Resin composition and molded article thereof
A resin composition with a copolymer of polycarbonate, aromatic vinyl monomer, and diene-based rubbery polymer, combined with isobutylene-based block copolymer and oxidized polyethylene wax, addresses the issues of impact resistance, fluidity, heat resistance, chemical resistance, and noise suppression in automobile and electronic components.
Patent Information
- Application Number
- JP2023549405
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2021-09-24
- Filing Date
- 2022-08-09
- Publication Date
- 2024-12-06
- Estimated Expiration
- 2042-08-09
AI Technical Summary
Existing resin compositions used in automobile parts and electronic equipment suffer from insufficient impact resistance, fluidity, heat resistance, chemical resistance, and appearance, while also generating abnormal noise when rubbed together, and existing noise suppression methods do not adequately address these issues without compromising mechanical properties.
A resin composition comprising a copolymer of polycarbonate resin, aromatic vinyl monomer, vinyl cyanide monomer, and diene-based rubbery polymer, with a graft copolymer and isobutylene-based block copolymer, along with oxidized polyethylene wax, to enhance impact resistance, fluidity, heat resistance, chemical resistance, and noise suppression.
The resin composition achieves excellent impact resistance, fluidity, heat resistance, chemical resistance, and effective noise suppression, making it suitable for automobile and electronic components with improved mechanical properties and appearance.
Smart Images

Figure 0007595780000001 
Figure 0007595780000002 
Figure 0007595780000003
Abstract
Description
[Technical field]
[0001] The present invention relates to a resin composition and a molded article thereof, and more particularly to a resin composition having excellent impact resistance, fluidity, heat resistance, chemical resistance, and good molded article appearance, and having a high effect of suppressing abnormal noise when the molded article is rubbed against another molded article, and a molded article thereof. [Background technology]
[0002] Polycarbonate resin has excellent mechanical and thermal properties, and is therefore used in a variety of applications, mainly in the fields of automobiles, office automation equipment, and electronic and electrical equipment. In addition, alloy resins obtained by blending polycarbonate resin with ABS resin or AS resin are used for applications such as automobile parts, printer parts, personal computer housings, and computer parts, taking advantage of their excellent fluidity. In recent years, particularly in the automobile field, the use of resin materials as interior materials has increased for the purpose of weight reduction, and abnormal noises generated when resin parts vibrate as the automobile is driven and rub against each other have become a problem. For this reason, studies have been made on imparting abnormal noise suppression effects to resins. Examples of methods for imparting abnormal noise suppression effects to resin materials include a method of blending an organosilicon compound with an alloy resin obtained by blending polycarbonate resin with ABS resin (see Patent Document 1), a method of blending silicone oil with ABS resin (see Patent Document 2), and a method of blending silane-modified polyethylene resin with polycarbonate resin (see Patent Document 3). However, these methods are not effective in suppressing abnormal noise sufficiently, and there are problems such as the deterioration of the mechanical properties and appearance of the resin material due to the blending. [Prior art documents] [Patent documents]
[0003] [Patent Document 1] Special Publication No. 63-56267 [Patent Document 2] Patent No. 2798396 [Patent Document 3] Japanese Patent Application Publication No. 5-247236 Summary of the Invention [Problem to be solved by the invention]
[0004] An object of the present invention is to provide a resin composition having excellent impact resistance, fluidity, heat resistance, chemical resistance and good molded article appearance, and having a high effect of suppressing abnormal noise when the molded article is rubbed against another molded article, and to provide a molded article made of the same. [Means for solving the problem]
[0005] As a result of intensive research to solve the above-mentioned problems, the inventors have found that by adding a graft copolymer in which the side chains are copolymerized with aromatic vinyl monomers and other vinyl monomers and the main chain is an ethylene-vinyl acetate copolymer, and an isobutylene-based block copolymer polymerized with a monomer mainly composed of isobutylene and a monomer not mainly composed of isobutylene, to a component consisting of a copolymer obtained by polymerizing a polycarbonate resin and an aromatic vinyl monomer, a vinyl cyanide monomer, and a diene-based rubber polymer, it is possible to obtain a resin composition and a molded article thereof which have excellent impact resistance, fluidity, heat resistance, chemical resistance, and good molded article appearance, and which are highly effective in suppressing abnormal noise when the molded article is rubbed against each other.
[0006] That is, the present invention is as follows. [1] A resin composition comprising 100 parts by weight of a component consisting of (A) 45 to 90 parts by weight of a polycarbonate resin (component A) and (B) 10 to 55 parts by weight of a copolymer (component B) obtained by polymerizing an aromatic vinyl monomer, a vinyl cyanide monomer, and a diene-based rubber polymer, with respect to 1 to 10 parts by weight of (C) a graft copolymer (component C) whose side chains are copolymerized with an aromatic vinyl monomer and other vinyl monomers and whose main chain is an ethylene-vinyl acetate copolymer, and 1 to 10 parts by weight of (D) an isobutylene-based block copolymer (component D) obtained by polymerizing a monomer mainly composed of isobutylene and a monomer not mainly composed of isobutylene.
[0007] [2] The resin composition according to the above [1], further comprising 0.05 to 1.5 parts by weight of (E) oxidized polyethylene wax (component E) per 100 parts by weight of the components consisting of components A and B.
[0008] [3] The resin composition according to the above [1] or [2], wherein component B is an ABS resin.
[0009] [4] The resin composition according to any one of the above [1] to [3], wherein component D is a styrene-isobutylene-styrene block copolymer.
[0010] [5] A molded article made of the resin composition according to any one of [1] to [4] above.
[0011] [6] The molded article according to the above [5], wherein the molded article is an automotive part. Effect of the Invention
[0012] INDUSTRIAL APPLICABILITY The resin composition of the present invention has excellent impact resistance, fluidity, heat resistance, chemical resistance and good appearance of molded products, and is highly effective in suppressing abnormal noises when molded products are rubbed together. Therefore, the resin composition can be suitably used as components in the fields of automobiles, office automation equipment, home appliances, electrical and electronics, etc., and is particularly suitable for automobile components, and the industrial effects thereof are exceptional. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0013] The above-mentioned problem to be solved by the present invention can be achieved by a resin composition characterized by containing, per 100 parts by weight of a component consisting of (A) 45 to 90 parts by weight of a polycarbonate resin (component A) and (B) 10 to 55 parts by weight of a copolymer (component B) obtained by polymerizing an aromatic vinyl monomer, a vinyl cyanide monomer, and a diene-based rubber polymer, 1 to 10 parts by weight of (C) a graft copolymer (component C) whose side chains are formed by polymerizing an aromatic vinyl monomer and other vinyl monomers and whose main chain is an ethylene-vinyl acetate copolymer, and 1 to 10 parts by weight of (D) an isobutylene-based block copolymer (component D) obtained by polymerizing a monomer having isobutylene as a main component and a monomer not having isobutylene as a main component.
[0014] Each of the components of the present invention will be described in detail below. (Component A: polycarbonate resin) The polycarbonate resin used in the present invention is obtained by reacting a dihydric phenol with a carbonate precursor. Examples of the reaction method include an interfacial polymerization method, a melt transesterification method, a solid-phase transesterification method of a carbonate prepolymer, and a ring-opening polymerization method of a cyclic carbonate compound.
[0015] Representative examples of the dihydric phenols used herein include hydroquinone, resorcinol, 4,4'-biphenol, 1,1-bis(4-hydroxyphenyl)ethane, 2,2-bis(4-hydroxyphenyl)propane (commonly known as bisphenol A), 2,2-bis(4-hydroxy-3-methylphenyl)propane, 2,2-bis(4-hydroxyphenyl)butane, 1,1-bis(4-hydroxyphenyl)-1-phenylethane, 1,1-bis(4-hydroxyphenyl)cyclohexane, 1,1-bis(4-hydroxyphenyl)-3,3,5-trimethylcyclohexane, 2,2-bis(4-hydroxyphenyl)pentane, 4,4'-(p-phenylene) Examples of the dihydric phenol include 4,4'-(m-phenylenediisopropylidene)diphenol, 1,1-bis(4-hydroxyphenyl)-4-isopropylcyclohexane, bis(4-hydroxyphenyl)oxide, bis(4-hydroxyphenyl)sulfide, bis(4-hydroxyphenyl)sulfoxide, bis(4-hydroxyphenyl)sulfone, bis(4-hydroxyphenyl)ketone, bis(4-hydroxyphenyl)ester, bis(4-hydroxy-3-methylphenyl)sulfide, 9,9-bis(4-hydroxyphenyl)fluorene, and 9,9-bis(4-hydroxy-3-methylphenyl)fluorene. The preferred dihydric phenol is a bis(4-hydroxyphenyl)alkane, and among them, bisphenol A is particularly preferred from the viewpoint of impact resistance and is widely used.
[0016] In the present invention, in addition to bisphenol A-based polycarbonates, which are general-purpose polycarbonates, it is possible to use special polycarbonates produced using other dihydric phenols as the A component.
[0017] For example, polycarbonates (homopolymers or copolymers) using 4,4'-(m-phenylenediisopropylidene)diphenol (hereinafter sometimes abbreviated as "BPM"), 1,1-bis(4-hydroxyphenyl)cyclohexane, 1,1-bis(4-hydroxyphenyl)-3,3,5-trimethylcyclohexane (hereinafter sometimes abbreviated as "Bis-TMC"), 9,9-bis(4-hydroxyphenyl)fluorene and 9,9-bis(4-hydroxy-3-methylphenyl)fluorene (hereinafter sometimes abbreviated as "BCF") as part or all of the dihydric phenol components are suitable for applications where dimensional changes due to water absorption and dimensional stability are particularly demanding. These dihydric phenols other than BPA are preferably used in an amount of 5 mol% or more, particularly 10 mol% or more, of the total dihydric phenol components constituting the polycarbonate.
[0018] In particular, when high rigidity and better hydrolysis resistance are required, it is particularly suitable that the component A constituting the resin composition is a copolymer polycarbonate of the following (1) to (3).
[0019] (1) A copolymer polycarbonate in which, relative to 100 mol % of the dihydric phenol component constituting the polycarbonate, BPM is 20 to 80 mol % (more preferably 40 to 75 mol %, and even more preferably 45 to 65 mol %) and BCF is 20 to 80 mol % (more preferably 25 to 60 mol %, and even more preferably 35 to 55 mol %).
[0020] (2) A copolymer polycarbonate in which, relative to 100 mol % of the dihydric phenol component constituting the polycarbonate, BPA is 10 to 95 mol % (more preferably 50 to 90 mol %, and even more preferably 60 to 85 mol %) and BCF is 5 to 90 mol % (more preferably 10 to 50 mol %, and even more preferably 15 to 40 mol %).
[0021] (3) A copolymer polycarbonate in which, relative to 100 mol % of the dihydric phenol component constituting the polycarbonate, BPM is 20 to 80 mol % (more preferably 40 to 75 mol %, and even more preferably 45 to 65 mol %) and Bis-TMC is 20 to 80 mol % (more preferably 25 to 60 mol %, and even more preferably 35 to 55 mol %).
[0022] These special polycarbonates may be used alone or in a suitable mixture of two or more kinds, or may be used in a mixture with the commonly used bisphenol A type polycarbonate.
[0023] The production methods and properties of these special polycarbonates are described in detail in, for example, JP-A-6-172508, JP-A-8-27370, JP-A-2001-55435 and JP-A-2002-117580.
[0024] Among the various polycarbonates mentioned above, those in which the copolymer composition and the like are adjusted to bring the water absorption rate and Tg (glass transition temperature) into the ranges described below have good hydrolysis resistance of the polymer itself and are also remarkably excellent in terms of low warpage after molding, and are therefore particularly suitable in fields where dimensional stability is required. (i) a polycarbonate having a water absorption rate of 0.05 to 0.15%, preferably 0.06 to 0.13%, and a Tg of 120 to 180° C., or (ii) Polycarbonate having a Tg of 160 to 250° C., preferably 170 to 230° C., and a water absorption of 0.10 to 0.30%, preferably 0.13 to 0.30%, more preferably 0.14 to 0.27%.
