Aromatic polyester resin expanded particles, their production method, expanded molded article, and automobile component
By controlling resin thickness and crystallinity through adjusted cooling water temperatures, the method enhances the mechanical properties of aromatic polyester resin foam particles, improving secondary foamability and moldability for automobile applications.
Patent Information
- Application Number
- JP2021044095
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2021-03-17
- Publication Date
- 2024-12-09
- Estimated Expiration
- 2041-03-17
AI Technical Summary
Existing methods for producing aromatic polyester resin foam particles result in foamed molded articles with poor mechanical strength due to high crystallinity and uneven cell diameters, leading to poor secondary foamability and moldability.
Control the thickness of the resin layer, degree of crystallinity, and cell diameter by adjusting the cooling water temperature during the water ring hot cut method to within specific ranges, ensuring a ratio of 0.30 to 1.40 for surface to center crystallinity and a ratio of 0.75 to 0.95 for cell diameters.
The method produces foamed aromatic polyester resin particles with excellent mechanical properties, including compressive strength and bending strength, suitable for automobile components.
Smart Images

Figure 0007596189000004 
Figure 0007596189000005 
Figure 0007596189000006
Abstract
Description
[Technical field]
[0001] The present invention relates to an aromatic polyester resin foamed bead for in-mold foam molding, a production method thereof, a foam molded article, and an automobile part. [Background technology]
[0002] In-mold foam molding has been widely used as a method for producing an aromatic polyester resin foam molded article by foaming aromatic polyester resin foam particles. In-mold foam molding is a molding method including a step of filling a mold with resin foam particles, and a step of heating the resin foam particles filled in the mold with a heat medium such as hot water or steam to cause secondary foaming, and heat-fusing and integrating the secondary foam particles together to produce an in-mold foam molded article having a desired shape. Expanded beads made of aromatic polyester resin are produced by extruding a base resin that has been melt-kneaded in an extruder in the presence of a blowing agent, and simultaneously expanding the resin. In this process, the hot cut method, underwater cut method, etc. are used.
[0003] In Patent Document 1, expanded aromatic polyester resin particles are produced by a water ring hot cut method, that is, a method in which a molten and kneaded resin extruded under a gas is cut and the cut particles are cooled with cooling water. In addition, in Patent Document 2, expanded aromatic polyester resin particles are produced by an underwater cutting method, that is, a method in which an extruded molten and kneaded resin is cut and cooled in water. [Prior art documents] [Patent documents]
[0004] [Patent Document 1] Patent No. 5974010 [Patent Document 2] European Patent Application Publication No. 2564799 Summary of the Invention [Problem to be solved by the invention]
[0005] The expanded beads manufacturing method of Patent Document 1 can produce expanded beads that can be stored for a long period after production. However, it has been difficult to increase the mechanical strength of an expanded molded article obtained from the expanded beads obtained by this manufacturing method. In the expanded bead manufacturing method of Patent Document 2, cut resin particles are turned into expanded beads and immediately released into water at about 80° C. to cool. However, according to the present inventors, the expanded beads manufactured by this method have poor secondary expandability and require improvement in moldability.
[0006] An object of the present invention is to provide an aromatic polyester resin foamed molded article having excellent mechanical properties.An object of the present invention is to provide an aromatic polyester resin foamed bead for producing the foamed molded article.An object of the present invention is to provide a method for producing the foamed bead. [Means for solving the problem]
[0007] The present inventors have found that the thickness of the surface resin of the expanded beads obtained by the manufacturing method of Patent Document 1 is extremely large, which results in poor secondary expandability of the expanded beads. Furthermore, the present inventors have found that in the expanded beads obtained by the manufacturing method of Patent Document 2, the thickness of the surface resin of the expanded beads is extremely large, the crystallinity of the surface layer resin is considerably higher than that of the central resin of the expanded beads, and the average cell diameter of the expanded beads is large and the difference between the average cell diameter of the surface layer is large, which results in poor secondary expandability of the expanded beads. More specifically, the present inventors have found that, since aromatic polyester resins are crystalline resins, if the crystallinity of the expanded beads is too high, the fusion property of the secondary expanded beads may be reduced when the secondary expanded beads are thermally fused and integrated. The present inventors have also found that if the resin layer on the surface of the expanded beads is too thick, the secondary expandability is reduced, and the surface elongation of the molded product and the fusion property of the secondary expanded beads in the expanded molded product are deteriorated. Furthermore, the present inventors have found that if the difference between the average cell diameter in the center of the expanded beads and the average cell diameter in the surface layer is too large, stress concentration is likely to occur in the bubbles when the expanded molded product is compressed, and the mechanical properties of the expanded molded product are deteriorated.
[0008] The inventors focused on the thickness of the resin on the surface of the expanded beads, the degree of crystallinity of the expanded beads, the bubble diameter of the expanded beads, etc., and discovered that by adjusting the cooling water temperature within a specific range in the water ring hot cut method, the surface resin thickness, degree of crystallinity, and bubble diameter of the expanded beads can be controlled within predetermined ranges, that these expanded beads have excellent secondary expandability, and that the expanded molded articles obtained by expansion molding of these expanded beads have excellent mechanical properties, such as compressive strength and bending strength, and thus completed the present invention.
[0009] The present invention typically includes the following aspects. Section 1. Expanded aromatic polyester resin particles, in which the crystallinity (A) at the center of the particle and the crystallinity (B) at the surface of the particle are both 10% or less, and the ratio of the crystallinity at the surface to the crystallinity at the center (B / A) is 0.30 to 1.40. Section 2. Item 2. The expanded aromatic polyester resin particles according to item 1, wherein the thickness of the resin layer on the particle surface is 5 μm to 40 μm. Section 3. Item 3. The expanded aromatic polyester resin particles according to item 1 or 2, wherein the average cell diameter (C) in the particle center and the average cell diameter (D) in the particle surface layer are both 50 μm to 300 μm, and the ratio (D / C) of the average cell diameter in the surface layer to the average cell diameter in the particle center is 0.75 to 0.95. Section 4. 4. The expanded aromatic polyester resin particles according to any one of items 1 to 3, wherein the ratio (B / A) of the crystallinity in the surface layer to the crystallinity in the center of the particle is 0.30 to 1.30. Section 5. 5. The expanded aromatic polyester resin particles according to any one of items 1 to 4, wherein the crystallinity (A) in the particle center and the crystallinity (B) in the particle surface are both 1 to 10%. Section 6. Item 6. An expansion molded product of the expanded aromatic polyester resin particles according to any one of items 1 to 5. Section 7. Density is 0.05g / cm 3 ~0.7g / cm 3 Item 7. The foamed molded article according to item 6, wherein Section 8. Item 8. An automotive component comprising the foamed molded article according to item 6 or 7. Section 9. A method for producing expanded aromatic polyester resin particles, comprising the steps of: supplying an aromatic polyester resin to an extruder and melt-kneading the resin in the presence of a foaming agent; extruding and foaming the melt-kneaded aromatic polyester resin under gaseous conditions from a nozzle die attached to the front end of the extruder while cutting the resin to produce granular cut pieces; and cooling the granular cut pieces with cooling water, wherein the temperature of the cooling water is 23°C to 55°C. Effect of the Invention
[0010] According to the present invention, it is possible to provide an aromatic polyester resin expanded particle capable of producing an expanded molded article having excellent mechanical properties and a method for producing the same. According to the present invention, it is possible to provide an expanded molded article having excellent mechanical properties, such as compressive strength and flexural strength, and an automobile member containing the same. [Brief description of the drawings]
[0011] [Figure 1] FIG. 1 is a schematic cross-sectional view showing an example of an apparatus for producing expanded aromatic polyester resin beads. [Diagram 2] FIG. 2 is a schematic diagram showing a multi-nozzle mold as viewed from the front. [Diagram 3]2 is a schematic diagram showing a state in which expanded aromatic polyester resin particles enter cooling water. FIG. [Figure 4] 1 shows SEM images of cross sections of the central portion (100x) and surface portion (100x and 500x) of the expanded beads produced in Examples 1 to 3. [Diagram 5] 1 shows SEM images of cross sections of the center portion (100x) and surface portion (100x and 500x) of the expanded beads produced in Examples 4 and 5. [Figure 6] 1 shows SEM images of cross sections of the central portion (100x) and surface portion (100x and 500x) of the expanded beads produced in Comparative Examples 1 to 3. [Figure 7] 1 shows SEM images of cross sections of the center portion (100x) and surface portion (100x and 500x) of the expanded beads produced in Comparative Examples 4 and 5. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0012] As used herein, the phrase "comprising" is intended to encompass the phrases "consisting essentially of" and "consisting of."
