Vapor deposition mask

The vapor deposition mask with a low thermal expansion frame and adhesive joints addresses warping and deformation issues, maintaining accuracy and reducing costs by using standard metal sheets.

JP7953794B2Active Publication Date: 2026-11-19KYUSHU SONOCOM CO LTD
View PDF 12 Cites 0 Cited by

Patent Information

Application Number
JP2025081696
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2025-05-15
Publication Date
2026-11-19
Estimated Expiration
2036-05-23

AI Technical Summary

Technical Problem

Existing vapor deposition masks face issues with warping and deformation due to thermal expansion, leading to reduced reproducibility and deposition accuracy, especially when enlarged, and the use of Invar material increases manufacturing costs.

Method used

A vapor deposition mask design featuring a mask body with a reinforcing frame made of metal plates with low thermal expansion, joined by adhesive layers, and specific frame dimensions to minimize thermal expansion differences, ensuring flatness and accuracy.

Benefits of technology

The design suppresses distortion and maintains flatness, ensuring high reproducibility and deposition accuracy while keeping manufacturing costs low by using commonly available metal sheets, even for larger masks.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007953794000001
    Figure 0007953794000001
  • Figure 0007953794000002
    Figure 0007953794000002
  • Figure 0007953794000003
    Figure 0007953794000003
Patent Text Reader

Abstract

To suppress generation of a distortion attributed to a thermal expansion by reducing a difference in an expansion amount due to heat in a frame in a vapor deposition mask.SOLUTION: A vapor deposition mask includes: a mask body 2 including a vapor deposition pattern 6 composed of multiple independent vapor deposition holes 5; and a frame body 3 for reinforcement, the frame body being arranged so as to surround the mask body 2 and made of a metal material with a low thermal linear expansion coefficient. The frame body 3 is constituted by an upper frame 16 and a lower frame 17. The upper frame 16 and the lower frame 17 are composed of a metal material with a low thermal linear expansion coefficient. The upper frame 16 and the lower frame 17 are integrated by bonding via an adhesion layer 18. The upper frame 16 and the lower frame 17 are bonded in a state where convex arc faces or concave arc faces are faced with each other.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to Regarding vapor deposition masks (metal masks).

Background Art

[0002] In mobile devices such as smartphones and tablet terminals equipped with display devices, for the purpose of reducing the weight of the devices and extending their operating time, the adoption of lighter and lower power consumption organic EL displays has started to replace liquid crystal displays. An organic EL display is manufactured by forming a light-emitting layer (vapor deposition layer) of an organic EL element on a substrate (vapor deposition target) by a vapor deposition mask method. At this time, by using an enlarged vapor deposition mask provided with a larger number of mask main bodies to manufacture more products in a single vapor deposition operation, the manufacturing cost of the organic EL display can be reduced. For this reason, demands from manufacturers of organic EL displays for larger vapor deposition masks are increasing.

[0003] A vapor deposition mask used in the vapor deposition mask method is disclosed in, for example, Patent Document 1. In such Patent Document 1, the vapor deposition mask is constituted by a metal mask (mask main body) provided with a plurality of mask portions (vapor deposition patterns), and a frame (frame body) made of Invar material formed in a frame shape to fix and hold the metal mask in a tensioned state. The metal mask is joined to the frame by spot welding.

[0004] This type of vapor deposition mask has also been proposed by the present applicant, and is disclosed in, for example, Patent Document 2. Such a vapor deposition mask consists of a plurality of mask main bodies provided with vapor deposition patterns, and a reinforcing frame body integrally and inseparably joined to the mask main bodies. The frame body is formed of an Invar material (a material with a low coefficient of linear thermal expansion), and the outer peripheral edge of each mask main body is joined to the frame body surrounding the mask main body by a metal layer formed by electroforming.

Prior Art Documents

Patent Documents

[0005] [Patent Document 1] Japanese Patent Publication No. 2004-323888 [Patent Document 2] Japanese Patent Publication No. 2005-15908 [Overview of the project] [Problems that the invention aims to solve]

[0006] As with the deposition masks described in Patent Documents 1 and 2, by constructing the frame that fixes and holds the metal mask, and the frame that reinforces the mask body, from Invar material, it is possible to suppress the expansion of the deposition mask even in high-temperature environments during deposition, thereby ensuring the reproducibility and deposition accuracy of the deposition layer (luminescent layer). However, in the deposition mask of Patent Document 1, although the metal mask is fixed and held in place by the frame under tension, when the deposition mask is enlarged, the area of ​​the metal mask not supported by the frame increases, causing the metal mask to warp and deform due to its own weight. Therefore, a decrease in reproducibility and deposition accuracy is unavoidable.

[0007] In this respect, in the vapor deposition mask of Patent Document 2, each mask body is joined to a frame surrounding the mask body, so even if the vapor deposition mask is enlarged, warping deformation of the mask body due to its own weight does not occur, and the reproducibility accuracy of the vapor deposition layer and the vapor deposition accuracy can be ensured. However, even if the frame is made of Invar material, it expands slightly during the vapor deposition process. In addition, the frame is formed from Invar metal sheets, but since metal sheets that are commonly available have thickness deviations, there is variation in thickness depending on the part of the frame. As a result, the amount of expansion differs in each part of the frame, and the difference in the amount of expansion may appear as distortion of the entire vapor deposition mask. When distortion occurs in the vapor deposition mask in this way, the flatness of the vapor deposition mask deteriorates, and the reproducibility accuracy and vapor deposition accuracy are severely reduced. This distortion becomes more pronounced as the size of the frame increases. The occurrence of such distortion originating from the thickness deviation of the base material can be suppressed by controlling the manufacturing process of the metal sheet material and manufacturing and using a base material with a small thickness deviation, but this makes the base material more expensive, leading to an increase in the manufacturing cost of the vapor deposition mask. Here, plate thickness deviation refers to the variation in thickness relative to the standard dimensions of a metal sheet material.

[0008] The objective of the present invention is, In a vapor deposition mask, the frame By minimizing the difference in the amount of thermal expansion, the generation of distortion caused by thermal expansion is suppressed. Conquer It is about that. The objective of the present invention is, To achieve larger masks while keeping manufacturing costs down and maintaining the flatness of the masks. It is possible. To obtain a deposition mask that can ensure the reproducibility and deposition accuracy of the deposited layer. Located . [Means for solving the problem]

[0009] The vapor deposition mask of the present invention comprises a mask body 2 having a vapor deposition pattern 6 consisting of a large number of independent vapor deposition holes 5, and a reinforcing frame 3 made of a metal plate material with a low coefficient of thermal expansion, arranged around the mask body 2. The frame 3 consists of an upper frame 16 and a lower frame 17. The upper frame 16 and the lower frame 17 are made of a metal material with a low coefficient of thermal expansion. The upper frame 16 and the lower frame 17 are joined together via an adhesive layer 18. The upper frame 16 and the lower frame 17 are joined with their protruding or concave surfaces facing each other.

[0010] Multiple frame bodies 3·3 are stacked, and adjacent frame bodies 3·3 in the stacking direction are joined together via an adhesive layer 19.

