Matte laminate, water-based matte coating agent, and ink set
The matte laminate with a urethane-acrylic resin matrix and fine particles addresses the balance of matte properties, abrasion resistance, and soft touch feeling, enhancing durability and aesthetic appeal.
Patent Information
- Application Number
- JP2026085149
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2025-10-31
- Filing Date
- 2026-05-20
- Publication Date
- 2026-11-19
- Estimated Expiration
- 2046-05-20
AI Technical Summary
Existing matte coatings face challenges in achieving a balance between matte properties, abrasion resistance, and soft touch feeling, with issues such as resin particle aggregation, reduced flexibility, and insufficient coating film strength in solvent-free active energy ray-curable coatings, and inadequate flexibility and abrasion resistance in water-based coatings.
A matte laminate with a resin matrix comprising a urethane resin structure and an acrylic resin structure, combined with fine resin particles, achieving specific surface roughness, composite modulus, and absorbance ratios to ensure a matte finish, abrasion resistance, and soft touch feeling.
The laminate provides excellent matte properties, abrasion resistance, and a soft touch feeling, balancing flexibility and hardness for improved durability and aesthetic appeal.
Smart Images

Figure 0007953796000001 
Figure 0007953796000002 
Figure 0007953796000003
Abstract
Description
[Technical Field]
[0001] This disclosure relates to a matte laminate, an aqueous matte coating agent, and an ink set. [Background technology]
[0002] In recent years, in the field of packaging using paper substrates, such as paperboard containers, research has been actively conducted on applying coating agents to various substrates after printing with color inks, with the aim of imparting durability and aesthetic appeal to printed materials. Regarding paperboard packaging, when displayed in stores after printing, there are cases where a glossy finish is desired for aesthetic purposes, and cases where a matte finish is desired. Matte finishes are also referred to as non-glossy finishes, and in recent years, the demand for printed materials with a non-glossy effect has been increasing.
[0003] Traditionally, matte coatings for paper packaging have typically used solvent-based matte coatings containing resin, matting agents, and solvents to provide a high-quality, matte finish. However, solvent-based matte coatings raise concerns about environmental pollution due to the volatilization of solvent components during film formation. Therefore, in recent years, solvent-free, active energy ray-curable matte coatings have been developed that offer improved workability and environmental friendliness.
[0004] Patent Document 1 discloses a solvent-free active energy ray curable composition containing a polyfunctional urethane (meth)acrylate, a monofunctional ethylenically unsaturated monomer, and resin fine particles, for providing a coating film with excellent substrate adhesion and matte properties.
[0005] It is known that by including resin microparticles in the composition, the coating film can be given not only a matte finish but also aesthetic properties. Patent Document 2 discloses that by including a urethane (meth)acrylate compound and a microparticle synthetic resin filler in a solvent-free active energy ray curable resin composition, it is possible to provide a coating layer with a moist, smooth feel.
[0006] Furthermore, demand for water-based matte coating agents is increasing from the perspective of improving workability and environmental friendliness.
[0007] Patent Document 3 discloses an aqueous ink composition for surface printing that can impart an excellent matte finish to the surface of articles, particularly plastic molded products, and is resistant to gloss return. This composition comprises a binder resin, a matting agent, and an aqueous medium, wherein the binder resin is at least one selected from the group consisting of aqueous urethane resin, aqueous acrylic resin, and aqueous acrylic urethane resin, and the matting agent contains an extender pigment and organic particles.
[0008] Patent Document 4 discloses an aqueous coating agent that provides a soft, velvet-like or suede-like texture to the substrate of printed materials such as paper containers, with the aim of enhancing their luxurious feel and appeal. This coating agent contains urethane resin and styrene-acrylic resin, and the urethane resin is in the form of beads with a specified particle size. The content of the urethane resin and acrylic resin is also specified.
[0009] Patent Document 5 discloses an aqueous ink composition that yields a coating film with excellent properties such as substrate adhesion, abrasion resistance, water abrasion resistance, heat resistance, and scratch resistance, and contains two types of acrylic emulsion resins with different acid values, and either or both titanium dioxide and precipitated barium sulfate. It also discloses that a curing agent and resin beads may be further included. [Prior art documents] [Patent Documents]
[0010] [Patent Document 1] Patent No. 6919110 [Patent Document 2] Japanese Patent Publication No. 2014-122338 [Patent Document 3] Japanese Patent Publication No. 2023-087626 [Patent Document 4] Japanese Patent Publication No. 2009-227707 [Patent Document 5] Patent No. 7567081 Publication SUMMARY OF THE INVENTION PROBLEMS TO BE SOLVED BY THE INVENTION
[0011] Since the solvent-free active energy ray-curable matting coating agent uses a large amount of reactive diluent to reduce viscosity, it is difficult to obtain sufficient coating film strength. When resin fine particles are used as a matting agent in the solvent-free active energy ray-curable matting coating agent, it is difficult to obtain dispersion stability, and the resin fine particles may aggregate in the matting coat layer, causing a decrease in matting properties. Along with these issues, the soft touch feeling of the matting coat layer may also deteriorate.
[0012] In the technique disclosed in Patent Document 3, an excellent matte feeling is obtained by including an extender pigment in the matting agent, and suppression of gloss reversion is attempted by including organic particles in the matting agent. In addition, the technique disclosed in Patent Document 3 attempts to obtain scratch resistance by incorporating fine extender pigment into a relatively soft water-based polyurethane resin. However, using the water-based polyurethane resin as the sole binder resin and further including an extender pigment in the matting agent may cause a reduction in the soft touch feeling.
[0013] In the technique disclosed in Patent Document 4, urethane resin beads and a styrene-acrylic resin are combined. Since the styrene-acrylic resin is a relatively hard resin, it alone provides poor flexibility of the coat layer. In addition, the technique disclosed in Patent Document 4 forms a coating film by heat fusion using a styrene-acrylic resin having an acid value, so while a soft hand feeling can be obtained, sufficient abrasion resistance and matting properties cannot be achieved.
[0014] In the technique disclosed in Patent Document 5, two types of acrylic emulsion resins with different acid values are used. However, since acrylic resins themselves tend to form hard coating films, it is difficult to obtain flexibility of the coating films, and sufficient friction resistance cannot be achieved. Furthermore, in the technique disclosed in Patent Document 5, the resin beads are used to improve the abrasion resistance, water abrasion resistance, and scratch resistance of the coating film, and no coating film with matting properties is provided.
[0015] One of the objects of the present disclosure is to provide a matte laminate excellent in matting properties, abrasion resistance and soft touch feeling, and an aqueous matte coating agent and an ink set for providing the same. [MEANS FOR SOLVING THE PROBLEMS]
[0016] Some embodiments of the present disclosure are described below.
[0017] <1>A matte laminate comprising a paper substrate and a matte coat layer, wherein the matte coat layer comprises a resin matrix having a urethane resin structure and an acrylic resin structure, and fine resin particles, and satisfies the following (1), (2) and (3). (1) The matte coat layer has a surface roughness Sq of 0.5 to 3.5 in a measurement visual field range of 506 μm × 675 μm. (2) The matte coat layer has a composite elastic modulus of 4 GPa or less (provided that the composite elastic modulus is the composite elastic modulus of the resin matrix portion measured by a nanoindentation method). (3) In the matte coat layer, the ratio (a / b) of the absorbance (a) of the following peak (A) and the absorbance (b) of the following peak (B), which are obtained at an incident angle of 45° using a germanium prism by an attenuated total reflection measurement method of Fourier transform infrared spectroscopy, is 0.40 to 1.50. Peak (A): 1070 to 1130 cm -1 1 point with the highest absorbance in the region of Peak (B): 1220 to 1280 cm -1 1 point with the highest absorbance in the region of
[0018] <2> The aforementioned resin matrix is a cured product of resin raw materials containing an emulsion-type urethane resin, an emulsion-type acrylic resin, and a curing agent. <1> The matte laminate described above. <3> The curing agent includes an isocyanate-based curing agent, an aziridine-based curing agent, or a combination thereof. <2> The matte laminate described above.
[0019] <4> The resin matrix is a cured product of a resin raw material comprising a polyfunctional urethane (meth)acrylate and at least one selected from the group consisting of hydroxyl group-containing ethylenically unsaturated monomers and alkylene oxy group-containing ethylenically unsaturated monomers. <1> The matte laminate described above. <5> The resin matrix further comprises a curing agent. <4> The matte laminate described above. <6> The curing agent includes an isocyanate-based curing agent, an aziridine-based curing agent, or a combination thereof. <5> The matte laminate described above.
[0020] <7> The aforementioned paper substrate further comprises a printed layer. <1> from <6> A matte laminate as described in any of the following. <8> The aforementioned printing layer includes a printing layer obtained using an active energy ray-curable offset ink, a printing layer obtained using an active energy ray-curable flexographic ink, or a combination thereof. <7> The matte laminate described above.
[0021] <9> An aqueous matte coating agent comprising a resin raw material for forming a resin matrix having a urethane resin structure and an acrylic resin structure, resin fine particles, and an aqueous medium, satisfying the following conditions (A), (B), and (C). (A) When a matte coat layer with a thickness of 4 μm ± 3 μm is formed on a paper substrate using an aqueous matte coat agent, the surface roughness Sq of the matte coat layer in a measurement field of view of 506 μm × 675 μm is 0.5 to 3.5. Here, the surface roughness Sq of the paper substrate used to measure the surface roughness Sq is 0.4 ± 0.2 in a measurement field of view of 506 μm × 675 μm before the matte coat layer is formed. (B) When a matte coating layer with a thickness of 4 μm ± 3 μm is formed on a paper substrate using an aqueous matte coating agent, the composite modulus is 4 GPa or less (however, the composite modulus is the composite modulus of the resin matrix portion measured by the nanoindentation method). (C) When a matte coating layer with a thickness of 4 μm ± 3 μm is formed on a paper substrate using an aqueous matte coating agent, the ratio (a / b) of the absorbance (a) of peak (A) below and the absorbance (b) of peak (B) below, obtained by attenuated total reflection measurement using a germanium prism at an incident angle of 45° by Fourier transform infrared spectroscopy, is 0.40 to 1.50. Peak (A): 1070-1130cm -1 The single point with the highest absorbance in this region. Peak (B): 1220~1280cm -1 The single point with the highest absorbance in this region.
[0022] <10> The aqueous medium has a content of 20 to 70% by mass. <9> The water-based matte coating agent described above.
[0023] <11> It is a non-active energy ray curing type, and the resin raw material includes an emulsion-type urethane resin, an emulsion-type acrylic resin, and a curing agent. <9> or <10> The water-based matte coating agent described above. <12> The curing agent includes an isocyanate-based curing agent, an aziridine-based curing agent, or a combination thereof. <11> The water-based matte coating agent described above.
[0024] <13> The active energy ray curing type, the resin raw material comprises a polyfunctional urethane (meth)acrylate and at least one selected from the group consisting of hydroxyl group-containing ethylenically unsaturated monomers and alkylene oxy group-containing ethylenically unsaturated monomers. <9> or <10> The water-based matte coating agent described above. <14> The aforementioned resin raw material further comprises a curing agent. <13> The water-based matte coating agent described above. <15> The curing agent includes an isocyanate-based curing agent, an aziridine-based curing agent, or a combination thereof. <14> The water-based matte coating agent described above.
[0025] <16> The aforementioned paper substrate further comprises a printed layer. <9> from <15> A water-based matte coating agent as described in any of the following.
[0026] <17> the above <9> from <16> An ink set comprising an aqueous matte coating agent as described in any of the above, and an active energy ray-curable offset ink, an active energy ray-curable flexographic ink, or a combination thereof. [Effects of the Invention]
[0027] According to this disclosure, it is possible to provide a matte laminate with excellent matte properties, abrasion resistance, and soft touch, as well as an aqueous matte coating agent and ink set for providing the same. [Modes for carrying out the invention]
[0028] Some embodiments of the present disclosure are described in detail below, but the descriptions of constituent elements described below are examples of embodiments of the present disclosure and the present disclosure is not limited to these unless it exceeds its gist.