[0025] The water absorption rate of polycarbonate is a value measured by using a disk-shaped test piece having a diameter of 45 mm and a thickness of 3.0 mm and measuring the moisture content after immersing it in water at 23°C for 24 hours in accordance with ISO62-1980. Also, Tg (glass transition temperature) is a value determined by differential scanning calorimetry (DSC) measurement in accordance with JIS K7121.
[0026] The carbonate precursor may be a carbonyl halide, a carbonic acid diester or a haloformate, and specific examples thereof include phosgene, diphenyl carbonate or a dihaloformate of a dihydric phenol.
[0027] When the aromatic polycarbonate resin is produced by the interfacial polymerization method of the dihydric phenol and the carbonate precursor, a catalyst, a terminal terminator, an antioxidant for preventing the oxidation of the dihydric phenol, etc. may be used as necessary. The aromatic polycarbonate resin of the present invention includes a branched polycarbonate resin copolymerized with a polyfunctional aromatic compound having three or more functionalities, a polyester carbonate resin copolymerized with an aromatic or aliphatic (including alicyclic) bifunctional carboxylic acid, a copolymerized polycarbonate resin copolymerized with a bifunctional alcohol (including alicyclic), and a polyester carbonate resin copolymerized with such a bifunctional carboxylic acid and a bifunctional alcohol. The aromatic polycarbonate resin may also be a mixture of two or more of the obtained aromatic polycarbonate resins.
[0028] The branched polycarbonate resin can impart drip prevention properties to the resin composition of the present invention. Examples of trifunctional or higher polyfunctional aromatic compounds used in such branched polycarbonate resins include phloroglucin, phloroglucide, 4,6-dimethyl-2,4,6-tris(4-hydroxyphenyl)heptene-2,2,4,6-trimethyl-2,4,6-tris(4-hydroxyphenyl)heptane, 1,3,5-tris(4-hydroxyphenyl)benzene, 1,1,1-tris(4-hydroxyphenyl)ethane, 1,1,1-tris(3,5-dimethyl-4-hydroxyphenyl)ethane, 2,6-bis(2-hydroxy-5-methylbenzyl)-4-methylphenol, 4-{4-[1,1-bis(4- Examples of the trisphenols include trisphenols such as 1,4-dimethylbenzylphenol, tetra(4-hydroxyphenyl)methane, bis(2,4-dihydroxyphenyl)ketone, 1,4-bis(4,4-dihydroxytriphenylmethyl)benzene, trimellitic acid, pyromellitic acid, benzophenonetetracarboxylic acid, and acid chlorides thereof. Among these, 1,1,1-tris(4-hydroxyphenyl)ethane and 1,1,1-tris(3,5-dimethyl-4-hydroxyphenyl)ethane are preferred, and 1,1,1-tris(4-hydroxyphenyl)ethane is particularly preferred.
[0029] The constituent units derived from a polyfunctional aromatic compound in the branched polycarbonate preferably account for 0.01 to 1 mol %, more preferably 0.05 to 0.9 mol %, and even more preferably 0.05 to 0.8 mol %, based on a total of 100 mol % of the constituent units derived from a dihydric phenol and the constituent units derived from such a polyfunctional aromatic compound.
[0030] In particular, in the case of the melt transesterification method, branched structural units may be generated as a side reaction, and the amount of such branched structural units is preferably 0.001 to 1 mol %, more preferably 0.005 to 0.9 mol %, and even more preferably 0.01 to 0.8 mol %, based on the total of 100 mol % including the structural units derived from the dihydric phenol.1 It can be calculated by H-NMR measurement.
[0031] The aliphatic difunctional carboxylic acid is preferably an α,ω-dicarboxylic acid. Examples of the aliphatic difunctional carboxylic acid include linear saturated aliphatic dicarboxylic acids such as sebacic acid (decanedioic acid), dodecanedioic acid, tetradecanedioic acid, octadecanedioic acid, and icosane diacid, and alicyclic dicarboxylic acids such as cyclohexane dicarboxylic acid. The bifunctional alcohol is more preferably an alicyclic diol, such as cyclohexane dimethanol, cyclohexane diol, and tricyclodecane dimethanol.
[0032] The reaction modes of the method for producing the polycarbonate resin of the present invention, such as the interfacial polymerization method, the melt transesterification method, the carbonate prepolymer solid-phase transesterification method, and the ring-opening polymerization method of a cyclic carbonate compound, are well known in various literatures and patent publications.
[0033] In producing the resin composition of the present invention, the viscosity average molecular weight (M) of the polycarbonate resin is not particularly limited, but is preferably 1.8×10 4 ~4.0×10 4 and more preferably 2.0×10 4 ~3.5×10 4 , and more preferably 2.2×10 4 ~3.0×10 4 The viscosity average molecular weight is 1.8 × 10 4 Polycarbonate resins with a viscosity average molecular weight of less than 4.0×10 may not provide good mechanical properties. 4 Resin compositions obtained from polycarbonate resins exceeding this limit are inferior in terms of flowability during injection molding and therefore are inferior in versatility.
[0034] The polycarbonate resin may be a mixture of polycarbonate resins having a viscosity average molecular weight outside the above range. 4) the entropy elasticity of the resin is improved. As a result, good molding processability is exhibited in gas-assisted molding and foam molding, which are sometimes used when molding reinforced resin materials into structural members. Such improvement in molding processability is even better than that of the branched polycarbonate. In a more preferred embodiment, component A has a viscosity average molecular weight of 7×10 4 ~3×10 5 Polycarbonate resin (A-1-1 component) and viscosity average molecular weight 1 × 10 4 ~3×10 4 The aromatic polycarbonate resin (A-1-2 component) has a viscosity average molecular weight of 1.6×10 4 ~3.5×10 4 A polycarbonate resin (A-1 component) (hereinafter, sometimes referred to as a "polycarbonate resin containing a high molecular weight component") can also be used.
[0035] In the polycarbonate resin containing a high molecular weight component (A-1 component), the molecular weight of the A-1-1 component is 7×10 4 ~2×10 5 is preferable, and more preferably 8×10 4 ~2×10 5 , and more preferably 1×10 5 ~2×10 5 , particularly preferably 1×10 5 ~1.6×10 5 The molecular weight of component A-1-2 is 1×10 4 ~2.5×10 4 is preferable, and more preferably 1.1×10 4 ~2.4×10 4 , and more preferably 1.2×10 4 ~2.4×10 4 , and particularly preferably 1.2×10 4 ~2.3×10 4 It is.
[0036] The high molecular weight component-containing polycarbonate resin (A-1 component) can be obtained by mixing the A-1-1 component and the A-1-2 component in various ratios and adjusting to satisfy a predetermined molecular weight range. Preferably, the A-1-1 component is 2 to 40% by weight, more preferably 3 to 30% by weight, even more preferably 4 to 20% by weight, and particularly preferably 5 to 20% by weight, of 100% by weight of the A-1 component.
[0037] Methods for preparing component A-1 include (1) independently polymerizing components A-1-1 and A-1-2 and mixing them, (2) using a method for producing an aromatic polycarbonate resin that shows multiple polymer peaks in a molecular weight distribution chart by GPC method, in the same system, as typified by the method shown in JP-A-5-306336, to produce such an aromatic polycarbonate resin so as to satisfy the conditions of component A-1 of the present invention, and (3) mixing an aromatic polycarbonate resin obtained by such a production method (production method (2)) with components A-1-1 and / or A-1-2 that have been produced separately.
[0038] The viscosity average molecular weight in the present invention is calculated by the specific viscosity (η SP ) was measured at 20°C using an Ostwald viscometer from a solution of 0.7 g of polycarbonate dissolved in 100 ml of methylene chloride. Specific viscosity (η SP )=(t-t0) / t0 [t0 is the number of seconds that methylene chloride falls, and t is the number of seconds that the sample solution falls] The specific viscosity (η SP ) and calculate the viscosity average molecular weight M using the following formula: η SP / c=[η]+0.45×[η] 2 c (where [η] is the intrinsic viscosity) [η]=1.23×10 -4 M 0.83 c=0.7
[0039] The viscosity average molecular weight of the polycarbonate resin in the resin composition of the present invention is calculated as follows. That is, the composition is mixed with methylene chloride in an amount 20 to 30 times its weight, and the soluble matter in the composition is dissolved. The soluble matter is collected by celite filtration. The solvent in the resulting solution is then removed. The solid after the solvent removal is thoroughly dried to obtain a solid of components that dissolve in methylene chloride. 0.7 g of the solid is dissolved in 100 ml of methylene chloride, and the specific viscosity at 20°C is determined in the same manner as above, and the viscosity average molecular weight M is calculated from the specific viscosity in the same manner as above.
[0040] A polycarbonate-polydiorganosiloxane copolymer resin can also be used as the polycarbonate resin (component A) of the present invention. The polycarbonate-polydiorganosiloxane copolymer resin is preferably a copolymer resin prepared by copolymerizing a dihydric phenol represented by the following general formula (1) and a hydroxyaryl-terminated polydiorganosiloxane represented by the following general formula (3).
[0041] [ka] [In the above general formula (1), R 1 and R 2 each independently represents a group selected from the group consisting of a hydrogen atom, a halogen atom, an alkyl group having 1 to 18 carbon atoms, an alkoxy group having 1 to 18 carbon atoms, a cycloalkyl group having 6 to 20 carbon atoms, a cycloalkoxy group having 6 to 20 carbon atoms, an alkenyl group having 2 to 10 carbon atoms, an aryl group having 6 to 14 carbon atoms, an aryloxy group having 6 to 14 carbon atoms, an aralkyl group having 7 to 20 carbon atoms, an aralkyloxy group having 7 to 20 carbon atoms, a nitro group, an aldehyde group, a cyano group, and a carboxyl group, and when there are a plurality of each, they may be the same or different, e and f each represent an integer of 1 to 4, and W represents a single bond or at least one group selected from the group consisting of groups represented by the following general formula (2):
[0042] [ka] [In the above general formula (2), R 11 ,R 12 ,R 13 ,R 14 ,R 15 ,R 16 ,R 17 and R 18 each independently represents a group selected from the group consisting of a hydrogen atom, an alkyl group having 1 to 18 carbon atoms, an aryl group having 6 to 14 carbon atoms, and an aralkyl group having 7 to 20 carbon atoms; R 19 and R 20 each independently represents a group selected from the group consisting of a hydrogen atom, a halogen atom, an alkyl group having 1 to 18 carbon atoms, an alkoxy group having 1 to 10 carbon atoms, a cycloalkyl group having 6 to 20 carbon atoms, a cycloalkoxy group having 6 to 20 carbon atoms, an alkenyl group having 2 to 10 carbon atoms, an aryl group having 6 to 14 carbon atoms, an aryloxy group having 6 to 10 carbon atoms, an aralkyl group having 7 to 20 carbon atoms, an aralkyloxy group having 7 to 20 carbon atoms, a nitro group, an aldehyde group, a cyano group, and a carboxyl group, and when there are a plurality of groups, they may be the same or different, g is an integer from 1 to 10, and h is an integer from 4 to 7.
[0043] [ka] [In the above general formula (3), R 3 , R 4 , R 5 , R 6 , R 7 and R 8 are each independently a hydrogen atom, an alkyl group having 1 to 12 carbon atoms, or a substituted or unsubstituted aryl group having 6 to 12 carbon atoms; R 9 and R 10 are each independently a hydrogen atom, a halogen atom, an alkyl group having 1 to 10 carbon atoms, or an alkoxy group having 1 to 10 carbon atoms, p is a natural number, q is 0 or a natural number, and p+q is a natural number of 10 to 300. X is a divalent aliphatic group having 2 to 8 carbon atoms.]