[0011] The mask body 2 is formed in a rectangular shape, and multiple mask bodies 2 are arranged in a matrix. The frame 3 comprises an outer frame 10 and grid-like vertical frames 12 and horizontal frames 13 that partition multiple mask openings 11 within the outer frame 10. When the width dimension of the vertical frame 12 parallel to the long side of the mask body 2 is W1, and the width dimension of the horizontal frame 13 parallel to the short side of the mask body 2 is W2, the width dimension W1 of the vertical frame 12 and the width dimension W2 of the horizontal frame 13 are set to satisfy the inequality (W1 ≤ W2 ≤ W1 × 1.1). [Effects of the Invention]

[0012] The vapor deposition mask according to the present invention reduces the difference in the amount of thermal expansion in each part of the frame 3, thereby suppressing the occurrence of distortion in the frame 3 caused by thermal expansion. Specifically, the thickness deviation of commonly available metal sheet material, which is the base material of the frame 3, tends to decrease as the thickness decreases, because the number of times it passes through the rolling mill in the manufacturing process increases as its thickness decreases. Therefore, by constructing the frame 3 with an upper frame 16 and a lower frame 17, and joining the upper and lower frames 16 and 17 together via an adhesive layer 18, it is possible to form the frame 3 using a thinner metal sheet material when forming a frame 3 of the same thickness as conventional frames, thereby reducing the overall thickness deviation of the frame 3. As a result, even with large vapor deposition masks, the occurrence of distortion due to thermal expansion caused by the thickness deviation of the metal sheet material can be suppressed. Furthermore, since only commonly available thin metal sheet material is used as the base material, there is no need to use a special metal sheet material to form the frame 3. As described above, according to the present invention, it is possible to enlarge the vapor deposition mask while suppressing the increase in manufacturing costs, and furthermore, the flatness of the vapor deposition mask can be maintained, ensuring good reproducibility and vapor deposition accuracy of the vapor-deposited layer. In addition, with the frame 3 having an adhesive layer 18 interposed between the upper frame 16 and the lower frame 17, when an external force that causes bending deformation is applied to the vapor deposition mask, the frame 3 flexibly and elastically deforms by the amount of the adhesive layer 18, effectively preventing damage to the vapor deposition mask.

[0013] By stacking multiple frame bodies 3, 3 and joining adjacent frame bodies 3, 3 in the stacking direction via adhesive layers 19, it is possible to form frame bodies 3 using even thinner metal sheets when forming frame bodies 3 of the same thickness as conventional methods. This further suppresses the generation of distortion due to thermal expansion resulting from thickness deviations of the metal sheets. Consequently, it is possible to enlarge the vapor deposition mask, maintain the flatness of the vapor deposition mask, and ensure better reproduction accuracy and vapor deposition accuracy of the vapor-deposited layer. In addition, the increased number of adhesive layers 18, 19 joining the frame bodies 3 allows for more flexible elastic deformation against external forces, thus more effectively preventing damage to the vapor deposition mask.

[0014] By joining the upper frame 16 and the lower frame 17 in a state where the two-dimensional or three-dimensional curved curvatures cancel each other out, the frame body 3 can be formed into a flat shape. This eliminates slight curvature originating from the metal plate material, further improving flatness and ensuring even better reproduction accuracy and deposition accuracy of the deposited layer.

[0015] By setting the width dimension W1 of the vertical frame 12 and the width dimension W2 of the horizontal frame 13 to satisfy the inequality (W1 ≤ W2 ≤ W1 × 1.1), the cross-sectional area of ​​the horizontal frame 13 can be made the same as or larger than the cross-sectional area of ​​the vertical frame 12. Furthermore, since the length of the horizontal frame 13 is smaller than the length of the vertical frame 12, the vertical frame 12 can be firmly supported by the horizontal frame 13, preventing the long vertical frame 12 from bending and deforming due to its own weight. Consequently, deformation of the frame 3 due to its own weight can be prevented, enabling a larger deposition mask, maintaining the flatness of the deposition mask, and improving the reproducibility and deposition accuracy of the deposition layer. In addition, since the rigidity of the vertical frame 12 and the horizontal frame 13 can be made approximately uniform overall, when an external force that causes bending deformation of the deposition mask 1 is applied, the external force can be evenly distributed, eliminating localized concentration and effectively preventing deformation and damage to the deposition mask 1. In addition, by setting the width dimension W2 of the horizontal frame 13 to (W2 ≤ W1 × 1.1), the increase in weight of the frame 3 due to an unnecessarily large cross-sectional area of ​​the horizontal frame 13 is suppressed, thereby preventing the overall weight of the deposition mask from becoming unnecessarily large while increasing the structural strength and rigidity of the frame 3. [Brief explanation of the drawing]

[0016] [Figure 1] It is a longitudinal front view showing the main part of the vapor deposition mask according to the first embodiment of the present invention. [Figure 2] It is a perspective view showing the entire vapor deposition mask according to the first embodiment of the present invention. [Figure 3] It is a longitudinal side view of the vapor deposition mask according to the first embodiment of the present invention. [Figure 4] It is a plan view showing the main part of the vapor deposition mask according to the first embodiment of the present invention. [Figure 5] It is a plan view of the frame body of the vapor deposition mask according to the first embodiment of the present invention. [Figure 6] It is an explanatory view showing the preceding stage of the frame body forming step in the method for manufacturing a vapor deposition mask according to the first embodiment of the present invention. [Figure 7] It is an explanatory view showing the subsequent stage of the frame body forming step in the method for manufacturing a vapor deposition mask according to the first embodiment of the present invention. [Figure 8] It is an explanatory view showing the primary patterning step and the first electroforming step in the method for manufacturing a vapor deposition mask according to the first embodiment of the present invention. [Figure 9] It is an explanatory view showing the activation treatment step in the method for manufacturing a vapor deposition mask according to the first embodiment of the present invention. [Figure 10] It is an explanatory view showing the secondary patterning step, the frame body arranging step, the second electroforming step, and the peeling step in the method for manufacturing a vapor deposition mask according to the first embodiment of the present invention. [Figure 11] It is a longitudinal front view showing the main part of the vapor deposition mask according to the second embodiment of the present invention. [Figure 12] It is an explanatory view showing the frame body arranging step, the second electroforming step, and the peeling step of the vapor deposition mask according to the second embodiment of the present invention. [Figure 13] It is a longitudinal front view showing the main part of the vapor deposition mask according to the third embodiment of the present invention. [Figure 14] It is an explanatory view showing the primary patterning step and the first electroforming step in the method for manufacturing a vapor deposition mask according to the third embodiment of the present invention. [Figure 15]This is an explanatory diagram showing the secondary patterning step, frame assembly step, second electroforming step, and peeling step in the manufacturing method of a vapor deposition mask according to the third embodiment of the present invention. [Figure 16] This is a longitudinal cross-sectional front view showing the main part of a deposition mask according to the fourth embodiment of the present invention. [Figure 17] This is an explanatory diagram showing a method for manufacturing a vapor deposition mask according to the fourth embodiment of the present invention. [Figure 18] This is a longitudinal cross-sectional front view showing a deposition mask according to a fifth embodiment of the present invention. [Figure 19] This is an exploded perspective view of a deposition mask according to a fifth embodiment of the present invention. [Figure 20] This is a plan view of a vapor deposition mask according to a fifth embodiment of the present invention. [Figure 21] This is an exploded perspective view showing a modified example of the deposition mask according to the fifth embodiment of the present invention. [Modes for carrying out the invention]

[0017] (First Embodiment) Figures 1 to 10 show the first embodiment of the vapor deposition mask and its manufacturing method according to the present invention. Note that the dimensions such as thickness and width in Figures 1 to 10 of this embodiment do not represent the actual dimensions, but are shown schematically. The same applies to the figures of the following embodiments.

