aminophenoxy)-3,3,3',3'-tetramethyl-1,1'-spirobiindane, 1,3-bis(3-aminopropyl)tetramethyldisiloxane, 1,3-bis(4-aminobutyl)tetramethyldisiloxane, α,ω-bis(3-aminopropyl)polydimethylsiloxane, α,ω-bis(3-aminobutyl)polydimethylsiloxane, bis(aminomethyl)ether, bis(2-aminoethyl)ether, bis(3-aminopropyl)ether, bis(2-aminomethoxy)ethyl]ether, bis[2-(2-aminoethoxy)ethyl]ether, bis[2-(3-aminoprotoxy)ethyl]ether, 1,2-bis(aminomethoxy)ethane, 1,2-bis(2-aminoethoxy)ethane, 1,2-bis[2-(aminomethoxy)ethoxy]ethane, 1,2-bis[2-(2-aminoethoxy)ethoxy]ethane, Examples of the amino groups include dimethylaminoethane, ethylene glycol bis(3-aminopropyl) ether, diethylene glycol bis(3-aminopropyl) ether, triethylene glycol bis(3-aminopropyl) ether, ethylenediamine, 1,3-diaminopropane, 1,4-diaminobutane, 1,5-diaminopentane, 1,6-diaminohexane, 1,7-diaminoheptane, 1,8-diaminooctane, 1,9-diaminononane, 1,10-diaminodecane, 1,11-diaminoundecane, and 1,12-diaminododecane.

[0070] (Polyimide composition) As described above, by adjusting the composition of the polyimide, i.e., the types and ratios of the acid dianhydrides and diamines, the polyimide has transparency and solubility in organic solvents, and also exhibits compatibility with ester polymers. The solubility parameter (SP value) can be used as an index of the solubility of polyimide in organic solvents and its compatibility with other resins.

[0071] The SP value of a polyimide is the sum of the products of the SP value of each monomer (acid dianhydride and diamine) and the composition ratio (molar ratio where the sum of the acid dianhydride and diamine is 1). The smaller the difference in SP value between the polyimide and the solvent and other resins, the higher the solubility and compatibility tends to be. From the viewpoint of compatibility with ester resins, the SP value of polyimide is 8.10 to 9.10 (cal / cm 3 ) 1 / 2 is preferable, and 8.15 to 9.00 (cal / cm 3 ) 1 / 2 may be also possible.

[0072] The polyimide preferably exhibits solubility in one or more solvents selected from methylene chloride, chloroform, 1,2-dichloroethane, 1,1,2,2-tetrachloroethane, N-methyl-2-pyrrolidone, chlorobenzene, dichlorobenzene, tetrahydrofuran, and 1,4-dioxane. The polyimide exhibits solubility in a solvent means that it dissolves at a concentration of 5% by weight or more. Among the above solvents, methylene chloride has a low boiling point and is easy to remove the remaining solvent during film production, so the polyimide is preferably soluble in methylene chloride.

[0073] (Preparation of polyimide resin) Polyamic acid as a polyimide precursor is obtained by the reaction of an acid dianhydride with a diamine, and polyimide is obtained by cyclization (imidization) of the polyamic acid.

[0074] The method for preparing the polyamic acid is not particularly limited, and any known method can be applied. For example, a polyamic acid solution can be obtained by dissolving an acid dianhydride and a diamine in approximately equimolar amounts (molar ratio of 95:100 to 105:100) in an organic solvent and stirring the mixture. The concentration of the polyamic acid solution is usually 5 to 35% by weight, and preferably 10 to 30% by weight. When the concentration is within this range, the polyamic acid obtained by polymerization has an appropriate molecular weight, and the polyamic acid solution has an appropriate viscosity.

[0075] In the polymerization of polyamic acid, it is preferable to add the diamine to the dianhydride in order to suppress ring-opening of the dianhydride. When adding a plurality of diamines or a plurality of dianhydrides, they may be added at once or in a plurality of portions. By adjusting the order of addition of the monomers, the physical properties of the polyimide can be controlled.

