Method for manufacturing cured products

An organopolysiloxane with a specific structural unit and amine-based catalyst addresses the hardness-flexibility trade-off in silicone resins, offering rapid curing and hydrophobic properties for coatings.

JP7948302B2Active Publication Date: 2026-11-11SHIN ETSU CHEMICAL CO LTD
View PDF 8 Cites 0 Cited by

Patent Information

Application Number
JP2024221246
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2024-12-18
Publication Date
2026-11-11
Estimated Expiration
2041-04-16

AI Technical Summary

Technical Problem

Silicone resins and silicone alkoxy oligomers face challenges in achieving both hardness and flexibility due to their high crosslink density, leading to cracking under stress, and require additional components that compromise curability and environmental safety.

Method used

An organopolysiloxane with an alkoxy-methylene-silicon bond, incorporating D units via a silethylene structure, and using an amine-based catalyst for rapid curing, providing a cured product with enhanced hardness, flexibility, and hydrophobic properties.

Benefits of technology

The organopolysiloxane achieves rapid curing, high hardness, flexibility, and excellent hydrophobicity, suitable for coating applications without the drawbacks of traditional methods.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007948302000001
    Figure 0007948302000001
  • Figure 0007948302000002
    Figure 0007948302000002
  • Figure 0007948302000003
    Figure 0007948302000003
Patent Text Reader

Abstract

To provide a method of producing a cured product having both hardness and bending resistance, and excellent in decontamination characteristics such as hydrophobicity, and slip drop property of water drops.SOLUTION: A method of producing a cured product includes curing a curable composition including: (A) an organopolysiloxane having a constitutional unit expressed by the following general formula (1), a constitutional unit expressed by the following general formula (2), and a group bonded directly to a silicon atom and expressed by the following general formula (3); and (B) a curing catalyst. R1 expresses an alkyl group, or an aryl group. R2 expresses each independently an alkyl group or aryl group, n is each independently 2 or 3, and m is an integer of 5-100. R3 expresses a hydrogen atom, an alkyl group, or an aryl group.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical Field]

[0001] This invention relates to a method for manufacturing a cured product. [Background technology]

[0002] Silicone resins are currently widely used in various fields due to their excellent properties such as water repellency, heat resistance, weather resistance, cold resistance, electrical insulation, chemical resistance, and safety for the human body. In particular, SiO 4 / 2 Units (Q units) and RSiO 3 / 2 Organopolysiloxanes, which have a three-dimensional cross-linked structure with units (T units) (where R is an organic group such as an alkyl group or phenyl group) as the main component, are called silicone resins or silicone alkoxy oligomers, and are widely used in paints, coatings, and binders due to their curing properties.

[0003] In particular, liquid silicone alkoxy oligomers with alkoxysilyl groups as crosslinking groups are used as the main component of solvent-free paints that do not contain flammable organic solvents harmful to the human body (Non-Patent Literature 1). Furthermore, since these alkoxysilyl groups undergo hydrolysis and dehydration condensation crosslinking reactions at room temperature due to moisture in the air, silicone alkoxy oligomers containing alkoxysilyl groups can form a siloxane network at room temperature by incorporating a curing catalyst. Such polysiloxane cured films have excellent heat resistance and weather resistance, and are used in a wide range of fields, from outdoor buildings to electronic components. Furthermore, as mentioned above, silicone alkoxy oligomers undergo a curing reaction even at room temperature, but the reaction can be accelerated by heating. Depending on the application, a heat curing process can be appropriately introduced, making it a technology with excellent coating adaptability.

[0004] However, such silicone resins and silicone alkoxy oligomers have the advantages of good curability and high surface hardness due to their three-dimensional crosslinked structure, but on the other hand, due to their high crosslink density, they lack flexibility and bending resistance, and have the problem that cracks occur in the coating film over time after film formation or when external stress is applied. In order to improve this flexibility and bending resistance, a method is generally adopted in which diorganosiloxane (R2SiO 2 / 2 ) units (D units) are incorporated by, for example, using diorganoxyalkoxysilane in combination during the synthesis of silicone resins or silicone alkoxy oligomers via hydrolytic condensation. However, in this case, since the D units are randomly incorporated into the structure, it is necessary to add a large amount of D units to impart flexibility, and there is a problem that the excellent curability and surface hardness, which are the advantages of silicone resins, are reduced.

[0005] In addition, a method of adding a silicone oil whose molecular terminals are blocked with TEOS (Si(OCH2CH3)4) has also been proposed (Non-Patent Document 1), but it has poor compatibility with silicone resins and silicone alkoxy oligomers, and causes clouding and cissing of the coating film.

[0006] As another method for introducing D units into silicone alkoxy oligomers, there is a method of chemically bonding a hydrosilyl group and an alkyl olefin using a platinum catalyst or the like. This reaction is generally called a hydrosilylation reaction, and it is known that by using this reaction, an alkoxysilyl group can be introduced into a linear silicone via a silethylene structure (Patent Documents 1 and 2).

[0007] Patent Document 1 discloses an organopolysiloxane that is obtained by subjecting a side-chain methyl / phenyl type silicone oil compound containing hydrosilyl groups and composed of a D-unit chain structure, and a silicone alkoxy oligomer compound having both olefin and alkoxysilyl groups in its side chains to a hydrosilylation reaction, and contains both a silicone alkoxy oligomer structure having alkoxysilyl groups in one molecule and a structure derived from the side-chain methyl / phenyl type silicone oil structure.

[0008] Since the organopolysiloxane of Patent Document 1 has a relatively long-chain, high-molecular-weight side-chain methyl / phenyl type silicone oil structure, it exerts an effect when added as a crack resistance imparting agent, but when cured alone, its hardness is insufficient, making it difficult to use alone in applications such as paints and coating agents.

[0009] In addition, the technique of Patent Document 2 is a technique that emphasizes the purpose of improving the feel with linear silicones such as hair treatment agents, and does not mention its application as a flexible coating material.

[0010] In the silicone alkoxy oligomer into which D units are introduced by hydrosilylation as described above, since the D units are locally introduced compared to the random hydrolysis condensation method described earlier, the properties of diorganopolysiloxane are easily exhibited, while the decrease in hydrolyzability of the alkoxysilyl moiety similarly occurs, and improvement in reactivity (moisture curability) is required.

[0011] In addition, in order to ensure sufficient reactivity (moisture curability) at room temperature, the addition of a catalyst such as an organometallic compound is generally indispensable, and the addition of an organotin compound is particularly effective. However, organotin compounds commonly used as catalysts have concerns over toxicity to the human body and the environment, and environmental regulations have become stricter in recent years, so their use has been avoided. Furthermore, when organometallic catalysts such as organotin compounds are used in de-alcoholized, room-temperature curable compositions, the generated alcohol can cleave (cracking) the siloxane bonds in the main chain, leading to problems such as decreased curability and increased viscosity over time, resulting in poor storage stability. [Prior art documents] [Patent Documents]

[0012] [Patent Document 1] Japanese Patent Application Publication No. 6-271650 [Patent Document 2] International Publication No. 2004 / 091562 [Non-patent literature]

[0013] [Non-Patent Document 1] Polymeric Materia1s Science and Engineering,1998,Vol.79,192 [Overview of the project] [Problems that the invention aims to solve]

[0014] This invention has been made in view of the above circumstances, and aims to provide a method for producing a cured product that achieves both hardness and flexibility, and further possesses excellent contamination removal properties such as hydrophobicity and water droplet sliding properties. [Means for solving the problem]

[0015] As a result of diligent research to solve the above problems, the present inventors have found that an organopolysiloxane having an alkoxy-methylene-silicon bond as a specific structural unit in one molecule, and having an alkoxysilyl group and / or a silanol group, and further having a D unit introduced as a block segment via a silethylene bond, exhibits excellent rapid curing properties even when an amine-based compound is used as a curing catalyst instead of an organotin compound, and provides a cured product that satisfies hardness, flexural resistance, and hydrophobic / hydrophobic properties at a high level. Furthermore, they have found that a composition containing this compound is suitable as a curable composition for forming materials such as coating agents, and have completed the present invention.