[0029] In this disclosure, (meth)acrylic and (meth)acrylate mean methacrylic and / or acrylic, and methacrylate and / or acrylate, respectively. (Meth)acryloyl means methacryloyl and / or acryloyl. Acrylic resin means a polymer polymerized using methacrylate and / or acrylate. Aqueous matte coating agents may also be simply referred to as matte coating agents.
[0030] In this disclosure, unless otherwise specified, the weight-average molecular weight (Mw) is a measurement value in polystyrene equivalent obtained by gel permeation chromatography. For example, the weight-average molecular weight can be measured using the Shodex GPC System-21 gel permeation chromatography system manufactured by Resonaq Corporation. GPC is a liquid chromatography system that separates and quantifies substances dissolved in a solvent based on the difference in their molecular size. Tetrohydrofuran is preferred as the solvent, and the determination of the weight-average molecular weight is preferred in polystyrene equivalent. Further details can be obtained by following the methods disclosed in the examples.
[0031] In this disclosure, unless otherwise specified, the glass transition temperature (Tg) is a measurement taken by differential scanning calorimeter (DSC). The glass transition temperature is defined as the midpoint between the endothermic start temperature and the end temperature based on the glass transition in the DSC curve. For details, it can be measured according to the method disclosed in the examples.
[0032] In this disclosure, viscosity can be measured using a cone-plate type viscometer with a cone diameter of 35 mm and a cone angle of 2° at a shear rate of 100 per second in a 25°C environment, in accordance with the method specified in JIS K5600-2.
[0033] In this disclosure, the total solid content of the aqueous matte coating agent is the total mass of non-volatile components in the aqueous matte coating agent. Solid content refers to the mass obtained by subtracting the total mass of volatile media from the total mass of the aqueous matte coating agent. Volatile media include aqueous media such as water and alcohol that do not remain in the film after film formation. However, monomers, oligomers, etc., although volatile themselves, are incorporated into the film by their active energy and are therefore not included in the media. The non-volatile content in the aqueous matte coating agent can be said to be, for example, the mass when the dried coating film of the aqueous matte coating agent is stored at 100°C for 1 hour and no mass change occurs.
[0034] The total amount of resin contained in an aqueous matte coating agent is the total mass of monomers, oligomers, polymers, and curing agents. However, the total amount of resin contained in an aqueous matte coating agent does not include resin microparticles. In this disclosure, the total amount of resin contained in an aqueous matte coating agent includes wax microparticles. The total solid content of the resin matrix contained in the matte coating layer is the total amount of the matte coating layer minus the mass of resin microparticles. However, if the matte coating layer contains inorganic solids, the total solid content of the resin matrix is the total amount of the matte coating layer minus the resin microparticles and then minus the mass of the inorganic solids. In this disclosure, the total solid content of the resin matrix includes wax microparticles.
[0035] In this disclosure, "non-active energy ray curable" means substantially free of unsaturated double bond groups. "Substantially" means that the material does not harden with active energy rays, and does not exclude cases that contain trace amounts of unsaturated double bonds.
[0036] <Matte laminate> In some embodiments of this disclosure, the matte laminate is It has a paper substrate and a matte coating layer. The matte coating layer comprises a resin matrix having a urethane resin structure and an acrylic resin structure, and resin fine particles. The following conditions (1), (2), and (3) must be met. (1) The surface roughness Sq of the matte coating layer in a measurement field of view of 506 μm × 675 μm is 0.5 to 3.5. (2) The matte coating layer has a composite modulus of 4 GPa or less (wherein the composite modulus is the composite modulus of the resin matrix portion measured by nanoindentation). (3) The matte coating layer has a ratio (a / b) of the absorbance (a) of peak (A) and the absorbance (b) of peak (B) obtained by the attenuated total reflection measurement method of Fourier transform infrared spectroscopy using a germanium prism at an incident angle of 45°, which is 0.4 or more and 1.5 or less. Peak (A): 1070-1130cm -1The single point with the highest absorbance in this region. Peak (B): 1220~1280cm -1 The single point with the highest absorbance in this region.
[0037] In this disclosure, the surface roughness Sq (hereinafter also simply referred to as surface roughness Sq) of the matte coat layer within a measurement field of view of 506 μm × 675 μm is a value measured according to the following procedure.
[0038] The surface roughness Sq is determined in accordance with the roughness standard ISO 25178-2:2012, and the average value obtained by measuring at five arbitrary locations on the surface of the matte coat layer using the following method is used. Equipment: Laser microscope VK-X3000 (Keyence Corporation), Measurement mode: Surface shape, Scan mode: Laser confocal, Measurement magnification: Objective lens magnification (20x, optical zoom 1x, numerical aperture (NA) 0.46), Measurement field of view: 506 μm vertical × 675 μm horizontal, Image processing: Reference plane setting processing, Filter type: Gaussian, S-filter: None, L-filter: None, F-operation: None, End effect correction: Enabled, Measurement pitch: 0.5 μm, Illumination filter: 100%, Double scan: Automatic (ON), Field curvature correction: ON, Light intensity eccentricity correction: ON, Received light intensity correction mode: γ correction, γ coefficient: 0.45, Offset: 0%.
[0039] In this disclosure, for the upper matte coat layer to satisfy the above surface roughness Sq, the average particle size of the resin fine particles in the composition of the matte coat agent filling the matte coat layer is set to 1 to 10 μm. This allows the resin fine particles to protrude from the coating surface while remaining incorporated into the coating film with a thickness of 4 μm ± 3 μm, thereby imparting the desired surface roughness to the coating surface. Furthermore, by including resin fine particles in the total solid content of the matte coat agent at a concentration of 5 to 70% by mass for inactive energy ray curable matte coat agents, or 5 to 90% by mass for active energy ray curable matte coat agents, the fine particles protrude from the coating surface at an optimal frequency, thereby imparting the desired surface roughness to the coating surface. At this time, by combining it with a flexible emulsion resin, the resin fine particles are more likely to orient themselves on the coating surface even during the drying process when the aqueous medium volatilizes, promoting the formation of a convex surface. Thus, the above range is satisfied by designing the resin fine particles in combination with a flexible resin at an optimal particle size and blending ratio.
[0040] In this disclosure, the composite modulus of the matte coat layer is a value measured according to the following procedure.
[0041] The composite modulus is measured by the nanoindentation method and is a measurement taken in the resin matrix portion. The composite modulus measured by the nanoindentation method is a parameter measured using a micro-area mechanical property evaluation device (nanoindenter), and in this disclosure, it is a parameter measured using a Hyzitron TI Premier (manufactured by Bruker). Because the nanoindenter indents only the very surface layer of the laminate, it is not affected by the substrate and can measure the mechanical properties of only the thin film mat coat layer. With other measurement methods, the indentation load and displacement are too large, making it difficult to measure only the thin film layer. In this disclosure, the composite modulus of only the mat coat layer is shown. In the mat coat layer, the resin matrix portion is the part other than the resin nanoparticles. Since the resin nanoparticles are observed as spherical in the mat coat layer, the composite modulus is measured in the portion excluding these spherically observed parts. In addition, the mat coat layer may show an uneven shape in a 50 μm square observation area. This is because, in the matte coat layer, areas with a high and low amount of resin matrix coating occur, influenced by factors such as the transfer state during printing and the dispersion state of solid components such as resin microparticles. In this case, the composite elastic modulus is measured in the matte coat layer, after obtaining an observation shape in a 20 μm square area, particularly in the taller convex portions, using the SPM function attached to the nanoindenter, within the 50 μm square observation area of the uneven surface, and then excluding the spherical resin microparticle portions.
[0042] The method for measuring the composite modulus (Er) of the matte coat layer is as follows: A triangular pyramidal cubecorner indenter is used as the indenter of the nanoindenter. The cubecorner indenter is pressed into the sample under the indentation conditions described below, and the indentation depth h (nm) for each indentation load F (μN) is continuously measured to create a load-displacement curve. The slope S (contact stiffness) of the unloading curve is determined from the created load-displacement curve, and the contact projected area Ac (μm) between the indenter and the sample is calculated. 2The following formula (1) is used to determine the value. Here, Ac is the contact projected area obtained by correcting the curvature of the indenter tip using the standard method of the apparatus with fused silica of the standard sample. The indentation conditions are as follows: at room temperature, first the indenter is pressed to a depth of 200 nm for 5 seconds (i.e., 40 nm / s), then held at a depth of 200 nm for 2 seconds, and finally unloaded to 0 nm in 5 seconds. The composite modulus of the matte coat layer means the arithmetic mean of 10 or more measured values.
[0043]
number
[0044] In this disclosure, for the upper matte coat layer to satisfy the above-mentioned composite modulus, flexibility can be imparted to the coating film by using an emulsified urethane resin in the resin composition of the matte coat agent filling the matte coat layer if it is an inactive energy ray curable matte coat agent, or by using a polyfunctional urethane (meth)acrylate if it is an active energy ray curable matte coat agent. In addition, by incorporating flexible soft segments such as long-chain alkyl or polyether skeletons into the molecules of these urethane resins, or by increasing the ratio of such soft segments, a coating film with even greater flexibility can be formed. Furthermore, in the case of an active energy ray curable matte coat agent, the crosslinking density in the cured film can be adjusted by appropriately controlling the number of functional groups of the ethylenically unsaturated monomer Ma used in combination, making it possible to obtain a coating film with the desired composite modulus. Moreover, by selecting an ethylenically unsaturated monomer Ma that has undergone alkylene oxide modification, the crosslinking density and flexibility can be adjusted. In this way, the above range can be satisfied by controlling the molecular structure of the urethane resin and the ethylenically unsaturated monomer Ma and designing a flexible coating film.
[0045] In this disclosure, the absorbance ratio (a / b) of the matte coating layer is a value measured according to the following procedure.
[0046] The absorbance ratio (a / b) is determined by performing attenuated total reflection (ATR) measurement by Fourier transform infrared spectroscopy (FT-IR) according to the following conditions, measuring the absorbance (a) of the following peak (A) and the absorbance (b) of the following peak (B), and calculating the ratio thereof.
[0047] Apparatus: Fourier transform infrared spectrophotometer (equivalent to Nicolet iS5, manufactured by Thermo Fisher Scientific Co., Ltd.) Detector: MCT detector (liquid nitrogen cooling type) Prism: Germanium (Ge) Incident angle: 45° Wavenumber resolution: 4cm -1 Number of integrations: 32 times Gain: 4 Measurement wavenumber range: 700 to 2000 cm -1 Peak (A): 1070 to 1130 cm -1 One point with the highest absorbance in the region Peak (B): 1220 to 1280 cm -1 One point with the highest absorbance in the region
[0048] In the present disclosure, in order for the upper matte coat layer to satisfy the absorbance ratio (a / b) of the matte coat layer, among the compositions of the matte coat agent that forms the matte coat layer, in particular, by adjusting the blending ratio of the resin matrix, polyfunctional urethane (meth)acrylate, fine resin particles, and ethylenically unsaturated monomer Ma, the ratio of the ether component and the ester component in the cured film varies, making it possible to adjust to the desired absorbance ratio (a / b). For example, it is considered that the absorbance ratio (a / b) increases when the composition contains a large amount of an emulsified urethane resin using polyether polyol as a raw material, or an ethylenically unsaturated monomer Ma containing a large amount of polyethylene glycol in its molecular structure. In this way, the above range is satisfied by controlling and designing the skeleton and blending ratio of the above composition.
[0049] In some embodiments, the matte coating layer of the matte laminate includes a resin matrix having a urethane resin structure and an acrylic resin structure, and resin fine particles. The matte coating layer forms a film that covers the paper substrate, and the resin component constituting the film is the resin matrix. The resin fine particles are dispersed and contained in particulate form within the film-like resin matrix.
[0050] Because the resin matrix has a urethane resin structure, the flexibility of the urethane resin structure provides abrasion resistance to the matte coat layer. Since the resin matrix, which has a flexible urethane resin structure, contains resin microparticles, the resin microparticles protrude from the surface of the matte coat layer, forming an uneven surface and achieving a matte finish. This uneven surface is covered by the flexible resin matrix, resulting in a soft touch feel.
[0051] Because the resin matrix has an acrylic resin structure, the coexistence of a flexible urethane resin structure and an acrylic resin structure that is more rigid than the urethane resin structure can further improve the abrasion resistance of the resin matrix. In addition, it is expected that durability against chemicals such as alcohol (chemical resistance) and deterioration over time due to ultraviolet rays and hydrolysis can be suppressed.
