Thermoplastic elastomer composition and molded article

A thermoplastic elastomer composition with specific hydrogenated copolymers addresses compatibility issues with polypropylene, providing enhanced abrasion resistance and soft feel for durable and comfortable applications.

JP7595456B2Active Publication Date: 2024-12-06ASAHI KASEI KOGYO KABUSHIKI KAISHA
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
JP2020213582
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2020-12-23
Publication Date
2024-12-06
Estimated Expiration
2040-12-23

AI Technical Summary

Technical Problem

Hydrogenated copolymers exhibit poor compatibility with thermoplastic resins like polypropylene, lacking a soft feel and showing poor appearance and compression set (CS), making them unsuitable for applications requiring compatibility with polypropylene, soft feel, abrasion resistance, and processability, such as automobile and medical parts.

Method used

A thermoplastic elastomer composition comprising specific hydrogenated copolymers with defined structures and molecular weights, including hydrogenated copolymers (a), (b), and (c), which are blended in specific ratios to enhance compatibility and balance properties like abrasion resistance and soft feel when mixed with thermoplastic resins.

Benefits of technology

The composition achieves excellent abrasion resistance, a soft feel, and a good balance of properties, making it suitable for applications like automobile interior materials that require high durability and comfort.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007595456000001
    Figure 0007595456000001
  • Figure 0007595456000002
    Figure 0007595456000002
  • Figure 0007595456000003
    Figure 0007595456000003
Patent Text Reader

Abstract

To obtain a thermoplastic elastomer composition capable of having excellent wear resistance, soft touch feeling, and the balance of various characteristics when mixed with a thermoplastic resin and a rubbery polymer.SOLUTION: There is provided a thermoplastic elastomer composition comprising hydrogenated copolymers (a) to (c), wherein (a) has a polymer block A2 having an St content of 25 mass% or more, (b) has a polymer block B1 mainly composed of St and a polymer block B2 mainly composed of a conjugated diene monomer unit, the St content in (b) is 10 to 40 mass%, the vinyl bond amount of the block B2 is 50 to 80 mol%, the Mw of (b) is 350000 or more, (c) has a polymer block C1 mainly composed of St and a polymer block C2 mainly composed of a conjugate diene monomer unit, the vinyl bond amount of the block C2 is less than 50 mol%, the Mw of (c) is 250000 or more and the thermoplastic elastomer composition comprises 1 to 99 pts.mass of (b), 1 to 99 pts.mass of (c) and 5 to 200 pts.mass of (a) based on the total 100 pts.mass of (b) and (c).SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a thermoplastic elastomer composition and a molded article. [Background technology]

[0002] Hydrogenated copolymers of block copolymers using conjugated diene compounds and vinyl aromatic compounds have elasticity similar to that of natural rubber or synthetic rubber at room temperature, and at high temperatures they have moldability similar to that of thermoplastic resins. Furthermore, they have excellent weather resistance and heat resistance. Therefore, they have been widely used as resin modifiers in a wide range of fields, including automobile parts, medical molded products, asphalt modifiers, footwear, molded products such as food containers, packaging materials, adhesive sheets, and home appliance and industrial parts.

[0003] For example, Patent Document 1 discloses a hydrogenated copolymer which is a hydrogenated product of a non-hydrogenated copolymer having a random copolymer structure having conjugated diene monomer units and vinyl aromatic monomer units, and a resin composition containing the hydrogenated copolymer and a thermoplastic resin or a rubber-like polymer. This resin composition has excellent mechanical properties and abrasion resistance, and is therefore used as an alternative material to soft polyvinyl chloride resin. [Prior art documents] [Patent documents]

[0004] [Patent Document 1] International Publication No. 2004 / 003027 Summary of the Invention [Problem to be solved by the invention]

[0005] However, the hydrogenated copolymer disclosed in Patent Document 1 has problems in that it lacks a soft touch due to poor compatibility with thermoplastic resins such as polypropylene, and also has poor appearance and compression set (compression set (C-set), hereinafter sometimes referred to as CS). Therefore, it has a problem in that it is difficult to apply it to applications requiring compatibility with polypropylene, a soft touch, abrasion resistance, processability, and CS, such as automobile parts and medical parts. In the fields of automotive components such as automotive interior skin materials, medical components such as infusion bags and infusion tubes, polyolefin-based adhesive films, and food and clothing packaging, properties required of resin compositions include excellent abrasion resistance, soft touch, good processability, CS, and a good balance of each property, but resin and thermoplastic elastomer compositions that satisfy all of these properties have not yet been obtained. In particular, in applications such as automotive interior materials, there is a demand for improved design, improved tactile feel, and more efficient molding. If the compatibility between the resin materials and the polypropylene resin of the thermoplastic elastomer composition is poor, the final resin composition will have a high hardness, and there is a risk that a soft tactile feel will not be obtained. Therefore, there is a demand for a thermoplastic elastomer composition that can achieve practically sufficient abrasion resistance while also providing a soft feel.

[0006] In view of the above-mentioned problems of the conventional art, the present invention aims to provide a thermoplastic elastomer composition which, when mixed with a thermoplastic resin such as polypropylene or a rubber-like polymer, provides excellent abrasion resistance, a soft touch, and a good balance of each property at a high level. [Means for solving the problem]

[0007] As a result of intensive investigations aimed at solving the above problems, the present inventors have found that a thermoplastic elastomer composition containing specific amounts of hydrogenated copolymers (a) to (c) having specific structures can solve the above problems of the conventional techniques, and have thus completed the present invention. That is, the present invention is as follows.

[0008] [1] Hydrogenated copolymers obtained by hydrogenating polymers containing vinyl aromatic monomer units and conjugated diene monomer units. A thermoplastic elastomer comprising the copolymer (a), the hydrogenated copolymer (b) and the hydrogenated copolymer (c). 1. A composition comprising: The hydrogenated copolymer (a) contains vinyl aromatic monomer units and conjugated diene monomer units. and has a polymer block A2 having a vinyl aromatic monomer unit content of 25% by mass or more; The hydrogenated copolymer (b) contains vinyl aromatic monomer units. Contains 80% or more by mass Polymer block B1 and conjugated diene monomer unit Contains 80% or more by mass and a polymer block B2, The content of vinyl aromatic monomer units in the hydrogenated copolymer (b) is 10 to 40 mass %, the amount of vinyl bonds in the polymer block B2 before hydrogenation is 50 to 80 mol %, The weight average molecular weight of the hydrogenated copolymer (b) is 350,000 or more; The hydrogenated copolymer (c) contains vinyl aromatic monomer units. Contains 80% or more by mass Polymer block C1 and conjugated diene monomer unit Contains 80% or more by mass and a polymer block C2, the amount of vinyl bonds in the polymer block C2 before hydrogenation is less than 50 mol %, The weight average molecular weight of the hydrogenated copolymer (c) is 250,000 or more; Relative to a total of 100 parts by mass of the hydrogenated copolymer (b) and the hydrogenated copolymer (c), 1 to 99 parts by mass of the hydrogenated copolymer (b); 1 to 99 parts by mass of the hydrogenated copolymer (c); 5 to 200 parts by mass of the hydrogenated copolymer (a); A thermoplastic elastomer composition comprising: [2] The content of vinyl aromatic monomer units in the hydrogenated copolymer (b) is 10 to 29 mass %. The thermoplastic elastomer composition according to [1] above. [3] A molded article of the thermoplastic elastomer composition according to [1] or [2] above. Effect of the Invention

[0009] According to the present invention, a thermoplastic elastomer composition can be obtained which, when mixed with a thermoplastic resin such as polypropylene or a rubber-like polymer, exhibits a good balance of abrasion resistance, soft touch, and other properties. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0010] Hereinafter, an embodiment for carrying out the present invention (hereinafter, simply referred to as "the present embodiment") will be described in detail. Note that the following embodiment is an example for explaining the present invention, and the present invention is not limited to the following content, and can be carried out in various modifications within the scope of the gist of the present invention.

[0011] [Thermoplastic elastomer composition] The thermoplastic elastomer composition of the present embodiment includes a hydrogenated copolymer (a), a hydrogenated copolymer (b), and a hydrogenated copolymer (c) obtained by hydrogenating a polymer containing a vinyl aromatic monomer unit and a conjugated diene monomer unit, The hydrogenated copolymer (a) has a polymer block A2 which contains a vinyl aromatic monomer unit and a conjugated diene monomer unit and has a content of the vinyl aromatic monomer unit of 25 mass% or more, The hydrogenated copolymer (b) has a polymer block B1 mainly composed of vinyl aromatic monomer units and a polymer block B2 mainly composed of conjugated diene monomer units, The content of vinyl aromatic monomer units in the hydrogenated copolymer (b) is 10 to 40 mass %, the amount of vinyl bonds in the polymer block B2 before hydrogenation is 50 to 80 mol %, The weight average molecular weight of the hydrogenated copolymer (b) is 350,000 or more; The hydrogenated copolymer (c) has a polymer block C1 mainly composed of vinyl aromatic monomer units and a polymer block C2 mainly composed of conjugated diene monomer units, the amount of vinyl bonds in the polymer block C2 before hydrogenation is less than 50 mol %, The weight average molecular weight of the hydrogenated copolymer (c) is 250,000 or more; Relative to a total of 100 parts by mass of the hydrogenated copolymer (b) and the hydrogenated copolymer (c), 1 to 99 parts by mass of the hydrogenated copolymer (b); 1 to 99 parts by mass of the hydrogenated copolymer (c); 5 to 200 parts by mass of the hydrogenated copolymer (a); Contains. Because the thermoplastic elastomer composition of the present embodiment has the above-described configuration, when it is mixed with a thermoplastic resin such as polypropylene or a rubber-like polymer, it has a good balance of abrasion resistance, soft touch, and other properties. Each component will be described in detail below.

[0012] In this specification, with regard to a monomer unit constituting a polymer block, the term "mainly composed of" means that the target monomer unit is contained in the target polymer block in an amount of 80% by mass or more and 100% by mass or less, and preferably 90% by mass or more and 100% by mass or less.

[0013] (vinyl aromatic compounds) Examples of vinyl aromatic compounds used to form the vinyl aromatic monomer units constituting the hydrogenated copolymers (a) to (c) include, but are not limited to, styrene, α-methylstyrene, p-methylstyrene, divinylbenzene, 1,1-diphenylethylene, N,N-dimethyl-p-aminoethylstyrene, and N,N-diethyl-p-aminoethylstyrene. Among these, styrene, α-methylstyrene, and 4-methylstyrene are preferred from the viewpoints of availability and productivity. From the viewpoint of reactivity, the vinyl aromatic monomer unit contained in a block containing a vinyl aromatic monomer unit and a conjugated diene monomer unit (so-called random block) is preferably styrene. These may be used alone or in combination of two or more.

[0014] (Conjugated diene compounds) The conjugated diene compound used to form the conjugated diene monomer units constituting the hydrogenated copolymers (a) to (c) is not particularly limited as long as it is a diolefin having a conjugated double bond, and examples thereof include 1,3-butadiene, 2-methyl-1,3-butadiene (isoprene), 2,3-dimethyl-1,3-butadiene, 1,3-pentadiene, 2-methyl-1,3-pentadiene, and 1,3-hexadiene. Among these, 1,3-butadiene and isoprene are preferred from the viewpoints of availability and productivity. These may be used alone or in combination of two or more.

[0015] (Hydrogenation rate) In the hydrogenated copolymer (a), the hydrogenated copolymer (b), and the hydrogenated copolymer (c) contained in the thermoplastic elastomer composition of the present embodiment, 70 mol % or more of the total conjugated diene compounds are preferably hydrogenated. Since the hydrogenation rate also affects the solubility parameter value, fluidity, and glass transition temperature of the copolymer, a preferable hydrogenation rate is set taking into consideration the effects on these. That is, the hydrogenation rate of all conjugated diene monomer units of the hydrogenated copolymer (a), the hydrogenated copolymer (b), and the hydrogenated copolymer (c) (hydrogenation rate of carbon-carbon double bonds derived from conjugated diene units) is preferably 70 mol% or more, more preferably 85 mol% or more, and even more preferably 95 mol%, with no particular upper limit. When the hydrogenation rates of the hydrogenated copolymers (a) to (c) are 70 mol % or more, the solubility parameter values ​​of the thermoplastic elastomer composition of the present embodiment and polypropylene become closer to each other, resulting in good dispersion. In addition, the blocking resistance of the thermoplastic elastomer composition also becomes good, resulting in improved abrasion resistance, processability, and soft touch. The hydrogenation rate can be controlled, for example, by adjusting the amount of catalyst used during hydrogenation, and the hydrogenation rate can be controlled, for example, by the amount of catalyst used during hydrogenation, the amount of hydrogen fed, the pressure, and the temperature, etc. This hydrogenation rate can be measured by a proton nuclear magnetic resonance (1H-NMR) method.

[0016] (Hydrogenated copolymer (a)) The thermoplastic elastomer composition of the present embodiment contains the hydrogenated copolymer (a). The hydrogenated copolymer (a) contains a vinyl aromatic monomer unit and a conjugated diene monomer unit, and has a polymer block A2 (hereinafter referred to as polymer block A2) in which the content of the vinyl aromatic monomer unit is 25 mass% or more. Furthermore, the hydrogenated copolymer (a) preferably has at least one block mainly composed of a vinyl aromatic compound (hereinafter, sometimes referred to as polymer block A1). The hydrogenated copolymer (a) preferably has a structure represented by the following general formula, for example. The hydrogenated copolymer (a) may be a mixture containing a plurality of types of the following structures in any ratio.

[0017] (A1-A2) n A1-(A2-A1) n A2-(A1-A2) n [(A1-A2) n ] m -Z [(A2-A1) n ] m -Z [(A1-A2) n -A1] m -Z [(A2-A1)n -A2] m -Z

[0018] In each of the general formulae representing the hydrogenated copolymer (a) described above, A1 is a polymer block mainly composed of vinyl aromatic monomer units, and A2 is a polymer block containing vinyl aromatic monomer units and conjugated diene monomer units and having a vinyl aromatic monomer unit content of 25 mass% or more.

