Method for manufacturing liquid crystal polymer molded product
The method of purging with specific resin compositions and mold adjustments reduces gas entrainment and delamination in liquid crystalline polymer molded products, effectively suppressing blistering and improving thermal stability.
Patent Information
- Application Number
- JP2021004906
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2021-01-15
- Publication Date
- 2024-12-09
- Estimated Expiration
- 2041-01-15
AI Technical Summary
Liquid crystalline polymer molded products experience blistering during heating due to gases generated from decomposition of residual foreign matter and molecular structure, which existing methods fail to adequately address.
A method involving specific purging sequences with polycarbonate, polyethylene, and styrene resin compositions, along with mold design adjustments, to reduce gas entrainment and delamination, ensuring the total gas collected during injection molding is 20 μg/g or less.
Effectively suppresses blistering in liquid crystalline polymer molded products by minimizing gas generation and delamination, enhancing thermal stability and reliability.
Smart Images

Figure 0007596030000001 
Figure 0007596030000002 
Figure 0007596030000003
Abstract
Description
[Technical field]
[0001] The present invention relates to a method for producing a liquid crystal polymer molded article, and more particularly to a method for producing a liquid crystal polymer molded article that effectively reduces blisters that may occur when the liquid crystal polymer molded article is heated. [Background technology]
[0002] Liquid crystal polymers have been used as materials for various electronic components because of their excellent heat resistance, flame retardancy, dimensional accuracy, and fluidity. Liquid crystal polymers have high fluidity that can accommodate the miniaturization and thinning of electronic components, and high heat resistance that allows reflow soldering, so demand is growing for applications such as surface mount connectors. Many liquid crystal polymer compositions have been developed that improve low warpage and electrical properties by blending various fillers and additives with liquid crystal polymers.
[0003] However, when a liquid crystal polymer molded article is heated, for example, when it is processed in a high-temperature environment such as lead-free reflow soldering, there are cases where swelling called blisters occurs on the surface of the molded article, which can be problematic.
[0004] One of the causes of the occurrence of blisters is a mechanism in which gas generated by decomposition of the liquid crystal polymer itself or its additives during the process of filling the liquid crystal polymer composition into a mold during injection molding is entrained in the liquid crystal polymer composition in a molten flow state and taken into the molded article, and the gas expands due to heating during reflow soldering, pushing up the surface of the molded article softened by heating. As a countermeasure against blisters caused by the decomposition gas of the liquid crystal polymer composition, in addition to material approaches such as the structure of the liquid crystal polymer and the type of filler and additives contained in the liquid crystal polymer composition, improvements in molding methods such as vent degassing during melt extrusion and shortening the residence time during molding have been considered (Patent Documents 1 to 5).
[0005] In addition to the decomposition gas of the liquid crystal polymer composition, air that exists in the mold is not properly discharged when the liquid crystal polymer composition is filled, and is taken into the molded product, which is also a cause of blisters, so that in order to prevent this, a manufacturing method for a molded product has been proposed in which the molding conditions and the structures of the molding machine and mold are adjusted so as to satisfy a specific relational expression (Patent Document 6).On the other hand, a liquid crystal resin composition has also been proposed in which the flow state of the liquid crystal polymer composition injected into the mold is specified (Patent Document 7).
[0006] However, even if these measures are taken, it is sometimes difficult to prevent the occurrence of blisters when a liquid crystal polymer molded article is heated. [Prior art documents] [Patent documents]
[0007] [Patent Document 1] Japanese Patent Application Publication No. 11-140283 [Patent Document 2] JP 2004-196886 A [Patent Document 3] JP 2016-089154 A [Patent Document 4] JP 2016-183308 A [Patent Document 5] JP 2018-095683 A [Patent Document 6] JP 2010-253890 A [Patent Document 7] International Publication WO2019 / 203157 Brochure Summary of the Invention [Problem to be solved by the invention]
[0008] An object of the present invention is to provide a method for producing a liquid crystal polymer molded article, which effectively reduces the occurrence of blisters when the liquid crystal polymer molded article is heated. [Means for solving the problem]
[0009] For this purpose, the present inventors have conducted extensive analysis of gases generated during injection molding, and have found that even if a liquid crystal polymer composition that suppresses the generation of decomposition gases is used, or if a mold design or molding conditions that reduce air entrapment in the mold are used, blisters in liquid crystal polymer molded products may not be completely prevented. The inventors have found that the cause of this is gas derived from components other than the liquid crystal polymer composition that is actually molded, specifically, gas derived from a material that was injection molded in the molding machine before molding the liquid crystal polymer composition, or gas derived from a purging agent when switching from that material to the liquid crystal polymer composition.