[0052] In this case, if the uneven surface formed by the resin microparticles is rubbed through the flexible resin matrix, the coating formed by the resin matrix may be damaged, leading to a decrease in abrasion resistance. On the other hand, if the resin matrix is made of a hard material, it leads to a decrease in the soft-touch feel. Furthermore, if the resin matrix is made of a hard material, the resin microparticles are less likely to protrude from the surface of the resin matrix, leading to a decrease in matteness. Thus, in a matte coating layer in which resin microparticles are contained within a flexible resin matrix made of urethane resin, it is difficult to simultaneously exhibit the conflicting effects of matteness, abrasion resistance, and soft-touch feel.
[0053] According to several embodiments, by satisfying conditions (1) and (2), the matte coat layer can be made flexible while allowing resin microparticles to protrude appropriately from the surface of the resin matrix, thereby providing a soft touch. In the matte coat layer, the resin microparticles are contained within a flexible resin matrix with a urethane resin structure, so the surface of the matte coat layer is appropriately formed with uneven surfaces created by the resin microparticles. This allows the matte finish to be imparted to the matte coat layer. Furthermore, while the coating strength of the matte coat layer may decrease due to the uneven surface shape, in resin matrices with a urethane resin structure and an acrylic resin structure, the coating strength is increased when the surface roughness Sq is 0.5 to 3.5, thereby providing abrasion resistance to the matte coat layer. In addition, when the surface roughness Sq is 0.5 to 3.5 and the composite modulus is 4 GPa or less, the tactile feel of the uneven surface shape formed by the resin microparticles via the flexible resin matrix with a urethane resin structure is excellent, providing a soft touch.
[0054] According to several embodiments, by satisfying condition (3), the matte coat layer maintains a good balance between flexibility and hardness, resulting in excellent soft-touch feel and wear resistance. In the absorbance ratio (a / b), the absorbance (a) at peak (A) is mainly due to the absorption of COC stretching vibrations derived from ether among the resin components contained in the matte coat layer. Also, in the absorbance ratio (a / b), the absorbance (b) at peak (B) is mainly due to the absorption of COC stretching vibrations derived from ester among the resin components contained in the matte coat layer. For example, the matte coat layer is formed as a cured film using a matte coat agent, preferably an aqueous matte coat agent, and the desired effect can be expected by adjusting the ratio of ether bonds and ester bonds contained in this cured film after the curing reaction to satisfy condition (3). Furthermore, by measuring the absorbance ratio (a / b) using a germanium prism at an incident angle of 45°, it is possible to identify the matte coat layer portion of the matte laminate, for example, the surface layer of the matte coat layer, and measure the absorbance (a) and absorbance (b). In this way, by identifying and measuring only the matte coat layer portion, it is possible to identify the matte coat layer with greater accuracy in satisfying condition (3), and the desired effect can be expected.
[0055] In the matte coating layer of the matte laminate, the surface roughness Sq is preferably 0.5 or higher, more preferably 0.7 or higher, or even more preferably 0.8 or higher. Within these ranges, sufficient matte properties and a soft touch can be obtained. Furthermore, while frictional resistance occurs on smooth surfaces due to the increased contact area between the matte coating layer and the mating material, within these ranges, frictional resistance is reduced, and sufficient wear resistance can be obtained.
[0056] In the matte coat layer of a matte laminate, the surface roughness Sq is preferably 3.5 or less, more preferably 3.0 or less, or even more preferably 2.0 or less. Within these ranges, sufficient wear resistance can be obtained. If the surface roughness Sq increases, the uneven surface shape of the matte coat layer becomes larger, reducing the soft touch feel, and the stress on the matte coat layer due to friction with the matting material increases, potentially reducing wear resistance. In some embodiments, the composite elastic modulus of the matte coat layer is 4 GPa or less, so such stress is alleviated and wear resistance can be obtained. For example, in the matte coat layer of a matte laminate, the surface roughness Sq may be 0.5 to 3.5, 0.7 to 3.0, or 0.8 to 2.0.
[0057] In the matte coating layer of the matte laminate, the composite modulus is preferably 4 GPa or less, more preferably 3.5 GPa or less, or even more preferably 3.0 GPa or less. Within these ranges, sufficient abrasion resistance can be obtained. Furthermore, the resin matrix having a urethane resin structure becomes flexible, making it easier for resin fine particles to protrude from the surface of the matrix layer, thereby achieving a matte finish. In addition, the uneven surface shape formed by the resin fine particles comes into contact with the flexible resin matrix, resulting in a soft-touch feel.
[0058] In the matte coat layer of a matte laminate, the composite modulus is not particularly limited, but is preferably 0.005 GPa or higher, more preferably 0.01 GPa or higher, and even more preferably 0.05 GPa or higher. Within these ranges, the coating strength of the matte coat layer is increased, and the abrasion resistance can be further improved. For example, in the matte coat layer of a matte laminate, the composite modulus may be 0.005 to 4, 0.01 to 3.5, or 0.05 to 3.
[0059] In the matte coating layer of the matte laminate, the absorbance ratio (a / b) is preferably 0.40 or higher, more preferably 0.50 or higher, and even more preferably 0.60 or higher. Within these ranges, a good balance between the flexibility and hardness of the matte coating layer is maintained, resulting in excellent soft-touch feel and wear resistance.
[0060] In the matte coat layer of a matte laminate, the absorbance ratio (a / b) is preferably 1.50 or less, more preferably 1.40 or less, and even more preferably 1.30 or less. Within these ranges, a good balance between the flexibility and hardness of the matte coat layer is maintained, resulting in excellent soft-touch feel and wear resistance. For example, in the matte coat layer of a matte laminate, the absorbance ratio (a / b) may be 0.40 to 1.50, 0.50 to 1.40, or 0.60 to 1.30.
[0061] As described later, in the matte coat layer, if the resin raw material is a cured product of a resin raw material containing an emulsion-type urethane resin, an emulsion-type acrylic resin, and a curing agent, it is more preferable that the absorbance ratio (a / b) is 0.40 to 1.50, 0.50 to 1.00, or 0.60 to 0.80. Furthermore, in the matte coat layer, if the resin raw material is a cured product of a resin raw material containing a polyfunctional urethane (meth)acrylate and at least one selected from the group consisting of a hydroxyl group-containing ethylenically unsaturated monomer and an alkylene oxy group-containing ethylenically unsaturated monomer, or a cured product of a resin raw material further containing a curing agent, it is more preferable that the absorbance ratio (a / b) is 0.40 to 1.50, 0.60 to 1.40, or 0.80 to 1.30.
[0062] In the matte coating layer of a matte laminate, the gloss level is not particularly limited, but is preferably 2 or higher, more preferably 3 or higher, or even more preferably 4 or higher. Within these ranges, a certain degree of gloss is achieved, while a more luxurious matte finish can be obtained. In the matte coating layer of a matte laminate, the gloss level is not particularly limited, but is preferably 20 or lower, more preferably 15 or lower, or even more preferably 10 or lower. Within these ranges, a more aesthetically pleasing matte finish can be obtained in a matte coating layer having a resin matrix with a urethane resin structure and an acrylic resin structure in which resin fine particles are embedded.
[0063] In this disclosure, the glossiness of the matte coating layer can be measured according to the method disclosed in the examples.
[0064] In some embodiments, the substrate of the matte laminate may be either a permeable substrate or a non-permeable substrate, for example, a paper substrate. In some embodiments, the laminate is preferably a combination of a paper substrate and a matte coat layer.
[0065] Paper substrates such as ordinary paper or corrugated cardboard are used. While there are no specific requirements for the thickness of these paper substrates, a range of 0.05 mm to 1.0 mm is preferable. Corona treatment may also be applied to the printed surface. Furthermore, the paper substrate may be coated with a metal such as aluminum to enhance its aesthetic appeal. This coating provides the paper substrate with a high-quality feel and a unique appearance. Surface coatings using acrylic resin, urethane resin, polyester resin, polyolefin resin, and other resins are also possible. This improves the durability and water resistance of the paper substrate, making it usable in a variety of environments. In addition to corona treatment, various other surface treatments may be applied, improving printability, adhesion, etc. Specific examples include coated cardboard and Mariecoat paper. These are widely used in printing and packaging applications, and the paper substrates provided can meet the diverse needs of users in various forms.
[0066] The thickness of the matte coat layer is usually preferably in the range of 1 to 50 μm. In particular, the range of 1 to 30 μm is more preferred, the range of 1 to 20 μm is even more preferred, the range of 1 to 10 μm is even more preferred, the range of 1 to 7 μm is particularly preferred, and it may also be 2 to 3 μm. By setting the thickness within this appropriate range, the uniformity and durability of the matte coat layer after curing are further improved, and the resin fine particles protrude appropriately from the surface of the cured layer, further improving the matte properties.
[0067] The method for measuring the thickness of the matte coat layer involves measuring the distance from the substrate or the interface between the printed layer and the coat layer to the apex of the spherical curved surface of the fine particles protruding from the surface at five randomly selected measurement points from a cross-sectional image of the matte coat layer, and then using the average value of these measurements. For details, please refer to the measurement method disclosed in the examples.
[0068] In some embodiments, the resin raw material included in the matte coat layer may be a cured product of resin raw material (1) comprising an emulsion-type urethane resin, an emulsion-type acrylic resin, and a curing agent. The cured product of resin raw material (1) can be obtained using an inactive energy ray-curable aqueous matte coat agent. In other examples, the resin raw material included in the matte coat layer may be a cured product of resin raw material (2) comprising a polyfunctional urethane (meth)acrylate and at least one selected from the group consisting of hydroxyl group-containing ethylenically unsaturated monomers and alkylene oxy group-containing ethylenically unsaturated monomers. Resin raw material (2) may further contain a curing agent. The cured product of resin raw material (2) can be obtained using an active energy ray-curable aqueous matte coat agent.
[0069] In some embodiments, the matte coat layer of a matte laminate can be formed using an aqueous matte coating agent comprising a resin raw material for forming a resin matrix having a urethane resin structure and an acrylic resin structure, resin fine particles, and an aqueous medium. By using an aqueous matte coating agent, the film strength of the resin matrix in the resulting matte coat layer can be increased, and the composite elastic modulus of the matte coat layer can be made more appropriate, further improving abrasion resistance. Furthermore, by using an aqueous matte coating agent, even if residual solvent is present in the resulting matte coat layer, a matte coat layer with low skin irritation can be obtained.
[0070] In one example, a matte coat layer can be formed using an inactive energy ray-curable aqueous matte coat agent containing an emulsion resin, resin fine particles, and a curing agent in an aqueous medium. The inactive energy ray-curable aqueous matte coat agent may contain an emulsion urethane resin, an emulsion acrylic resin, and a curing agent as resin raw materials.
[0071] In another example, a matte coat layer can be formed using an active energy ray-curable aqueous matte coat agent containing each polymerizable compound, resin fine particles, and optionally a curing agent in an aqueous medium. The active energy ray-curable aqueous matte coat agent may contain a polyfunctional urethane (meth)acrylate and other unsaturated monomers as resin raw materials. The other unsaturated monomer may be, for example, at least one selected from the group consisting of hydroxyl group-containing ethylenically unsaturated monomers and alkylene oxy group-containing ethylenically unsaturated monomers. In the following description, at least one selected from the group consisting of hydroxyl group-containing ethylenically unsaturated monomers and alkylene oxy group-containing ethylenically unsaturated monomers will also be referred to as ethylenically unsaturated monomer Ma.
[0072] In the matte coating layer, the resin fine particles may be present in amounts of 10 to 200 parts by mass, 15 to 180 parts by mass, or 20 to 150 parts by mass per 100 parts by mass of the total solid content of the resin matrix. Furthermore, it is preferable that the resin fine particles are present in amounts of 30 to 150 parts by mass, 40 to 130 parts by mass, or 45 to 80 parts by mass per 100 parts by mass of the total solid content of the resin matrix.