[0018] As shown in Figures 2 and 3, the deposition mask 1 includes a plurality of mask bodies 2 and a reinforcing frame 3 arranged around the mask bodies 2. The mask bodies 2 are formed in a rectangular shape with rounded corners and have a pattern forming region 4 inside. A deposition pattern 6 consisting of a large number of independent deposition holes 5 is formed in the pattern forming region 4. As shown in Figure 4, the mask body 2 is provided with a large number of joining holes 7 around the entire circumference of the outer edge 4a of the pattern forming region 4.

[0019] The mask body 2 is formed by electroforming using an electrodeposited metal made of nickel as the material. The thickness of the mask body 2 is preferably in the range of 10 to 20 μm, and in this embodiment it is set to 12 μm. In addition, the dimensions of the mask body 2 in a plan view are set to 108 mm in the longitudinal direction and 62 mm in the transverse direction, and 30 mask bodies 2 are arranged in a matrix of 6 rows and 5 columns. The mask body 2 can be formed from materials other than nickel, such as nickel-cobalt alloys or other electrodeposited metals. When the vapor deposition mask 1 of this embodiment is applied as a vapor deposition mask for an organic EL element, the vapor deposition pattern 6 is formed to correspond to the light-emitting layer of the organic EL element.

[0020] As shown in Figure 5, the frame 3 comprises an outer frame 10 and grid-like vertical frames 12 and horizontal frames 13 that demarcate the mask opening 11 within the outer frame 10. The vertical frames 12 are provided parallel to the long side of the mask body 2, and the horizontal frames 13 are provided parallel to the short side of the mask body 2. In this embodiment, the frame 3 is made of a metal plate material with a low coefficient of thermal expansion, which is made of Invar, a nickel-iron alloy, and is formed to be sufficiently thicker than the mask body 2, with a thickness of 1.6 mm. In plan view, the dimensions of the frame 3 are set to 460 × 730 mm, and the dimensions of the mask opening 11 are set to 110 mm in the longitudinal direction and 64 mm in the short direction. The frame 3 may also be made of Super Invar, a nickel-iron-cobalt alloy, and its thickness can be set to, for example, about 1 to 5 mm. Furthermore, the reason for using Invar material or Super Invar material as the forming material for the frame 3 is that its coefficient of thermal expansion is extremely small, which effectively suppresses dimensional changes in the mask body 2 due to thermal effects during the vapor deposition process.

[0021] When the width dimension of the vertical frame 12 is W1 and the width dimension of the horizontal frame 13 is W2, the width dimension W1 of the vertical frame 12 and the width dimension W2 of the horizontal frame 13 are set to satisfy the inequality (W1 ≤ W2 ≤ W1 × 1.1). In this embodiment, the width dimension W1 of the vertical frame 12 is set to 10 mm and the width dimension W2 of the horizontal frame 13 is set to 10.64 mm. By setting the width dimension W2 of the horizontal frame 13 to be larger than the width dimension W1 of the vertical frame 12 in this way, the cross-sectional area of ​​the horizontal frame 13 can be made larger than the cross-sectional area of ​​the vertical frame 12, and since the length of the horizontal frame 13 is smaller than the length of the vertical frame 12, the vertical frame 12 can be firmly supported by the horizontal frame 13, preventing the long vertical frame 12 from bending and deforming due to its own weight. Therefore, deformation of the frame body 3 due to its own weight can be prevented, enabling a larger vapor deposition mask 1, and furthermore, the flatness of the vapor deposition mask 1 can be maintained, and the reproduction accuracy of the vapor deposition pattern and the vapor deposition accuracy can be improved. Furthermore, since the rigidity of the vertical frame 12 and horizontal frame 13 can be made nearly uniform overall, when an external force that causes the deposition mask 1 to bend or deform is applied, the external force is evenly distributed, eliminating localized concentration and effectively preventing deformation or damage to the deposition mask 1. In addition, since the width dimension W2 of the horizontal frame 13 is set to (W2 ≤ W1 × 1.1), the increase in weight of the frame 3 due to an unnecessarily large cross-sectional area of ​​the horizontal frame 13 is suppressed, thereby increasing the structural strength and rigidity of the frame 3 while preventing the overall weight of the deposition mask from becoming unnecessarily large.

[0022] As shown in Figures 1 and 6(a), the frame 3 is composed of an upper frame 16 and a lower frame 17, which are formed to the same thickness and shape, and the upper frame 16 and the lower frame 17 are joined and integrated via an adhesive layer 18. More specifically, as shown in Figure 6(b), the upper frame 16 and the lower frame 17 are joined with their protruding curved surfaces facing each other, so that the two-dimensional curved curvature is canceled out and the frame 3 is formed to be flat. Note that the two-dimensional curved curvature is a slight curvature originating from the metal sheet material, and there may also be a three-dimensional curved curvature. In this embodiment, the adhesive layer 18 is made of a sheet of uncured photosensitive dry film resist, and after joining the upper frame 16 and the lower frame 17, the excess adhesive layer 18 is removed. Various commercially available adhesives may be used for the adhesive layer 18. The reason the upper and lower frames 16 and 17 constituting the frame 3 have the same thickness is to facilitate the formation of a flat frame 3 by joining them in a state where the two-dimensional curved curvature cancels out. The protruding arc surface may also be a concave arc surface, or it may include both. However, the thickness dimensions of the upper and lower frames 16 and 17 do not need to be different as long as they can be joined in a flat state with the two-dimensional curved curvature canceling out.

[0023] As described above, by joining the upper frame 16 and the lower frame 17 in a state where the two-dimensional curved warping cancels each other out, the frame body 3 can be formed into a flat shape. This eliminates slight warping originating from the metal plate material, further improving flatness and ensuring even better reproduction accuracy and deposition accuracy of the deposited layer.

[0024] As shown in Figure 1, in this embodiment, a pair (or more) of frame bodies 3·3 formed by the above method were stacked, and adjacent frame bodies 3·3 in the stacking direction were joined together via an adhesive layer 19. The thickness dimensions of the upper and lower frames 16·17 constituting the upper frame body 3 were set to 0.3 mm each, and the thickness dimensions of the upper and lower frames 16·17 constituting the lower frame body 3 were set to 0.5 mm each.

[0025] In Figure 1, reference numeral 8 indicates a metal layer formed on the upper surface of the outer edge 4a of the pattern-forming region 4 of the mask body 2. The metal layer 8 is formed by layering nickel using electroforming. Each mask body 2 is placed in the mask opening 11, and the outer edge 4a of the pattern-forming region 4 of the mask body 2 is inseparably joined to the frame 3 by the metal layer 8 formed by electroforming. As shown in Figures 1 and 4, the metal layer 8 is formed in a hat-shape in cross-section, extending across the upper surface of the outer edge 4a of the pattern-forming region 4, the upper surface of the frame 3, the side surface facing the pattern-forming region 4, and the gap between the mask body 2 and the frame 3. The metal layer 8 is also formed inside the joining through-hole 7, thereby improving the bonding strength between the mask body 2 and the frame 3. In addition to nickel, the metal layer 8 can be formed using nickel alloys such as nickel-cobalt or other electrodeposited metals as the material.

[0026] Figures 6 to 10 show the manufacturing method of the deposition mask 1 according to this embodiment, in which, first, a frame formation step is performed to form a reinforcing frame 3.