[0010] Usually, when materials are changed in an injection molding machine, if the material is changed by purging in an appropriate procedure, the generation of gas due to such residual foreign matter in the cylinder (such as resin material previously molded or purging agent) rarely becomes a problem. However, since the liquid crystal polymer itself has a low viscosity and its fluidity is highly dependent on the injection speed, even if the liquid crystal polymer is purged at a high injection speed, it is difficult to obtain the effect of scraping off and discharging the residual foreign matter in the cylinder. On the other hand, even if residual foreign matter exists in the cylinder, if the molding temperature of the material to be molded next is lower than the heat resistance temperature of the residual foreign matter, the risk of the residual foreign matter melting or decomposing is reduced. However, liquid crystal polymers belong to a class of resins that are particularly high in heat resistance, and the molding temperature is inevitably high, so that the residual foreign matter is likely to thermally decompose under the molding conditions, and as a result, gas derived from components other than the liquid crystal polymer composition as described above is likely to be generated.
[0011] In addition, in liquid crystal polymers, a highly molecular-oriented structure called a skin layer is formed on the surface layer of the molded product during injection molding due to its molecular structure. If the above-mentioned generated gas is entrained between the skin layer and the core layer inside the molded product, blisters are likely to occur due to delamination. In other words, liquid crystal polymer molded products are fundamentally more likely to generate blisters than molded products made of other resins due to reasons from the molding conditions (ease of generation of decomposition gas due to high processing temperature) and reasons from the molecular structure (ease of delamination between the skin layer and the core layer). However, in terms of molecular structure, it is the orientation that gives the liquid crystal polymer excellent specific physical properties, and it is difficult to avoid this. Therefore, the present inventors have found that suppressing the generation of gas derived from residual foreign matter and preventing the promotion of delamination due to the entrainment is effective in reducing blisters derived from causes specific to liquid crystal polymers.
[0012] The present invention is characterized as follows: The amount of gas (μg / g) in the present invention means the amount of gas generated per 1 g of liquid crystalline polymer composition, which is calculated by dividing the amount of gas (μg) collected during molding of a liquid crystalline polymer molded article by the weight (g) of the liquid crystalline polymer molded article obtained by molding the specific number of shots.
[0013] (1) A method for producing a liquid crystalline polymer molded article, comprising injection molding a liquid crystalline polymer composition using a mold having a gate, a cavity, and a gas vent, characterized in that a total amount of gas captured in the gas vent during the injection molding is 20 μg / g or less.
[0014] (2) The method for producing a liquid crystal polymer molded product according to (1), characterized in that in the injection molding, the total amount of gas is set to 20 μg / g or less by at least one of lowering the cylinder temperature and / or injection speed of the molding machine, or increasing the size and / or number of gates of the mold.
[0015] (3) The method for producing the liquid crystal polymer molded article according to (1) or (2), characterized in that, in the injection molding, before injection molding of the liquid crystal polymer composition, purging with (a) a polycarbonate resin composition containing glass fiber and purging with the liquid crystal polymer composition (b) are carried out in this order.
[0016] (4) The method for producing a liquid crystal polymer molded article according to (3), characterized in that, before purging with the (a) polycarbonate resin composition, purging with the (b) liquid crystal polymer composition, or purging with the (c) polyethylene-based resin composition, or purging with the (d) styrene-based resin composition is further carried out.
[0017] (5) A method for producing a liquid crystal polymer molded product according to (4), characterized in that an additional purge is carried out before the purge with the liquid crystal polymer composition (b), before the purge with the polyethylene resin composition (c), or before the purge with the styrene-based resin composition (d), which is carried out before the purge with the polycarbonate resin composition (a), and the additional purge is at least one selected from the group consisting of a purge with the polycarbonate resin composition (a), a purge with the liquid crystal polymer composition (b), a purge with the polyethylene resin composition (c), and a purge with the styrene-based resin composition (d), which is different from the purge carried out immediately after the additional purge.
[0018] (6) In the case where the purging with the (c) polyethylene-based resin composition and / or the (d) styrene-based resin composition is carried out, the method for producing a liquid crystal polymer molded product according to (4) or (5) is characterized in that after the purging with the (c) polyethylene-based resin composition and / or the (d) styrene-based resin composition, the screw of the molding machine is cleaned.
[0019] (7) A method for suppressing blisters in a liquid crystal polymer molded product when a liquid crystal polymer composition is injection molded using a mold having a gate, a cavity, and a gas vent to produce the liquid crystal polymer molded product, the method being characterized in that the total amount of gas captured in the gas vent during the injection molding is 20 μg / g or less.
[0020] (8) The method for suppressing blisters in a liquid crystal polymer molded product according to (7), characterized in that in the injection molding, the total gas amount is set to 20 μg / g or less by at least one of reducing the cylinder temperature and / or injection speed of the molding machine, or increasing the size and / or number of gates of the mold.