[0076] The organic solvent used for the polymerization of polyamic acid is not particularly limited as long as it does not react with diamines and acid dianhydrides and can dissolve polyamic acid. Examples of the organic solvent include urea-based solvents such as methylurea and N,N-dimethylethylurea, sulfoxide or sulfone-based solvents such as dimethylsulfoxide, diphenylsulfone, and tetramethylsulfone, amide-based solvents such as N,N-dimethylacetamide (DMAc), N,N-dimethylformamide (DMF), N,N'-diethylacetamide, N-methyl-2-pyrrolidone (NMP), γ-butyrolactone, and hexamethylphosphoric acid triamide, halogenated alkyl solvents such as chloroform and methylene chloride, aromatic hydrocarbon solvents such as benzene and toluene, and ether-based solvents such as tetrahydrofuran, 1,3-dioxolane, 1,4-dioxane, dimethyl ether, diethyl ether, and p-cresol methyl ether. Usually, these solvents are used alone or in appropriate combination of two or more as necessary. From the viewpoint of the solubility and polymerization reactivity of the polyamic acid, DMAc, DMF, NMP, etc. are preferably used.

[0077] Polyimide is obtained by dehydration cyclization of polyamic acid. As a method for preparing polyimide from a polyamic acid solution, a method of adding a dehydrating agent, an imidization catalyst, etc. to the polyamic acid solution and proceeding with imidization in the solution can be mentioned. In order to promote the progress of imidization, the polyamic acid solution may be heated. By mixing a solution containing polyimide generated by imidization of polyamic acid with a poor solvent, polyimide resin is precipitated as a solid. By isolating the polyimide resin as a solid, impurities generated during the synthesis of polyamic acid, residual dehydrating agents, imidization catalysts, etc. can be washed and removed with a poor solvent, and coloring of polyimide and increase in yellowness can be prevented. In addition, by isolating the polyimide resin as a solid, a solvent suitable for film formation, such as a low boiling point solvent, can be applied when preparing a solution for producing a film.

[0078] The molecular weight of the polyimide (weight average molecular weight in terms of polyethylene oxide measured by gel permeation chromatography (GPC)) is preferably 10,000 to 200,000, more preferably 20,000 to 180,000, and even more preferably 40,000 to 180,000. If the molecular weight is too small, the strength of the film may be insufficient. If the molecular weight is too large, the compatibility with the ester resin may be poor.

[0079] <Ester resin> The ester resin in this embodiment is a polycarbonate or a polyarylate, and contains a structural unit represented by the above general formula (2).

[0080] (Polycarbonate) Polycarbonate is a carbonate ester of bisphenol and has a repeating unit represented by general formula (7).

[0081] [ka]

[0082] Z and R in general formula (7) 3 and j represents Z, R in general formula (2). 3 and j.

[0083] From the viewpoints of solubility in organic solvents and compatibility with the above-mentioned polyimide, the polycarbonate is preferably one in which the divalent organic group Z is an isopropylidene group and j=0, i.e., a carbonate ester of bisphenol A having a repeating unit of formula (8).

[0084] [ka]

[0085] Commercially available polycarbonates containing the repeating unit of formula (8) include Teijin's Panlite AD-5503, K-1300Y, L-1225L, L-1225LM, L-1225Y, L-1225Z100, L-1225Z100M, L-1225ZL100, L-1250Y, L-1250Z100, LD-1000RM, LN-1010RM, LN-2250Y, LN-2250Z, and LN-25 20A, LN-2520HA, LN-2525ZA, LN-3000RM, LN-3050RM, LS-2250, LV-2225L, LV-2225Y, LV-2225Z, LV-2250Y, LV-2250Z, MN-4800, MN-4800Z, MN-4805Z; Iupilon K4100, ML200, ML300, ML400 manufactured by Mitsubishi Engineering Plastics Corporation, and the like.