[0073] Furthermore, the constituent components having a urethane resin structure (urethane resin or urethane acrylate) may be present in amounts of 15-100% by mass, 30-95% by mass, or 40-90% by mass relative to the total solid content of the resin matrix. Furthermore, the constituent components having an acrylic resin structure may be 0-60% by mass, 5-50% by mass, or 10-40% by mass relative to the total solid content of the resin matrix. These can be determined from the mass ratio relative to the total solid content of the resin matrix. The same applies hereafter.
[0074] When the matte coat layer contains structural units derived from emulsion-type urethane resin and structural units derived from emulsion-type acrylic resin, and cross-linked structures derived from the curing agent, the emulsion-type urethane resin solids may be 30-100% by mass, 40-95% by mass, or 45-80% by mass relative to the total solids content of the resin matrix. The curing agent may be 1-40% by mass, 2-30% by mass, or 3-20% by mass relative to the total solids content of the resin matrix. The emulsion-type acrylic resin solids may be 0.1-50% by mass, 1-40% by mass, or 10-30% by mass relative to the total solids content of the resin matrix.
[0075] If the matte coat layer contains structural units derived from polyfunctional urethane (meth)acrylate, the amount of polyfunctional urethane (meth)acrylate may be 10-100% by mass, 12-80% by mass, or 15-50% by mass relative to the total solid content of the resin matrix. If it contains ethylenically unsaturated monomer Ma, the total amount of ethylenically unsaturated monomer Ma may be 0.03-90% by mass, 5-80% by mass, or 10-70% by mass relative to the total solid content of the resin matrix. If it contains cross-linked structures derived from the curing agent, the amount of curing agent may be 2-30% by mass, 3-20% by mass, or 4-15% by mass relative to the total solid content of the resin matrix.
[0076] In some embodiments of the matte laminate, the paper substrate may include a printed layer. The printed layer is formed between the paper substrate and the matte coat layer, and any additional layer, such as a primer layer, may be formed between these layers. Details of the printed layer will be described later.
[0077] In some embodiments, the laminate can be suitably used to constitute a packaging material. The laminate may be used alone as a packaging material, or it may be used in combination with other materials. The packaging material may be a packaging container.
[0078] <Water-based matte coating agent> In some embodiments, the aqueous matte coating agent preferably comprises a resin raw material for forming a resin matrix having a urethane resin structure and an acrylic resin structure, resin fine particles, and an aqueous medium. As the aqueous matte coating agent, inactive energy ray curable aqueous matte coating agents, active energy ray curable aqueous matte coating agents, and the like can be used.
[0079] The inactive energy ray-curable aqueous matte coating agent may contain an emulsion-type urethane resin, an emulsion-type acrylic resin, resin fine particles, and a curing agent in an aqueous medium. In this case, the inactive energy ray-curable aqueous matte coating agent may be provided as a two-component type, consisting of a first liquid containing an emulsion-type urethane resin and an emulsion-type acrylic resin, and a second liquid containing a curing agent. For example, when using a two-component inactive energy ray-curable aqueous matte coating agent, a method for producing a matte laminate can be provided, which includes the steps of mixing the first liquid and the second liquid to obtain an aqueous matte coating agent, and printing the aqueous matte coating agent onto a substrate.
[0080] One example of a method for manufacturing laminates involves printing or coating a substrate with an inactive energy ray-curable aqueous matte coating agent, drying it using far-infrared radiation, and then optionally adding a heating step to accelerate curing and obtain a matte coating layer. In some cases, it is preferable to repeat this process multiple times. Another example involves pre-forming a printed layer on the substrate using printing ink, then re-printing or coating the inactive energy ray-curable aqueous matte coating agent onto the printed layer, and then optionally performing a heat treatment to accelerate curing and obtain a matte coating layer. Due to their simplicity and efficient processes, these methods for manufacturing laminates can reduce costs and improve production efficiency.
[0081] The printing and coating methods for the inactive energy ray curing aqueous matte coating agent are not particularly limited and include, for example, spray, shower, dipping, flow coating, gravure printing, flexographic printing, offset printing, roll, spin, dispenser, inkjet printing, and screen printing. Among these, gravure printing and flexographic printing are preferred because they allow for high-speed printing.
[0082] The active energy ray curing aqueous matte coating agent may contain a polyfunctional urethane (meth)acrylate, resin fine particles, and optionally a curing agent in an aqueous medium.
[0083] One example of a method for manufacturing laminates involves printing or coating a substrate with an active energy ray-curable aqueous matte coating agent, drying it using far-infrared radiation, and then curing it by irradiation with active energy rays. In some cases, it is preferable to repeat this process multiple times. Another example involves pre-forming a printed layer on the substrate using printing ink, then re-printing or coating the substrate with an active energy ray-curable aqueous matte coating agent over the printed layer, and finally curing it by irradiation with active energy rays. Due to their simplicity and efficient processes, these methods for manufacturing laminates can reduce costs and improve production efficiency.
[0084] In this configuration, it is preferable to use ultraviolet light, such as far-ultraviolet, ultraviolet, or near-ultraviolet light, as the active energy ray. This is because curing with ultraviolet light is desirable in terms of curing speed, availability of irradiation equipment, and cost. Furthermore, it is also possible to use electron beams, proton beams, etc., in which case curing is possible without the use of a photopolymerization initiator, but for the reasons mentioned above, the curing method using ultraviolet light is particularly recommended. Thus, the curing method can be selected according to the type of active energy ray, and in certain embodiments, the curing method using ultraviolet light is preferred. This makes it possible to achieve an efficient and economical curing process.
[0085] In curing methods using ultraviolet irradiation, for example, high-pressure mercury lamps, ultra-high-pressure mercury lamps, carbon arc lamps, metal halide lamps, xenon lamps, chemical lamps, electrodeless discharge lamps, and LEDs can be used as ultraviolet irradiation devices. The light emitted from these devices has a wavelength range of 150 nm to 450 nm, and it is preferable to perform ultraviolet irradiation using light in this wavelength range. The integrated amount of ultraviolet light irradiated is 30 mJ / cm². 2 From 5000 mJ / cm 2 This is acceptable, preferably 100 mJ / cm². 2 From 1000 mJ / cm 2It is preferable that the curing reaction is accelerated by UV irradiation within these ranges. Furthermore, heat treatment may be applied after UV irradiation. This heat treatment improves the completeness of curing and allows for a more reliable curing effect.
[0086] A drying process may be included between the application of the matte coating agent to the substrate and the irradiation with active energy rays, by heating the coating atmosphere, heating the substrate, etc. By removing the aqueous medium from the matte coating agent on the substrate surface through the drying process, the effectiveness of the subsequent irradiation with active energy rays can be further enhanced.
[0087] The printing and coating methods for the active energy ray-curable aqueous matte coating agent may be those listed above for the inactive energy ray-curable aqueous matte coating agent, and gravure printing and flexographic printing are preferred because they allow for high-speed printing.
[0088] In some embodiments, when a printing layer is further provided between the paper substrate and the matte coat layer, the printing ink for forming the printing layer may be, for example, an aqueous ink, an oil-based ink, an active energy ray-curable ink, etc. The printing layer can be formed by, for example, gravure printing, flexographic printing, offset printing, screen printing, inkjet printing, etc. Preferably, gravure ink, flexographic ink, or offset ink is used, and among these, active energy ray-curable offset ink and active energy ray-curable flexographic ink are preferred, and active energy ray-curable offset ink is more preferred.
[0089] The thickness of the printed layer is preferably 0.1 to 15 μm. The thickness of the printed layer is more preferably 0.5 to 12 μm, and may be 10 μm or less, 5 μm or less, or 3 μm or less, and more preferably less than 1 μm. The printing ink may be organic solvent-based, water-based, or oil-based, and may also be an active energy ray-curable ink, such as an ultraviolet-curable ink. Multiple of the above printing inks may be combined to form the printed layer, and the printed layer can be formed by drying or ultraviolet curing after printing. When a matte coat layer is formed on the printed layer, the thickness of the matte coat layer formed on the printed layer is preferably 1 μm or more, 2 μm or more, or 3 μm or more.
[0090] When the matte coating agent contains an aqueous medium, a thin film coating can be applied. Thin film coating is also possible when using gravure printing and flexographic printing, and even when printing at high speeds. Thin film coating causes resin microparticles to protrude from the surface of the matte coating layer, forming an uneven surface, thereby providing a more aesthetically pleasing matte finish. Furthermore, because the resin microparticles protrude from the surface of the matte coating layer, which is given flexibility by the urethane resin structure contained in the resin matrix, the abrasion resistance of the matte coating layer can also be improved. The matte coating agent may be applied in multiple layers to form the matte coating layer.
[0091] One example of a method for forming a multilayer matte coating is to apply a matte coating agent to the substrate to form the first layer, and then apply another layer of matte coating agent to the first layer to form the second layer. Heat curing or irradiation with active energy rays may be performed after the formation of each layer or only after the formation of the last layer. By applying the matte coating agent as the first layer and then providing a drying step to remove the aqueous medium from the coating film, and then applying the matte coating agent to the uncured or partially cured first layer to form the second layer, the process can be simplified, and the adhesion between the first and second layers can be further improved. Furthermore, with this method, the thin film coating of the second layer makes it easier for resin fine particles to protrude from the surface of the matte coating layer, resulting in a matte finish with superior aesthetic appeal.
[0092] In some embodiments, the aqueous matte coating agent preferably contains 10 to 80% by mass of aqueous medium, more preferably 20 to 70% by mass, and even more preferably 25 to 65% by mass, relative to the total mass of the aqueous matte coating agent. Within these ranges, the skin irritation of the aqueous matte coating agent is reduced, thereby improving the handling of the aqueous matte coating agent in the manufacturing method of the matte laminate. Furthermore, when the aqueous matte coating agent contains a large amount of aqueous medium, the aqueous matte coating agent can be applied thinly to achieve a thin matte coating layer. This allows resin fine particles to protrude appropriately from the resin matrix film, further enhancing the desired effect.
[0093] The viscosity of the aqueous matte coating agent at 25°C is preferably 10 to 2000 mPa·s, 30 to 1500 mPa·s, or 50 to 1300 mPa·s, and more preferably 100 to 1000 mPa·s.
[0094] <Inactive energy ray curing type aqueous matte coating agent> Below, we will describe a non-active energy ray curing type aqueous matte coating agent as an example of an aqueous matte coating agent.
[0095] One embodiment of the inactive energy ray curable aqueous matte coating agent comprises an emulsion resin, resin fine particles, an aqueous medium, and a curing agent, wherein the emulsion resin includes an emulsion urethane resin and an emulsion acrylic resin. This inactive energy ray curable aqueous matte coating agent offers excellent workability and environmental friendliness, and when the coating film is cured, it can form a matte coating layer with excellent matte properties and adhesion to the substrate. Since the emulsion resin includes an emulsion urethane resin and an emulsion acrylic resin, it functions as a resin raw material for forming a resin matrix having a urethane resin structure and an acrylic resin structure.
[0096] Inactive energy ray curing aqueous matte coating agents use an aqueous medium, thus reducing or eliminating the need for organic solvents and further reducing the amount of reactive compounds used, thereby improving workability and environmental friendliness. The inclusion of an aqueous medium in inactive energy ray curing aqueous matte coating agents reduces the amount of volatile organic components. Furthermore, the inclusion of an aqueous medium in inactive energy ray curing aqueous matte coating agents reduces the content of reactive compounds, thus lowering the overall reactivity of the inactive energy ray curing aqueous matte coating agent and improving handling. Inactive energy ray curing aqueous matte coating agents are applied to a substrate, and a coating film is formed as the curing reaction proceeds while the aqueous medium is removed. The inclusion of an emulsified urethane resin in inactive energy ray curing aqueous matte coating agents allows for substrate adhesion and abrasion resistance even with an aqueous solution, and the inclusion of an emulsified acrylic resin further enhances abrasion resistance.
[0097] Furthermore, because the inactive energy ray curing aqueous matte coating agent uses an aqueous medium, it can be used to apply a thin film coating to a substrate. When the resulting matte coating layer is thin, resin fine particles protrude from the surface of the matte coating layer, and the resulting uneven shape makes it easier to obtain a matte finish with excellent aesthetic appeal.
