Antibacterial polycarbonate resin composition and molded article

A combination of specific aromatic polycarbonate resin, thermoplastic resin, and inorganic oxides with Ag, Zn, or Cu elements, along with a phosphorus stabilizer, addresses the issue of transparency and impact resistance in antibacterial polycarbonate resin, resulting in a composition with enhanced properties for diverse applications.

JP7596177B2Active Publication Date: 2024-12-09MITSUBISHI ENG PLASTICS CORP
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
JP2021028496
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2020-12-10
Filing Date
2021-02-25
Publication Date
2024-12-09
Estimated Expiration
2041-02-25

AI Technical Summary

Technical Problem

Existing antibacterial polycarbonate resin compositions compromise transparency and impact resistance when antibacterial agents are added, leading to insufficient performance in these critical properties.

Method used

A combination of aromatic polycarbonate resin with specific viscosity average molecular weight, thermoplastic resin with specific tensile modulus and refractive index, and inorganic oxides containing Ag, Zn, or Cu elements, along with a phosphorus stabilizer, to create a composition that maintains high transparency, impact resistance, and antibacterial properties.

Benefits of technology

The composition achieves a balanced performance with high transparency, impact resistance, and excellent antibacterial properties, along with heat and chemical resistance, suitable for various applications.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007596177000010
    Figure 0007596177000010
  • Figure 0007596177000001
    Figure 0007596177000001
  • Figure 0007596177000002
    Figure 0007596177000002
Patent Text Reader

Abstract

To provide an antibacterial polycarbonate resin composition having all of high transparency, high antibacterial properties and high shock resistance, and heat resistance, wet heat resistance and chemical resistance.SOLUTION: An antibacterial polycarbonate resin composition contains, based on 100 pts.mass of an aromatic polycarbonate resin (A) having a viscosity average molecular weight of 17,000-28,000, 5-80 pts.mass of a thermoplastic resin (B) excluding the aromatic polycarbonate resin (A), having a tension elastic modulus according to ISO527-1.2 of 1.0-2.5 GPa and an elastic modulus according to ISO489 of 1.45-1.59, and 0.1-2.5 pts.mass of an inorganic oxide (C) containing at least one of Ag, Zn, Zr and Cu elements, and has a haze value in a plate of a thickness of 2 mm of 20% or less.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to an antibacterial polycarbonate resin composition and a molded article thereof, and more particularly to an antibacterial polycarbonate resin composition having high transparency and excellent impact resistance and a molded article thereof. [Background technology]

[0002] Polycarbonate resin is a resin with high light transmittance and excellent transparency, and because it has excellent heat resistance, moldability and practical strength, it is widely used in electrical products, automobile parts, stationery, furniture, daily necessities and the like.

[0003] In recent years, due to growing awareness of hygiene and cleanliness, antibacterial products have become popular for various resin molded products. Furthermore, due to the recent coronavirus outbreak, there has been a particularly strong demand for resin materials to have antibacterial properties.

[0004] There are many products in which antibacterial properties are imparted to polycarbonate resins, but there is a problem that the addition of an antibacterial agent reduces transparency, which is one of the significant properties of polycarbonate resins. Therefore, various antibacterial polycarbonate resin compositions that impart antibacterial properties while suppressing the decrease in transparency have been proposed. For example, Patent Document 1 proposes that a polycarbonate resin composition containing a glass of a specific composition that elutes silver ions and an antioxidant has excellent antibacterial properties without causing changes in color or poor transparency.

[0005] However, inorganic antibacterial agents have a drawback in that, when blended with a polycarbonate resin, they significantly reduce the inherent transparency of the polycarbonate resin, and the polycarbonate resin composition of the invention described in Patent Document 1 has insufficient transparency and also has poor impact resistance. [Prior art documents] [Patent documents]

[0006] [Patent Document 1] Patent No. 5388326 Summary of the Invention [Problem to be solved by the invention]

[0007] An object (object) of the present invention is to solve the above-mentioned conventional problems and to provide an antibacterial polycarbonate resin composition having excellent impact resistance without reducing transparency. [Means for solving the problem]

[0008] Means for Solving the Problems The present inventors have conducted extensive research in order to solve the above problems, and as a result have found that an antibacterial polycarbonate resin composition having high transparency, high impact resistance and high antibacterial properties, and further having all of heat resistance, moist heat resistance and chemical resistance, can be obtained by combining an aromatic polycarbonate resin having a specific viscosity average molecular weight with a thermoplastic resin having a specific tensile modulus and a specific refractive index, and an inorganic oxide containing a specific element, each in specific amounts, and have thus completed the present invention. The present invention relates to the following antibacterial polycarbonate resin composition and molded article.

[0009] 1. An antibacterial polycarbonate resin composition comprising 100 parts by mass of an aromatic polycarbonate resin (A) having a viscosity average molecular weight of 17,000 to 28,000, 5 to 80 parts by mass of a thermoplastic resin (B) other than the aromatic polycarbonate resin (A) having a tensile modulus of elasticity of 1.0 to 2.5 GPa according to ISO 527-1.2 and a refractive index of 1.45 to 1.59 according to ISO 489, and 0.1 to 2.5 parts by mass of an inorganic oxide (C) containing at least one of Ag, Zn, Zr, or Cu, and wherein the haze value when measured on a 2 mm thick plate is 20% or less. 2. The polycarbonate resin composition according to the above 1, further comprising 0.01 to 0.15 parts by mass of a phosphorus-based stabilizer (D) per 100 parts by mass of the aromatic polycarbonate resin (A). 3. The polycarbonate resin composition according to the above 1 or 2, wherein the thermoplastic resin (B) is an amorphous thermoplastic polyester resin. 4. The polycarbonate resin composition according to any one of the above 1 to 3, wherein the thermoplastic resin (B) is a thermoplastic polyester resin containing a terephthalic acid residue, a 1,4-cyclohexanedimethanol residue, and a 2,2,4,4-tetramethyl-1,3-cyclobutanediol residue. 5. The polycarbonate resin composition according to any one of 1 to 3 above, wherein the thermoplastic resin (B) is a thermoplastic polyester resin in which the carboxylic acid constituent units are at least one selected from the group consisting of terephthalic acid residues, isophthalic acid residues and 1,4-cyclohexanedicarboxylic acid residues, and the diol-derived constituent units are 3,9-bis(1,1-dimethyl-2-hydroxyethyl)-2,4,8,10-tetraoxaspiro[5.5]undecane in an amount of 10 to 100 mol % of all diol constituent units, and ethylene glycol or 1,4-cyclohexanedimethanol in an amount of 90 to 0 mol % of all diol constituent units.

[0010] 6. The polycarbonate resin composition according to any one of 1 to 5 above, wherein the inorganic oxide (C) has a refractive index according to ISO 489 of 1.45 to 1.59. 7. The polycarbonate resin composition according to any one of the above 1 to 6, wherein the inorganic oxide (C) is an inorganic oxide capable of eluting Ag, Zn, Zr or Cu ions. 8. The polycarbonate resin composition according to the above item 2, wherein the phosphorus-based stabilizer (D) is a stearyl acid phosphate-based stabilizer. 9. Charpy notched impact strength according to ISO179 is 20kJ / m 2 9. The polycarbonate resin composition according to any one of 1 to 8 above. 10. A molded article made of the polycarbonate resin composition according to any one of 1 to 9 above. Effect of the Invention

[0011] The antibacterial polycarbonate resin composition of the present invention has high transparency, high antibacterial activity, high impact resistance, and further heat resistance, moist heat resistance, and chemical resistance all in a well-balanced manner. By combining an aromatic polycarbonate resin (A) having a viscosity average molecular weight of 17,000 to 28,000 with a thermoplastic resin (B) that is soft and has a tensile modulus of elasticity of 1.0 to 2.5 GPa and a refractive index at the same level as that of the aromatic polycarbonate resin (A), and further with an antibacterial inorganic oxide (C), it is possible to obtain a polycarbonate resin composition that has higher levels of both the impact resistance and transparency of the aromatic polycarbonate resin (A) and that has excellent antibacterial properties, as well as excellent heat resistance, moist heat resistance, and chemical resistance. [Brief description of the drawings]

[0012] [Figure 1] FIG. 2 is a side view showing the shape of a three-point bending load jig used in evaluating chemical resistance in the examples. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0013] Hereinafter, the present invention will be described in detail with reference to embodiments and examples, but the present invention should not be construed as being limited to the embodiments and examples shown below.