[0016] In other words, the present invention is 1. A method for curing a curable composition containing (A) an organopolysiloxane having a constituent unit represented by the following general formula (1), a constituent unit represented by the following general formula (2), and a group represented by the following general formula (3) that is directly bonded to a silicon atom, and (B) a curing catalyst, [ka] (In the formula, R 1 This represents an unsubstituted or substituted alkyl group with 1 to 12 carbon atoms, or an unsubstituted or substituted aryl group with 6 to 10 carbon atoms. [ka] (In the formula, R 2 Each of these independently represents an unsubstituted or substituted alkyl group with 1 to 12 carbon atoms, or an unsubstituted or substituted aryl group with 6 to 10 carbon atoms, where n is independently 2 or 3, and m is an integer between 5 and 100. [ka] (In the formula, R 3 (This represents a hydrogen atom, an unsubstituted or substituted alkyl group with 1 to 10 carbon atoms, or an unsubstituted or substituted aryl group with 6 to 10 carbon atoms.) 2. The method for producing a cured product according to 1, comprising applying the curable composition to a surface of a solid substrate and then curing the applied composition, 3. The method for producing a cured product according to 1 or 2, wherein the average structure of the organopolysiloxane is represented by the following formula (4), [Chemical Formula] (wherein R 1 , R 2 , R 3 , n and m each represent the same meaning as defined above, R 4 , R 5 and R 6 each independently represent a monovalent organic group, and a, b, c, d, e, f and g represent numbers satisfying a>0, b>0, c≧0, d≧0, e≧0, f≧0, and g>0.) 4. The method for producing a cured product according to 3, wherein the average structure of the organopolysiloxane is represented by the following formula (5), [Chemical Formula] (wherein R 1 , R 2 , R 3 , R 4 , n, m, a, b and g each represent the same meaning as defined above, and d represents a number satisfying d>0.) 5. The method for producing a cured product according to any one of 1 to 4, wherein the (B) curing catalyst is an amine-based compound is provided. [Advantageous Effects of Invention]

[0017] The organopolysiloxane of the present invention has an alkoxy-methylene-silicon bond as a specific structural unit in one molecule, dimethylsiloxy units (D units) are introduced into the polymer as a polydimethylsiloxy structure via a silethylene structure, and the organopolysiloxane has an alkoxysilyl group and / or a silanol group, so that it is excellent in flexibility as compared with conventional silicone resins and silicone alkoxy oligomers, and is also excellent in surface antifouling properties such as hydrophobicity and water-sliding property. Furthermore, the organopolysiloxane of the present invention also exhibits excellent rapid curing properties even when an amine-based compound is used as a curing catalyst instead of an organotin compound, and provides a cured product that achieves both hardness and flexibility. Compositions containing organopolysiloxanes having such properties can be suitably used as curable compositions for forming materials such as coating agents. [Modes for carrying out the invention]

[0018] The present invention will be described in detail below. The organopolysiloxane according to the present invention has a constituent unit represented by the following general formula (1), a constituent unit represented by the following general formula (2), and a group represented by the following general formula (3) that is directly bonded to a silicon atom.

[0019] [ka]

[0020] Here, R 1 This represents an unsubstituted or substituted alkyl group having 1 to 12 carbon atoms, preferably 1 to 3 carbon atoms, or an unsubstituted or substituted aryl group having 6 to 10 carbon atoms. R 1 The alkyl group having 1 to 12 carbon atoms may be linear, cyclic, or branched, but linear or branched alkyl groups are preferred, and linear alkyl groups are more preferred. Specific examples include methyl, ethyl, n-propyl, n-butyl, s-butyl, t-butyl, n-pentyl, n-hexyl, n-heptyl, n-octyl, n-nonyl, n-decyl, n-undecyl, and n-dodecyl groups, but methyl, ethyl, and t-butyl groups are preferred, methyl and ethyl groups are more preferred, and methyl groups are even more preferred. Furthermore, specific examples of aryl groups having 6 to 10 carbon atoms include phenyl and naphthyl groups, but the phenyl group is preferred. In particular, from the viewpoint of curability and hardness, R 1A alkyl group having 1 to 3 carbon atoms is preferred.

[0021] The above R 2 This represents an unsubstituted or substituted alkyl group having 1 to 12 carbon atoms, preferably 1 to 3 carbon atoms, or an unsubstituted or substituted aryl group having 6 to 10 carbon atoms. R 2 The alkyl group having 1 to 12 carbon atoms may be linear, cyclic, or branched, but linear or cyclic alkyl groups are preferred, and linear alkyl groups are more preferred. Specific examples include methyl, ethyl, n-propyl, n-butyl, s-butyl, t-butyl, n-pentyl, n-cyclopentyl, n-hexyl, n-cyclohexyl, n-heptyl, n-octyl, n-nonyl, n-decyl, n-undecyl, and n-dodecyl groups, but methyl and ethyl groups are preferred, and methyl groups are more preferred. Specific examples of aryl groups having 6 to 10 carbon atoms include phenyl and naphthyl groups, but the phenyl group is preferred. In particular, from the viewpoint of imparting flexibility, hydrophobicity, and water-repellent properties, R 2 A alkyl group having 1 to 3 carbon atoms is preferred.

[0022] The above n corresponds to an introduction unit into the siloxane resin or oligomer main structure, and can be 2 or 3, but 2 is preferred. The above m represents the number of units in the dimethylpolysiloxane chain, and can range from 5 to 100, but is preferably 10 to 90, and more preferably 20 to 60. If m is greater than 100, problems arise such as poor reactivity with the vinylsiloxane portion of the main chain in the hydrosilylation reaction described later.

[0023] The above R 3 This represents a hydrogen atom, an unsubstituted or substituted alkyl group having 1 to 10 carbon atoms, or an unsubstituted or substituted aryl group having 6 to 10 carbon atoms. R 3The alkyl group having 1 to 10 carbon atoms may be linear, cyclic, or branched, but linear alkyl groups are more preferred. Specific examples include methyl, ethyl, n-propyl, n-butyl, n-pentyl, n-hexyl, n-heptyl, n-octyl, n-nonyl, and n-decyl groups, with methyl, ethyl, n-propyl, n-hexyl, and n-octyl groups being preferred, methyl and ethyl groups being more preferred, and methyl groups being even more preferred. Specific examples of aryl groups having 6 to 10 carbon atoms include phenyl and naphthyl groups, but the phenyl group is preferred. In particular, from the standpoint of curability, R 3 The hydrogen atom or an alkyl group having 1 to 3 carbon atoms is preferred, and a hydrogen atom, a methyl group, or an ethyl group is more preferred.

[0024] Note that the above R 1 , R 2 and R 3 Some or all of the hydrogen atoms of the alkyl or aryl group may be substituted with halogen atoms such as F, Cl, or Br, or other substituents such as cyano groups. Specific examples of such groups include halogen-substituted alkyl groups such as 3,3,3-trifluoropropyl group, and cyano-substituted alkyl groups such as 2-cyanoethyl group.

[0025] The organopolysiloxane of the present invention is not particularly limited as long as it has a constituent unit represented by the above general formula (1), a constituent unit represented by the above general formula (2), and a group represented by the above general formula (3) directly bonded to a silicon atom, and may have a linear structure, a branched structure, or a cross-linked structure consisting of an organopolysiloxane skeleton.

[0026] More specifically, the organopolysiloxane of the present invention is preferably one whose average structure is represented by the following formula (4), and by using such an organopolysiloxane, even better rapid curing properties, hardness, flexibility, hydrophobicity, and water-repellent properties can be achieved.

[0027] [ka] (In the formula, R 1 , R 2 , R 3 ,n and m have the same meaning as above.

[0028] Here, R 4 , R 5 and R 6 Each of these independently represents a monovalent organic group. The monovalent organic group mentioned above is not particularly limited; for example, R in the general formula (1) above. 1 Examples include alkyl groups with 1 to 12 carbon atoms and aryl groups with 6 to 10 carbon atoms, as exemplified above. Furthermore, some or all of the hydrogen atoms of these alkyl and aryl groups may be substituted with substituents. Examples of such substituents include halogen atoms, alkenyl groups such as vinyl groups, glycidyl epoxy groups, alicyclic epoxy groups, thiirane groups, (meth)acryloyloxy groups, mercapto groups, iso(thio)cyanate groups, succinic anhydride groups, amino groups, ethylenediamino groups, perfluoroalkyl groups, polyether groups such as polyoxyethylene groups, and perfluoropolyether groups.