[0086] The polycarbonate may contain a bisphenol component other than bisphenol A. Specific examples of bisphenols include 1,2-bis(4-hydroxyphenyl)ethane, 2-(4-hydroxyphenyl)-2-(3-hydroxyphenyl)propane, 1,2,2-bis(3-methyl-4-hydroxyphenyl)propane, 2,2-bis(3-ethyl-4-hydroxyphenyl)propane, 2,2-bis(3-n-propyl-4-hydroxyphenyl)propane, 2,2-bis(3-isopropyl-4-hydroxyphenyl)propane, 2,2-bis(3-sec-butyl-4-hydroxyphenyl)propane, 2,2-bis(3-t-butyl-4-hydroxyphenyl)propane, 2,2-bis(3-cyclohexyl-4-hydroxyphenyl)propane, 2,2-bis(3-allyl-4-hydroxyphenyl)propane, 2,2-bis(3-methoxy-4-hydroxyphenyl)propane, bis(4-hydroxyphenyl)ether, bis(4-hydroxyphenyl)sulfide, and bis(4-hydroxyphenyl). Sulfoxide, bis(4-hydroxyphenyl)sulfone, 1,6-dihydroxynaphthalene, 2,6-dihydroxynaphthalene, 6,6'-dihydroxy-3,3,3',3'-tetramethylspiro(bis)indan, 2,6-dihydroxydibenzo-p-dioxin, 2,6-dihydroxyanthrene, 2,7-dihydroxyphenoxathin, 2,7-dihydroxy-9,10-dimethylphenazine, 3,6-dihydroxybenzofuran, 3,6-dihydroxya Examples of the phenolic compounds include toluene, tert-butylhydroquinone, 2,5-di-tert-butylhydroquinone, 2,5-di-tert-amylhydroquinone, 2,2'-dimethylbiphenyl-4,4'-diol, 3,3'-dimethylbiphenyl-4,4'-diol, isopropylidenediphenol, 3,3',5,5'-tetramethylbiphenyl-4,4'-diol, 2,2',3,3',5,5'-hexamethylbiphenyl-4,4'-diol, and resorcinol.

[0087] The divalent organic group Z in formula (7) may contain a cyclic structure. Examples of the cyclic structure include aromatics such as fluorene skeleton and phthalimide skeleton; and alicyclic skeletons such as cyclohexylmethylidene, 2-[2.2.1]-bicycloheptylidene, cyclohexylidene, cyclopentylidene, cyclododecylidene, and adamantylidene. Specific examples of bisphenols in which Z contains a cyclic structure include 9,9-bis(4-hydroxyphenyl)fluorene, 9,9-bis[4-(2-hydroxyethoxy)phenyl]fluorene, 9,9-bis(4-hydroxy-3-methylphenyl)fluorene, 3,3-bis(4-hydroxyphenyl)phthalimidine, 2-phenyl-3,3-bis(4-hydroxyphenyl)phthalimidine, and 1,1-bis(4-hydroxy-3-methylphenyl)cyclohexane.

[0088] From the viewpoints of film strength and compatibility with polyimide, the weight average molecular weight (polystyrene equivalent) of the polycarbonate is preferably from 5,000 to 250,000, more preferably from 10,000 to 200,000, and even more preferably from 15,000 to 150,000.

[0089] (Polyarylate) Polyarylates are esters of bisphenol and phthalic acid (terephthalic acid and / or isophthalic acid), and have repeating units represented by the general formula (9).

[0090] [ka]

[0091] Z and R in general formula (9) 3 and j represents Z, R in general formula (2). 3 and j.

[0092] The ratio of the isophthalic acid-derived structure to the terephthalic acid-derived structure in the polyarylate is not particularly limited and is 0:100 to 100:0. From the viewpoints of solubility in a solvent and compatibility with the polyimide, the ratio of isophthalic acid to terephthalic acid is preferably 2:98 to 98:2, and may be 5:95 to 95:5, or 10:90 to 90:10.

[0093] From the viewpoints of solubility in organic solvents and compatibility with the above-mentioned polyimides, the polyarylate is preferably one in which the divalent organic group Z is an isopropylidene group and j=0, i.e., an ester of bisphenol A and phthalic acid having a repeating unit of formula (10).

[0094] [ka]

[0095] Commercially available polyarylates containing the repeating unit of formula (10) include U-100 and T-200 manufactured by Unitika Co., Ltd. Commercially available polyarylates include U-8000, U-8400H, FUN-8000, C300VN, P-1001, P-3001, P-5001, P-1001A, P-3001S, and P-5001S manufactured by Unitika Co., Ltd.

[0096] The polyarylate may contain a bisphenol component other than bisphenol A. Specific examples of bisphenols other than bisphenol A include those previously listed as the bisphenol components of polycarbonate.

[0097] From the viewpoints of film strength and compatibility with polyimide, the weight average molecular weight (polystyrene equivalent) of the polyarylate is preferably from 5,000 to 150,000, more preferably from 10,000 to 130,000, and even more preferably from 15,000 to 100,000.

[0098] <Preparation of Resin Composition> The polyimide resin and the ester resin are mixed to prepare a resin composition. The resin composition may contain both polycarbonate and polyarylate as the ester resin.