[0014] The antibacterial polycarbonate resin composition of the present invention is characterized in that it contains 100 parts by mass of an aromatic polycarbonate resin (A) having a viscosity average molecular weight of 17,000 to 28,000, 5 to 80 parts by mass of a thermoplastic resin (B) other than the aromatic polycarbonate resin (A) having a tensile modulus of elasticity of 1.0 to 2.5 GPa according to ISO 527-1.2 and a refractive index of 1.45 to 1.59 according to ISO 489, and 0.1 to 2.5 parts by mass of an inorganic oxide (C) containing at least one of Ag, Zn, Zr and Cu, and has a haze value of 20% or less on a 2 mm thick plate.

[0015] [Aromatic polycarbonate resin (A)] There is no limitation on the type of aromatic polycarbonate resin (A) used in the polycarbonate resin composition of the present invention, and only one type may be used, or two or more types may be used in any combination and in any ratio. Aromatic polycarbonate resins are polymers with a basic structure having a carbonate bond, represented by the general formula: -[-OXOC(=O)-]-. In the formula, X is an aromatic hydrocarbon, but X containing a heteroatom or heterobond may be used to impart various properties.

[0016] There is no restriction on the specific type of aromatic polycarbonate resin, but examples thereof include aromatic polycarbonate polymers obtained by reacting an aromatic dihydroxy compound with a carbonate precursor. In this case, in addition to the aromatic dihydroxy compound and the carbonate precursor, a polyhydroxy compound or the like may be reacted. A method of reacting carbon dioxide as a carbonate precursor with a cyclic ether may also be used. The aromatic polycarbonate polymer may be linear or branched. Furthermore, the aromatic polycarbonate polymer may be a homopolymer consisting of one type of repeating unit, or may be a copolymer having two or more types of repeating units. In this case, the copolymer may be selected from various copolymerization forms such as a random copolymer and a block copolymer. In addition, such an aromatic polycarbonate polymer is usually a thermoplastic resin.

[0017] Examples of aromatic dihydroxy compounds as raw material monomers for aromatic polycarbonate resins include the following. Dihydroxybenzenes such as 1,2-dihydroxybenzene, 1,3-dihydroxybenzene (i.e., resorcinol), and 1,4-dihydroxybenzene; Dihydroxybiphenyls such as 2,5-dihydroxybiphenyl, 2,2'-dihydroxybiphenyl, and 4,4'-dihydroxybiphenyl;

[0018] dihydroxynaphthalenes such as 2,2'-dihydroxy-1,1'-binaphthyl, 1,2-dihydroxynaphthalene, 1,3-dihydroxynaphthalene, 2,3-dihydroxynaphthalene, 1,6-dihydroxynaphthalene, 2,6-dihydroxynaphthalene, 1,7-dihydroxynaphthalene, and 2,7-dihydroxynaphthalene;

[0019] dihydroxydiaryl ethers such as 2,2'-dihydroxydiphenyl ether, 3,3'-dihydroxydiphenyl ether, 4,4'-dihydroxydiphenyl ether, 4,4'-dihydroxy-3,3'-dimethyldiphenyl ether, 1,4-bis(3-hydroxyphenoxy)benzene, and 1,3-bis(4-hydroxyphenoxy)benzene;

[0020] 2,2-bis(4-hydroxyphenyl)propane (i.e., bisphenol A), 1,1-bis(4-hydroxyphenyl)propane, 2,2-bis(3-methyl-4-hydroxyphenyl)propane, 2,2-bis(3-methoxy-4-hydroxyphenyl)propane, 2-(4-hydroxyphenyl)-2-(3-methoxy-4-hydroxyphenyl)propane, 1,1-bis(3-tert-butyl-4-hydroxyphenyl)propane, 2,2-bis(4-hydroxy-3,5-dimethylphenyl)propane, 2,2-bis(3-cyclohexyl-4-hydroxyphenyl)propane, 2-(4-hydroxyphenyl)-2-(3-cyclohexyl-4-hydroxyphenyl)propane, α,α'-bis(4-hydroxyphenyl)-1,4-diisopropylbenzene, 1,3-bis[2-(4-hydroxyphenyl)-2-propyl]benzene, bis(4-hydroxyphenyl)methane, Bis(4-hydroxyphenyl)cyclohexylmethane, Bis(4-hydroxyphenyl)phenylmethane, Bis(4-hydroxyphenyl)(4-propenylphenyl)methane, Bis(4-hydroxyphenyl)diphenylmethane, Bis(4-hydroxyphenyl)naphthylmethane, 1,1-bis(4-hydroxyphenyl)ethane, 1,2-bis(4-hydroxyphenyl)ethane, 1,1-bis(4-hydroxyphenyl)-1-phenylethane, 1,1-bis(4-hydroxyphenyl)-1-naphthylethan, 1,1-bis(4-hydroxyphenyl)butane, 2,2-bis(4-hydroxyphenyl)butane, 2,2-bis(4-hydroxyphenyl)pentane, 1,1-bis(4-hydroxyphenyl)hexane, 2,2-bis(4-hydroxyphenyl)hexane, 1,1-bis(4-hydroxyphenyl)octane, 2,2-bis(4-hydroxyphenyl)octane, 4,4-bis(4-hydroxyphenyl)heptane, 2,2-bis(4-hydroxyphenyl)nonane, 1,10-bis(4-hydroxyphenyl)decane, 1,1-bis(4-hydroxyphenyl)dodecane, Bis(hydroxyaryl)alkanes such as;

[0021] 1,1-bis(4-hydroxyphenyl)cyclopentane, 1,1-bis(4-hydroxyphenyl)cyclohexane, 1,4-bis(4-hydroxyphenyl)cyclohexane, 1,1-bis(4-hydroxyphenyl)-3,3-dimethylcyclohexane, 1,1-bis(4-hydroxyphenyl)-3,4-dimethylcyclohexane, 1,1-bis(4-hydroxyphenyl)-3,5-dimethylcyclohexane, 1,1-bis(4-hydroxyphenyl)-3,3,5-trimethylcyclohexane, 1,1-bis(4-hydroxy-3,5-dimethylphenyl)-3,3,5-trimethylcyclohexane, 1,1-bis(4-hydroxyphenyl)-3-propyl-5-methylcyclohexane, 1,1-bis(4-hydroxyphenyl)-3-tert-butyl-cyclohexane, 1,1-bis(4-hydroxyphenyl)-4-tert-butyl-cyclohexane, 1,1-bis(4-hydroxyphenyl)-3-phenylcyclohexane, 1,1-bis(4-hydroxyphenyl)-4-phenylcyclohexane, Bis(hydroxyaryl)cycloalkanes such as;

[0022] Cardo structure-containing bisphenols such as 9,9-bis(4-hydroxyphenyl)fluorene and 9,9-bis(4-hydroxy-3-methylphenyl)fluorene; Dihydroxydiaryl sulfides such as 4,4'-dihydroxydiphenyl sulfide and 4,4'-dihydroxy-3,3'-dimethyldiphenyl sulfide; Dihydroxydiaryl sulfoxides such as 4,4'-dihydroxydiphenyl sulfoxide and 4,4'-dihydroxy-3,3'-dimethyldiphenyl sulfoxide; dihydroxydiarylsulfones such as 4,4'-dihydroxydiphenylsulfone and 4,4'-dihydroxy-3,3'-dimethyldiphenylsulfone; and the like.

[0023] Among these, bis(hydroxyaryl)alkanes are preferred, bis(4-hydroxyphenyl)alkanes are more preferred, and 2,2-bis(4-hydroxyphenyl)propane (ie, bisphenol A) is particularly preferred from the standpoint of impact resistance and heat resistance. The aromatic dihydroxy compounds may be used alone or in any combination of two or more in any ratio.

[0024] Among the monomers that are raw materials for aromatic polycarbonate resins, examples of carbonate precursors include carbonyl halides, carbonate esters, etc. The carbonate precursors may be used alone or in any combination and ratio of two or more.

[0025] Specific examples of carbonyl halides include phosgene; haloformates such as bischloroformates of dihydroxy compounds and monochloroformates of dihydroxy compounds; and the like.