[0029] Also, R 4 , R 5 and R 6 The group may be two or more different monovalent organic groups, in which case the ratio of the two or more different monovalent organic groups is arbitrary and not particularly limited as long as the sum of the ratios of the two or more different monovalent organic groups equals 1. For example, R 4 For example, if the alkyl group is 0.5 and the aryl group is 0.5, or R 5 It is possible to arbitrarily select from the various monovalent organic groups mentioned above, such as having 0.2 alkyl groups and 0.8 alkyl groups containing glycidyl epoxy groups, and any content ratio is possible.

[0030] Among these, R 4 , R 5 and R 6From the viewpoint of rapid curing, hardness, and flexural resistance, the alkyl group is preferably an unsubstituted alkyl group having 1 to 12 carbon atoms, an unsubstituted aryl group having 6 to 10 carbon atoms, a glycidyl epoxy group, a (meth)acrylic group, or a mercapto group, and more preferably an unsubstituted alkyl group having 1 to 12 carbon atoms. Even more preferably, a methyl group or a phenyl group can be cited from the viewpoint of raw material availability.

[0031] a, b, c, d, e, f, and g represent the numbers a>0, b>0, c≧0, d≧0, e≧0, f≧0, and g>0. From the viewpoint of rapid curing, hardness, flexural resistance, hydrophobicity, and water repellency, the numbers 1000≧a>0, 1000≧b>0, 500≧c≧0, 1000≧d≧0, 1000≧e≧0, 100≧f≧0, and 1000≧g>0 are preferred, the numbers 500≧a>0, 500≧b>0, 100≧c≧0, 500≧d≧0, 500≧e≧0, 50≧f≧0, and 500≧g>0 are more preferred, and the numbers 500≧a>0, 500≧b>0, c=0, 500≧d>0, e=0, f=0, and 500≧g>0 are even more preferred.

[0032] Therefore, the organopolysiloxane of the present invention is preferably one whose average structure is represented by the following formula (5), and by using such an organopolysiloxane, even better rapid curing properties, hardness, flexural resistance, hydrophobicity, and water-repellent properties can be achieved.

[0033] [ka] (In the formula, R 1 , R 2 , R 3 , R 4 n, m, a, b, and g have the same meanings as above, and d represents a number where d > 0.

[0034] The weight-average molecular weight of the organopolysiloxane of the present invention is not particularly limited, but considering the need to impart sufficient rapid curing properties, hardness, flexibility, hydrophobicity, and water-repellent properties to the cured product obtained by curing a curable composition containing the compound, it is preferably 1,500 to 200,000, more preferably 5,000 to 100,000, and even more preferably 10,000 to 80,000. The weight-average molecular weight in the present invention is the polystyrene equivalent value obtained by gel permeation chromatography (GPC).

[0035] The organopolysiloxane of the present invention can be produced by copolymerizing a trialkoxysilane represented by the following structural formula (6) (hereinafter referred to as trialkoxysilane (6)), a vinylalkoxysilane represented by the following structural formula (7) (hereinafter referred to as vinylalkoxysilane (7)), and various alkoxysilanes represented by the following structural formulas (9), (10), (11), and (12) (hereinafter referred to as alkoxysilane (9), (10), (11), or (12), respectively) and / or their partially hydrolyzed condensates by hydrolysis and dehydration condensation to obtain the corresponding vinyl group-containing organopolysiloxane, and then by hydrosilylation reaction of this vinyl group-containing organopolysiloxane with an organohydrogenpolysiloxane represented by the following structural formula (8).

[0036] [ka] (In the formula, R 1 ~R 6 ,n and m have the same meaning as above.

[0037] Specific examples of trialkoxysilane (6) include methoxymethyltrimethoxysilane and ethoxymethyltriethoxysilane, but considering the rapid curing, hardness, flexibility, hydrophobicity, and water-repellent properties of the resulting organopolysiloxane, methoxymethyltrimethoxysilane and ethoxymethyltriethoxysilane are preferred.

[0038] Specific examples of trialkoxysilane (7) include vinyltrimethoxysilane, vinyltriethoxysilane, vinylmethyldimethoxysilane, vinylmethyldiethoxysilane, vinylethyldimethoxysilane, vinylethyldiethoxysilane, vinylhexyldimethoxysilane, vinylhexyldiethoxysilane, vinyloctyldimethoxysilane, vinyloctyldiethoxysilane, vinylphenyldimethoxysilane, vinylphenyldiethoxysilane, etc. However, considering the rapid curing properties, hardness, flexibility, hydrophobicity and water-repellent properties of the resulting organopolysiloxane, as well as market availability as a raw material, vinyltrimethoxysilane, vinyltriethoxysilane, and vinylmethyldimethoxysilane are preferred.

[0039] Specific examples of optional components, such as alkoxysilanes (9), include tetramethoxysilane, tetraethoxysilane, tetrapropoxysilane, tetraisopropoxysilane, tetrabutoxysilane, and tetraoctoxysilane.

[0040] Specific examples of optional components, alkoxysilanes (10), include methyltrimethoxysilane, propyltrimethoxysilane, hexyltrimethoxysilane, octyltrimethoxysilane, decyltrimethoxysilane, phenyltrimethoxysilane, naphthyltrimethoxysilane, allyltrimethoxysilane, hexenyltrimethoxysilane, octenyltrimethoxysilane, methyltriethoxysilane, propyltriethoxysilane, hexyltriethoxysilane, octyltriethoxysilane, decyltriethoxysilane, and phenyltriethoxysilane. Lan, naphthyltriethoxysilane, allyltriethoxysilane, hexenyltriethoxysilane, octenyltriethoxysilane, 2-(3,4-epoxycyclohexyl)ethyltrimethoxysilane, 2-(3,4-epoxycyclohexyl)ethyltriethoxysilane, 3-glycidoxypropyltrimethoxysilane, 3-glycidoxypropyltriethoxysilane, 8-glycidoxyoctyltrimethoxysilane, 8-glycidoxyoctyltriethoxysilane, p-styryltrimethoxysilane, p-styryltriethoxysilane, meta Acryloxymethyltrimethoxysilane, methacryloxymethyltriethoxysilane, 3-methacryloxypropyltrimethoxysilane, 3-methacryloxypropyltriethoxysilane, 8-methacryloxyoctyltrimethoxysilane, 8-methacryloxyoctyltriethoxysilane, acryloxymethyltrimethoxysilane, acryloxymethyltriethoxysilane, 3-acryloxypropyltrimethoxysilane, 3-acryloxypropyltriethoxysilane, 8-acryloxyoctyltrimethoxysilane, 8-acryloxyoctyl Triethoxysilane, N-2-(aminoethyl)-aminomethyltrimethoxysilane, N-2-(aminoethyl)-aminomethyltriethoxysilane, N-2-(aminoethyl)-3-aminopropyltrimethoxysilane, N-2-(aminoethyl)-3-aminopropyltriethoxysilane, N-2-(aminoethyl)-8-aminooctyltrimethoxysilane, N-2-(aminoethyl)-8-aminooctyltriethoxysilane, aminomethyltrimethoxysilane, aminomethyltriethoxysilane, 3-aminopropyltrimethoxysilane,3-aminopropyltriethoxysilane, 8-aminooctyltrimethoxysilane, 8-aminooctyltriethoxysilane, N-phenyl-aminomethyltrimethoxysilane, N-phenyl-aminoethyltrimethoxysilane, N-phenyl-3-aminopropyltrimethoxysilane, N-phenyl-3-aminopropyltriethoxysilane, N-phenyl-8-aminooctyltrimethoxysilane, N-phenyl-8-aminooctyltriethoxysilane, 3-isocyanatetopropyltrimethoxysilane, 3-isocyanatetopropyltriethoxysilane, mercaptomethyltrimethoxysilane, mercaptomethyltriethoxysilane, 3-mercaptopropyltrimethoxysilane, 3-mercaptopropyltriethoxysilane, 8-mercaptooctyltrimethoxysilane, 8-mercaptooctyltriethoxy Examples include silane, 3-trimethoxysilylpropyl succinic anhydride, 3-triethoxysilylpropyl succinic anhydride, chloromethyltrimethoxysilane, chloromethyltriethoxysilane, 3-chloropropyltrimethoxysilane, 3-chloropropyltriethoxysilane, 8-chlorooctyltrimethoxysilane, 8-chlorooctyltriethoxysilane, trifluoropropyltrimethoxysilane, nonafluorohexyltrimethoxysilane, tridecafluorooctyltrimethoxysilane, polyethylene glycol methyl-3-trimethoxysilylpropyl ether, polyethylene glycol methyl-3-triethoxysilylpropyl ether, polypropylene glycol methyl-3-trimethoxysilylpropyl ether, and polypropylene glycol methyl-3-triethoxysilylpropyl ether.

