Transparent resin composition and molded article

The transparent resin composition with chemically recycled monomers and ultraviolet absorbers addresses weather resistance and mechanical property issues, ensuring environmental friendliness and quality equivalence to virgin materials.

JP7948682B2Active Publication Date: 2026-11-11LG CHEM LTD
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
JP2024519098
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2021-10-01
Filing Date
2022-09-29
Publication Date
2026-11-11
Estimated Expiration
2042-09-29

AI Technical Summary

Technical Problem

Existing transparent resins face challenges in maintaining weather resistance and mechanical properties when using chemically recycled monomers, particularly due to the inclusion of foreign matter and metals during recycling, which can decrease transparency and quality.

Method used

A transparent resin composition comprising a transparent graft copolymer with chemically recycled alkyl (meth)acrylate monomer units, a transparent matrix resin, and an ultraviolet absorber, specifically benzophenone-based or benzotriazole-based ultraviolet absorbers, to enhance weather resistance and mechanical properties.

Benefits of technology

The composition achieves excellent mechanical properties and weather resistance while reducing carbon emissions, maintaining transparency and quality comparable to virgin materials.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007948682000001
    Figure 0007948682000001
  • Figure 0007948682000002
    Figure 0007948682000002
  • Figure 0007948682000003
    Figure 0007948682000003
Patent Text Reader

Abstract

The present invention relates to a transparent resin composition which contains a transparent matrix resin containing chemically recycled monomer units, is environmentally friendly due to its carbon emission reducing effect, and has excellent mechanical properties and weather resistance, and to a molded article molded from the composition.
Need to check novelty before this filing date? Find Prior Art

Description

TECHNICAL FIELD

[0001] The present invention claims the benefit of priority based on Korean Patent Application No. 10-2021-0130840 filed on October 1, 2021, and all contents disclosed in the documents of the said Korean patent application are incorporated as part of the present specification.

[0002] The present invention relates to a transparent resin composition that includes a matrix resin containing chemically recycled monomer units, is eco-friendly due to its carbon generation reduction effect, and has excellent mechanical properties and weather resistance, as well as a molded article molded therefrom.

BACKGROUND ART

[0003] Eco-related policies and regulations are being strengthened globally. In particular, measures to recycle waste plastics to reduce carbon emissions have emerged, among which research and development on PCR (Post Consumer Recycled) materials are being carried out.

[0004] PCR materials refer not to low-cost recycled materials merely for the purpose of cost reduction, but to materials that can contribute to the environment by recycling products that have been discarded after consumers have finished using them. Methods for recycling as PCR materials can be broadly divided into mechanical recycling methods and chemical recycling methods in major categories.

[0005] Mechanical recycling methods involve crushing and washing plastic waste for recycling, and the ability to separate foreign matter and metals is crucial. Mechanical recycling methods have the advantage of significant carbon reduction due to the low consumption of thermal energy during the mechanical decomposition process for recycling. However, even with sorting during recycling, it is difficult to completely remove foreign matter and metals, resulting in a decrease in quality compared to virgin materials and difficulty in ensuring uniformity of quality. In particular, in the case of transparent resins used in products where transparency is required, the inclusion of foreign matter and metals during recycling can lead to a decrease in transparency.

[0006] Chemical recycling is a method of recycling that uses chemical processes to break down the molecular structure of plastics themselves and return them to a pure raw material state, and the pace of technological development has been accelerating in recent years. Because chemical recycling recycles materials to a pure raw material state, it has the advantage of achieving a quality level equivalent to virgin materials compared to mechanical recycling methods.

[0007] On the other hand, if transparent resins are used outdoors or continuously exposed to external light even when used indoors, a problem arises where transparency decreases if sufficient weather resistance is not ensured. Therefore, ensuring weather resistance in transparent resins is important. [Prior art documents] [Patent Documents]

[0008] [Patent Document 1] KR10-2012-0088090A [Overview of the project] [Problems that the invention aims to solve]

[0009] The problem that this invention aims to solve is to improve weather resistance by using PCR material as a transparent resin, thereby ensuring environmental friendliness, mechanical properties equivalent to those of virgin material, and solving the problems described in the background technology of the invention above.

[0010] In other words, the present invention aims to provide a transparent resin composition and molded articles formed therefrom that comprises a matrix resin containing chemically recycled monomer units, which is environmentally friendly due to its carbon emission reduction effect, and which also has excellent mechanical properties and weather resistance. [Means for solving the problem]

[0011] To solve the above problems, the present invention provides a transparent resin composition and a molded article. (1) The present invention provides a transparent resin composition comprising a transparent graft copolymer containing a rubbery polymer, a transparent matrix resin, and an ultraviolet absorber, wherein the transparent matrix resin contains chemically recycled alkyl (meth)acrylate monomer units, and the ultraviolet absorber comprises one or more selected from the group consisting of benzophenone-based ultraviolet absorbers and benzotriazole-based ultraviolet absorbers.