[0099] The polyimide resin and the ester resin can be compatible at any ratio, so the ratio of the polyimide resin and the ester resin in the resin composition is not particularly limited. The mixing ratio (weight ratio) of the polyimide resin and the ester resin may be 98:2 to 2:98, 95:5 to 10:90, or 90:10 to 15:85. The higher the ratio of the polyimide resin, the higher the elastic modulus of the film and the more excellent the mechanical strength. The higher the ratio of the ester resin, the smaller the birefringence of the film (particularly the birefringence in the thickness direction).

[0100] Polyimide is a polymer having a special molecular structure, and generally has low solubility in organic solvents and is not compatible with other polymers. In this embodiment, the polyimide contains a bis(trimellitic anhydride) ester of general formula (3) as an acid anhydride component, and has a structural unit of general formula (1), so that the polyimide exhibits high solubility in organic solvents and exhibits compatibility with polycarbonate and polyarylate. One of the reasons why the polyimide exhibits solubility in polycarbonate and polyarylate is that the structure of the phenol ester in general formula (1) and general formula (3) is highly similar to the structure of the bisphenol ester in polycarbonate and polyarylate.

[0101] In order to have compatibility with polycarbonate, the polyimide is prepared by mixing the acid dianhydride represented by the general formula (3) with respect to the total of 100 mol % of the acid dianhydride components. 60 It is preferable that the content is mol % or more. 、6 It is more preferable that the acid dianhydride of the formula (6) is contained in an amount of 5 mol % or more. 60 It is preferable that the content is mol % or more. 、6 It is more preferable that the content is 5 mol % or more.

[0102] In order to have compatibility with polyarylate, the polyimide preferably contains 30 mol % or more, more preferably 40 mol % or more, and even more preferably 45 mol % or more of the acid dianhydride of general formula (3) relative to 100 mol % in total of the acid dianhydride components. Among them, the polyimide preferably contains 30 mol % or more, more preferably 40 mol % or more, and even more preferably 45 mol % or more of the acid dianhydride of formula (6).

[0103] The resin composition may be a mixed solution containing a polyimide resin and an ester resin. The method of mixing the resins is not particularly limited, and the resins may be mixed in a solid state or in a liquid to form a mixed solution. A polyimide resin solution and an ester resin solution may be prepared separately, and the two may be mixed to prepare a mixed solution of the polyimide resin and the ester resin.

[0104] The solvent of the solution containing the polyimide resin and the ester resin is not particularly limited as long as it is soluble in both the polyimide resin and the ester resin. Examples of the solvent include N,N-dimethylformamide, N,N-dimethylacetamide, N-methylpyrrolidone, chloroform, 1,2-dichloroethane, 1,1,2,2-tetrachloroethane, N-methyl-2-pyrrolidone, chlorobenzene, dichlorobenzene, tetrahydrofuran, 1,4-dioxane, methylene chloride, etc. Methylene chloride is particularly preferred as the solvent because it has excellent compatibility with the polyimide resin and the ester resin, has a low boiling point, and is easy to remove the remaining solvent during film production.

[0105] For the purpose of improving the processability of the film and imparting various functions, an organic or inorganic low-molecular or high-molecular compound may be blended into the resin composition (solution). The resin composition may contain a flame retardant, an ultraviolet absorber, a crosslinking agent, a dye, a pigment, a surfactant, a leveling agent, a plasticizer, fine particles, a sensitizer, etc. The fine particles include organic fine particles such as polystyrene and polytetrafluoroethylene, and inorganic fine particles such as colloidal silica, carbon, and layered silicate, and may have a porous or hollow structure.

[0106] [film] A solution containing the above-mentioned polyimide resin and ester resin is applied onto a support, and the solvent is then dried and removed to obtain a film.

[0107] The resin solution can be applied to the support by a known method using a bar coater or a comma coater. The support can be a glass substrate, a metal substrate such as SUS, a metal drum, a metal belt, a plastic film, or the like. From the viewpoint of improving productivity, it is preferable to use an endless support such as a metal drum or a metal belt, or a long plastic film, or the like, as the support and produce the film by roll-to-roll. When using a plastic film as the support, it is only necessary to appropriately select a material that is not dissolved in the solvent of the film-forming dope, and the plastic material can be polyethylene terephthalate, polyacrylate, polyethylene naphthalate, or the like.