[0041] Among these, methyltrimethoxysilane, methyltriethoxysilane, phenyltrimethoxysilane, 3-glycidoxypropyltrimethoxysilane, 3-glycidoxypropyltriethoxysilane, 3-methacryloxypropyltrimethoxysilane, 3-acryloxypropyltrimethoxysilane, 3-mercaptopropyltrimethoxysilane, 3-mercaptopropyltriethoxysilane, nonafluorohexyltrimethoxysilane, tridecafluorooctyltrimethoxysilane, and polyethylene glycol methyl-3-trimethoxysilylpropyl ether are preferred as alkoxysilane (10), with methyltrimethoxysilane and methyltriethoxysilane being more preferred.

[0042] Specific examples of the optional component alkoxysilane (11) include dimethyldimethoxysilane, dimethyldiethoxysilane, methylphenyldimethoxysilane, methylphenyldiethoxysilane, diphenyldimethoxysilane, diphenyldiethoxysilane, octenylmethyldimethoxysilane, 2-(3,4-epoxycyclohexyl)ethylmethyldimethoxysilane, 3-glycidoxypropylmethyldimethoxysilane, 3-glycidoxypropylmethyldiethoxysilane, 3-methacryloxypropylmethyldimethoxysilane, 3-methacryloxy Examples include cypropylmethyldiethoxysilane, 3-acryloxypropylmethyldimethoxysilane, N-2-(aminoethyl)-3-aminopropylmethyldimethoxysilane, N-2-(aminoethyl)-3-aminopropylmethyldiethoxysilane, 3-aminopropylmethyldimethoxysilane, 3-aminopropylmethyldiethoxysilane, 3-mercaptopropylmethyldimethoxysilane, 3-mercaptopropylmethyldiethoxysilane, 3-chloropropylmethyldimethoxysilane, and 3-chloropropylmethyldiethoxysilane.

[0043] Among these, dimethyldimethoxysilane, dimethyldiethoxysilane, diphenyldimethoxysilane, 3-glycidoxypropylmethyldimethoxysilane, and 3-glycidoxypropylmethyldiethoxysilane are preferred as alkoxysilane(11), with dimethyldimethoxysilane and dimethyldiethoxysilane being more preferred.

[0044] Specific examples of the optional component alkoxysilane (12) include trimethylmethoxysilane, trimethylethoxysilane, vinyldimethylmethoxysilane, 3-methacryloxypropyldimethylmethoxysilane, 3-methacryloxypropyldimethylethoxysilane, 3-acryloxypropyldimethylmethoxysilane, 3-acryloxypropyldimethylethoxysilane, N-2-(aminoethyl)-3-aminopropyldimethylmethoxysilane, N-2-(aminoethyl)-3-aminopropyldimethylethoxysilane, etc., but trimethylmethoxysilane is preferred.

[0045] Specific examples of organohydrogenpolysiloxane (8) include those in which the number of dimethylsiloxy units m is 8, 20, 40, 60, and 90 on average. Of these, those with m of 20 and 40 are preferred from the viewpoint of hydrosilylation reactivity, hydrophobicity exhibited, water repellency, and imparting flexibility to the coating.

[0046] The copolymerization of trialkoxysilanes (6) and (7) with optional alkoxysilanes (9) to (12) by hydrolysis and dehydration condensation is usually carried out without solvents, but may also be carried out in the presence of an organic solvent that dissolves all of the alkoxysilanes used in the reaction (e.g., methanol, ethanol, isopropyl alcohol, butanol, diacetone alcohol, propylene glycol monomethyl ether, propylene glycol monomethyl ether acetate, acetone, toluene, and xylene). When using an organic solvent, there are no particular restrictions on the amount used, but it is generally preferable to use 20 parts by mass or less, more preferably 0.1 to 10 parts by mass, and even more preferably 0.5 to 5 parts by mass, per 1 part by mass of the total mass of trialkoxysilane (6), (7) and the optional alkoxysilane (9) to (12).

[0047] Copolymerization by hydrolysis and dehydration condensation is carried out by adding or adding an acid or base that acts as a catalyst for the hydrolysis reaction, along with water, dropwise to the above-mentioned mixture or solution of alkoxysilanes. In this case, the acid or base may be added dropwise as an aqueous solution. The acid is not particularly limited and includes, for example, hydrochloric acid, sulfuric acid, nitric acid, acetic acid, formic acid, phosphoric acid, p-toluenesulfonic acid and its hydrate, methanesulfonic acid, trifluoromethanesulfonic acid, and cation exchange resins. Hydrochloric acid, methanesulfonic acid, and cation exchange resins are preferred, hydrochloric acid and cation exchange resins are more preferred, and hydrochloric acid is even more preferred. The amount of acid used is usually preferably 0.001 to 1 mole, and more preferably 0.01 to 0.2 moles, per mole of trialkoxysilane (6), (7) and the optional alkoxysilane (9) to (12).

[0048] The base is not particularly limited and includes, for example, sodium hydroxide, potassium hydroxide, lithium hydroxide, sodium acetate, potassium acetate, lithium acetate, sodium carbonate, sodium bicarbonate, sodium methoxide, sodium ethoxide, potassium methoxide, potassium ethoxide, potassium tertifoxide, triethylamine, anion exchange resin, etc. Sodium hydroxide, potassium hydroxide, and sodium acetate are preferred, and sodium acetate is more preferred. The amount of base used is usually preferably 0.001 to 1 mole, and more preferably 0.01 to 0.2 moles, per mole of trialkoxysilane (6), (7) and the optional alkoxysilane (9) to (12).

[0049] The amount of water used in copolymerization by hydrolysis and condensation is usually preferably 0.1 to 100 moles, more preferably 0.3 to 10 moles, and even more preferably 0.5 to 2.0 moles, per mole of trialkoxysilane (6), (7) and the optional alkoxysilane (9) to (12). The reaction temperature for copolymerization by hydrolysis and dehydration condensation is not particularly limited, but is usually 20 to 150°C, preferably 30 to 120°C, more preferably 40 to 100°C, and even more preferably 50 to 80°C. The reaction time is usually 1 hour or more, preferably 2 to 72 hours. There are no particular restrictions on the concentration temperature of the reaction mixture, but it is usually 10 to 150°C, preferably 60 to 120°C. There are no particular restrictions on the pressure during concentration, and it may be at atmospheric pressure or under reduced pressure.

[0050] The stoichiometric ratio of trialkoxysilanes (6) and (7) and the optional alkoxysilanes (9) to (12) is not particularly limited, but considering the rapid curing, hardness, and flexural resistance of the resulting organopolysiloxane, it is preferable that the ratio is 0.001 to 1,000 moles of alkoxysilane (7), 0 to 1,000 moles of alkoxysilane (9), 0 to 1,000 moles of alkoxysilane (10), 0 to 1,000 moles of alkoxysilane (11), and 0 to 1,000 moles of alkoxysilane (12) per mole of trialkoxysilane (6), and more preferably For every mole of trialkoxysilane(6), the ratios are 0.01 to 100 moles of alkoxysilane(7), 0 to 100 moles of alkoxysilane(9), 0.001 to 100 moles of alkoxysilane(10), 0 to 100 moles of alkoxysilane(11), and 0 to 100 moles of alkoxysilane(12). More preferably, for every mole of trialkoxysilane(6), the ratios are 0.1 to 50 moles of alkoxysilane(7), 0 moles of alkoxysilane(9), 0.001 to 50 moles of alkoxysilane(10), 0 moles of alkoxysilane(11), and 0 moles of alkoxysilane(12).