[0012] (2) In the present invention, the transparent graft copolymer comprises a conjugated diene rubber polymer, an alkyl (meth)acrylate monomer unit, an aromatic vinyl monomer unit, and a vinyl cyanide monomer unit, providing the transparent resin composition described in (1).

[0013] (3) The present invention provides a transparent resin composition according to (1) or (2) above, wherein the content of the transparent graft copolymer is 5 parts by weight or more and 60 parts by weight or less with respect to 100 parts by weight of the total content of the transparent graft copolymer and the transparent matrix resin.

[0014] (4) The present invention provides a transparent resin composition according to any one of (1) to (3) above, wherein the content of the transparent matrix resin is 40 parts by weight or more and 95 parts by weight or less with respect to 100 parts by weight of the total content of the transparent graft copolymer and the transparent matrix resin.

[0015] (5) The present invention provides a transparent resin composition according to any one of (1) to (4) above, wherein the transparent matrix resin comprises a first transparent matrix resin and a second transparent matrix resin, and the second transparent matrix resin comprises chemically recycled alkyl (meth)acrylate monomer units.

[0016] (6) In the present invention, the first transparent matrix resin provides the transparent resin composition described in (5) above, comprising alkyl (meth)acrylate monomer units, aromatic vinyl monomer units, and vinyl cyanide monomer units.

[0017] (7) The present invention provides the transparent resin composition described in (5) or (6) above, wherein the second transparent matrix resin comprises chemically recycled alkyl (meth)acrylate monomer units, aromatic vinyl monomer units, and vinyl cyanide monomer units.

[0018] (8) The present invention provides a transparent resin composition according to any one of (5) to (7), wherein the content of the first transparent matrix resin is 10 parts by weight or more and 70 parts by weight or less with respect to 100 parts by weight of the total content of the transparent graft copolymer and the transparent matrix resin, and the content of the second transparent matrix resin is 10 parts by weight or more and 80 parts by weight or less with respect to 100 parts by weight of the total content of the transparent graft copolymer and the transparent matrix resin.

[0019] (9) In the present invention, the chemically recycled alkyl (meth)acrylate-based monomer that forms the chemically recycled alkyl (meth)acrylate-based monomer unit is chemically recycled from waste artificial marble, and the transparent resin composition according to any one of the above (1) to (8) is provided.

[0020] (10) In the present invention, the benzophenone-based ultraviolet absorber is one or more selected from the group consisting of 2-hydroxy-4-(octyloxy)benzophenone and 2,2'-dihydroxy-4-methoxybenzophenone, and the transparent resin composition according to any one of the above (1) to (9) is provided.

[0021] (11) In the present invention, the benzotriazole-based ultraviolet absorber is 2-(2-hydroxy-5-tert-octylphenyl)benzotriazole, and the transparent resin composition according to any one of the above (1) to (10) is provided.

[0022] (12) In the present invention, the content of the ultraviolet absorber is 0.01 parts by weight or more and 1.00 parts by weight or less based on 100 parts by weight of the total content of the transparent graft copolymer and the transparent matrix resin, and the transparent resin composition according to any one of the above (1) to (11) is provided.

[0023] (13) The present invention provides a molded article molded from the transparent resin composition according to any one of the above (1) to (12). [Effects of the Invention]

[0024] The transparent resin composition according to the present invention contains a matrix resin including chemically recycled monomer units, is environmentally friendly due to the carbon emission reduction effect, and is excellent in mechanical properties and weather resistance. [Mode for Carrying Out the Invention]

[0025] Hereinafter, the present invention will be described in more detail to facilitate understanding of the present invention. The terms and words used in the description and claims of this invention should not be interpreted in a manner limited to their ordinary or dictionary meanings, but rather should be interpreted in a manner consistent with the technical idea of ​​this invention, in accordance with the principle that inventors may appropriately define the concepts of terms in order to best describe their invention.

[0026] The term "monomer unit" as used in this invention may refer to a component, structure, or the substance itself that originates from a monomer. A specific example is the repeating unit formed in a polymer when a monomer introduced during polymerization participates in the polymerization reaction.

[0027] As used in the present invention, the term "composition" includes not only reaction products and decomposition products formed from the materials of the composition, but also mixtures of materials containing the composition.

[0028] The present invention provides a transparent resin composition containing PCR material. In the present invention, the PCR material refers to PCR material obtained by a chemical recycling method using chemically recycled monomers.

[0029] According to one embodiment of the present invention, the transparent resin composition comprises a transparent graft copolymer containing a rubbery polymer, a transparent matrix resin, and an ultraviolet absorber, wherein the transparent matrix resin contains chemically recycled alkyl (meth)acrylate monomer units, and the ultraviolet absorber may contain one or more selected from the group consisting of benzophenone-based ultraviolet absorbers and benzotriazole-based ultraviolet absorbers.

[0030] According to one embodiment of the present invention, the transparent resin composition is characterized by containing a transparent matrix resin as a PCR material. When a transparent matrix resin is included as a PCR material in this way, the amount of carbon dioxide, a greenhouse gas, emitted can be reduced compared to when only a virgin transparent matrix resin is used, and this carbon emission reduction effect has the advantage of being environmentally friendly.

