Laser joining method and laser joined product
The laser joining method integrates rotational integration and Brewster angle irradiation to prevent deformation of inner cylindrical members during welding, ensuring effective and low occlusion lumens for fluid transport.
Patent Information
- Application Number
- JP2021082960
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2021-05-17
- Publication Date
- 2024-12-09
- Estimated Expiration
- 2041-05-17
AI Technical Summary
When welding two cylindrical members using a laser, the inner side of the inner cylindrical member expands and deforms due to heat, leading to impaired flow path uniformity and reduced transportability of liquids or gases.
A laser joining method where the first and second cylindrical members are rotated integrally, with the second member inserted into the first, and laser light is applied from the outside at an angle equal to or greater than the Brewster angle between the second member and air, minimizing heat absorption and deformation.
This method suppresses deformation of the inner surface of the inner cylindrical member, ensuring a low occlusion rate of the lumen and maintaining the transport performance of liquids or gases.
Smart Images

Figure 0007595860000001 
Figure 0007595860000002 
Figure 0007595860000003
Abstract
Description
[Technical field]
[0001] The present invention relates to a laser joining method for welding and joining two cylindrical members by irradiating them with laser light, and to a laser-joined molded product. [Background technology]
[0002] Conventionally, in the medical field, automotive field, and the like, a laser joining method has been proposed in which two resin cylindrical members are welded and joined by a laser (see, for example, Patent Document 1).The laser joining method proposed in Patent Document 1 is a method in which, in a state in which at least a part of the inner cylindrical member is disposed in the space inside the outer cylindrical member so as to overlap in the radial direction, the outer cylindrical member and the inner cylindrical member are joined by irradiating the overlapping part of the outer cylindrical member and the inner cylindrical member with laser light from the outside in the radial direction of the outer cylindrical member. [Prior art documents] [Patent documents]
[0003] [Patent Document 1] Patent No. 4279674 Summary of the Invention [Problem to be solved by the invention]
[0004] When two cylindrical members are welded together with a laser, the inside of the inner cylindrical member placed inside may expand and deform due to heat, resulting in deformation of the inner surface of the inner cylindrical member. If the inner surface of the inner cylindrical member is deformed, for example when the cylindrical member is used as a flow path for liquid or gas, the uniformity of the flow path may be lost, and the transportability of the liquid or gas may be reduced.
[0005] Therefore, an object of the present invention is to provide a laser joining method and a laser-joined molded body that can suppress deformation of the inner surface of the inner cylindrical member when two cylindrical members are welded and joined with laser light. [Means for solving the problem]
[0006] The present invention relates to a laser joining method for welding and joining a first cylindrical member having a first inner cavity and capable of transmitting laser light, and a second cylindrical member having a second inner cavity and capable of transmitting laser light, by irradiating them with laser light, the laser joining method comprising: an insertion step of inserting at least a part of the second cylindrical member into the first inner cavity with an outer circumferential surface in contact with the first inner cavity; a rotation step of rotating the first cylindrical member and the second cylindrical member integrally around central axes of the first cylindrical member and the second cylindrical member as centers of rotation; and a laser irradiation step of irradiating laser light from a radial outside of the first cylindrical member to an overlapping portion of the first cylindrical member and the second cylindrical member being rotated in the rotation step, wherein in the laser irradiation step, the laser light is irradiated at an irradiation angle such that the angle of incidence on the inner circumference of the second cylindrical member is equal to or greater than the Brewster's angle between the second cylindrical member and air.