[0013] (Aromatic polyester resin foam particles) The expanded aromatic polyester resin particles contain an aromatic polyester resin as a main component. Here, the term "main component" means that the resin constituting the expanded aromatic polyester resin particles contains 80 to 100 mass %, preferably 90 to 100 mass %, of the aromatic polyester resin.
[0014] (Aromatic polyester resin) The aromatic polyester resin is a polyester containing an aromatic dicarboxylic acid component and a diol component, and examples thereof include polyethylene terephthalate, polypropylene terephthalate, polybutylene terephthalate, polycyclohexane dimethylene terephthalate, polyethylene naphthalate, polybutylene naphthalate, etc., with polyethylene terephthalate being preferred. The aromatic polyester resin may be used alone or in combination of two or more kinds.
[0015] In addition to the aromatic dicarboxylic acid component and the diol component, the aromatic polyester resin may contain, as a constituent component, for example, a trivalent or higher polyvalent carboxylic acid such as a tricarboxylic acid such as trimellitic acid, a tetracarboxylic acid such as pyromellitic acid, or an anhydride thereof, a triol such as glycerin, or a trivalent or higher polyhydric alcohol such as a tetraol such as pentaerythritol.
[0016] The aromatic polyester resin may be derived not only from petroleum but also from plants or recycled materials recovered and regenerated from used PET bottles.
[0017] The intrinsic viscosity (IV value) of the aromatic polyester resin is preferably 0.7 to 1.1, and more preferably 0.75 to 1.05, in order to provide excellent extrusion foamability and excellent secondary foamability of the resulting expanded beads.
[0018] The intrinsic viscosity (IV value) of the aromatic polyester resin refers to a value measured in accordance with JIS K7367-5 (2000). Specifically, the aromatic polyester resin is dried at 40° C. under a vacuum of 133 Pa for 15 hours.
[0019] Take 0.1000g of the aromatic polyester resin as a sample and place it in a 20mL measuring flask, then add about 15mL of a mixed solvent (phenol 50% by weight, 1,1,2,2-tetrachloroethane 50% by weight) to the measuring flask. Place the sample in the measuring flask on a hot plate and heat it to about 130°C to melt it. After melting the sample, cool it to room temperature and adjust the volume to 20mL to prepare a sample solution (sample concentration: 0.500g / 100mL).
[0020] 8 mL of the sample solution is supplied to the viscometer using a whole pipette, and the temperature of the sample is stabilized using a water bath filled with 25°C water, after which the flow time of the sample is measured. To change the concentration of the sample solution, 8 mL of the mixed solvent is added to the viscometer in sequence, mixed, and diluted to produce a diluted sample solution. The flow time of the diluted sample solution is then measured. The flow time of the mixed solvent is measured separately from the sample solution.
[0021] The intrinsic viscosity of the aromatic polyester resin was calculated based on the following formula: The following was calculated from the flow time (t0) of the mixed solvent and the flow time (t) of the sample solution. Relative viscosity (η r ) =t / t0 Specific viscosity (η sp )=(t-t0) / t0=η r -1 Reduced viscosity = η sp / C From the measurement results of diluted sample solutions with various sample solution concentrations C (g / 100 mL), a graph was created with the reduced viscosity on the vertical axis and the sample solution concentration C on the horizontal axis, and the intrinsic viscosity [η] was calculated from the vertical intercept obtained by extrapolating the linear relationship to C = 0.
[0022]
number
[0023] The aromatic polyester resin constituting the aromatic polyester resin foamed particles may be modified aromatic polyester resin crosslinked by a crosslinking agent.As the crosslinking agent, a known one is used, for example, an acid dianhydride such as pyromellitic anhydride, a polyfunctional epoxy compound, an oxazoline compound, an oxazine compound, etc.In addition, the crosslinking agent may be used alone or in combination of two or more kinds.
[0024] When the aromatic polyester resin is modified by crosslinking with a crosslinking agent, the aromatic polyester resin and the crosslinking agent are fed to an extruder during the production of the expanded aromatic polyester resin particles, and the aromatic polyester resin is crosslinked with the crosslinking agent in the extruder. The amount of the crosslinking agent fed to the extruder is preferably 0.01 to 5 parts by mass, more preferably 0.1 to 1 part by mass, per 100 parts by mass of the aromatic polyester resin, from the viewpoint of performing the extrusion foaming well.
[0025] The mass average molecular weight of the aromatic polyester resin constituting the expanded beads of the present invention is preferably 45,000 to 100,000, more preferably 60,000 to 90,000, in order to provide excellent extrusion foamability and excellent secondary foamability of the resulting expanded beads. When the aromatic polyester resin constituting the expanded beads is a modified aromatic polyester resin, the mass average molecular weight of the aromatic polyester resin means the mass average molecular weight of the modified aromatic polyester resin.
[0026] The mass average molecular weight (Mw) of the aromatic polyester resin constituting the expanded beads of the present invention means the mass average molecular weight in terms of polystyrene (PS) measured using gel permeation chromatography (GPC). Specifically, the mass average molecular weight is measured as follows. 0.5 mL of hexafluoroisopropanol (HFIP) and 0.5 mL of chloroform are added to 5 mg of sample in this order to dissolve the sample (immersion time: 6.0±1.0 hr (complete dissolution)) to obtain a sample solution. After confirming that the sample is completely dissolved in the solution, chloroform is added to the sample solution to dilute it to a volume of 10 mL, and the solution is shaken and mixed. The sample solution is filtered through a non-aqueous 0.45 μm syringe filter manufactured by Shimadzu GLC Co., Ltd. to obtain a filtrate. The filtrate is measured using a chromatograph under the following measurement conditions. The mass average molecular weight (Mw) is determined from a standard polystyrene calibration curve prepared in advance. Equipment used: Tosoh Corporation's "HLC-8320GPC EcoSEC" gel permeation chromatograph (with built-in RI and UV detectors) (GPC measurement conditions) column Sample side Guard column = TSK guardcolumn HXL-H (6.0mm x 4.0cm) x 1, manufactured by Tosoh Corporation Measurement column: Tosoh Corporation's TSKgel GMHXL (7.8 mm I.D. x 30 cm) x 2 in series Reference Side Resistance tube (inner diameter 0.1 mm x 2 m) x 2 in series Column temperature = 40 °C Mobile phase = chloroform Mobile phase flow rate Sample pump: 1.0 mL / min Reference pump = 0.5mL / min Detector: UV detector Wavelength: 254nm Injection volume: 15μL Measurement time: 10 minutes - 32 minutes Runtime: 20min Sampling pitch: 500msec The standard polystyrene samples used for the calibration curve were "STANDARD SM-105" and "STANDARD SH-75" manufactured by Showa Denko K.K., with mass average molecular weights of 5,620,000, 3,120,000, 1,250,000, 442,000, 151,000, 53,500, 17,000, 7,660, 2,900, and 1,320. The above-mentioned standard polystyrene for the calibration curve is grouped into A (5,620,000, 1,250,000, 151,000, 17,000, 2,900) and B (3,120,000, 442,000, 53,500, 7,660, 1,320), and then A (2mg, 3mg, 4mg, 4mg, 4mg) is weighed and dissolved in 30mL of chloroform, and B (3mg, 4mg, 4mg, 4mg) is also weighed and dissolved in 30mL of chloroform. The standard polystyrene calibration curve is obtained by injecting 50μL of each prepared A and B solution and creating a calibration curve (cubic equation) from the retention time obtained after measurement. The mass average molecular weight is calculated using the calibration curve.