[0044] Examples of the dihydric phenol (I) represented by the general formula (1) include 4,4'-dihydroxybiphenyl, bis(4-hydroxyphenyl)methane, 1,1-bis(4-hydroxyphenyl)ethane, 1,1-bis(4-hydroxyphenyl)-1-phenylethane, 2,2-bis(4-hydroxyphenyl)propane, 2,2-bis(4-hydroxy-3-methylphenyl)propane, 1,1-bis(4-hydroxyphenyl)-3,3,5-trimethylcyclohexane, 2,2-bis(4-hydroxy-3,3'-biphenyl)propane, 2,2- Bis(4-hydroxy-3-isopropylphenyl)propane, 2,2-bis(3-t-butyl-4-hydroxyphenyl)propane, 2,2-bis(4-hydroxyphenyl)butane, 2,2-bis(4-hydroxyphenyl)octane, 2,2-bis(3-bromo-4-hydroxyphenyl)propane, 2,2-bis(3,5-dimethyl-4-hydroxyphenyl)propane, 2,2-bis(3-cyclohexyl-4-hydroxyphenyl)propane, 1,1-bis(3-cyclohexyl-4-hydroxyphenyl)cyclohexane, bis(4-hydroxyphenyl)propane, 4,4'-dihydroxydiphenylmethane, 9,9-bis(4-hydroxyphenyl)fluorene, 9,9-bis(4-hydroxy-3-methylphenyl)fluorene, 1,1-bis(4-hydroxyphenyl)cyclohexane, 1,1-bis(4-hydroxyphenyl)cyclopentane, 4,4'-dihydroxydiphenyl ether, 4,4'-dihydroxy-3,3'-dimethyldiphenyl ether, 4,4'-sulfonyldiphenol, 4,4'-dihydroxydiphenyl sulfoxide, 4,4'-dihydroxydiphenyl sulfide, 2,2'- Dimethyl-4,4'-sulfonyldiphenol, 4,4'-dihydroxy-3,3'-dimethyldiphenyl sulfoxide, 4,4'-dihydroxy-3,3'-dimethyldiphenyl sulfide, 2,2'-diphenyl-4,4'-sulfonyldiphenol, 4,4'-dihydroxy-3,3'-diphenyldiphenyl sulfoxide, 4,4'-dihydroxy-3,3'-diphenyldiphenyl sulfide, 1,3-bis{2-(4-hydroxyphenyl)propyl}benzene, 1,4-bis{2-(4-hydroxyphenyl)propyl}benzene, 1,Examples of the cyclohexane derivatives include 4-bis(4-hydroxyphenyl)cyclohexane, 1,3-bis(4-hydroxyphenyl)cyclohexane, 4,8-bis(4-hydroxyphenyl)tricyclo[5.2.1.02,6]decane, 4,4'-(1,3-adamantanediyl)diphenol, and 1,3-bis(4-hydroxyphenyl)-5,7-dimethyladamantane.
[0045] Among these, 1,1-bis(4-hydroxyphenyl)-1-phenylethane, 2,2-bis(4-hydroxyphenyl)propane, 2,2-bis(4-hydroxy-3-methylphenyl)propane, 1,1-bis(4-hydroxyphenyl)cyclohexane, 1,1-bis(4-hydroxyphenyl)-3,3,5-trimethylcyclohexane, 4,4'-sulfonyldiphenol, 2,2'-dimethyl-4,4'-sulfonyldiphenol, 9,9-bis(4-hydroxy-3-methylphenyl)fluorene, 1,3-bis{2-(4-hydroxyphenyl)propyl}benzene, and 1,4-bis{2-(4-hydroxyphenyl)propyl}benzene are preferred, and 2,2-bis(4-hydroxyphenyl)propane, 1,1-bis(4-hydroxyphenyl)cyclohexane (BPZ), 4,4'-sulfonyldiphenol, and 9,9-bis(4-hydroxy-3-methylphenyl)fluorene are particularly preferred. Among these, 2,2-bis(4-hydroxyphenyl)propane, which has excellent strength and good durability, is most suitable. These may be used alone or in combination of two or more kinds.
[0046] As the hydroxyaryl-terminated polydiorganosiloxane represented by the above general formula (3), for example, the compounds shown below are suitably used.
[0047] [ka]
[0048] Hydroxyaryl-terminated polydiorganosiloxane (II) is easily produced by hydrosilylation reaction of phenols having an olefinic unsaturated carbon-carbon bond, preferably vinylphenol, 2-allylphenol, isopropenylphenol, or 2-methoxy-4-allylphenol, with the end of a polysiloxane chain having a predetermined degree of polymerization. Among them, (2-allylphenol)-terminated polydiorganosiloxane and (2-methoxy-4-allylphenol)-terminated polydiorganosiloxane are preferred, and (2-allylphenol)-terminated polydimethylsiloxane and (2-methoxy-4-allylphenol)-terminated polydimethylsiloxane are particularly preferred. The molecular weight distribution (Mw / Mn) of the hydroxyaryl-terminated polydiorganosiloxane (II) is preferably 3 or less. In order to achieve even better low outgassing properties during high-temperature molding and low-temperature impact properties, the molecular weight distribution (Mw / Mn) is more preferably 2.5 or less, and even more preferably 2 or less. If the upper limit of this preferred range is exceeded, the amount of outgassing during high-temperature molding will be large, and low-temperature impact resistance may be poor.
[0049] Furthermore, in order to achieve a high level of impact resistance, the diorganosiloxane polymerization degree (p+q) of the hydroxyaryl-terminated polydiorganosiloxane (II) is suitably 10 to 300. The diorganosiloxane polymerization degree (p+q) is preferably 10 to 200, more preferably 12 to 150, and even more preferably 14 to 100. Below the lower limit of this preferred range, the impact resistance that is a characteristic of the polycarbonate-polydiorganosiloxane copolymer is not effectively exhibited, while above the upper limit of this preferred range, poor appearance appears.
[0050] The polydiorganosiloxane content in the total weight of the polycarbonate-polydiorganosiloxane copolymer resin used in component A is preferably 0.1 to 50% by weight. The polydiorganosiloxane content is more preferably 0.5 to 30% by weight, and even more preferably 1 to 20% by weight. At or above the lower limit of this preferred range, excellent impact resistance and flame retardancy are obtained, while at or below the upper limit of this preferred range, a stable appearance that is not easily affected by molding conditions is easily obtained. The polydiorganosiloxane polymerization degree and polydiorganosiloxane content are 1 It can be calculated by H-NMR measurement.
[0051] In the present invention, the hydroxyaryl-terminated polydiorganosiloxane (II) may be used alone or in combination of two or more kinds.
[0052] In addition, as long as it does not interfere with the present invention, other comonomers than the dihydric phenol (I) and hydroxyaryl-terminated polydiorganosiloxane (II) can be used in an amount of up to 10% by weight based on the total weight of the copolymer.
[0053] In the present invention, a mixed solution containing an oligomer having a terminal chloroformate group is prepared in advance by reacting a dihydric phenol (I) with a carbonate-forming compound in a mixed solution of a water-insoluble organic solvent and an aqueous alkaline solution.
[0054] In producing an oligomer of the dihydric phenol (I), the entire amount of the dihydric phenol (I) used in the method of the present invention may be converted into an oligomer at once, or a part of it may be added as a post-added monomer as a reaction raw material to the interfacial polycondensation reaction in the latter stage. The post-added monomer is added to quickly advance the polycondensation reaction in the latter stage, and there is no need to add it if it is not necessary.
[0055] The method of this oligomer formation reaction is not particularly limited, but it is usually preferable to carry out the reaction in a solvent in the presence of an acid binder.
[0056] The proportion of the carbonate ester-forming compound used may be appropriately adjusted in consideration of the stoichiometric ratio (equivalent) of the reaction. When a gaseous carbonate ester-forming compound such as phosgene is used, it is preferable to employ a method of blowing the gaseous compound into the reaction system.
[0057] As the acid binder, for example, an alkali metal hydroxide such as sodium hydroxide or potassium hydroxide, an alkali metal carbonate such as sodium carbonate or potassium carbonate, an organic base such as pyridine, or a mixture thereof can be used. The proportion of the acid binder used can be appropriately determined in consideration of the stoichiometric ratio (equivalent) of the reaction, as described above. Specifically, it is preferable to use 2 equivalents or a slightly excess amount of the acid binder relative to the number of moles of the dihydric phenol (I) used to form the oligomer (usually 1 mole corresponds to 2 equivalents).
[0058] As the solvent, a solvent inert to various reactions, such as those used in the production of known polycarbonates, may be used alone or as a mixed solvent. Representative examples include hydrocarbon solvents such as xylene, and halogenated hydrocarbon solvents such as methylene chloride and chlorobenzene. In particular, halogenated hydrocarbon solvents such as methylene chloride are preferably used.
[0059] The reaction pressure for oligomer formation is not particularly limited, and may be normal pressure, elevated pressure, or reduced pressure, but it is usually advantageous to carry out the reaction under normal pressure. The reaction temperature is selected from the range of -20 to 50°C, and since heat is generated during polymerization in many cases, it is desirable to cool the reaction with water or ice. The reaction time depends on other conditions and cannot be generally specified, but is usually carried out for 0.2 to 10 hours. The pH range for the oligomer formation reaction is the same as that of known interfacial reaction conditions, and the pH is always adjusted to 10 or higher.
[0060] In the present invention, after obtaining a mixed solution containing an oligomer of dihydric phenol (I) having terminal chloroformate groups in this manner, the mixed solution is stirred while adding hydroxyaryl-terminated polydiorganosiloxane (II) represented by general formula (3) that has been highly refined to a molecular weight distribution (Mw / Mn) of 3 or less to the dihydric phenol (I), and the hydroxyaryl-terminated polydiorganosiloxane (II) and the oligomer are subjected to interfacial polycondensation to obtain a polycarbonate-polydiorganosiloxane copolymer.
[0061] [ka] [In the above general formula (3), R 3 , R 4 , R 5 , R 6 , R 7 and R 8 are each independently a hydrogen atom, an alkyl group having 1 to 12 carbon atoms, or a substituted or unsubstituted aryl group having 6 to 12 carbon atoms; R 9 and R 10 are each independently a hydrogen atom, a halogen atom, an alkyl group having 1 to 10 carbon atoms, or an alkoxy group having 1 to 10 carbon atoms, p is a natural number, q is 0 or a natural number, and p+q is a natural number of 10 to 300. X is a divalent aliphatic group having 2 to 8 carbon atoms.]
[0062] In carrying out the interfacial polycondensation reaction, an acid binder may be appropriately added in consideration of the stoichiometric ratio (equivalent) of the reaction. For example, alkali metal hydroxides such as sodium hydroxide and potassium hydroxide, alkali metal carbonates such as sodium carbonate and potassium carbonate, organic bases such as pyridine, or mixtures thereof, are used as the acid binder. Specifically, when the hydroxyaryl-terminated polydiorganosiloxane (II) used or a part of the dihydric phenol (I) as described above is added to this reaction stage as a post-added monomer, it is preferable to use 2 equivalents or more of alkali relative to the total mole number of the post-added dihydric phenol (I) and the hydroxyaryl-terminated polydiorganosiloxane (II) (usually 1 mole corresponds to 2 equivalents).
[0063] The polycondensation by the interfacial polycondensation reaction between the oligomer of the dihydric phenol (I) and the hydroxyaryl-terminated polydiorganosiloxane (II) is carried out by vigorously stirring the above mixture.