[0026] Specific examples of carbonate esters include diaryl carbonates such as diphenyl carbonate and ditolyl carbonate; dialkyl carbonates such as dimethyl carbonate and diethyl carbonate; biscarbonates of dihydroxy compounds, monocarbonates of dihydroxy compounds, and carbonates of dihydroxy compounds such as cyclic carbonates.

[0027] Manufacturing method for aromatic polycarbonate resin The method for producing the aromatic polycarbonate resin is not particularly limited, and any method can be used, such as interfacial polymerization, melt transesterification, pyridine method, ring-opening polymerization of a cyclic carbonate compound, and solid-phase transesterification of a prepolymer. Among these methods, particularly preferred methods will be specifically described below.

[0028] Interfacial polymerization method First, the production of an aromatic polycarbonate resin by interfacial polymerization will be described. In the interfacial polymerization method, a dihydroxy compound is reacted with a carbonate precursor (preferably phosgene) in the presence of an organic solvent inert to the reaction and an aqueous alkaline solution, usually at a pH of 9 or higher, and then interfacial polymerization is carried out in the presence of a polymerization catalyst to obtain an aromatic polycarbonate resin. Note that a molecular weight regulator (terminal terminator) may be present in the reaction system as necessary, and an antioxidant may be present to prevent oxidation of the dihydroxy compound.

[0029] The dihydroxy compound and the carbonate precursor are as described above. Among the carbonate precursors, it is preferable to use phosgene, and the method using phosgene is particularly called the phosgene method.

[0030] Examples of organic solvents inert to the reaction include chlorinated hydrocarbons such as dichloromethane, 1,2-dichloroethane, chloroform, monochlorobenzene, and dichlorobenzene; aromatic hydrocarbons such as benzene, toluene, and xylene; etc. The organic solvents may be used alone or in any combination and ratio of two or more.

[0031] Examples of the alkaline compound contained in the alkaline aqueous solution include alkali metal compounds and alkaline earth metal compounds such as sodium hydroxide, potassium hydroxide, lithium hydroxide, and sodium hydrogencarbonate, among which sodium hydroxide and potassium hydroxide are preferred. The alkaline compounds may be used alone or in any combination and ratio of two or more.

[0032] Although there is no limitation on the concentration of the alkali compound in the alkaline aqueous solution, it is usually used at 5 to 10 mass % in order to control the pH of the alkaline aqueous solution in the reaction to 10 to 12. Furthermore, for example, when blowing in phosgene, in order to control the pH of the aqueous phase to 10 to 12, preferably 10 to 11, it is preferable that the molar ratio of the bisphenol compound to the alkali compound is usually 1:1.9 or more, preferably 1:2.0 or more, and usually 1:3.2 or less, preferably 1:2.5 or less.

[0033] Examples of the polymerization catalyst include aliphatic tertiary amines such as trimethylamine, triethylamine, tributylamine, tripropylamine, and trihexylamine; alicyclic tertiary amines such as N,N'-dimethylcyclohexylamine and N,N'-diethylcyclohexylamine; aromatic tertiary amines such as N,N'-dimethylaniline and N,N'-diethylaniline; quaternary ammonium salts such as trimethylbenzylammonium chloride, tetramethylammonium chloride, and triethylbenzylammonium chloride; pyridine; and salts of guanidine. The polymerization catalyst may be used alone or in any combination and ratio of two or more.

[0034] Examples of the molecular weight regulator include aromatic phenols having a monovalent phenolic hydroxyl group, aliphatic alcohols such as methanol and butanol, mercaptans, and phthalic acid imides, among which aromatic phenols are preferred.Specific examples of such aromatic phenols include alkyl group-substituted phenols such as m-methylphenol, p-methylphenol, m-propylphenol, p-propylphenol, p-tert-butylphenol, and p-long chain alkyl-substituted phenols, vinyl group-containing phenols such as isopropenylphenol, epoxy group-containing phenols, carboxyl group-containing phenols such as o-hydroxybenzoic acid and 2-methyl-6-hydroxyphenylacetic acid, and the like. The molecular weight regulator may be used alone or in any combination of two or more in any ratio.

[0035] The amount of the molecular weight regulator used is usually 0.5 mol or more, preferably 1 mol or more, and usually 50 mol or less, preferably 30 mol or less, based on 100 mol of the dihydroxy compound. By setting the amount of the molecular weight regulator used within this range, the thermal stability and hydrolysis resistance of the resin composition can be improved.

[0036] In the reaction, the order of mixing the reaction substrate, reaction medium, catalyst, additives, etc. is arbitrary as long as the desired aromatic polycarbonate resin can be obtained, and an appropriate order may be set arbitrarily. For example, when phosgene is used as the carbonate precursor, the molecular weight regulator can be mixed at any time between the reaction of the dihydroxy compound with phosgene (phosgenation) and the start of the polymerization reaction. The reaction temperature is usually 0 to 40° C., and the reaction time is usually several minutes (eg, 10 minutes) to several hours (eg, 6 hours).

[0037] Melt transesterification Next, the production of an aromatic polycarbonate resin by the melt transesterification method will be described. In the melt transesterification method, for example, a transesterification reaction is carried out between a carbonic acid diester and a dihydroxy compound.

[0038] The dihydroxy compound is as described above. On the other hand, examples of the carbonic acid diester include dialkyl carbonate compounds such as dimethyl carbonate, diethyl carbonate, and di-tert-butyl carbonate; diphenyl carbonate; and substituted diphenyl carbonates such as ditolyl carbonate. Among these, diphenyl carbonate and substituted diphenyl carbonate are preferred, and diphenyl carbonate is more preferred. The carbonic acid diester may be used alone or in any combination and ratio of two or more.

[0039] The ratio of dihydroxy compound and carbonic acid diester is arbitrary as long as the desired aromatic polycarbonate resin can be obtained, but it is preferable to use the carbonic acid diester in an equimolar amount or more with respect to 1 mole of dihydroxy compound, and more preferably to use 1.01 mole or more. The upper limit is usually 1.30 moles or less. By adjusting it to such a range, the amount of terminal hydroxyl groups can be adjusted to a suitable range.

[0040] In aromatic polycarbonate resins, the amount of terminal hydroxyl groups tends to have a large effect on thermal stability, hydrolysis stability, color tone, etc. Therefore, the amount of terminal hydroxyl groups may be adjusted as necessary by any known method. In the transesterification reaction, an aromatic polycarbonate resin having an adjusted amount of terminal hydroxyl groups can usually be obtained by adjusting the mixing ratio of the carbonic acid diester and the aromatic dihydroxy compound, the degree of reduced pressure during the transesterification reaction, etc. In addition, this operation can usually also adjust the molecular weight of the resulting aromatic polycarbonate resin.

[0041] When the amount of terminal hydroxyl groups is adjusted by adjusting the mixing ratio of the carbonic acid diester and the dihydroxy compound, the mixing ratio is as described above. In addition, as a more active adjustment method, a method of separately mixing a terminal terminator during the reaction can be mentioned. In this case, examples of the terminal terminator include monohydric phenols, monovalent carboxylic acids, and carbonic acid diesters. The terminal terminator may be used alone or in any combination and ratio of two or more.

[0042] When producing an aromatic polycarbonate resin by the melt transesterification method, a transesterification catalyst is usually used. Any transesterification catalyst can be used. Among them, it is preferable to use, for example, an alkali metal compound and / or an alkaline earth metal compound. In addition, a basic compound such as a basic boron compound, a basic phosphorus compound, a basic ammonium compound, or an amine compound may be used in combination as an auxiliary. The transesterification catalyst may be used alone or in any combination and ratio of two or more kinds.

[0043] In the melt transesterification method, the reaction temperature is usually 100 to 320° C. The pressure during the reaction is usually reduced pressure of 2 mmHg or less. As a specific operation, a melt polycondensation reaction may be carried out under the above conditions while removing by-products such as aromatic hydroxy compounds.

[0044] The melt polycondensation reaction can be carried out by either a batch method or a continuous method. When the batch method is carried out, the order of mixing the reaction substrate, reaction medium, catalyst, additives, etc. is arbitrary as long as the desired aromatic polycarbonate resin is obtained, and an appropriate order may be set arbitrarily. However, in particular, in consideration of the stability of the aromatic polycarbonate resin, etc., the melt polycondensation reaction is preferably carried out by a continuous method.