[0007] The present invention also provides a laser-joined molded product manufactured by a laser joining method in which a first cylindrical member having a first inner cavity and capable of transmitting laser light and a second cylindrical member having a second inner cavity and capable of transmitting laser light are welded and joined by irradiating a laser beam, the laser joining method including an insertion step of inserting at least a part of the second cylindrical member into the first inner cavity with an outer circumferential surface of the second cylindrical member being in contact with the first inner cavity, and a rotation step of rotating the first cylindrical member and the second cylindrical member integrally about central axes of the first cylindrical member and the second cylindrical member. The present invention relates to a laser-bonded molded body, which comprises a rotating process, and a laser irradiation process in which laser light is irradiated from the radial outside of the first cylindrical member to the overlapping portions of the first cylindrical member and the second cylindrical member being rotated in the rotating process, wherein the laser light is irradiated in the laser irradiation process at an irradiation angle such that the angle of incidence on the inner circumference of the second cylindrical member is equal to or greater than the Brewster's angle between the second cylindrical member and air, thereby producing a laser-bonded molded body with a blockage rate of the second inner cavity of less than 50%. Effect of the Invention
[0008] According to the present invention, it is possible to provide a laser joining method capable of suppressing deformation of the inner surface of the inner cylindrical member when two cylindrical members are welded and joined by laser light. [Brief description of the drawings]
[0009] [Figure 1] 1 is a diagram showing an infusion circuit for administering medication that includes an extension tube that is manufactured by joining using a laser joining method according to one embodiment of the present invention. [Diagram 2] 1A and 1B are diagrams showing the arrangement of an outer cylindrical member and an inner cylindrical member to be joined by a laser joining method. [Diagram 3] 1 is a diagram showing the optical path of a laser beam when an inner cylindrical member and an outer cylindrical member are joined by a laser joining method. FIG. [Figure 4] 1 is a table showing optical paths of laser light and test results of examples and comparative examples. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0010] Hereinafter, one embodiment of the laser joining method of the present invention will be described with reference to the drawings. The laser joining method of the present invention is used, for example, when manufacturing an extension tube 10 of an infusion circuit 100 for administering medicine.
[0011] As shown in Fig. 1, an infusion circuit 100 for administering medicine includes an extension tube 10 manufactured by the laser joining method according to the present invention. The extension tube 10 has a plurality of connectors 11 (one end connector 12, intermediate connector 13, other end connector 14) and a plurality of tubes 15, and is configured by connecting the plurality of tubes 15 with the plurality of connectors 11.
[0012] In this embodiment, the extension tube 10 has a one-end connector 12, an intermediate connector 13, an other-end connector 14, a tube 15 connecting the one-end connector 12 and the intermediate connector 13, and a tube 15 connecting the intermediate connector 13 and the other-end connector 14. The one-end connector 12 and the tube 15 are welded and joined by irradiating them with a laser beam. The intermediate connector 13 and the tube 15 are welded and joined by irradiating them with a laser beam. The other-end connector 14 and the tube 15 are welded and joined by irradiating them with a laser beam.
[0013] For example, the one-end connector 12 is disposed at the end of the extension tube 10. Therefore, when the one-end connector 12 and the tube 15 are welded and joined by irradiating them with laser light, the one-end connector 12 is disposed on the outside of the tube 15, a core material for suppressing deformation of the inner surface of the tube 15 is disposed on the inside of the tube 15, and the one-end connector 12 is irradiated with laser light from the outside, thereby welding and joining the one-end connector 12 and the tube 15. The same applies when the other-end connector 14 and the tube 15 are welded and joined by irradiating them with laser light.
[0014] On the other hand, for example, the intermediate connector 13 is disposed in the middle of the extension tube 10. Therefore, when the intermediate connector 13 and the tube 15 are welded and joined by irradiating them with laser light, it is difficult to insert a core material if the tubes 15 are connected to both ends of the intermediate connector 13. Furthermore, it is similarly difficult to remove the core material after welding.
[0015] Therefore, when welding and joining the intermediate connector 13 and the tube 15 by irradiating them with laser light, the intermediate connector 13 is placed on the outside of the tube 15, and without placing a core material inside the tube 15, the intermediate connector 13 and the tube 15 are welded and joined by irradiating laser light from the outside of the intermediate connector 13.
[0016] The present invention is a laser joining method that is preferably used in the case where an intermediate connector 13 is placed outside a tube 15 as shown in FIG. 2, and a core material is not placed inside the tube 15, but the intermediate connector 13 is welded and joined by irradiating laser light L from outside the intermediate connector 13.
[0017] 2, in this embodiment, the intermediate connector 13 will be described as an outer cylindrical member 2 (first cylindrical member). The outer cylindrical member 2 is formed in a tubular shape extending in the direction in which the central axis O extends. Ends of a tube 15 serving as an inner cylindrical member 3 are inserted inside both ends of the outer cylindrical member 2 in the direction in which the central axis O extends.
[0018] Moreover, the tube 15 will be described as the inner cylindrical member 3 (second cylindrical member). The inner cylindrical member 3 is formed in a tubular shape extending in the direction of the central axis O. An end of the inner cylindrical member 3 is disposed inside an end of the intermediate connector 13 serving as the outer cylindrical member 2.