[0064] In such a polymerization reaction, a terminal terminator or a molecular weight regulator is usually used. Examples of the terminal terminator include compounds having a monovalent phenolic hydroxyl group, such as ordinary phenol, p-tert-butylphenol, p-cumylphenol, tribromophenol, etc., as well as long-chain alkylphenols, aliphatic carboxylic acid chlorides, aliphatic carboxylic acids, hydroxybenzoic acid alkyl esters, hydroxyphenyl alkyl acid esters, and alkyl ether phenols. The amount of the terminal terminator is in the range of 100 to 0.5 mol, preferably 50 to 2 mol, relative to 100 mol of all dihydric phenol compounds used, and it is naturally possible to use two or more compounds in combination.
[0065] To accelerate the polycondensation reaction, a catalyst such as a tertiary amine, such as triethylamine, or a quaternary ammonium salt may be added.
[0066] The reaction time of such a polymerization reaction is preferably 30 minutes or more, more preferably 50 minutes or more. If desired, a small amount of an antioxidant such as sodium sulfite or hydrosulfide may be added.
[0067] A branching agent can be used in combination with the above dihydric phenol compound to produce a branched polycarbonate-polydiorganosiloxane. Examples of polyfunctional aromatic compounds having three or more functional groups that can be used in such branched polycarbonate-polydiorganosiloxane copolymer resins include phloroglucin, phloroglucide, 4,6-dimethyl-2,4,6-tris(4-hydroxyphenyl)heptene-2,2,4,6-trimethyl-2,4,6-tris(4-hydroxyphenyl)heptane, 1,3,5-tris(4-hydroxyphenyl)benzene, 1,1,1-tris(4-hydroxyphenyl)ethane, 1,1,1-tris(3,5-dimethyl-4-hydroxyphenyl)ethane, 2,6-bis(2-hydroxy-5-methylbenzyl)-4-methylphenol, 4-{4-[1 Examples of the hydroxyphenyl ether include trisphenols such as {α,α-dimethylbenzylphenol}-α-dimethylbenzylphenol, tetra(4-hydroxyphenyl)methane, bis(2,4-dihydroxyphenyl)ketone, 1,4-bis(4,4-dihydroxytriphenylmethyl)benzene, trimellitic acid, pyromellitic acid, benzophenonetetracarboxylic acid, and acid chlorides thereof. Among these, 1,1,1-tris(4-hydroxyphenyl)ethane and 1,1,1-tris(3,5-dimethyl-4-hydroxyphenyl)ethane are preferred, and 1,1,1-tris(4-hydroxyphenyl)ethane is particularly preferred. The proportion of the polyfunctional compound in the branched polycarbonate-polydiorganosiloxane copolymer resin is preferably 0.001 to 1 mol %, more preferably 0.005 to 0.9 mol %, further preferably 0.01 to 0.8 mol %, and particularly preferably 0.05 to 0.4 mol %, based on the total amount of the aromatic polycarbonate-polydiorganosiloxane copolymer resin. 1 It can be calculated by H-NMR measurement.
[0068] The reaction pressure may be reduced, normal, or increased, but is usually preferably normal pressure or the reaction system's own pressure. The reaction temperature is selected from the range of -20 to 50°C, and in many cases, since heat is generated during polymerization, it is desirable to cool the reaction system with water or ice. The reaction time varies depending on other conditions such as the reaction temperature and cannot be generally specified, but is usually carried out for 0.5 to 10 hours.
[0069] In some cases, the obtained polycarbonate-polydiorganosiloxane copolymer resin is subjected to a suitable physical treatment (mixing, fractionation, etc.) and / or chemical treatment (polymer reaction, crosslinking treatment, partial decomposition treatment, etc.) to obtain a desired reduced viscosity [η SP It can also be obtained as a polycarbonate-polydiorganosiloxane copolymer resin of formula [1 / c].
[0070] The resulting reaction product (crude product) can be subjected to various post-treatments such as known separation and purification methods to recover a polycarbonate-polydiorganosiloxane copolymer resin of a desired purity (degree of purification).
[0071] The average size of the polydiorganosiloxane domains in the polycarbonate-polydiorganosiloxane copolymer resin molded article is preferably in the range of 1 to 60 nm. Such an average size is more preferably 3 to 55 nm, and even more preferably 5 to 50 nm. Below the lower limit of such a suitable range, impact resistance and flame retardancy may not be sufficiently exhibited, and above the upper limit of such a suitable range, impact resistance may not be stably exhibited. This may provide a resin composition with excellent impact resistance and appearance.
[0072] (Component B: A copolymer obtained by polymerizing an aromatic vinyl monomer, a vinyl cyanide monomer, and a diene rubber polymer) The component B of the present invention is a copolymer obtained by polymerizing an aromatic vinyl monomer, a vinyl cyanide monomer, and a diene rubber polymer. The component B preferably comprises 40-80% by weight of an aromatic vinyl monomer, 10-30% by weight of a vinyl cyanide monomer, 10-50% by weight of a diene rubber polymer, and 0-30% by weight of other monomers.
[0073] Examples of aromatic vinyl monomers include styrene, α-methylstyrene, o-methylstyrene, p-methylstyrene, vinylxylene, ethylstyrene, dimethylstyrene, p-tert-butylstyrene, vinylnaphthalene, methoxystyrene, monobromostyrene, dibromostyrene, fluorostyrene, and tribromostyrene, with styrene being particularly preferred.
[0074] The proportion of the aromatic vinyl monomer in component B, relative to 100% by weight of component B, is more preferably 45% by weight, even more preferably 50% by weight, and particularly preferably 55% by weight, and the upper limit is more preferably 75% by weight, even more preferably 70% by weight, and particularly preferably 65% by weight.
[0075] Examples of the vinyl cyanide monomer include acrylonitrile and methacrylonitrile, with acrylonitrile being particularly preferred.
[0076] The proportion of the vinyl cyanide monomer in component B, relative to 100% by weight of component B, is more preferably 12% by weight, further preferably 14% by weight, and particularly preferably 15% by weight, and more preferably 28% by weight, further preferably 26% by weight, and particularly preferably 25% by weight.
[0077] As the diene rubbery polymer, for example, rubber components such as polybutadiene, polyisoprene, and styrene-butadiene copolymer are used, and the proportion of the diene rubbery polymer in component B, based on 100% by weight of component B, is more preferably 13% by weight at the lower end, even more preferably 14% by weight, and particularly preferably 15% by weight at the upper end, and more preferably 45% by weight at the upper end.
[0078] Furthermore, they may be copolymerized with other monomers copolymerizable therewith. In this case, examples of the other copolymerizable vinyl monomers include maleimide-based monomers such as maleimide, N-methylmaleimide, N-cyclohexylmaleimide, and N-phenylmaleimide, acrylamide-based monomers such as acrylamide and N-methylacrylamide, unsaturated acid anhydrides such as maleic anhydride and itaconic anhydride, unsaturated acids such as acrylic acid and methacrylic acid, glycidyl acrylate, glycidyl methacrylate, 2-hydroxyethyl acrylate, 2-hydroxyethyl methacrylate, and methoxypolyethylene glycol methacrylate.
[0079] The upper limit of the proportion of the other monomer in component B is more preferably 20% by weight, and even more preferably 10% by weight, based on 100% by weight of component B.
[0080] Specific preferred examples of component B include acrylonitrile-butadiene-styrene copolymer, acrylonitrile-butadiene-styrene-α-methylstyrene copolymer, acrylonitrile-butadiene-styrene-N-phenylmaleimide copolymer, etc., and among these, acrylonitrile-butadiene-styrene copolymer is preferred. These copolymers may be used alone or in combination of two or more.
[0081] Component B may be produced by any of the polymerization methods of bulk polymerization, solution polymerization, suspension polymerization, and emulsion polymerization, and the copolymerization method may be either one-stage grafting or multi-stage grafting. It may also be a mixture with a copolymer of only the graft component that is a by-product during production.
[0082] The content of component B is 10 to 55 parts by weight, preferably 15 to 45 parts by weight, and more preferably 20 to 35 parts by weight, per 100 parts by weight of the components consisting of components A and B. If the content of component B is less than 10 parts by weight, sufficient fluidity cannot be obtained, and if it exceeds 55 parts by weight, impact resistance and heat resistance decrease.
[0083] (Component C: a graft copolymer in which the side chain is a copolymer formed by polymerizing an aromatic vinyl monomer and other vinyl monomers, and the main chain is an ethylene-vinyl acetate copolymer) The component C of the present invention is a copolymer in which the side chains are formed by polymerizing an aromatic vinyl monomer and other vinyl monomers, and is a graft copolymer in which the main chain is an ethylene-vinyl acetate copolymer.
[0084] The proportion of vinyl acetate units in the ethylene-vinyl acetate copolymer which is the main chain is preferably 1 to 20% by weight, more preferably 3 to 10% by weight, based on 100% by weight of the ethylene-vinyl acetate copolymer.
[0085] Examples of aromatic vinyl monomers used in the side chain include styrene, α-methylstyrene, o-methylstyrene, p-methylstyrene, vinylxylene, ethylstyrene, dimethylstyrene, p-tert-butylstyrene, vinylnaphthalene, methoxystyrene, monobromostyrene, dibromostyrene, fluorostyrene, and tribromostyrene, with styrene being particularly preferred.
[0086] Other vinyl monomers used in the side chain include vinyl cyanide monomers, glycidyl esters of acrylic acid or methacrylic acid, and alkyl esters of acrylic acid or methacrylic acid. Examples of vinyl cyanide monomers include acrylonitrile and methacrylonitrile, with acrylonitrile being particularly preferred. Examples of glycidyl esters of acrylic acid or methacrylic acid include glycidyl esters of acrylic acid and glycidyl esters of methacrylic acid, with glycidyl esters of methacrylic acid being preferred. Examples of alkyl esters of acrylic acid or methacrylic acid include alkyl esters having 1 to 8 carbon atoms, with examples including methyl acrylate, n-butyl acrylate, isobutyl acrylate, t-butyl acrylate, 2-ethylhexyl acrylate, methyl methacrylate, ethyl methacrylate, n-butyl methacrylate, and isobutyl methacrylate.
[0087] As the other vinyl monomer, among the above, glycidyl esters of acrylic acid or methacrylic acid, and vinyl cyanide monomer are preferred, glycidyl esters of acrylic acid or methacrylic acid are more preferred, and glycidyl esters of methacrylic acid are particularly preferred.
[0088] The content of the aromatic vinyl monomer is preferably 50 to 100 parts by weight in 100 parts by weight of the total of the aromatic vinyl monomer and the other vinyl monomers.
[0089] The content of the side chain is preferably 10 to 50 parts by weight based on 100 parts by weight of the ethylene-vinyl acetate copolymer which is the main chain.
[0090] Component C can be produced by various known methods, including a preferred method in which an aromatic vinyl monomer, other vinyl monomers, and a radically polymerizable organic peroxide are mixed into an aqueous suspension of an ethylene-vinyl acetate copolymer to which a suspending agent has been added, and the mixture is heated and stirred to impregnate the ethylene-vinyl acetate copolymer with the above components, and then the mixture is heated to polymerize the components.
[0091] In addition, component C is commercially available and can be obtained, for example, by selecting from the NOF Corporation's "Modiper" series.
[0092] The content of component C is 1 to 10 parts by weight, preferably 2 to 8 parts by weight, and more preferably 2 to 6 parts by weight, based on 100 parts by weight of the components consisting of components A and B. If the content of component C is less than 1 part by weight, sufficient improvement in chemical resistance and suppression of abnormal noise cannot be obtained, whereas if it exceeds 10 parts by weight, impact resistance decreases and the appearance of the molded product also deteriorates.