[0045] In the melt transesterification method, a catalyst deactivator may be used as necessary. As the catalyst deactivator, any compound that neutralizes the transesterification catalyst may be used. Examples of the catalyst deactivator include sulfur-containing acidic compounds and their derivatives. The catalyst deactivator may be used alone or in any combination and ratio of two or more.

[0046] The amount of the catalyst deactivator used is usually 0.5 equivalents or more, preferably 1 equivalent or more, and usually 10 equivalents or less, preferably 5 equivalents or less, based on the alkali metal or alkaline earth metal contained in the transesterification catalyst. Furthermore, the amount is usually 1 ppm or more, and usually 100 ppm or less, preferably 20 ppm or less, based on the aromatic polycarbonate resin.

[0047] The aromatic polycarbonate resin (A) used has a viscosity average molecular weight (Mv) in the range of 17,000 to 28,000. By using a resin having a viscosity average molecular weight (Mv) in this range, a resin composition having excellent impact resistance and transparency can be obtained. If Mv is lower than 17,000, the impact resistance is insufficient, and if it exceeds 28,000, uniform dispersion with the thermoplastic resin (B) becomes difficult, and the transparency of the resin composition tends to deteriorate. The viscosity average molecular weight (Mv) is preferably 18,000 or more, more preferably 19,000 or more, and even more preferably 20,000 or more, and is preferably 27,000 or less, and more preferably 26,000 or less. Two or more aromatic polycarbonate resins having different viscosity average molecular weights may be mixed and used. In this case, an aromatic polycarbonate resin having a viscosity average molecular weight outside the above range may be mixed to adjust the viscosity average molecular weight within the above range.

[0048] The viscosity average molecular weight [Mv] is calculated by using methylene chloride as a solvent, measuring the intrinsic viscosity [η] (unit: dl / g) at 25°C using an Ubbelohde viscometer, and calculating the viscosity average molecular weight [Mv] using the Schnell viscosity formula, i.e., η = 1.23 × 10 -4 Mv 0.83 The intrinsic viscosity [η] is the value calculated from the specific viscosity [η sp ] was measured and the value was calculated according to the following formula.

number

[0049] The terminal hydroxyl group concentration of the aromatic polycarbonate resin is arbitrary and may be appropriately selected and determined, but is usually 1000 ppm or less, preferably 800 ppm or less, more preferably 600 ppm or less. This can further improve the residence heat stability and color tone of the aromatic polycarbonate resin. The lower limit is usually 10 ppm or more, preferably 30 ppm or more, more preferably 40 ppm or more, particularly for aromatic polycarbonate resins produced by the melt transesterification method. This can suppress the decrease in molecular weight and further improve the mechanical properties of the resin composition.

[0050] The unit of the terminal hydroxyl group concentration is the mass of the terminal hydroxyl group relative to the mass of the aromatic polycarbonate resin, expressed in ppm. The measurement method is colorimetric determination using the titanium tetrachloride / acetic acid method (the method described in Macromol. Chem. 88 215 (1965)).

[0051] The aromatic polycarbonate resin may be used alone (the term "sole polycarbonate resin" is not limited to an embodiment including only one type of polycarbonate resin, but is used to mean an embodiment including, for example, a plurality of types of polycarbonate resins having different monomer compositions or molecular weights), or may be used in combination with an alloy (mixture) of an aromatic polycarbonate resin and another thermoplastic resin.

[0052] [Thermoplastic resin (B)] The polycarbonate resin composition of the present invention contains a thermoplastic resin (B) other than an aromatic polycarbonate resin (A) having a tensile modulus of elasticity of 1.0 to 2.5 GPa according to ISO 527-1.2 and a refractive index of 1.45 to 1.59 according to ISO 489. By containing a thermoplastic resin (B) other than an aromatic polycarbonate resin (A) having a tensile modulus and refractive index within such ranges in combination with the aromatic polycarbonate resin (A), the impact resistance of the resin composition is improved, and the refractive index is close to the refractive index (1.584) of the aromatic polycarbonate resin (A), making it possible to obtain a resin composition with excellent transparency. The tensile modulus of the thermoplastic resin (B) is preferably 1.1 GPa or more, more preferably 1.2 GPa or more, even more preferably 1.3 GPa or more, and particularly preferably 1.4 GPa or more, and is preferably 2.4 GPa or less, more preferably 2.3 GPa or less, and even more preferably 2.2 GPa or less, and among these, it is preferable that the modulus is 2.1 GPa or less, 2.0 GPa or less, 1.9 GPa or less, 1.8 GPa or less, or 1.7 GPa or less.

[0053] The thermoplastic resin (B) is not limited as long as it is a thermoplastic resin other than the aromatic polycarbonate resin (A) that satisfies the above-mentioned tensile modulus and refractive index. Preferred examples of the thermoplastic resin (B) include thermoplastic polyester resins and methyl methacrylate-based resins (e.g., polymethyl methacrylate, methyl methacrylate-phenyl methacrylate copolymer resins). In addition, aliphatic polycarbonate resins that satisfy the above tensile modulus and refractive index other than the aromatic polycarbonate resin (A) can also be preferably used. Aliphatic polycarbonate resins are made from aliphatic dihydroxy compounds, and representative examples include 1,4-butanediol, 1,5-pentanediol, neopentyl glycol, 1,6-hexanediol, 1,7-heptanediol, 1,8-octanediol, 1,4-cyclohexanediol, 2-ethyl-1,6-hexanediol, 2,2,4-trimethyl-1,6-hexanediol, 1,10-decanediol, etc. In addition, those made from dihydroxy compounds having a cyclic ether structure such as isosorbide and isomannide are also preferably mentioned.

[0054] As the thermoplastic resin (B), a thermoplastic polyester resin is preferred, and a non-crystalline polyester resin is particularly preferred. The term "amorphous" in the amorphous polyester resin means that the resin does not exhibit a distinct melting point (Tm) when measured by a differential scanning calorimeter (DSC).

[0055] The amorphous polyester resin is preferably an amorphous polyester resin having a structural unit derived from an alicyclic diol and / or a diol having a cyclic acetal skeleton. Preferred examples of the alicyclic diol include 2,2,4,4-tetramethyl-1,3-cyclobutanediol (which may be cis, trans, or a mixture thereof), and 1,4-cyclohexanedimethanol (or a mixture of 1,3- and 1,4-cyclohexanedimethanol, which may be cis, trans, or a mixture thereof).

[0056] Preferred examples of the diol having a cyclic acetal skeleton include diols represented by the following general formula (1). [ka] In formula (1), R 1 and R 2each independently represents an aliphatic hydrocarbon group having 1 to 10 carbon atoms, an alicyclic hydrocarbon group having 3 to 10 carbon atoms, or an aromatic hydrocarbon group having 6 to 10 carbon atoms.

[0057] In the above general formula (1), R 1 and R 2 are each independently a hydrocarbon group selected from the group consisting of an aliphatic hydrocarbon group having 1 to 10 carbon atoms, an alicyclic hydrocarbon group having 3 to 10 carbon atoms, and an aromatic hydrocarbon group having 6 to 10 carbon atoms, and are preferably a methylene group, an ethylene group, a propylene group, a butylene group, or a structural isomer thereof, such as a dimethylethylenyl group, an isopropylene group, or an isobutylene group. The diol compound having a cyclic acetal skeleton of the general formula (1) is R 1 and R 2 Particularly preferred is 3,9-bis(1,1-dimethyl-2-hydroxyethyl)-2,4,8,10-tetraoxaspiro[5.5]undecane, in which is a dimethylethylenyl group.

[0058] The composition ratio of the alicyclic diol and the diol component having a cyclic acetal skeleton is preferably 10 to 100 mol %, more preferably 20 to 100 mol %, and even more preferably 30 to 100 mol %, when the total mol % of the diol components is 100 mol %.

[0059] The amorphous polyester resin may contain a diol component other than the alicyclic diol and the diol having a cyclic acetal skeleton. The content of the other diol is preferably 90 mol % or less, more preferably 80 mol % or less, and even more preferably 70 mol % or less, when the total number of moles of the diol components in the amorphous polyester resin is 100 mol %. Other diols include diols containing 2 to 16 carbon atoms, such as ethylene glycol, diethylene glycol, 1,2-propanediol, 1,3-propanediol, neopentyl glycol, 1,4-butanediol, 1,5-pentanediol, 1,6-hexanediol, or mixtures thereof.