[0031] The conjugated diene rubber polymer described in the present invention may be a rubber polymer containing conjugated diene monomer units. As a specific example, the conjugated diene monomer that forms the conjugated diene monomer unit may be one or more selected from the group consisting of 1,3-butadiene, 2,3-dimethyl-1,3-butadiene, piperylene, 3-butyl-1,3-octadiene, isoprene, and 2-phenyl-1,3-butadiene. As a more specific example, it may be 1,3-butadiene.

[0032] The alkyl(meth)acrylate monomers for forming the alkyl(meth)acrylate monomer units described in the present invention may be C1-C18 alkyl(meth)acrylates, C1-C12 alkyl(meth)acrylates, or C1-C6 alkyl(meth)acrylates. Here, (meth)acrylate can mean acrylate or methacrylate. The C1-C18 alkyl(meth)acrylate monomer may also be methyl(meth)acrylate, and a specific example may be methyl methacrylate. Furthermore, the alkyl(meth)acrylate monomer may be a virgin monomer or a chemically recycled monomer, but unless specifically mentioned as a chemically recycled monomer, it can mean a virgin monomer.

[0033] The aromatic vinyl monomer used to form the aromatic vinyl monomer unit described in the present invention may be one or more selected from the group consisting of styrene, α-methylstyrene, 3-methylstyrene, 4-methylstyrene, 4-propylstyrene, 1-vinylnaphthalene, 4-cyclohexylstyrene, 4-(p-methylphenyl)styrene, and 1-vinyl-5-hexylnaphthalene, and a specific example may be styrene.

[0034] The vinyl cyanide monomer used to form the vinyl cyanide monomer unit described in the present invention may be one or more selected from the group consisting of acrylonitrile, methacrylonitrile, ethacrylonitrile, phenylacrylonitrile, and α-chloroacrylonitrile, and a specific example may be acrylonitrile.

[0035] According to one embodiment of the present invention, the transparent graft copolymer may contain a conjugated diene rubber polymer, alkyl (meth)acrylate monomer units, aromatic vinyl monomer units, and vinyl cyanide monomer units. As a specific example, the transparent graft copolymer may be a conjugated diene rubber polymer graft polymerized with alkyl (meth)acrylate monomers, aromatic vinyl monomers, and vinyl cyanide monomers, and may have a core-shell configuration. In this case, the core contains the conjugated diene rubber polymer, and the shell may contain alkyl (meth)acrylate monomer units, aromatic vinyl monomer units, and vinyl cyanide monomer units.

[0036] According to one embodiment of the present invention, the conjugated diene rubber polymer of the transparent graft copolymer may be included in a content of 30% or more by weight, 35% or more by weight, 40% or more by weight, or 45% or more by weight relative to the transparent graft copolymer, or in a content of 70% or less by weight, 65% or less by weight, 60% or less by weight, or 55% or less by weight. Within this range, there is an effect of having excellent mechanical properties of the transparent resin composition.

[0037] According to one embodiment of the present invention, the alkyl (meth)acrylate monomer units of the transparent graft copolymer may be present in a content of 10% or more by weight, 15% or more by weight, 20% or more by weight, 25% or more by weight, or 30% or more by weight relative to the transparent graft copolymer, or in a content of 50% or less by weight, 45% or less by weight, 40% or less by weight, or 35% or less by weight. Within this range, there is an effect of excellent compatibility with the transparent matrix resin, as well as excellent transparency and mechanical properties.

[0038] According to one embodiment of the present invention, the alkyl (meth)acrylate monomer units of the transparent graft copolymer may be formed from virgin alkyl (meth)acrylate monomers and / or chemically recycled alkyl (meth)acrylate monomers, and the eco-friendliness can be further improved when monomer units formed from chemically recycled alkyl (meth)acrylate monomers are included.

[0039] According to one embodiment of the present invention, the aromatic vinyl monomer units of the transparent graft copolymer may be present in an amount of 1% by weight or more, 3% by weight or more, 5% by weight or more, or 10% by weight or more relative to the transparent graft copolymer, or in an amount of 30% by weight or less, 25% by weight or less, 20% by weight or less, or 15% by weight or less. Within this range, there is an effect of excellent compatibility with the transparent matrix resin, as well as excellent transparency and mechanical properties.

[0040] According to one embodiment of the present invention, the vinyl cyanide monomer units of the transparent graft copolymer may be present in a content of 1% or more by weight, 2% or more by weight, 3% or more by weight, 4% or more by weight, or 5% or more by weight relative to the transparent graft copolymer, or in a content of 20% or less by weight, 15% or less by weight, 10% or less by weight, or 8% or less by weight. Within this range, there is an effect of excellent compatibility with the transparent matrix resin, as well as excellent transparency and mechanical properties.

[0041] According to one embodiment of the present invention, the refractive index of the transparent graft copolymer may be 1.500 or higher, 1.505 or higher, 1.510 or higher, or 1.515 or higher, and may also be 1.530 or lower, 1.525 or lower, 1.520 or lower, or 1.518 or lower. In this case, the refractive index can be measured using an Abbe refractometer.