[0093] (Component D: isobutylene-based block copolymer obtained by polymerizing a monomer mainly composed of isobutylene and a monomer not mainly composed of isobutylene) Component D of the present invention is an isobutylene-based block copolymer obtained by polymerizing a monomer mainly composed of isobutylene and a monomer other than isobutylene, and is not particularly limited as long as it has a unit composed of a monomer mainly composed of isobutylene and a unit composed of a monomer other than isobutylene, and for example, any of block copolymers having a linear, branched, star-shaped structure, diblock copolymers, triblock copolymers, multiblock copolymers, etc. can be selected. Note that, if a block copolymer other than the above is used as component D, sufficient chemical resistance improvement effect and abnormal noise suppression effect cannot be obtained. Preferred block copolymers, from the viewpoint of the balance of physical properties and the absorption capacity of softeners, include triblock copolymers consisting of units of monomer components other than isobutylene as the main component-units of monomer components mainly composed of isobutylene-units of monomer components other than isobutylene as the main component, diblock copolymers consisting of units of monomer components other than isobutylene as the main component-units of monomer components mainly composed of isobutylene, and star block copolymers having three or more arms consisting of units of monomer components other than isobutylene as the main component and units of monomer components mainly composed of isobutylene, etc. These can be used alone or in combination of two or more kinds to obtain the desired physical properties and molding processability.
[0094] A monomer not mainly composed of isobutylene is a monomer having an isobutylene content of 30% by weight or less.
[0095] In the present invention, the monomer other than isobutylene in the monomer component not mainly composed of isobutylene is not particularly limited as long as it is a monomer component capable of cationic polymerization, and examples thereof include monomers such as aliphatic olefins, aromatic vinyls, dienes, vinyl ethers, silanes, vinylcarbazole, β-pinene, acenaphthylene, etc. These are used alone or in combination of two or more.
[0096] Examples of the aliphatic olefin monomer include ethylene, propylene, 1-butene, 2-methyl-1-butene, 3-methyl-1-butene, pentene, hexene, cyclohexene, 4-methyl-1-pentene, vinylcyclohexane, octene, and norbornene.
[0097] Examples of aromatic vinyl monomers include styrene, o-, m-, or p-methylstyrene, α-methylstyrene, β-methylstyrene, 2,6-dimethylstyrene, 2,4-dimethylstyrene, α-methyl-o-methylstyrene, α-methyl-m-methylstyrene, α-methyl-p-methylstyrene, β-methyl-o-methylstyrene, β-methyl-m-methylstyrene, β-methyl-p-methylstyrene, 2,4,6-trimethylstyrene, α-methyl-2,6-dimethylstyrene, α-methyl-2,4-dimethylstyrene, β-methyl-2,6-dimethylstyrene, β-methyl-2,4-dimethylstyrene, o-, m-, or p-chlorostyrene, 2,6-dichlorostyrene, 2,4-dichloros Examples of the styrene-substituted styrene include styrene, α-chloro-o-chlorostyrene, α-chloro-m-chlorostyrene, α-chloro-p-chlorostyrene, β-chloro-o-chlorostyrene, β-chloro-m-chlorostyrene, β-chloro-p-chlorostyrene, 2,4,6-trichlorostyrene, α-chloro-2,6-dichlorostyrene, α-chloro-2,4-dichlorostyrene, β-chloro-2,6-dichlorostyrene, β-chloro-2,4-dichlorostyrene, o-, m-, or pt-butylstyrene, o-, m-, or p-methoxystyrene, o-, m-, or p-chloromethylstyrene, o-, m-, or p-bromomethylstyrene, styrene derivatives substituted with a silyl group, indene, and vinylnaphthalene.
[0098] Examples of the diene monomer include butadiene, isoprene, hexadiene, cyclopentadiene, cyclohexadiene, dicyclopentadiene, divinylbenzene, and ethylidenenorbornene.
[0099] Examples of the vinyl ether monomer include methyl vinyl ether, ethyl vinyl ether, (n-, iso)propyl vinyl ether, (n-, sec-, tert-, iso)butyl vinyl ether, methyl propenyl ether, and ethyl propenyl ether.
[0100] Examples of the silane compound include vinyltrichlorosilane, vinylmethyldichlorosilane, vinyldimethylchlorosilane, vinyldimethylmethoxysilane, vinyltrimethylsilane, divinyldichlorosilane, divinyldimethoxysilane, divinyldimethylsilane, 1,3-divinyl-1,1,3,3-tetramethyldisiloxane, trivinylmethylsilane, γ-methacryloyloxypropyltrimethoxysilane, and γ-methacryloyloxypropylmethyldimethoxysilane.
[0101] In the present invention, the monomer component not mainly composed of isobutylene is preferably a monomer component mainly composed of an aromatic vinyl monomer in terms of the balance between physical properties and polymerization characteristics. The aromatic vinyl monomer in the present invention refers to a monomer component having an aromatic vinyl monomer content of 60% by weight or more, preferably 80% by weight or more. As the aromatic vinyl monomer, it is preferable to use one or more monomers selected from the group consisting of styrene, α-methylstyrene, p-methylstyrene, and indene, and it is particularly preferable to use styrene in terms of cost.
[0102] The monomer mainly composed of isobutylene may contain a monomer other than isobutylene, and is a monomer having an isobutylene content of more than 30% by weight. The monomer other than isobutylene is not particularly limited as long as it is a monomer capable of cationic polymerization, and examples thereof include the above-mentioned monomers.
[0103] There are no particular restrictions on the ratio of units consisting of monomers whose main component is isobutylene and units consisting of monomers whose main component is not isobutylene, but from the standpoint of various physical properties, it is preferable that units consisting of monomers whose main component is isobutylene be 95 to 40% by weight and units consisting of monomers whose main component is not isobutylene be 5 to 60% by weight, and it is even more preferable that units consisting of monomers whose main component is isobutylene be 85 to 50% by weight and units consisting of monomers whose main component is not isobutylene be 15 to 50% by weight.
[0104] There is also no particular restriction on the number average molecular weight of component D, but in terms of fluidity, processability, physical properties, etc., it is preferably 30,000 to 500,000, and more preferably 50,000 to 400,000. If the number average molecular weight of component D is lower than the above range, the softener tends to bleed out and mechanical properties may not be fully expressed, while if it exceeds the above range, it may be disadvantageous in terms of fluidity and processability.
[0105] There are no particular limitations on the method for producing component D, but it can be obtained, for example, by polymerizing a monomer containing isobutylene as a main component and a monomer not containing isobutylene as a main component in the presence of a compound represented by the following general formula (4).
[0106] [ka] [In the formula, X is a substituent selected from a halogen atom, an alkoxy group having 1 to 6 carbon atoms, and an acyloxy group; R 1 , R 2 are each a hydrogen atom or a monovalent hydrocarbon group having 1 to 6 carbon atoms, and may be the same or different; R 3 is a polyvalent aromatic hydrocarbon group or a polyvalent aliphatic hydrocarbon group, and n is a natural number of 1 to 6.
[0107] The compound represented by the above general formula (4) acts as an initiator and is believed to generate a carbocation in the presence of a Lewis acid or the like, thereby serving as the initiation point for cationic polymerization. Examples of the compound of general formula (4) used in the present invention include (1-chloro-1-methylethyl)benzene [C6H5C(CH3)2Cl], 1,4-bis(1-chloro-1-methylethyl)benzene [1,4-Cl(CH3)2CC6H4C(CH3)2Cl], 1,3-bis(1-chloro-1-methylethyl)benzene [1,3-Cl(CH3)2CC6H4C(CH3)2Cl], 1,3,5-tris(1-chloro-1-methylethyl)benzene [1,3,5-(ClC(CH3)2)3C6H3], and 1,3-bis(1-chloro-1-methylethyl)-5-(tert-butyl)benzene [1,3-(C(CH3)2Cl)2-5-(C(CH3)3)C6H3].
[0108] Among these, bis(1-chloro-1-methylethyl)benzene [C6H4(C(CH3)2Cl)2] and tris(1-chloro-1-methylethyl)benzene [(ClC(CH3)2)3C6H3] are particularly preferred. Note that bis(1-chloro-1-methylethyl)benzene is also called bis(α-chloroisopropyl)benzene, bis(2-chloro-2-propyl)benzene or dicumyl chloride, and tris(1-chloro-1-methylethyl)benzene is also called tris(α-chloroisopropyl)benzene, tris(2-chloro-2-propyl)benzene or tricumyl chloride.
[0109] When producing component D by polymerization, a Lewis acid catalyst can also be used. Such Lewis acids may be any that can be used in cationic polymerization, and metal halides such as TiCl4, TiBr4, BCl3, BF3, BF3·OEt2, SnCl4, SbCl5, SbF5, WCl6, TaCl5, VCl5, FeCl3, ZnBr2, AlCl3, and AlBr3; and organometallic halides such as Et2AlCl and EtAlCl2 can be preferably used. Among them, TiCl4, BCl3, and SnCl4 are preferred in terms of catalytic ability and industrial availability. The amount of Lewis acid used is not particularly limited, but can be set in consideration of the polymerization characteristics or polymerization concentration of the monomer used. Usually, 0.1 to 100 molar equivalents can be used relative to the compound represented by general formula (4), and preferably in the range of 1 to 50 molar equivalents.
[0110] In the polymerization of component D, an electron donor component can be added as necessary. This electron donor component is believed to have the effect of stabilizing the growing carbocation during cationic polymerization, and the addition of the electron donor produces a polymer with a narrow molecular weight distribution and a controlled structure. Usable electron donor components are not particularly limited, but examples include pyridines, amines, amides, sulfoxides, esters, and metal compounds having an oxygen atom bonded to a metal atom.
[0111] Polymerization of component D can be carried out in an organic solvent as necessary, and the organic solvent can be used without any particular restrictions as long as it does not essentially inhibit cationic polymerization.Specific examples include halogenated hydrocarbons such as methyl chloride, dichloromethane, chloroform, ethyl chloride, dichloroethane, n-propyl chloride, n-butyl chloride, and chlorobenzene; alkylbenzenes such as benzene, toluene, xylene, ethylbenzene, propylbenzene, and butylbenzene; linear aliphatic hydrocarbons such as ethane, propane, butane, pentane, hexane, heptane, octane, nonane, and decane; branched aliphatic hydrocarbons such as 2-methylpropane, 2-methylbutane, 2,3,3-trimethylpentane, and 2,2,5-trimethylhexane; cyclic aliphatic hydrocarbons such as cyclohexane, methylcyclohexane, and ethylcyclohexane; and paraffin oil obtained by hydrogenating and refining petroleum fractions.
[0112] These solvents are used alone or in combination of two or more kinds, taking into consideration the balance between the polymerization characteristics of the monomers constituting component D and the solubility of the resulting polymer.
[0113] The amount of the solvent used is determined so that the polymer concentration is 1 to 50% by weight, preferably 5 to 35% by weight, taking into consideration the viscosity of the resulting polymer solution and ease of heat removal.
[0114] In carrying out the actual polymerization, the components are mixed under cooling, for example, at a temperature of −100° C. or higher and lower than 0° C. In order to balance the energy cost and the stability of the polymerization, a particularly preferred temperature range is −30° C. to −80° C.
[0115] The content of component D is 1 to 10 parts by weight, preferably 2 to 8 parts by weight, and more preferably 2 to 6 parts by weight, based on 100 parts by weight of the components consisting of components A and B. If the content of component D is less than 1 part by weight, sufficient improvement in chemical resistance and suppression of abnormal noise cannot be obtained, whereas if it exceeds 10 parts by weight, impact resistance decreases and the appearance of the molded product also deteriorates.
[0116] (Component E: oxidized polyethylene wax) The oxidized polyethylene wax used in the present invention is not particularly limited, and examples thereof include oxides of polyethylene wax produced by low pressure polymerization, oxides of polyethylene wax produced by high pressure polymerization, and oxides of high density polyethylene polymers. These oxidized polyethylene waxes may be used alone or in combination of two or more.
[0117] The dropping point of the oxidized polyethylene wax is preferably 100° C. or higher and 140° C. or lower, and more preferably 110° C. or higher and 130° C. or lower. The dropping point can be measured by a method in accordance with ASTM D127.