[0060] The dicarboxylic acid component of the amorphous polyester resin may be an alicyclic dicarboxylic acid or an aromatic dicarboxylic acid, with aromatic dicarboxylic acid being preferred. The aromatic dicarboxylic acid is preferably terephthalic acid, and the amount of the aromatic dicarboxylic acid is preferably 80 mol% or more, more preferably 90 mol% or more. In addition to terephthalic acid, the dicarboxylic acid component may have up to less than 50 mol% of other dicarboxylic acids. Examples of aromatic dicarboxylic acids other than terephthalic acid include isophthalic acid, 4,4'-biphenyldicarboxylic acid, 1,4-, 1,5-, 2,6-, and 2,7-naphthalenedicarboxylic acid, and 4,4'-stilbene dicarboxylic acid. Furthermore, it is possible to contain aliphatic dicarboxylic acids such as malonic acid, succinic acid, glutaric acid, adipic acid, pimelic acid, suberic acid, and azalenic acid, but the amount thereof is preferably 10 mol % or less.

[0061] The intrinsic viscosity of the amorphous polyester resin is preferably in the range of 0.3 to 1.2 dl / g, more preferably 0.5 to 1.0 dl / g, and even more preferably 0.7 to 0.9 dl / g. When the intrinsic viscosity is in the above range, the moldability and strength are excellent. In the present invention, the intrinsic viscosity [η] of the polyester resin is measured at 25° C. in a mixed solvent of 1,1,2,2-tetrachloroethane and phenol in a 1:1 (mass ratio).

[0062] Particularly preferred amorphous polyester resins are polyester resins containing terephthalic acid residues, 1,4-cyclohexanedimethanol (hereinafter also referred to as "CHDM") residues, and 2,2,4,4-tetramethyl-1,3-cyclobutanediol (hereinafter also referred to as "TMCD") residues. From the viewpoint of transparency and heat resistance, it is preferable that the total proportion of CHDM residues and TMCD residues in all diol residues is 85 mol % or more, particularly 90 to 100 mol %, and even more particularly 95 to 100 mol %. Furthermore, the proportion of CHDM residues in the total of CHDM residues and TMCD residues (100 mol %) is preferably 10 to 90 mol %, with the proportion of TMCD residues being 90 to 10 mol %, more preferably the proportion of CHDM residues being 20 to 85 mol % and the proportion of TMCD residues being 15 to 80 mol %, and particularly preferably the proportion of CHDM residues being 30 to 80 mol % and the proportion of TMCD residues being 20 to 70 mol %.

[0063] As such an amorphous polyester resin, a commercially available product can be used, and for example, a product selected from the "Tritan" series manufactured by Eastman Chemical Company can be used.

[0064] Furthermore, particularly preferred amorphous polyester resins are polyester resins in which the carboxylic acid constituent units are at least one selected from the group consisting of terephthalic acid residues, isophthalic acid residues, and 1,4-cyclohexanedicarboxylic acid residues, and the diol-derived constituent units are 3,9-bis(1,1-dimethyl-2-hydroxyethyl)-2,4,8,10-tetraoxaspiro[5.5]undecane (hereinafter also referred to as "spiroglycol") in an amount of 10 to 100 mol % of all diol constituent units, and ethylene glycol or 1,4-cyclohexanedimethanol in an amount of 90 to 0 mol % of all diol constituent units.

[0065] The spiro glycol-derived structural units preferably account for 10 to 80 mol %, more preferably 30 to 75 mol %, of all diol structural units, and the ethylene glycol-derived structural units preferably account for 0 to 65 mol %. The carboxylic acid constituent units preferably contain 90 to 100 mol % terephthalic acid residues.

[0066] Such amorphous polyester resins may be commercially available. For example, The product can be selected from the "Altesta" series manufactured by Mitsubishi Gas Chemical Company, Inc.

[0067] The content of the thermoplastic resin (B) is 5 to 80 parts by mass, preferably 10 parts by mass or more, more preferably 20 parts by mass or more, and preferably 70 parts by mass or less, more preferably 60 parts by mass or less, even more preferably 55 parts by mass or less, and particularly preferably 50 parts by mass or less, relative to 100 parts by mass of the aromatic polycarbonate resin (A). By containing it in such a range, it is possible to improve the impact resistance and transparency, as well as the heat resistance, moist heat resistance, and chemical resistance in a well-balanced manner.

[0068] [Inorganic oxide (C)] The polycarbonate resin composition of the present invention contains an inorganic oxide (C) containing at least one of Ag, Zn, Zr, and Cu. The inorganic oxide (C) is an antibacterial inorganic oxide particle containing at least one of Ag, Zn, Zr, and Cu elements (atoms). By containing such an inorganic oxide (C) in combination with an aromatic polycarbonate resin (A) and a thermoplastic resin (B), an antibacterial resin composition having excellent transparency while maintaining the impact resistance of the resin composition can be obtained.

[0069] The inorganic oxide (C) may contain at least one of Ag, Zn, Zr, or Cu elements (atoms), and the type is not particularly limited. The form of Ag, Zn, Zr, or Cu elements (atoms) is also not particularly limited, and may be, for example, in the form of metal, ion, oxide, salt (including complex), etc. The inorganic oxide (C) is preferably an inorganic oxide having the ability to dissolve Ag, Zn, Zr, or Cu ions. For example, in the case of silver, representative examples include silver particles that slowly release silver ions and antibacterial agents of inorganic oxides that contain silver.

[0070] The Ag, Zn, Zr, and Cu elements (atoms) may be used alone or in combination of two or more. Among these, Ag, Zn, and Cu are preferred because of their excellent antibacterial properties, and Ag-based, Ag-Zn-based, Zn-based, and Ag-Cu-based are preferred, with Ag or a combination of Ag and Zn being preferred.

[0071] Examples of inorganic oxides having antibacterial properties include oxides of Ag, Zn, Zr, or Cu, or composite oxides thereof, and preferred examples include silver oxide, zinc oxide, zirconium oxide, copper oxide, and composite oxides thereof. In addition, copper oxide sol, silver oxide sol, zinc sol, zirconia sol, etc. may also be used.

[0072] As the antibacterial inorganic oxide (C), metals, ions, metal oxides, metal salts, etc. of Ag, Zn, Zr, or Cu supported on an inorganic oxide carrier can also be used. Metal salts include nitrates, sulfates, and halides of Ag, Zn, Zr, or Cu. Examples of inorganic oxide supports include glass, ceramics, silica, silica gel, zinc oxide, zirconium oxide, copper oxide, titanium oxide, zeolite, clay minerals, etc. These supports are preferably in the form of particles, particularly in the form of fine particles.

[0073] The inorganic oxide (C) preferably has a refractive index of 1.45 to 1.59 according to ISO 489. When the refractive index is in such a range, the transparency of the resin composition can be made more favorable.

[0074] As the antibacterial inorganic oxide (C), silver or silver-zinc supported on glass, ceramics, etc. is particularly preferred.

[0075] The antibacterial inorganic oxide (C) is preferably particulate, and its average particle size is preferably 0.1 to 20 μm, more preferably 0.5 μm or more, even more preferably 1 μm or more, more preferably 15 μm or less, and even more preferably 13 μm or less. When the average particle size is within such a range, the antibacterial effect is high, the blending amount can be made smaller, and the transparency of the resin composition can be improved.

[0076] The content of Ag, Zn, Zr and Cu elements (atoms) in the inorganic oxide (C) is preferably 0.1 to 10 mass % relative to the total mass of the inorganic oxide (C) (100 mass %).

[0077] The content of the inorganic oxide (C) is 0.1 to 2.5 parts by mass, preferably 0.2 parts by mass or more, more preferably 0.3 parts by mass or more, particularly preferably 0.4 parts by mass or more, and preferably 2 parts by mass or less, more preferably 1.8 parts by mass or less, and further preferably 1.5 parts by mass or less, relative to 100 parts by mass of the aromatic polycarbonate resin (A). By containing it in such a range, it is possible to maintain impact resistance while having excellent transparency, and further to maintain a good balance between heat resistance, moist heat resistance, and chemical resistance.