[0042] According to one embodiment of the present invention, in the transparent resin composition, the content of the transparent graft copolymer may be 5 parts by weight or more and 60 parts by weight or less per 100 parts by weight of the total content of the transparent graft copolymer and the transparent matrix resin. Specifically, the content of the transparent graft copolymer may be 5 parts by weight or more, 10 parts by weight or more, 15 parts by weight or more, 20 parts by weight or more, or 25 parts by weight or more per 100 parts by weight of the total content of the transparent graft copolymer and the transparent matrix resin, or it may be 60 parts by weight or less, 55 parts by weight or less, 50 parts by weight or less, 45 parts by weight or less, 40 parts by weight or less, or 35 parts by weight or less. Within this range, the color, processability, and mechanical properties of the transparent resin composition can be adjusted according to the content of the rubbery polymer contained in the graft copolymer.

[0043] According to one embodiment of the present invention, the transparent matrix resin may contain chemically recycled alkyl (meth)acrylate monomer units, and as specific examples, it may contain chemically recycled alkyl (meth)acrylate monomer units, aromatic vinyl monomer units, and vinyl cyanide monomer units.

[0044] According to one embodiment of the present invention, the chemically recycled alkyl (meth)acrylate monomer units of the transparent matrix resin may be included in the transparent matrix resin in a content of 50% or more by weight, 55% or more by weight, 60% or more by weight, 65% or more by weight, or 58% or more by weight, or in a content of 80% or less by weight, 75% or less by weight, 70% or less by weight, or 69% or less by weight. Within this range, there is an effect of excellent compatibility with the transparent graft copolymer, as well as excellent transparency and mechanical properties.

[0045] According to one embodiment of the present invention, the aromatic vinyl monomer units of the transparent matrix resin may be present in a content of 5% by weight or more, 10% by weight or more, 15% by weight or more, or 20% by weight or more relative to the transparent matrix resin, or in a content of 40% by weight or less, 35% by weight or less, 30% by weight or less, or 25% by weight or less. Within this range, there is an effect of excellent compatibility with the transparent graft copolymer, as well as excellent transparency and mechanical properties.

[0046] According to one embodiment of the present invention, the vinyl cyanide monomer units of the transparent matrix resin may be present in a content of 1% or more by weight, 2% or more by weight, 3% or more by weight, 4% or more by weight, or 5% or more by weight relative to the transparent matrix resin, or in a content of 20% or less by weight, 15% or less by weight, 10% or less by weight, or 8% or less by weight. Within this range, there is an effect of excellent compatibility with the transparent graft copolymer, as well as excellent transparency and mechanical properties.

[0047] According to one embodiment of the present invention, the refractive index of the transparent matrix resin may be 1.500 or higher, 1.505 or higher, 1.510 or higher, or 1.515 or higher, and may also be 1.530 or lower, 1.525 or lower, 1.520 or lower, or 1.518 or lower. In this case, the refractive index can be measured using an Abbe refractometer.

[0048] According to one embodiment of the present invention, in the transparent resin composition, the content of the transparent matrix resin may be 40 parts by weight or more and 95 parts by weight or less per 100 parts by weight of the total content of the transparent graft copolymer and the transparent matrix resin. Specifically, the content of the transparent matrix resin may be 40 parts by weight or more, 45 parts by weight or more, 50 parts by weight or more, 55 parts by weight or more, 60 parts by weight or more, or 65 parts by weight or more per 100 parts by weight of the total content of the transparent graft copolymer and the transparent matrix resin, or it may be 95 parts by weight or less, 90 parts by weight or less, 85 parts by weight or less, 80 parts by weight or less, or 75 parts by weight or less. Within this range, the color, processability, and mechanical properties of the transparent resin composition can be adjusted according to the content of the rubbery polymer contained in the graft copolymer.

[0049] According to one embodiment of the present invention, the transparent matrix resin comprises a first transparent matrix resin and a second transparent matrix resin, wherein the second transparent matrix resin may contain chemically recycled alkyl (meth)acrylate monomer units. Specifically, the first transparent matrix resin may contain alkyl (meth)acrylate monomer units, aromatic vinyl monomer units, and vinyl cyanide monomer units, and the second transparent matrix resin may contain chemically recycled alkyl (meth)acrylate monomer units, aromatic vinyl monomer units, and vinyl cyanide monomer units. In this case, the first matrix resin containing virgin alkyl (meth)acrylate monomer units further improves the transparency and mechanical properties of the transparent resin composition, while the second matrix resin containing chemically recycled alkyl (meth)acrylate monomer units simultaneously ensures the advantage of being environmentally friendly.