[0027] (Frame formation process) First, a cutting process is performed to cut the metal sheet material to the size of the upper frame 16 and lower frame 17, for example, using a wire electrical discharge machine or the like, which has minimal thermal influence on the metal sheet material. Next, a mask opening formation process is performed to form multiple openings that will become the mask opening 11 by etching or laser processing on the cut-out upper frame 16 and lower frame 17, as shown in Figure 6(a). Then, as shown in Figure 6(b), a joining process is performed to form the frame body 3 in a flat state by joining the two frames 16 and 17 with an adhesive layer 18, with the protruding curved surfaces of the upper frame 16 and lower frame 17, which originate from the metal sheet material, facing each other, so that the two-dimensional curved warp is canceled out. The adhesive layer 18 consists of a sheet-like uncured photosensitive dry film resist.

[0028] Next, as shown in Figure 6(c), a fixing process is performed in which the mask is passed between upper and lower rolling rolls 22-22 positioned at a predetermined distance between the rolls and then clamped. Furthermore, the frame 3 is obtained by removing (developing) the unnecessary portion of the adhesive layer 18 (the portion exposed outside the mask opening 11 and the outer peripheral frame 10). The reason for using a sheet-like uncured photosensitive dry film resist for the adhesive layer 18 is that the uncured photosensitive dry film resist has adhesive properties and is also a material used in the primary patterning process described later, so there is no need to prepare a separate commercially available adhesive, and thus the manufacturing cost of the deposition mask 1 can be reduced. In the cutting process, the upper and lower frames 16-17 can also be cut out while cooling the metal plate material using a laser cutting machine.

[0029] A pair of frame bodies 3·3 are manufactured from metal plates of different thicknesses by performing the above steps, as shown in Figure 7(a). These frame bodies 3·3 are stacked as shown in Figure 7(b), and the frame bodies 3·3 are joined together with an adhesive layer 19 made of a sheet of uncured photosensitive dry film resist. After this, a stacking process is performed in which the frame bodies are passed and compressed between upper and lower rolling rolls 22·22 positioned at a predetermined distance between the rolls, as shown in Figure 7(c). This gives the stacked pair of frame bodies 3·3.

[0030] (Patterning pre-processing step) As shown in Figure 8(a), a photoresist layer 25 is formed on the surface of a conductive matrix 24 made of, for example, stainless steel or brass. This photoresist layer 25 is formed by laminating one or more negative-type sheet-like photosensitive dry film resists and heat-pressing them to a predetermined thickness. Next, a pattern film 26 (glass mask) having light-transmitting holes 26a corresponding to deposition holes 5 and bonding holes 7 (primary patterning) is placed in close contact with the photoresist layer 25 to obtain a patterning pre-stage body 27.

[0031] (Preheating process) The patterning pre-assembly unit 27 is preheated to the furnace temperature of the ultraviolet irradiation device used during exposure, for example, using a heater plate or a preheating furnace. In parallel with the preheating of the patterning pre-assembly unit 27, the furnace of the ultraviolet irradiation device is also preheated to the furnace temperature used during exposure. Preheating of the furnace of the ultraviolet irradiation device is performed by turning on the ultraviolet lamp 28 with the object to be irradiated not placed inside the furnace, or with a dummy mold (mold + photoresist layer + protective film) placed inside. The patterning pre-assembly unit 27 and the furnace are preheated to, for example, 23±3℃. Incidentally, the maximum temperature inside the furnace of the ultraviolet irradiation device during exposure is around 26℃.

[0032] (Primary patterning process) Once the preheating of the furnace of the ultraviolet irradiation device and the patterning pre-stage body 27 is complete, the patterning pre-stage body 27 is placed inside the furnace of the ultraviolet irradiation device, and exposure is performed by irradiating it with ultraviolet light from the ultraviolet light lamp 28, as shown in Figure 8(a), followed by development and drying processes. Next, by dissolving and removing the unexposed portions, a primary pattern resist 29 having resist bodies 29a corresponding to the deposition holes 5 and bonding holes 7 is formed on the matrix 24, as shown in Figure 8(b). In this way, by performing the exposure work with the furnace of the ultraviolet irradiation device and the patterning pre-stage body 27 preheated to the furnace temperature for the exposure work, it is possible to eliminate the problem of the patterning pre-stage body 27 being heated and expanding by ultraviolet irradiation, causing the relative positional relationship of the three components 24, 25, and 26 to shift during the exposure work. Therefore, it is possible to create a primary pattern resist 29 on the matrix 24 with good positional accuracy and in the intended shape, contributing to improved reproduction accuracy of the deposition layer and high deposition accuracy.

[0033] (First electroforming process) Next, the master mold 24 was placed in an electroforming bath prepared with an electroforming solution at a temperature of 40-50°C. As shown in Figure 8(c), an electrodeposited metal made of nickel was primary electroformed onto the surface of the master mold 24 that was not covered by the resist body 29a, within the height range of the resist body 29a, to form a primary electroformed layer 30, i.e., a layer that would become the mask body 2. Next, by dissolving and removing the resist body 29a, a mask body 2 was obtained, as shown in Figure 8(d), which had a deposition pattern 6 consisting of numerous independent deposition holes 5 and bonding holes 7. In Figure 8(d), reference numeral 30a indicates the primary electrodeposited layer formed between the mask bodies 2 and 2, which will be removed in the peeling process described later.

[0034] (Activation process) As shown in Figure 9(a), a photoresist layer 33 is formed on the entire surface of the primary electroformed layers 30 and 30a. Then, a pattern film 34 having light-transmitting holes 34a corresponding to the periphery of the bonding holes 7 is placed in close contact with the surface and placed in the furnace of an ultraviolet irradiation device. The surface is exposed by irradiation with ultraviolet light from an ultraviolet lamp 28, followed by development and drying. The photoresist layer 33 here is formed by laminating one or more negative-type sheet-shaped photosensitive dry film resists and heat-pressing them together to a predetermined thickness, as described above. Next, the unexposed portion of the photoresist layer 33 is dissolved and removed to obtain a pattern resist 35 having openings 35a corresponding to the periphery of the bonding holes 7, as shown in Figure 9(b). In other words, the pattern resist 35 is formed so that only the periphery of the bonding holes 7 is exposed on the surface.

[0035] Next, the portion of the primary electroformed layer 30 exposed at the opening 35a of the pattern resist 35, i.e., the primary electroformed layer 30 around the joining hole 7, was subjected to activation treatment such as acid immersion or electrolytic treatment, and the pattern resist 35 was further dissolved and removed as shown in Figure 9(c). In Figure 9(c), reference numeral 36 indicates the portion that underwent activation treatment, and more specifically, the inner wall surface of the joining hole 7 and the upper surface of the primary electroformed layer 30 around the joining hole 7 were subjected to activation treatment. By performing activation treatment around the joining hole 7 in this way, the bonding strength between the primary electroformed layer 30 and the metal layer 8 formed in the second electroforming process described later can be significantly improved compared to the case without treatment. Alternatively, instead of the above activation treatment, a thin layer of strike nickel or matte nickel may be formed on the primary electroformed layer 30 around the joining hole 7. This also improves the bonding strength between the portion around the joining hole 7 and the metal layer 8.

[0036] (Secondary patterning process and frame assembly process) As shown in Figure 10(a), a photoresist layer 38 is formed on the entire surface of the matrix 24, including the portion where the primary electroformed layers 30·30a are formed. This photoresist layer 38 is formed by laminating one or more negative-type sheet-like photosensitive dry film resists and heat-pressing them together to achieve a predetermined thickness, as described above. Next, a pattern film 39 having light-transmitting holes 39a corresponding to the pattern formation region 4 is placed in close contact with the pattern film and placed in the furnace of an ultraviolet irradiation device. The pattern film is exposed by irradiating it with ultraviolet light from an ultraviolet lamp 28, and then developed and dried. In this state, the portion related to the pattern formation region 4 (38a) is exposed, and the rest of the photoresist layer 38 is unexposed (38b) (see Figure 10(b)).