[0027] (Method of producing expanded aromatic polyester resin particles) The expanded beads of the present invention can be produced by a production method that includes, for example, a step of feeding an aromatic polyester resin to an extruder and melt-kneading it in the presence of a foaming agent, a step of cutting the melt-kneaded aromatic polyester resin while extruding and foaming it under gas conditions from a nozzle die attached to the front end of the extruder to produce particulate cut pieces, and a step of cooling the particulate cut pieces with cooling water, the temperature of the cooling water being 23°C to 55°C. Such a production method is also one of the present invention. Note that, although this production method will be described below, the production method of the expanded aromatic polyester resin beads of the present invention is not limited to the following method.
[0028] First, an example of a manufacturing apparatus used for manufacturing expanded aromatic polyester resin particles will be described. In FIG. 1, a nozzle die 1 is attached to the front end of an extruder. The nozzle die 1 is preferable because it can extrude and foam an aromatic polyester resin to form uniform fine bubbles. As shown in FIG. 2, a plurality of nozzle outlets 11 are formed at equal intervals on the same imaginary circle A on the front end surface 1a of the nozzle die 2. The nozzle die attached to the front end of the extruder is not particularly limited as long as the aromatic polyester resin does not foam in the nozzle.
[0029] The number of nozzles in the nozzle die 1 is preferably 2 to 80, more preferably 5 to 60, and particularly preferably 8 to 50, from the standpoint of production efficiency and ability to suppress coalescence of cut pieces on particles.
[0030] The diameter of the nozzle outlet 11 in the nozzle die 1 is preferably 0.2 to 2 mm, more preferably 0.3 to 1.6 mm, and particularly preferably 0.4 to 1.2 mm, in order to set the extrusion pressure and the diameter of the expanded beads in appropriate ranges.
[0031] The length of the land portion of the nozzle die 1 is preferably 4 to 30 times the diameter of the outlet portion 11 of the nozzle of the nozzle die 1, and more preferably 5 to 20 times the diameter of the outlet portion 11 of the nozzle of the nozzle die 1. When the length of the land portion of the nozzle die is within the above range, it is advantageous in that the occurrence of fractures is suppressed and stable extrusion foaming can be performed.
[0032] In the portion of the front end face 1a of the nozzle die 1 surrounded by the nozzle outlet portion 11, a rotating shaft 2 is arranged so as to protrude forward, and this rotating shaft 2 penetrates a front portion 41a of a cooling drum 41 constituting a cooling member 4 described later, and is connected to a driving member 3 such as a motor.
[0033] Furthermore, one or more rotary blades 5 are integrally provided on the outer circumferential surface of the rear end of the rotating shaft 2, and all of the rotary blades 5 are constantly in contact with the front end surface 1a of the nozzle die 1 during rotation. When multiple rotary blades 5 are integrally provided on the rotating shaft 2, the multiple rotary blades 5 are arranged at equal intervals in the circumferential direction of the rotating shaft 2. Also, FIG. 2 shows, as an example, a case in which four rotary blades 5 are integrally provided on the outer circumferential surface of the rotating shaft 2.
[0034] As the rotating shaft 2 rotates, the rotating blade 5 moves on an imaginary circle A on which the nozzle outlet 11 is formed while constantly contacting the front end face 1a of the nozzle die 1, and is configured to be able to sequentially and continuously cut the aromatic polyester resin extrudate extruded from the nozzle outlet 11.
[0035] A cooling member 4 is disposed so as to surround at least the front end of the nozzle die 1 and the rotating shaft 2. This cooling member 4 is equipped with a bottomed cylindrical cooling drum 41 having a front part 41a with a circular front shape having a larger diameter than the nozzle die 1, and a cylindrical peripheral wall part 41b extending rearward from the outer periphery of this front part 41a.
[0036] Furthermore, a supply port 41c for supplying cooling water 42 is formed in a portion of the peripheral wall portion 41b of the cooling drum 41 that corresponds to the outside of the nozzle die 1, so as to penetrate between the inner and outer peripheral surfaces. A supply pipe 41d for supplying the cooling water 42 into the cooling drum 41 is connected to an outer opening of the supply port 41c of the cooling drum 41.
[0037] The cooling water 42 is configured to be supplied obliquely forward through the supply pipe 41d along the inner circumferential surface of the peripheral wall portion 41b of the cooling drum 41. The cooling water 42 advances forward in a spiral shape along the inner circumferential surface of the peripheral wall portion 41b of the cooling drum 41 due to centrifugal force associated with the flow speed when the cooling water 42 is supplied from the supply pipe 41d to the inner circumferential surface of the peripheral wall portion 41b of the cooling drum 41. The cooling water 42 gradually spreads in a direction perpendicular to the advancing direction while advancing along the inner circumferential surface of the peripheral wall portion 41b, so that the inner circumferential surface of the peripheral wall portion 41b in front of the supply port 41c of the cooling drum 41 is entirely covered with the cooling water 42.
[0038] The temperature of the cooling water is 23°C to 55°C, more preferably 24°C to 50°C, and particularly preferably 25°C to 45°C, from the viewpoint of appropriately adjusting the crystallinity of the expanded beads, the bubble size, or the thickness of the surface resin layer.
[0039] A discharge port 41e is formed in the lower surface of the front end of the peripheral wall portion 41b of the cooling drum 41 so as to penetrate from the inner to the outer circumferential surface. A discharge pipe 41f is connected to the outer opening of the discharge port 41e. The expanded aromatic polyester resin particles and the cooling water 42 are configured to be continuously discharged through the discharge port 41e.
[0040] The expanded aromatic polyester resin particles are preferably produced by extrusion foaming. For example, an aromatic polyester resin is fed to an extruder and melt-kneaded in the presence of a foaming agent, and then the aromatic polyester resin extrudate is extruded from a nozzle die 1 attached to the front end of the extruder and foamed while being cut by a rotary blade 5 to produce expanded aromatic polyester resin particles.
[0041] The extruder is not particularly limited as long as it is a conventionally and widely used extruder, and examples thereof include a single screw extruder, a twin screw extruder, and a tandem extruder in which a plurality of extruders are connected together.
[0042] The foaming agent may be one that has been widely used in the past. Examples of the foaming agent include chemical foaming agents such as azodicarbonamide, dinitrosopentamethylenetetramine, hydrazoyldicarbonamide, and sodium bicarbonate; saturated aliphatic hydrocarbon foaming agents such as propane, normal butane, isobutane, normal pentane, isopentane, and hexane; ether foaming agents such as dimethyl ether; fluorocarbon foaming agents such as methyl chloride, 1,1,1,2-tetrafluoroethane, 1,1-difluoroethane, and monochlorodifluoromethane; and inorganic foaming agents such as carbon dioxide and nitrogen. Dimethyl ether, propane, normal butane, isobutane, and carbon dioxide are preferred, propane, normal butane, isobutane, and carbon dioxide are more preferred, and normal butane, isobutane, and carbon dioxide are particularly preferred. The foaming agent may be used alone or in combination of two or more.
[0043] The amount of the foaming agent supplied to the extruder is preferably 0.1 to 5 parts by mass, more preferably 0.2 to 4 parts by mass, and particularly preferably 0.2 to 3 parts by mass, per 100 parts by mass of the aromatic polyester resin, in order to easily set the expansion ratio of the expanded beads in an appropriate range.
[0044] It is preferable that a bubble regulator is supplied to the extruder, and examples of such bubble regulators include polytetrafluoroethylene powder, polytetrafluoroethylene powder modified with an acrylic resin, and talc.
[0045] The amount of the cell control agent supplied to the extruder is preferably 0.01 to 5 parts by mass, more preferably 0.05 to 3 parts by mass, and particularly preferably 0.1 to 2 parts by mass, per 100 parts by mass of the aromatic polyester resin, in order to set the cell diameter of the expanded beads in an appropriate range.
[0046] The aromatic polyester resin extrudate extruded and foamed from the nozzle die 1 is then subjected to a cutting step. The aromatic polyester resin extrudate is cut by rotating the rotary shaft 2 to rotate the rotary blade 5 disposed on the front end surface 1a of the nozzle die 1. The rotation speed of the rotary blade 5 is preferably 2000 rpm to 10000 rpm. It is preferable that the rotary blade is rotated at a constant rotation speed.