[0098] Furthermore, by using a non-active energy ray curing aqueous matte coating agent, the coating strength of the cured film using emulsion acrylic resin, the flexibility of the cured film using emulsion urethane resin, and the flexibility of the resin fine particles distributed in the cured film result in a matte coating layer that is both abrasion-resistant and flexible, with a smooth texture and excellent aesthetic appeal.
[0099] Furthermore, in addition to the coating strength of the cured film using emulsion-type acrylic resin, the flexibility of the cured film using emulsion-type urethane resin, and the flexibility of the resin fine particles distributed in the cured film, the emulsion-type acrylic resin and emulsion-type urethane resin exhibit hydrophilicity to the extent that they can be emulsified in an aqueous medium. As a result, the surface of the matte coat layer maintains appropriate strength while possessing flexibility, and the occurrence of damage due to repeated friction can be reduced. For example, when multiple laminates are arranged with the matte coat layers overlapping each other, the occurrence of damage due to repeated friction between the matte coat layers can be reduced. Therefore, it is possible to provide laminates with excellent scratch resistance at the consumer use stage and even at the distribution stage.
[0100] <Acid value and hydroxyl value of emulsion-type acrylic resin and emulsion-type urethane resin> The non-active energy ray curable aqueous matte coating agent preferably has an acid value of 40 mgKOH / g or less and a hydroxyl value of 20 mgKOH / g or more relative to the total mass of the emulsion acrylic resin and emulsion urethane resin.
[0101] The acid value (also known as the weighted average acid value; hereinafter also referred to as acid value A1) relative to the total mass of the emulsion-type acrylic resin and emulsion-type urethane resin is preferably 40 mg KOH / g or less, 20 mg KOH / g or less, or 10 mg KOH / g or less. Within these ranges, the water resistance and alcohol resistance of the matte coat layer can be further enhanced while maintaining the stability of the inactive energy ray-curable aqueous matte coat agent, and the abrasion resistance can be further improved.
[0102] The lower limit of this acid value A1 may be 0 mg KOH / g or higher, 1 mg KOH / g or higher, or 5 mg KOH / g or higher, from the viewpoint of the reactivity of the stability of the inactive energy ray-curable aqueous matte coating agent. Within these ranges, the stability of the inactive energy ray-curable aqueous matte coating agent can be further improved. For example, this acid value A1 may be 0 to 40 mg KOH / g, 1 to 20 mg KOH / g, or 5 to 10 mg KOH / g.
[0103] In this disclosure, the acid value of the resin is expressed as the number of milligrams of potassium hydroxide required to neutralize 1 g of the sample. The acid value can be measured according to the method described in JIS K 0070 (1992).
[0104] The acid value A1 can be determined from the acid value of the emulsion-type acrylic resin and the acid value of the emulsion-type urethane resin as follows. Total mass of emulsion acrylic resin: XM Acid value of emulsified acrylic resin: XA Total mass of emulsified urethane resin: YM Acid value of emulsified urethane resin: YA A1=XA×(XM / (XM+YM))+YA×(YM / (XM+YM))
[0105] The hydroxyl value (also known as the weighted average hydroxyl value; hereinafter also referred to as hydroxyl value H1) relative to the total mass of the emulsion-type acrylic resin and emulsion-type urethane resin is preferably 20 mg KOH / g or more, 30 mg KOH / g or more, or 40 mg KOH / g or more, from the viewpoint of reactivity with the curing agent. Within these ranges, the film strength of the matte coat layer can be further increased by reaction with the curing agent while maintaining the stability of the inactive energy ray-curable aqueous matte coat agent, thereby further improving water resistance and alcohol resistance. Furthermore, abrasion resistance can be further improved.
[0106] The upper limit of this hydroxyl value H1 may be 100 mg KOH / g or less, 80 mg KOH / g or less, or 60 mg KOH / g or less. Within these ranges, sufficient water resistance and abrasion resistance can be obtained for the matte coating layer. For example, this hydroxyl value H1 may be 20-100 mg KOH / g, 30-80 mg KOH / g, or 40-60 mg KOH / g.
[0107] In this disclosure, the hydroxyl value is expressed as the number of milligrams of potassium hydroxide required to neutralize the acetic acid needed to acetylate 1 g of a sample. The hydroxyl value can be measured according to the method described in JIS K 0070 (1992).
[0108] The acid value H1 can be determined from the hydroxyl value of the emulsion-type acrylic resin and the hydroxyl value of the emulsion-type urethane resin as follows. Total mass of emulsion acrylic resin: XM Hydroxyl value of emulsified acrylic resin: XH Total mass of emulsified urethane resin: YM Hydroxyl value of emulsified urethane resin: YH H1=XH×(XM / (XM+YM))+YH×(YM / (XM+YM))
[0109] The acid value (hereinafter also referred to as acid value Au) of the emulsified urethane resin may be 0-50 mgKOH / g, 1-30 mgKOH / g, or 5-10 mgKOH / g. The hydroxyl value (hereinafter also referred to as hydroxyl value Hu) of the emulsified urethane resin may be 10-60 mgKOH / g, 20-50 mgKOH / g, or 30-40 mgKOH / g.
[0110] The acid value of the emulsion-type acrylic resin (hereinafter also referred to as acid value Aa) may be 1-100 mg KOH / g, 5-50 mg KOH / g, or 10-30 mg KOH / g. The hydroxyl value of the emulsion-type acrylic resin (hereinafter also referred to as hydroxyl value Ha) may be 20-200 mg KOH / g, 60-170 mg KOH / g, or 80-100 mg KOH / g.
[0111] The absolute difference between the acid value of the emulsified acrylic resin and the acid value of the urethane resin is preferably 100 or less, 50 or less, 20 or less, or 10 or less, and preferably 0.1 or more, 1 or more, or 3 or more. Within these ranges, even when two or more resins are used in combination in a non-active energy ray curable aqueous matte coating agent, dispersion stability is maintained more stably, the viscosity of the coating agent is improved, and the uniformity of components in the matte coating layer can be further improved.
[0112] <Emulsified urethane resin> The emulsified urethane resin preferably exhibits hydrophilicity and is soluble or dispersible in aqueous media. The emulsified urethane resin is preferably provided as an aqueous urethane resin emulsion. An advantage of this aqueous urethane resin emulsion is that, being an aqueous dispersion, it releases fewer volatile organic compounds (VOCs). Furthermore, the inclusion of the emulsified urethane resin in the aqueous media helps maintain the stability of the non-active energy ray curable aqueous matte coating agent. Additionally, the emulsified urethane resin can impart flexibility and abrasion resistance to the matte coating layer.
[0113] The emulsion-type urethane resin may be, for example, a urethane resin synthesized from a polyol, a hydroxy acid, and a polyisocyanate, or a urethane resin having urea bonds (urethane urea resin) obtained by extending the chain of a urethane prepolymer having isocyanate groups at the terminals, synthesized from a polyol, a hydroxy acid, and a polyisocyanate, with a polyamine.
[0114] Emulsified urethane resins can be made aqueous by introducing and neutralizing ionic groups into the resin during the reaction of a polyol and a polyisocyanate. The ionic groups may be acidic or basic groups such as carboxyl groups, sulfonic acid groups, phosphate groups, phosphonic acid groups, or quaternary ammonium bases, with acidic groups being preferred and carboxyl groups being particularly preferred.
[0115] One method for introducing carboxyl groups into emulsified urethane resins is to use compounds having active hydrogen that can react with the following anionic groups and isocyanate groups.
[0116] Examples of compounds having active hydrogen that can react with anionic groups and isocyanate groups include dimethylolalkanoates such as 2,2-dimethylolpropionic acid, 2,2-dimethylolbutanoic acid, 2,2-dimethylolbutyric acid, and 2,2-dimethylolvaleric acid; diamine-type amino acids such as glutamine, asparagine, lysine, diaminopropionic acid, ornithine, diaminobenzoic acid, and diaminobenzenesulfonic acid; and monoamine-type amino acids such as glycine, alanine, glutamic acid, taurine, aspartic acid, aminobutyric acid, valine, aminocaproic acid, aminobenzoic acid, aminoisophthalic acid, and sulfamic acid. These may be used individually or in combination of two or more.
[0117] In particular, from the viewpoint of compatibility and reactivity with other urethane raw materials, it is preferable to use 2,2-dimethylolpropionic acid and / or 2,2-dimethylolbutanoic acid. When polyhydroxycarboxylic acid is used in the production of emulsion-type urethane resin, the hydroxyl group reacts with the polyisocyanate to form a urethane bond, but the carboxyl group is poorly reactive with the isocyanate group, so most of it remains as a carboxyl group and is neutralized in the emulsion-type urethane resin, becoming an acid group that converts it to aqueous.
[0118] (Polyol) Polyols do not include hydroxy acids, which will be discussed later. Examples of polyols include polyester polyols, polyether polyols, polylactone polyols, polycarbonate polyols, polyolefin polyols, dimer ols, and hydrogenated dimer ols. These may be used individually or in combination of two or more. The emulsion-type urethane resin preferably contains a constituent unit consisting of at least one polyol selected from polyester polyols, polyether polyols, and polycarbonate polyols. The number-average molecular weight of the polyol is preferably 500 to 5000.
[0119] Polyester polyol The polyester polyol is preferably in a form having a structural unit consisting of a diol containing a dibasic acid and a branched diol. Examples of dibasic acids include sebacic acid, adipic acid, and succinic acid. The branched diol is a form in which at least one hydrogen atom on the carbon of an alkylene glycol has a substituent. Specifically, it is preferable to contain at least one selected from the group consisting of propylene glycol, 3-methyl-1,5-pentanediol, neopentyl glycol, 2-butyl-2-ethyl-1,3-propanediol, and 2-methyl-1,3-propanediol in an amount of 50% by mass or more relative to the total mass of the diol.
[0120] Polyether polyol Examples of polyether polyols include polyethylene glycol, polypropylene glycol, polytrimethylene glycol, polytetramethylene glycol, and copolymers thereof. More preferably, the emulsion-type urethane resin contains constituent units derived from polyethylene glycol. The constituent units derived from polyethylene glycol are preferably contained in an amount of 0.1 to 25% by mass, more preferably 2 to 15% by mass, and even more preferably 2 to 10% by mass, based on the total mass of the emulsion-type urethane resin.
[0121] Polycarbonate polyol The polycarbonate polyol is not limited by its manufacturing method or the type of diol that constitutes it, but examples include polycondensates resulting from transesterification reactions between diols and carbonate compounds. Preferably, the polycarbonate polyol is an alicyclic and / or aliphatic polycarbonate diol.
[0122] Examples of diols include ethylene glycol, 1,2-propanediol, 1,3-propanediol, 1,4-butanediol, 1,5-pentanediol, 2-methyl-1,3-propanediol, neopentyl glycol, 3-methyl-1,5-pentanediol, 1,6-hexanediol, 1,8-octanediol, 1,9-nonanediol, 2-methyl-1,8-octanediol, 1,10-decanediol, 2-butyl-2-ethyl-1,3-propanediol, 1,4-butynediol, 2,2,4-trimethyl-1,3-pentanediol, 1,4-cyclohexanedimethanol, diethylene glycol, polypropylene glycol, and dipropylene glycol. These may be used individually or in combination of two or more. The polycarbonate polyol preferably has a diol structure derived from an alkanediol, particularly 1,6-hexanediol.
[0123] Examples of carbonate compounds include dialkyl carbonates, diaryl carbonates, and alkylene carbonates. Specific examples of carbonate compounds include dialkyl carbonates such as dimethyl carbonate, diethyl carbonate, and dibutyl carbonate, diaryl carbonates such as diphenyl carbonate, and alkylene carbonates such as ethylene carbonate. These may be used individually or in combination of two or more.
[0124] (Hydroxy acid) Hydroxy acids are not limited to those listed below, but polyols containing carboxyl groups can be used. Examples include dimethylolalkanoates such as 2,2-dimethylolpropionic acid, 2,2-dimethylolbutyric acid, and 2,2-dimethylolvaleric acid. These may be used alone or in combination of two or more. Hydroxy acids are used in the manufacturing process of aqueous polyurethane resins, and their carboxyl groups are introduced into the resulting polyurethane resin, giving it an acid value. Unreacted carboxyl groups are neutralized to make the resin aqueous.