[0019] The laser joining method of this embodiment is a method of welding and joining an intermediate connector 13 as an outer cylindrical member 2 (first cylindrical member) and a tube 15 as an inner cylindrical member 3 (second cylindrical member) by irradiating them with laser light L. By the laser joining method of this embodiment, the outer cylindrical member 2 and the inner cylindrical member 3 are welded and joined, thereby producing a laser-joined molded product 1.
[0020] As shown in Fig. 2, the outer cylindrical member 2 is formed in a tubular shape and extends in the direction of the central axis O. The outer cylindrical member 2 has a first inner cavity 21. The first inner cavity 21 extends in the direction of the central axis O with the same diameter. The outer cylindrical member 2 is capable of transmitting laser light L. In this embodiment, the outer cylindrical member 2 is constituted by, for example, an intermediate connector 13 made of resin.
[0021] The inner cylindrical member 3 is formed in a tubular shape and extends in the direction of the central axis O. The inner cylindrical member 3 is inserted into the first lumen 21 of the outer cylindrical member 2 with its outer peripheral surface in contact with the first lumen 21. The inner cylindrical member 3 has a second lumen 31. The second lumen 31 extends in the direction of the central axis O with the same diameter. The inner cylindrical member 3 is capable of transmitting laser light L. In this embodiment, the inner cylindrical member 3 is formed of, for example, a long resin tube 15.
[0022] The outer cylindrical member 2 and the inner cylindrical member 3 are molded bodies made of a resin material. The resin materials forming the outer cylindrical member 2 and the inner cylindrical member 3 may be the same type of resin material or different types of resin materials. The outer cylindrical member 2 and the inner cylindrical member 3 are made of, for example, a polyolefin resin such as polypropylene (PP) or a resin such as polycarbonate (PC).
[0023] In this embodiment, as shown in Fig. 3, for example, the outer cylindrical member 2 has an outer diameter of Do, an inner diameter of Di, and a refractive index of Na. Also, for example, the inner cylindrical member 3 has an outer diameter of do, an inner diameter of di, and a refractive index of Nb.
[0024] In this embodiment, for example, both the outer cylindrical member 2 and the inner cylindrical member 3 are formed of the same homogeneous resin material, such as polypropylene (PP), so that the refractive index Na ≈ refractive index Nb. For example, in the case of polypropylene (PP), the refractive index is 1.48. Even when the refractive index Na ≠ refractive index Nb, the refraction angle based on Snell's law is calculated at the boundary between the outer cylindrical member 2 and the inner cylindrical member 3, and the distance x (described later) is controlled so that the refracted laser light is irradiated at an irradiation angle such that the incidence angle θ of the refracted laser light on the inner circumference of the inner cylindrical member 3 is equal to or greater than the Brewster angle between the inner cylindrical member 3 and the air, as described later, to obtain the same effect.
[0025] Furthermore, when both the outer cylindrical member 2 and the inner cylindrical member 3 are made of a resin material, even if the types of resin materials are different, the difference in refractive index between different types of resin materials is almost negligible compared to the difference in refractive index between the resin material and the air. Therefore, even if the types of resin materials for the outer cylindrical member 2 and the inner cylindrical member 3 are different, the refractive index Na of the outer cylindrical member 2 and the refractive index Nb of the inner cylindrical member 3 can be approximated to be almost the same.
[0026] When the outer cylindrical member 2 and the inner cylindrical member 3 are joined by the laser joining method of the present invention, the laser joining method performs an insertion step, a rotation step, and a laser irradiation step to join the outer cylindrical member 2 and the inner cylindrical member 3. In this way, a laser-joined molded product 1 is manufactured.
[0027] In the insertion step, as shown in Figures 2 and 3, at least a portion of the inner cylindrical member 3 is inserted into the first inner cavity 21 of the outer cylindrical member 2. More specifically, in the insertion step, as shown in Figures 2 and 3, a portion on one end side of the inner cylindrical member 3 is inserted into the first inner cavity 21 of the outer cylindrical member 2 with its outer peripheral surface in contact with the first inner cavity 21. As a result, a portion of the outer cylindrical member 2 and a portion of the inner cylindrical member 3 overlap each other in the radial direction.