[0019] The polymer block A2 contains a vinyl aromatic monomer unit and a conjugated diene monomer unit, and the content of the vinyl aromatic monomer unit is preferably 25% by mass or more and 25 to less than 80% by mass. This allows the polymer block A1 and the polymer block A2 to be clearly distinguished. The boundary between the polymer block A1 and the polymer block A2 does not necessarily have to be clearly distinguished.

[0020] In each formula representing the hydrogenated copolymer (a), n is an integer of 1 or more, and preferably an integer of 1-5. m is an integer of 2 or more, preferably an integer of 2 to 12, and more preferably an integer of 2 to 8. Z represents a residue of a coupling agent. The coupling agent is not limited to the following, but examples thereof include polyhalogen compounds and acid esters described below.

[0021] When the polymer block A1 is a copolymer of vinyl aromatic monomer units and other monomer units, the vinyl aromatic monomer units in the polymer block A1 may be distributed uniformly or tapered, and there may be a plurality of uniformly distributed portions and / or a plurality of tapered portions. Furthermore, the polymer block A1 may have a plurality of portions with different contents of vinyl aromatic monomer units. The vinyl aromatic monomer units in the polymer block A2 may be distributed uniformly or in a tapered shape. The vinyl aromatic monomer units may have a plurality of uniformly distributed portions and / or a plurality of taperedly distributed portions. The polymer block A2 may have a plurality of portions with different contents of the vinyl aromatic monomer units.

[0022] <Total vinyl aromatic compound content> The content of all vinyl aromatic monomer units in the hydrogenated copolymer (a) is preferably from 30 to 90% by mass, more preferably from 35 to 80% by mass, and further preferably from 40 to 70% by mass. The content of the conjugated diene monomer unit in the hydrogenated copolymer (a) is preferably from 10% by mass to 70% by mass, more preferably from 20% by mass to 65% by mass, and further preferably from 30% by mass to 60% by mass. By making the total vinyl aromatic compound content in the hydrogenated copolymer (a) 30% by mass or more, the thermoplastic elastomer composition of the present embodiment tends to have excellent abrasion resistance.By making the total vinyl aromatic monomer unit content 90% by mass or less, the thermoplastic elastomer composition of the present embodiment tends to have excellent soft touch, CS, and appearance. The total content of vinyl aromatic monomer units can be calculated by measuring the absorption intensity at 262 nm using an ultraviolet spectrophotometer according to the method described in the Examples below.

[0023] <Content of vinyl aromatic monomer unit in polymer block A2> The content of the vinyl aromatic monomer unit in the polymer block A2 in the hydrogenated copolymer (a) is 25% by mass or more, and preferably from 25 to less than 80% by mass. The upper limit of the content is more preferably 75% by mass, and even more preferably 70% by mass. The lower limit of the content is preferably 30% by mass, more preferably 35% by mass, and even more preferably 40% by mass. When the content of vinyl aromatic monomer units in the polymer block A2 in the hydrogenated copolymer (a) is 25 mass% or more, the effect of providing a composition of the thermoplastic elastomer composition of the present embodiment with a polypropylene resin or a rubber-like polymer having excellent abrasion resistance can be obtained. When the content of the vinyl aromatic compound is 80% by mass or less, the thermoplastic elastomer composition has the effect of exhibiting a soft touch, excellent CS, appearance and low-temperature mechanical properties. The content of the vinyl aromatic monomer unit in the polymer block A2 can be controlled within the above-mentioned numerical range by adjusting the amount of the vinyl aromatic compound fed during polymerization, and can be measured by a nuclear magnetic resonance (NMR) spectrometer.

[0024] <Content of Polymer Block A1> In the hydrogenated copolymer (a), the content of the polymer block A1 mainly composed of the vinyl aromatic monomer unit is preferably 1 mass % to 40 mass %, more preferably 5 mass % to 35 mass %, and further preferably 10 mass % to 30 mass %, based on the total mass of the hydrogenated copolymer (a). When the content of the polymer block A1 in the hydrogenated copolymer (a) is 1% by mass or more, the thermoplastic elastomer composition of the present embodiment tends to be excellent in abrasion resistance, CS, and low stickiness. When the content of the block polymer A1 is 40% by mass or less, the thermoplastic elastomer composition of the present embodiment tends to have excellent soft touch. The content of the polymer block A1 can be controlled by adjusting the amount of the monomer fed.

[0025] The content of polymer block A1 in the hydrogenated copolymer (a) can be calculated using the mass of a polymer mainly composed of vinyl aromatic monomer units (however, vinyl aromatic compounds having an average degree of polymerization of about 30 or less are excluded) determined by a method of oxidatively decomposing the unhydrogenated copolymer (a') with t-butyl hydroperoxide using osmium tetroxide as a catalyst (the method described in I. M. KOLTHOFF, et al., Polym. Sci. 1, 429 (1946)) (hereinafter referred to as the osmium tetroxide decomposition method).

[0026] The content of the polymer block A1 in the hydrogenated copolymer (a) can be measured by a nuclear magnetic resonance (NMR) spectrometer using the copolymer after hydrogenation (hydrogenated copolymer (a)) according to the method described in Y. Tanaka, et al., RUBBER CHEMISTRY and TECHNOLOGY 54, 685 (1981). The NMR method will be specifically explained by taking as an example a case where the vinyl aromatic compound is styrene and the conjugated diene compound is 1,3-butadiene. A sample of 30 mg of hydrogenated copolymer (a) dissolved in 1 g of deuterated chloroform was used. 1 1 H-NMR was measured, and the content (Ns value) of polymer block A1 (polystyrene block in this case) was calculated from the ratio of the integrated value of chemical shifts from 6.9 ppm to 6.3 ppm to the total integrated value. Block styrene strength (b-St strength) = (integrated value of 6.9 ppm to 6.3 ppm) / 2 Random styrene strength (r-St strength) = (integrated value of 7.5 ppm to 6.9 ppm) - 3 × (b-St) Ethylene-butylene strength (EB strength) = Total integrated value - 3 x {(b-St intensity) + (r-St intensity)} / 8 Polystyrene block content (Ns value) obtained by NMR method =104×(b-St strength) / [104×{(b-St strength)+(r-St strength)}+56×(EB strength)] Here, there is a correlation represented by the following formula between the content of block polymer A in copolymer (a') before hydrogenation measured by the osmium tetroxide decomposition method (referred to as the "Os value") and the content of block polymer A1 in hydrogenated copolymer (a) after hydrogenation measured by the NMR method (referred to as the "Ns value"). Os value = -0.012 (Ns value)2 + 1.8 (Ns value) -13.0

[0027] <Vinyl bond content> The amount of vinyl bonds in the conjugated diene monomer units in the hydrogenated copolymer (a) before hydrogenation is preferably from 1 mol % to 39 mol %, more preferably from 5 mol % to 38 mol %, and further preferably from 10 mol % to 37 mol %. Since the amount of vinyl bonds in the hydrogenated copolymer (a) before hydrogenation is 1 mol% or more, the compatibility between the hydrogenated copolymer (a) and the polypropylene resin in the thermoplastic elastomer composition of the present embodiment is excellent. In addition, the thermoplastic elastomer composition of the present embodiment tends to have a soft touch, excellent CS and excellent appearance. The vinyl bond portion before hydrogenation becomes ethylene bonded to the main chain after hydrogenation. Since this structure is similar to that of polypropylene in which methyl is bonded to the main chain as a side chain, it is considered that the greater the amount of vinyl bonds before hydrogenation, the greater the compatibility between the two and the closer the solubility parameter values ​​become. Since the amount of vinyl bonds before hydrogenation is 39 mol % or less, the thermoplastic elastomer composition of the present embodiment tends to have excellent abrasion resistance. In the present embodiment, the vinyl bond content refers to the total content of 1,2-vinyl bonds (conjugated dienes incorporated into the polymer via 1,2-bonds) and 3,4-vinyl bonds (conjugated dienes incorporated into the polymer via 3,4-bonds) relative to the total conjugated dienes (here, when 1,3-butadiene is used as the conjugated diene, the 1,2-vinyl bond content, and when isoprene is used as the conjugated diene, the 3,4-vinyl bond content). The vinyl bond content based on the conjugated diene before hydrogenation can be measured using a nuclear magnetic resonance (NMR) spectrometer. The microstructure (ratio of cis, trans, and vinyl) derived from the conjugated diene compound monomer unit in the hydrogenated copolymer (a) can be controlled by using a polar compound, etc., which will be described later.

[0028] <Weight average molecular weight> The weight average molecular weight of the hydrogenated copolymer (a) is preferably from 100,000 to 800,000, more preferably from 120,000 to 500,000, and further preferably from 140,000 to 400,000. When the weight average molecular weight of the hydrogenated copolymer (a) is 100,000 or more, the thermoplastic elastomer composition of the present embodiment tends to be excellent in abrasion resistance and CS. When the weight average molecular weight of the hydrogenated copolymer (a) is 800,000 or less, flowability enabling molding process and molded appearance tend to be good. The weight average molecular weight of the hydrogenated copolymer (a) can be determined by using the molecular weight of a peak in a chromatogram measured by gel permeation chromatography (GPC) according to the method described in the Examples below, and a calibration curve (created using the peak molecular weight of the standard polystyrene) obtained by measuring commercially available standard polystyrene.

[0029] The shape of the molecular weight distribution of the hydrogenated copolymer (a) measured by GPC is not particularly limited, and the molecular weight distribution may be a polymodal molecular weight distribution having two or more peaks, or a monomodal molecular weight distribution having one peak. The weight average molecular weight of the hydrogenated copolymer (a) can be controlled by adjusting the amount of monomer added during the polymerization step, the amount of reaction initiator added, the polymerization time, and the polymerization temperature. The melt flow rate (MFR; in accordance with ISO 1133) of the hydrogenated copolymer (a) is preferably in the range of 0.01 to 200 g / 10 min, more preferably 0.1 to 150 g / 10 min, and even more preferably 1.0 to 100 g / 10 min. When the hydrogenated copolymer (a) has an MFR of 0.01 g / 10 min or more, the flowability of the thermoplastic elastomer composition of the present embodiment tends to be sufficiently ensured, and when it is 200 g / 10 min or less, the low stickiness of the thermoplastic elastomer composition of the present embodiment tends to be sufficiently ensured.

[0030] (Hydrogenated copolymer (b)) The thermoplastic elastomer composition of the present embodiment contains the hydrogenated copolymer (b). The hydrogenated copolymer (b) has at least one polymer block B1 mainly composed of vinyl aromatic monomer units and at least one polymer block B2 mainly composed of conjugated diene monomer units. The hydrogenated copolymer (b) preferably has a structure represented by the following general formula, for example: The hydrogenated copolymer (b) may be a mixture containing a plurality of the following structures in any ratio.

[0031] (B1-B2) n B1-(B2-B1) n B2-(B1-B2) n [(B1-B2) n ] m -Z [(B2-B1) n ] m -Z [(B1-B2) n -B1] m -Z [(B2-B1) n -B2] m -Z

[0032] In each of the general formulae representing the hydrogenated copolymer (b), B1 is a polymer block mainly composed of vinyl aromatic monomer units, and B2 is a polymer block mainly composed of conjugated diene monomer units, so that the polymer block B1 and the polymer block B2 are clearly distinguished from each other. The boundary between the polymer block B1 and the polymer block B2 does not necessarily have to be clearly distinguished.

[0033] In the above formula, n is an integer of 1 or more, and preferably an integer of 1 to 5. m is an integer of 2 or more, preferably an integer of 2 to 12, and more preferably an integer of 2 to 8. Z represents a residue of a coupling agent. The coupling agent is not limited to the following, but examples thereof include polyhalogen compounds and acid esters described below.

[0034] The hydrogenated copolymer (b) preferably has a structure obtained by hydrogenating a coupling polymer represented by the following formula (1). [(B1-B2) n ] m -Z (1) (In formula (1), B1 is a polymer block mainly composed of vinyl aromatic monomer units, B2 is a polymer block mainly composed of conjugated diene monomer units, n is 1, m is an integer of 1 or more, and Z is a residue of a coupling agent or a residue of a polymerization initiator.) The hydrogenated copolymer (b) having such a structure can be obtained, for example, by polymerizing the polymer block B1 and the polymer block B2 in this order, coupling them, and hydrogenating the coupling polymer.

[0035] In the hydrogenated copolymer (b), the proportion of the two-branched component, which corresponds to m=2 in the above formula (1), is preferably 10% by mass to 30% by mass, more preferably 10% by mass to 20% by mass, and further preferably 12% by mass to 18% by mass, of the entire hydrogenated copolymer (b). In the hydrogenated copolymer (b), the proportion of the 3-branched component, which corresponds to m=3 in the above formula (1), is preferably 40% by mass to 70% by mass, more preferably 45% by mass to 65% by mass, and further preferably 50% by mass to 60% by mass of the entire hydrogenated copolymer (b). In the hydrogenated copolymer (b), the ratio of the 3-branched component to the 2-branched component (mass of the 3-branched component / mass of the 2-branched component) is preferably 2 or more, more preferably 2-7, and further preferably 2-6. By setting the ratio of each component of the hydrogenated copolymer (b) within the above range, the thermoplastic elastomer composition of the present embodiment tends to be excellent in abrasion resistance and appearance.

[0036] <Contents of Polymer Block B1 and Polymer Block B2> In the hydrogenated copolymer (b), the content of the polymer block B1 mainly composed of the vinyl aromatic monomer unit is preferably 10 mass% to 40 mass%, more preferably 10 mass% to 35 mass%, and further preferably 10 mass% to 29 mass%, based on the mass of the hydrogenated copolymer (b). When the content of the polymer block B1 in the hydrogenated copolymer (b) is 10% by mass or more, the thermoplastic elastomer composition of the present embodiment tends to be excellent in abrasion resistance and CS. When the content of the block polymer B1 is 40% by mass or less, the thermoplastic elastomer composition of the present embodiment tends to have a soft feel and excellent appearance. The contents of the polymer block B1 and the polymer block B2 can be controlled by adjusting the amounts of the monomers fed.