[0108] It is preferable to perform heating when drying the solvent. The heating temperature is not particularly limited as long as it can remove the solvent and can suppress coloration of the obtained film, and is appropriately set at about room temperature to 250°C, and preferably 50°C to 220°C. If the temperature is within this range, coloration of the film can be suppressed and the retardation (birefringence) in the thickness direction of the film can be reduced. The heating temperature may be increased stepwise. In order to increase the efficiency of removing the solvent, the resin film may be peeled off from the support and dried after drying has progressed to a certain extent. In order to promote the removal of the solvent, heating may be performed under reduced pressure.

[0109] The thickness of the film is not particularly limited and may be appropriately set depending on the application. The thickness of the film is, for example, 5 to 300 μm. From the viewpoint of obtaining a film that is both self-supporting and flexible and has high transparency, the thickness of the film is preferably 20 μm to 100 μm, and may be 30 μm to 90 μm, 40 μm to 85 μm, or 50 μm to 80 μm. The thickness of the film used as a cover film for a display is preferably 50 μm or more.

[0110] The haze of the film is preferably 5% or less, more preferably 4% or less, even more preferably 3.5% or less, and may be 3% or less, 2% or less, or 1% or less. The lower the haze of the film, the better. As described above, the polyimide resin and the ester resin are compatible with each other, so that a film with low haze and high transparency can be obtained. The higher the ratio of the dianhydride of general formula (3) among the dianhydride components of the polyimide, the lower the haze of the film tends to be, and in particular, the higher the ratio of the dianhydride of formula (6), the lower the haze of the film tends to be.

[0111] The yellowness index (YI) of the film is preferably not more than 5.0. As described above, the polyimide having the structural unit represented by the general formula (1) has low visible light absorption, and therefore a film having high transparency and a small YI can be obtained.

[0112] From the viewpoint of suppressing the decrease in visibility due to the coloring of the screen, the thickness direction retardation Rth of the film is preferably 3000 nm or less. From the viewpoint of strength, the tensile modulus of the film is preferably 3.0 GPa or more. Since the polyimide resin and the ester resin are compatible with each other, the Rth and the tensile modulus are intermediate values ​​between a film made of only the polyimide resin and a film made of only the ester resin, and by adjusting the compounding ratio of the two, a film that satisfies both the above Rth and the tensile modulus can be obtained. EXAMPLES

[0113] Hereinafter, the embodiment of the present invention will be described in more detail based on examples and comparative examples. However, the present invention is not limited to the following examples.

[0114] [Polyimide resin manufacturing example] Dimethylformamide was added to a separable flask and stirred under a nitrogen atmosphere. Diamine and acid dianhydride were added in the ratios (mol%) shown in Table 2, and the mixture was reacted by stirring for 5 to 10 hours under a nitrogen atmosphere to obtain a polyamic acid solution with a solid concentration of 18% by weight. In Production Examples 1A to 1C, Production Examples 3A and 3B, Production Examples 4A and 4B, Production Examples 6A and 6B, and Production Examples 11A and 11B, the molecular weight was adjusted by changing the reaction time.

[0115] 5.5g of pyridine was added as an imidization catalyst to 100g of polyamic acid solution, and after complete dispersion, 8g of acetic anhydride was added and stirred at 90°C for 3 hours. After cooling to room temperature, 100g of 2-propyl alcohol (hereinafter referred to as IPA) was added at a rate of 2-3 drops / second while stirring the solution, and polyimide was precipitated. Further, 150g of IPA was added, and after stirring for about 30 minutes, suction filtration was performed using a Kiriyama funnel. The obtained solid was washed with IPA and then dried for 12 hours in a vacuum oven set at 120°C to obtain a polyimide resin.

[0116] [Film production example] <Films 1-14> The polyimide (PI) obtained in the above Production Example and a commercially available polyarylate (PC) were mixed in methylene chloride in the ratio shown in Table 3 to prepare a methylene chloride solution with a resin content of 11% by weight. This solution was applied to a non-alkali glass plate and dried by heating in an air atmosphere at 40°C for 60 minutes, 70°C for 30 minutes, 150°C for 30 minutes, 170°C for 30 minutes, and 200°C for 60 minutes to produce films 1 to 14 with a thickness of approximately 50 μm.

[0117] <Films 21-28> The polyimide (PI) obtained in the above Production Example and a commercially available polycarbonate (PC) were mixed in methylene chloride in the ratio shown in Table 4 to prepare a methylene chloride solution with a resin content of 11% by weight. Using this solution, coating and drying were performed under the same conditions as in the preparation of the above films 1 to 14, to prepare films 21 to 28 with a thickness of approximately 50 μm.