[0125] (Polyisocyanate) Examples of polyisocyanates include aromatic diisocyanates, aliphatic diisocyanates, and alicyclic diisocyanates. These may also exist as trimers forming an isocyanurate ring structure.
[0126] Examples of aromatic diisocyanates include 1,5-naphthylene diisocyanate, 4,4'-diphenylmethane diisocyanate (MDI), 4,4'-diphenyldimethylmethane diisocyanate, 4,4'-dibenzyli isocyanate, dialkyldiphenylmethane diisocyanate, tetraalkyldiphenylmethane diisocyanate, 1,3-phenylenedi isocyanate, 1,4-phenylenedi isocyanate, and tolylene diisocyanate.
[0127] Examples of aliphatic diisocyanates include butane-1,4-diisocyanate, hexamethylene diisocyanate, isopropyl diisocyanate, methylene diisocyanate, 2,2,4-trimethylhexamethylene diisocyanate, and lysine diisocyanate.
[0128] Examples of alicyclic diisocyanates include cyclohexane-1,4-diisocyanate, xylylene diisocyanate, isophorone diisocyanate, dicyclohexylmethane-4,4'-diisocyanate, 1,3-bis(isocyanatomethyl)cyclohexane, methylcyclohexane diisocyanate, norbornane diisocyanate, m-tetramethylxylylene diisocyanate, hydrogenated 4,4-diphenylmethane diisocyanate, and dimer isocyanates obtained by converting the carboxyl groups of dimer acids to isocyanate groups. These may be used individually or in combination of two or more.
[0129] Preferably, it is at least one selected from tolylene diisocyanate, isophorone diisocyanate, dicyclohexylmethane-4,4'-diisocyanate, m-tetramethylxylylene diisocyanate, xylylene diisocyanate, bis(isocyanatomethyl)cyclohexane, hexamethylene diisocyanate, and trimers of hexamethylene diisocyanate.
[0130] (Polyamines) Compounds that can be used as polyamines include various known amines, such as 2-hydroxyethylpropylenediamine, di-2-hydroxyethylethylenediamine, di-2-hydroxyethylpropylenediamine, 2-hydroxypropylethylenediamine, di-2-hydroxypropylethylenediamine, ethylenediamine, propylenediamine, hexamethylenediamine, 2-methyl-1,5-pentanediamine, isophoronediamine, dicyclohexylmethane-4,4'-diamine, and dimeramines obtained by converting the carboxyl group of a dimer acid to an amino group. These may be used individually or in combination of two or more.
[0131] (Reaction inhibitor) Reaction stoppers can also be used in combination with polyamines. Examples of reaction stoppers include dialkylamines such as di-n-dibutylamine, monoethanolamine, diethanolamine, 2-amino-2-methyl-1-propanol, tri(hydroxymethyl)aminomethane, 2-amino-2-ethyl-1,3-propanediol, N-di-2-hydroxyethylethylenediamine, N-di-2-hydroxyethylpropylenediamine, N-di-2-hydroxypropylethylenediamine, 2-(2-aminoethylamino)ethanol, and other amines having hydroxyl groups, as well as monoamine-type amino acids such as glycine, alanine, glutamic acid, taurine, aspartic acid, aminobutyric acid, valine, aminocaproic acid, aminobenzoic acid, aminoisophthalic acid, and sulfamic acid. These may be used alone or in combination of two or more.
[0132] (Neutralizing agent) To make polyurethane resins aqueous, it is preferable to neutralize carboxyl groups and other ionizable groups in the resin with a basic compound. Examples of basic compounds include sodium hydroxide, potassium hydroxide, ammonia, methylamine, ethylamine, propylamine, butylamine, hexylamine, octylamine, ethanolamine, propanolamine, diethanolamine, N-methyldiethanolamine, dimethylamine, diethylamine, triethylamine, N,N-dimethylethanolamine, 2-dimethylamino-2-methyl-1-propanol, 2-amino-2-methyl-1-propanol, and morpholine. These may be used individually or in combination of two or more. From the viewpoint of water resistance of printed materials and residual odor, triethylamine and ammonia are preferred.
[0133] (synthesis method) Polyurethane resins can be manufactured by known methods as appropriate. Examples include the acetone method, which uses an organic solvent that is inert and hydrophilic to isocyanates, and solvent-free synthesis methods that do not use any solvents. For example, the method described in Japanese Patent Publication No. 2013-234214 can be used as appropriate.
[0134] The emulsified urethane resin may have a weight-average molecular weight (Mw) of 1,000 to 100,000, 5,000 to 80,000, or 10,000 to 50,000. Within these ranges, it is possible to improve the coatability while appropriately maintaining the viscosity of the inactive energy ray curable aqueous matte coating agent. The resulting matte coating layer has uniformity and maintains appropriate hardness, further improving substrate adhesion and abrasion resistance.
[0135] The emulsified urethane resin preferably has a glass transition temperature (Tg) of -80 to 120°C, more preferably -60 to 100°C, and even more preferably -50 to 90°C. Within these ranges, the adhesion and abrasion resistance of the matte coat layer to the substrate can be further improved. A glass transition temperature of 120°C or lower for the emulsified urethane resin can impart more matte properties to the matte coat layer. A glass transition temperature of -80°C or higher can impart flexibility to the matte coat layer, further improving its abrasion resistance.
[0136] The emulsion-type urethane resin preferably has an average particle size (mode diameter) of less than 1 μm. For example, the average particle size (mode diameter) of the emulsion-type urethane resin is preferably between 10 nm and less than 0.9 μm, between 30 nm and 0.6 μm, or between 30 nm and 0.5 μm. Within these ranges, the stability and applicability of the inactive energy ray-curable aqueous matte coating agent, as well as the uniformity of the matte coating layer, can be further improved.
[0137] The average particle size (mode diameter) of emulsified urethane resin is the volume-based mode diameter measured by dynamic light scattering, and can be measured using, for example, NanoTrac UPA (manufactured by MicroTrac Bell). A sample of emulsified urethane resin diluted 500 times with water is recommended. The mode diameter (most frequent value) represents the particle size with the highest frequency of occurrence in the particle size distribution (the same applies below).
[0138] The emulsified urethane resin solids content is preferably 5-50% by mass, 10-45% by mass, or 15-40% by mass relative to the total solids content of the inactive energy ray curable aqueous matte coating agent. Within these ranges, the stability of the inactive energy ray curable aqueous matte coating agent and the appearance of the matte coating layer can be further improved.
[0139] <Emulsified acrylic resin> The emulsion-type acrylic resin preferably exhibits hydrophilicity and is soluble or dispersible in aqueous media. The emulsion-type acrylic resin is preferably provided as an aqueous acrylic resin emulsion. An advantage of this aqueous acrylic resin emulsion is that, being an aqueous dispersion, it releases fewer volatile organic compounds (VOCs). Furthermore, the inclusion of the emulsion-type acrylic resin in the aqueous media helps maintain the stability of the non-active energy ray curable aqueous matte coating agent. Additionally, the emulsion-type acrylic resin can impart film strength and abrasion resistance to the matte coating layer, particularly improving scratch resistance.
[0140] Emulsified acrylic resins have acrylic monomer constituent units. Furthermore, emulsion-type acrylic resins obtained by copolymerizing styrene monomers, maleic acid monomers, etc., are also preferred.
[0141] Emulsified acrylic resins are preferably those having ionic groups and being aqueous in the presence of an emulsifier and / or a basic compound. The ionic groups may be acidic or basic groups such as carboxyl groups, sulfonic acid groups, phosphoric acid groups, phosphonic acid groups, and quaternary ammonium bases, with acidic groups being preferred and carboxyl groups being particularly preferred. One method for introducing carboxyl groups is to use an ethylenically unsaturated compound having a carboxyl group as a monomer. Examples of ethylenically unsaturated compounds having a carboxyl group include (meth)acrylic acid; carboxyl group-containing (meth)acrylates such as 2-(meth)acryloyloxypropyl phthalate, β-carboxyethyl (meth)acrylate, (meth)acrylic acid dimer, and ω-carboxy-polycaprolactone mono(meth)acrylate; polymerizable unsaturated carboxylic acids such as itaconic acid, maleic acid, fumaric acid, and crotonic acid, and their anhydrides. These can be used individually or in combination of two or more.
[0142] Examples of the above acrylic monomers include aromatic group-containing acrylic monomers such as benzyl (meth)acrylate, phenoxyethyl (meth)acrylate, phenoxydiethylene glycol (meth)acrylate, phenoxytetraethylene glycol (meth)acrylate, phenoxyhexaethylene glycol (meth)acrylate, and phenyl (meth)acrylate; methyl (meth)acrylate, ethyl (meth)acrylate, propyl (meth)acrylate, n-butyl (meth)acrylate, t-butyl (meth)acrylate, pentyl (meth)acrylate, heptyl (meth)acrylate, and hexyl (meth)acrylate. Acrylic monomers containing linear or branched alkyl groups such as acrylate, 2-ethylhexyl (meth)acrylate, octyl (meth)acrylate, nonyl (meth)acrylate, decyl (meth)acrylate, undecyl (meth)acrylate, dodecyl (meth)acrylate, tridecyl (meth)acrylate, and tetradecyl (meth)acrylate; acrylic monomers containing alicyclic alkyl groups such as cyclohexyl (meth)acrylate and isovonyl (meth)acrylate; acrylic monomers containing fluorinated alkyl groups such as trifluoroethyl (meth)acrylate and heptadecafluorodecyl (meth)acrylate;(meth)acrylamide, N-methoxymethyl-(meth)acrylamide, N-ethoxymethyl-(meth)acrylamide, N-propoxymethyl-(meth)acrylamide, N-butoxymethyl-(meth)acrylamide, N-pentoxymethyl-(meth)acrylamide, N,N-di(methoxymethyl)acrylamide, N-ethoxymethyl-N-methoxymethylmethacrylamide, N,N-di(ethoxymethyl)acrylamide, N-ethoxymethyl-N-propoxymethylmethacrylamide, N,N-di(propoxymethyl)acrylamide, N-butoxymethyl-N-(propoxymethyl)methacrylamide, N,N-di(butoxymethyl)acrylamide, N-butoxymethyl-N-(methoxymethyl)methacrylamide, N,N-di(pentoxymethyl)acrylamide, N-methoxymethyl-N-(pentoxymethyl)methacrylamide, N,N-dimethylaminopropylacrylamide, N,N-diethylaminopropyl Examples include amide group-containing acrylic monomers such as pyracrylamide, N,N-dimethylacrylamide, and N,N-diethylacrylamide; hydroxy group-containing acrylic monomers such as 2-hydroxyethyl (meth)acrylate, 2-hydroxypropyl (meth)acrylate, 4-hydroxybutyl (meth)acrylate, glycerol mono(meth)acrylate, 4-hydroxyvinylbenzene, 1-ethynyl-1-cyclohexanol, and allyl alcohol; polyethylene oxide group-containing acrylic monomers such as polyethylene glycol monoacrylate (manufactured by Nippon Oil & Fats Co., Ltd., Bremmer PE-90, 200, 350, 350G, AE-90, 200, 400, etc.), polyethylene glycol / polypropylene glycol monoacrylate (manufactured by Nippon Oil & Fats Co., Ltd., Bremmer 50PEP-300, 70PEP-350, etc.), and methoxypolyethylene glycol monoacrylate (manufactured by Nippon Oil & Fats Co., Ltd., Bremmer PME-400, 550, 1000, 4000, etc.).
[0143] Among the above acrylic monomers, it is preferable that one or more are selected from the group consisting of alkyl esters of (meth)acrylic acid, alkylamides of (meth)acrylic acid, and hydroxyalkyl esters of (meth)acrylic acid. The number of carbon atoms in the alkyl group constituting the alkyl ester, etc., is preferably 1 to 18, 2 to 12, or 4 to 8.
[0144] Examples of the styrene monomers mentioned above include styrene, α-methylstyrene, o-methylstyrene, p-methylstyrene, and m-methylstyrene. Examples of maleic acid monomers include maleic anhydride and maleic acid, and may be alkyl esters with 1 to 18 carbon atoms, alkylamides with 1 to 18 carbon atoms, or hydroxyalkyl esters with 2 to 4 carbon atoms. Furthermore, the emulsion acrylic resin may also use other known monomers commonly used as reaction components in emulsion acrylic resins as reaction components.