[0050] According to one embodiment of the present invention, in the transparent resin composition, if the transparent matrix resin includes a first transparent matrix resin and a second transparent matrix resin, the content of the first transparent matrix resin may be 10 parts by weight or more and 70 parts by weight or less with respect to 100 parts by weight of the total content of the transparent graft copolymer and the transparent matrix resin, and the content of the second transparent matrix resin may be 10 parts by weight or more and 80 parts by weight or less with respect to 100 parts by weight of the total content of the transparent graft copolymer and the transparent matrix resin. As a specific example, the content of the first transparent matrix resin may be 10 parts by weight or more, 20 parts by weight or more, 25 parts by weight or more, or 30 parts by weight or more with respect to 100 parts by weight of the total content of the transparent graft copolymer and the transparent matrix resin, or it may be 70 parts by weight or less, 60 parts by weight or less, 50 parts by weight or less, or 40 parts by weight or less. Furthermore, the content of the second transparent matrix resin may be 10 parts by weight or more, 20 parts by weight or more, 25 parts by weight or more, or 30 parts by weight or more, based on 100 parts by weight of the total content of the transparent graft copolymer and the transparent matrix resin, or it may be 80 parts by weight or less, 75 parts by weight or less, 70 parts by weight or less, 60 parts by weight or less, 50 parts by weight or less, or 40 parts by weight or less. In this case, the transparency and mechanical properties of the transparent resin composition can be further improved by the first matrix resin containing virgin alkyl (meth)acrylate monomer units, while the advantage of being environmentally friendly can be simultaneously ensured by the second matrix resin containing chemically recycled alkyl (meth)acrylate monomer units.

[0051] According to one embodiment of the present invention, the chemically recycled alkyl(meth)acrylate monomers that form the chemically recycled alkyl(meth)acrylate monomer units may be chemically recycled from waste artificial marble. As a specific example, the chemically recycled alkyl(meth)acrylate monomers can be obtained by crushing waste artificial marble and separating the alkyl(meth)acrylate compound, which is the alkyl(meth)acrylate monomer, from aluminum hydroxide by thermal decomposition of the crushed waste artificial marble powder or granules. As a more specific example, the alkyl(meth)acrylate compound can be obtained by removing aluminum hydroxide, water, and other impurities at high temperature from the thermal decomposition product obtained by thermal decomposition of the waste artificial marble. The alkyl(meth)acrylate compound obtained above may undergo a distillation process via a distillation column to improve its purity. In this way, the purity of the chemically recycled alkyl(meth)acrylate monomer may be 95% or higher.

[0052] According to one embodiment of the present invention, even if the purity of the chemically recycled alkyl (meth)acrylate monomer is improved, it still contains some impurities compared to the virgin monomer, and such impurities cause a decrease in the weather resistance of the transparent resin composition. Therefore, a transparent resin composition containing a transparent matrix resin containing chemically recycled alkyl (meth)acrylate monomer units has lower weather resistance than a transparent resin composition manufactured using only virgin monomers, and in order to improve this, it is necessary to include an ultraviolet absorber as in the present invention. However, not all ultraviolet absorbers show the same level of improvement in weather resistance for a transparent resin composition containing the transparent matrix resin according to the present invention, so it is important to include an ultraviolet absorber that is particularly suitable for the transparent matrix resin according to the present invention. Typically, UV absorbers used in resins include organic UV absorbers such as benzophenone-based UV absorbers, benzotriazole-based UV absorbers, cyanoacrylate-based UV absorbers, formamidine-based UV absorbers, triazine-based UV absorbers, salicylic acid ester-based UV absorbers, and hindered amine-based UV absorbers (HALS), as well as inorganic UV absorbers such as nickel-based and cerium-based UV absorbers. However, inorganic UV absorbers are unsuitable for use in transparent resin compositions because they reduce the transparency of the transparent resin composition. Therefore, excluding inorganic UV absorbers and considering only organic UV absorbers, benzophenone-based UV absorbers, benzotriazole-based UV absorbers, and hindered amine-based UV absorbers are preferred considering compatibility with low-polarity transparent graft copolymers and transparent matrix resins, colorability, and transparency. However, hindered amine-based UV absorbers (HALS) do not have the function of blocking ultraviolet rays through a screen effect, so the improvement in weather resistance in transparent resin compositions is insufficient. As a result, the transparent resin composition of the present invention is characterized by containing one or more ultraviolet absorbers selected from the group consisting of benzophenone-based ultraviolet absorbers and benzotriazole-based ultraviolet absorbers.

[0053] According to one embodiment of the present invention, the benzophenone-based ultraviolet absorber can be any commercially available benzophenone-based ultraviolet absorber without limitation. However, considering compatibility with the transparent matrix resin according to the present invention, a specific example may be one or more selected from the group consisting of 2-hydroxy-4-(octyloxy)benzophenone and 2,2'-dihydroxy-4-methoxybenzophenone.

[0054] According to one embodiment of the present invention, the benzotriazole-based ultraviolet absorber can be any commercially available benzotriazole-based ultraviolet absorber without limitation, but considering compatibility with the transparent matrix resin according to the present invention, a specific example may be 2-(2-hydroxy-5-tert-octylphenyl)benzotriazole.