[0021] (9) The method for suppressing blisters in a liquid crystal polymer molded product according to (7) or (8), characterized in that, in the injection molding, purging with (a) a polycarbonate resin composition containing glass fiber and purging with (b) the liquid crystal polymer composition are carried out in this order before injection molding of the liquid crystal polymer composition.
[0022] (10) The method for suppressing blisters in a liquid crystal polymer molded product according to (9), characterized in that, prior to purging with the (a) polycarbonate resin composition, purging with the (b) liquid crystal polymer composition, or purging with the (c) polyethylene-based resin composition, or purging with the (d) styrene-based resin composition is further carried out.
[0023] (11) The method for suppressing blisters in a liquid crystal polymer molded product according to (10), characterized in that an additional purge is performed before the purge with the (b) liquid crystal polymer composition, before the purge with the (c) polyethylene-based resin composition, or before the purge with the (d) styrene-based resin composition, which is performed before the purge with the (a) polycarbonate resin composition, and the additional purge is at least one selected from the group consisting of a purge with the (a) polycarbonate resin composition, a purge with the (b) liquid crystal polymer, a purge with the (c) polyethylene-based resin composition, and a purge with the (d) styrene-based resin composition, which is different from the purge performed immediately after the additional purge.
[0024] (12) In the case where the purging with the (c) polyethylene-based resin composition and / or the (d) styrene-based resin composition is carried out, the method for suppressing blisters in a liquid crystal polymer molded product according to (10) or (11) is characterized in that after the purging with the (c) polyethylene-based resin composition and / or the (d) styrene-based resin composition, the screw of the molding machine is cleaned. Effect of the Invention
[0025] According to the present invention, by controlling the amount of gas discharged during injection molding of a liquid crystalline polymer composition to be equal to or less than a specific value, the risk of gas generated due to the decomposition of residual foreign matter in the cylinder, etc., being entrained in the liquid crystalline polymer molded product can be reduced, and the occurrence of blisters when the liquid crystalline polymer molded product is heated can be effectively suppressed. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0026] The embodiments will be described in detail below. One embodiment is a method for producing a liquid crystalline polymer molded article, which comprises injection molding a liquid crystalline polymer composition using a mold having a gate, a cavity, and a gas vent, and is characterized in that the total amount of gas collected in the gas vent during the injection molding is 20 μg / g or less.
[0027] The liquid crystal polymer constituting the liquid crystal polymer composition molded in the embodiment is not particularly limited as long as it is a melt-processable polymer having the property of being able to form an optically anisotropic molten phase, but is preferably an aromatic polyester or an aromatic polyester amide. Also, a polyester partially containing an aromatic polyester or an aromatic polyester amide in the same molecular chain can be used.
[0028] The aromatic polyester or aromatic polyesteramide is particularly preferably an aromatic polyester or aromatic polyesteramide having at least one compound selected from the group consisting of aromatic hydroxycarboxylic acid, aromatic hydroxyamine, and aromatic diamine as a constituent component. The liquid crystal polymer may be a mixture of two or more liquid crystal polymers selected from the above.
[0029] More specifically, (1) (a) Polyesters mainly composed of one or more aromatic hydroxycarboxylic acids and their derivatives; (2) polyesters obtained by polymerizing mainly (a) one or more aromatic hydroxycarboxylic acids and their derivatives, (b) one or more aromatic dicarboxylic acids, alicyclic dicarboxylic acids, and their derivatives, and (c) at least one or more aromatic diols, alicyclic diols, aliphatic diols, and their derivatives; (3) polyesteramides obtained by polymerizing mainly (a) one or more aromatic hydroxycarboxylic acids and their derivatives, (b) one or more aromatic dicarboxylic acids, alicyclic dicarboxylic acids, and their derivatives, and (c) one or more aromatic hydroxyamines, aromatic diamines, and their derivatives; (4) Mainly, examples include polyesteramides obtained by polymerizing (a) one or more aromatic hydroxycarboxylic acids and their derivatives, (b) one or more aromatic dicarboxylic acids, alicyclic dicarboxylic acids, and their derivatives, (c) at least one or more aromatic diols, alicyclic diols, aliphatic diols, and their derivatives, and (d) one or more aromatic hydroxyamines, aromatic diamines, and their derivatives. Furthermore, a molecular weight modifier may be used in combination with the above-mentioned components as necessary.