[0118] <Reference examples A~D> In Reference Examples A and C, a methylene chloride solution of polyimide resin was prepared, and a film of about 50 μm thickness was produced under the same conditions as above. In Reference Example B, a methylene chloride solution of polyarylate was prepared, and a film of about 50 μm thickness was produced under the same conditions as above. In Reference Example D, a methylene chloride solution of polyalicarbonate was prepared, and coating and drying were performed under the same conditions as above to produce a film of about 50 μm thickness.

[0119] [Evaluation method] <Evaluation of polyimide resin> (Solubility in methylene chloride) Methylene chloride was added to the polyimide resin so that the solid concentration was 10% by weight, and after stirring at room temperature for 12 hours, the solution was visually confirmed. No insoluble matter was found in any of the polyimide resins of the production examples, and they were soluble in methylene chloride.

[0120] (molecular weight) The polyimide was dissolved in an eluent to a concentration of 0.4% by weight, and analyzed by GPC under the conditions shown in Table 1 to determine the weight average molecular weight (Mw).

[0121] [Table 1]

[0122] <Film evaluation> (Hayes) The film was cut into 3 cm squares and measured using a haze meter "HZ-V3" manufactured by Suga Test Instruments in accordance with JIS K7136. For films with a haze of more than 20%, the following measurements of yellowness, tensile modulus, and thickness direction retardation were not performed (represented as ND in Tables 3 and 4).

[0123] (yellowness) The film was cut into 3 cm squares, and the yellowness index (YI) was measured according to JIS K7373 using a spectrophotometer "SC-P" manufactured by Suga Test Instruments.

[0124] (tensile modulus) The film was cut into strips 10 mm wide and measured using Shimadzu Corporation's "AUTOGRAPH AGS-X" at a gripping distance of 100 mm and a pulling speed of 20.0 mm / min.

[0125] (Thickness direction phase difference) The film was cut into 3 cm squares, and the in-plane retardation and oblique retardation at a wavelength of 590 nm were measured using a retardation measurement device "KOBRA" manufactured by Oji Scientific Instruments, and the thickness direction retardation Rth was calculated assuming an average refractive index of 1.60.

[0126] [Evaluation Results] The compositions of diamines and dianhydrides in the polyimide production examples, as well as the SP values ​​and weight average molecular weights (Mw) of the polyimides are shown in Table 2. The unit of the SP values ​​in Table 2 is (cal / cm 3 ) 1 / 2 The SP value of the polyimide is the sum of the products of the SP value of each monomer and the molar ratio to the total of the diamine and the acid dianhydride.

[0127] In Table 2, the compounds are described by the following abbreviations. <Diamine> TFMB: 2,2'-bis(trifluoromethyl)benzidine 3,3'-DDS: 3,3'-diaminodiphenyl sulfone <Acid dianhydride> TAHMBP: Bis(1,3-dioxo-1,3-dihydroisobenzofuran-5-carboxylic acid)-2,2',3,3',5,5'-hexamethylbiphenyl-4,4'-diyl OCBP-TME: Bis(1,3-dioxo-1,3-dihydroisobenzofuran-5-carboxylic acid)-3,3'-dimethylbiphenyl-4,4'-diyl BP-TME: Bis(1,3-dioxo-1,3-dihydroisobenzofuran-5-carboxylic acid)-biphenyl-4,4'-diyl Bis-DA2000: 4,4'-(4,4'-isopropylidenediphenoxy)diphthalic dianhydride TMHQ: p-phenylene bis(trimellitic acid monoester anhydride) s-BPDA: 3,3',4,4'-biphenyltetracarboxylic dianhydride α-BPDA: Diphenyl-2,3,3',4'-tetracarboxylic dianhydride CBDA: 1,2,3,4-cyclobutanetetracarboxylic dianhydride 6FDA: 2,2-bis(3,4-dicarboxyphenyl)-1,1,1,3,3,3-hexafluoropropane dianhydride

[0128] [Table 2]

[0129] The resin compositions and film properties of Films 1 to 14 (compositions of polyimide and polyarylate) produced in the Film Production Examples are shown in Table 3, and the resin compositions and film properties of Films 21 to 28 (compositions of polyimide and polycarbonate) are shown in Table 4. Table 3 shows the results of Reference Examples A and B, and Table 4 shows the results of Reference Examples C and D.