[0051] Therefore, the organopolysiloxane of the present invention is preferably a vinyl group-containing organopolysiloxane obtained by copolymerizing trialkoxysilane (6), (7) and alkoxysilane (10) by hydrolysis and dehydration condensation, and by using a compound obtained by subsequent hydrosilylation with organohydrogenpolysiloxane (8), even better rapid curing properties, hardness, flexural resistance, hydrophobicity, and water-repellent properties can be exhibited.

[0052] [ka] (In the formula, R 1 ~R 4 ,n and m have the same meaning as above.

[0053] The hydrosilylation of the vinyl group-containing organopolysiloxane and organohydrogenpolysiloxane (8) can be carried out in a solvent system or a solvent-free system in the presence of a platinum catalyst or a rhodium catalyst.

[0054] The reaction ratio between the vinyl group-containing organopolysiloxane and the organohydrogenpolysiloxane is preferably 0.1 to 2.0 Si-H groups of the organohydrogenpolysiloxane for every vinyl group of the vinyl group-containing organopolysiloxane, and more preferably 0.25 to 1.2 groups. If the ratio is too low, an excess of unreacted vinyl group-containing organopolysiloxane may remain, and if it is too high, intermolecular crosslinking may proceed too much, leading to unnecessary high molecular weight and reduced stability of the product.

[0055] For the hydrosilylation reaction catalyst, known catalysts such as platinum (Pt), complex compounds with Pt as the central metal, and complex compounds with rhodium as the central metal can be used. Specifically, examples include alcoholic solutions of chloroplatinic acid, 1,3-divinyltetramethyldisiloxane complexes of chloroplatinic acid, compounds obtained by neutralizing the said complexes, 1,3-divinyltetramethyldisiloxane complexes with a central metal oxidation state of Pt(II) or Pt(0), and Wilkinson catalysts of rhodium. Preferably, the complex has a central metal oxidation state other than Pt(IV) and is preferred from the viewpoint of addition regioselectivity, and 1,3-divinyltetramethyldisiloxane complexes having Pt(0) or Pt(II) as the central metal are particularly preferred.

[0056] The amount of hydrosilylation catalyst used is not particularly limited as long as it is an amount that exhibits the catalytic effect of the hydrosilylation reaction, but is preferably 0.000001 to 1 mol%, more preferably 0.0001 to 0.01 mol%, per mole of vinyl group (i). If it is less than 0.000001 mol%, a sufficient catalytic effect may not be exhibited, and if it is more than 1 mol%, the effect will saturate, which may increase production costs and make it uneconomical.

[0057] The temperature for the hydrosilylation reaction is preferably 50 to 150°C, more preferably 60 to 130°C, and even more preferably 70 to 110°C. Below 50°C, the reaction rate is low and production efficiency may be poor. Above 150°C, it becomes difficult to control the addition position, and addition isomers may be formed, as well as side reactions such as dehydrogenation reactions originating from the hydrosilyl group. The reaction time is preferably 30 minutes to 10 hours.

[0058] A solvent may be used when carrying out the hydrosilylation reaction. The solvent is not particularly limited as long as it does not inhibit the reaction or react with the starting materials. Examples include alcoholic solvents such as methanol, ethanol, and propanol; etheric solvents such as diethyl ether, dimethoxyethane, and tetrahydrofuran; polar solvents containing heteroatoms such as acetonitrile and dimethylformamide; aliphatic hydrocarbon solvents such as hexane and heptane; and aromatic hydrocarbon solvents such as toluene and xylene. These solvents may be used individually or in combination of two or more.

[0059] The kinematic viscosity of the organopolysiloxane of the present invention at 25°C is 10 to 10,000 mm². 2 / s is preferred, and 30-5000mm 2 / s is preferable. Kinematic viscosity is 10 mm 2 If the value is lower than / s, the desired hydrophobicity and water-repellent properties may not be achieved. On the other hand, 10000mm 2 If the value is higher than / s, the resulting polymer may have poor storage stability and be difficult to handle. The kinematic viscosity in this invention is measured using a Cannon-Fenske viscometer according to the method described in JIS Z 8803:2011.

[0060] The curable composition and coating agent composition of the present invention (hereinafter collectively referred to as "the composition") contain at least the above-mentioned (A) organopolysiloxane and (B) curing catalyst. Since the composition of the present invention contains the organopolysiloxane of the present invention as described above, when a solid substrate is coated using this composition, the curing speed, hardness, flexibility, hydrophobicity, and water-repellent properties of the cured film are improved compared to when conventional organopolysiloxanes are used, due to the structure of the organopolysiloxane of the present invention.

[0061] The curing catalyst (B) is a component that promotes the hydrolysis and condensation reaction of the hydrolyzable silyl groups contained in (A) organopolysiloxane with moisture in the air, thereby accelerating the curing of the composition, and is added to ensure efficient curing. The amount of curing catalyst (B) to be added is not particularly limited, but considering the ability to adjust the curing speed to an appropriate range to produce a cured film with desired physical properties, improve workability during application, and the economic benefits associated with the addition, 0.01 to 50 parts by mass, more preferably 0.05 to 10 parts by mass, and even more preferably 0.1 to 5 parts by mass per 100 parts by mass of component (A) is preferred.

[0062] The curing catalyst is not particularly limited as long as it is a curing catalyst used for curing general moisture condensation curing type compositions. Specific examples include alkyl tin compounds such as dibutyltin oxide and dioctyl tin oxide; alkyl tin ester compounds such as dibutyltin diacetate, dibutyltin dilaurate, dioctyl tin dilaurate, dibutyltin dioctoate, dioctyl tin dioctoate, and dioctyl tin diversate; tetraisopropoxytitanium, tetra-n-butoxytitanium, tetrakis(2-ethylhexoxy)titanium, dipropoxybis( Titanium esters such as acetylacetonate titanium, titanium diisopropoxybis(ethylacetoacetate), titanium isopropoxyoctylene glycol, and titanium chelate compounds and their partial hydrolysates; zinc naphthenate, zinc stearate, zinc-2-ethyloctoate, iron-2-ethylhexoate, cobalt-2-ethylhexoate, manganese-2-ethylhexoate, cobalt naphthenate, aluminum trihydroxylate, aluminum alcoholate, aluminum acylate, salts of aluminum acylate, aluminum Organometallic compounds such as minosiloxy compounds and aluminum chelate compounds; 3-aminopropyltrimethoxysilane, 3-aminopropyltriethoxysilane, 3-aminopropylmethyldimethoxysilane, 3-aminopropylmethyldiethoxysilane, N-β(aminoethyl)γ-aminopropyltrimethoxysilane, N-β(aminoethyl)γ-aminopropyltriethoxysilane, N-β(aminoethyl)γ-aminopropylmethyldimethoxysilane, N-β(aminoethyl)γ-aminopropylmethyldiethoxysilane, bis[3-(t [Dimethoxysilyl)propyl]amine, bis[3-(triethoxysilyl)propyl]amine, N,N′-bis[3-(triethoxysilyl)propyl]ethane-1,2-diamine, N,N′-bis[3-(triethoxysilyl)propyl]ethane-1,2-diamine, aminoalkyl-substituted alkoxysilanes such as N-phenyl-3-aminopropyltrimethoxysilane; amine compounds and their salts such as hexylamine, dodecylamine phosphate, and tetramethylguanidine; quaternary ammonium salts such as benzyltriethylammonium acetate;Examples include alkali metal lower fatty acid salts such as potassium acetate, sodium acetate, and lithium oxalate; dialkylhydroxylamines such as dimethylhydroxylamine and diethylhydroxylamine; silanes and siloxanes containing a guanidyl group, such as tetramethylguanidylpropyltrimethoxysilane, tetramethylguanidylpropylmethyldimethoxysilane, tetramethylguanidylpropyltriethoxysilane, tetramethylguanidylpropylmethyldiethoxysilane, and tetramethylguanidylpropyltris(trimethylsiloxy)silane; and silanes and siloxanes containing a phosphazene base, such as N,N,N',N',N'',N''-hexamethyl-N'''-[3-(trimethoxysilyl)propyl]-phosphorimidictriamide. These may be used individually or in combination of two or more types.