[0078] [Phosphorus-based stabilizer (D)] The polycarbonate resin composition of the present invention preferably contains a phosphorus-based stabilizer. Any known phosphorus-based stabilizer can be used. Specific examples include phosphorus oxoacids such as phosphoric acid, phosphonic acid, phosphorous acid, phosphinic acid, and polyphosphoric acid; acid pyrophosphate metal salts such as sodium acid pyrophosphate, potassium acid pyrophosphate, and calcium acid pyrophosphate; phosphates of Group 1 or Group 2C metals such as potassium phosphate, sodium phosphate, cesium phosphate, and zinc phosphate; organic phosphate compounds, organic phosphite compounds, and organic phosphonite compounds, with organic phosphite compounds and organic phosphate compounds being preferred, and organic phosphate compounds being particularly preferred.

[0079] Examples of organic phosphite compounds include triphenyl phosphite, tris(mononylphenyl)phosphite, tris(mononyl / dinonyl phenyl)phosphite, tris(2,4-di-tert-butylphenyl)phosphite, monooctyl diphenyl phosphite, dioctyl monophenyl phosphite, monodecyl diphenyl phosphite, didecyl monophenyl phosphite, tridecyl phosphite, trilauryl phosphite, tristearyl phosphite, and 2,2-methylenebis(4,6-di-tert-butylphenyl)octyl phosphite. Specific examples of such organic phosphite compounds include "ADK STAB 1178", "ADK STAB 2112", and "ADK STAB HP-10" manufactured by ADEKA CORPORATION, "JP-351", "JP-360", and "JP-3CP" manufactured by Johoku Chemical Industry Co., Ltd., and "IRGAFOS 168" manufactured by BASF. The phosphorus-based stabilizer may be contained either as one type or as two or more types in any combination and ratio.

[0080] As the organic phosphate compound, an organic phosphate represented by the following general formula is preferable. [ka] In the formula, R 1 represents an alkyl group or an aryl group. n represents an integer of 1 to 2. When n is 1, two R 1 may be the same or different.

[0081] In the above general formula, R 1 R represents an alkyl group or an aryl group. 1 is more preferably an alkyl group having 1 or more, preferably 2 or more, and usually 30 or less, preferably 25 or less, carbon atoms, or an aryl group having 6 or more, usually 30 or less, carbon atoms. 1 is preferably an alkyl group rather than an aryl group. 1 If there are two or more, R 1 They may be the same or different.

[0082] Preferred compounds represented by the above general formula are 1 and long-chain alkyl acid phosphate compounds having 8 to 30 carbon atoms. Specific examples of long-chain alkyl groups having 8 to 30 carbon atoms include an octyl group, a 2-ethylhexyl group, an isooctyl group, a nonyl group, an isononyl group, a decyl group, an isodecyl group, a dodecyl group, a tridecyl group, an isotridecyl group, a tetradecyl group, a hexadecyl group, an octadecyl group, an eicosyl group, and a triacontyl group.

[0083] Examples of long-chain alkyl acid phosphates include octadecyl acid phosphate (i.e., stearyl acid phosphate), 2-ethylhexyl acid phosphate, decyl acid phosphate, lauryl acid phosphate, octadecyl acid phosphate, oleyl acid phosphate, behenyl acid phosphate, phenyl acid phosphate, nonylphenyl acid phosphate, cyclohexyl acid phosphate, phenoxyethyl acid phosphate, and alkoxypolyethylene glycol. Examples of the acid phosphate include cholesteryl acid phosphate, bisphenol A acid phosphate, dimethyl acid phosphate, diethyl acid phosphate, dipropyl acid phosphate, diisopropyl acid phosphate, dibutyl acid phosphate, dioctyl acid phosphate, di-2-ethylhexyl acid phosphate, dioctyl acid phosphate, dilauryl acid phosphate, distearyl acid phosphate, diphenyl acid phosphate, and bisnonylphenyl acid phosphate.

[0084] Among these, octadecyl acid phosphate (i.e., stearyl acid phosphate) or mono- and di-stearyl acid phosphate are preferred because they have high heat resistance, so they generate little decomposition gas at resin processing temperatures, and because they have good compatibility with resins and good dispersibility in resins, they bleed out little onto the surface of resin-processed products. These are commercially available under the product name "ADEKA STAB AX-71" manufactured by ADEKA Corporation.

[0085] As the organic phosphate compound, organic phosphate metal salts can be suitably used, specifically, a mixture of zinc salt of distearyl acid phosphate and zinc salt of monostearyl acid phosphate, mono- and di-stearyl acid phosphate, etc. can be mentioned. Specific examples of such organic phosphate metal salts include "JP-518Zn" manufactured by Johoku Chemical Industry Co., Ltd., and examples of mono- and di-stearyl acid phosphates include "AX-71" manufactured by ADEKA Corporation.

[0086] Among the above, mono- or di-stearyl acid phosphate and mixtures thereof are preferred since they exhibit resin stability even with a small amount added, and therefore are less likely to cause changes in appearance, such as whitening, in a moist and hot environment.

[0087] The content of the phosphorus-based stabilizer is preferably 0.01 to 0.15 parts by mass, more preferably 0.015 parts by mass or more, more preferably 0.14 parts by mass or less, and more preferably 0.13 parts by mass or less, relative to 100 parts by mass of the aromatic polycarbonate resin (A). When the content of the phosphorus-based stabilizer is within the above range, a good heat stabilizing effect is exhibited.

[0088] [Phenol-based stabilizer] The polycarbonate resin composition of the present invention preferably contains a phenol-based stabilizer, such as a hindered phenol-based antioxidant. Specific examples thereof include pentaerythritol tetrakis[3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate], octadecyl-3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate, thiodiethylene bis[3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate], N,N'-hexane-1,6-diylbis[3-(3,5-di-tert-butyl-4-hydroxyphenylpropionamide)], 2,4-dimethyl-6-(1-methylpentadecyl)phenol, diethyl[[3,5-bis(1,1-dimethylethyl)-4-hydroxyphenyl]methyl]phosphonate, 3,3',3",5,5',5"-hexa-tert-butyl-a,a',a"-(mesitylene-2,4,6- triyl)tri-p-cresol, 4,6-bis(octylthiomethyl)-o-cresol, ethylene bis(oxyethylene)bis[3-(5-tert-butyl-4-hydroxy-m-tolyl)propionate], hexamethylene bis[3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate], 1,3,5-tris(3,5-di-tert-butyl-4-hydroxybenzyl)-1,3,5-triazine-2,4,6(1H,3H,5H)-trione, 2,6-di-tert-butyl-4-(4,6-bis(octylthio)-1,3,5-triazin-2-ylamino)phenol, 2-[1-(2-hydroxy-3,5-di-tert-pentylphenyl)ethyl]-4,6-di-tert-pentylphenyl acrylate, and the like.

[0089] Among them, pentaerythritol tetrakis[3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate] and octadecyl-3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate are preferred.Specific examples of such phenol-based antioxidants include "Irganox 1010" and "Irganox 1076" manufactured by BASF, and "Adeka STAB AO-50" and "Adeka STAB AO-60" manufactured by ADEKA. The phenol-based stabilizer may be contained either as one type or as two or more types in any combination and ratio.

[0090] The content of the phenol-based stabilizer is usually 0.001 parts by mass or more, preferably 0.01 parts by mass or more, and usually 1 part by mass or less, preferably 0.5 parts by mass or less, based on 100 parts by mass of the aromatic polycarbonate resin (A). If the content of the phenol-based stabilizer is less than the lower limit of the above range, the effect of the phenol-based stabilizer may be insufficient, and if the content of the phenol-based stabilizer exceeds the upper limit of the above range, the effect may plateau and become uneconomical.

[0091] [Release agent] The polycarbonate resin composition of the present invention also preferably contains a release agent, such as an aliphatic carboxylic acid, an ester of an aliphatic carboxylic acid and an alcohol, an aliphatic hydrocarbon compound having a number average molecular weight of 200 to 15,000, or a polysiloxane-based silicone oil.