[0030] Preferable specific examples of the compound (monomer compound) constituting the liquid crystal polymer include: (A) Aromatic hydroxycarboxylic acids such as p-hydroxybenzoic acid and 6-hydroxy-2-naphthoic acid, (c) Aromatic diols such as 2,6-dihydroxynaphthalene, 1,4-dihydroxynaphthalene, 4,4'-dihydroxybiphenyl, hydroquinone, resorcinol, compounds represented by the following general formula (I), and compounds represented by the following general formula (II): (a) Aromatic dicarboxylic acids such as terephthalic acid, isophthalic acid, 4,4'-diphenyldicarboxylic acid, 2,6-naphthalenedicarboxylic acid, and compounds represented by the following general formula (III), (d) Aromatic amines such as p-aminophenol and p-phenylenediamine. [ka] (X is a group selected from alkylene (C1 to C4), alkylidene, -O-, -SO-, -SO2-, -S-, and -CO-) [ka] [ka] (Y:-(CH2) n -(n=1 to 4) and -O(CH2) n O-(n=1 to 4).
[0031] The method for preparing the liquid crystal polymer is not particularly limited, and the above-mentioned monomer compounds are selected and mixed to obtain the above-mentioned combination to prepare a monomer mixture, which can be polymerized by a known method such as a direct polymerization method or an ester exchange method. The monomer mixture is usually polymerized by a melt polymerization method or a slurry polymerization method. When the monomer compound is a compound capable of forming an ester, it can be used in the polymerization in its original form, or a compound modified from a precursor to a derivative capable of forming an ester in a pre-polymerization stage may be used. Various catalysts can be used when polymerizing the monomer mixture. Representative examples of catalysts that can be used include dialkyltin oxide, diaryltin oxide, titanium dioxide, alkoxytitanium silicates, titanium alcoholates, alkali and alkaline earth metal salts of carboxylic acids, Lewis acid salts such as BF3, and the like. The amount of the catalyst used is generally about 0.001 to 1% by mass, and particularly about 0.01 to 0.2% by mass, based on the total weight of the monomer mixture. If necessary, the liquid crystal polymer produced by these polymerization methods can be further increased in molecular weight by solid-phase polymerization in which the polymer is heated under reduced pressure or in an inert gas.
[0032] The melt viscosity of the liquid crystal polymer is not particularly limited, and is preferably set at a cylinder temperature 10 to 30°C higher than the melting point of the liquid crystal polymer at a shear rate of 1000 sec -1The melt viscosity measured at is preferably 5 Pa·s or more and 100 Pa·s or less, more preferably 10 Pa·s or more and 50 Pa·s or less. "Cylinder temperature 10 to 30°C higher than the melting point of the liquid crystal polymer" means a cylinder temperature at which the liquid crystal polymer can be melted to a degree at which the melt viscosity can be measured, and the cylinder temperature higher than the melting point varies depending on the type of liquid crystal polymer within the range of 10 to 30°C. For example, JP 2010-3661 A (see especially paragraphs 0048 and 0051) discloses a liquid crystal polymer 1 containing 2 mol% of structural units introduced from 4-hydroxybenzoic acid, 48 mol% of structural units introduced from 6-hydroxy-2-naphthoic acid, 25 mol% of structural units introduced from terephthalic acid, and 25 mol% of structural units introduced from 4,4'-dihydroxybiphenyl. The melting point of this liquid crystal polymer 1 is 352°C, and the melt viscosity is measured at a cylinder temperature of 380°C. Also, as liquid crystal polymer 2, a liquid crystal polymer containing 50 mol% of structural units introduced from 4-hydroxybenzoic acid, 2.5 mol% of structural units introduced from 6-hydroxy-2-naphthoic acid, 23.9 mol% of structural units introduced from terephthalic acid, 18.6 mol% of structural units introduced from 4,4'-dihydroxybiphenyl, and 5 mol% of structural units introduced from 4-acetamidophenol is disclosed. The melting point of this liquid crystal polymer 2 is 367°C, and the melt viscosity is measured at a cylinder temperature of 380°C. Furthermore, as liquid crystal polymer 3, a liquid crystal polymer containing 60 mol% of structural units introduced from 4-hydroxybenzoic acid, 5 mol% of structural units introduced from 6-hydroxy-2-naphthoic acid, 17.7 mol% of structural units introduced from terephthalic acid, 112.3 mol% of structural units introduced from 4,4'-dihydroxybiphenyl, and 5 mol% of structural units introduced from 4-acetamidophenol is disclosed. The melting point of this liquid crystalline polymer 3 is 335°C, and the melt viscosity is measured at a cylinder temperature of 350°C.
[0033] In the embodiment, the liquid crystal polymer used is preferably a polymer with a narrow molecular weight distribution or a polymer with a small content of oligomers, because it can reduce the generation of gas due to the decomposition of low molecular weight components during melt kneading. In addition, when an additive selected from other resins such as alloy materials and elastomers and other components is added to the liquid crystal polymer to use it as a liquid crystal polymer composition, it is preferable to select an additive with a high melting point or high boiling point within a range that does not impair the properties of the liquid crystal polymer composition.