[0063] Among these, dioctyl tin dilaurate, dioctyl tin diversate, tetraisopropoxytitanium, tetra-n-butoxytitanium, titanium diisopropoxybis(ethyl acetate), 3-aminopropyltrimethoxysilane, 3-aminopropyltriethoxysilane, N-β(aminoethyl)γ-aminopropyltrimethoxysilane, bis[3-(trimethoxysilyl)propyl]amine, N,N′-bis[3-(trimethoxysilyl)propyl]ethane-1,2-diamine, and tetramethylguanidylpropyltrimethoxysilane are preferred due to their superior reactivity, from the viewpoint of curability of the composition. Dioctyl tin dilaurate, dioctyl tin diversate, tetra-n-butoxytitanium, 3-aminopropyltrimethoxysilane, 3-aminopropyltriethoxysilane, and tetramethylguanidylpropyltrimethoxysilane are more preferred, and since they do not contain organotin compounds and have lower toxicity, tetra-n-butoxytitanium, 3-aminopropyltrimethoxysilane, 3-aminopropyltriethoxysilane, and tetramethylguanidylpropyltrimethoxysilane are even more preferred, and from the viewpoint of curability of the composition, tetra-n-butoxytitanium and 3-aminopropyltriethoxysilane are particularly preferred.

[0064] Furthermore, for the purpose of adjusting the viscosity of the composition of the present invention to improve workability, and for the purpose of adjusting the curability of the composition, the hardness and flexibility of the resulting coating film, one or more compounds selected from silane compounds containing alkoxysilyl groups, silicone alkoxy oligomers having alkoxysilyl groups and / or silanol groups in one molecule, and silicone resins may be mixed separately from the organopolysiloxane of component (A), depending on the intended use.

[0065] The silane compounds containing an alkoxysilyl group are not particularly limited, but specific examples include those exemplified in the above alkoxysilanes (9) to (12). The silicone alkoxy oligomer having an alkoxysilyl group and / or a silanol group in one molecule is not particularly limited and may be a commercially available product. Specific examples include X-40-9250, X-40-9246, X-40-9225, KR-500, KR-515, KC-89S, KR-401N, X-40-9227, KR-510, KR-9218, KR-400, X-40-2327, KR-401, etc., manufactured by Shin-Etsu Chemical Co., Ltd. Furthermore, the silicone resin used is not particularly limited and can be any commercially available product. Specific examples include KR-220L, KR-251, KR-112, KR-300, KR-311, KR-480, and KR-216, all manufactured by Shin-Etsu Chemical Co., Ltd.

[0066] Furthermore, while the compositions of the present invention are preferably in a solvent-free form that substantially does not contain organic solvents (often harmful to the human body and flammable), solvents may be added depending on their application and ease of use. Here, "substantially" means that the amount of solvent contained in the composition is 1% by mass or less, and more particularly 0.1% by mass or less. Specific examples of usable solvents include (A) organic solvents similar to those used in the production of organopolysiloxanes. Furthermore, the term "solvent" includes reaction solvents that could not be completely removed by reduced-pressure distillation, as well as other components that were not intentionally added to the curable composition or coating agent composition.

[0067] Depending on the intended use, the composition of the present invention may contain various additives such as adhesion modifiers, inorganic and organic ultraviolet absorbers, light stabilizers, storage stability modifiers, plasticizers, fillers, and pigments.

[0068] By applying the composition of the present invention described above to the surface of a solid substrate and curing it to form a coating layer, a coated solid substrate, which is a cured article, can be obtained. The application method is not particularly limited, and specific examples include spray coating, spin coating, dip coating, roller coating, brush coating, bar coating, flow coating, and other known methods which can be appropriately selected and used. The solid substrate is not particularly limited, and specific examples include epoxy resins, phenolic resins, polycarbonates and polycarbonate blends, acrylic resins such as poly(methyl methacrylate), polyester resins such as poly(ethylene terephthalate), poly(butylene terephthalate), and unsaturated polyester resins, polyamide resins, polyimide resins, acrylonitrile-styrene copolymers, styrene-acrylonitrile-butadiene copolymers, polyvinyl chloride resins, polystyrene resins, blends of polystyrene and polyphenylene ether, cellulose acetate butyrate, polyethylene resins and other organic polymer substrates, metal substrates such as steel plates, painted surfaces, glass, ceramics, concrete, slate boards, textiles, wood, stone, roof tiles, inorganic fillers such as (hollow) silica, titania, zirconia, and alumina, and glass fiber products such as glass cloth, glass tape, glass mat, and glass paper, among others. The material and shape of the substrate are not particularly limited, but the composition of the present invention can be used particularly suitably for coating steel plates and glass.

[0069] The composition of the present invention undergoes a hydrolysis condensation reaction of (A) organopolysiloxane upon contact with moisture in the atmosphere, initiating a curing reaction. Any humidity between 10 and 100% RH can be used as an indicator of moisture in the atmosphere, and moisture in the air is sufficient. However, generally, hydrolysis proceeds faster at higher humidity levels, so moisture may be added to the atmosphere if desired. The curing reaction temperature and time can be appropriately adjusted depending on factors such as the substrate used, moisture concentration, catalyst concentration, and type of hydrolyzable group. Typically, this ranges from 1 minute to 1 week, provided that it does not exceed the heat resistance temperature of the substrate used. The composition of the present invention hardens well even at room temperature, and therefore, even when room temperature curing is essential, such as in on-site construction, the stickiness (tack) of the coating surface disappears in a few minutes to a few hours, resulting in excellent workability. However, heat treatment may be performed within a range that does not exceed the heat resistance temperature of the substrate. [Examples]

[0070] The present invention will be specifically described below using examples and comparative examples, but the present invention is not limited to these.

[0071] In the following, the kinematic viscosity of each product is the measurement value at 25°C using a Cannon-Fenske viscometer measured according to the method described in JIS Z 8803:2011, and the molecular weight is the weight-average molecular weight in polystyrene equivalent, determined by GPC (gel permeation chromatography) measurement using a Tosoh Corporation GPC (gel permeation chromatography) apparatus with toluene as the solvent and a radioisotope (RI) as the detector. The average structure of organopolysiloxanes was determined using a 300MHz-NMR spectrometer manufactured by JEOL Ltd. 1 H-NMR and 29 It was calculated from the integrated value of the detection spectrum in Si-NMR. The amount of silanol hydroxyl groups contained in each product (mass%), hereinafter referred to as silanol content, was quantified from the amount of methane gas generated when each product was reacted with a Grignard reagent (methylmagnesium iodide). The vinyl group content (moles / 100g, hereafter referred to as vinyl value) in each product was quantified by treating each product with Hanus solution, reacting it with an aqueous potassium iodide solution, and then titrating the resulting iodine with sodium thiosulfate.

[0072] [1] Synthesis of organopolysiloxanes [Synthesis Example 1] Synthesis of organopolysiloxane (1A) In a 5 L separable flask equipped with a stirrer, reflux condenser, dropping funnel, and thermometer, add 1850 g (13.6 mol) of methyltrimethoxysilane, 300 g (1.8 mol) of methoxymethyltrimethoxysilane, and vinylmethyldimethoxysilane. 357 2.7 mol of iodine (g) and 0.7 g of maleic anhydride were charged, and under stirring, 347 g of deionized water was added dropwise at 15°C. Hydrolysis and condensation were carried out at 70°C for 3 hours. Subsequently, 60 g of strongly acidic cation exchange resin (Lanxess Levatit K2629) was added, and hydrolysis and condensation were carried out again at 70°C for 3 hours. The resulting reaction solution was distilled off under atmospheric pressure, and after no more fractions were released, the condensation reaction was accelerated at 105°C for 3 hours. Finally, the fractions were removed by reduced-pressure distillation (90°C, 1.3 kPa) to obtain organopolysiloxane (1A) (yield 1410 g). The obtained organopolysiloxane 1A is a colorless, transparent liquid represented by the average structural formula shown below, with a kinematic viscosity of 62 mmHg. 2 The values ​​were / s, Mw2700, silanol hydroxyl group content 0.3% by mass, and vinyl value 0.15 mol / 100g.