[0047] All of the rotary blades 5 rotate while constantly in contact with the front end face 1a of the nozzle die 1, and the aromatic polyester resin extrudate extruded and foamed from the nozzle die 1 is cut into granular cut pieces in the atmosphere at regular time intervals by shear stress generated between the rotary blades 5 and the edge of the nozzle outlet portion 11 of the nozzle die 1.
[0048] In the present invention, the aromatic polyester resin is prevented from foaming in the nozzle of the nozzle mold 1. The aromatic polyester resin is not foamed immediately after being discharged from the outlet 11 of the nozzle of the nozzle mold 1, and starts to foam after a short time has passed since being discharged. Therefore, the aromatic polyester resin extrudate is composed of an unfoamed portion immediately after being discharged from the outlet 11 of the nozzle of the nozzle mold 1, and a foamed portion that is continuous with the unfoamed portion and is in the process of foaming, extruded ahead of the unfoamed portion.
[0049] The unfoamed portion maintains its state from the time it is discharged from the outlet 11 of the nozzle of the nozzle mold 1 until foaming begins. The time during which this unfoamed portion is maintained can be adjusted by the resin pressure at the outlet 11 of the nozzle of the nozzle mold 1, the amount of foaming agent, etc. If the resin pressure at the outlet 11 of the nozzle of the nozzle mold 1 is high, the aromatic polyester resin extrudate does not foam immediately after being extruded from the nozzle mold 1 and maintains an unfoamed state. The resin pressure at the outlet 11 of the nozzle of the nozzle mold 1 can be adjusted by the nozzle diameter, the extrusion amount, and the melt viscosity and melt tension of the aromatic polyester resin. By adjusting the amount of foaming agent to an appropriate amount, it is possible to prevent the aromatic polyester resin from foaming inside the mold and reliably form an unfoamed portion.
[0050] Since all of the rotary blades 5 are constantly in contact with the front end face 1a of the nozzle die 1 while cutting the aromatic polyester resin extrudate, the aromatic polyester resin extrudate is cut in the unfoamed portion immediately after being discharged from the nozzle outlet 11 of the nozzle die 1, producing particulate cut material.
[0051] As described above, the rotary blade 5 rotates at a constant rotation speed, and the rotation speed of the rotary blade 5 is preferably 2000 rpm to 10000 rpm, more preferably 2000 rpm to 9000 rpm, and particularly preferably 2000 rpm to 8000 rpm. If the rotation speed is within the above range, it is advantageous in that the reliability of cutting is improved or that adhesion of cut pieces on particles to each other can be suppressed.
[0052] The particulate cut pieces obtained as described above are scattered toward the cooling drum 41 at the same time as being cut by the cutting stress of the rotary blade 5, and immediately collide with the cooling water 42 that covers the inner peripheral surface of the peripheral wall portion 41b of the cooling drum 41. The particulate cut pieces continue to foam even before colliding with the cooling water 42, and the particulate cut pieces grow into a substantially spherical shape due to foaming. Therefore, the obtained aromatic polyester resin foamed particles are substantially spherical. When the aromatic polyester resin foamed particles are filled into a mold to perform in-mold foaming, the aromatic polyester resin foamed particles have excellent fillability into the mold, and the aromatic polyester resin foamed particles can be uniformly filled into the mold, and a homogeneous in-mold foamed product can be obtained.
[0053] The inner surface of the peripheral wall 41b of the cooling drum 41 is entirely covered with cooling water 42 (23°C to 55°C). This cooling water 42 is supplied diagonally forward along the inner surface of the peripheral wall 41b of the cooling drum 41 through the supply pipe 41d. Due to the centrifugal force associated with the flow speed when the cooling water 42 is supplied from the supply pipe 41d to the inner surface of the peripheral wall 41b of the cooling drum 41, the cooling water 42 advances forward in a spiral shape along the inner surface of the peripheral wall 41b of the cooling drum 41. As the cooling water 42 advances along the inner surface of the peripheral wall 41b, it gradually spreads in a direction perpendicular to the traveling direction. As a result, the inner surface of the peripheral wall 41b forward of the supply port 41c of the cooling drum 41 is entirely covered with the cooling water 42.
[0054] As described above, after the aromatic polyester resin extrudate is cut by the rotary blade 5, the particulate cut pieces are immediately cooled with cooling water 42 (23°C to 55°C), thereby preventing the aromatic polyester resin foam particles from expanding excessively.
[0055] Furthermore, the particulate cut pieces obtained by cutting the aromatic polyester resin extrudate with the rotary blade 5 are scattered toward the cooling water 42. As described above, the cooling water 42 flowing along the inner peripheral surface of the peripheral wall portion 41b of the cooling drum 41 flows while swirling in a spiral. Therefore, it is preferable to collide the particulate cut pieces P with the cooling water 42 obliquely and from the upstream side to the downstream side of the flow of the cooling water 42 (see FIG. 3) to enter the cooling water 42. In FIG. 3, the flow direction of the cooling water is indicated as "F".
[0056] In this way, when the particulate cut pieces are made to enter the cooling water 42, they are made to enter the cooling water 42 in a direction following the flow of the cooling water 42. Therefore, the particulate cut pieces are not repelled by the surface of the cooling water 42, but smoothly and reliably enter the cooling water 42 and are cooled by the cooling water 42, thereby producing aromatic polyester resin foamed particles.
[0057] Therefore, the expanded aromatic polyester resin particles have a substantially spherical shape without cooling unevenness or shrinkage, and exhibit excellent expandability during in-mold expansion molding. In the case of a crystalline resin such as polyethylene terephthalate, the particulate cut pieces are cooled with cooling water 42 at 23°C to 55°C after cutting the aromatic polyester resin extrudate, so that the crystallinity, bubble diameter, and thickness of the surface resin layer are suitable for producing an expansion molded product with excellent mechanical properties.
[0058] The bulk density of the aromatic polyester resin expanded particles is 0.05 g / cm from the viewpoint of improving the expansion power and the fusion power of the secondary expanded particles. 3 ~0.7g / cm 3 is preferred, and 0.07 g / cm 3 ~0.6g / cm 3 More preferably, 0.08 g / cm 3 ~0.5g / cm 3is particularly preferred. The bulk density of the expanded aromatic polyester resin particles can be adjusted by the resin pressure at the nozzle outlet 11 of the nozzle mold 1, the amount of the blowing agent, etc. The resin pressure at the nozzle outlet 11 of the nozzle mold 1 can be adjusted by the nozzle diameter, the extrusion amount, and the melt viscosity of the aromatic polyester resin.
[0059] The bulk density of the expanded aromatic polyester resin particles is measured in accordance with JIS K6911: 1995 "General testing method for thermosetting plastics." In detail, it is determined by the method described in the examples.
[0060] Although the aromatic polyester resin expanded particles have improved heat resistance of the expanded molded article when the crystallinity is high, the fusion strength of the secondary expanded particles is not increased, and as a result, it is difficult to improve the mechanical strength of the expanded molded article. For this reason, the crystallinity (A) at the particle center and the crystallinity (B) at the particle surface are both preferably 10% or less, more preferably 1 to 10%, and particularly preferably 2 to 8%.
[0061] The central portion and the surface portion of the expanded beads are determined as follows. The expanded bead is divided into approximately two equal parts at the center using a razor blade, and the portion of the exposed cross-section ranging from the center of the particle to 20% of the expanded bead in the radial direction is defined as the central portion, and the portion of the exposed cross-section ranging from the surface of the particle to 20% of the expanded bead in the radial direction is defined as the surface portion.
[0062] The crystallinity of the expanded beads is determined by the method described in JIS K7122:1987 and JIS K7122:2012, and more specifically, by the method described in the Examples.
[0063] The ratio (B / A) of the crystallinity (B) in the surface layer to the crystallinity (A) in the center of the expanded aromatic polyester resin particles is preferably 0.30 to 1.30, more preferably 0.35 to 1.25, and particularly preferably 0.40 to 1.20, from the viewpoint of improving the expandability or the fusion strength of the secondary expanded particles.