[0034] In the embodiment, injection molding is a method for molding a liquid crystalline polymer composition, in which a molten liquid crystalline polymer composition is fed into a mold and solidified by cooling. The injection molding in this embodiment can be performed using an injection molding machine such as that described in JP 2019-181890 A.
[0035] An injection molding machine that can be used in this embodiment is, for example, an in-line screw type, and has a cylinder extending in a substantially horizontal direction, a screw built into the cylinder, and a drive mechanism for rotating the screw, etc. The cylinder is provided with a hopper which is an inlet for the molding material, a band heater which heats the cylinder, and a nozzle which is an outlet for injecting the molten molding material into a mold.
[0036] The mold has a movable mold and a fixed mold corresponding to the movable mold. The fixed mold has a sprue, which is a flow path that guides the liquid crystal polymer composition injected from a nozzle at the end of the cylinder of the injection molding machine to the mating surface of the fixed mold and the movable mold. At the mating surface of the fixed mold and the movable mold, a space (cavity in the narrow sense) corresponding to the molded product main body, a gate which is an inlet to the molded product main body, and a runner which is a flow path from the sprue to the gate are provided across either or both of the fixed mold and the movable mold. In this specification, in addition to the molded product main body (cavity in the narrow sense), the entire area including the runner and sprue through the gate of the mold is referred to as the cavity. At least one of the fixed mold and the movable mold is provided with a mold gas vent that discharges gas from the cavity. The mold gas vent is formed of a porous material or fine pores. The mold gas vent may be provided in either the fixed or movable mold, but in order to efficiently exhaust gas, it is best to provide it near the flow end of the main body of the molded product. It is also desirable to install a vacuum pump via an exhaust path from the mold gas vent to suck out the gas from inside the mold.
[0037] In an injection molding machine, the liquid crystalline polymer composition in pellet form stored in a hopper falls under its own weight and is supplied to a cylinder located directly below the hopper. The cylinder is heated to a predetermined temperature by a band heater. The liquid crystalline polymer composition supplied to the cylinder is melted by heating by the band heater and by shear heat generated by the rotation of the screw while being transported by a rotating screw, and is kneaded by the screw, and is further injected from a nozzle into a mold as the screw advances. The liquid crystalline polymer composition injected into the mold fills the cavity of the mold, and is cooled and solidified, and then removed from the mold as a liquid crystalline polymer molded product.
[0038] In an embodiment, the liquid crystal polymer composition filled in the cavity of the mold may generate gas due to shear heating when passing through a gate or a thin wall of the cavity. This gas is discharged from the cavity through a mold gas vent formed in the mold. The mold exhaust gas discharged from the mold gas vent is exhausted through an exhaust path leading from the mold gas vent to a vacuum pump. In addition, a mold exhaust gas collection tube for collecting the mold exhaust gas is connected to the mold gas vent, and can collect the mold exhaust gas generated during injection molding. The mold exhaust gas collection tube may have an analysis device for qualitatively and / or quantitatively analyzing the gas discharged from the mold exhaust gas collection tube.
[0039] In the embodiment, the mold exhaust gas discharged from the cavity can be collected through the above-mentioned mold gas vent. The total amount of gas generated per 1 g of the liquid crystal polymer composition is expressed as the total gas amount (μg / g), which is calculated by dividing the total amount of gas (μg) collected during one shot of molding the liquid crystal polymer molded product by the weight (g) of the liquid crystal polymer composition injected during one shot.
[0040] Analysis of the mold exhaust gas collected through the mold gas vent can also be appropriately performed following the method described in JP 2019-181890 A (see especially paragraph 0038). In the present invention, the total amount of gas collected in the mold gas vent is 20 μg / g or less, preferably 15 μg / g or less, and more preferably 10 μg / g or less. In addition, of the total amount of gas, the amount of mixed gas other than that derived from the liquid crystalline polymer composition is preferably 5 μg / g or less, more preferably 3 μg / g or less, and even more preferably 1 μg / g or less. Here, whether the generated gas is derived from the liquid crystalline polymer composition can be determined by performing qualitative and / or quantitative analysis of the collected gas by a known method.
[0041] The conditions for injection molding the liquid crystal polymer composition can be adjusted so that the total amount of gas or the amount of mixed gas falls within the above ranges. Specifically, by lowering either or both of the cylinder temperature and the injection speed of the molding machine, the heat received by the liquid crystal polymer composition and the residual foreign matter in the cylinder can be reduced, and the generation of decomposition gas can be suppressed.