[0037] In the hydrogenated copolymer (b), the content of the polymer block B2 mainly composed of the conjugated diene monomer units is preferably 60 mass% to 90 mass%, more preferably 65 mass% to 90 mass%, and further preferably 71 mass% to 90 mass%, based on the mass of the hydrogenated copolymer (b).

[0038] The content of polymer block B1 in the hydrogenated copolymer (b) can be calculated using the mass of a polymer mainly composed of vinyl aromatic monomer units (however, vinyl aromatic compounds having an average degree of polymerization of about 30 or less are excluded) determined by a method of oxidatively decomposing the unhydrogenated copolymer (b') with t-butyl hydroperoxide using osmium tetroxide as a catalyst (the method described in I. M. KOLTHOFF, et al., Polym. Sci. 1, 429 (1946)) (hereinafter referred to as the osmium tetroxide decomposition method).

[0039] The content of the polymer block B1 in the hydrogenated copolymer (b) can be measured by a nuclear magnetic resonance (NMR) apparatus using the copolymer after hydrogenation (hydrogenated copolymer (b)) according to the method described in Y. Tanaka, et al., RUBBER CHEMISTRY and TECHNOLOGY 54, 685 (1981). The NMR method will be specifically explained by taking as an example a case where the vinyl aromatic compound is styrene and the conjugated diene compound is 1,3-butadiene. 30 mg of the hydrogenated copolymer (b) was dissolved in 1 g of deuterated chloroform and the 1H-NMR was measured to determine the content (Ns value) of the polymer block B1 (in this case, the polystyrene block) from the ratio of the integrated value of the chemical shift from 6.9 ppm to 6.3 ppm to the total integrated value. Block styrene strength (b-St strength) = (integrated value of 6.9 ppm to 6.3 ppm) / 2 Random styrene strength (r-St strength) = (integrated value of 7.5 ppm to 6.9 ppm) - 3 × (b-St) Ethylene-butylene strength (EB strength) = Total integrated value - 3 x {(b-St intensity) + (r-St intensity)} / 8 Polystyrene block content (Ns value) obtained by NMR method =104×(b-St strength) / [104×{(b-St strength)+(r-St strength)}+56×(EB strength)] Here, there is a correlation represented by the following formula between the content of block polymer B1 in copolymer (b') before hydrogenation measured by the osmium tetroxide decomposition method (referred to as the "Os value") and the content of block polymer B1 in hydrogenated copolymer (b) after hydrogenation measured by the NMR method (referred to as the "Ns value"). Os value = -0.012 (Ns value)2 + 1.8 (Ns value) -13.0

[0040] <Content of vinyl aromatic monomer units in hydrogenated copolymer (b)> The content of all vinyl aromatic monomer units in the hydrogenated copolymer (b) is from 10 to 40 mass %, preferably from 10 to 29 mass %, and more preferably from 10 to 25 mass %. The thermoplastic elastomer composition of the present embodiment tends to have excellent abrasion resistance and CS when the total content of vinyl aromatic monomer units in the hydrogenated copolymer (b) is 10% by mass or more. The thermoplastic elastomer composition of the present embodiment tends to have excellent soft touch and appearance when the total content of vinyl aromatic monomer units in the hydrogenated copolymer (b) is 40% by mass or less. The total content of vinyl aromatic compounds can be calculated by measuring the absorption intensity at 262 nm using an ultraviolet spectrophotometer.

[0041] <Vinyl bond content> The vinyl bond amount of the polymer block B2 of the hydrogenated copolymer (b) before hydrogenation is 50 mol % to 80 mol %, preferably 52 mol % to 77 mol %, and more preferably 55 mol % to 75 mol %. When the polymer block B2 of the hydrogenated copolymer (b) has a vinyl bond amount of 50 mol % or more before hydrogenation, the thermoplastic elastomer composition of this embodiment has excellent compatibility between the hydrogenated copolymer and the polypropylene resin, and the thermoplastic elastomer composition of this embodiment tends to have a soft feel, excellent appearance and excellent CS. The vinyl bond portion before hydrogenation becomes ethylene bonded to the main chain after hydrogenation. Since this structure is similar to that of polypropylene in which methyl is bonded to the main chain as a side chain, it is considered that the greater the amount of vinyl bonds before hydrogenation, the greater the compatibility between the two and the closer the solubility parameter values ​​become.

[0042] In addition, since the vinyl bond amount in the polymer block B2 of the hydrogenated copolymer (b) before hydrogenation is 80 mol % or less, the thermoplastic elastomer composition of the present embodiment tends to have excellent abrasion resistance.

[0043] In the present embodiment, the vinyl bond content refers to the total content of 1,2-vinyl bonds (conjugated dienes incorporated into the polymer via 1,2-bonds) and 3,4-vinyl bonds (conjugated dienes incorporated into the polymer via 3,4-bonds) relative to the total conjugated dienes (here, when 1,3-butadiene is used as the conjugated diene, the 1,2-vinyl bond content, and when isoprene is used as the conjugated diene, the 3,4-vinyl bond content).

[0044] The vinyl bond content before hydrogenation of the polymer block B2 of the hydrogenated copolymer (b) can be measured by using a nuclear magnetic resonance (NMR) apparatus. The microstructure (ratio of cis, trans, vinyl) derived from the conjugated diene compound monomer units in the hydrogenated copolymer (b) can be controlled within a predetermined numerical range by using a polar compound described later and adjusting the amount of the polar compound added.

[0045] <Weight average molecular weight> The weight average molecular weight of the hydrogenated copolymer (b) is 350,000 or more, preferably 350,000 to 500,000, more preferably 370,000 to 470,000, and further preferably 400,000 to 500,000. When the weight average molecular weight of the hydrogenated copolymer (b) is 350,000 or more, the thermoplastic elastomer composition of the present embodiment tends to be excellent in abrasion resistance and CS.

[0046] The weight average molecular weight of the hydrogenated copolymer (b) can be determined by using the molecular weight of a peak in a chromatogram measured by gel permeation chromatography (GPC) according to the method described in the Examples below, and a calibration curve (created using the peak molecular weight of the standard polystyrene) obtained by measuring commercially available standard polystyrene. The shape of the molecular weight distribution of the hydrogenated copolymer (b) measured by GPC is not particularly limited, and the molecular weight distribution may be a polymodal molecular weight distribution having two or more peaks, or a monomodal molecular weight distribution having one peak.

[0047] The weight average molecular weight of the hydrogenated copolymer (b) can be controlled by adjusting the amount of monomer added during the polymerization step, the amount of reaction initiator added, the polymerization time, and the polymerization temperature.

[0048] (Hydrogenated copolymer (c)) The thermoplastic elastomer composition of the present embodiment contains the hydrogenated copolymer (c). The hydrogenated copolymer (c) has at least one polymer block C1 mainly composed of vinyl aromatic monomer units and at least one polymer block C2 mainly composed of conjugated diene monomer units. The hydrogenated copolymer (c) preferably has a structure represented by the following general formula, for example: The hydrogenated copolymer (c) may be a mixture containing a plurality of the following structures in any ratio.

[0049] (C1-C2) n C1-(C2-C1) n C2-(C1-C2) n [(C1-C2) n ] m -Z [(C2-C1) n ] m -Z [(C1-C2) n -C1] m -Z [(C2-C1) n -C2] m-Z

[0050] In each general formula representing the hydrogenated copolymer (c), C1 is a polymer block mainly composed of vinyl aromatic monomer units, and C2 is a polymer block mainly composed of conjugated diene monomer units. This allows the polymer block C1 and the polymer block C2 to be clearly distinguished. The boundary between the polymer block C1 and the polymer block C2 does not necessarily need to be clearly distinguished. Furthermore, n is an integer of 1 or more, and preferably an integer of 1-5. m is an integer of 2 or more, preferably an integer of 2 to 12, and more preferably an integer of 2 to 8. Z represents a residue of a coupling agent. The coupling agent is not limited to the following, but examples thereof include polyhalogen compounds and acid esters described below.

[0051] <Contents of Polymer Block C1 and Polymer Block C2> In the hydrogenated copolymer (c), the content of the polymer block C1 mainly composed of the vinyl aromatic monomer unit is preferably 10 mass% to 40 mass%, more preferably 20 mass% to 40 mass%, and further preferably 30 mass% to 40 mass%, based on the mass of the hydrogenated copolymer (c). When the content of the polymer block C1 in the hydrogenated copolymer (c) is 10% by mass or more, the thermoplastic elastomer composition of the present embodiment tends to have excellent CS. When the content of the block polymer C1 in the hydrogenated copolymer (c) is 40% by mass or less, the thermoplastic elastomer composition of the present embodiment tends to have excellent soft touch. The contents of the polymer block C1 and the polymer block C2 can be controlled by adjusting the amounts of the monomers fed.

[0052] In the hydrogenated copolymer (c), the content of the polymer block C2 mainly composed of the conjugated diene monomer units is preferably 60 mass% to 90 mass%, more preferably 60 mass% to 80 mass%, and further preferably 60 mass% to 70 mass%, based on the mass of the hydrogenated copolymer (c).

[0053] The content of polymer block C1 in the hydrogenated copolymer (c) can be calculated using the mass of a polymer mainly composed of vinyl aromatic monomer units (however, vinyl aromatic compounds having an average degree of polymerization of about 30 or less are excluded) determined by a method of oxidatively decomposing the unhydrogenated copolymer (c') with t-butyl hydroperoxide using osmium tetroxide as a catalyst (the method described in I. M. KOLTHOFF, et al., Polym. Sci. 1, 429 (1946)) (hereinafter referred to as the osmium tetroxide decomposition method).

[0054] The content of the polymer block C1 in the hydrogenated copolymer (c) can be measured by a nuclear magnetic resonance (NMR) apparatus using the copolymer after hydrogenation (hydrogenated copolymer (c)) according to the method described in Y. Tanaka, et al., RUBBER CHEMISTRY and TECHNOLOGY 54, 685 (1981). The NMR method will be specifically explained by taking as an example a case where the vinyl aromatic compound is styrene and the conjugated diene compound is 1,3-butadiene. 30 mg of the hydrogenated copolymer (c) was dissolved in 1 g of deuterated chloroform and the 1H-NMR was measured to determine the content (Ns value) of the polymer block C1 (in this case, the polystyrene block) from the total integrated value of the chemical shift of 6.9 ppm to 6.3 ppm. Block styrene strength (b-St strength) = (integrated value of 6.9 ppm to 6.3 ppm) / 2 Random styrene strength (r-St strength) = (integrated value of 7.5 ppm to 6.9 ppm) - 3 × (b-St) Ethylene-butylene strength (EB strength) = Total integrated value - 3 x {(b-St intensity) + (r-St intensity)} / 8 Polystyrene block content (Ns value) obtained by NMR method =104×(b-St strength) / [104×{(b-St strength)+(r-St strength)}+56×(EB strength)] Here, there is a correlation represented by the following formula between the content of block polymer C1 in copolymer (b') before hydrogenation measured by the osmium tetroxide decomposition method (referred to as the "Os value") and the content of block polymer C1 in hydrogenated copolymer (c) after hydrogenation measured by the NMR method (referred to as the "Ns value"). Os value = -0.012 (Ns value)2 + 1.8 (Ns value) -13.0

[0055] <Vinyl bond content> The vinyl bond amount of the polymer block C2 in the hydrogenated copolymer (c) before hydrogenation is less than 50 mol %, preferably less than 45 mol %, more preferably less than 40 mol %. The vinyl bond amount of the polymer block C2 in the hydrogenated copolymer (c) before hydrogenation is preferably 15 mol % or more, more preferably 18 mol % or more, and further preferably 20 mol % or more.

[0056] Since the amount of vinyl bonds in the polymer block C2 in the hydrogenated copolymer (c) before hydrogenation is less than 50 mol %, the thermoplastic elastomer composition of the present embodiment tends to have excellent CS. When the vinyl bond amount of the polymer block C2 in the hydrogenated copolymer (c) before hydrogenation is 15 mol % or more, the elastomer composition using the hydrogenated copolymer of this embodiment tends to have excellent abrasion resistance and appearance.

[0057] In the present embodiment, the vinyl bond content refers to the total content of 1,2-vinyl bonds (conjugated dienes incorporated into the polymer via 1,2-bonds) and 3,4-vinyl bonds (conjugated dienes incorporated into the polymer via 3,4-bonds) relative to the total conjugated dienes (here, when 1,3-butadiene is used as the conjugated diene, the 1,2-vinyl bond content, and when isoprene is used as the conjugated diene, the 3,4-vinyl bond content). The vinyl bond content based on the conjugated diene before hydrogenation can be measured using a nuclear magnetic resonance (NMR) spectrometer. The microstructure (ratio of cis, trans, and vinyl) derived from the conjugated diene compound monomer unit in the hydrogenated copolymer (c) can be controlled by using a polar compound, etc., described later, and adjusting the amount of the polar compound.

[0058] <Weight average molecular weight> The weight average molecular weight of the hydrogenated copolymer (c) is 250,000 or more, preferably 250,000 to 500,000, more preferably 250,000 to 450,000, and further preferably 250,000 to less than 400,000. When the weight average molecular weight of the hydrogenated copolymer (c) is 250,000 or more, the thermoplastic elastomer composition of the present embodiment tends to have excellent CS. The weight average molecular weight of the hydrogenated copolymer (c) can be determined by using the molecular weight of a peak in a chromatogram measured by gel permeation chromatography (GPC) according to the method described in the Examples below, and a calibration curve (created using the peak molecular weight of the standard polystyrene) obtained by measuring commercially available standard polystyrene. The shape of the molecular weight distribution of the hydrogenated copolymer (c) measured by GPC is not particularly limited, and the molecular weight distribution may be a polymodal molecular weight distribution having two or more peaks, or a monomodal molecular weight distribution having one peak. The weight average molecular weight of the hydrogenated copolymer (c) depends on the amount of monomer added during the polymerization process, the amount of reaction initiator, It can be controlled by adjusting the amount added, the polymerization time and the polymerization temperature.