[0092] Examples of the aliphatic carboxylic acid include saturated or unsaturated aliphatic mono-, di- or tri-carboxylic acids. Here, the aliphatic carboxylic acid also includes alicyclic carboxylic acids. Among these, preferred aliphatic carboxylic acids are mono- or di-carboxylic acids having 6 to 36 carbon atoms, and more preferred are saturated aliphatic mono-carboxylic acids having 6 to 36 carbon atoms. Specific examples of such aliphatic carboxylic acids include palmitic acid, stearic acid, caproic acid, capric acid, lauric acid, arachic acid, behenic acid, lignoceric acid, cerotic acid, melissic acid, tetralinic acid, montanic acid, adipic acid, and azelaic acid.

[0093] The aliphatic carboxylic acid in the ester of aliphatic carboxylic acid and alcohol can be, for example, the same as the aliphatic carboxylic acid. On the other hand, the alcohol can be, for example, a saturated or unsaturated monohydric or polyhydric alcohol. These alcohols may have a substituent such as a fluorine atom or an aryl group. Among these, a monohydric or polyhydric saturated alcohol having 30 or less carbon atoms is preferred, and an aliphatic saturated monohydric alcohol or an aliphatic saturated polyhydric alcohol having 30 or less carbon atoms is more preferred. Here, the term aliphatic is used to include alicyclic compounds.

[0094] Specific examples of such alcohols include octanol, decanol, dodecanol, stearyl alcohol, behenyl alcohol, ethylene glycol, diethylene glycol, glycerin, pentaerythritol, 2,2-dihydroxyperfluoropropanol, neopentylene glycol, ditrimethylolpropane, and dipentaerythritol.

[0095] The above ester may contain an aliphatic carboxylic acid and / or alcohol as an impurity. The above ester may be a pure substance, or may be a mixture of a plurality of compounds. The aliphatic carboxylic acid and alcohol that are combined to form an ester may each be one type, or two or more types may be used in any combination and ratio.

[0096] Specific examples of esters of aliphatic carboxylic acids and alcohols include beeswax (a mixture mainly composed of myricyl palmitate), stearyl stearate, behenyl behenate, stearyl behenate, glycerin monopalmitate, glycerin monostearate, glycerin distearate, glycerin tristearate, pentaerythritol monopalmitate, pentaerythritol monostearate, pentaerythritol distearate, pentaerythritol tristearate, and pentaerythritol tetrastearate.

[0097] Examples of aliphatic hydrocarbons having a number average molecular weight of 200 to 15,000 include liquid paraffin, paraffin wax, microwax, polyethylene wax, Fischer-Tropsch wax, and α-olefin oligomers having 3 to 12 carbon atoms. The aliphatic hydrocarbons also include alicyclic hydrocarbons. These hydrocarbons may be partially oxidized.

[0098] Among these, paraffin wax, polyethylene wax, or a partial oxide of polyethylene wax is preferred, and paraffin wax and polyethylene wax are more preferred. The number average molecular weight of the aliphatic hydrocarbon is preferably 5,000 or less. The aliphatic hydrocarbon may be a single substance, but a mixture of substances having various constituent components and molecular weights can also be used as long as the main component is within the above range.

[0099] Examples of polysiloxane-based silicone oils include dimethyl silicone oil, methylphenyl silicone oil, diphenyl silicone oil, and fluorinated alkyl silicone.

[0100] The above-mentioned release agents may be contained alone or in any combination and ratio of two or more kinds.

[0101] The content of the release agent is usually 0.001 parts by mass or more, preferably 0.01 parts by mass or more, and usually 2 parts by mass or less, preferably 1 part by mass or less, based on 100 parts by mass of the aromatic polycarbonate resin (A). If the content of the release agent is less than the lower limit of the above range, the effect of releasability may be insufficient, whereas if the content of the release agent is more than the upper limit of the above range, there is a possibility that the hydrolysis resistance may decrease and the mold may be contaminated during injection molding.

[0102] [Other ingredients] The polycarbonate resin composition of the present invention may contain other components in addition to those described above, as necessary, as long as the desired physical properties are not significantly impaired. Examples of other components include resins other than polycarbonate resins, various resin additives, etc. Note that the other components may be contained in one type, or in any combination and ratio of two or more types.

[0103] Other resins Other resins include, for example, thermoplastic polyester resins such as polyethylene terephthalate, polytrimethylene terephthalate, and polybutylene terephthalate; styrene-based resins such as polystyrene resin, high impact polystyrene resin (HIPS), and acrylonitrile-styrene copolymer (AS resin); polyolefin resins such as polyethylene resin and polypropylene resin; polyamide resins; polyimide resins; polyetherimide resins; polyurethane resins; polyphenylene ether resins; polyphenylene sulfide resins; polysulfone resins; polymethacrylate resins, and the like.

[0104] The other resins may be contained either alone or in any combination and ratio of two or more kinds. However, when other resins are contained, the content is preferably 20 parts by mass or less, more preferably 10 parts by mass or less, even more preferably 5 parts by mass or less, of which 3 parts by mass or less, and particularly preferably 1 part by mass or less, per 100 parts by mass of the aromatic polycarbonate resin (A).

[0105] Resin additives Examples of resin additives include ultraviolet absorbers, dyes and pigments, antistatic agents, antifogging agents, antiblocking agents, flow improvers, plasticizers, dispersants, etc. The resin additives may be contained alone or in any combination and ratio of two or more kinds.

[0106] [Method for producing polycarbonate resin composition] There is no limitation on the method for producing the polycarbonate resin composition of the present invention, and a wide variety of known methods for producing polycarbonate resin compositions can be used. Specific examples include a method in which the above-mentioned essential components and other components to be blended as necessary are premixed using various mixers such as a tumbler or a Henschel mixer, and then melt-kneaded using a mixer such as a Banbury mixer, a roll, a Brabender, a single-screw kneading extruder, a twin-screw kneading extruder, or a kneader.

[0107] Also, for example, the polycarbonate resin composition of the present invention can be produced by not mixing the components in advance, or by mixing only some of the components in advance, feeding the mixture to an extruder using a feeder, and melt-kneading the mixture. In addition, for example, some of the components are mixed in advance, fed to an extruder, and melt-kneaded to obtain a resin composition, which is used as a masterbatch, and this masterbatch is then mixed again with the remaining components and melt-kneaded to produce the polycarbonate resin composition of the present invention. In addition, for example, when mixing a component that is difficult to disperse, the dispersibility can be improved by dissolving or dispersing the component in advance in a solvent such as water or an organic solvent, and kneading the component with the solution or dispersion.

[0108] The polycarbonate resin composition of the present invention has high transparency, and a 2 mm thick plate molded using the composition exhibits a haze value of 20% or less. The haze value is preferably 15% or less, more preferably 12% or less, and even more preferably 10% or less, with the lower limit being preferably 2% or more, and even more preferably 3% or more. The details of the method for measuring the haze value are as described in the Examples, but the haze value is measured on the obtained plate of 2 mm thickness, 50 mm length × 50 mm width with a haze meter in accordance with JIS K7136 and JIS K7361, with a D65 light source and a 10° visual field.

[0109] The polycarbonate resin composition of the present invention has high impact resistance, and preferably has a Charpy notched impact strength according to ISO179 of 20 kJ / m 2 More preferably, the Charpy impact strength is 25 kJ / m 2 More preferably, 30 kJ / m 2 Above 35kJ / m 2 More than 40kJ / m 2 More than 45kJ / m 2 More than 50kJ / m 2 More than 55kJ / m 2 Above 60kJ / m 2 That's all.

[0110] The manufacturing method of the molded body can be any molding method generally used for polycarbonate resin compositions. Examples of the molding method include injection molding, ultra-high speed injection molding, injection compression molding, two-color molding, gas-assisted hollow molding, molding using a heat-insulating mold, molding using a rapid heating mold, foam molding (including supercritical fluid), insert molding, IMC (in-mold coating molding) molding, extrusion molding, sheet molding, thermoforming, rotational molding, lamination molding, press molding, blow molding, and the like. Also, molding using a hot runner system can be used. Among them, injection molding methods such as injection molding, ultra-high speed injection molding, and injection compression molding are preferred.