[0042] In order to make the total gas amount or the mixed gas amount fall within the above range, the size of the gate of the mold can be enlarged, or the number of gates can be increased, or both can be performed. By performing these, it is possible to reduce the shear heat generated when the liquid crystal polymer composition passes through the gate, and it is also possible to easily fill the liquid crystal polymer composition into the cavity, so that it is easy to adjust the resin temperature and injection speed as described above while ensuring moldability. In addition, it is preferable to use a coating such as DLC, TiN, TiCN, CrN, or ceramic as the surface treatment of the mold, since this can suppress decomposition due to shear heat on the mold surface.
[0043] In an embodiment, prior to injection molding of the liquid crystal polymer composition, residual foreign matter is removed by purging the inside of the cylinder. Purging is preferably performed in the order of (a) purging with a polycarbonate resin composition containing glass fiber and (b) purging with a liquid crystal polymer composition used for molding. More preferably, (a) the polycarbonate resin composition contains 10% by mass or more and 50% by mass or less of glass fiber.
[0044] As for the purging, it is also preferable to perform a purge with (b) a liquid crystal polymer composition, or a purge with (c) a polyethylene-based resin composition, or a purge with (d) a styrene-based resin composition before the above-mentioned (a) purging with a polycarbonate resin composition containing glass fibers. In order to more reliably discharge the residual foreign matter in the cylinder, it is preferable to perform an additional purge before the above-mentioned (a) purging with a polycarbonate resin composition, (b) a purge with a liquid crystal polymer composition, (c) a purge with a polyethylene-based resin composition, or (d) a purge with a styrene-based resin composition. It is more preferable that the additional purge is at least one of the following purges, which are different from the purge performed immediately after the additional purge: (a) a purge with a polycarbonate resin composition, (b) a purge with a liquid crystal polymer composition, (c) a purge with a polyethylene-based resin composition, or (d) a purge with a styrene-based resin composition. For example, a series of purging in the order (c)(d)(a)(b), where a purge (a) is followed by a purge (d) before a purge (b), with an additional purge (c) before the purge (d), or a series of purging in the order (c)(a)(d)(a)(b), where a purge (a) is followed by a purge (d) before a purge (b), with an additional purge (c) before the purge (d), and then a purge (a), are highly preferred.
[0045] As the polyethylene-based resin composition, in addition to homopolymers such as high density polyethylene (HDPE), low density polyethylene (LDPE), and linear low density polyethylene (LLDPE), copolymers obtained by copolymerizing ethylene with other monomers can be used. From the viewpoint of reducing gas derived from foreign matter such as additives contained in the purging agent itself, it is preferable to use a polyethylene homopolymer. In addition, in purging a liquid crystal polymer composition in which the cylinder temperature is set high, it is more preferable to use a high density polyethylene from the viewpoint of heat resistance. The polyethylene-based resin composition may contain a filler such as glass fiber. In particular, from the viewpoint of effectively discharging residual foreign matter in the cylinder, it is preferable that the polyethylene-based resin composition has a high viscosity, and the melt flow rate (MFR) measured in accordance with ISO1133 is preferably 3g / 10min or less, and more preferably 0.1g / 10min or more and 1g / 10min or less. In addition, as the styrene-based resin composition, it is preferable to use a styrene-based copolymer such as an acrylonitrile-styrene copolymer, and it may contain a filler such as glass fiber. After purging with the polyethylene-based resin composition or the styrene-based resin composition, it is preferable to disassemble and clean the screw. That is, when purging with (c) the polyethylene-based resin composition or (d) the styrene-based resin composition is performed in the series of purging, it is preferable to clean the screw of the molding machine after purging with the (c) the polyethylene-based resin composition or purging with the (d) the styrene-based resin composition.
[0046] The conditions of the molding machine during purging can be appropriately set by those skilled in the art by referring to the standard molding conditions of each liquid crystal polymer composition and each purging agent. For example, the screw rotation speed can be selected from the range of about 100 rpm to 300 rpm, the back pressure from about 0 MPa to 10 MPa, and the injection speed from about 5 mm / sec to 300 mm / sec. The cylinder temperature can be appropriately set within the range of the melting point to the decomposition temperature of the material and purging agent to be discharged from the cylinder, and the final molding material.
[0047] By carrying out the above-mentioned various adjustments, it becomes possible to effectively suppress the occurrence of blisters in the liquid crystal polymer molded article, which is caused by decomposition gases of residual foreign matter and the like in the cylinder. EXAMPLES
[0048] [Liquid crystal polymer composition] The following liquid crystal polymers and additives were mixed in the ratios shown in Table 1, and melt-kneaded at a cylinder temperature of 350° C. using a twin-screw extruder TEX-44 manufactured by The Japan Steel Works, Ltd. to obtain pellets of liquid crystal polymer compositions (LCP1 to 6). <Liquid crystal polymer> Polyplastics Co., Ltd., liquid crystal polymer with a melting point of 335°C, LAPEROS (registered trademark) E950iSX <Additives> GF: Chopped strands with an average fiber diameter of 10 μm and an average fiber length of 3 mm, manufactured by Nippon Electric Glass Co., Ltd., ECS03T-786H MF: Glass milled fiber with an average fiber diameter of 10 μm and an average fiber length of 70 μm, manufactured by Nitto Boseki Co., Ltd., PF 70E-001 Talc: Crown Talc PP (average particle size 12.8 μm), manufactured by Matsumura Sangyo Co., Ltd. Release agent: Pentaerythritol tetrastearate, LOXIOL VPG861, manufactured by Emery Oleochemicals Japan Co., Ltd.