[0130] In Tables 3 and 4, the polyimides represented by general formula (3) are extracted from the dianhydride components of polyimide (PI) and listed. The numbers in parentheses indicate the ratio (mol%) of the dianhydride to the total amount of dianhydride components.

[0131] The polyarylates (PAR) in Table 3 and the polycarbonates (PC) in Table 4 are as follows. Mw is the weight average molecular weight measured by GPC in terms of polystyrene. PAR1: Unitika "U-100 D Series" Mw=71,000 PAR2: Unitika "U-100 L Series" Mw=45,600 PC1: Mitsubishi Engineering Plastics "Iupilon K4100" Mw=38,400 PC2: Teijin "Panlite L-1225LM" Mw=42,000

[0132] [Table 3]

[0133] [Table 4]

[0134] The polyimide film of Reference Example A made using only polyimide 1A and the polyimide film of Reference Example C made using only polyimide 10 had low haze, excellent transparency, and showed high tensile modulus, but had large Rth. The polyarylate film of Reference Example B made using only polyarylate and the polycarbonate film of Reference Example D made using only polycarbonate had excellent transparency and showed small Rth, but had a tensile modulus of about 2 GPa, which was not enough for mechanical strength.

[0135] As shown in Table 3, films 1 to 10 using compositions of polyimide containing a bis(trimellitic anhydride) ester represented by general formula (3), such as TAHMBP, as an acid dianhydride component and polyarylate exhibited high transparency and showed tensile modulus and Rth values ​​intermediate between those of polyimide and polyarylate.

[0136] Comparing Film 1 and Film 2, it can be seen that the higher the ratio of polyimide, the higher the tensile modulus, and the higher the ratio of polyarylate, the smaller the Rth tends to be. Comparing Film 2 and Film 3, it is considered that the difference in the molecular weight of polyimide does not have a significant effect on the haze, tensile modulus, or Rth.

[0137] Films 11 to 14 using compositions of polyimide not containing bis(trimellitic anhydride) ester represented by general formula (3) as an acid dianhydride component and polyarylate had high haze and were poorly suited for practical optical applications. Since the polyimide resin and polyarylate used in the preparation of these films each give a transparent film when used alone, it is believed that the poor compatibility of the resins is the cause of the cloudiness.

[0138] These results show that polyimides containing the bis(trimellitic anhydride) ester represented by the general formula (3) and polyarylates are compatible, making it possible to prepare highly transparent films, and that by adjusting the mixing ratio of the two, it is possible to prepare films that can achieve both a high tensile modulus and a low Rth.

[0139] Film 4, which was a mixture of polyimide 2, in which the amount of TAHMBP relative to the total amount of dianhydride was 45 mol%, and polyarylate in a weight ratio of 80:20, maintained transparency, but showed an increase in haze compared to film 1. Film 10, which was a mixture of polyimide 9, in which the amount of TAHMBP relative to the total amount of dianhydride was 40 mol%, and polyarylate in a weight ratio of 80:20, showed an even higher increase in haze. These results show that the higher the ratio of TAHMBP in the dianhydride component of the polyimide, the better the compatibility with polyarylate.

[0140] As an acid dianhydride, in addition to 50 mol% TAHMBP 、B Film 5, which was a mixture of polyimide 3A containing is-DA2000 and polyarylate, showed small haze similar to that of films 1 to 3. The same was true for films 6 and 7.

[0141] Film 8, which was prepared by mixing polyimide 7 containing 40 mol % TAHMBP as an acid dianhydride component, as well as BP-TME, an ester of biphenol and trimellitic anhydride, with polyarylate, showed a haze of about 3%, similar to film 10. Film 9, which used polyimide 8 containing OCBP-TME as an acid dianhydride component, also showed a haze of about 3%.

[0142] From the above results, it can be seen that, among the compounds of general formula (3), TAHMBP, which contains a biphenyl skeleton having three substituents on each benzene ring, contributes particularly greatly to improving compatibility with polyarylate.

[0143] As shown in Table 4, film 21 using a composition of polyimide containing a bis(trimellitic anhydride) ester represented by general formula (3), such as TAHMBP, as an acid dianhydride component and polycarbonate exhibited high transparency and a tensile modulus and Rth that were intermediate between those of polyimide and polycarbonate.