[0028] 3, in a state in which at least a portion of the inner cylindrical member 3 is inserted into the first lumen 21 of the outer cylindrical member 2, the outer cylindrical member 2 and the inner cylindrical member 3 are rotated together around the central axis O of the outer cylindrical member 2 and the inner cylindrical member 3 as the center of rotation. In this embodiment, in the rotating step, the outer cylindrical member 2 and the inner cylindrical member 3 are rotated together in the clockwise direction around the central axis O of the outer cylindrical member 2 and the inner cylindrical member 3 as the center of rotation.
[0029] 3, in the laser irradiation step, a portion where the outer cylindrical member 2 and the inner cylindrical member 3 are overlapped with each other in the outer cylindrical member 2 and the inner cylindrical member 3 being rotated in the rotation step is irradiated with laser light L from the outside in the radial direction of the outer cylindrical member 2. In the laser irradiation step, the laser light L is irradiated at an irradiation angle such that the angle of incidence θ on the inner circumference of the inner cylindrical member 3 is equal to or larger than the Brewster angle between the inner cylindrical member 3 and the air.
[0030] As the laser light, a laser light having a wavelength (700 to 4000 nm) in the near infrared region or mid-infrared region can be used, and for example, a laser light having a wavelength of 1200 to 2500 nm is preferable. For example, a Tm laser (thulium laser, wavelength: 2000 nm) having a suitable absorptivity can be used as the laser light, taking into consideration the absorptivity to the resin material. The amount of heat generated by the laser light is at a level that melts the inner circumferential surface of the outer cylindrical member 2 and the outer circumferential surface of the inner cylindrical member 3. However, the amount of heat generated by the laser light is preferably at a level that does not directly melt the inner periphery (second lumen 31) of the inner cylindrical member 3 due to attenuation in the middle of the optical path of the laser light.
[0031] The Brewster angle is the angle of incidence at which the reflectance of P polarization becomes 0 (zero) at the boundary surface between two materials with different refractive indices. When the angle of incidence of the laser light L is equal to or larger than the Brewster angle, the reflectance increases rapidly, and the amount of light transmitted to the air in the second lumen 31 decreases. This makes it possible to prevent the second lumen 31 of the inner cylindrical member 3 from melting and deforming.
[0032] The Brewster angle θB is generally expressed by the following equation (1). Brewster angle θB = Arctan(n2 / n1) (1) In formula (1), n1 is the refractive index on the incident side, and n2 is the refractive index on the transmitting side. For example, the Brewster angle θB of laser light passing from polypropylene (PP) with a refractive index of 1.48 to air with a refractive index of 1 is approximately 34.0°.
[0033] 3, for example, when the position of the laser light L when its optical path is incident on the outer cylindrical member 2 at an incident angle of 90 degrees and passes through the central axis O of the outer cylindrical member 2 and the inner cylindrical member 3 is taken as a reference position RP, the laser light L is irradiated in parallel with the laser light L passing through the reference position RP at a position shifted by a distance x1 from the reference position RP on a plane perpendicular to the direction of the central axis O between the incident position of the irradiated laser light L on the outer cylindrical member 2 and the reference position RP. The position shifted by the distance x1 from the reference position RP is a position at which the laser light L is irradiated, which is calculated in advance, in order to set the Brewster angle θB to a desired angle.
[0034] As a result, for example, laser light L incident at a distance x1 from the reference position RP is incident at an incident angle α with respect to the perpendicular to the surface of the outer cylindrical member 2 at the incident position P, and according to Snell's law, is refracted at a refraction angle β, penetrates the interior of the outer cylindrical member 2, passes through the boundary a between the outer cylindrical member 2 and the inner cylindrical member 3, and penetrates into the interior of the inner cylindrical member 3.
[0035] The laser light L that has passed through into the inside of the inner cylindrical member 3 is irradiated at an irradiation angle such that the incident angle θ at the incident position C1 on the inner circumference of the second lumen 31 of the inner cylindrical member 3 is equal to or greater than the Brewster's angle between the inner cylindrical member 3 and air.
[0036] At the incident position C1 on the inner circumference of the second lumen 31 of the inner cylindrical member 3, the reflected light from the inner surface of the second lumen 31 is reflected at a reflection angle θ that is the same as the incident angle θ, and is refracted at the inner surface of the second lumen 31 to be incident inside the second lumen 31.