[0037] Next, as shown in Figure 10(b), the frame 3 was positioned on the mold 24 so as to surround the primary electroformed layer 30. Here, the frame 3 was temporarily fixed to the mold 24 by utilizing the adhesive properties of the unexposed photoresist layer 38b. Furthermore, as shown in Figure 10(c), the unexposed photoresist layer 38b exposed on the surface was dissolved and removed to form a secondary pattern resist 40 having a resist body 40a that covers the pattern formation region 4. At this time, the unexposed photoresist layer 38b on the lower surface of the frame 3 was covered by the frame 3 and remained on the mold 24 without being dissolved and removed.

[0038] (Second electroforming process) The matrix 24 described above was placed in an electroforming bath prepared at a temperature of 23±3℃, and as shown in Figure 10(d), a nickel electrodeposited metal was electroformed onto the upper surface of the primary electroformed layer 30 facing the outer edge 4a of the pattern formation region 4, the surface of the frame 3, the surface of the matrix 24 exposed between the frame 3 and the primary electroformed layer 30, and inside the joining through-holes 7 to form a metal layer 8. This allows the primary electroformed layer 30 and the frame 3 to be joined together inseparably by the metal layer 8.

[0039] (Peeling process) After peeling off the primary electroformed layer 30 and the metal layer 8 from the matrix 24, the primary electroformed layer 30a located on the lower surface of the frame 3 was peeled off from both layers 30 and 8. Finally, by removing the secondary pattern resist 40 and the unexposed photoresist layer 38b, the deposition mask 1 shown in Figure 3 was obtained.

[0040] In this embodiment, the temperature range of the electroforming solution in the first electroforming process is set to a higher temperature range than that of the electroforming solution in the second electroforming process. This allows the mask body 2 to be held against the frame 3 with tension applied such that a stress acts on it in the direction of inward contraction. Therefore, the expansion of the mask body 2 due to the temperature rise in the deposition furnace can be absorbed by this tension, preventing misalignment of the mask body 2 relative to the frame 3 and the occurrence of wrinkles due to expansion.

[0041] (Second Embodiment) Figures 11 and 12 show a second embodiment of the vapor deposition mask and its manufacturing method according to the present invention. In this embodiment, as shown in Figure 11, in order to prevent the occurrence of distortion in the frame 3 due to internal stress of the metal layer 8 that inseparably joins the mask body 2 and the frame 3, the metal layer 8 is not formed on the upper surface of the frame 3 except on the periphery of the mask opening 11, thereby dividing the metal layer 8 and providing a stress relief portion 42, which is different from the first embodiment.

[0042] In the first embodiment, the frame 3 is surrounded on three sides by a metal layer 8 on its upper surface and on both edges of the mask opening 11 continuous with the upper surface. Therefore, if the metal layer 8 is formed by electroforming under conditions where internal stress is present, this internal stress can cause distortion in the frame 3, which may adversely affect the flatness of the vapor deposition mask 1. However, as in this embodiment, by providing a stress relief section 42, the internal stress in the metal layer 8 can be released by the stress relief section 42, preventing distortion in the frame 3. Note that "dividing the metal layer 8" here means that the metal layer 8 is not formed continuously across the entire upper surface of the frame 3, and the manner is not limited to that of this embodiment. The rest is the same as in the first embodiment, so the same reference numerals are used for the same components and their descriptions are omitted. The same applies to the following embodiments.

[0043] In the manufacturing method of the deposition mask 1 according to this embodiment, at the final stage of the frame formation step, a step is performed to form a resist body 42a corresponding to the stress relaxation portion 42 on the upper surface of the frame 3, thereby providing the resist body 42a on the upper surface of the frame 3. The subsequent patterning pre-formation step to the secondary patterning step is the same as the method shown in Figures 8(a) to (d), 9(a) to (c), and 10(a) described in the first embodiment, but the first electroforming step is performed with the electroforming solution temperature range set to 23±2℃.

[0044] (Frame assembly process) As shown in Figure 12(a), a frame 3 with a resist body 42a was positioned on the master mold 24 so as to surround the primary electroformed layer 30. Here, the frame 3 was temporarily fixed to the master mold 24 by utilizing the adhesive properties of the unexposed photoresist layer 38b. Furthermore, as shown in Figure 12(b), the unexposed photoresist layer 38b exposed on the surface was dissolved and removed to form a secondary pattern resist 40 having a resist body 40a that covers the pattern formation region 4. At this time, the unexposed photoresist layer 38b on the lower surface of the frame 3 was covered by the frame 3 and remained on the master mold 24 without being dissolved and removed.

[0045] (Second electroforming process) The matrix 24 described above was placed in an electroforming bath prepared with the electroforming solution temperature set to 23±3℃. As shown in Figure 12(c), a metal layer 8 was formed by electroforming a nickel electrodeposited metal onto the upper surface of the primary electroformed layer 30 facing the outer edge 4a of the pattern formation region 4, the surface of the frame 3 not covered by the resist body 42a, the surface of the matrix 24 exposed between the frame 3 and the primary electroformed layer 30, and inside the joining holes 7. This allows the primary electroformed layer 30 and the frame 3 to be joined inseparably and integrally by the metal layer 8. In this embodiment, the temperature range of the electroforming solution used in the first electroforming process and the second electroforming process was set to the same (23±3℃). This prevents the primary electroformed layer 30, i.e., the mask body 2, from expanding due to heat and joining with the frame 3 as much as possible, thereby improving the positional accuracy of the joining position of the mask body 2 to the frame 3, and enabling the acquisition of a vapor-deposited mask with higher accuracy in vapor deposition layer reproducibility and vapor deposition accuracy. Furthermore, in both the first and second electroforming processes, the lower the temperature of the electroforming fluid in the electroforming tank, the more effectively the thermal expansion of the primary electroformed layer 30 and the metal layer 8 can be suppressed. In this case, it is more preferable that the temperature of the electroforming fluid in the electroforming tank in the first electroforming process and the temperature of the electroforming fluid in the electroforming tank in the second electroforming process be the same or ±3°C.

[0046] (Peeling process) After peeling off the primary electroformed layer 30 and the metal layer 8 from the matrix 24, the primary electroformed layer 30a located on the lower surface of the frame 3 was peeled off from both layers 30 and 8. Finally, by removing the secondary pattern resist 40, the resist body 42a, and the unexposed photoresist layer 38b, a deposition mask 1 with a stress relaxation section 42 as shown in Figure 11 was obtained.

[0047] (Third Embodiment) Figures 13 to 15 show a third embodiment of the vapor deposition mask and its manufacturing method according to the present invention. This embodiment differs from the first embodiment in that, as shown in Figure 13, the frame 3 is made of a single frame 3 to reinforce the mask body 2, and the joining through-holes 7 in the mask body 2 into which the metal layer 8 enters are eliminated. In this embodiment, the upper frame 16 and lower frame 17 are formed from a 0.8 mm metal plate material, and the frame 3 is set to the same thickness dimensions as in the first embodiment.

[0048] Figures 14 and 15 show the manufacturing method of the deposition mask 1 according to this embodiment, in which, first, the frame formation process shown in Figure 6 described in the first embodiment is performed to form a reinforcing frame 3.