[0055] According to one embodiment of the present invention, in the transparent resin composition, the content of the ultraviolet absorber may be 0.01 parts by weight or more and 1.00 parts by weight or less per 100 parts by weight of the total content of the transparent graft copolymer and the transparent matrix resin. Specifically, the content of the ultraviolet absorber may be 0.01 parts by weight or more, 0.05 parts by weight or more, 0.10 parts by weight or more, 0.20 parts by weight or more, 0.30 parts by weight or more, 0.40 parts by weight or more, or 0.50 parts by weight or more per 100 parts by weight of the total content of the transparent graft copolymer and the transparent matrix resin, or it may be 1.00 parts by weight or less, 0.90 parts by weight or less, 0.80 parts by weight or less, 0.70 parts by weight or less, 0.60 parts by weight or less, or 0.50 parts by weight or less per 100 parts by weight of the total content of the transparent graft copolymer and the transparent matrix resin. Within this range, it is possible to prevent a decrease in the transparency and mechanical properties of the transparent resin composition and to further improve weather resistance.

[0056] The present invention provides a molded article formed from the transparent resin composition described above. According to one embodiment of the present invention, the molded article may be an extruded and / or injected molded article using the transparent resin composition, and is suitable for products that require transparency despite the possibility of being exposed to external light. [Examples]

[0057] The embodiments of the present invention will be described in detail below so that they can be easily implemented by a person with ordinary skill in the art to which the present invention pertains. However, the present invention may be realized in various different forms and is not limited to the embodiments described herein.

[0058] Manufacturing example Manufacturing Example 1: Production of Graft Copolymers A mixed solution was prepared containing 100 parts by weight of deionized water, 32 parts by weight of methyl methacrylate, 11 parts by weight of styrene, 7 parts by weight of acrylonitrile, 0.04 parts by weight of cumene hydroperoxide, 1 part by weight of sodium dodecylbenzenesulfonate, 0.3 parts by weight of t-dodecyl mercaptan, 0.048 parts by weight of sodium formaldehyde sulfoxylate, 0.012 parts by weight of ethylenediaminetetraacetic acid, and 0.001 parts by weight of ferrous sulfate.

[0059] Fifty parts by weight (based on solid content) of butadiene rubber latex (average particle size: 300 nm, refractive index: 1.516, gel content: 70% by weight) were added to a nitrogen-purged reactor. Polymerization was then carried out by continuously adding the mixed solution at a constant rate at 75°C for 5 hours. After the completion of continuous addition, the internal temperature of the reactor was raised to 80°C, and the reactor was allowed to mature for 1 hour to complete the polymerization, yielding a graft copolymer latex containing a graft copolymer. The final polymerization conversion rate was 99%.

[0060] The graft copolymer latex produced as described above was agglomerated with an aqueous calcium chloride solution, then aged, washed, dehydrated, and dried to obtain graft copolymer powder. The refractive index of the produced graft copolymer powder was 1.516.

[0061] Manufacturing Example 2: Manufacturing of the First Matrix Resin A mixed solution was prepared containing 69 parts by weight of methyl methacrylate, 24 parts by weight of styrene, 7 parts by weight of acrylonitrile, 30 parts by weight of toluene, and 0.15 parts by weight of t-dodecyl mercaptan.

[0062] The mixed solution was continuously fed into a nitrogen-purged reactor at a constant rate to maintain a residence time of 3 hours, and the reactor temperature was maintained at 148°C. The polymerization solution discharged from the reactor was heated in a preheating tank, and unreacted monomers were volatilized in a volatilization tank. Next, the mixture was extruded at 210°C using a polymer transfer pump extruder to obtain pelletized first matrix resin. The refractive index of the produced first matrix resin pellets was 1.516.

[0063] Manufacturing Example 3: Manufacturing of the Second Matrix Resin A pelletized second matrix resin was obtained using the same method as in Production Example 2, except that the methyl methacrylate was replaced with an equal amount of methyl methacrylate obtained by chemical recycling from waste artificial marble. The refractive index of the produced second matrix resin pellets was 1.516.

[0064] Examples and Comparative Examples Each of the components listed below was blended with 0.5 parts by weight of lubricant and 0.25 parts by weight of antioxidant in the amounts shown in Tables 1 to 3, and extruded in a twin-screw extruder at a cylinder temperature of 210°C to produce a pellet-shaped transparent resin composition.

[0065] In this case, the content of each component is based on a total of 100 parts by weight of the graft copolymer and matrix resin. (1) Graft copolymer: Graft copolymer produced in Production Example 1 (2) First matrix resin: The first matrix resin produced in Production Example 2 (3) Second matrix resin: Second matrix resin manufactured in manufacturing example 3

[0066] (4) UV absorber 1: 2-hydroxy-4-(octyloxy)benzophenone (GLOBAL PLANNING, Inc., BPH, CAS No. 1843-05-6)

[0067] (5) UV absorber 2: 2,2'-dihydroxy-4-methoxybenzophenone (Sigma-Aldrich, CAS No. 131-53-3)

[0068] (6) UV absorber 3: 2-(2-hydroxy-5-tert-octylphenyl)benzotriazole (GLOBAL PLANNING, Inc., UV-329, CAS No. 3147-75-9)

[0069] (7) UV absorber 4: Bis(2,2,6,6-tetramethyl-4-piperidinyl)decandioate (GLOBAL PLANNING Co., Ltd., UV-770, CAS No. 52829-07-9)

[0070] [Table 1]

[0071] [Table 2]

[0072] [Table 3]

[0073] Experimental example Experimental Example 1 The pellets produced in Examples 1 to 13 and Comparative Examples 1 to 4, and test specimens produced by injecting them using an injection machine at an injection temperature of 210°C, were used to measure transparency, melt index, impact strength, tensile properties, bending properties, and weather resistance using the following methods, and the results are shown in Tables 4 to 6 below.