[0145] Using these reaction components, an emulsion-type acrylic resin can be produced by known manufacturing methods. Furthermore, it can be made aqueous by methods such as using a known emulsifier or polymer protective colloid, or by introducing a carboxyl group into the molecule and neutralizing it with a basic compound. Examples of basic compounds include those exemplified in the production of emulsion-type urethane resin described later, with amine compounds being preferred, and the use of ammonia being preferred. In addition, the emulsion-type acrylic resin is preferably an aqueous emulsion.
[0146] The emulsified acrylic resin may have a weight-average molecular weight (Mw) of 1,000 to 100,000, 5,000 to 80,000, or 10,000 to 50,000. Within these ranges, it is possible to improve the coatability while appropriately maintaining the viscosity of the inactive energy ray curable aqueous matte coating agent. The resulting matte coating layer has uniformity and maintains appropriate hardness, further improving substrate adhesion and abrasion resistance.
[0147] The emulsified acrylic resin preferably has a glass transition temperature (Tg) of 10 to 120°C, more preferably 20 to 100°C, even more preferably 30 to 80°C, and particularly preferably 40 to 60°C. Within these ranges, the adhesion and abrasion resistance of the matte coat layer to the substrate can be further improved. A glass transition temperature of 120°C or lower for the emulsified acrylic resin can impart more matte properties to the matte coat layer. A glass transition temperature of 10°C or higher can improve the film strength of the matte coat layer and further improve its abrasion resistance.
[0148] The emulsion-type acrylic resin preferably has an average particle size (mode diameter) of less than 1 μm. For example, the average particle size (mode diameter) of the emulsion-type acrylic resin is preferably between 10 nm and less than 1 μm, between 50 nm and 500 nm, or between 100 nm and 200 nm. Within these ranges, the stability and applicability of the inactive energy ray-curable aqueous matte coating agent, as well as the uniformity of the matte coating layer, can be further improved.
[0149] The average particle size (mode diameter) of emulsion-type acrylic resin can be measured according to the method described above for emulsion-type urethane resin.
[0150] The emulsified acrylic resin solids content is preferably 0.5 to 30% by mass, 1 to 25% by mass, 3 to 20% by mass, or 5 to 15% by mass, relative to the total solids content of the inactive energy ray-curable aqueous matte coating agent. Within these ranges, the stability of the inactive energy ray-curable aqueous matte coating agent and the matte properties and abrasion resistance of the matte coating layer can be further improved.
[0151] In some embodiments, by setting the solid content ratio of emulsion acrylic resin to emulsion urethane resin within a specific range, a matte coat layer with excellent durability and weather resistance can be provided. Specifically, the mass ratio of emulsion urethane resin to the total amount of emulsion acrylic resin and emulsion urethane resin may be 20 to 150% by mass, and is preferably 30 to 120% by mass, 40 to 110% by mass, or 60 to 100% by mass. These solid content ratios allow the matte coat layer to possess sufficient flexibility and hardness, thereby improving its resistance to the external environment.
[0152] In an inactive energy ray-curable aqueous matte coating agent, the emulsion-type urethane resin and emulsion-type acrylic resin function as a resin matrix but can also function as a binder resin. The inactive energy ray-curable aqueous matte coating agent may also contain other binder resins, and it is preferable that the other binder resins are aqueous resins. Examples of other aqueous resins include aqueous styrene-maleic acid copolymer resin, aqueous polyester resin, aqueous shellac, aqueous rosin-modified maleic acid resin, aqueous vinyl chloride-vinyl acetate copolymer resin, aqueous chlorinated polypropylene resin, aqueous hydroxyethyl cellulose resin, aqueous hydroxypropyl cellulose resin, aqueous butyral resin, etc. The total mass of the solids of the emulsion-type acrylic resin and emulsion-type urethane resin may be 50% by mass or more, 80% by mass or more, or 90% by mass or more, or 100% by mass, relative to the total solids of the resin contained in the inactive energy ray-curable aqueous matte coating agent.
[0153] <Resin fine particles> The inactive energy ray curable aqueous matte coating agent contains resin fine particles. Here, resin fine particles refer to particles with an average particle diameter of 1 μm or more. This improves the matte properties of the matte coating layer. The resin fine particles play an important role in providing the matte properties, and their average particle diameter is preferably 1 to 10 μm, more preferably 1.2 to 9 μm, even more preferably 1.5 to 8 μm, and even more preferably 1.5 to 6 μm. On the other hand, the average particle diameter is preferably 1 to 8 μm, more preferably 1 to 5 μm, and even more preferably 1 to 4 μm. In particular, a range of 1.8 to 4 μm is preferred. However, this excludes cases where the resin fine particles are polyolefin wax particles. Here, resin fine particles and resin beads (also called beads) are synonymous. When resin fine particles are used as a raw material, they may be a dry raw material or an aqueous dispersion. Preferably, they are an aqueous dispersion.
[0154] The average particle size (mode diameter) of resin microparticles is the volume-based mode diameter measured by dynamic light scattering, and can be measured using, for example, NanoTrac UPA (manufactured by MicroTrac Bell). The sample used for measurement should be a 500-fold dilution of the resin microparticles with water.
[0155] The average particle size of the emulsion-type acrylic resin particles and the average particle size of the emulsion-type urethane resin particles are preferably 1-20%, 1.2-10%, or 2-8%, respectively, when the average particle size of the resin fine particles is set to 100%. When polyolefin wax particles, as described later, are used, the average particle size of the polyolefin wax particles is preferably 0.1-80%, 0.5-50%, or 1-10%, when the average particle size of the resin fine particles is set to 100%.
[0156] Specific examples of resin microparticles include urethane resin microparticles, silicone resin microparticles, melamine resin microparticles, melamine-benzoguanamine resin microparticles, acrylic resin microparticles, acrylic-styrene copolymer resin microparticles, polycarbonate resin microparticles, polystyrene resin microparticles, and benzoguanamine resin microparticles. Examples of acrylic resin microparticles include polymethyl methacrylate resin microparticles. Examples of benzoguanamine resin microparticles include polycondensate microparticles of benzoguanamine and formaldehyde. Furthermore, the resin microparticles may be biodegradable. The resin microparticles may contain trace amounts of inorganic microparticles on their surface and / or inside. The resin microparticles may be used alone or in combination of two or more types. Inactive energy ray curable aqueous matte coating agents can have their matte properties improved by resin microparticles, and are therefore expected to have applications in a wide range of industrial fields.
[0157] The resin fine particles are preferably present in an amount of 5 to 70% by mass in the total solid content of the inactive energy ray-curable aqueous matte coating agent. More preferably, they are present in an amount of 8 to 65% by mass, and particularly preferably in an amount of 10 to 40% by mass. This is expected to further improve the physical properties of the inactive energy ray-curable aqueous matte coating agent.
[0158] The glass transition temperature (Tg) of the resin microparticles is preferably in the range of -80 to 130°C, more preferably -60 to 100°C, and even more preferably -50 to 60°C. Within this range of glass transition temperatures, the resin microparticles are more likely to protrude from the surface of the matte coat layer, thereby enhancing the matte properties. Furthermore, the flexibility of the resin microparticles can further improve the abrasion resistance of the matte coat layer. Setting the specific resin microparticle content and glass transition temperature as described above is important for improving the stability and applicability of the inactive energy ray curable aqueous matte coat agent and for improving the physical properties of the matte coat layer.
[0159] Specific examples of urethane resin microparticles include cross-linked urethane beads such as ART PEARL C-1000 transparent, ART PEARL C-600 transparent, ART PEARL C-400 transparent, ART PEARL C-800, ART PEARL MM-120T, ART PEARL JB-800T, ART PEARL JB-600T, ART PEARL P-800T, and ART PEARL P-400T (manufactured by Negami Kogyo Co., Ltd.).
[0160] Specific examples of silicone resin microparticles include KMP-594, KMP-597, KMP-598, KMP-600, KMP-601, KMP-602 (manufactured by Shin-Etsu Chemical Co., Ltd.), Trefil E-506S, EP-9215 (manufactured by Toray Dow Corning Co., Ltd.), and others.
[0161] Specific examples of melamine resin microparticles include Epostor SS, Epostor S, Epostor FS, Epostor S6, and Epostor S12 (manufactured by Nippon Shokubai Co., Ltd.). Specific examples of melamine-benzoguanamine resin microparticles include Epostor M30 (manufactured by Nippon Shokubai Co., Ltd.).
[0162] Specific examples of acrylic resin fine particles include Epostor MA1002, Epostor MA1004, Epostor MA1006, Epostor MA1010 (manufactured by Nippon Shokubai Co., Ltd.), Toughtick FH-S005, Toughtick FH-S008, Toughtick FH-S010, Toughtick FH-S015, Toughtick FH-S020 (manufactured by Toyobo Co., Ltd.), Chemisnow MX-80H3wT, MX-150, MX-180TA, MX-300, MX-500, MX-1000, MX-1500H, MX-2000, MX-3000 (manufactured by Soken Chemical Co., Ltd.), and ART PEARL J-4P (manufactured by Negami Kogyo Co., Ltd.).
[0163] Specific examples of acrylic-styrene copolymer resin fine particles include Epostor MA2003 (manufactured by Nippon Shokubai Co., Ltd.), FS-102, FS-201, FS-301, MG-451, and MG-351 (manufactured by Nippon Paint Industrial Coatings Co., Ltd.).
[0164] Specific examples of polycarbonate resin fine particles include the fine particles described in Japanese Patent Publication No. 2014-125495, the fine particles obtained by the manufacturing method described in Japanese Patent Publication No. 2011-26471, and the fine particles obtained by the method described in Japanese Patent Publication No. 2001-213970.
[0165] Specific examples of polystyrene-based microparticles include Chemisnow SX-130H, SX-350H, and SX-500H (manufactured by Soken Chemical Co., Ltd.). Specific examples of benzoguanamine resin microparticles include Epostor MS, Epostor M05, and Epostor L15 (manufactured by Nippon Shokubai Co., Ltd.).
[0166] The inactive energy ray curable aqueous matte coating agent preferably contains urethane resin fine particles, acrylic resin fine particles, or a combination thereof, and more preferably contains urethane resin fine particles alone or a combination of urethane resin fine particles and acrylic resin fine particles. Since urethane resin fine particles tend to orient themselves on the surface of the matte coating layer and protrude from the surface to form an uneven shape, they can impart a greater matte finish. Furthermore, since urethane resin fine particles are flexible, they impart flexibility to the matte coating layer, further improving its abrasion resistance. A combination of urethane resin fine particles and acrylic resin fine particles can further improve blocking resistance and abrasion resistance. When using a combination of urethane resin fine particles and acrylic resin fine particles, the mass of the urethane resin fine particles relative to the total mass of the urethane resin fine particles and acrylic resin fine particles should be, for example, 10 to 90% by mass, 15 to 70% by mass, or 30 to 60% by mass.
[0167] <Polyolefin wax particles> The inactive energy ray curable aqueous matte coating agent may further contain polyolefin wax particles. By using polyolefin wax particles, matte properties and abrasion resistance can be imparted to the matte coating layer. Examples of polyolefin wax particles include polyethylene wax particles and polypropylene wax particles. The hardness (penetration) of the polyolefin wax particles at 25°C as specified in JIS K2207 is preferably 10 or less, 4 or less, or 2 or less. The average particle diameter (mode diameter) of the polyolefin wax particles is the volume-based mode diameter measured by dynamic light scattering, and is preferably 0.01 to 10 μm, 0.02 to 1 μm, or 0.03 to 0.1 μm. From the viewpoint of enhancing the matte properties of the matte coating layer, it is preferable that it be 0.3 μm or less, or 0.1 μm or less. Furthermore, from the viewpoint of enhancing the matte properties of the matte coating layer, it is preferable that it be 0.01 to 0.1 μm, or 0.01 to 0.05 μm. The average particle diameter of the polyolefin wax particles can be measured using the same procedure as for the resin fine particles described above. When using polyolefin fine particles, it is preferable to use a combination of polyolefin wax particles and urethane fine particles.