[0118] The acid value of the oxidized polyethylene wax is preferably 10 mgKOH / g or more and 50 mgKOH / g or less, more preferably 15 mgKOH / g or more and 40 mgKOH / g or less. The acid value can be measured by a method in accordance with JIS K3504. The number average molecular weight of the oxidized polyethylene wax is preferably 500 or more and 5000 or less, more preferably 1000 or more and 4000 or less.
[0119] The content of component E is preferably 0.05 to 1.5 parts by weight based on 100 parts by weight of components A and B. By including component E in such an amount, it may be possible to improve releasability and suppress abnormal noise. The lower limit of the content of component D is more preferably 0.3 parts by weight, and even more preferably 0.5 parts by weight, and the upper limit is preferably 1.3 parts by weight, and even more preferably 1.0 parts by weight.
[0120] (Other Ingredients) The resin composition of the present invention may also contain phosphorus-based stabilizers, hindered phenol-based stabilizers, release agents, ultraviolet absorbers, impact modifiers, dyes and pigments (carbon black, titanium oxide, etc.), and the like.
[0121] (i) Phosphorus stabilizers, hindered phenol stabilizers, other heat stabilizers It is preferable that various heat stabilizers are blended in the resin composition of the present invention. Phosphorus-based stabilizers are suitable as such heat stabilizers. Examples of phosphorus-based stabilizers include phosphorous acid, phosphoric acid, phosphonous acid, phosphonic acid and their esters, and tertiary phosphines. Such phosphorus-based stabilizers can be used alone or in combination of two or more. Examples of phosphite compounds include trialkyl phosphites such as tridecyl phosphite, dialkyl monoaryl phosphites such as didecyl monophenyl phosphite, monoalkyl diaryl phosphites such as monobutyl diphenyl phosphite, triaryl phosphites such as triphenyl phosphite and tris(2,4-di-tert-butylphenyl)phosphite, distearyl pentaerythritol diphosphite, bis(2,4-di-tert-butylphenyl)pentaerythritol, and the like. Examples of the phosphate compound include pentaerythritol phosphites such as bis(2,4-dicumylphenyl)pentaerythritol diphosphite, bis(2,6-di-tert-butyl-4-methylphenyl)pentaerythritol diphosphite, and cyclic phosphites such as 2,2-methylenebis(4,6-di-tert-butylphenyl)octyl phosphite and 2,2'-methylenebis(4,6-di-tert-butylphenyl)(2,4-di-tert-butylphenyl)phosphite. Examples of the phosphate compound include tributyl phosphate, trimethyl phosphate, tricresyl phosphate, triphenyl phosphate, triethyl phosphate, diphenylcresyl phosphate, diphenylmonoorthoxenyl phosphate, tributoxyethyl phosphate, and diisopropyl phosphate, and preferably triphenyl phosphate and trimethyl phosphate. Preferred examples of the phosphonite compound include tetrakis(di-tert-butylphenyl)-biphenylene diphosphonite and bis(di-tert-butylphenyl)-phenyl-phenyl phosphonite, and more preferred are tetrakis(2,4-di-tert-butylphenyl)-biphenylene diphosphonite and bis(2,4-di-tert-butylphenyl)-phenyl-phenyl phosphonite.Such phosphonite compounds can be used in combination with the phosphite compounds having an aryl group substituted with two or more alkyl groups, and are preferred. Examples of the phosphonate compounds include dimethyl benzenephosphonate, diethyl benzenephosphonate, and dipropyl benzenephosphonate. Examples of the tertiary phosphine include triphenylphosphine.
[0122] The content of such phosphorus-based stabilizer is preferably 0.001 to 3.0 parts by weight, more preferably 0.01 to 2.0 parts by weight, and even more preferably 0.05 to 1.0 part by weight, based on 100 parts by weight of the components A and B.
[0123] As the hindered phenol-based stabilizer, various compounds that are usually blended in resins can be used. Examples of such hindered phenol-based stabilizers include α-tocopherol, butyl hydroxytoluene, sinapyl alcohol, vitamin E, octadecyl-3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate, 2-tert-butyl-6-(3'-tert-butyl-5'-methyl-2'-hydroxybenzyl)-4-methylphenyl acrylate, 2,6-di-tert-butyl-4-(N,N-dimethylaminomethyl)phenol, 3,5-di-tert-butyl-4-hydroxybenzyl, and the like. diethyl ester, 2,2'-methylenebis(4-methyl-6-tert-butylphenol), 2,2'-methylenebis(4-ethyl-6-tert-butylphenol), 4,4'-methylenebis(2,6-di-tert-butylphenol), 2,2'-methylenebis(4-methyl-6-cyclohexylphenol), 2,2'-dimethylene-bis(6-α-methyl-benzyl-p-cresol), 2,2'-ethylidene-bis(4,6-di-tert-butylphenol), 2,2'-butylidene-bis( 4-Methyl-6-tert-butylphenol), 4,4'-butylidenebis(3-methyl-6-tert-butylphenol), triethylene glycol-N-bis-3-(3-tert-butyl-4-hydroxy-5-methylphenyl)propionate, 1,6-hexanediol bis[3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate], bis[2-tert-butyl-4-methyl-6-(3-tert-butyl-5-methyl-2-hydroxybenzyl)phenyl]terephthalate, 3,9 -Bis{2-[3-(3-tert-butyl-4-hydroxy-5-methylphenyl)propionyloxy]-1,1-dimethylethyl}-2,4,8,10-tetraoxaspiro[5,5]undecane, 4,4'-thiobis(6-tert-butyl-m-cresol), 4,4'-thiobis(3-methyl-6-tert-butylphenol), 2,2'-thiobis(4-methyl-6-tert-butylphenol), bis(3,5-di-tert-butyl-4-hydroxybenzyl)sulfide, 4,4'-dithiobis(2,6-di-tert-butylphenol), 4,4'-tri-thiobis(2,6-di-tert-butylphenol), 2,2-thiodiethylene bis-[3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate], 2,4-bis(n-octylthio)-6-(4-hydroxy-3,5-di-tert-butylanilino)-1,3,5-triazine, N,N'-hexamethylene bis-(3,5-di-tert-butyl-4-hydroxyhydrocinnamide), N,N'-bi S[3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionyl]hydrazine, 1,1,3-tris(2-methyl-4-hydroxy-5-tert-butylphenyl)butane, 1,3,5-trimethyl-2,4,6-tris(3,5-di-tert-butyl-4-hydroxybenzyl)benzene, tris(3,5-di-tert-butyl-4-hydroxyphenyl)isocyanurate, tris(3,5-di-tert-butyl-4-hydroxybenzyl)isocyanurate , 1,3,5-tris(4-tert-butyl-3-hydroxy-2,6-dimethylbenzyl)isocyanurate, 1,3,5-tris2[3(3,5-di-tert-butyl-4-hydroxyphenyl)propionyloxy]ethyl isocyanurate, tetrakis[methylene-3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate]methane, triethylene glycol-N-bis-3-(3-tert-butyl-4-hydroxy-5-methylphenyl)propionate ester, triethylene glycol-N-bis-3-(3-tert-butyl-4-hydroxy-5-methylphenyl)acetate, 3,9-bis[2-{3-(3-tert-butyl-4-hydroxy-5-methylphenyl)acetyloxy}-1,1-dimethylethyl]-2,4,8,10-tetraoxaspiro[5,5]undecane, tetrakis[methylene-3-(3-tert-butyl-4-hydroxy-5-methylphenyl)propionate]methane, 1,3,5-trimethyl-2,4,Examples of the compounds include 6-tris(3-tert-butyl-4-hydroxy-5-methylbenzyl)benzene and tris(3-tert-butyl-4-hydroxy-5-methylbenzyl)isocyanurate. Among the above compounds, tetrakis[methylene-3-(3-tert-butyl-4-hydroxy-5-methylphenyl)propionate]methane, octadecyl-3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate, and 3,9-bis[2-{3-(3-t-butyl-4-hydroxy-5-methylphenyl)propionyloxy}-1,1-dimethylethyl]-2,4,8,10-tetraoxaspiro[5,5]undecane are preferably used in the present invention. Particularly preferred is 3,9-bis[2-{3-(3-t-butyl-4-hydroxy-5-methylphenyl)propionyloxy}-1,1-dimethylethyl]-2,4,8,10-tetraoxaspiro[5,5]undecane. The above hindered phenol-based antioxidants can be used alone or in combination of two or more kinds.
[0124] The content of the hindered phenol-based stabilizer is preferably 0.001 to 3.0 parts by weight, more preferably 0.01 to 2.0 parts by weight, and even more preferably 0.05 to 1.0 part by weight, relative to 100 parts by weight of the components A and B.
[0125] The resin composition of the present invention may also contain other heat stabilizers than the phosphorus-based stabilizer and the hindered phenol-based stabilizer. Such other heat stabilizers are preferably used in combination with either one of these stabilizers and the antioxidant, and particularly preferably used in combination with both. Suitable examples of such other heat stabilizers include lactone-based stabilizers such as the reaction product of 3-hydroxy-5,7-di-tert-butyl-furan-2-one and o-xylene (details of such stabilizers are described in JP-A-7-233160). Such a compound is commercially available as Irganox HP-136 (trademark, manufactured by CIBA SPECIALTY CHEMICALS), and this compound can be used. Furthermore, stabilizers in which this compound is mixed with various phosphite compounds and hindered phenol compounds are commercially available. Suitable examples include Irganox HP-2921 manufactured by the above company. Such premixed stabilizers can also be used in the present invention. The amount of the lactone-based stabilizer to be added is preferably 0.0005 to 0.05 parts by weight, and more preferably 0.001 to 0.03 parts by weight, based on 100 parts by weight of the components consisting of the A component and the B component.
[0126] Other examples of the stabilizer include sulfur-containing stabilizers such as pentaerythritol tetrakis (3-mercaptopropionate), pentaerythritol tetrakis (3-laurylthiopropionate), and glycerol-3-stearylthiopropionate. Such stabilizers are particularly effective when the resin composition is applied to rotational molding. The amount of such sulfur-containing stabilizers is preferably 0.001 to 0.1 parts by weight, more preferably 0.01 to 0.08 parts by weight, based on 100 parts by weight of the components A and B.
[0127] (ii) Release agent The resin composition of the present invention may contain a release agent other than component E for the purpose of improving the productivity during molding and reducing distortion of the molded product, within a range that does not impair the effects of the present invention. Known release agents can be used. Examples of such release agents include saturated fatty acid esters, unsaturated fatty acid esters, silicone compounds, fluorine compounds (such as fluorine oils typified by polyfluoroalkyl ethers), paraffin wax, and beeswax. Among them, fatty acid esters are preferred release agents. Such fatty acid esters are esters of aliphatic alcohols and aliphatic carboxylic acids. Such aliphatic alcohols may be monohydric alcohols or polyhydric alcohols having dihydric or higher valences. The carbon number of the alcohol is in the range of 3 to 32, more preferably in the range of 5 to 30. Examples of such monohydric alcohols include dodecanol, tetradecanol, hexadecanol, octadecanol, eicosanol, tetracosanol, ceryl alcohol, and triacontanol. Examples of such polyhydric alcohols include pentaerythritol, dipentaerythritol, tripentaerythritol, polyglycerol (triglycerol to hexaglycerol), ditrimethylolpropane, xylitol, sorbitol, and mannitol. In the fatty acid ester of the present invention, polyhydric alcohols are more preferred. On the other hand, the aliphatic carboxylic acid preferably has 3 to 32 carbon atoms, and particularly preferably has 10 to 22 carbon atoms. Examples of the aliphatic carboxylic acid include saturated aliphatic carboxylic acids such as decanoic acid, undecanoic acid, dodecanoic acid, tridecanoic acid, tetradecanoic acid, pentadecanoic acid, hexadecanoic acid (palmitic acid), heptadecanoic acid, octadecanoic acid (stearic acid), nonadecanoic acid, behenic acid, icosanoic acid, and docosanoic acid, and unsaturated aliphatic carboxylic acids such as palmitoleic acid, oleic acid, linoleic acid, linolenic acid, eicosenoic acid, eicosapentaenoic acid, and cetoleic acid. Among the above, the aliphatic carboxylic acid is preferably one having 14 to 20 carbon atoms. Among them, saturated aliphatic carboxylic acids are preferred. Stearic acid and palmitic acid are particularly preferred.The above-mentioned aliphatic carboxylic acids such as stearic acid and palmitic acid are usually produced from natural fats and oils such as animal fats and oils typified by beef tallow and lard, and vegetable fats and oils typified by palm oil and sunflower oil, and therefore these aliphatic carboxylic acids are usually mixtures containing other carboxylic acid components with different numbers of carbon atoms. Therefore, in the production of the fatty acid ester of the present invention, aliphatic carboxylic acids produced from such natural fats and oils and in the form of a mixture containing other carboxylic acid components, particularly stearic acid and palmitic acid, are preferably used. The fatty acid ester may be either a partial ester or a full ester (full ester). However, partial esters usually have a high hydroxyl value and tend to induce decomposition of the resin at high temperatures, so full esters are more preferable. The acid value of the fatty acid ester of the present invention is preferably 20 or less, more preferably in the range of 4 to 20, and even more preferably in the range of 4 to 12, from the viewpoint of thermal stability. The acid value can be substantially 0. The hydroxyl value of the fatty acid ester is more preferably in the range of 0.1 to 30. Furthermore, the iodine value is preferably 10 or less. Furthermore, the iodine value can be substantially 0. These properties can be determined by the method specified in JIS K 0070.