[0049] (Frame formation process) First, a cutting process is performed to cut the metal sheet material to the size of the upper frame 16 and lower frame 17, for example, using a wire electrical discharge machine or the like, which has minimal thermal influence on the metal sheet material. Next, a mask opening formation process is performed to form multiple openings that will become the mask opening 11 by etching or laser processing on the cut-out upper frame 16 and lower frame 17, as shown in Figure 6(a). Then, as shown in Figure 6(b), a joining process is performed to form the frame body 3 in a flat state by joining the two frames 16 and 17 with an adhesive layer 18, with the protruding curved surfaces of the upper frame 16 and lower frame 17, which originate from the metal sheet material, facing each other, so that the two-dimensional curved warp is canceled out. The adhesive layer 18 consists of a sheet-like uncured photosensitive dry film resist.

[0050] Next, as shown in Figure 6(c), a fixing process is performed in which the mask is passed between upper and lower rolling rolls 22-22, which are positioned at a predetermined distance between the rolls, and pressed. Furthermore, the frame 3 is obtained by removing (developing) the unnecessary portion of the adhesive layer 18 (the portion exposed outside the mask opening 11 and the outer peripheral frame 10). The reason for using a sheet-like uncured photosensitive dry film resist for the adhesive layer 18 is that the uncured photosensitive dry film resist has adhesive properties and is also a material used in the primary patterning process described later, so there is no need to prepare a separate commercially available adhesive, and thus the manufacturing cost of the deposition mask 1 can be reduced.

[0051] (Patterning pre-processing step) As shown in Figure 14(a), a photoresist layer 25 is formed on the surface of a conductive matrix 24 made of, for example, stainless steel or brass. This photoresist layer 25 is formed by laminating one or more negative-type sheet-like photosensitive dry film resists and heat-pressing them to a predetermined thickness. Next, a pattern film 26 (glass mask) having light-transmitting holes 26a corresponding to the vapor deposition holes 5 is placed in close contact with the photoresist layer 25 to obtain a patterning pre-assembly 27.

[0052] (Preheating process) The patterning pre-assembly unit 27 is preheated to the furnace temperature of the ultraviolet irradiation device used during exposure, for example, using a heater plate or a preheating furnace. In parallel with the preheating of the patterning pre-assembly unit 27, the furnace of the ultraviolet irradiation device is also preheated to the furnace temperature used during exposure. Preheating of the furnace of the ultraviolet irradiation device is performed by turning on the ultraviolet lamp 28 with the object to be irradiated not placed inside the furnace, or with a dummy mold (mold + photoresist layer + protective film) placed inside. The patterning pre-assembly unit 27 and the furnace are preheated to, for example, 23±3℃. Incidentally, the maximum temperature inside the furnace of the ultraviolet irradiation device during exposure is around 26℃.

[0053] (Primary patterning process) Once the furnace of the ultraviolet irradiation device and the patterning pre-stage body 27 have been preheated, the patterning pre-stage body 27 is placed inside the furnace of the ultraviolet irradiation device, and as shown in Figure 14(a), exposure is performed by irradiating it with ultraviolet light from the ultraviolet lamp 28, followed by development and drying. Next, by dissolving and removing the unexposed portions, a primary pattern resist 29 having a resist body 29a corresponding to the deposition holes 5 (primary patterning) is formed on the matrix 24, as shown in Figure 14(b). In this way, by performing the exposure work with the furnace of the ultraviolet irradiation device and the patterning pre-stage body 27 preheated to the furnace temperature for the exposure work, it is possible to eliminate the problem of the patterning pre-stage body 27 being heated and expanding by ultraviolet irradiation, causing the relative positional relationship of the three components 24, 25, and 26 to shift during the exposure work. Therefore, it is possible to create a primary pattern resist 29 on the matrix 24 with good positional accuracy and in the intended shape, contributing to improved reproduction accuracy of the deposition layer and high deposition accuracy.

[0054] (First electroforming process) Next, the master mold 24 was placed in an electroforming bath prepared with an electroforming solution at a temperature of 40-50°C. As shown in Figure 14(c), a nickel electrodeposited metal was primary electroformed onto the surface of the master mold 24 that was not covered by the resist 29a, within the height range of the resist 29a, to form a primary electroformed layer 30, which would become the mask body 2. Then, by dissolving and removing the resist 29a, a mask body 2 was obtained having a deposition pattern 6 consisting of numerous independent deposition holes 5, as shown in Figure 14(d).

[0055] (Secondary patterning process and frame assembly process) As shown in Figure 15(a), a photoresist layer 38 was formed on the entire surface of the matrix 24, including the portion where the primary electroformed layer 30 is formed. This photoresist layer 38 was formed by laminating one or more negative-type sheet-like photosensitive dry film resists and heat-pressing them together to achieve a predetermined thickness, as described above. Next, a pattern film 39 having light-transmitting holes 39a corresponding to the pattern formation region 4 was placed in close contact with the pattern film and placed in the furnace of an ultraviolet irradiation device, and exposure was performed by irradiating it with ultraviolet light from an ultraviolet lamp 28. In this state, the portion related to the pattern formation region 4 (38a) was exposed, and the rest of the photoresist layer 38 remained unexposed (38b) (see Figure 15(b)). In this embodiment as well, an activation treatment step may be performed prior to the secondary patterning step, and the primary electroformed layer 30, which will become the outer edge 4a of the pattern formation region 4, may be subjected to activation treatments such as acid immersion or electrolytic treatment.

[0056] Next, as shown in Figure 15(b), the frame 3 was positioned on the mold 24 so as to surround the primary electroformed layer 30. Here, the frame 3 was temporarily fixed to the mold 24 by utilizing the adhesive properties of the unexposed photoresist layer 38b. Furthermore, as shown in Figure 15(c), the unexposed photoresist layer 38b exposed on the surface was dissolved and removed to form a secondary pattern resist 40 having a resist body 40a that covers the pattern formation region 4. At this time, the unexposed photoresist layer 38b on the lower surface of the frame 3 was covered by the frame 3 and remained on the mold 24 without being dissolved and removed.

[0057] (Second electroforming process) Next, the matrix 24 is placed in an electroforming bath prepared with an electroforming solution at a temperature of 23±3℃. As shown in Figure 15(d), a nickel electrodeposited metal is electroformed onto the upper surface of the primary electroformed layer 30 facing the outer edge 4a of the pattern formation region 4, the surface of the frame 3, and the surface of the matrix 24 exposed between the frame 3 and the primary electroformed layer 30 to form a metal layer 8. This allows the primary electroformed layer 30 and the frame 3 to be joined together inseparably by the metal layer 8.

[0058] (Peeling process) After peeling off the primary electroformed layer 30 and the metal layer 8 from the matrix 24, the primary electroformed layer 30a located on the lower surface of the frame 3 was peeled off from both layers 30 and 8. Finally, by removing the secondary pattern resist 40 and the unexposed photoresist layer 38b, the deposition mask 1 shown in Figure 13 was obtained.

[0059] (Fourth Embodiment) Figures 16 and 17 show a fourth embodiment of the vapor deposition mask and its manufacturing method according to the present invention. In this embodiment, as shown in Figure 16, the mask body 2 and the frame 3 are joined inseparably by a metal layer 8, but the difference from the previous embodiments is that the metal layer 8 is integrally formed with the primary electroformed layer 30 that constitutes the mask body 2. By integrally forming the metal layer 8 with the mask body 2 in this way, the effort of separately forming the metal layer 8 and joining the mask body 2 and the frame 3 is eliminated, thus reducing the manufacturing process and time required, and thus the manufacturing cost of the vapor deposition mask 1 can be reduced.