[0059] (Mass ratio of hydrogenated copolymer (a), hydrogenated copolymer (b), and hydrogenated copolymer (c)) The thermoplastic elastomer composition of the present embodiment contains 1 to 99 parts by mass of the hydrogenated copolymer (b), 1 to 99 parts by mass of the hydrogenated copolymer (c), and 5 to 200 parts by mass of the hydrogenated copolymer (a) relative to 100 parts by mass in total of the hydrogenated copolymer (b) and the hydrogenated copolymer (c). The mass ratio (b) / (c) of the hydrogenated copolymer (b) to the hydrogenated copolymer (c) (wherein the total of (b) and (c) is 100 parts by mass) is from 1 / 99 to 99 / 1, preferably from 10 / 90 to 90 / 10, and more preferably from 20 / 80 to 80 / 20, from the viewpoints of the abrasion resistance, soft touch, and balance of each property of the thermoplastic elastomer composition of this embodiment.

[0060] By including hydrogenated copolymer (b) in the thermoplastic elastomer composition of this embodiment, the thermoplastic elastomer composition of this embodiment has excellent abrasion resistance, soft touch, and appearance. By including hydrogenated copolymer (c), the thermoplastic elastomer composition of this embodiment has excellent CS. Furthermore, by using hydrogenated copolymer (b) and hydrogenated copolymer (c) in combination, the thermoplastic elastomer composition of this embodiment has further improved abrasion resistance, a soft touch, and an excellent balance of other properties (appearance, CS).

[0061] The hydrogenated copolymer (a) is contained in an amount of 5 to 200 parts by mass, preferably 5 to 160 parts by mass, and more preferably 5 to 120 parts by mass, per 100 parts by mass in total of the hydrogenated copolymers (b) and (c), from the viewpoint of improving the abrasion resistance of the thermoplastic elastomer composition of the present embodiment.

[0062] The thermoplastic elastomer composition of the present embodiment has a specific structure and contains the hydrogenated copolymer (a), the hydrogenated copolymer (b), and the hydrogenated copolymer (c) in a specific ratio, and when mixed with a thermoplastic resin such as polypropylene or a rubber-like polymer, the thermoplastic elastomer composition has excellent abrasion resistance and a soft feel, and the respective properties are well balanced.

[0063] The method for producing the thermoplastic elastomer composition of the present embodiment is not particularly limited, but examples thereof include (1) a method in which the hydrogenated copolymer (a), the hydrogenated copolymer (b), and the hydrogenated copolymer (c) are polymerized, respectively, and mixed before being recovered from the production solvent, and (2) a method in which the hydrogenated copolymer (a), the hydrogenated copolymer (b), and the hydrogenated copolymer (c) are mixed after removing the solvent and the catalyst, respectively.

[0064] (Methods for Producing Hydrogenated Copolymer (a), Hydrogenated Copolymer (b), and Hydrogenated Copolymer (c)) Examples of methods for producing the hydrogenated copolymer (a), the hydrogenated copolymer (b), and the hydrogenated copolymer (c) include, but are not limited to, methods described in JP-B-36-19286, JP-B-43-17979, JP-B-46-32415, JP-B-49-36957, JP-B-48-2423, JP-B-48-4106, JP-B-51-49567, and JP-A-59-166518.

[0065] The hydrogenated copolymers (a) to (c) before hydrogenation can be obtained, for example, by a method of carrying out living anionic polymerization using a predetermined monomer in a hydrocarbon solvent using a polymerization initiator such as an organic alkali metal compound, but is not limited thereto.

[0066] The hydrocarbon solvent is not particularly limited, and examples thereof include aliphatic hydrocarbons such as n-butane, isobutane, n-pentane, n-hexane, n-heptane, and n-octane; alicyclic hydrocarbons such as cyclohexane, cycloheptane, and methylcycloheptane; and aromatic hydrocarbons such as benzene, toluene, xylene, and ethylbenzene.

[0067] As the polymerization initiator, an organic alkali metal compound that is generally known to have anionic polymerization activity toward conjugated diene compounds and vinyl aromatic compounds can be used. For example, there may be mentioned an aliphatic hydrocarbon alkali metal compound having 1 to 20 carbon atoms, an aromatic hydrocarbon alkali metal compound having 1 to 20 carbon atoms, an organic amino alkali metal compound having 1 to 20 carbon atoms, and the like. The alkali metal contained in the polymerization initiator is not limited to the following, but examples thereof include lithium, sodium, and potassium. One or more types of alkali metals may be contained in one molecule.

[0068] Examples of the polymerization initiator include, but are not limited to, n-propyllithium, n-butyllithium, sec-butyllithium, tert-butyllithium, n-pentyllithium, n-hexyllithium, benzyllithium, phenyllithium, tolyllithium, a reaction product of diisopropenylbenzene and sec-butyllithium, and a reaction product of divinylbenzene, sec-butyllithium, and a small amount of 1,3-butadiene. Furthermore, 1-(t-butoxy)propyllithium disclosed in U.S. Patent No. 5,708,092 and lithium compounds into which one or several molecules of an isoprene monomer have been inserted to improve the solubility thereof, siloxy group-containing alkyllithiums such as 1-(t-butyldimethylsiloxy)hexyllithium disclosed in British Patent No. 2,241,239, amino group-containing alkyllithiums disclosed in U.S. Patent No. 5,527,753, diisopropylamide lithium, hexamethyldisilazide lithium and other aminolithiums can also be used.

[0069] The amount of the lithium compound used as a polymerization initiator depends on the molecular weight of the target copolymer, but generally can be 0.01 to 0.5 phm (parts by mass per 100 parts by mass of monomer). The amount of the lithium compound used as a polymerization initiator is preferably 0.03 to 0.3 phm, more preferably 0.05 to 0.15 phm.

[0070] When a conjugated diene compound and a vinyl aromatic compound are copolymerized using an organic alkali metal compound as a polymerization initiator, a tertiary amine compound or an ether compound can be added as a vinyl bond amount regulator to adjust the content of vinyl bonds (1,2-bonds or 3,4-bonds) resulting from the conjugated diene compound incorporated in the copolymer and to adjust the random copolymerizability of the conjugated diene compound and the vinyl aromatic compound.

[0071] The tertiary amine compound is not particularly limited, but examples thereof include compounds represented by the following formula: R1R2R3N (In the formula, R1, R2, and R3 are a hydrocarbon group having 1 to 20 carbon atoms or a hydrocarbon group having a tertiary amino group.) Examples of such compounds include, but are not limited to, trimethylamine, triethylamine, tributylamine, N,N-dimethylaniline, N-ethylpiperidine, N-methylpyrrolidine, N,N,N',N'-tetramethylethylenediamine, N,N,N',N'-tetraethylethylenediamine, 1,2-dipiperidinoethane, trimethylaminoethylpiperazine, N,N,N',N'',N''-pentamethylethylenetriamine, N,N'-dioctyl-p-phenylenediamine, etc. Among these, N,N,N',N'-tetramethylethylenediamine is preferred.

[0072] As the ether compound, a linear ether compound or a cyclic ether compound can be used. Examples of the linear ether compound include dialkyl ether compounds of ethylene glycol, such as dimethyl ether, diethyl ether, diphenyl ether, ethylene glycol dimethyl ether, ethylene glycol diethyl ether, and ethylene glycol dibutyl ether; and dialkyl ether compounds of diethylene glycol, such as diethylene glycol dimethyl ether, diethylene glycol diethyl ether, and diethylene glycol dibutyl ether. Examples of cyclic ether compounds include tetrahydrofuran, dioxane, 2,5-dimethyloxolane, 2,2,5,5-tetramethyloxolane, 2,2-bis(2-oxolanyl)propane, and alkyl ethers of furfuryl alcohol.

[0073] The amount of the tertiary amine compound or ether compound used is preferably 0.1 to 4 (mol / mol of alkali metal), more preferably 0.2 to 3 (mol / mol of alkali metal), relative to the amount of the polymerization initiator of the organic alkali metal compound.

[0074] In the process for producing the hydrogenated copolymer (a), the hydrogenated copolymer (b), and the hydrogenated copolymer (c), sodium alkoxide may be present during copolymerization. The sodium alkoxide is, for example, a compound represented by the following formula, but is not limited thereto: In particular, sodium alkoxides having an alkyl group having 3 to 6 carbon atoms are preferred, and sodium t-butoxide and sodium t-pentoxide are more preferred. NaOR (wherein R is an alkyl group having 2 to 12 carbon atoms). The amount of sodium alkoxide used in the polymerization process of the hydrogenated copolymer (a), the hydrogenated copolymer (b), and the hydrogenated copolymer (c) is preferably 0.01 or more and less than 0.1 (molar ratio), more preferably 0.01 or more and less than 0.08 (molar ratio), even more preferably 0.03 or more and less than 0.08 (molar ratio), and still more preferably 0.04 or more and less than 0.06 (molar ratio), relative to the vinyl bond amount adjuster (tertiary amine compound or ether compound). By using sodium alkoxide in this range, it tends to be possible to produce at a high productivity a copolymer having a narrow molecular weight distribution and high strength, which has a copolymer block containing a conjugated diene monomer unit with a high vinyl bond amount and a polymer block mainly composed of a vinyl aromatic monomer unit with a narrow molecular weight distribution.

[0075] The method for copolymerizing a conjugated diene compound and a vinyl aromatic compound using an organic alkali metal compound as a polymerization initiator is not particularly limited, and may be batch polymerization, continuous polymerization, or a combination thereof. The polymerization temperature is not particularly limited, but is usually from 0 to 180°C, and preferably from 30 to 150°C. The time required for polymerization varies depending on the conditions, but is usually within 48 hours, and preferably 0.1 to 10 hours. It is also preferable to carry out the polymerization in an atmosphere of an inert gas such as nitrogen gas. The polymerization pressure is not particularly limited as long as it is within a pressure range sufficient to maintain the monomer and the solvent in a liquid phase within the above-mentioned polymerization temperature range.

[0076] Furthermore, at the end of the polymerization, a required amount of a coupling agent having two or more functional groups may be added to carry out a coupling reaction. The coupling agent having two or more functional groups is not particularly limited, and any known coupling agent can be used. Examples of bifunctional coupling agents include, but are not limited to, dihalogen compounds such as dimethyldichlorosilane and dimethyldibromosilane, acid esters such as methyl benzoate, ethyl benzoate, phenyl benzoate, and phthalates. Examples of polyfunctional coupling agents having three or more functional groups include, but are not limited to, polyalcohols having three or more valences, polyfunctional epoxy compounds such as epoxidized soybean oil and diglycidyl bisphenol A, halogenated silicon compounds represented by the formula R1(4-n)SiXn (wherein R1 is a hydrocarbon group having 1 to 20 carbon atoms, X is a halogen, and n is an integer of 3 or 4), and halogenated tin compounds. Examples of halogenated silicon compounds include, but are not limited to, methylsilyl trichloride, t-butylsilyl trichloride, silicon tetrachloride, and brominated versions of these compounds. Examples of the tin halide compound include, but are not limited to, polyvalent halogen compounds such as methyltin trichloride, t-butyltin trichloride, tin tetrachloride, etc. Dimethyl carbonate, diethyl carbonate, etc. can also be used.

[0077] The hydrogenated copolymer (a), the hydrogenated copolymer (b), and the hydrogenated copolymer (c) may be obtained by subjecting the living terminal of the copolymer obtained by the above-mentioned method to an addition reaction with a modifier that generates a functional group-containing atomic group. Examples of functional group-containing atomic groups include, but are not limited to, atomic groups containing at least one functional group selected from the group consisting of a hydroxyl group, a carbonyl group, a thiocarbonyl group, an acid halide group, an acid anhydride group, a carboxyl group, a thiocarboxyl acid group, an aldehyde group, a thioaldehyde group, a carboxylate group, an amide group, a sulfonic acid group, a sulfonate group, a phosphoric acid group, a phosphoric acid ester group, an amino group, an imino group, a nitrile group, a pyridyl group, a quinoline group, an epoxy group, a thioepoxy group, a sulfide group, an isocyanate group, an isothiocyanate group, a silicon halide group, a silanol group, an alkoxy silicon group, a tin halide group, an alkoxy tin group, and a phenyl tin group.

[0078] Examples of modifying agents having a functional group-containing atomic group include, but are not limited to, tetraglycidyl meta-xylylene diamine, tetraglycidyl-1,3-bisaminomethylcyclohexane, ε-caprolactone, δ-valerolactone, 4-methoxybenzophenone, γ-glycidoxyethyl trimethoxysilane, γ-glycidoxypropyl trimethoxysilane, γ-glycidoxypropyl dimethylphenoxysilane, bis(γ-glycidoxypropyl)methylpropoxysilane, 1,3-dimethyl-2-imidazolidinone, 1,3-diethyl-2-imidazolidinone, N,N'-dimethylpropylene urea, and N-methylpyrrolidone.

[0079] The amount of the modifier added is preferably from 0.01 to 40 parts by mass, more preferably from 0.1 to 20 parts by mass, and further preferably from 0.3 to 10 parts by mass, based on 100 parts by mass of the hydrogenated copolymer before modification. The temperature for the addition reaction of the modifying agent is preferably 0 to 150°C, more preferably 20 to 120°C. The time required for the modification reaction varies depending on the modification reaction conditions, but is preferably within 24 hours, and more preferably 0.1 to 10 hours.

[0080] The hydrogenation catalyst used for producing the hydrogenated copolymer (a), the hydrogenated copolymer (b), and the hydrogenated copolymer (c) is not particularly limited, and examples thereof include the hydrogenation catalysts described in JP-B-42-8704, JP-B-43-6636, JP-B-63-4841, JP-B-1-37970, JP-B-1-53851, JP-B-2-9041, and the like. Preferred hydrogenation catalysts include titanocene compounds and / or mixtures with reducing organometallic compounds. The titanocene compound is not particularly limited, but examples thereof include compounds described in JP-A-8-109219, and specific examples thereof include compounds having at least one ligand having a (substituted) cyclopentadienyl structure, an indenyl structure, and a fluorenyl structure, such as biscyclopentadienyltitanium dichloride and monopentamethylcyclopentadienyltitanium trichloride. The reducing organometallic compound is not particularly limited, but examples thereof include organoalkali metal compounds such as organolithium compounds, organomagnesium compounds, organoaluminum compounds, organoboron compounds, and organozinc compounds.