[0128] The content of the release agent is preferably 0.01 to 4.0 parts by weight, more preferably 0.05 to 3.0 parts by weight, and even more preferably 0.1 to 2.5 parts by weight, based on 100 parts by weight of the components A and B.
[0129] (iii) Ultraviolet absorber The resin composition of the present invention can contain an ultraviolet absorber. Benzophenone-based compounds include, for example, 2,4-dihydroxybenzophenone, 2-hydroxy-4-methoxybenzophenone, 2-hydroxy-4-octoxybenzophenone, 2-hydroxy-4-benzyloxybenzophenone, 2-hydroxy-4-methoxy-5-sulfoxybenzophenone, 2-hydroxy-4-methoxy-5-sulfoxytrihydridyl benzophenone, 2,2'-dihydroxy-4-methoxybenzophenone, 2,2',4,4'-tetrahydroxybenzophenone, 2,2'-dihydroxy-4,4'-dimethoxybenzophenone, 2,2'-dihydroxy-4,4'-dimethoxy-5-sodium sulfoxybenzophenone, bis(5-benzoyl-4-hydroxy-2-methoxyphenyl)methane, 2-hydroxy-4-n-dodecyloxybenzophenone, and 2-hydroxy-4-methoxy-2'-carboxybenzophenone.Benzotriazoles include, for example, 2-(2-hydroxy-5-methylphenyl)benzotriazole, 2-(2-hydroxy-5-tert-octylphenyl)benzotriazole, 2-(2-hydroxy-3,5-dicumylphenyl)phenylbenzotriazole, 2-(2-hydroxy-3-tert-butyl-5-methylphenyl)-5-chlorobenzotriazole, 2,2'-methylenebis[4-(1,1,3,3-tetramethylbutyl)-6-(2H-benzotriazol-2-yl)phenol], 2-(2-hydroxy-3,5-di-tert-butylphenyl)benzotriazole, 2-(2-hydroxy-3,5-di-tert-butylphenyl)-5-chlorobenzotriazole, 2-(2-hydroxy-3,5-di-tert-amylphenyl)benzotriazole, 2-(2-hydroxy-5-tert-octylphenyl)benzotriazole, Examples of the polymer include polymers having a 2-hydroxyphenyl-2H-benzotriazole skeleton, such as azole, 2-(2-hydroxy-5-tert-butylphenyl)benzotriazole, 2-(2-hydroxy-4-octoxyphenyl)benzotriazole, 2,2'-methylenebis(4-cumyl-6-benzotriazolephenyl), 2,2'-p-phenylenebis(1,3-benzoxazin-4-one), and 2-[2-hydroxy-3-(3,4,5,6-tetrahydrophthalimidomethyl)-5-methylphenyl]benzotriazole, as well as copolymers of 2-(2'-hydroxy-5-methacryloxyethylphenyl)-2H-benzotriazole and vinyl monomers copolymerizable with the monomer, and copolymers of 2-(2'-hydroxy-5-acryloxyethylphenyl)-2H-benzotriazole and vinyl monomers copolymerizable with the monomer.Examples of hydroxyphenyl triazines include 2-(4,6-diphenyl-1,3,5-triazin-2-yl)-5-hexyloxyphenol, 2-(4,6-diphenyl-1,3,5-triazin-2-yl)-5-methyloxyphenol, 2-(4,6-diphenyl-1,3,5-triazin-2-yl)-5-ethyloxyphenol, 2-(4,6-diphenyl-1,3,5-triazin-2-yl)-5-propyloxyphenol, and 2-(4,6-diphenyl-1,3,5-triazin-2-yl)-5-butyloxyphenol.Further examples include compounds in which the phenyl group of the above-mentioned compounds is replaced with a 2,4-dimethylphenyl group, such as 2-(4,6-bis(2,4-dimethylphenyl)-1,3,5-triazin-2-yl)-5-hexyloxyphenol. Examples of cyclic imino esters include 2,2'-p-phenylenebis(3,1-benzoxazin-4-one), 2,2'-(4,4'-diphenylene)bis(3,1-benzoxazin-4-one), and 2,2'-(2,6-naphthalene)bis(3,1-benzoxazin-4-one).
[0130] Examples of cyanoacrylates include 1,3-bis-[(2'-cyano-3',3'-diphenylacryloyl)oxy]-2,2-bis[(2-cyano-3,3-diphenylacryloyl)oxy]methyl)propane and 1,3-bis-[(2-cyano-3,3-diphenylacryloyl)oxy]benzene.
[0131] Furthermore, the ultraviolet absorber may be a polymer type ultraviolet absorber obtained by copolymerizing such an ultraviolet absorbing monomer and / or a light stable monomer having a hindered amine structure with a monomer such as an alkyl (meth)acrylate by adopting a structure of a radically polymerizable monomer compound. Suitable examples of the ultraviolet absorbing monomer include compounds containing a benzotriazole skeleton, a benzophenone skeleton, a triazine skeleton, a cyclic imino ester skeleton, and a cyanoacrylate skeleton in the ester substituent of a (meth)acrylic acid ester.
[0132] The content of the ultraviolet absorber is preferably 0.01 to 2.0 parts by weight, more preferably 0.02 to 1.5 parts by weight, and even more preferably 0.03 to 1.0 part by weight, based on 100 parts by weight of the components consisting of the A component and the B component.
[0133] (iv) Other resins and elastomers The resin composition of the present invention may contain other resins or elastomers in small proportions within the range in which the effects of the present invention are exhibited. Examples of such other resins include polypropylene resins, polyethylene terephthalate resins, polybutylene terephthalate resins, polyamide resins, polyimide resins, polyetherimide resins, polyurethane resins, silicone resins, polyphenylene ether resins, polyphenylene sulfide resins, polysulfone resins, polymethacrylate resins, phenolic resins, and fluororesins. Examples of elastomers include isobutylene / isoprene rubber, styrene / butadiene rubber, ethylene / propylene rubber, acrylic elastomers, polyester elastomers, polyamide elastomers, and core-shell elastomers such as MBS (methyl methacrylate / styrene / butadiene) rubber, MB (methyl methacrylate / butadiene) rubber, and MAS (methyl methacrylate / acrylonitrile / styrene) rubber.
[0134] (v) Dyes and pigments The resin composition of the present invention can further contain various dyes and pigments to provide molded products with a variety of designs. By blending fluorescent whitening agents or other fluorescent dyes that emit light, it is possible to provide even better design effects that make use of the emitted color. It is also possible to provide resin compositions that are colored with extremely small amounts of dyes and pigments and have vivid color development. Examples of the fluorescent dyes (including fluorescent whitening agents) used in the present invention include coumarin-based fluorescent dyes, benzopyran-based fluorescent dyes, perylene-based fluorescent dyes, anthraquinone-based fluorescent dyes, thioindigo-based fluorescent dyes, xanthene-based fluorescent dyes, xanthone-based fluorescent dyes, thioxanthene-based fluorescent dyes, thioxanthone-based fluorescent dyes, thiazine-based fluorescent dyes, and diaminostilbene-based fluorescent dyes. Among these, coumarin-based fluorescent dyes, benzopyran-based fluorescent dyes, and perylene-based fluorescent dyes are preferred because they have good heat resistance and are less likely to deteriorate during molding of polycarbonate resin.
[0135] Examples of dyes other than the above bluing agents and fluorescent dyes include perylene dyes, coumarin dyes, thioindigo dyes, anthraquinone dyes, thioxanthone dyes, ferrocyanides such as Prussian blue, perinone dyes, quinoline dyes, quinacridone dyes, dioxazine dyes, isoindolinone dyes, and phthalocyanine dyes. Furthermore, the resin composition of the present invention can be blended with a metallic pigment to obtain a better metallic color. As the metallic pigment, those having a metal coating or a metal oxide coating on various plate-like fillers are suitable.
[0136] The content of the dye or pigment is preferably 0.00001 to 1 part by weight, and more preferably 0.00005 to 0.5 parts by weight, per 100 parts by weight of the components consisting of the A component and the B component.
[0137] (vi) Flame retardants The resin composition of the present invention can be applied with various compounds that are conventionally known as flame retardants for thermoplastic resins, particularly polycarbonate-based resins, but more preferably, (i) halogen-based flame retardants (e.g., brominated polycarbonate compounds, etc.), (ii) phosphorus-based flame retardants (e.g., monophosphate compounds, phosphate oligomer compounds, phosphonate oligomer compounds, phosphonitrile oligomer compounds, phosphonic acid amide compounds, and phosphazene compounds, etc.), (iii) metal salt-based flame retardants (e.g., organic sulfonic acid alkali (earth) metal salts, boric acid metal salt-based flame retardants, and stannic acid metal salt-based flame retardants, etc.), and (iv) silicone-based flame retardants made of silicone compounds. The incorporation of compounds used as flame retardants not only improves flame retardancy, but also improves antistatic properties, fluidity, rigidity, and thermal stability, etc., based on the properties of each compound.
[0138] The content of the flame retardant is preferably 0.01 to 30 parts by weight, more preferably 0.05 to 28 parts by weight, and further preferably 0.08 to 25 parts by weight, based on 100 parts by weight of the components consisting of components A and B. If the content of the flame retardant is less than 0.01 part by weight, sufficient flame retardancy may not be obtained, whereas if it exceeds 30 parts by weight, mechanical properties may be significantly reduced.
[0139] (vii) Highly light-reflecting white pigments The resin composition of the present invention can be blended with a highly light-reflective white pigment to impart a light-reflecting effect. Examples of such white pigments include zinc sulfide, zinc oxide, barium sulfate, calcium carbonate, and calcined kaolin. The content of such highly light-reflective white pigment is preferably 1 to 30 parts by weight, more preferably 3 to 25 parts by weight, per 100 parts by weight of the components A and B. Two or more types of highly light-reflective white pigments can be used in combination.
[0140] (viii) Other additives In addition, the resin composition of the present invention may contain small amounts of additives known per se to impart various functions to the molded product or improve its characteristics. These additives may be added in normal amounts as long as they do not impair the object of the present invention. Examples of such additives include sliding agents (e.g., PTFE particles), colorants (e.g., pigments such as carbon black, dyes), light diffusing agents (e.g., acrylic crosslinked particles, silicon crosslinked particles, ultrathin glass flakes, calcium carbonate particles), fluorescent dyes, inorganic phosphors (e.g., phosphors with aluminate as the parent crystal), antistatic agents, crystal nucleating agents, inorganic and organic antibacterial agents, photocatalytic antifouling agents (e.g., fine titanium oxide particles, fine zinc oxide particles), radical generators, infrared absorbing agents (heat ray absorbing agents), and photochromic agents.