[0144] Films 26 to 28 made of compositions of polyimide not containing bis(trimellitic anhydride) ester represented by general formula (3) as an acid dianhydride component and polycarbonate had high haze and were poorly suited for practical optical applications. Since the polyimide resin and polycarbonate used in the preparation of these films each give a transparent film when used alone, it is believed that the cloudiness is due to poor compatibility of the resins.

[0145] Polyimides 22 to 25, which contained Bis-DA2000 in addition to 50 mol % TAHMBP as an acid dianhydride, had smaller haze than films 26 to 28, but had higher haze than film 21. These results show that TAHMBP, as an acid dianhydride component of polyimide, contributes greatly to improving compatibility even when polyimide is mixed with polycarbonate.

Claims

1. Contains polyimide resin and polyarylate, the polyimide resin is a polyimide containing a structural unit represented by general formula (1) obtainable by a reaction between an acid dianhydride represented by general formula (3) and a diamine represented by general formula (4), [Formula 1] [Case 2] [C3] The amount of the tetracarboxylic acid dianhydride represented by the general formula (3) is 30 mol % or more based on the total amount of the acid dianhydride components of the polyimide. Resin composition: however, In general formula (1) and general formula (3), X is a divalent organic group represented by group (I), [C4] R 1 and R 2 are each a fluorine atom, an alkyl group having 1 to 20 carbon atoms, or a fluoroalkyl group having 1 to 20 carbon atoms, m is an integer of 1 to 4, and n is an integer of 0 to 4; In general formula (1) and general formula (4), Y is a divalent group containing one or more selected from the group consisting of a fluorine group, a trifluoromethyl group, a sulfone group, a fluorene structure, and an alicyclic structure.

2. The resin composition according to claim 1 , wherein the polyimide contains 30 mol % or more of the acid dianhydride represented by formula (6) based on the total amount of the acid dianhydride components. [C5]

3. The resin composition according to claim 1 or 2, wherein the polyarylate contains a repeating unit represented by formula (10). [C7]

4. The resin composition according to any one of claims 1 to 3, comprising the polyimide resin and the polyarylate in a weight ratio ranging from 98:2 to 2:

98.

5. Contains polyimide resin and polycarbonate, the polyimide resin is a polyimide containing a structural unit represented by general formula (1) obtainable by a reaction between an acid dianhydride represented by general formula (3) and a diamine represented by general formula (4), [C8] [C9] [C10] The amount of the tetracarboxylic acid dianhydride represented by the general formula (3) is 60 mol % or more based on the total amount of the acid dianhydride components of the polyimide. Resin composition: however, In general formula (1) and general formula (3), X is a divalent organic group represented by group (I), [C11] R 1 and R 2 are each a fluorine atom, an alkyl group having 1 to 20 carbon atoms, or a fluoroalkyl group having 1 to 20 carbon atoms, m is an integer of 1 to 4, and n is an integer of 0 to 4; In general formula (1) and general formula (4), Y is a divalent group containing one or more selected from the group consisting of a fluorine group, a trifluoromethyl group, a sulfone group, a fluorene structure, and an alicyclic structure.

6. The resin composition according to claim 5 , wherein the polyimide contains 60 mol % or more of the acid dianhydride represented by formula (6) based on the total amount of the acid dianhydride components. [C12]

7. The resin composition according to claim 5 or 6, wherein the polycarbonate contains a repeating unit represented by formula (8). [C6]

8. The resin composition according to any one of claims 5 to 7, comprising the polyimide resin and the polycarbonate in a weight ratio ranging from 98:2 to 2:

98.

9. The resin composition according to any one of claims 1 to 8, wherein the polyimide resin is soluble in methylene chloride.

10. The solubility parameter of the polyimide is 8.10 to 9.10 (cal / cm 3 ) 1/2 The resin composition according to any one of claims 1 to 9.

11. A film comprising the resin composition according to any one of claims 1 to 10.

12. 12. The film according to claim 11, having a thickness of 5 μm or more and 300 μm or less, a haze of 3.5% or less, a YI of 5.0 or less, a thickness retardation Rth of 3000 nm or less, and a tensile modulus of elasticity of 3.0 GPa or more.

Citation Information

Patent Citations

  • Carrier for cell adhesion

    JP1986074580A

  • Transparent blend of polyetherimide resin

    JP1998273591A

  • Polyestercarbonate / Polyimide composition

    JP2001240743A

  • Composite porous film, method for manufacturing the same, and prepreg and heat-resistant insulating base material using the same

    JP2001323092A

  • Laminate, and utilization thereof

    JP2012040836A