[0081] The reaction temperature for the hydrogenation reaction is usually from 0 to 200°C, and preferably from 30 to 150°C. The pressure of hydrogen used in the hydrogenation reaction is preferably 0.1 to 30 MPa, more preferably 0.2 to 10 MPa, and further preferably 0.3 to 5 MPa. The reaction time for the hydrogenation reaction is usually 3 minutes to 10 hours, and preferably 10 minutes to 5 hours.

[0082] The hydrogenation reaction may be carried out by any of a batch process, a continuous process, or a combination thereof. After completion of the hydrogenation reaction, the catalyst residue may be removed from the reaction solution, if necessary. Methods for separating the hydrogenated copolymer from the solvent include, but are not limited to, a method in which a polar solvent that is a poor solvent for the hydrogenated copolymer, such as acetone or alcohol, is added to a solution of the hydrogenated copolymer to precipitate and recover the hydrogenated copolymer; a method in which the solution of the hydrogenated copolymer is poured into hot water with stirring and the solvent is removed by steam stripping to recover the hydrogenated copolymer; and a method in which the solvent is distilled off by directly heating the solution of the hydrogenated copolymer. The hydrogenated copolymer of the present embodiment may contain an antioxidant on its surface and / or inside, for example, by adding an antioxidant during the production.

[0083] The following antioxidant may also be added to the resin composition of the present embodiment, which will be described later. Examples of the antioxidant include, but are not limited to, phenol-based antioxidants, phosphorus-based antioxidants, sulfur-based antioxidants, and amine-based antioxidants.

[0084] Specifically, 2,6-di-t-butyl-4-methylphenol, n-octadecyl-3-(4'-hydroxy-3',5'-di-t-butyl-phenyl)propionate, tetrakis-[methylene-3-(3',5'-di-t-butyl-4'-hydroxyphenyl)propionate]methane], tris-(3,5-di-t-butyl-4-hydroxybenzyl)isocyanurate, 4,4'-butylidene-bis-(3-methyl-6-t-butylphenol), 3,9-bis[2-{3-(3-t-butyl-4-hydroxy-5-methyl n-octylthio)-6-(4-hydroxy-3,5-di-t-butylanilino)-1,3,5-triazine, pentaerythrityl-tetrakis[3 -(3,5-di-t-butyl-4-hydroxyphenyl)propionate], 2,2-thio-diethylenebis[3-(3,5-di-t-butyl-4-hydroxyphenyl)propionate], N,N'-hexamethylenebis(3,5-di-t-butyl-4-hydroxy-hydrocinnamamide), 3,5-di-t-butyl-4-hydroxybenzylphosphonate-diethyl ester, 1,3,5-trimethyl-2,4,6-tris(3,5-di-t-butyl-4-hydroxybenzyl)benzene, bis(3,5-di-t-butyl-4 -Hydroxybenzylphosphonic acid ethyl) calcium and polyethylene wax (50%) mixture, octylated diphenylamine, 2,4-bis[(octylthio)methyl]-o-cresol, isooctyl-3-(3,5-di-t-butyl-4-hydroxyphenyl)propionate, butyric acid, 3,3-bis(3-t-butyl-4-hydroxyphenyl)ethylene ester, 1,1,3-tris-(2-methyl-4-hydroxy-5-t-butylphenyl)butane, 1,3,5-tris(4-t-butyl-3-hydroxy-2,6-dimethylbenzyl) isocyanurate, 2-t-butyl-6-(3'-t-butyl-5'-methyl-2'-hydroxybenzyl)-4-methylphenyl-acrylate, and 2-[1-(2-hydroxy-3,5-di-t-pentylphenyl)-ethyl]-4,6-di-t-pentylphenyl acrylate.

[0085] The hydrogenated copolymer (a) may be pelletized. Examples of the pelletizing method include a method in which the hydrogenated copolymer (a) is extruded in the form of a strand from a single-screw or twin-screw extruder, and cut in water with a rotary blade installed in front of a die section; a method in which the hydrogenated copolymer is extruded in the form of a strand from a single-screw or twin-screw extruder, cooled with water or air, and then cut with a strand cutter; and a method in which the copolymer is melt-mixed using an open roll or Banbury mixer, formed into a sheet using a roll, the sheet is cut into strips, and then cut into cubic pellets using a pelletizer. The size and shape of the pellets of the hydrogenated copolymer (a) are not particularly limited.

[0086] The hydrogenated copolymer (b) and the hydrogenated copolymer (c) may be crumbed. When these polymerization and hydrogenation steps are carried out in an inert hydrocarbon solvent, for example, the inert hydrocarbon solvent is removed to isolate the hydrogenated copolymer, thereby obtaining crumbs. Specific methods for removing the solvent are not particularly limited, but include, for example, steam stripping. Hydrous crumbs are obtained by steam stripping, and the obtained hydrous crumbs are dried to obtain crumbs of the hydrogenated copolymer.

[0087] In steam stripping, it is preferable to use a surfactant as a crumb forming agent. Such surfactants are not particularly limited, but examples thereof include the same anionic surfactants, cationic surfactants, and nonionic surfactants as those mentioned above. These surfactants can generally be added to the water in the stripping zone in an amount of 0.1 ppm to 3000 ppm. In addition to the surfactants, water-soluble salts of metals such as Li, Na, Mg, Ca, Al, and Zn can also be used as crumb dispersion aids.

[0088] The concentration of the crumb-like hydrogenated copolymer (b) and hydrogenated copolymer (c) dispersed in water obtained through the polymerization process of hydrogenated copolymer (b) and hydrogenated copolymer (c) and the steam stripping is generally 0.1% by mass to 20% by mass (ratio to the water in the stripping zone). Within this range, crumbs having good particle size can be obtained without causing operational problems. It is preferable to adjust the moisture content of the crumbs of hydrogenated copolymer (b) and hydrogenated copolymer (c) to 1% by mass to 30% by mass by dehydration, and then dry them until the moisture content is 1% by mass or less.

[0089] In the dehydration step of the crumbs, dehydration may be performed using a compression water wringer such as a roll, a Banbury type dehydrator, or a screw extruder type wringer dehydrator, or dehydration and drying may be performed simultaneously using a conveyer or a box-type hot air dryer.

[0090] In the method for producing the hydrogenated copolymer (b) and the hydrogenated copolymer (c) of the present embodiment, a step of deashing metals derived from the polymerization initiator, etc. may be adopted as necessary. Furthermore, a step of adding an antioxidant, a neutralizing agent, a surfactant, etc. may be adopted as necessary.

[0091] If necessary, the hydrogenated copolymers (a), (b) and (c) may be blended with an antiblocking agent in the pellets and crumbs in order to prevent blocking between the pellets and crumbs. Examples of the anti-blocking agent include, but are not limited to, calcium stearate, magnesium stearate, zinc stearate, polyethylene, polypropylene, ethylene bisstearylamide, talc, and amorphous silica. The amount of the pellet antiblocking agent is preferably 500 to 10,000 ppm, more preferably 1,000 to 5,000 ppm, based on the hydrogenated copolymer (a), the hydrogenated copolymer (b), and the hydrogenated copolymer (c). The antiblocking agent is preferably incorporated in a state of adhering to the pellet and crumb surfaces, but may also be contained to some extent inside the pellet and crumb.

[0092] (thermoplastic resin) The thermoplastic elastomer composition of the present embodiment containing the above-mentioned hydrogenated copolymer (a), hydrogenated copolymer (b), and hydrogenated copolymer (c) may contain a thermoplastic resin. Examples of thermoplastic resins include polyethylene, polypropylene, polyvinyl chloride, polyethylene terephthalate, polycaprolactone, acrylonitrile-butadiene-styrene resin, polystyrene, methacrylic resin, polyamide, polycarbonate, polybutylene terephthalate, polyphenylene sulfide, polyacetal, modified polyphenylene ether, polysulfone, and acrylonitrile-styrene resin. These thermoplastic resins may be used alone or in combination of two or more. Among them, polypropylene is preferred from the viewpoints of strength, oil resistance, hardness adjustment, and processability of the thermoplastic elastomer composition. Examples of polypropylene include homopolymers of propylene, crystalline copolymers mainly composed of propylene, and block polypropylenes containing an olefin-based elastomer. Examples of the copolymer include block copolymers, random copolymers, and block-random copolymers. Specific examples include crystalline propylene-based polymers such as isotactic polypropylene, propylene-ethylene copolymers, propylene-butene-1 copolymers, and propylene-ethylene-butene-1 terpolymers. These polypropylenes may be used alone or in combination of two or more.

[0093] From the viewpoints of abrasion resistance, soft touch, and balance of various performance properties, the ratio of the sum of the masses of the hydrogenated copolymer (a), the hydrogenated copolymer (b), and the hydrogenated copolymer (c) contained in the thermoplastic elastomer composition of this embodiment to the total mass of the above-mentioned thermoplastic resins is preferably [(a)+(b)+(c)] / (thermoplastic resin)=1 / 99 to 99 / 1, more preferably 10 / 90 to 90 / 10, and even more preferably 20 / 80 to 80 / 20.

[0094] (Softener) The thermoplastic elastomer composition of the present embodiment containing the above-mentioned hydrogenated copolymer (a), hydrogenated copolymer (b), and hydrogenated copolymer (c) may contain a softener. Examples of the softener include, but are not limited to, paraffinic oil, naphthenic oil, aromatic oil, paraffin wax, liquid paraffin, white mineral oil, vegetable softener, etc. Among these, paraffinic oil, liquid paraffin, and white mineral oil are more preferable from the viewpoints of low-temperature properties and bleeding resistance of the thermoplastic elastomer composition and the molded article.

[0095] The kinetic viscosity of the softener at 40°C is preferably 500mm 2 The lower limit of the kinetic viscosity of the softener at 40°C is not particularly limited, but is preferably 10 mm 2 The kinematic viscosity of the softener at 40°C is preferably 500 mm 2 / second or less, the flowability of the thermoplastic elastomer composition is improved, and the molding processability tends to be improved. The kinetic viscosity of the softener can be measured by a method using a glass capillary viscometer.

[0096] In the thermoplastic elastomer composition, the amount of the softener is preferably 5 to 100 parts by mass, more preferably 10 to 80 parts by mass, and even more preferably 15 to 60 parts by mass, per 100 parts by mass of the total amount of the hydrogenated copolymers (a) to (c) and the thermoplastic resin.

[0097] (Olefin elastomer) The thermoplastic elastomer composition of the present embodiment may further contain an olefin-based elastomer. Examples of the olefin-based elastomer include an α-olefin polymer or copolymer having 2 to 20 carbon atoms, and a copolymer of ethylene and an unsaturated carboxylic acid or an unsaturated carboxylate ester. Examples of olefin-based elastomers include, but are not limited to, ethylene-propylene copolymers, ethylene-1-butene copolymers, ethylene-1-hexene copolymers, ethylene-4-methylpentene copolymers, ethylene-1-octene copolymers, propylene homopolymers, propylene-ethylene copolymers, propylene-ethylene-1-butene copolymers, 1-butene homopolymers, 1-butene-ethylene copolymers, 1-butene-propylene copolymers, 4-methylpentene homopolymers, 4-methylpentene-1-propylene copolymers, 4-methylpentene-1-butene copolymers, 4-methylpentene-1-propylene-1-butene copolymers, propylene-1-butene copolymers, ethylene-vinyl acetate copolymers, ethylene-methacrylic acid copolymers, and ethylene-methyl methacrylate copolymers.

[0098] (tackifier) The thermoplastic elastomer composition of the present embodiment may contain a tackifier. Examples of tackifiers include, but are not limited to, coumarone-indene resin, pt-butylphenol-acetylene resin, phenol-formaldehyde resin, xylene-formaldehyde resin, terpene resin, hydrogenated terpene resin, terpene-phenol resin, hydrogenated terpene phenol resin, aromatic modified terpene resin, aromatic modified hydrogenated phenol resin, styrene resin, alpha-methylstyrene resin, aromatic hydrocarbon resin, aliphatic hydrocarbon resin, aliphatic cyclic hydrocarbon resin, aliphatic and alicyclic petroleum resin, aliphatic and aromatic hydrocarbon resin, hydrogenated modified alicyclic hydrocarbon resin, hydrogenated alicyclic hydrocarbon resin, hydrocarbon tackifying resin, polybutene, liquid polybutadiene, cis-1,4-polyisoprene rubber, hydrogenated polyisoprene rubber, liquid polyisoprene rubber, and rosin resin.

[0099] (Additives) The thermoplastic elastomer composition containing the hydrogenated copolymer of the present embodiment may further contain other additives in addition to the above-mentioned components, as long as the object of the present invention is not impaired. Examples of such additives include inorganic fillers, talc, heat stabilizers, antioxidants, ultraviolet absorbers, antiaging agents, plasticizers, light stabilizers, crystal nucleating agents, impact modifiers, pigments, lubricants, antistatic agents, flame retardants, flame retardant assistants, compatibilizers, and tackifiers. These additives may be used alone or in combination of two or more.

[0100] (Method of producing thermoplastic elastomer composition) The method for producing the thermoplastic elastomer composition is not particularly limited, and it can be produced by a conventionally known method. For example, a melt-kneading method using a general mixer such as a pressure kneader, a Banbury mixer, an internal mixer, a lab plastomill, a mix lab, a single screw extruder, a twin screw extruder, a co-kneader, or a multi-screw extruder, or a method in which each component is dissolved or dispersed and mixed, and then the solvent is removed by heating, etc. are used. The shape of the thermoplastic elastomer is not particularly limited, and examples thereof include pellets, sheets, strands, and chips. In addition, after melt-kneading, it can be directly molded into a molded product.

[0101] [Molded Articles of Thermoplastic Elastomer Composition] The molded article of this embodiment is an article molded from the thermoplastic elastomer composition of this embodiment described above. The molded article of the thermoplastic elastomer composition of the present embodiment is excellent in abrasion resistance, processability, and a balance of various performances. Taking advantage of such properties, the article can be suitably used for extrusion molded articles, injection molded articles, blow molded articles, compressed air molded articles, vacuum molded articles, high-frequency fusion molded articles, overmolded articles, slush molded articles, and the like.