[0064] From the viewpoint of improving the expandability or the fusion strength of the secondary expanded particles, the expanded aromatic polyester resin particles preferably have a surface resin layer thickness of 5 μm to 40 μm, more preferably 7 μm to 37 μm. Here, the thickness of the resin layer on the surface of the expanded particles is determined from an image of the surface layer of a cross section of the expanded particle approximately divided into two at the center, taken with a scanning electron microscope at a magnification of 500 times, and in detail is determined by the method described in the Examples.
[0065] It is preferable that the average cell diameter (C) at the particle center of the expanded aromatic polyester resin particles and the average cell diameter (D) at the particle surface layer portion are both 50 μm to 300 μm from the viewpoint of improving the expandability or the fusion strength of the secondary expanded particles.
[0066] It is preferable that the bubble diameter of the surface layer of the expanded aromatic polyester resin particles is slightly smaller than that of the center, because the expansion is good and the fusion strength of the secondary expanded particles is high. Therefore, the ratio (D / C) of the average bubble diameter (D) of the surface layer to the average bubble diameter (C) of the center of the expanded beads is preferably 0.75 to 0.95, more preferably 0.80 to 0.95, and particularly preferably 0.80 to 0.90.
[0067] The aromatic polyester resin foamed particles of the present invention are filled into the cavity of a mold, heated, and expanded, and the secondary expanded particles obtained by expanding the aromatic polyester resin foamed particles are heat-fused together by their expansion pressure, thereby obtaining an in-mold foamed article having a desired shape and excellent mechanical properties. The heating medium for the aromatic polyester resin foamed particles filled in the mold is not particularly limited, and examples thereof include hot air, hot water, and the like in addition to steam.
[0068] The present invention also includes an expansion molded article of the expanded aromatic polyester resin beads of the present invention. This expansion molded article is obtained by in-mold expansion molding of the expanded aromatic polyester resin beads of the present invention.
[0069] The density of the aromatic polyester resin foam molded body is set to 0.05 g / cm3 from the viewpoints of light weight and mechanical strength. 3 ~0.7g / cm 3 is preferred, and 0.07 g / cm 3 ~0.6g / cm 3 More preferably, 0.08 g / cm 3 ~0.5g / cm 3 is particularly preferred.
[0070] Furthermore, the aromatic polyester resin foam particles may be impregnated with an inert gas immediately before the in-mold foaming to improve the foaming power of the aromatic polyester resin foam particles. By improving the foaming power of the aromatic polyester resin foam particles in this way, the thermal fusion between the aromatic polyester resin foam particles during the in-mold foaming is improved, and the obtained in-mold foamed article has even better mechanical strength. Examples of the inert gas include carbon dioxide, nitrogen, helium, and argon, and carbon dioxide is preferred.
[0071] As a method for impregnating the expanded aromatic polyester resin particles with an inert gas, for example, a method for impregnating the expanded aromatic polyester resin particles with an inert gas by placing the expanded aromatic polyester resin particles in an inert gas atmosphere having a pressure equal to or higher than normal pressure can be mentioned. In such a case, the expanded aromatic polyester resin particles may be impregnated with an inert gas before being filled into a mold, or the expanded aromatic polyester resin particles may be impregnated with an inert gas by placing the expanded aromatic polyester resin particles together with the mold in an inert gas atmosphere after being filled into the mold.
[0072] The temperature when the expanded aromatic polyester resin particles are impregnated with an inert gas is preferably from 5°C to 40°C, and more preferably from 10°C to 30°C.
[0073] The pressure when the expanded aromatic polyester resin particles are impregnated with an inert gas is preferably 0.2 to 2.0 MPa, more preferably 0.25 to 1.5 MPa. When the inert gas is carbon dioxide, the pressure is preferably 0.2 to 1.5 MPa, more preferably 0.25 to 1.2 MPa.
[0074] The time for impregnating the expanded aromatic polyester resin particles with the inert gas is preferably from 10 minutes to 72 hours, more preferably from 15 minutes to 64 hours, and particularly preferably from 20 minutes to 48 hours.
[0075] The expanded aromatic polyester resin particles impregnated with the inert gas are expanded (pre-expanded) by heating to, for example, 55° C. to 90° C. to produce pre-expanded particles.
[0076] A composite structural member can be produced by using a foamed molded body as a core material and laminating and integrating a skin material onto the surface of the foamed molded body. A composite structural member including a foamed molded body and a skin material laminated and integrated onto the surface of the foamed molded body can also be one aspect of the present invention. The thickness of the foamed molded body used as the core material of the composite structural member is preferably 1 mm to 40 mm in terms of strength, weight, and impact resistance.
[0077] The skin material is not particularly limited, and examples thereof include a fiber-reinforced synthetic resin sheet, a metal sheet, a synthetic resin sheet, etc. The skin material is preferably a fiber-reinforced synthetic resin because of its excellent mechanical strength and light weight.
[0078] The fiber-reinforced synthetic resin sheet is a sheet formed by bonding fibers together with a matrix resin. The fibers constituting the fiber-reinforced synthetic resin sheet are not particularly limited, and examples thereof include carbon fibers, glass fibers, aramid fibers, boron fibers, and metal fibers. As the fibers, carbon fibers, glass fibers, and aramid fibers are preferred, and carbon fibers are more preferred, because they have excellent mechanical strength and heat resistance.
[0079] The matrix resin constituting the fiber-reinforced synthetic resin includes thermosetting resin and thermoplastic resin. Examples of the thermosetting resin include epoxy resin, unsaturated polyester resin, and phenol resin. The thermosetting resin may be used alone or in combination of two or more. Examples of the thermoplastic resin include polyamide (nylon 6, nylon 66, etc.), polyolefin (polyethylene, polypropylene, etc.), polyphenylene sulfide, polyethylene terephthalate, polybutylene terephthalate, polycarbonate, polystyrene, ABS, and copolymers of acrylonitrile and styrene. The thermoplastic resin may be used alone or in combination of two or more.
[0080] The thickness of the fiber-reinforced synthetic resin sheet is preferably 0.2 mm to 2.0 mm in terms of strength, weight, and impact resistance.
[0081] The method for producing the composite structural member is not particularly limited. For example, the method may be a method in which a skin material is laminated onto the surface of a foamed molded body that serves as a core material using an adhesive, or a method generally used for molding a fiber-reinforced synthetic resin sheet. Examples of methods used in molding fiber-reinforced synthetic resin sheets include the autoclave method, the hand lay-up method, the spray-up method, the PCM (Prepreg Compression Molding) method, the RTM (Resin Transfer Molding) method, and the VaRTM (Vacuum assisted Resin Transfer Molding) method.
[0082] Such composite structural members are useful for applications such as automobile members, aircraft members, railroad vehicle members, building materials, etc. Examples of automobile members include door panels, door inners, bumpers, fenders, fender supports, engine covers, roof panels, trunk lids, floor panels, center tunnels, crash boxes, etc. For example, when a composite structural member is used for a door panel that has conventionally been made of steel plate, the door panel has substantially the same rigidity as a steel plate door panel, but the weight can be significantly reduced, resulting in a significant effect in reducing the weight of the automobile. EXAMPLES
[0083] Hereinafter, one embodiment of the present invention will be described in more detail with reference to examples, but the present invention is not limited to these. The methods for determining various physical properties in the examples are described below.