[0074] *Transparency: After storing the test specimens prepared as described above at 25°C and 50±5% relative humidity for 12 hours, the total light transmittance (Tt,%) and haze (Haze,%) for a test specimen measuring 80mm × 40mm in area and 3.0mm in thickness were measured using a SUGA HZ-V3 in accordance with ASTM D1003.

[0075] *Color Coordinates: After storing the test specimens prepared as described above at 25°C and 50±5% relative humidity for 12 hours, the color coordinates (L, a, and b) in the CIE LAB color space for a 40mm × 80mm, 3.0mm thick specimen were measured using an Ultrascan PRO from Hunter Labs.

[0076] *Impact strength ( kgf·cm / cm The test specimens prepared as described above were stored for 12 hours at 25°C and 50±5% relative humidity. Then, in accordance with ASTM D256, the notched Izod impact strength at room temperature (25°C) was measured for the specimens with 1 / 4" and 1 / 8" thick notches using an IT504 / 104 from TINIUS-OLSEN.

[0077] *Melting index (g / 10min): The melting index was measured at a temperature of 220°C with a load of 10 kg using the pellets produced in Examples 1-13 and Comparative Examples 1-4, in accordance with ASTM D1238.

[0078] *Tensile properties: After storing the test specimens prepared above at 25°C and 50±5% relative humidity for 12 hours, the tensile strength of a 13mm × 115mm, 3mm thick test specimen was measured in accordance with ASTM D638 using a Zwick / Roell universal material testing machine at a crosshead speed of 50mm / min. kg / cm 2 The growth rate (%) and the percentage of growth were measured.

[0079] *Bending properties: After storing the test specimens prepared as described above at 25°C and 50±5% relative humidity for 12 hours, the bending strength (MPa) and bending modulus (MPa) of a 25mm x 80mm, 3.2mm thick test specimen were measured using a Zwich / Roell universal material testing machine in accordance with ASTM D790.

[0080] *Weather resistance (△E): After storing the test specimens prepared above at 25°C and 50±5% relative humidity for 12 hours, they were tested using AMETEK UV-A at a light intensity of 0.77 W / m². 2 The weather resistance of a test specimen measuring 40 mm x 80 mm in area and 3.2 mm in thickness was measured after exposure to ultraviolet light for 150 hours. The weather resistance was calculated using the following formula 1.

[0081] [Formula 1] △E={(L-L') 2 +(a-a') 2 +(b-b') 2} 1 / 2 In the above formula 1, L, a, and b are the color coordinates in the CIE LAB color space of the test specimen before UV exposure, and L', a', and b' are the color coordinates in the CIE LAB color space of the test specimen after UV exposure.

[0082] [Table 4]

[0083] [Table 5]

[0084] [Table 6]

[0085] As shown in Tables 4-6 above, the transparent resin compositions produced in Examples 1-7, despite containing a second matrix resin with chemically recycled monomers, exhibited comparable levels of transparency and processability to the transparent resin composition of Comparative Example 1, which was produced using only virgin monomers and did not contain UV absorbers. Furthermore, it was confirmed that they exhibited superior mechanical properties as well as weather resistance.

[0086] In particular, the transparent resin compositions of Examples 1 to 5 and Example 7, which were manufactured containing a benzophenone-based UV absorber, were found to exhibit even greater transparency compared to the transparent resin composition of Example 6, which was manufactured containing a benzotriazole-based UV absorber.

[0087] Furthermore, although the transparent resin composition of Example 7 does not contain a first matrix resin manufactured using only virgin monomers as the matrix resin, and only contains a second matrix resin containing chemically recycled monomers, it was confirmed that it exhibits equivalent levels of transparency, processability, mechanical properties, and weather resistance compared to the transparent resin composition of Example 2, which contains a first matrix resin and the same amount of benzophenone-based UV absorber.

[0088] Furthermore, from Examples 8 to 13, in which the content of the graft copolymer in the transparent resin composition was changed compared to Example 2, it was confirmed that the b value, processability, and mechanical properties change depending on the content of the rubbery polymer contained in the graft copolymer. However, it was confirmed that this is due to the content of the rubbery polymer contained in the graft copolymer, and that the transparency provided by the second matrix resin containing chemically recycled monomers and the weather resistance improvement effect provided by the benzophenone-based UV absorber are maintained at equivalent levels.