[0141] (Method for preparing resin composition) The resin composition of the present invention is prepared by mixing the above-mentioned components simultaneously or in any order using a mixer such as a tumbler, a V-type blender, a Nauter mixer, a Banbury mixer, a kneading roll, or an extruder. As a mixer, melt kneading using a twin-screw extruder is preferred, and if necessary, any component is preferably fed into the other melt-mixed components from a second feed port using a side feeder or the like. The resin extruded as described above is directly cut and pelletized, or is pelletized by cutting the strands with a pelletizer after forming them. When it is necessary to reduce the influence of external dust during pelletization, it is preferable to purify the atmosphere around the extruder. The shape of the obtained pellets can be a general shape such as a cylinder, a rectangular column, or a sphere, but is more preferably a cylinder. The diameter of such a cylinder is preferably 1 to 5 mm, more preferably 1.5 to 4 mm, and even more preferably 2 to 3.5 mm. On the other hand, the length of the cylinder is preferably 1 to 30 mm, more preferably 2 to 5 mm, and even more preferably 2.5 to 4 mm.
[0142] (Regarding molded articles made of resin compositions obtained by the manufacturing method of the present invention) The resin composition obtained by the manufacturing method of the present invention can be used to manufacture various products by injection molding the pellets obtained by the above-mentioned method. In such injection molding, molded products can be obtained using not only ordinary molding methods but also injection molding methods such as injection compression molding, injection press molding, gas-assisted injection molding, foam molding (including injection of supercritical fluid), insert molding, in-mold coating molding, heat-insulating mold molding, rapid heating and cooling mold molding, two-color molding, sandwich molding, and ultra-high speed injection molding, depending on the purpose. The advantages of these various molding methods are already widely known. In addition, molding can be performed using either a cold runner method or a hot runner method. EXAMPLES
[0143] The present invention will be described in more detail below with reference to examples. In the following, "parts" means "parts by weight" and "%" means "% by weight" unless otherwise specified.
[0144] (1) Preparation of resin composition (1-1) Raw materials used (Component A) A-1: Polycarbonate resin powder with a molecular weight of 19,800 obtained by the following method A three-stage six-blade stirrer and a reflux condenser were attached to the baffled reaction vessel. 45.6 parts of bisphenol A, 2.78 mol % of p-tert-butylphenol relative to bisphenol A, 265 parts of dichloromethane, and 200 parts of water were placed in the reaction vessel, and nitrogen purging was performed to remove oxygen from the reaction vessel. At this stage, the contents in the reaction vessel were slightly less than 80% of the vessel volume. Next, about 80 parts of an aqueous solution for supplying 0.09 parts of sodium hydrosulfite and 21.8 parts of sodium hydroxide were supplied to the suspension, and bisphenol A was dissolved at 15°C. 23.35 parts of phosgene were supplied to this mixture under stirring for 30 minutes. Then, 0.016 parts of triethylamine (0.08 mol % relative to bisphenol A) was added and stirred for 60 minutes to terminate the reaction. Then, the reaction mixture was left to stand, and the organic phase was separated. Methylene chloride was added to the dichloromethane solution of the obtained polycarbonate resin to make a solution with a concentration of 14% by weight, and further, using a centrifugal extractor with a perforated plate (KCC Centrifugal Extractor manufactured by Kawasaki Engineering Co., Ltd.), 0.5% aqueous sodium hydroxide solution was supplied at a flow rate of 1,000 ml / min and the organic phase was supplied at a flow rate of 1,000 ml / min under conditions of 3,500 rpm, after which the organic phase was acidified with hydrochloric acid, and then repeatedly washed with water. When the conductivity of the aqueous phase became almost the same as that of ion-exchanged water, the methylene chloride was evaporated to obtain polycarbonate resin powder.
[0145] (B component) B-1: ABS resin (MAGNUM A156 manufactured by TRISEO HOLDINGS ASIA PTE.LTD.)
[0146] (C component) C-1: A graft copolymer in which the side chain is a vinyl copolymer containing acrylonitrile and styrene and the main chain is an ethylene-vinyl acetate copolymer (Modiper AS100, manufactured by NOF Corporation)
[0147] (D component) D-1: Styrene-isobutylene-styrene block copolymer (SIBSTAR103T manufactured by Kaneka Corporation) D-2 (Comparative Example): Styrene-ethylene-propylene-styrene block copolymer (Septon 2104 manufactured by Kuraray Co., Ltd.) D-3 (Comparative Example): A graft copolymer having a core-shell structure in which the core is butadiene rubber and the shell is methyl methacrylate and styrene (Kane Ace M-701, manufactured by Kaneka Corporation)
[0148] (E component) E-1: Oxidized polyethylene wax (Hiwax 310MP, manufactured by Mitsui Chemicals, Inc.)
[0149] (Other Ingredients) F-1: Release agent (fatty acid ester, Riken Vitamin Co., Ltd., Rikestar EW-400) F-2: Phosphorus stabilizer (Adeka Stab 2112 manufactured by Adeka Corporation) F-3: Hindered phenol stabilizer (Adeka STAB AO-50 manufactured by Adeka Corporation) F-4: Carbon black (Koshigaya Chemical Industries, Ltd.: ROYAL BLACK RB90003S (product name))
[0150] (1-2) Preparation of resin composition The components shown in Table 1 were mixed in the ratios shown, and the mixture was fed from the first feed port of the extruder. The mixture was obtained by mixing in a V-type blender. Extrusion was performed using a vented twin-screw extruder (TEX30α-38.5BW-3V, Japan Steel Works, Ltd.) with a diameter of 30 mm, and pellets were obtained by melt kneading at a screw rotation speed of 230 rpm, a discharge rate of 25 kg / h, and a vent vacuum of 3 kPa. The extrusion temperature was 260°C from the first feed port to the die.
[0151] (2) Preparation of test specimens (2-1) How to prepare test specimens for measuring Charpy impact strength The obtained pellets were dried in a hot air circulation dryer at 110°C for 6 hours, and then molded into ISO bending test specimens using an injection molding machine [EC130XII-4Y, manufactured by Toshiba Machine Co., Ltd.] under conditions of a cylinder temperature of 260°C and a mold temperature of 70°C.
[0152] (2-2) Method of preparing test pieces for evaluating the appearance of molded products and for evaluating chemical resistance The obtained pellets were dried in a hot air circulation dryer at 110°C for 6 hours, and then molded into a plate with a width of 100 mm, length of 100 mm, and thickness of 2 mm using an injection molding machine [EC130XII-4Y, manufactured by Toshiba Machine Co., Ltd.] under conditions of a cylinder temperature of 260°C and a mold temperature of 70°C.
[0153] (2-3) How to create test pieces for evaluating abnormal noise The obtained pellets were dried in a hot air circulation dryer at 110°C for 6 hours, and then molded into a plate with a width of 100 mm, length of 100 mm, and thickness of 1 mm using an injection molding machine [EC130XII-4Y, manufactured by Toshiba Machine Co., Ltd.] under conditions of a cylinder temperature of 260°C and a mold temperature of 70°C.
[0154] (3) Evaluation items (3-1) Charpy impact strength Using the ISO bending test piece obtained by the above method, the notched Charpy impact strength was measured in accordance with ISO 179 under an atmosphere of a temperature of 23° C. and a relative humidity of 50% RH. The resin composition of the present invention had a Charpy impact strength of 40 J / m 2 It needs to be more than that.
[0155] (3-2) Appearance of molded product The appearance of the plate having a width of 100 mm, a length of 100 mm, and a thickness of 2 mm obtained by the above method was visually evaluated according to the following criteria. ○: No visible defects ×: Molded products have poor appearance such as whitening or silvering.
[0156] (3-3) Chemical resistance Using the plate of width 100mm x length 100mm x thickness 2mm produced by the above method, 0.5g of a car deodorant / air freshener [Febreze Premium Clip Aqua Waltz (manufactured by P&G Japan LLC)] was applied to the center of the molded product, spread evenly over the entire surface with a finger, and then kept in a thermostatic chamber kept at 80°C for 4 hours. The molded product was then removed from the thermostatic chamber, washed with water, and visually evaluated for its appearance. The evaluation was performed according to the following criteria. ◯: No whitening was observed in the chemical-applied area. ×: Whitening is observed in the area where the drug was applied.
[0157] (3-4) Abnormal noise The abnormal noise evaluation was carried out using a reciprocating friction and wear tester AFT-15M manufactured by Orientec Co., Ltd. A test piece of width 20 mm x length 20 mm x thickness 1 mm was cut out from a plate of width 100 mm x length 100 mm x thickness 1 mm obtained by the above method, and the cut out test piece was placed perpendicularly against a plate of width 100 mm x length 100 mm x thickness 1 mm obtained by the above method as a mating material, and rubbed under two conditions of load 5N, speed 0.5 mm / s and load 10N, speed 0.5 mm / s, and evaluation was carried out according to the following criteria. The resin composition of the present invention needs to be "◯" under the condition of load 5N, speed 0.5 mm / s. ○: No abnormal noise was heard during the test (no noise of 80 dB or more occurred) ×: Abnormal noise is heard during the test (sounds of 80 dB or more occur)
[0158] (3-5) Heat resistance Using the ISO bending test pieces obtained by the above method, the deflection temperature under load (HDT) was measured in accordance with ISO75-1.2 using a HDT / VICAT tester (Heat Distortion Tester 6M-2 manufactured by Toyo Seiki Seisakusho Co., Ltd.) under a load of 1.8 MPa.
[0159] (3-6) Fluidity The obtained pellets were dried in a hot air circulation dryer at 110°C for 6 hours, and then the melt volume rate (MVR) was measured using a semi-automatic melt indexer (Semi-automatic melt indexer 2A manufactured by Toyo Seiki Seisakusho Co., Ltd.) at a temperature of 250°C and a load of 5000 g.
[0160] [Table 1]
Claims
1. A resin composition comprising 100 parts by weight of a component consisting of 45 to 90 parts by weight of (A) a polycarbonate resin (component A) and 10 to 55 parts by weight of (B) a copolymer obtained by polymerizing an aromatic vinyl monomer, a vinyl cyanide monomer, and a diene-based rubber polymer, 1 to 10 parts by weight of (C) a graft copolymer (component C) whose side chains are formed by polymerizing an aromatic vinyl monomer and another vinyl monomer and whose main chain is an ethylene-vinyl acetate copolymer, and 1 to 10 parts by weight of (D) an isobutylene-based block copolymer (component D) obtained by polymerizing a monomer having isobutylene as a main component and a monomer not having isobutylene as a main component.
2. 2. The resin composition according to claim 1, further comprising 0.05 to 1.5 parts by weight of oxidized polyethylene wax (component E) per 100 parts by weight of the components consisting of components A and B.
3. 3. The resin composition according to claim 1, wherein the component B is an ABS resin.
4. 4. The resin composition according to claim 1, wherein component D is a styrene-isobutylene-styrene block copolymer.
5. A molded article made of the resin composition according to any one of claims 1 to 4.
6. 6. The molded article according to claim 5, which is an automobile part.
Citation Information
Patent Citations
Scratch-resistant polycarbonate (PC) / acrylonitrile-butadiene-styenecolymer (ABS) alloy for automotive interiors and preparation method thereof
CN102807725A
Noise reduction and high-strength PC (polycarbonate) / ABS (acrylonitrile butadiene styrene) alloy and preparation method thereof
CN109354852A
Powerful anti-impact septic tank and preparation method thereof
CN110028721A
Food additive substance
JP1988056267A
Sliding material
JP1993247236A