[0084] (Bulk density) The bulk density was measured in accordance with JIS K6911:1995 "General testing method for thermosetting plastics" using an apparent density measuring device in accordance with JIS K6911. Bulk density of foam particles (g / cm 3 ) = [mass of the measuring cylinder containing the sample (g) - mass of the measuring cylinder (g)] / [capacity of the measuring cylinder (cm 3 )〕
[0085] (Crystallization degree) The crystallinity was measured according to the methods described in JIS K7122:1987 and JIS K7122:2012. However, the sampling method and temperature conditions were as follows. Samples were taken from the surface and center of the expanded beads. The surface samples were taken from a portion that was approximately bisected at the center of the expanded beads using a razor blade, and was located within 20% of the area in the radial direction of the expanded beads from the surface of the expanded beads. Similarly, the center samples were taken from a portion that was approximately 20% of the area in the radial direction of the expanded beads from the center of the bisected expanded beads. 5.5±0.5mg of sample was packed into an aluminum measuring container so that there were no gaps at the bottom, and then an aluminum lid was placed on it. Differential scanning calorimetry was then performed using a Hitachi High-Tech Science DSC7000X, AS-3 differential scanning calorimeter. The sample was heated in the following steps under a nitrogen gas flow rate of 20mL / min to obtain a DSC curve. (Step 1) Hold at 30°C for 2 minutes. (Step 2) The temperature was raised from 30°C to 290°C at a rate of 10°C / min. Alumina was used as the reference material. The difference between the heat of fusion (J / g) calculated from the area of the melting peak and the heat of crystallization (J / g) calculated from the area of the crystallization peak was calculated. The ratio obtained by dividing this difference by the theoretical heat of fusion of 140.1 J / g for polyethylene terephthalate perfect crystal was taken as the degree of crystallization. The heat of fusion and the heat of crystallization were calculated using the analysis software attached to the device. Specifically, the heat of fusion was calculated from the straight line connecting the point where the DSC curve leaves the low-temperature baseline and the point where the DSC curve returns to the high-temperature baseline, and the part enclosed by the DSC curve. The heat of crystallization was calculated from the straight line connecting the point where the DSC curve leaves the low-temperature baseline and the point where the DSC curve returns to the high-temperature baseline, and the area enclosed by the DSC curve. In other words, the degree of crystallization was calculated from the following formula. Crystallinity (%) = (heat of fusion (J / g) - heat of crystallization (J / g)) / 140.1 (J / g) x 100
[0086] (crystallinity ratio) The crystallinity ratio was calculated by the following formula. Crystallinity ratio = Crystallinity of the surface layer of the expanded bead (%) / Crystallinity of the center of the expanded bead (%)
[0087] (average bubble diameter) The surface layer and the center of a cross section of an expanded bead roughly divided in two at the center were photographed at 100x magnification using a scanning electron microscope "SU1510" manufactured by Hitachi High-Technologies Corp. The surface layer was taken as the area within 20% of the expanded bead surface in the radial direction, and the center was taken as the area within 20% of the expanded bead surface in the radial direction. The captured microscopic images were arranged side by side on one A4 sheet of paper in landscape orientation and printed on A4 paper. For each image of the cross section of the printed foamed beads, three arbitrary straight lines (60 mm long) parallel to the vertical and horizontal directions were drawn. That is, for each of two microscopic images, six arbitrary straight lines were drawn in the vertical direction and six in the horizontal direction. The lines were drawn so that they would not come into contact with the bubbles only at their contact points as much as possible. The number of bubbles that the straight lines passed through was then counted. If a bubble came into contact with the line only at its contact point, this bubble was also included in the count. The number of bubbles counted for the six arbitrary straight lines in each of the vertical and horizontal directions was calculated as the number of bubbles in each direction. The average chord length t of the bubbles was calculated from the magnification of the image where the number of bubbles was counted and the number of bubbles using the following formula. Average chord length t(mm)=60 / (number of bubbles x image magnification) The image magnification was calculated by measuring the scale bar on the image to the nearest 1 / 100 mm using a Mitutoyo Digimatic Caliper and using the following formula: Image magnification = Scale bar actual value (mm) / Scale bar display value (mm) The bubble diameters in the vertical and horizontal directions were calculated using the following formula. Vertical or horizontal bubble diameter D(mm)=t / 0.616 Furthermore, the square root of the product of the air bubble diameter D in the vertical direction and the air bubble diameter D in the horizontal direction was defined as the air bubble diameter. Bubble diameter (μm) = 1000 x (D length x D width) 1 / 2 The above operation was carried out on the surface and center with an N number of 10, and the average value was taken as the average bubble diameter.
[0088] (Average bubble diameter ratio) The average cell diameter ratio was calculated by the following formula. Average bubble diameter ratio = Average bubble diameter at the surface of the expanded particle (μm) / Average bubble diameter at the center of the expanded particle (μm)
[0089] (Thickness of surface resin) The surface layer of a cross section roughly divided in two at the center of an expanded bead was photographed at 500x magnification using a Hitachi High-Technologies Corporation "SU1510" scanning electron microscope. At any position on the surface of the expanded bead in the microscope image, five straight lines perpendicular to the tangent were drawn in the radial direction of the expanded bead, and the distance from the surface to the first air bubble that came into contact with each straight line was measured. In other words, five such distances were measured for one cross-sectional image. The above procedure was carried out with an N number of 10, and the average value was taken as the thickness (μm) of the surface resin.
[0090] (Moldability evaluation) The moldability was evaluated according to the following criteria. ○: The foam particles were thermally fused together, firmly bonded, and integrated. ×: The expanded particles were not bonded to each other and easily fell off.
[0091] (Density of foamed molded body) The mass (a) and volume (b) of a rectangular parallelepiped test piece (e.g., 75 mm x 300 mm x 30 mm) cut out from a foamed molded product (dried at 55°C for 20 hours or more after molding) are measured to have three or more significant figures, and the density of the foamed molded product (g / cm3) is calculated using the formula (a) / (b). 3 ) was sought.
[0092] (Bending test: maximum bending strength and bending modulus) The maximum bending strength and bending modulus were measured in accordance with JIS K7221-1:2006. That is, the maximum bending strength was measured using a universal testing machine "Autograph AG-X plus 100kN" manufactured by Shimadzu Corporation, and a universal testing machine data processing software "TRAPEZIUM X" manufactured by Shimadzu Corporation. A test piece was cut out from a foam molded body (dried at 55°C for 20 hours or more after molding) with a width of 25 mm, length of 130 mm, and thickness of 20 mm. The number of test pieces was 5. The test pieces were conditioned for 16 hours under the standard atmosphere of JIS K 7100:1999 symbol "23 / 50" (temperature 23°C, relative humidity 50%), class 2, and then used for measurement under the same standard atmosphere. The test speed was 10 mm / min. The radius of the tip of the pressure wedge and the fulcrum was 5R, and the distance between the fulcrums was 100 mm. From the obtained graph, the load region where the slope was maximum was set, and the apparent flexural modulus was calculated by the universal testing machine data processing. The intersection point of the straight line of this elastic modulus and the stroke was set as the origin of elongation, and the corresponding maximum flexural strength was automatically calculated.
[0093] (Compression test: 5% compressive strength and compressive modulus) The 5% compression strength and compression modulus were measured in accordance with JIS K6767:1999. That is, the 5% compression strength was measured using a Shimadzu Corporation "Autograph AG-X plus 100kN" universal testing machine and Shimadzu Corporation "TRAPEZIUM X" universal testing machine data processing software. The test piece size was 50mm x 50mm x thickness 25mm, and the number of test pieces was 3. The test pieces were conditioned for 16 hours under the standard atmosphere of JIS K 7100:1999 symbol "23 / 50" (temperature 23°C, relative humidity 50%), class 2, and then used for measurement under the same standard atmosphere. The compression speed was 2.5mm / min. From the obtained graph, the load region with the maximum slope was set, and the compression modulus was calculated using the universal testing machine data processing software. The intersection point of the straight line of this elastic modulus and the stroke was set as the origin of elongation, and the compression strength at 5% compression was automatically calculated.
[0094] (Evaluation of mechanical properties of molded products) The mechanical properties of the molded product were evaluated according to the following criteria. ○: Maximum bending strength is 1.20 MPa or more, and 5% compressive strength is 0.70 MPa or more. ×: Maximum bending strength is less than 1.20 MPa, or 5% compressive strength is less than 0.70 MPa.