[0102] Specific applications of the material include, but are not limited to, automotive parts such as side moldings, grommets, shift knobs, weather strips, window frames and their sealing materials, arm rests, assist grips, door grips, door trims, handle grips, console boxes, head rests, instrument panels, bumpers, spoilers, and airbag covers. Examples of medical devices include, but are not limited to, medical tubes, medical hoses, catheters, blood bags, infusion bags, platelet storage bags, and artificial dialysis bags. Examples of building materials include, but are not limited to, wall materials, floor materials, and the like. Other examples include, but are not limited to, industrial hoses, food hoses, vacuum cleaner hoses, electrical cooling packing, various covering materials for electrical wires and the like, covering materials for grips, soft dolls, and the like. Examples of the fiber material include sound absorbing materials, clothing components, nonwoven fabrics for filters, and sanitary products. The molded article of this embodiment may be appropriately subjected to processing such as foaming, powdering, stretching, bonding, printing, painting, plating, and the like.

[0103] In recent years, autonomous driving and mobility services have been attracting attention as new directions for automobiles. This trend is also causing changes in the performance required for automotive interior materials. For example, with the advent of autonomous driving, it is expected that automobiles will play a stronger role as living spaces. As a result, interiors are becoming more luxurious and interior designs are becoming more diverse in order to create spaces where passengers can feel more comfortable. This means that thermoplastic elastomer compositions, which are used as materials for automobile interior materials, are required to have a softer feel than before. From the viewpoint of mobility services, it is believed that the spread of car sharing will lead to increased demand for longer life and cleanliness of automobiles. Therefore, automobile interior materials will be cleaned more frequently than before, and the thermoplastic elastomer compositions used as materials for automobile interior materials will need to have higher abrasion resistance. Due to the spread of autonomous driving and mobility services as described above, in recent years, hydrogenated copolymers, which are materials for thermoplastic elastomer compositions, are required to have a softer feel than conventional products while also having high abrasion resistance. However, in general, the soft touch and abrasion resistance of hydrogenated copolymers are physical properties that tend to be exhibited by polymer structures that are mutually contradictory. For example, by decreasing the molecular weight of the hydrogenated copolymer and / or increasing the amount of vinyl bonds in the conjugated diene, the hardness of the hydrogenated copolymer tends to decrease and the soft touch tends to improve, but on the other hand, the abrasion resistance tends to decrease. In consideration of the above-mentioned changes in performance required for automobile interior materials and the problems of hydrogenated copolymers and thermoplastic elastomer compositions containing the same, the thermoplastic elastomer composition of the present embodiment has high abrasion resistance while having a soft touch, and therefore provides a comfortable interior space, imparts a sense of luxury, and can withstand long-term use. It is particularly suitable for molded products of the thermoplastic elastomer composition that require a high level of abrasion resistance, soft touch, and a balance of various performances. For example, these include packaging materials for food, beverages, medicines, precision instruments, etc., tubes (including catheters), bags, containers, trays, automobile parts and automobile interior covering materials (door trim, instrument panels, airbag covers, etc.), home appliances and office equipment parts, industrial parts, household goods, toys, etc. The above-mentioned extrusion molded product or injection molded product may be a multi-layer extrusion molded product or a multi-layer injection molded product, in which the thermoplastic elastomer composition of the present embodiment may be used in all layers, only one layer, or two or more layers. EXAMPLES

[0104] The present invention will be described in detail below with reference to specific examples and comparative examples, but the present invention is not limited to the following examples. First, the evaluation methods and the methods for measuring physical properties applied to the examples and comparative examples are described below.

[0105] [Method of identifying the structures of hydrogenated copolymer (a), hydrogenated copolymer (b), and hydrogenated copolymer (c), and method of measuring physical properties] (Content of total vinyl aromatic monomer units in hydrogenated copolymer) The total vinyl aromatic monomer unit content in each of the hydrogenated copolymers (a), (b) and (c) was measured by the following method. The total vinyl aromatic monomer unit content (mass%) of each copolymer was calculated from the absorption intensity at 262 nm using an ultraviolet spectrophotometer (Shimadzu Corporation, UV-2450) before hydrogenation. Incidentally, since the content of all vinyl aromatic monomer units does not change significantly before and after hydrogenation, the content of all vinyl aromatic monomer units (styrene monomer units) obtained for the copolymer before hydrogenation was taken as the content of all vinyl aromatic monomer units (total styrene content) of the hydrogenated copolymer.

[0106] (Contents (Os values) of polymer blocks A1 to C1 in hydrogenated copolymers (a) to (c)) The contents of the polymer blocks A1 to C1 mainly composed of vinyl aromatic monomer units in the hydrogenated copolymers (a) to (c) were measured by the following method. The copolymer before hydrogenation was measured by the osmium tetroxide decomposition method described in I. M. KOLTHOFF et al., J. Polym. Soi. 1, 429 (1946). To decompose the copolymer before hydrogenation, a 0.1 g / 125 mL tertiary butanol solution of osmic acid was used. The content of the polystyrene blocks obtained here was designated as the "Os value."

[0107] (Amount of vinyl aromatic monomer units in polymer block A2) The content of the vinyl aromatic monomer unit in the polymer block A2 in the hydrogenated polymer block (a) was measured by the following method. The hydrogenated block copolymer was used as a measurement sample, and a polymer block mainly composed of vinyl aromatic monomer units and a polymer block composed of vinyl aromatic monomer units and conjugated diene monomer units were distinguished by proton nuclear magnetic resonance (1H-NMR, JOEL RESONABCE ECS400). Deuterated chloroform was used as the solvent, the sample concentration was 50 mg / mL, the observation frequency was 400 MHz, tetramethylsilane was used as the chemical shift standard, the pulse delay was 2.904 seconds, the number of scans was 256, and the measurement temperature was 23° C. From the integral intensity of the signal assigned to aromatics, the random and block aromatics were calculated from the integral value per 1H of each bonding mode, and then the total styrene content was calculated by the above-mentioned method, and the content ratio was calculated.

[0108] (Amount of vinyl bonds in polymer blocks (A2, B2, C2)) The vinyl bond amounts before hydrogenation of the polymer block A2 of the hydrogenated copolymer (a), the polymer block B2 of the hydrogenated copolymer (b) and the polymer block C2 of the hydrogenated copolymer (c) were measured by the following method. The polymer samples taken at each step of the polymerization process of the copolymer before hydrogenation were measured for the vinyl bond amount (1,2-bond amount) by proton nuclear magnetic resonance (1H-NMR) using a nuclear magnetic resonance apparatus (BRUKER, DPX-400). Deuterated chloroform was used as the solvent, the sample concentration was 50 mg / mL, the observation frequency was 400 MHz, tetramethylsilane was used as the chemical shift standard, the pulse delay was 2.904 seconds, the number of scans was 64, the pulse width was 45°, and the measurement temperature was 26°C. The amount of vinyl bonds was calculated from the ratio of 1,2-bonds to the sum of 1,4-bonds and 1,2-bonds after calculating the integral value per 1H of each bond type from the integral values ​​of the signals assigned to 1,4-bonds and 1,2-bonds.

[0109] (Weight average molecular weight of hydrogenated copolymer) The weight average molecular weights of the hydrogenated copolymers (a), (b) and (c) were measured by the following method. Measurements were performed using GPC (equipment: Tosoh HLC8220, column TSKgel SuperH-RC x 2). Tetrahydrofuran was used as the solvent. Measurements were performed at a temperature of 35°C. A calibration curve was created using commercially available standard polystyrene with a known weight average molecular weight, and the weight average molecular weight converted into polystyrene was calculated.

[0110] (Hydrogenation rate of hydrogenated copolymer (hydrogenation rate)) The hydrogenation rates of the hydrogenated copolymers (a), (b) and (c) were measured by the following method. The hydrogenation rate of the hydrogenated copolymer was measured by a nuclear magnetic resonance apparatus (BRUKER, DPX-400). The hydrogenated copolymer, which is the copolymer after hydrogenation, was used to measure by proton nuclear magnetic resonance (1H-NMR). Specifically, the integral values ​​of the signal derived from the residual double bond at 4.5 to 5.5 ppm and the signal derived from the hydrogenated conjugated diene were calculated, and the ratio was calculated.

[0111] [Production of Thermoplastic Elastomer Composition] Hydrogenated copolymer (a) / hydrogenated copolymer (b) / hydrogenated copolymer (c) / polypropylene resin / softener were blended in the proportions shown in Tables 4 to 6, and melt-kneaded at a set temperature of 200°C using a twin-screw extruder (Japan Steel Works, Ltd., "TEX-30αII", cylinder diameter 30 mm) to obtain pellets of a thermoplastic elastomer composition. Molding was performed at an injection molding temperature of 210° C. and a mold temperature of 40° C. to obtain a molded article of the thermoplastic elastomer composition (thickness 2.0 mm, with leather grain). The hydrogenated copolymers (a) used were a-1 to a-4 shown in Table 1, the hydrogenated copolymers (b) used were b-1 to b-8 shown in Table 2, and the hydrogenated copolymers (c) used were c-1 to c-2 shown in Table 3. The polypropylene resin used was PM801A (homopolypropylene / Sunallomer; MFR (230° C., 2.16 kg)=15). The softener used was paraffin oil, PW-90 (manufactured by Idemitsu Kosan Co., Ltd.).

[0112] [Evaluation of physical properties of molded products of thermoplastic elastomer compositions] (Wear resistance) The abrasion resistance of the molded thermoplastic elastomer composition was evaluated by measuring the mass loss of the sample after rubbing the surface of the molded product (embossed leather surface) with a friction cloth Kanakin No. 3 cotton under a load of 500 g using a Gakushin type friction tester (AB-301 model, manufactured by Tester Sangyo Co., Ltd.). The smaller the mass loss, the higher the abrasion resistance of the thermoplastic elastomer composition is, and the evaluation was performed according to the following criteria. 5: After 10,000 friction cycles, the mass loss is less than 0.010g 4: After 10,000 friction cycles, the mass loss is 0.010g or more and less than 0.030g 3: After 10,000 friction cycles, the mass loss is 0.030g or more and less than 0.045g 2: After 10,000 friction cycles, the mass loss is 0.045g or more and less than 0.060g 1: After 10,000 friction cycles, the mass loss is 0.060g or more.

[0113] (Soft touch: hardness) Regarding the feel of the thermoplastic elastomer, the hardness (hardness after 10 seconds) of the thermoplastic elastomer composition was measured using a durometer type A in accordance with JIS K6253. The lower the hardness value, the softer the feel of the molded article of the thermoplastic elastomer composition tends to be. The hardness was evaluated according to the following criteria. 5: Hardness after 10 seconds is less than 55 4: Hardness after 10 seconds is 55 or more but less than 60 3: Hardness after 10 seconds is between 60 and 65 2: Hardness after 10 seconds is between 65 and 70 1: After 10 seconds, the hardness is 70 or more

[0114] (exterior) The thermoplastic elastomer composition was injection molded at a temperature of 210°C and a mold temperature of 40°C to form a flat plate (length 150 mm, width 100 mm, thickness 2 mm, with leather grain), and the appearance of the molded product was evaluated. The appearance was evaluated based on the following criteria from six viewpoints (presence or absence of problems): mold releasability, embossing transferability, warpage (molding shrinkage), sink marks, flow marks, and shine when the thermoplastic elastomer composition was injection molded. 5: No problems at all 4: One out of six problems occur 3: Two out of six problems occur 2: Three out of six problems occur 1: Four or more of the six problems occur (molding is not possible)

[0115] (CS (Compression set (C-set)) In accordance with JIS K6262, the CS was measured after compressing the sample by 25% and leaving it at rest at a temperature of 70°C for 72 hours, and the evaluation was carried out according to the following criteria. 5: CS is less than 65% 4: CS is 65% or more but less than 70% 3: CS is between 70% and 75% 2: CS is between 75% and 80% 1: CS is 80% or more

[0116] [Production of hydrogenated copolymer] (Preparation of hydrogenation catalyst) The hydrogenation catalyst used in the hydrogenation reaction of the copolymer was prepared by the following method. A nitrogen-purged reaction vessel was charged with 1 liter of dried and purified cyclohexane, and 100 mmol of biscyclopentadienyltitanium dichloride was added. With sufficient stirring, an n-hexane solution containing 200 mmol of trimethylaluminum was added, and the mixture was allowed to react at room temperature for approximately 3 days to obtain a hydrogenation catalyst.

[0117] (Hydrogenated copolymer) Hydrogenated copolymers (a-1) to (a-4), hydrogenated copolymers (b-1) to (b-8), and hydrogenated copolymers (c-1) to (c-2) were prepared as follows. <Hydrogenated copolymer (a-1)> Batch polymerization was carried out using a tank-type reactor (internal volume: 10 L) equipped with a stirrer and a jacket. First, a cyclohexane solution containing 20 parts by mass of styrene (concentration: 20% by mass) was added. Next, 0.084 parts by mass of n-butyllithium per 100 parts by mass of the total monomers and 0.35 mol of N,N,N',N'-tetramethylethylenediamine per 1 mol of n-butyllithium were added, and polymerization was carried out at 70°C for 20 minutes. Next, a cyclohexane solution containing 47 parts by mass of styrene and a cyclohexane solution containing 33 parts by mass of butadiene (concentration: 20% by mass) were added and polymerized at 70° C. for 1 hour. Next, 0.25 mol of ethyl benzoate was added per mol of n-butyllithium, and the mixture was reacted at 70° C. for 10 minutes. Thereafter, methanol was added to terminate the polymerization reaction. The copolymer obtained as above had a styrene content of 67% by mass, a polymer block A1 content of 20% by mass, a vinyl bond amount in polymer block A2 before hydrogenation of 25%, and a weight average molecular weight of 193,000. The coupling rate determined from the peak area ratio of the GPC curve was 50%. Further, the hydrogenation catalyst prepared as described above was added to the resulting copolymer in an amount of 50 ppm (Ti standard) per 100 parts by mass of the copolymer, and a hydrogenation reaction was carried out at a hydrogen pressure of 0.7 MPa and a temperature of 80°C. The hydrogenation rate of the resulting hydrogenated copolymer was 98%. Next, 0.3 parts by mass of octadecyl-3-(3,5-di-t-butyl-4-hydroxyphenyl)propionate was added as a stabilizer based on 100 parts by mass of the hydrogenated copolymer to obtain a hydrogenated copolymer (a-1).