[0037] The laser light L refracted at the inner circumferential surface of the second lumen 31 and incident on the second lumen 31 is refracted in the opposite direction to the center side of the second lumen 31 at an incident position C1 on the inner circumference of the second lumen 31 of the inner cylindrical member 3. The laser light L refracted to the inside of the second lumen 31 is refracted in the opposite direction to the center side of the second lumen 31 and is re-incident on the inner cylindrical member 3 at an incident position C2 on the inner circumference of the second lumen 31 of the inner cylindrical member 3. The incidence angle and refraction angle of the laser light L are calculated taking into consideration the refractive index of the outer cylindrical member 2 and the refractive index of the inner cylindrical member 3.
[0038] Next, a brief description will be given of the overall flow of the laser joining method of the present invention. The laser joining method of this embodiment is a method for joining an outer cylindrical member 2 and an inner cylindrical member 3 by welding them with a laser.
[0039] First, at least a portion of the inner cylindrical member 3 is inserted and positioned in the first inner cavity 21 inside the outer cylindrical member 2 (insertion step). As a result, at least a portion of the inner cylindrical member 3 and at least a portion of the outer cylindrical member 2 are positioned in a radially overlapping state.
[0040] Next, the outer cylindrical member 2 and the inner cylindrical member 3 are rotated together, for example, as shown in FIG. 3, about the central axis O of the outer cylindrical member 2 and the inner cylindrical member 3 (rotation step).
[0041] Next, the overlapping portion of the outer cylindrical member 2 and the inner cylindrical member 3 is irradiated with laser light L from the outside in the radial direction of the outer cylindrical member 2 (laser light irradiation step).
[0042] Here, the laser light L is irradiated at a position shifted by x1 from the reference position RP in parallel with the laser light passing through the reference position RP. As a result, the laser light L transmitted into the inside of the inner cylindrical member 3 is irradiated at an irradiation angle such that the incident angle θ at the incident position C1 on the inner circumference of the second lumen 31 of the inner cylindrical member 3 is equal to or larger than the Brewster angle between the inner cylindrical member 3 and air.
[0043] As a result, at an incidence position C1 on the inner circumference of the second lumen 31 of the inner cylindrical member 3, the laser light is reflected from the inner peripheral surface of the second lumen 31 at a reflection angle θ and is refracted inside the second lumen 31. The light refracted inside the second lumen 31 is refracted in the opposite direction to the center side of the second lumen 31. Then, the laser light L refracted in the opposite direction to the center side of the second lumen 31 is re-incident on the inner cylindrical member 3 at an incidence position C2 on the inner circumference of the second lumen 31 of the inner cylindrical member 3.
[0044] Therefore, the laser-bonded molded product 1 can be manufactured by satisfactorily bonding the outer cylindrical member 2 and the inner cylindrical member 3 while suppressing melting and deformation of the second lumen 31 of the inner cylindrical member 3. The laser-bonded molded product 1 is manufactured by bonding the outer cylindrical member 2 and the inner cylindrical member 3 so that the blockage rate of the second lumen 31 of the inner cylindrical member 3 is less than 50%.
[0045] The occlusion rate of the second lumen 31 of the inner cylindrical member 3 is the percentage of occlusion of the second lumen 31 relative to the diameter of the second lumen 31 of the inner cylindrical member 3 before the outer cylindrical member 2 and the inner cylindrical member 3 are joined, with a state in which the second lumen 31 is not occluded at all being taken as 0% and a state in which the second lumen 31 is completely occluded being 100%. If the occlusion rate of the second lumen 31 of the inner cylindrical member 3 is less than 50%, transport performance for transporting liquids and gases can be ensured.
[0046] According to the laser joining method of the present embodiment described above, the following effects are achieved.
[0047] The laser joining method of this embodiment includes an insertion step of welding and joining an outer cylindrical member 2 having a first inner cavity 21 and an inner cylindrical member 3 having a second inner cavity 31 by irradiating them with laser light L, and inserting at least a portion of the inner cylindrical member 3 into the first inner cavity 21; a rotation step of rotating the outer cylindrical member 2 and the inner cylindrical member 3 integrally; and a laser irradiation step of irradiating the laser light L from the radial outside of the outer cylindrical member 2 to the overlapping portion of the outer cylindrical member 2 and the inner cylindrical member 3 being rotated in the rotation step, where the outer cylindrical member 2 and the inner cylindrical member 3 overlap. In the laser irradiation step, the laser light L is irradiated at an irradiation angle such that the incident angle θ on the inner circumference of the inner cylindrical member 3 is equal to or greater than the Brewster's angle between the inner cylindrical member 3 and the air.