[0073] [ka]

[0074] [Production Example 1-1] Synthesis of organopolysiloxane (1B) In a 1 L separable flask equipped with a stirrer, reflux condenser, dropping funnel, and thermometer, 200 g of organopolysiloxane (1A) obtained in Synthesis Example 1, 95 g of the following hydrogensiloxane (8-1) (reaction molar ratio, vinyl group:Si-H group = 4:1), and 180 g of toluene were charged. Under stirring, at 80°C, 0.0004 molars of the Pt(0) 1,3-divinyltetramethyldisiloxane complex were added per mole of Si-H groups, and hydrosilylation was performed at 80°C for 3 hours. Subsequently, the fraction was removed by vacuum distillation (90°C, 1.3 kPa) to obtain organopolysiloxane (1B) (yield 282 g). The obtained organopolysiloxane (1B) is a colorless, transparent liquid represented by the following average structural formula, with a kinematic viscosity of 635 mmHg. 2 The pH was / s, Mw 26400, and the silanol hydroxyl group content was 0.1% by mass.

[0075] [ka]

[0076] [ka]

[0077] [Production Example 1-2] Synthesis of organopolysiloxane (1C) In a 1 L separable flask equipped with a stirrer, reflux condenser, dropping funnel, and thermometer, 200 g of organopolysiloxane (1A) obtained in Synthesis Example 1, 45 g of the following hydrogensiloxane (8-2) (reaction molar ratio, vinyl group:Si-H group = 4:1), and 180 g of toluene were charged. Under stirring, at 80°C, 0.0004 molars of the Pt(0) 1,3-divinyltetramethyldisiloxane complex were added per mole of Si-H groups, and hydrosilylation was performed at 80°C for 3 hours. Subsequently, the fraction was removed by vacuum distillation (90°C, 1.3 kPa) to obtain organopolysiloxane (1C) (yield 240 g). The obtained organopolysiloxane (1C) is a colorless, transparent liquid represented by the following average structural formula, with a kinematic viscosity of 341 mmHg. 2 The pH was / s, Mw 17800, and the silanol hydroxyl group content was 0.1% by mass.

[0078] [ka]

[0079] [ka]

[0080] [Production Examples 1-3] Synthesis of Organopolysiloxane (1D) In a 1 L separable flask equipped with a stirrer, reflux condenser, dropping funnel, and thermometer, 200 g of organopolysiloxane (1A) obtained in Synthesis Example 1, 123 g of the following hydrogensiloxane (8-3) (reaction molar ratio, vinyl group:Si-H group = 4:1), and 180 g of toluene were charged. Under stirring, at 80°C, 0.0004 molars of the Pt(0) 1,3-divinyltetramethyldisiloxane complex were added per mole of Si-H groups, and hydrosilylation was performed at 80°C for 3 hours. Subsequently, the fraction was removed by vacuum distillation (90°C, 1.3 kPa) to obtain organopolysiloxane (1D) (yield 313 g). The obtained organopolysiloxane (1D) is a colorless, transparent liquid represented by the following average structural formula, with a kinematic viscosity of 1329 mmHg. 2 The pH was / s, Mw 34300, and the silanol hydroxyl group content was 0.1% by mass.

[0081] [ka]

[0082] [ka]

[0083] [Production Examples 1-4] Synthesis of Organopolysiloxane (1E) In a 1 L separable flask equipped with a stirrer, reflux condenser, dropping funnel, and thermometer, 200 g of organopolysiloxane (1A) obtained in Synthesis Example 1, 193 g of the following hydrogensiloxane (8-4) (reaction molar ratio, vinyl group:Si-H group = 4:1), and 180 g of toluene were charged. Under stirring, at 80°C, 0.0004 molars of the Pt(0) 1,3-divinyltetramethyldisiloxane complex were added per mole of Si-H groups, and hydrosilylation was performed at 80°C for 3 hours. Subsequently, the fraction was removed by vacuum distillation (90°C, 1.3 kPa) to obtain organopolysiloxane (1E) (yield 385 g). The obtained organopolysiloxane (1E) is a colorless, transparent liquid represented by the following average structural formula, with a kinematic viscosity of 4714 mmHg. 2 The pH was / s, Mw 70000, and the silanol hydroxyl group content was 0.1% by mass.

[0084] [ka]

[0085] [ka]

[0086] [Synthesis Example 2] Synthesis of organopolysiloxane (2A) A 1 L separable flask equipped with a stirrer, reflux condenser, dropping funnel, and thermometer contains methyltrimethoxysilane. 420 g (3.08 mol), vinylmethyldimethoxysilane 71 0.54 mol of ionized water and 0.14 g of maleic anhydride were charged, and under stirring, 69.4 g of deionized water was added dropwise at 15°C, followed by hydrolysis and condensation at 70°C for 3 hours. Then, 12 g of strongly acidic cation exchange resin (Lanxess Levatit K2629) was added, and hydrolysis and condensation were carried out again at 70°C for 3 hours. The resulting reaction solution was distilled off under atmospheric pressure, and after no more fractions were released, the condensation reaction was accelerated at 105°C for 3 hours. Finally, the fractions were removed by reduced-pressure distillation (90°C, 1.3 kPa) to obtain organopolysiloxane (2A) (yield 290 g). The obtained organopolysiloxane (2A) is a colorless, transparent liquid represented by the average structural formula shown below, with a kinematic viscosity of 66 mmHg.2 The values ​​were / s, Mw3100, silanol hydroxyl group content 0% by mass, and vinyl value 0.15 mol / 100g.

[0087] [ka]

[0088] [Comparative Example 1-1] Synthesis of organopolysiloxane (2B) In a 1 L separable flask equipped with a stirrer, reflux condenser, dropping funnel, and thermometer, 200 g of organopolysiloxane (2A) obtained in Synthesis Example 2, 95 g of the above-mentioned hydrogensiloxane (8-1) (reaction molar ratio, vinyl group:Si-H group = 4:1), and 180 g of toluene were charged. Under stirring, at 80°C, 0.0004 molars of the Pt(0) 1,3-divinyltetramethyldisiloxane complex were added per mole of Si-H groups, and hydrosilylation was performed at 80°C for 3 hours. Subsequently, the fraction was removed by vacuum distillation (90°C, 1.3 kPa) to obtain organopolysiloxane (2B) (yield 290 g). The obtained organopolysiloxane (2B) is a colorless, transparent liquid represented by the average structural formula below, with a kinematic viscosity of 191 mmHg. 2 The saturation level was 13000, and the content of silanol hydroxyl groups was 0% by mass.

[0089] [ka]

[0090] [2] Coating composition [Examples 2-1 to 2-6, Comparative Examples 2-1 to 2-3, Reference Example 2-1] The organopolysiloxanes obtained in Production Examples 1-1 to 1-4, Comparative Example 1-1, and Synthesis Example 1 were mixed with the curing catalyst in the amounts shown in Table 1 to prepare the coating compositions of Examples 2-1 to 2-6, Comparative Examples 2-1 to 2-3, and Reference Example 2-1.

[0091] [Table 1] KR-400: Methyl-based silicone coating agent (manufactured by Shin-Etsu Chemical Co., Ltd.) TBT: Tetrabutyl titanate KBE-903: 3-aminopropyltriethoxysilane MGPM: Tetramethylguanidylpropyltrimethoxysilane

[0092] Each coating composition obtained above was applied to a glass plate or polished steel plate using a bar coater No. 14 under air conditions of 25°C and 50% RH. The mixture was then dried and cured for one day under air conditions of 25°C and 50% RH to produce a cured film. The following evaluations were performed on the obtained cured films. The results are shown in Table 2. [Dry time to touch] The above method of coating the coating agent composition was applied to a glass plate to obtain a test piece. The test piece was left in air at 25°C and 50% RH, and the time until the coating film no longer adhered to the finger when pressed on the coated surface was indicated as moisture curing progressed. A smaller value indicates better curing performance. [Pencil hardness] Test specimens in which a hardened film was formed on a glass plate using the above coating method were subjected to a 750g load in accordance with the pencil scratch test described in JIS K 5600-5-4, and the results are shown. [Bending resistance] Test specimens in which a hardened film was formed on polished steel plates using the above coating method were measured using a cylindrical mandrel (Type 1) in accordance with the method described in JIS K 5600-5-1, and the results are shown. [Water repellency / sliding property] A hardened film was formed on a polished steel plate using the above coating method. One drop (approximately 2 μl) of purified water was dropped onto the test piece, and the water contact angle was measured using a contact angle meter (device name: Drop Master DM-701, manufactured by Kyowa Interface Science Co., Ltd.) to evaluate water repellency. A contact angle of approximately 100° or higher is desirable for water repellency. In addition, one drop (approximately 20 μl) of purified water was dropped onto the same test piece, and the angle at which the water droplet began to flow was defined as the water sliding angle to evaluate water sliding properties. The evaluation criteria were as follows: ○ for a water sliding angle of less than 35°, △ for an angle between 35 and 45°, and × for an angle exceeding 45°.