[0118] <Hydrogenated copolymer (a-2)> Batch polymerization was carried out using a tank-type reactor (internal volume: 10 L) equipped with a stirrer and a jacket. First, a cyclohexane solution containing 10 parts by mass of styrene (concentration: 20% by mass) was added. Next, 0.067 parts by mass of n-butyllithium per 100 parts by mass of the total monomers and 0.35 mol of N,N,N',N'-tetramethylethylenediamine per 1 mol of n-butyllithium were added, and polymerization was carried out at 70°C for 20 minutes. Next, a cyclohexane solution containing 47 parts by mass of styrene and a cyclohexane solution containing 33 parts by mass of butadiene (concentration: 20% by mass) were added and polymerized at 70° C. for 1 hour. Next, a cyclohexane solution containing 10 parts by mass of styrene (concentration: 20% by mass) was added, and polymerization was carried out at 70° C. for 20 minutes. Thereafter, methanol was added to terminate the polymerization reaction. The copolymer obtained as above had a styrene content of 67% by mass, a polymer block A1 content of 20% by mass, a vinyl bond amount in polymer block A2 before hydrogenation of 18%, and a weight average molecular weight of 154,000. Further, the hydrogenation catalyst prepared as described above was added to the resulting copolymer in an amount of 50 ppm (Ti standard) per 100 parts by mass of the copolymer, and a hydrogenation reaction was carried out at a hydrogen pressure of 0.7 MPa and a temperature of 80°C. The hydrogenation rate of the resulting hydrogenated copolymer was 98%. Next, 0.3 parts by mass of octadecyl-3-(3,5-di-t-butyl-4-hydroxyphenyl)propionate was added as a stabilizer based on 100 parts by mass of the hydrogenated copolymer to obtain a hydrogenated copolymer (a-2).

[0119] <Hydrogenated copolymer (a-3)> Batch polymerization was carried out using a tank reactor (inner volume 10 L) equipped with a stirrer and a jacket. went. First, a cyclohexane solution containing 15 parts by mass of styrene (concentration: 20% by mass) was added. Next, 0.085 parts by mass of n-butyllithium per 100 parts by mass of the total monomers and 0.8 mol of N,N,N',N'-tetramethylethylenediamine per 1 mol of n-butyllithium were added, and polymerization was carried out at 70°C for 5 minutes. Next, a cyclohexane solution containing 3 parts by mass of butadiene (concentration: 20% by mass) was added and polymerization was carried out at 70° C. for 5 minutes. Next, a cyclohexane solution containing 29 parts by mass of butadiene and 50 parts by mass of styrene (concentration: 20% by mass) was supplied so as to maintain a constant reaction temperature, and polymerization was carried out at 70° C. for 45 minutes. Next, a cyclohexane solution containing 3 parts by mass of butadiene was added, and polymerization was carried out at 70° C. for 5 minutes. Finally, 0.2 mol of tetraethoxysilane was added per mol of n-butyllithium, and the mixture was reacted at 70° C. for 30 minutes. Thereafter, methanol was added to terminate the polymerization reaction. The copolymer obtained as described above had a styrene content of 65% by mass, a polymer block A1 content of 15% by mass, a vinyl bond amount of block copolymer A2 before hydrogenation of 23%, and a weight average molecular weight of 301,000. The coupling rate determined from the peak area ratio of the GPC curve was 70%. Further, the hydrogenation catalyst prepared as described above was added to the resulting copolymer in an amount of 50 ppm (Ti standard) per 100 parts by mass of the copolymer, and a hydrogenation reaction was carried out at a hydrogen pressure of 0.7 MPa and a temperature of 80°C. The hydrogenation rate of the resulting hydrogenated copolymer was 98%. Next, 0.3 parts by mass of octadecyl-3-(3,5-di-t-butyl-4-hydroxyphenyl)propionate was added as a stabilizer based on 100 parts by mass of the hydrogenated copolymer to obtain a hydrogenated copolymer (a-3).

[0120] <Hydrogenated copolymer (a-4)> Batch polymerization was carried out using a tank-type reactor (internal volume: 10 L) equipped with a stirrer and a jacket. First, a cyclohexane solution containing 9 parts by mass of styrene (concentration: 20% by mass) was added. Next, 0.084 parts by mass of n-butyllithium per 100 parts by mass of the total monomers, 1.8 mol of N,N,N',N'-tetramethylethylenediamine per 1 mol of n-butyllithium, and 0.05 mol of sodium-t-pentoxide per 1 mol of n-butyllithium were added, and polymerization was carried out at 70°C for 20 minutes. Next, a cyclohexane solution containing 25 parts by mass of styrene and a cyclohexane solution containing 21 parts by mass of butadiene (concentration: 20% by mass) were added and polymerized at 70° C. for 45 minutes. Next, a cyclohexane solution containing 45 parts by mass of butadiene was added, and polymerization was carried out at 60° C. for 1 hour. Thereafter, methanol was added to terminate the polymerization reaction. The polymer obtained as above had a styrene content of 34% by mass, a polymer block A content of 9% by mass, a vinyl bond amount in polymer block A2 of 39%, and a weight average molecular weight of 148,000. Further, the hydrogenation catalyst prepared as described above was added to the resulting copolymer in an amount of 50 ppm (Ti standard) per 100 parts by mass of the copolymer, and a hydrogenation reaction was carried out at a hydrogen pressure of 0.7 MPa and a temperature of 80°C. The hydrogenation rate of the resulting hydrogenated copolymer was 98%. Next, 0.3 parts by mass of octadecyl-3-(3,5-di-t-butyl-4-hydroxyphenyl)propionate was added as a stabilizer based on 100 parts by mass of the hydrogenated copolymer to obtain a hydrogenated copolymer (a-4).

[0121] <Hydrogenated copolymer (b-1)> Batch polymerization was carried out using a tank-type reactor (internal volume: 100 L, charged cyclohexane: 38 L) equipped with a stirrer and a jacket. First, a cyclohexane solution containing 20 parts by mass of styrene was added. Next, 0.056 part by mass of n-butyllithium relative to 100 parts by mass of the total monomers and 1.2 mol of N,N,N',N'-tetramethylethylenediamine relative to 1 mol of n-butyllithium were added, and polymerization was carried out at 70°C for 20 minutes. Next, a cyclohexane solution containing 80 parts by mass of butadiene was added, and polymerization was carried out at 80° C. for 1 hour. Next, tetramethoxysilane was added so that the molar ratio of Si to Li (Si / Li) became 0.24 mol, and the reaction was carried out at 80° C. for 20 minutes. Thereafter, methanol was added to terminate the polymerization reaction. The copolymer obtained as described above had a styrene content of 20% by mass, a polymer block B1 content of 20% by mass, a vinyl bond amount in polymer block A2 before hydrogenation of 65%, and a weight average molecular weight of 407,000. The coupling ratio calculated from the peak area ratio of the GPC curve was 71% (branching ratio (mass %): 2-branch / 3-branch / 4-branch=14 / 50 / 7). Further, the hydrogenation catalyst prepared as described above was added to the resulting copolymer in an amount of 50 ppm (Ti standard) per 100 parts by mass of the copolymer, and a hydrogenation reaction was carried out at a hydrogen pressure of 0.7 MPa and a temperature of 90°C. The hydrogenation rate of the resulting hydrogenated copolymer was 99%. Next, 0.3 parts by mass of octadecyl-3-(3,5-di-t-butyl-4-hydroxyphenyl)propionate was added as a stabilizer based on 100 parts by mass of the hydrogenated copolymer to obtain a hydrogenated copolymer (b-1).

[0122] <Hydrogenated copolymer (b-2)> Batch polymerization was carried out using a tank-type reactor (internal volume: 100 L, charged cyclohexane: 38 L) equipped with a stirrer and a jacket. First, a cyclohexane solution containing 20 parts by mass of styrene was added. Next, 0.056 part by mass of n-butyllithium relative to 100 parts by mass of the total monomers and 1.0 mol of N,N,N',N'-tetramethylethylenediamine relative to 1 mol of n-butyllithium were added, and polymerization was carried out at 70°C for 20 minutes. Next, a cyclohexane solution containing 80 parts by mass of butadiene was added, and polymerization was carried out at 80° C. for 1 hour. Next, tetramethoxysilane was added so that the molar ratio of Si to Li (Si / Li) became 0.24 mol, and the reaction was carried out at 80° C. for 20 minutes. Thereafter, methanol was added to terminate the polymerization reaction. The copolymer obtained as above had a styrene content of 20% by mass, a polymer block B1 content of 20% by mass, a vinyl bond amount in polymer block A2 before hydrogenation of 53%, and a weight average molecular weight of 423,000. The coupling ratio calculated from the peak area ratio of the GPC curve was 78% (branching ratio (mass %): 2-branch / 3-branch / 4-branch=16 / 53 / 9). Further, the hydrogenation catalyst prepared as described above was added to the resulting copolymer in an amount of 50 ppm (Ti standard) per 100 parts by mass of the copolymer, and a hydrogenation reaction was carried out at a hydrogen pressure of 0.7 MPa and a temperature of 90°C. The hydrogenation rate of the resulting hydrogenated copolymer was 99%. Next, 0.3 parts by mass of octadecyl-3-(3,5-di-t-butyl-4-hydroxyphenyl)propionate was added as a stabilizer based on 100 parts by mass of the hydrogenated copolymer to obtain a hydrogenated copolymer (b-2).

[0123] <Hydrogenated copolymer (b-3)> Batch polymerization was carried out using a tank-type reactor (internal volume: 100 L, charged cyclohexane: 38 L) equipped with a stirrer and a jacket. First, a cyclohexane solution containing 20 parts by mass of styrene was added. Next, 0.056 part by mass of n-butyllithium per 100 parts by mass of the total monomers and 1.8 mol of N,N,N',N'-tetramethylethylenediamine per 1 mol of n-butyllithium were added, and polymerization was carried out at 50°C for 20 minutes. Next, a cyclohexane solution containing 80 parts by mass of butadiene was added, and polymerization was carried out at 80° C. for 1 hour. Next, tetramethoxysilane was added so that the molar ratio of Si to Li (Si / Li) became 0.24 mol, and the reaction was carried out at 80° C. for 20 minutes. Thereafter, methanol was added to terminate the polymerization reaction. The copolymer obtained as above had a styrene content of 20% by mass, a polymer block B1 content of 20% by mass, a vinyl bond amount in polymer block A2 before hydrogenation of 77%, and a weight average molecular weight of 407,000. The coupling ratio calculated from the peak area ratio of the GPC curve was 71% (branching ratio (mass %): 2-branch / 3-branch / 4-branch=14 / 50 / 7). Further, the hydrogenation catalyst prepared as described above was added to the resulting copolymer in an amount of 50 ppm (Ti standard) per 100 parts by mass of the copolymer, and a hydrogenation reaction was carried out at a hydrogen pressure of 0.7 MPa and a temperature of 90°C. The hydrogenation rate of the resulting hydrogenated copolymer was 99%. Next, 0.3 parts by mass of octadecyl-3-(3,5-di-t-butyl-4-hydroxyphenyl)propionate was added as a stabilizer based on 100 parts by mass of the hydrogenated copolymer to obtain a hydrogenated copolymer (b-3).

[0124] <Hydrogenated copolymer (b-4)> Batch polymerization was carried out using a tank-type reactor (internal volume: 100 L, charged cyclohexane: 38 L) equipped with a stirrer and a jacket. First, a cyclohexane solution containing 28 parts by mass of styrene was added. Next, 0.056 part by mass of n-butyllithium relative to 100 parts by mass of the total monomers and 1.2 mol of N,N,N',N'-tetramethylethylenediamine relative to 1 mol of n-butyllithium were added, and polymerization was carried out at 70°C for 20 minutes. Next, a cyclohexane solution containing 72 parts by mass of butadiene was added, and polymerization was carried out at 80° C. for 1 hour. Next, tetramethoxysilane was added so that the molar ratio of Si to Li (Si / Li) became 0.24 mol, and the reaction was carried out at 80° C. for 20 minutes. Thereafter, methanol was added to terminate the polymerization reaction. The copolymer obtained as above had a styrene content of 28% by mass, a polymer block B1 content of 28% by mass, a vinyl bond amount in polymer block A2 before hydrogenation of 65%, and a weight average molecular weight of 407,000. The coupling ratio calculated from the peak area ratio of the GPC curve was 71% (branching ratio (mass %): 2-branch / 3-branch / 4-branch=14 / 50 / 7). Further, the hydrogenation catalyst prepared as described above was added to the resulting copolymer in an amount of 50 ppm (Ti standard) per 100 parts by mass of the copolymer, and a hydrogenation reaction was carried out at a hydrogen pressure of 0.7 MPa and a temperature of 90°C. The hydrogenation rate of the resulting hydrogenated copolymer was 99%. Next, 0.3 parts by mass of octadecyl-3-(3,5-di-t-butyl-4-hydroxyphenyl)propionate was added as a stabilizer based on 100 parts by mass of the hydrogenated copolymer to obtain a hydrogenated copolymer (b-4).