[0048] As a result, since the incidence angle θ of the laser light L is an irradiation angle equal to or larger than the Brewster angle, the reflectance increases rapidly, and the amount of light transmitted to the air in the second lumen 31 is reduced. This makes it possible to prevent the second lumen 31 of the inner cylindrical member 3 from melting and deforming. Therefore, the outer cylindrical member 2 and the inner cylindrical member 3 can be joined by welding at the boundary a between the outer cylindrical member 2 and the inner cylindrical member 3, while preventing deformation of the second lumen 31 of the inner cylindrical member 3.
[0049] Furthermore, the laser-bonded molded product 1 of this embodiment is manufactured by irradiating the laser light L at an irradiation angle in the laser irradiation step of the laser bonding method such that the angle of incidence on the inner circumference of the inner cylindrical member 3 is equal to or larger than the Brewster angle between the inner cylindrical member 3 and the air, so that the blockage rate of the second lumen 31 of the inner cylindrical member 3 is less than 50%. This makes it possible to manufacture a good laser-bonded molded product 1 in which deformation of the second lumen 31 of the inner cylindrical member 3 is suppressed.
[0050] The present invention is not limited to the above-described embodiment, and includes modifications and improvements within the scope of the present invention that can achieve the object of the present invention. EXAMPLES
[0051] The present invention will be described in detail below with reference to examples, but the present invention is not limited to these examples. Examples and comparative examples of the laser joining method according to the present invention will be described.
[0052] In the examples and comparative examples, with a part of the inner cylindrical member 3 inserted into the first inner cavity 21 inside the outer cylindrical member 2, the outer cylindrical member 2 and the inner cylindrical member 3 were rotated together clockwise, and the laser light L was irradiated onto the outer peripheral surface of the outer cylindrical member 2 under the following test conditions. In this way, a laser-bonded molded product 1 was produced.
[0053] In the examples and comparative examples, the outer cylindrical member 2 had an outer diameter (Do) of 5.35 mm, an inner diameter (Di) of 2.7 mm, was made of polypropylene (PP) and had a refractive index of 1.48. The inner cylindrical member 3 had an outer diameter (do) of 2.7 mm, an inner diameter (di) of 1.0 mm, was made of polypropylene (PP) and had a refractive index of 1.48. The outer cylindrical member 2 and the inner cylindrical member 3 were rotated one and a half revolutions at a rotation speed of 3.5 mm / s. The scanning width of the laser light L was 1 mm.
[0054] 3, the rotation direction of the outer cylindrical member 2 and the inner cylindrical member 3 is a direction in which the irradiated laser light L rotates from the incident position P of the laser light L on the outer cylindrical member 2 toward the reference position RP when the incident position P of the laser light L on the first cylindrical member 2 is located at a position shifted from the reference position RP when the laser light passes through the central axis O of the outer cylindrical member 2 and the inner cylindrical member 3. In this embodiment, the outer cylindrical member 2 and the inner cylindrical member 3 are rotated clockwise.
[0055] <Test conditions> In Example 1, as shown in FIG. 4, laser light L was irradiated at an irradiation angle such that the incident angle θ on the inner circumference of the inner cylindrical member 3 was equal to or larger than the Brewster angle between the inner cylindrical member 3 and air. In Comparative Example 1, the laser light L was irradiated at an irradiation angle such that the incident angle θ on the inner circumference of the inner cylindrical member 3 was less than the Brewster angle between the inner cylindrical member 3 and air.
[0056] <Test Results> As shown in Fig. 4, in Example 1, no deformation or collapse occurred in the second lumen 31 of the inner cylindrical member 3 (blockage rate less than 50%) (judgment: OK). The laser light L passed through the boundary between the outer cylindrical member 2 and the inner cylindrical member 3, and the outer cylindrical member 2 and the inner cylindrical member 3 were satisfactorily joined (joining state: OK). Therefore, in Example 1, the outer cylindrical member 2 and the inner cylindrical member 3 were satisfactorily joined without any deformation or collapse occurring in the second lumen 31 of the inner cylindrical member 3, and the overall judgment was good (OK).