[0111] [Molded body] Examples of molded articles include parts for electric / electronic devices, office automation equipment, information terminal devices, machine parts, home appliances, vehicle parts, building materials, various containers, leisure goods / miscellaneous goods, lighting equipment, etc. They are particularly suitable for products and parts that are touched by human hands, such as switches and buttons for miscellaneous goods and general home appliances, elevator operation buttons, buttons and front covers for amusement machines such as pachinko and slot machines, leisure goods and play equipment, etc. EXAMPLES

[0112] The present invention will be described in more detail below with reference to examples, but the present invention should not be construed as being limited to the following examples. The components used in the examples and comparative examples are as shown in Table 1 below.

[0113] [Table 1]

[0114] (Examples 1 to 15, Comparative Examples 1 to 12) [Resin pellet manufacturing] The components shown in Table 1 above were mixed in the ratios (mass ratios) shown in Table 2 below, and kneaded in a twin-screw extruder (Shibaura Machine Co., Ltd., "TEM26SX") at a barrel temperature of 280°C and 200 rpm, producing polycarbonate resin composition pellets at a discharge rate of 20 kg / hr.

[0115] [Molding conditions] The obtained pellets were dried at 80°C for 5 hours, and then injection molded using an injection molding machine (Japan Steel Works, Ltd., "J85AD") under conditions of a resin temperature of 280°C and a mold temperature of 80°C to obtain ASTM D790 bending test pieces.

[0116] [Chemical resistance test] Using a jig that can apply a three-point bending load as shown in Figure 1, an ASTM D790 bending test piece 1, with ethanol applied to it, is attached to the central lower part of a test piece attachment jig 2, and a caulking adjustment cylinder 3 for adjusting the amount of deflection is attached to the test piece attachment jig 2 and fixed with a thumbscrew 4, making it possible to adjust the amount of deflection (deformation rate %). After applying ethanol to the longitudinal center of the test piece, it was bent at three points so that the deformation rate was 1%. After leaving it for 48 hours in an environment of room temperature 23°C and 50% Rh, the ethanol-applied area was observed with an optical microscope to check for the presence or absence of cracks.

[0117] [Chemical resistance evaluation] The chemical resistance was evaluated according to the following criteria. A: No cracks occur. If cracks occur and the length of all cracks is less than 5 mm, it is classified as B. If cracks occurred and any of the cracks were 5 mm or longer, the test was rated C.

[0118] [Preparation of plates for antibacterial evaluation and haze measurement] The obtained pellets were dried at 80°C for 5 hours, and then injection molded using an injection molding machine (Japan Steel Works, Ltd., "J85AD") under conditions of a resin temperature of 280°C and a mold temperature of 80°C to obtain plates of 2 mm thickness, 100 mm length x 100 mm width. These were then cut to 2 mm thickness, 50 mm length x 50 mm width to obtain plates for antibacterial evaluation and haze measurement.

[0119] [Antibacterial evaluation] Using the obtained 2 mm thick, 50 mm long x 50 mm wide plate, the viable E. coli count after 24 hours in a room temperature of 35°C and 90% Rh environment was confirmed according to the method described in JIS Z2801. If there was no increase in the viable cell count after 24 hours, it was marked with an "O"; if there was an increase, it was marked with an "X".

[0120] [Transparency: HAZE measurement] The haze value (%) of the obtained 2 mm thick, 50 mm long x 50 mm wide plate was measured in accordance with JIS K7136 and JIS K7361 using a haze meter "NDH4000" manufactured by Nippon Denshoku Industries Co., Ltd., with a D65 light source and a 10° visual field.

[0121] [Heat and humidity resistance evaluation] The obtained plate having a thickness of 2 mm and a length of 50 mm×width of 50 mm was left to stand in a humid heat environment of 85° C. and 85% Rh for 100 hours, and the difference in haze value (%) before and after the standing was measured.

[0122] [Impact resistance: Notched Charpy impact test] The pellets obtained were dried at 80°C for 5 hours, and then injection molded using an injection molding machine (Japan Steel Works, Ltd., "J85AD") under conditions of a resin temperature of 280°C and a mold temperature of 80°C. ISO527-1,2 dumbbell test pieces Type 1A were prepared with a thickness of 3 mm, which were then cut into the shape of a notched Charpy test piece as specified in ISO179, and the Charpy impact strength (unit: kJ / m 2 ) was measured.

[0123] [Heat resistance: DTUL measurement (temperature deflection under load, unit: °C)] The obtained pellets were dried at 80°C for 5 hours, and then injection molded using a Japan Steel Works "J85AD" injection molding machine under conditions of a resin temperature of 280°C and a mold temperature of 80°C. Dumbbell test pieces Type 1A of ISO527-1,2 were prepared with a thickness of 4 mm, which were then cut into the test piece shape specified in ISO75-2, and the DTUL (unit: °C) at a load of 1.8 MPa was measured using the method specified in ISO75-2. The results are shown in Table 2-5 below. In the table, "Act n" represents Example n, and "Comparative n" represents Comparative Example n.

[0124] [Table 2]

[0125] [Table 3]

[0126] [Table 4]

[0127] [Table 5]

[0128] [Antibacterial evaluation - Antibacterial activity value] Furthermore, for Example 1 and Comparative Example 1, the following antibacterial test was carried out. The obtained plate, 2 mm thick, 50 mm long x 50 mm wide, was immersed in 50°C water for 18 hours (corresponding to water resistance category 2 in the sustainability criteria of the Council of Antibacterial Product Technology), and then the antibacterial activity value R against Staphylococcus aureus (NBRC 12732) after 24 hours in a room temperature of 35°C and 90% Rh environment was measured using the method described in JIS Z2801. If the obtained antibacterial activity value R was 2 or more, it was judged as A; if the antibacterial activity value R was 1 or more and less than 2, it was judged as B; and if the antibacterial activity value R was less than 1, it was judged as C. The results are shown in Table 6 below.

[0129] [Table 6] [Industrial Applicability]

[0130] INDUSTRIAL APPLICABILITY The antibacterial polycarbonate resin composition of the present invention has high transparency, high antibacterial activity, high impact resistance, and further excellent heat resistance, moist heat resistance, and chemical resistance, and can therefore be widely and suitably used for parts of home appliances, daily necessities, miscellaneous goods, amusement machines, game equipment, play equipment, etc. that are touched by people's hands, and has extremely high industrial applicability.

Claims

1. An antibacterial polycarbonate resin composition comprising 100 parts by mass of an aromatic polycarbonate resin (A) having a viscosity average molecular weight of 17,000 to 28,000, 5 to 80 parts by mass of a thermoplastic resin (B) other than the aromatic polycarbonate resin (A) having a tensile modulus of elasticity of 1.0 to 2.5 GPa according to ISO 527-1 and -2 and a refractive index of 1.45 to 1.59 according to ISO 489, and 0.2 to 2.5 parts by mass of an inorganic oxide (C) containing at least one of Ag, Zn, Zr and Cu elements, wherein the thermoplastic resin (B) is a thermoplastic polyester resin containing terephthalic acid residues, 1,4-cyclohexanedimethanol residues, and 2,2,4,4-tetramethyl-1,3-cyclobutanediol residues, and the haze value measured on a 2 mm thick plate is 20% or less.

2. 2. The polycarbonate resin composition according to claim 1, further comprising a phosphorus-based stabilizer (D) in an amount of 0.01 to 0.15 parts by mass per 100 parts by mass of the aromatic polycarbonate resin (A).

3. 3. The polycarbonate resin composition according to claim 1, wherein the inorganic oxide (C) has a refractive index according to ISO 489 of 1.45 to 1.

59.

4. 4. The polycarbonate resin composition according to claim 1, wherein the inorganic oxide (C) is an inorganic oxide capable of eluting Ag, Zn, Zr or Cu ions.

5. 3. The polycarbonate resin composition according to claim 2, wherein the phosphorus-based stabilizer (D) is a stearyl acid phosphate-based stabilizer.

6. ISO179 notched Charpy impact strength is 20 kJ / m 2 The polycarbonate resin composition according to any one of claims 1 to 5.

7. A molded article comprising the polycarbonate resin composition according to any one of claims 1 to 6.

Citation Information

Patent Citations

  • Bark beetle inducing agent

    JP1978088326A

  • Thermoplastic resin composition

    JP2003246925A

  • Antimicrobial resin composition and its molding

    JP2004359755A

  • Antibacterial phosphate glass with adjusted refractive index

    JP2005255517A

  • Thermoplastic resin composition, and method for manufacturing molded article

    WO2019146807A2