[0049] [Table 1]
[0050] [purge] The cylinder was initially filled with the liquid crystal polymer composition (E130i), which is a liquid crystal polymer composition manufactured by Polyplastics Co., Ltd., and is molded at a cylinder temperature of 350°C. Purging was performed using the following purging agent and the above liquid crystal polymer composition (LCP compositions 1 to 6) in the combination and order shown in Table 2, and the inside of the cylinder was replaced with the liquid crystal polymer composition to be molded. The cylinder temperature during purging was the temperature listed for each material during purging in Table 2. When two temperatures are listed with an arrow between them, this means that purging was performed while increasing or decreasing the temperature from the temperature before the arrow to the temperature after the arrow. For example, in the case of "PC: 320°C → 350°C", purging was performed using the following polycarbonate resin composition while increasing the cylinder temperature from 320°C to 350°C. The screw rotation speed, back pressure, and other conditions were set appropriately based on the standard conditions disclosed by the manufacturer of each material, and purging was continued until it was possible to visually confirm that the resin discharged from the nozzle had completely replaced the previous material. <Purging agent> PC: Teijin Limited, polycarbonate resin composition containing 30% by mass of glass fiber, Panlite G3430 PE: Prime Polymer Co., Ltd., high-density polyethylene resin, Hi-Zex 6203B Styrene-based resin composition 1 (St1): Celpurge NX-VG2, manufactured by Daicel Miraize Co., Ltd. Styrene-based resin composition 2 (St2): Asahi Kasei Corporation, Asaclean newEX Styrene-based resin composition 3 (St3): Asaclean IMX, manufactured by Asahi Kasei Corporation
[0051] [Injection molding and gas analysis] A mold having a cavity in the fixed side mold, a mold gas vent connected to a mold exhaust gas collection tube, and an exhaust path connected to a vacuum pump was mounted on an injection molding machine S2000i-30A manufactured by FANUC Corporation, and injection molding of a liquid crystal polymer composition was performed continuously under the molding conditions shown in Table 2. The gates were installed at two locations on one long side end face of the mold, one-quarter (32.5 mm) and three-quarters (97.5 mm) from the end in the longitudinal direction, and side gates with a width of 1 mm and a thickness of 0.8 mm were installed. A rectangular molded piece of 130 mm x 13 mm x 0.8 mm was obtained by injection molding. The injection molding machine was operated continuously for a predetermined time, and the gas generated from the mold gas vent was vacuum-collected using a mold exhaust gas collection tube. The amount of generated gas was analyzed by gas chromatography (GC, column used: Agilent Technologies DB5-MS, heating rate 10 ° C / min). The amount of gas collected from the mold part within a predetermined time was divided by the total weight of the molded pieces injection molded within the predetermined time to obtain the total amount of gas (μg / g) per 1 g of the liquid crystal polymer composition, and the amount of gas other than that derived from the liquid crystal polymer composition was divided by the total weight of the molded pieces injection molded within the predetermined time to obtain the amount of mixed gas (μg / g) per 1 g of the liquid crystal polymer composition. The results are shown in Table 2. In each example, in order to stabilize the molding state in the actual sampling, the first 20 shots were discarded, and then a mold exhaust gas collection tube was set, and evaluation was performed in the subsequent molding shots. In addition, in each example, the mold temperature was 80°C and the holding pressure was 50 MPa.
[0052] [Blister occurrence evaluation] Injection molding was performed continuously under the above conditions, and the obtained rectangular molded pieces were heat-treated in a conveyor-type hot air circulation dryer DFC-27-022S manufactured by Futaba Scientific Co., Ltd. In this case, the feed rate was set to 0.45 cm / min, and an infrared heater set to 190 ° C and a hot air heater set to 185 ° C were used in the preheat zone, and an infrared heater set to 500 ° C and a hot air heater set to 300 ° C were used in the reflow zone, so that the surface peak temperature of the molded pieces was 273 ° C. The molded pieces after the treatment were visually observed to evaluate the occurrence of blisters. Those with no blisters at all were rated A, those with almost no blisters were rated B, those with some blisters but not noticeable were rated C, those with slightly noticeable blisters were rated D, and those with noticeable blisters were rated E. The results are shown in Table 2. In this specification, the above evaluations A to C are considered to be suppressed in the occurrence of blisters. [Table 2]
[0053] From Table 2, it was confirmed that the production method of the present invention can suppress the generation of blisters after heat treatment in liquid crystalline polymer molded articles obtained from various materials and under various molding conditions.