[0089] In contrast, the transparent resin composition of Comparative Example 2, which further contains a benzophenone-based ultraviolet absorber compared to the transparent resin composition of Comparative Example 1, showed some improvement in weather resistance due to the presence of the benzophenone-based ultraviolet absorber. However, it was confirmed that the improvement in weather resistance was not as significant as that of the transparent resin compositions of Examples 1 to 13.

[0090] Furthermore, it was confirmed that the transparent resin composition of Comparative Example 3, which contains the same amount of a second matrix resin containing chemically recycled monomers as in Examples 1 to 6, but does not contain an ultraviolet absorber, exhibits significantly lower weather resistance compared to the transparent resin composition of Comparative Example 1.

[0091] Furthermore, the transparent resin composition of Comparative Example 4, which includes a second matrix resin containing chemically recycled monomers as in Examples 1-6 and contains a HALS (hindered amine light stabilizer) type UV absorber as an UV absorber, showed slightly improved weather resistance compared to the transparent resin composition of Comparative Example 3, but it was confirmed that its weather resistance was still lower than that of the transparent resin composition of Comparative Example 1.

[0092] These results indicate that when a transparent resin composition containing a second matrix resin with chemically recycled monomers does not contain an ultraviolet absorber, as in the transparent resin composition of Comparative Example 3, its weather resistance rapidly deteriorates. Furthermore, even when an ultraviolet absorber is included to address this issue, unlike in the present invention, the weather resistance cannot be sufficiently improved unless a suitable ultraviolet absorber is included.

[0093] On the other hand, separate from the above experiments, the carbon footprint was calculated from the amount of carbon dioxide (unit: kgCO2 / kg), a greenhouse gas, generated during the production of the transparent resin composition using Examples 1 to 6. The results showed that the amount of carbon dioxide generated during the production of the transparent resin composition using Comparative Example 1 was reduced by at least 7% by weight.

[0094] These results confirm that the transparent resin composition according to the present invention contains a matrix resin containing chemically recycled monomer units, is environmentally friendly due to its carbon emission reduction effect, and has excellent mechanical properties and weather resistance.

Claims

1. The material comprises a transparent graft copolymer containing a rubbery polymer, a transparent matrix resin, and an ultraviolet absorber. The transparent matrix resin contains alkyl (meth)acrylate monomer units having 1 to 18 carbon atoms, which are chemically recycled from waste artificial marble. The aforementioned ultraviolet absorber is 2-hydroxy-4-(octyloxy)benzophenone, The content of the ultraviolet absorber is 0.10 parts by weight or more and 1.00 parts by weight or less, based on 100 parts by weight of the total content of the transparent graft copolymer and the transparent matrix resin. A transparent resin composition in which the content of the transparent graft copolymer is 5 parts by weight or more and 40 parts by weight or less, based on 100 parts by weight of the total content of the transparent graft copolymer and the transparent matrix resin.

2. The transparent resin composition according to claim 1, wherein the transparent graft copolymer comprises a conjugated diene rubber polymer, an alkyl (meth)acrylate monomer unit, an aromatic vinyl monomer unit, and a vinyl cyanide monomer unit.

3. The transparent resin composition according to claim 1, wherein the content of the transparent graft copolymer is 5 parts by weight or more and 35 parts by weight or less with respect to 100 parts by weight of the total content of the transparent graft copolymer and the transparent matrix resin.

4. The transparent resin composition according to claim 1, wherein the content of the transparent matrix resin is 40 parts by weight or more and 95 parts by weight or less with respect to 100 parts by weight of the total content of the transparent graft copolymer and the transparent matrix resin.

5. The transparent matrix resin comprises a first transparent matrix resin and a second transparent matrix resin. The transparent resin composition according to claim 1, wherein the second transparent matrix resin comprises chemically recycled alkyl (meth)acrylate monomer units.

6. The transparent resin composition according to claim 5, wherein the first transparent matrix resin comprises alkyl (meth)acrylate monomer units, aromatic vinyl monomer units, and vinyl cyanide monomer units.

7. The transparent resin composition according to claim 5, wherein the second transparent matrix resin comprises chemically recycled alkyl (meth)acrylate monomer units, aromatic vinyl monomer units, and vinyl cyanide monomer units.

8. The content of the first transparent matrix resin is 10 parts by weight or more and 70 parts by weight or less, based on 100 parts by weight of the total content of the transparent graft copolymer and the transparent matrix resin. The transparent resin composition according to claim 5, wherein the content of the second transparent matrix resin is 10 parts by weight or more and 80 parts by weight or less with respect to 100 parts by weight of the total content of the transparent graft copolymer and the transparent matrix resin.

9. A molded article formed from the transparent resin composition described in any one of claims 1 to 8.

Citation Information

Patent Citations

  • Transparent thermoplastic resin composition and molded product

    JP2005263902A

  • Rubber-reinforced resin composition and its molding and laminate

    JP2008156577A

  • Optical film and method for manufacturing the same

    JP2009084574A

  • MMA and Alumina recovery system from waste artificial marble, and recovery method thereof

    KR101579116B1

  • Thermoplastic resin having good flame retardancy and transparence

    KR1020120088090A