[0093] [Table 2]

[0094] [Examples 3-1 to 3-6, Comparative Examples 3-1 to 3-3, Reference Example 3-1] The organopolysiloxanes obtained in Production Examples 1-1 to 1-4, Comparative Example 1-1, and Synthesis Example 1 were mixed with the curing catalyst in the amounts shown in Table 3 to prepare the coating compositions of Examples 3-1 to 3-6, Comparative Examples 3-1 to 3-3, and Reference Example 3-1.

[0095] [Table 3] KR-400: Methyl-based silicone coating agent (manufactured by Shin-Etsu Chemical Co., Ltd.) TBT: Tetrabutyl titanate MGPM: Tetramethylguanidylpropyltrimethoxysilane DX9740: Aluminum alkoxide compound (manufactured by Shin-Etsu Chemical Co., Ltd.) Isopar G: Isoparaffinic organic solvent (initial boiling point 166°C, dry point 177°C, manufactured by ExxonMobil)

[0096] The following evaluations were performed using each of the coating agent compositions obtained above. The results are shown in Table 4. [Workability] Two ml of each of the above coating compositions was dropped onto a black painted board (material: SPCC-SD, standard: JIS-G-3141, dimensions: 0.8 mm x 70 mm x 150 mm, with one side coated with amino alkyd black paint after chemical electrodeposition, manufactured by Asahi B-Techno Co., Ltd.), and thinly applied by hand using tissue paper. The board was then left to stand at 25°C for 5 minutes. After that, any excess was wiped off with a dry microfiber cloth. ○ indicated that wiping was easy and even, △ indicated that slight unevenness occurred or that wiping was somewhat difficult, and × indicated that unevenness occurred significantly or that wiping was difficult and the application was difficult. [Curability] Test specimens coated with the coating composition were prepared using the same method as for the workability evaluation. These were then cured by standing at 25°C for 2 hours to obtain test specimens with a cured film. When the coated surface of the obtained test specimens was touched with a finger, specimens that showed no tackiness and exhibited slipperiness were marked with ○, specimens that showed no tackiness but did not exhibit slipperiness were marked with △, and specimens that showed tackiness were marked with ×. [Water repellency / sliding property] Test specimens coated with the coating composition were prepared using the same method as for the workability evaluation. These were then cured at 25°C for 2 hours to obtain test specimens with a cured film. One drop (approximately 2 μl) of purified water was dropped onto the obtained test specimen, and the water contact angle was measured using a contact angle meter (device name: Drop Master DM-701, manufactured by Kyowa Interface Science Co., Ltd.) to evaluate water repellency. A contact angle of approximately 100° or higher is desirable for water repellency. In addition, one drop (approximately 20 μl) of purified water was dropped onto the same test specimen, and the specimen was gradually tilted from a horizontal position. The angle at which the water droplet began to flow was defined as the water sliding angle, and the water sliding ability was evaluated. The evaluation criteria were as follows: a water sliding angle of less than 35° was marked with ○, an angle between 35 and 45° was marked with △, and an angle exceeding 45° was marked with ×. [Abrasion resistance] Test specimens coated with the coating composition were prepared using the same method as for the workability evaluation. These were then cured by standing at 25°C for 12 hours to obtain test specimens with a cured film. An abrasion resistance test was performed on the surface of the obtained test specimens with the cured film using a simple friction tester (manufactured by Imoto Seisakusho Co., Ltd.). Specifically, a movable plate to which the test specimen was fixed moved at a speed of 30 times per minute over a distance of 100 mm per reciprocating motion. A friction object with a load of 500 g attached by a weight was placed at the center of the plate and abrasion was induced by reciprocating motion 400 times. The water contact angle of the surface after abrasion was measured using the same method as for the water repellency / hydrophobicity test, and the abrasion resistance was evaluated. For the evaluation of abrasion resistance, a water contact angle after 400 reciprocating motions was judged as follows: ○ if it was more than 90% of the water contact angle before abrasion, △ if it was in the range of 75-90%, and × if it was less than 75%. The friction material used in the test consisted of a dry, clean cloth (absorbent cloth made of cellulose / cotton composite fibers, ThreeBond product "ThreeBond 6644E") with a width of 40 mm, soaked in distilled water, and wrapped around a stainless steel cylinder with a diameter of 20 mm. The cylinder was positioned so that its axis was perpendicular to the direction of movement of the moving plate.

[0097] [Table 4]

[0098] As shown in Tables 2 and 4, the coating agents using organopolysiloxanes obtained in Production Examples 1-1 to 1-4 exhibit excellent rapid curing properties even when amine compounds are used as curing catalysts. Furthermore, the resulting cured films possess both hardness and flexibility, as well as excellent water repellency and hydrophobicity. On the other hand, coating agents using organopolysiloxanes that do not have the constituent units represented by general formula (1) have a long touch-dry time and poor curing properties, and the resulting cured film has poor abrasion resistance. Furthermore, it was found that coatings obtained from coating agents using organopolysiloxanes that do not have the constituent units represented by the above general formula (2) are inferior in water repellency, water-sliding properties, workability, and abrasion resistance.

Claims

1. A method for producing a cured product by curing a curable composition containing (A) an organopolysiloxane having a constituent unit represented by the following general formula (1), a constituent unit represented by the following general formula (2), and a group represented by the following general formula (3) that is directly bonded to a silicon atom, and (B) a curing catalyst. 【Chemistry 1】 (In the formula, R 1 (This represents an unsubstituted or substituted alkyl group with 1 to 12 carbon atoms, or an unsubstituted or substituted aryl group with 6 to 10 carbon atoms.) 【Chemistry 2】 (In the formula, R 2 Each of these independently represents an unsubstituted or substituted alkyl group with 1 to 12 carbon atoms, or an unsubstituted or substituted aryl group with 6 to 10 carbon atoms, where n is independently 2 or 3, and m is an integer from 5 to 100. 【Transformation 3】 (In the formula, R 3 (This represents a hydrogen atom, an unsubstituted or substituted alkyl group having 1 to 10 carbon atoms, or an unsubstituted or substituted aryl group having 6 to 10 carbon atoms.)

2. A method for producing a cured product according to claim 1, wherein the curable composition is applied to the surface of a solid substrate and then cured.

3. A method for producing a cured product according to claim 1 or 2, wherein the average structure of the organopolysiloxane is represented by the following formula (4). 【Chemistry 4】 (wherein, R 1 , R 2 , R 3 , n and m represent the same meaning as defined above, R 4 , R 5 and R 6 each independently represent an unsubstituted alkyl group having 1 to 12 carbon atoms, an unsubstituted aryl group having 6 to 10 carbon atoms, or a group obtained by substituting these alkyl group or aryl group with a substituent selected from a glycidyl-type epoxy group, a (meth)acryl group, and a mercapto group, and a, b, c, d, e, f and g represent numbers satisfying a>0, b>0, c≥0, d≥0, e≥0, f≥0, and g>0.)

4. A method for producing a cured product according to claim 3, wherein the average structure of the organopolysiloxane is represented by the following formula (5). 【Transformation 5】 (In the formula, R 1 , R 2 , R 3 , R 4 n, m, a, b, and g have the same meanings as above, and d represents the number d > 0.

5. A method for producing a cured product according to any one of claims 1 to 4, wherein the curing catalyst (B) is an amine-based compound.

Citation Information

Patent Citations

  • Curable resin composition

    JP1994271650A

  • Alkoxy-crosslinkable one-component moisture-curing materials

    JP2004536957A

  • Composition for use in membrane formation, forming method for membrane, and silica-based membrane

    JP2005179587A

  • Curable composition

    JP2014114434A

  • Organopolysiloxane and coating composition containing the same

    JP2021080307A