Claims
1. A method for producing a liquid crystalline polymer molded article, comprising injection molding a liquid crystalline polymer composition using a mold having a gate, a cavity, and a gas vent, characterized in that the total amount of gas captured in the gas vent during the injection molding is 20 μg / g or less, and characterized in that prior to injection molding of the liquid crystalline polymer composition, (a) purging with a polycarbonate resin composition containing glass fibers and (b) purging with the liquid crystalline polymer composition are carried out in this order.
2. The method for producing a liquid crystal polymer molded product according to claim 1, characterized in that in the injection molding, the total amount of gas is set to 20 μg / g or less by at least one of lowering the cylinder temperature and / or injection speed of the molding machine, or increasing the size and / or number of gates of the mold.
3. 3. The method for producing a liquid crystal polymer molded article according to claim 1 or 2, characterized in that, before purging with the (a) polycarbonate resin composition, purging with the (b) liquid crystal polymer composition, or purging with the (c) polyethylene-based resin composition, or purging with the (d) styrene-based resin composition is further carried out.
4. The method for producing a liquid crystal polymer molded article according to claim 3, characterized in that an additional purge is performed before the purge with the liquid crystal polymer composition (b), before the purge with the polyethylene resin composition (c), or before the purge with the styrene resin composition (d), which is performed before the purge with the polycarbonate resin composition (a), and the additional purge is at least one selected from the purge with the polycarbonate resin composition (a), the purge with the liquid crystal polymer (b), the purge with the polyethylene resin composition (c), or the purge with the styrene resin composition (d), which is different from the purge performed immediately after the additional purge.
5. 5. The method for producing a liquid crystal polymer molded product according to claim 3 or 4, characterized in that, when purging with the (c) polyethylene-based resin composition and / or purging with the (d) styrene-based resin composition is performed, cleaning of the screw of the molding machine is performed after purging with the (c) polyethylene-based resin composition and / or purging with the (d) styrene-based resin composition.
6. A method for suppressing blistering in a liquid crystal polymer molded article when a liquid crystal polymer composition is injection molded using a mold having a gate, a cavity, and a gas vent to produce the liquid crystal polymer molded article, the method being characterized in that the total amount of gas captured in the gas vent during the injection molding is 20 μg / g or less, the method being characterized in that, prior to injection molding of the liquid crystal polymer composition, (a) purging with a polycarbonate resin composition containing glass fiber, and (b) purging with the liquid crystal polymer composition are carried out in this order.
7. The method for suppressing blisters in a liquid crystal polymer molded product described in claim 6, characterized in that in the injection molding, the total gas amount is set to 20 μg / g or less by at least one of reducing the cylinder temperature and / or injection speed of the molding machine, or increasing the size and / or number of gates of the mold.
8. The method for suppressing blisters in a liquid crystal polymer molded product according to claim 6 or 7, characterized in that, before purging with the (a) polycarbonate resin composition, purging with the (b) liquid crystal polymer composition, or purging with the (c) polyethylene-based resin composition, or purging with the (d) styrene-based resin composition is further carried out.
9. 9. The method for suppressing blisters in a liquid crystal polymer molded product according to claim 8, characterized in that an additional purge is performed before the purge with the liquid crystal polymer composition (b), before the purge with the polyethylene resin composition (c), or before the purge with the styrene-based resin composition (d), which is performed before the purge with the polycarbonate resin composition (a), and the additional purge is at least one selected from the group consisting of a purge with the polycarbonate resin composition (a), a purge with the liquid crystal polymer (b), a purge with the polyethylene resin composition (c), and a purge with the styrene-based resin composition (d), which is different from the purge performed immediately after the additional purge.
10. The method for suppressing blisters in a liquid crystal polymer molded product according to claim 8 or claim 9, characterized in that, when purging with the (c) polyethylene-based resin composition and / or purging with the (d) styrene-based resin composition is performed, cleaning of the screw of the molding machine is performed after purging with the (c) polyethylene-based resin composition and / or purging with the (d) styrene-based resin composition.
Citation Information
Patent Citations
Molding device and molding method
JP1995009474A
Liquid crystal polyester molded product
JP1999140283A
Thermoplastic resin composition for cleaning, and cleaning method
JP1999227000A
Purge material and purging method therefor
JP2003342484A
Liquid crystal polyester resin composition and its molded article
JP2004196886A