[0125] <Hydrogenated copolymer (b-5)> Batch polymerization was carried out using a tank-type reactor (internal volume: 100 L, charged cyclohexane: 38 L) equipped with a stirrer and a jacket. First, a cyclohexane solution containing 33 parts by mass of styrene was added. Next, 0.056 part by mass of n-butyllithium relative to 100 parts by mass of the total monomers and 1.2 mol of N,N,N',N'-tetramethylethylenediamine relative to 1 mol of n-butyllithium were added, and polymerization was carried out at 70°C for 20 minutes. Next, a cyclohexane solution containing 67 parts by mass of butadiene was added, and polymerization was carried out at 80° C. for 1 hour. Next, tetramethoxysilane was added so that the molar ratio of Si to Li (Si / Li) became 0.24 mol, and the reaction was carried out at 80° C. for 20 minutes. Thereafter, methanol was added to terminate the polymerization reaction. The copolymer obtained as above had a styrene content of 33% by mass, a polymer block B1 content of 33% by mass, a vinyl bond amount in polymer block A2 before hydrogenation of 65%, and a weight average molecular weight of 407,000. The coupling ratio calculated from the peak area ratio of the GPC curve was 71% (branching ratio (mass %): 2-branch / 3-branch / 4-branch=14 / 50 / 7). Further, the hydrogenation catalyst prepared as described above was added to the resulting copolymer in an amount of 50 ppm (Ti standard) per 100 parts by mass of the copolymer, and a hydrogenation reaction was carried out at a hydrogen pressure of 0.7 MPa and a temperature of 90°C. The hydrogenation rate of the resulting hydrogenated copolymer was 99%. Next, 0.3 parts by mass of octadecyl-3-(3,5-di-t-butyl-4-hydroxyphenyl)propionate was added as a stabilizer based on 100 parts by mass of the hydrogenated copolymer to obtain a hydrogenated copolymer (b-5).

[0126] <Hydrogenated copolymer (b-6)> Batch polymerization was carried out using a tank-type reactor (internal volume: 100 L, charged cyclohexane: 38 L) equipped with a stirrer and a jacket. First, a cyclohexane solution containing 20 parts by mass of styrene was added. Next, 0.056 part by mass of n-butyllithium relative to 100 parts by mass of the total monomers and 0.7 mol of N,N,N',N'-tetramethylethylenediamine relative to 1 mol of n-butyllithium were added, and polymerization was carried out at 70°C for 20 minutes. Next, a cyclohexane solution containing 80 parts by mass of butadiene was added, and polymerization was carried out at 80° C. for 1 hour. Next, tetramethoxysilane was added so that the molar ratio of Si to Li (Si / Li) became 0.24 mol, and the reaction was carried out at 80° C. for 20 minutes. Thereafter, methanol was added to terminate the polymerization reaction. The copolymer obtained as described above had a styrene content of 20% by mass, a polymer block B1 content of 20% by mass, a vinyl bond amount in polymer block A2 before hydrogenation of 45%, and a weight average molecular weight of 407,000. The coupling ratio calculated from the peak area ratio of the GPC curve was 71% (branching ratio (mass %): 2-branch / 3-branch / 4-branch=14 / 50 / 7). Further, the hydrogenation catalyst prepared as described above was added to the resulting copolymer in an amount of 50 ppm (Ti standard) per 100 parts by mass of the copolymer, and a hydrogenation reaction was carried out at a hydrogen pressure of 0.7 MPa and a temperature of 90°C. The hydrogenation rate of the resulting hydrogenated copolymer was 99%. Next, 0.3 parts by mass of octadecyl-3-(3,5-di-t-butyl-4-hydroxyphenyl)propionate was added as a stabilizer based on 100 parts by mass of the hydrogenated copolymer to obtain a hydrogenated copolymer (b-6).

[0127] <Hydrogenated copolymer (b-7)> Batch polymerization was carried out using a tank-type reactor (internal volume: 100 L, charged cyclohexane: 38 L) equipped with a stirrer and a jacket. First, a cyclohexane solution containing 42 parts by mass of styrene was added. Next, 0.056 part by mass of n-butyllithium relative to 100 parts by mass of the total monomers and 1.2 mol of N,N,N',N'-tetramethylethylenediamine relative to 1 mol of n-butyllithium were added, and polymerization was carried out at 70°C for 20 minutes. Next, a cyclohexane solution containing 58 parts by mass of butadiene was added, and polymerization was carried out at 80° C. for 1 hour. Next, tetramethoxysilane was added so that the molar ratio of Si to Li (Si / Li) became 0.24 mol, and the reaction was carried out at 80° C. for 20 minutes. Thereafter, methanol was added to terminate the polymerization reaction. The copolymer obtained as above had a styrene content of 42% by mass, a polymer block B1 content of 42% by mass, a vinyl bond amount in polymer block A2 before hydrogenation of 65%, and a weight average molecular weight of 407,000. The coupling ratio calculated from the peak area ratio of the GPC curve was 71% (branching ratio (mass %): 2-branch / 3-branch / 4-branch=14 / 50 / 7). Further, the hydrogenation catalyst prepared as described above was added to the resulting copolymer in an amount of 50 ppm (Ti standard) per 100 parts by mass of the copolymer, and a hydrogenation reaction was carried out at a hydrogen pressure of 0.7 MPa and a temperature of 90°C. The hydrogenation rate of the resulting hydrogenated copolymer was 99%. Next, 0.3 parts by mass of octadecyl-3-(3,5-di-t-butyl-4-hydroxyphenyl)propionate was added as a stabilizer based on 100 parts by mass of the hydrogenated copolymer to obtain a hydrogenated copolymer (b-7).

[0128] <Hydrogenated copolymer (b-8)> Batch polymerization was carried out using a tank-type reactor (internal volume: 100 L, charged cyclohexane: 38 L) equipped with a stirrer and a jacket. First, a cyclohexane solution containing 20 parts by mass of styrene was added. Next, 0.089 part by mass of n-butyllithium relative to 100 parts by mass of the total monomers and 1.2 mol of N,N,N',N'-tetramethylethylenediamine relative to 1 mol of n-butyllithium were added, and polymerization was carried out at 70°C for 20 minutes. Next, a cyclohexane solution containing 80 parts by mass of butadiene was added, and polymerization was carried out at 80° C. for 1 hour. Next, tetramethoxysilane was added so that the molar ratio of Si to Li (Si / Li) became 0.24 mol, and the reaction was carried out at 80° C. for 20 minutes. Thereafter, methanol was added to terminate the polymerization reaction. The copolymer obtained as described above had a styrene content of 20% by mass, a polymer block B1 content of 20% by mass, a vinyl bond amount in polymer block A2 before hydrogenation of 65%, and a weight average molecular weight of 250,000. The coupling ratio calculated from the peak area ratio of the GPC curve was 75% (branching ratio (mass %): 2-branch / 3-branch / 4-branch=12 / 55 / 8). Further, the hydrogenation catalyst prepared as described above was added to the resulting copolymer in an amount of 50 ppm (Ti standard) per 100 parts by mass of the copolymer, and a hydrogenation reaction was carried out at a hydrogen pressure of 0.7 MPa and a temperature of 90°C. The hydrogenation rate of the resulting hydrogenated copolymer was 99%. Next, 0.3 parts by mass of octadecyl-3-(3,5-di-t-butyl-4-hydroxyphenyl)propionate was added as a stabilizer based on 100 parts by mass of the hydrogenated copolymer to obtain a hydrogenated copolymer (b-8).

[0129] <Hydrogenated copolymer (c-1)> Batch polymerization was carried out using a tank-type reactor (internal volume: 10 L) equipped with a stirrer and a jacket. First, a cyclohexane solution containing 15 parts by mass of styrene (concentration: 20% by mass) was added. Next, 0.045 parts by mass of n-butyllithium per 100 parts by mass of the total monomers and 0.35 mol of N,N,N',N'-tetramethylethylenediamine per 1 mol of n-butyllithium were added, and polymerization was carried out at 70°C for 20 minutes. Next, a cyclohexane solution containing 69 parts by mass of butadiene (concentration: 20% by mass) was added, and polymerization was carried out at 70° C. for 1 hour. Next, a cyclohexane solution containing 16 parts by mass of styrene (concentration: 20% by mass) was added, and polymerization was carried out at 70° C. for 20 minutes. Thereafter, methanol was added to terminate the polymerization reaction. The copolymer obtained as described above had a styrene content of 31% by mass, a polymer block C1 content of 31% by mass, a vinyl bond amount in polymer block C2 before hydrogenation of 40%, and a weight average molecular weight of 280,000. Further, the hydrogenation catalyst prepared as described above was added to the resulting copolymer in an amount of 50 ppm (Ti standard) per 100 parts by mass of the copolymer, and a hydrogenation reaction was carried out at a hydrogen pressure of 0.7 MPa and a temperature of 80°C. The hydrogenation rate of the resulting hydrogenated copolymer was 98%. Next, 0.3 parts by mass of octadecyl-3-(3,5-di-t-butyl-4-hydroxyphenyl)propionate was added as a stabilizer based on 100 parts by mass of the hydrogenated copolymer to obtain a hydrogenated copolymer (c-1).

[0130] <Hydrogenated copolymer (c-2)> Batch polymerization was carried out using a tank-type reactor (internal volume: 10 L) equipped with a stirrer and a jacket. First, a cyclohexane solution containing 15 parts by mass of styrene (concentration: 20% by mass) was added. Next, 0.021 part by mass of n-butyllithium per 100 parts by mass of the total monomers and 0.3 mol of N,N,N',N'-tetramethylethylenediamine per 1 mol of n-butyllithium were added, and polymerization was carried out at 70°C for 20 minutes. Next, a cyclohexane solution containing 70 parts by mass of butadiene (concentration: 20% by mass) was added, and polymerization was carried out at 70° C. for 1 hour. Next, a cyclohexane solution containing 15 parts by mass of styrene (concentration: 20% by mass) was added, and polymerization was carried out at 70° C. for 20 minutes. Thereafter, methanol was added to terminate the polymerization reaction. The copolymer obtained as described above had a styrene content of 30% by mass, a polymer block C1 content of 30% by mass, a vinyl bond amount in polymer block C2 before hydrogenation of 35%, and a weight average molecular weight of 450,000. Further, the hydrogenation catalyst prepared as described above was added to the resulting copolymer in an amount of 50 ppm (Ti standard) per 100 parts by mass of the copolymer, and a hydrogenation reaction was carried out at a hydrogen pressure of 0.7 MPa and a temperature of 80°C. The hydrogenation rate of the resulting hydrogenated copolymer was 98%. Next, 0.3 parts by mass of octadecyl-3-(3,5-di-t-butyl-4-hydroxyphenyl)propionate was added as a stabilizer based on 100 parts by mass of the hydrogenated copolymer to obtain a hydrogenated copolymer (c-2).

[0131] The physical properties of the hydrogenated copolymer (a) are shown in Table 1, the physical properties of the hydrogenated copolymer (b) are shown in Table 2, and the physical properties of the hydrogenated copolymer (c) are shown in Table 3. The compositions and properties of thermoplastic elastomer compositions using these are shown in the following Tables 4 to 6.

[0132] [Table 1]

[0133] [Table 2]

[0134] [Table 3]

[0135] [Table 4]

[0136] [Table 5]

[0137] [Table 6]

[0138] From Tables 4 to 6, it is clear that in Examples 1 to 16, there were no scores of "1" in terms of abrasion resistance, soft touch, and balance of various performances, and thus they were excellent. In Comparative Examples 1 to 7, some of the samples were given a score of "1" in terms of abrasion resistance, soft touch, and balance of various performances, and were therefore found to be inferior. [Industrial Applicability]

[0139] The thermoplastic elastomer composition of the present invention has industrial applicability in a wide range of fields, including packaging for various types of clothing, packaging for various types of food, packaging for daily necessities, packaging for industrial materials, laminates for various types of rubber products, resin products, leather products, etc., industrial products such as elastic tapes used in disposable diapers, dicing films, etc., adhesive protective films used to protect building materials and steel plates, base materials for adhesive films, members around drinking water (tubes, hoses, gaskets), sheet products such as trays for fresh meat and fish, fruit and vegetable packs, and frozen food containers, home appliance applications such as televisions, stereos, and vacuum cleaners, materials for automobile interior and exterior parts such as bumper parts, body panels, side seals, and interior (instrument panels, door trims, airbag covers, etc.) skin materials, road paving materials, waterproof materials, waterproof sheets, civil engineering packing, daily necessities, leisure goods, toys, industrial goods, furniture supplies, stationery such as writing utensils, transparent pockets, holders, and file spines, and medical tools such as infusion bags and tubes (including catheters).

Claims

1. Hydrogenated copolymers obtained by hydrogenating polymers containing vinyl aromatic monomer units and conjugated diene monomer units. A thermoplastic elastomer comprising the copolymer (a), the hydrogenated copolymer (b) and the hydrogenated copolymer (c).

1. A composition comprising: The hydrogenated copolymer (a) contains vinyl aromatic monomer units and conjugated diene monomer units. and a polymer block A2 having a vinyl aromatic monomer unit content of 25% by mass or more; The hydrogenated copolymer (b) has a polymer block B1 containing 80% by mass or more of vinyl aromatic monomer units and a polymer block B2 containing 80% by mass or more of conjugated diene monomer units, The content of vinyl aromatic monomer units in the hydrogenated copolymer (b) is 10 to 40 mass %, the amount of vinyl bonds in the polymer block B2 before hydrogenation is 50 to 80 mol %, The weight average molecular weight of the hydrogenated copolymer (b) is 350,000 or more, The hydrogenated copolymer (c) has a polymer block C1 containing 80% by mass or more of vinyl aromatic monomer units and a polymer block C2 containing 80% by mass or more of conjugated diene monomer units, the amount of vinyl bonds in the polymer block C2 before hydrogenation is less than 50 mol %, The weight average molecular weight of the hydrogenated copolymer (c) is 250,000 or more, Relative to 100 parts by mass of the hydrogenated copolymer (b) and the hydrogenated copolymer (c), 1 to 99 parts by mass of the hydrogenated copolymer (b); 1 to 99 parts by mass of the hydrogenated copolymer (c); 5 to 200 parts by mass of the hydrogenated copolymer (a); A thermoplastic elastomer composition comprising:

2. The content of vinyl aromatic monomer units in the hydrogenated copolymer (b) is 10 to 29% by mass. The thermoplastic elastomer composition according to claim 1 .

3. A molded article of the thermoplastic elastomer composition according to claim 1 or 2.

Citation Information

Patent Citations

  • Thermoplastic elastomer composition, extrusion molded article, and medical tube

    US20190309157A1

  • Hydrogenated copolymer and composition thereof

    WO2004003027A1

  • Block copolymer composition for flexographic printing plate

    WO2019188604A1