[0060] Figure 17 shows the manufacturing method of the deposition mask 1 according to this embodiment, in which, first, the frame formation process shown in Figures 6 and 7 described in the first embodiment is performed to form a reinforcing frame 3.

[0061] (Frame formation process) First, a cutting process is performed to cut the metal sheet material to the size of the upper frame 16 and lower frame 17, for example, using a wire electrical discharge machine or the like, which has minimal thermal influence on the metal sheet material. Next, a mask opening formation process is performed to form multiple openings that will become the mask opening 11 by etching or laser processing on the cut-out upper frame 16 and lower frame 17, as shown in Figure 6(a). Then, as shown in Figure 6(b), a joining process is performed to form the frame body 3 in a flat state by joining the two frames 16 and 17 with an adhesive layer 18, with the protruding curved surfaces of the upper frame 16 and lower frame 17, which originate from the metal sheet material, facing each other, so that the two-dimensional curved warp is canceled out. The adhesive layer 18 consists of a sheet-like uncured photosensitive dry film resist.

[0062] Next, as shown in Figure 6(c), a fixing process is performed in which the mask is passed between upper and lower rolling rolls 22-22, which are positioned at a predetermined distance between the rolls, and pressed. Furthermore, the frame 3 is obtained by removing (developing) the unnecessary portion of the adhesive layer 18 (the portion exposed outside the mask opening 11 and the outer peripheral frame 10). The reason for using a sheet-like uncured photosensitive dry film resist for the adhesive layer 18 is that the uncured photosensitive dry film resist has adhesive properties and is also a material used in the primary patterning process described later, so there is no need to prepare a separate commercially available adhesive, and thus the manufacturing cost of the deposition mask 1 can be reduced.

[0063] A pair of frame bodies 3·3 are manufactured from metal plates of different thicknesses by performing the above steps, as shown in Figure 7(a). These frame bodies 3·3 are stacked as shown in Figure 7(b), and the frame bodies 3·3 are joined together with an adhesive layer 19 made of a sheet of uncured photosensitive dry film resist. After this, a stacking process is performed in which the frame bodies are passed and compressed between upper and lower rolling rolls 22·22 positioned at a predetermined distance between the rolls, as shown in Figure 7(c). This gives the stacked pair of frame bodies 3·3.

[0064] (Patterning pre-processing step) As shown in Figure 17(a), a photoresist layer 25 is formed on the surface of a conductive matrix 24 made of, for example, stainless steel or brass. This photoresist layer 25 is formed by laminating one or more negative-type sheet-like photosensitive dry film resists and heat-pressing them to a predetermined thickness. Next, a pattern film 26 (glass mask) having light-transmitting holes 26a corresponding to the mask body 2 is pressed onto the photoresist layer 25 to obtain a patterning pre-body 27.

[0065] (Preheating process) The patterning pre-assembly unit 27 is preheated to the furnace temperature of the ultraviolet irradiation device used during exposure, for example, using a heater plate or a preheating furnace. In parallel with the preheating of the patterning pre-assembly unit 27, the furnace of the ultraviolet irradiation device is also preheated to the furnace temperature used during exposure. Preheating of the furnace of the ultraviolet irradiation device is performed by turning on the ultraviolet lamp 28 with the object to be irradiated not placed inside the furnace, or with a dummy mold (mold + photoresist layer + protective film) placed inside. The patterning pre-assembly unit 27 and the furnace are preheated to, for example, 23±3℃. Incidentally, the maximum temperature inside the furnace of the ultraviolet irradiation device during exposure is around 26℃.

[0066] (Primary patterning process) Once the furnace of the ultraviolet irradiation device and the patterning pre-stage body 27 have been preheated, the patterning pre-stage body 27 is placed inside the furnace of the ultraviolet irradiation device, and as shown in Figure 17(a), exposure is performed by irradiating it with ultraviolet light from the ultraviolet light lamp 28, followed by development and drying. Next, by dissolving and removing the unexposed portions, a primary pattern resist 29 having a resist body 29a corresponding to the mask body 2 (primary patterning) is formed on the master mold 24, as shown in Figure 17(b). In this way, by performing the exposure work with the furnace of the ultraviolet irradiation device and the patterning pre-stage body 27 preheated to the furnace temperature for the exposure work, it is possible to eliminate the problem of the patterning pre-stage body 27 being heated and expanding by ultraviolet irradiation, causing the relative positional relationship of the three components 24, 25, and 26 to shift during the exposure work. Therefore, it is possible to create a primary pattern resist 29 on the master mold 24 with good positional accuracy and in the intended shape, contributing to improved reproduction accuracy and high deposition accuracy of the deposited layer.

[0067] (Frame assembly process) As shown in Figure 17(c), an adhesive resist 43 was formed on the entire surface of the matrix 24, including the area where the primary pattern resist 29 was to be formed. This adhesive resist 43 was formed by laminating one or more negative-type sheet-like photosensitive dry film resists and then heat-pressing them together to achieve a predetermined thickness. Next, the frame 3 was positioned on the matrix 24 so as to surround the primary pattern resist 29. Here, the frame 3 was temporarily fixed to the matrix 24 by utilizing the adhesive properties of the unexposed adhesive resist 43. Furthermore, as shown in Figure 17(d), the unexposed adhesive resist 43 exposed on the surface was dissolved and removed. At this time, the adhesive resist 43 on the underside of the frame 3 remained on the matrix 24, covered by the frame 3 and not dissolved and removed.

[0068] (integrated electroforming process) The above-mentioned master mold 24 was placed in an electroforming bath prepared at a temperature of 23±3℃, and as shown in Figure 17(e), a nickel electrodeposited metal was electroformed onto the surface of the master mold 24 that was not covered with the resist 29a and the surface of the frame 3 to form a metal layer 8. This made it possible to integrally form the primary electroformed layer 30 that constitutes the mask body 2 and the metal layer 8 that joins the mask body 2 and the frame 3.

[0069] (Peeling process) The primary electroformed layer 30, the metal layer 8, and the frame 3 were peeled off integrally from the matrix 24, and then the adhesive resist 43 located on the lower surface of the frame 3 was removed from both layers 30 and 8 to obtain the vapor deposition mask 1 shown in Figure 16.

[0070] According to the manufacturing method of the fourth embodiment described above, the effort required to form the metal layer 8 is eliminated, thereby reducing the number of manufacturing steps and shortening the time required, while simultaneously increasing the rigidity of the frame 3 in the same manner as described above. Therefore, it is possible to achieve a larger size while further suppressing the increase in manufacturing costs, while maintaining flatness, and to obtain a vapor deposition mask 1 that ensures good reproducibility and vapor deposition accuracy of the vapor-deposited layer.