[0057] In other words, in Example 1, when the laser light L passes through the boundary where the outer cylindrical member 2 (first cylindrical member) and the inner cylindrical member 3 (second cylindrical member) overlap, and the well-joined laser-joined molded body 1 is cut along the radial direction of the outer cylindrical member 2 and the inner cylindrical member 3, the cross section shows little deformation of the second inner cavity 31 of the inner cylindrical member 3, and the overlapping portion of the outer cylindrical member 2 and the inner cylindrical member 3 is melted and joined.
[0058] In Comparative Example 1, the second lumen 31 of the inner cylindrical member 3 was deformed, crushed, and clogged (100% blockage rate) (Judgment: NG). The laser light L passed through the boundary between the outer cylindrical member 2 and the inner cylindrical member 3, and the outer cylindrical member 2 and the inner cylindrical member 3 were joined well (joining state: OK). Therefore, since the second lumen 31 of the inner cylindrical member 3 was deformed, crushed, and clogged due to the transmission of the laser light L, the overall judgment was poor (NG).
[0059] From the above test results, it was found that, with regard to the deformation of the second lumen 31 of the inner cylindrical member 3, when the laser light L is irradiated at an irradiation angle where the incident angle θ on the inner circumference of the inner cylindrical member 3 is equal to or greater than the Brewster angle between the inner cylindrical member 3 and air, the second lumen 31 of the inner cylindrical member 3 is not deformed or crushed, as in Example 1, and therefore the deformation of the second lumen 31 of the inner cylindrical member 3 can be suppressed. On the other hand, when the laser light L is irradiated at an irradiation angle where the incident angle θ on the inner circumference of the inner cylindrical member 3 is less than the Brewster angle between the inner cylindrical member 3 and air, the second lumen 31 of the inner cylindrical member 3 is deformed, crushed, and blocked, as in Comparative Example 1, and therefore the deformation of the second lumen 31 of the inner cylindrical member 3 cannot be suppressed. [Explanation of symbols]
[0060] 1 Laser-bonded molded product 2 Outer cylindrical resin molded body (first cylindrical member) 3. Inner cylindrical resin molded body (second cylindrical member) 21 1st lumen 31 Second lumen L Laser light O center axis
Claims
1. A laser joining method for joining a first cylindrical member having a first inner cavity and capable of transmitting laser light to a second cylindrical member having a second inner cavity and capable of transmitting laser light by irradiating the first cylindrical member with laser light, the method comprising the steps of: an inserting step of inserting at least a portion of the second cylindrical member into the first cavity with an outer circumferential surface of the second cylindrical member in contact with the first cavity; a rotating step of rotating the first cylindrical member and the second cylindrical member integrally about central axes of the first cylindrical member and the second cylindrical member; a laser irradiation step of irradiating a laser beam from a radial outside of the first cylindrical member to an overlapping portion of the first cylindrical member and the second cylindrical member being rotated in the rotation step, A laser joining method, wherein in the laser irradiation step, the laser light is irradiated at an irradiation angle such that the angle of incidence on the inner circumference of the second cylindrical member is equal to or greater than the Brewster angle between the second cylindrical member and air.
2. A laser-joined molded product manufactured by a laser joining method in which a first cylindrical member having a first inner cavity and capable of transmitting laser light and a second cylindrical member having a second inner cavity and capable of transmitting laser light are welded and joined by irradiating the first cylindrical member with a laser light, The laser joining method includes: an inserting step of inserting at least a portion of the second cylindrical member into the first cavity with an outer circumferential surface of the second cylindrical member in contact with the first cavity; a rotating step of rotating the first cylindrical member and the second cylindrical member integrally about central axes of the first cylindrical member and the second cylindrical member; a laser irradiation step of irradiating a laser beam from a radial outside of the first cylindrical member to an overlapping portion of the first cylindrical member and the second cylindrical member being rotated in the rotation step, In the laser irradiation process, a laser-bonded molded body is produced by irradiating laser light at an irradiation angle such that the angle of incidence on the inner circumference of the second cylindrical member is equal to or greater than the Brewster's angle between the second cylindrical member and air, so that the blockage rate of the second inner cavity is less than 50%.
Citation Information
Patent Citations
Method for coating welded joint part for pipe
JP1995091589A
Weld joint for fuel tank
JP2009132200A
CATHETER HAVING A MULTI-SECTION TUBULAR MEMBER AND METHOD OF MANUFACTURE THEREOF
JP2009533200A
Bonding device
JP2010162832A
Medical instrument and method for manufacturing medical instrument
JP2013180158A