[0095] Example 1 (Expanded particle manufacturing process) Expanded beads were produced using the production apparatus shown in Figures 1 and 2. First, plant-derived polyethylene terephthalate (intrinsic viscosity: 0.80, density: 1400 kg / m 3 A polyethylene terephthalate composition containing 100 parts by mass of a polyethylene terephthalate copolymer having a melting point of 247.2°C, a glass transition temperature of 78.7°C, a mass average molecular weight of 74,000, and a plant content of 30%), 1.8 parts by mass of a master batch obtained by incorporating talc into polyethylene terephthalate (polyethylene terephthalate content: 60% by weight, talc content: 40% by weight, intrinsic viscosity of polyethylene terephthalate: 0.82), and 0.22 parts by mass of pyromellitic anhydride was supplied to a single-screw extruder having a diameter of 65 mm and an L / D ratio of 34, and melt-kneaded at 300°C. Next, butane consisting of 35% by weight of isobutane and 65% by weight of normal butane was pressurized into the molten polyethylene terephthalate composition from the middle of the extruder in an amount of 1.15 parts by weight per 100 parts by weight of polyethylene terephthalate as a foaming agent, and uniformly dispersed in the polyethylene terephthalate.
[0096] Thereafter, the molten polyethylene terephthalate composition was cooled to 280°C at the front end of the extruder, and then the polyethylene terephthalate composition was extruded and foamed from each nozzle of the multi-nozzle die 1 attached to the front end of the extruder. The extrusion rate of the polyethylene terephthalate composition was 30 kg / h. The multi-nozzle mold 1 had 20 nozzles with an outlet portion 11 having a diameter of 1 mm, and all of the nozzle outlet portions 11 were arranged at equal intervals on an imaginary circle A with a diameter of 139.5 mm, which was assumed to be on the front end face 1a of the multi-nozzle mold 1. Two rotary blades 5 were integrally provided on the outer peripheral surface of the rear end of the rotary shaft 2 with a phase difference of 180° in the circumferential direction of the rotary shaft 2, and each rotary blade 5 was configured to move on an imaginary circle A while always in contact with the front end surface 1a of the multi-nozzle mold 1. The cooling member 4 further includes a cooling drum 41, which is made up of a front part 41a having a circular shape at the front and a cylindrical peripheral wall part 41b extending rearward from the outer periphery of the front part 41a and having an inner diameter of 320 mm. Cooling water 42 at 25°C was supplied into the cooling drum 41 through a supply pipe 41d and a supply port 41c of the cooling drum 41. The internal volume of the cooling drum 41 was 17684 cm3. 3 It was.
[0097] The cooling water 42 advances forward in a spiral manner along the inner surface of the peripheral wall portion 41b of the cooling drum 41 due to the centrifugal force associated with the flow speed when it is supplied from the supply pipe 41d to the inner surface of the peripheral wall portion 41b of the cooling drum 41. As the cooling water 42 advances along the inner surface of the peripheral wall portion 41b, the cooling water 42 gradually spreads in a direction perpendicular to the direction of advancement. As a result, the inner surface of the peripheral wall portion 41b forward of the supply port 41c of the cooling drum 41 is completely covered with the cooling water 42. The rotary blade 5 disposed on the front end surface 1a of the multi-nozzle die 1 was rotated at a rotational speed of 3200 rpm, and the polyethylene terephthalate extrudate extruded and foamed from the outlet 11 of each nozzle of the multi-nozzle die 1 was cut by the rotary blade 5 to produce approximately spherical particulate cut products. The polyethylene terephthalate extrudate consisted of an unfoamed portion immediately after being extruded from the nozzle of the multi-nozzle die 1 and a foamed portion in the process of foaming that was continuous with the unfoamed portion. The polyethylene terephthalate extrudate was cut at the open end of the outlet 11 of the nozzle, and the cutting of the polyethylene terephthalate extrudate was carried out in the unfoamed portion.
[0098] In the production of the polyethylene terephthalate expanded particles, the rotating shaft 2 was not attached to the multi-nozzle die 1 and the cooling member 4 was withdrawn from the multi-nozzle die 1. In this state, a polyethylene terephthalate extrudate was extruded and foamed from the extruder, and it was confirmed that the polyethylene terephthalate extrudate consisted of an unfoamed portion immediately after being extruded from the nozzle of the multi-nozzle die 1 and a foamed portion in the process of foaming that was continuous with the unfoamed portion. Next, the rotating shaft 2 was attached to the multi-nozzle die 1 and the cooling member 4 was disposed at a predetermined position, and then the rotating shaft 2 was rotated to cut the polyethylene terephthalate extrudate with the rotating blade 5 at the open end of the outlet portion 11 of the nozzle to produce particulate cut products. The granular cut pieces are thrown outward or forward by the cutting stress of the rotating blade 5 and collide with the cooling water 42 flowing along the inner surface of the cooling drum 41 of the cooling member 4 from a direction oblique to the surface of the cooling water 42 so as to follow the cooling water 42 from the upstream side to the downstream side of the flow of the cooling water 42, and the granular cut pieces enter the cooling water 42 and are immediately cooled, thereby producing polyethylene terephthalate foam particles for in-mold foam molding. The obtained polyethylene terephthalate foamed particles were discharged together with cooling water 42 through the discharge port 41e of the cooling drum 41, and then separated from the cooling water 42 by a dehydrator.
[0099] (molding process) The resulting polyethylene terephthalate foam particles were left at 23° C. and atmospheric pressure for 30 days immediately after production, then filled into a 30 mm×300 mm×400 mm molding die, heated with 0.05 MPa water vapor for 180 seconds and with 0.10 MPa water vapor for 30 seconds, and then cooled until the maximum surface pressure of the foamed molded product decreased to 0.01 MPa, thereby obtaining a foamed molded product.
[0100] Example 2 Polyethylene terephthalate (intrinsic viscosity: 0.82, density: 1400 kg / m 3 , melting point: 248.0°C, glass transition temperature: 78.7°C, mass average molecular weight: 72,000) 95% by weight, polyethylene naphthalate (density: 1330 kg / m3 The procedure of Example 1 was repeated except that a thermoplastic polyester resin composition containing 100 parts by mass of a thermoplastic polyester resin containing 5% by weight of a polyethylene terephthalate copolymer (polyethylene terephthalate content: 60% by weight, talc content: 40% by weight, intrinsic viscosity of polyethylene terephthalate: 0.82) was used, as well as 0.24 parts by mass of pyromellitic anhydride.
[0101] Example 3 Recycled polyethylene terephthalate (intrinsic viscosity: 0.80, density: 1400 kg / m 3 , melting point: 248.3°C, glass transition temperature: 78.9°C, mass average molecular weight: 78,000) 95% by weight, polyethylene naphthalate (density: 1330 kg / m 3 The procedure of Example 1 was repeated except that a thermoplastic polyester resin composition was used that contained 100 parts by mass of a thermoplastic polyester resin containing 5% by weight of polyethylene terephthalate (polyethylene terephthalate content: 60% by weight, talc content: 40% by weight, intrinsic viscosity of polyethylene terephthalate: 0.82), 0.5 parts by mass of a masterbatch obtained by incorporating talc in polyethylene terephthalate (polyethylene terephthalate content: 70% by weight, carbon black content: 30% by weight, intrinsic viscosity of polyethylene terephthalate: 0.82), and 0.26 parts by mass of pyromellitic anhydride.
[0102] Example 4 (Expanded particle manufacturing process) Expanded beads were obtained in the same manner as in Example 1, except that carbon dioxide was injected into the molten polyethylene terephthalate composition midway through the extruder in an amount of 0.3 parts by mass per 100 parts by mass of polyethylene terephthalate, and uniformly dispersed in the polyethylene terephthalate.
[0103] (molding process) The resulting polyethylene terephthalate foam particles were left at 23°C and atmospheric pressure for 1 day immediately after production, then sealed in a pressure vessel, and compressed air was pumped into the pressure vessel up to 0.5MPa (gauge pressure). The temperature inside the pressure vessel was kept at 20°C, and the pressure curing was carried out for 24 hours. After removal, the particles were filled into a molding die of 30mm x 300mm x 400mm, heated with steam at 0.05MPa for 180 seconds and with steam at 0.10MPa for 30 seconds, and then cooled until the maximum surface pressure of the foamed molded product was reduced to 0.01MPa, to obtain a foamed molded product.