[0071] (Fifth Embodiment) Figures 18 to 20 show a fifth embodiment of the vapor deposition mask according to the present invention. In this embodiment, as shown in Figure 18, the vapor deposition mask 1 comprises a support frame 46 fixed to the lower surface of a frame 3 and an auxiliary frame 47 fixed to the lower surface of the support frame 46. The external shapes of the support frame 46 and the auxiliary frame 47 are matched to those of the frame 3. As shown in Figures 19 and 20, the support frame 46 has a frame opening 48 that corresponds to the mask opening 11 of the frame 3, and the frame opening 48 is formed to be slightly larger than the mask opening 11. The entire vertical frame 12 and horizontal frame 13 of the frame 3 are supported by the support frame 46. Furthermore, the auxiliary frame 47 is formed in the shape of a picture frame, and the four periphery edges of the support frame 46 are supported by the auxiliary frame 47. The vapor deposition mask 1, the support frame 46, and the auxiliary frame 47 are aligned and then joined and integrated by spot welding the three components 1, 46, and 47. Spot welds 49 are provided at the four corners and on the four peripheral edges along the extensions of the vertical frame 12 and horizontal frame 13 (see Figure 20).

[0072] As described above, by supporting the entire vertical frame 12 and horizontal frame 13 of the frame 3 with the support frame 46, and further supporting the four periphery of the support frame 46 with the auxiliary frame 47, the structural strength and rigidity of the entire deposition mask are further enhanced, preventing the deposition mask 1 from bending and deforming, maintaining flatness, and enabling higher accuracy in the reproduction and deposition of the deposition layer.

[0073] Figure 21 shows a modified example of the fifth embodiment of the vapor deposition mask according to the present invention. In this embodiment, the vapor deposition mask 1 has 10 mask bodies 2 arranged in a 2x5 matrix. Three of these vapor deposition masks 1 are manufactured, and these three vapor deposition masks 1 are supported by a support frame 46 and an auxiliary frame 47. Specifically, first, one vapor deposition mask 1 is prepared, its position and tension are adjusted, and then it is fixed to the support frame 46. This fixing is done by spot welding the corner portion of the frame 3 and the peripheral portion on the extension line of the vertical frame 12 and horizontal frame 13. The remaining two vapor deposition masks 1 are fixed to the support frame 46 in the same manner. Finally, the auxiliary frame 47 is fixed (spot welded) to the side of the support frame 46 opposite to the side where the vapor deposition masks 1 are fixed. In this configuration, where multiple vapor deposition masks 1 are supported by a support frame 46 and an auxiliary frame 47, the relative positions of adjacent vapor deposition masks 1 can be finely adjusted and positioned, improving the relative positional accuracy of the mask bodies 2 of adjacent vapor deposition masks 1. Therefore, good reproducibility and deposition accuracy can be ensured. In addition, the deposition mask 1 can be freely set to the desired size.

[0074] As described above, in the vapor deposition masks and vapor deposition mask manufacturing methods of each embodiment, the frame 3 is composed of an upper frame 16 and a lower frame 17, and the upper and lower frames 16 and 17 are joined together via an adhesive layer 18 to form a single unit. Therefore, when forming a frame 3 of the same thickness as conventional frames, a thinner metal sheet material can be used to form the frame 3, and the thickness deviation of the entire frame 3 can be reduced. As a result, even with a large vapor deposition mask 1, the occurrence of distortion due to thermal expansion caused by the thickness deviation of the metal sheet material can be suppressed. Furthermore, since a commonly available thin metal sheet material is used as the base material, there is no need to use a special metal sheet material to form the frame 3. As described above, the vapor deposition masks of each embodiment can be made larger while suppressing an increase in manufacturing costs, and the flatness of the vapor deposition mask 1 can be maintained, ensuring good reproducibility and vapor deposition accuracy. Furthermore, with a frame 3 having an adhesive layer 18 interposed between the upper frame 16 and the lower frame 17, when an external force that causes bending deformation is applied to the vapor deposition mask 1, the frame 3 flexibly and elastically deforms by the amount of the adhesive layer 18, effectively preventing damage to the vapor deposition mask 1.

[0075] Furthermore, in the vapor deposition masks of the first, second, fourth, and fifth embodiments, multiple frame bodies 3·3 are stacked and adjacent frame bodies 3·3 in the stacking direction are joined together via an adhesive layer 19. Therefore, when forming frame bodies 3 of the same thickness as conventional methods, it is possible to form the frame bodies 3 using even thinner metal sheets, thereby further suppressing the generation of distortion due to thermal expansion resulting from thickness deviations of the metal sheets.

[0076] As shown in the embodiments described above, the number and arrangement of mask bodies 2 in the deposition mask 1 are not limited to those shown in the embodiments. Also, there is no need for multiple mask bodies 2; there may be only one. Prior to the joining process of the upper and lower frames 16 and 17, the cut upper frame 16 and lower frame 17 can be press-formed using upper and lower molds for creating curved surfaces to create two-dimensional or three-dimensional curved surfaces. In this case, by creating two-dimensional or three-dimensional curved surfaces that are symmetrical, it is possible to form the frame 3 into a flat shape in the subsequent joining process. The primary electroformed layer 30 and the metal layer 8 may be a two-layer structure of bright nickel and matte nickel electroformed on top of it. In this case, the bright nickel does not adhere easily to the master mold 24, and the peeling process of the deposition mask 1 from the master mold 24 in the manufacturing process can be carried out efficiently. [Explanation of Symbols]

[0077] 1. Evaporation mask 2. Mask body 3 Frame 4 Pattern formation regions 4a Outer edge 5 Vapor deposition hole 6 Deposition Patterns 8 metal layer 10 Outer frame 11 Mask opening 12 Vertical frame 13 Horizontal frame 16 Upper frame 17 Bottom frame 18 Adhesive layer 19 Adhesive layer 24 Maternal blood type 25 Photoresist layer 26 Pattern Film 26a Transparent hole 27 Patterning Pre-stage 29 Primary Pattern Resist 29a Resist 30 Primary electroformed layer 43 Adhesive Resist 46 Support frame 47 Auxiliary frame 48 Frame opening W1 Vertical frame width dimension W2 Horizontal frame width dimension

Claims

1. A vapor deposition mask comprising a mask body (2) having a vapor deposition pattern (6) consisting of numerous independent vapor deposition holes (5), and a reinforcing frame (3) arranged around the mask body (2), The frame (3) is composed of an upper frame (16) and a lower frame (17), the upper frame (16) and the lower frame (17) are made of Invar material or Super Invar material, and the upper frame (16) and the lower frame (17) are joined and integrated via an adhesive layer (18). A vapor deposition mask characterized in that the upper frame (16) and the lower frame (17) are joined together with their protruding or concave surfaces facing each other.

2. The vapor deposition mask according to claim 1, wherein multiple frame bodies (3,3) are stacked and adjacent frame bodies (3,3) in the stacking direction are joined together via an adhesive layer (19).

3. The mask body (2) is formed in a rectangular shape, and multiple mask bodies (2) are arranged in a matrix. The frame (3) comprises an outer frame (10) and grid-like vertical frames (12) and horizontal frames (13) that partition a plurality of mask openings (11) within the outer frame (10). The vapor deposition mask according to claim 1 or 2, wherein the width dimension of the vertical frame (12) parallel to the long side of the mask body (2) is (W1), and the width dimension of the horizontal frame (13) parallel to the short side of the mask body (2) is (W2), and the width dimension of the vertical frame (12) (W1) and the width dimension of the horizontal frame (13) (W2) are set to satisfy the inequality (W1 ≤ W2 ≤ W1 × 1.1).

Citation Information

Patent Citations

  • Manufacture of core structure for electromagnetic device

    JP1987283613A

  • Manufacture of x-ray mask

    JP1989074721A

  • Manufacturing method of organic electroluminescent device

    JP2002083679A

  • Vapor deposition mask and vapor deposition method

    JP2004323888A

  • Vapor deposition mask for organic el element and its manufacturing method

    JP2004349086A