[0104] Example 5 Expanded beads and expanded molded articles were obtained in the same manner as in Example 1, except that the temperature of the cooling water was set to 45°C.
[0105] Comparative Example 1 Except for changing the temperature of the cooling water to 60°C, the same procedure as in Example 1 was carried out to obtain expanded beads and an expanded molded article.
[0106] Comparative Example 2 Except for changing the temperature of the cooling water to 10°C, the same procedure as in Example 1 was carried out to obtain expanded beads and an expanded molded article.
[0107] Comparative Example 3 Except for changing the temperature of the cooling water to 20°C, the same procedure as in Example 1 was carried out to obtain expanded beads and an expanded molded article.
[0108] Comparative Example 4 (Expanded particle manufacturing process) An underwater cutting type granulator was used, which had a diverter valve, a die with five die holes with a diameter of 2.0 mm and a land length of 2.0 mm, and the diverter valve was set so that the molten polyethylene terephthalate resin supplied from the extruder to the die through the resin flow path on the outside discharge side of the diverter valve was discharged outside the machine. In addition, an underwater cutting type granulator equipped with a single screw extruder with a diameter of 65 mm and an L / D ratio of 34 was used as the extruder to which the die was attached. First, the temperature was adjusted by a heater so that the temperature of the die hole of the die was 300° C., and the temperature of the extruder was also adjusted. Specifically, the upstream extruder was set at a higher temperature than the downstream extruder to increase the solubility of the foaming agent, and the extruder temperature was set so that the molten resin was finally supplied to the die at a resin temperature of 290° C. The same polyethylene terephthalate composition as used in Example 1 was fed to this extruder at a rate of 30 kg / h and melt-kneaded. Thereafter, butane consisting of 35% by weight of isobutane and 65% by weight of normal butane as a foaming agent was pressure-fed into the extruder in an amount of 3.0 parts by weight per 100 parts by weight of polyethylene terephthalate, and the molten polyethylene terephthalate composition was melt-kneaded and supplied to the die, and then discharged outside the machine through the resin flow path of the diverter valve.
[0109] When the temperature of the extruder, the pressure of the foaming agent, etc. became stable, a cutter was operated in the chamber attached in front of the die, the flow path of the molten polyethylene terephthalate composition was switched by the diverter valve, and 12 m of circulating water at 80°C and a water pressure of 0.3 MPa was introduced into the chamber. 3 / h and granulation was started. The molten polyethylene terephthalate extrudate extruded while foaming in the circulating water was cut with a rotary blade to produce foamed particles. The cut particles were foamed in the circulating water to produce polyethylene terephthalate foamed particles. The circulating water containing the foamed particles was conveyed from the chamber to a centrifugal dryer, where water was removed from the foamed particles.
[0110] (molding process) The resulting polyethylene terephthalate foam particles were left at 23° C. and atmospheric pressure for 30 days immediately after production, then filled into a 30 mm×300 mm×400 mm molding die and heated with 0.05 MPa water vapor for 180 seconds and with 0.10 MPa water vapor for 30 seconds, but molding was not possible.
[0111] Comparative Example 5 (Expanded particle manufacturing process) Expanded beads were obtained in the same manner as in Comparative Example 4, except that butane consisting of 35% by weight of isobutane and 65% by weight of normal butane was used as a foaming agent, and an amount of 2.2 parts by weight per 100 parts by weight of polyethylene terephthalate was pressurized into the molten polyethylene terephthalate composition to uniformly disperse the butane in the polyethylene terephthalate. (molding process) The molding step was carried out in the same manner as in Comparative Example 4, but molding was not possible.
[0112] Scanning electron microscope (SEM) photographs of the cross sections of the expanded beads obtained in the above Examples and Comparative Examples are shown in Figures 4 to 7. In addition, physical properties measured for the expanded beads and foamed molded articles obtained in the above Examples and Comparative Examples are shown in Tables 1 and 2.
[0113] [Table 1]
[0114] [Table 2]
[0115] It was presumed that the secondary foaming property was poor and the mechanical properties of the foamed molded article were poor due to the large crystallinity ratio of the expanded beads in Comparative Example 1. It was also presumed that the secondary foaming property was poor and the mechanical properties of the foamed molded article were poor due to the small crystallinity ratio of the expanded beads in Comparative Examples 2 and 3. It was also presumed that the secondary foaming property was very poor and foam molding was not possible due to the large crystallinity in the center and surface layer of the expanded beads in Comparative Examples 4 and 5, and the large crystallinity ratio.
[0116] Furthermore, the resin layer on the surface of the expanded beads in Comparative Example 1 was thin (cross-sectional photograph). This was presumably due to the high cooling water temperature of 60°C. The resin layers on the surface of the expanded beads in Comparative Examples 2 and 3 were thick (cross-sectional photograph). This was presumably due to the low cooling water temperatures of 10°C and 20°C, respectively. The resin layers on the surface of the expanded beads in Comparative Examples 4 and 5 were thick (cross-sectional photograph). This was presumably due to the rapid cooling of the expanded beads in the underwater cutting method.
[0117] On the other hand, the foamed molded articles obtained from the foamed beads of Examples 1 to 5 showed superior physical properties to those of the comparative examples in both bending tests and compression tests. This is presumably because the crystallinity of the center and surface layer of the foamed beads could be kept within an appropriate range by setting the cooling water temperature within an appropriate range in the watering hot cut method, and / or the thickness of the surface resin layer was appropriately adjusted.
[0118] In Examples 1 to 3, the expanded beads and expanded molded articles of the present invention were obtained even when the aromatic polyester resin was a plant-derived product, a petroleum-derived product, or a recycled product. In Example 4, the expanded beads and expanded molded articles of the present invention were obtained even when the blowing agent was an inorganic gas. [Explanation of symbols]
[0119] 1 Nozzle mold 2 Rotation Axis 3 Driving member 4 Cooling material 41 Cooling drum 42 Cooling water 5 Rotary blade P Aromatic polyester resin foam particles for in-mold foam molding
Claims
1. The expanded aromatic polyester resin particles have a crystallinity (A) in the particle center and a crystallinity (B) in the particle surface layer, each of which is 1 to 10%, and the ratio of the crystallinity in the surface layer to the crystallinity in the particle center (B / A) is 0.30 to 1.
40.
2. 2. The expanded aromatic polyester resin particles according to claim 1, wherein the thickness of the resin layer on the particle surface is 5 μm to 40 μm.
3. 3. The expanded aromatic polyester resin particles according to claim 1, wherein the average cell diameter (C) in the particle center and the average cell diameter (D) in the particle surface layer are both 50 μm to 300 μm, and the ratio (D / C) of the average cell diameter in the surface layer to the average cell diameter in the particle center is 0.75 to 0.
95.
4. 4. The expanded aromatic polyester resin particle according to claim 1, wherein the ratio (B / A) of the crystallinity in the surface layer to the crystallinity in the center of the particle is 0.30 to 1.
30.
5. 5. An expansion molded product of the expanded aromatic polyester resin particles according to claim 1.
6. Density is 0.05 g / cm 3 ~0.7g / cm 3 The foamed molded article according to claim 5,
7. An automobile component comprising the foamed molded article according to claim 5 or 6.
8. 5. The method for producing expanded aromatic polyester resin beads according to claim 1, comprising the steps of: supplying an aromatic polyester resin to an extruder and melt-kneading the resin in the presence of a foaming agent; extruding and foaming the melt-kneaded aromatic polyester resin under gaseous conditions through a nozzle die attached to the front end of the extruder while cutting the resin to produce granular cut pieces; and cooling the granular cut pieces with cooling water, wherein the temperature of the cooling water is 23° C. to 55° C.
Citation Information
Patent Citations
Surgical metatarsal compression nail
EP2564799A1
Manufacture of film package with plug
JP1984074010A
Thermoplastic polyester resin foamed particles, method for producing the same, foam-molded product, and composite molded product
JP2014043528A
Manufacturing method of fiber-reinforced composite foam and thermoplastic resin foam particles usable for the method
JP2017043011A
Polyamide resin foamed particles and method for producing same
WO2020049802A1