[0168] When polyolefin wax particles are used, the amount of polyolefin wax particles is preferably 0.1 to 20% by mass, 1 to 10% by mass, or 2 to 8% by mass relative to the total mass of the non-active energy ray curable aqueous matte coating agent. Having 0.1% by mass or more of polyolefin wax particles can further impart surface smoothness to the matte coating layer. Having 20% by mass or less of polyolefin wax particles can further improve the stability and applicability of the non-active energy ray curable aqueous matte coating agent. The amount of polyolefin wax is preferably 1 to 70 parts by mass, 2 to 50 parts by mass, or 3 to 30 parts by mass per 100 parts by mass of resin fine particles. Preferably, the amount of polyolefin wax particles is 2 to 60 parts by mass, 3 to 40 parts by mass, or 5 to 30 parts by mass per 100 parts by mass of the total of the emulsion-type acrylic resin and emulsion-type urethane resin.
[0169] Specific examples of polyolefin wax particles include Mipelon XM-220, XM221U, Chemipearl W500 (manufactured by Mitsui Chemicals, Inc.), and Flowbeads LE-1080 (manufactured by Sumitomo Seika Co., Ltd.).
[0170] <Aqueous medium> The inactive energy ray-curable aqueous matte coating agent contains an aqueous medium. The aqueous medium contains water, and may be water alone or a mixture of water and an organic solvent. The aqueous medium may be 10-80% by mass, 20-75% by mass, 20-70% by mass, or 35-70% by mass relative to the total mass of the inactive energy ray-curable aqueous matte coating agent. Within these ranges, an appropriate viscosity is maintained during coating, thereby improving workability. Furthermore, the environmental impact can be further reduced, and the working environment can be improved.
[0171] The amount of water relative to the total mass of the aqueous medium may be 100% by mass, but if an organic solvent is included, the amount of the organic solvent may be 0.1 to 20% by mass, 0.5 to 15% by mass, 1 to 10% by mass, or 1 to 8% by mass. The organic solvent is preferably a water-soluble organic solvent that forms the same phase in a mixture with the same volume of water at 1 atmosphere and a temperature of 20°C. Examples of water-soluble organic solvents include lower alcohols such as ethanol, n-propanol, and isopropanol, and glycols such as ethylene glycol and propylene glycol.
[0172] Inactive energy ray-curable aqueous matte coating agents preferably do not contain water-insoluble organic solvents. The amount of water-insoluble organic solvent relative to the total mass of the inactive energy ray-curable aqueous matte coating agent may be 5% by mass or less, 3% by mass or less, 1.5% by mass or less, or 1% by mass or less, and preferably 0.5% by mass or less, or 0.1% by mass or less. Within these ranges, the stability of the inactive energy ray-curable aqueous matte coating agent can be better maintained from the viewpoint of compatibility with aqueous media. This improves coating properties, thereby further improving the film strength of the matte coating layer. Furthermore, it is possible to reduce the environmental impact. The water-insoluble organic solvent is an organic solvent other than the water-soluble organic solvent mentioned above. In particular, it is preferable that water-insoluble organic solvents with a solubility in water of 10 g / 100 ml or less are not included in the inactive energy ray-curable aqueous matte coating agent, and their content should be within the above range.
[0173] <Surfactants> The inactive energy ray-curable aqueous matte coating agent may contain a surfactant. The surfactant may be a nonionic surfactant, a cationic surfactant, anionic surfactant, or an amphoteric surfactant, or a combination of two or more of these. Furthermore, the surfactant can function as an antifoaming agent, leveling agent, slip agent, foam suppressant, defoaming agent, dispersant, etc. in the inactive energy ray-curable aqueous matte coating agent.
[0174] (Nonionic surfactant) Inactive energy ray curing aqueous matte coating agents preferably contain a nonionic surfactant. Nonionic surfactants can improve the coating stability of the inactive energy ray curing aqueous matte coating agent and further improve the surface properties of the matte coating layer. Furthermore, nonionic surfactants can improve the wettability and dispersibility of resin fine particles in the inactive energy ray curing aqueous matte coating agent.
[0175] Examples of nonionic surfactants include polyethylene glycol, polypropylene glycol, or copolymers thereof, polyisobutylene glycol, fluorine-based surfactants, silicone-based surfactants, acetylene glycol-based surfactants, and acetylene alcohol-based surfactants.
[0176] The HLB value of the nonionic surfactant may be 15 or less or 13 or less, but is preferably 10 or less, and more preferably 8 or less, 5 or less, or 4 or less. Within these ranges, the surface properties of the matte coat layer can be improved, and the wettability of resin fine particles in the inactive energy ray curable aqueous matte coat agent can be further improved.
[0177] The nonionic surfactant is preferably an acetylene glycol-based surfactant or an acetylene alcohol-based surfactant, and more preferably an acetylene glycol-based surfactant. Examples of acetylene glycol-based surfactants include acetylene glycol and derivatives obtained by adding alkylene oxide to the hydroxyl group of acetylene glycol. Here, the number of carbon atoms in the alkylene group of the alkylene oxide may be 1 to 4 or 2 to 3, and is preferably ethylene oxide. The number of moles of alkylene oxide added may be 1 to 30, 2 to 20, or 5 to 15.
[0178] Acetylene glycol or its derivatives are preferred if they have a symmetrical molecular structure with an acetylene group at the center, from the viewpoint of imparting a moist feel to the matte coat layer and the wettability of resin fine particles. Acetylene glycol or its derivatives are preferred if hydroxyl groups are bonded to two α-carbons of the acetylene group, or if alkylene oxide chains are introduced to two α-carbons, from the viewpoint of imparting a moist feel to the matte coat layer and the wettability of resin fine particles. The number of carbon atoms in the main chain of one of the carbon chains bonded to the acetylene group may be 1 to 12, 2 to 8, or 3 to 4, and some or all of the hydrogen atoms of these carbon chains may have substituents. Preferred acetylene glycol-based surfactants may be 2,4,7,9-tetramethyl-5-decine-4,7-diol, or derivatives in which ethylene oxide is added to the two hydroxyl groups. The HLB value of the acetylene glycol-based surfactant is preferably 1 to 10, and more preferably 2 to 8, 2.5 to 5, or 3 to 4.
[0179] The total mass of the surfactant should be 0.1 to 20%, 0.5 to 10%, or 1 to 5% based on the total mass of the inactive energy ray curable aqueous matte coating agent.
[0180] Inactive energy ray-curable aqueous matte coating agents may use a surfactant as an antifoaming agent or slip agent. In this case, the inactive energy ray-curable aqueous matte coating agent may contain a silicone-based surfactant. When using a silicone-based surfactant, the amount of the silicone-based surfactant should be 0.01 to 5% by mass, 0.05 to 4% by mass, or 0.1 to 3% by mass, based on the total mass of the inactive energy ray-curable aqueous matte coating agent. Within these ranges, the formation of air bubbles in the matte coating layer is suppressed, and the appearance of the matte coating layer can be further improved. Furthermore, slip properties are imparted to the matte coating layer, further improving its abrasion resistance. In addition, within these ranges, the decrease in the stability of the inactive energy ray-curable aqueous matte coating agent is suppressed, and the coating properties are improved, further improving the appearance of the matte coating layer.
[0181] <Additives> Inactive energy ray-curable aqueous matte coating agents may optionally contain additives. Examples of additives include leveling agents, UV absorbers, light stabilizers, plasticizers, adhesion aids, defoamers, slip agents, antistatic agents, pH adjusters, and thickeners. These additives are selected according to the properties of the inactive energy ray-curable aqueous matte coating agent, and each plays a specific role. Thickeners can be used to adjust the viscosity of the inactive energy ray-curable aqueous matte coating agent to a range suitable for the printing method. These additives may be included in the inactive energy ray-curable aqueous matte coating agent as appropriate, and their content may be adjusted as appropriate according to their function. If additives are included, they may be present in an amount of 0.1 to 20% by mass, 0.5 to 15% by mass, or 1 to 10% by mass relative to the total mass of the one-component or inactive energy ray-curable aqueous matte coating agent.
[0182] <Hardening agent> The curing agent can crosslink emulsion-type urethane resin and emulsion-type acrylic resin to increase the strength of the coating film. The curing agent is preferably a compound that can react with the hydroxyl groups, carboxyl groups, etc., present in the emulsion-type urethane resin and emulsion-type acrylic resin, respectively. For example, compounds having two or more crosslinkable groups such as isocyanate groups, blocked isocyanate groups, amino groups, epoxy groups, carbodiimide groups, and aziridine groups can be used. In particular, from the viewpoint of reactivity with hydroxyl groups, it is preferable to include an isocyanate-based curing agent, and for example, polyisocyanate-based curing agents and blocked polyisocyanate-based curing agents can be included. In one embodiment, from the viewpoint of blocking resistance, a carbodiimide-based curing agent having a carbodiimide group is also preferred. Furthermore, from the viewpoint of reactivity with carboxyl groups, an aziridine-based curing agent having an aziridine group is also preferred.
[0183] Examples of isocyanate-based curing agents include aromatic polyisocyanates, aliphatic polyisocyanates, alicyclic polyisocyanates, dimers or trimers of these polyisocyanate compounds, and prepolymers obtained using these polyisocyanate compounds.
[0184] Examples of isocyanate-based curing agents include aromatic isocyanate-based curing agents such as m-phenylenediisocyanate, p-phenylenediisocyanate, 4,4'-diphenylmethane diisocyanate, 2,4'-diphenylmethane diisocyanate, 2,2'-diphenylmethane diisocyanate, 3,3'-dimethyl-4,4'-biphenylenediisocyanate, 3,3'-dimethoxy-4,4'-biphenylenediisocyanate, 3,3'-dichloro-4,4'-biphenylenediisocyanate, 1,5-naphthalenediisocyanate, 1,5-tetrahydronaphthalenediisocyanate, xylylenediisocyanate, and tetramethylxylylenediisocyanate; and tetramethylenediisocyanate, 1,6-hexamethylenediisocyanate, dodecamethylenediisocyanate, and trimethylhexamethylenediisocyanate. Examples of curing agents include aliphatic isocyanate curing agents such as 1,3-cyclohexylene diisocyanate, 1,4-cyclohexylene diisocyanate, hydrogenated xylylene diisocyanate, lysine diisocyanate, isophorone diisocyanate, 4,4'-dicyclohexylmethane diisocyanate, and 3,3'-dimethyl-4,4'-dicyclohexylmethane diisocyanate; alicyclic isocyanate curing agents such as cyclohexane-1,4-diisocyanate, hydrogenated xylylene diisocyanate, isophorone diisocyanate, dicyclohexylmethane-4,4'-diisocyanate, 1,3-bis(isocyanate methyl)cyclohexane, methylcyclohexane diisocyanate, and norbornane diisocyanate; and adduct-type isocyanate curing agents, which are adducts of the above isocyanate curing agents with polyhydric alcohols. Furthermore, the use of isocyanurate-modified curing agents, which are modified isocyanate-based curing agents, is also preferable.
[0185] Examples of polyhydric alcohols used in adduct-side isocyanate curing agents include 1,2-propylene glycol (divalent), diethylene glycol (divalent), dipropylene glycol (divalent), 1,3-butanediol (divalent), neopentyl glycol (divalent), trimethylolpropane (trivalent), 2,2,4-trimethyl-1,3-pentanediol (trivalent), polyethylene glycol (polyvalent), and polypropylene glycol (polyvalent).
[0186] Commercially available isocyanate-based curing agents can be used, such as 24A-100, 22A-75, TPA-100, TSA-100, TSS-100, TAE-100, TKA-100, P301-75E, E402-808, E405-70B, AE700-100, D101, D201, A201H (manufactured by Asahi Kasei), Mytec Y260A (manufactured by Mitsubishi Chemical Corporation), Coronate HX, and Coronate. HL, Coronate L (manufactured by Nippon Polyurethane Co., Ltd.), Desmodul One example is the N75MPA / X (manufactured by Bayer).
[0187] As a blocked polyisocyanate-based curing agent, for example, a compound obtained by blocking the isocyanate group of the above-mentioned polyisocyanate compound with various blocking agents can be used.
[0188] Commercially available curing agents containing carbodiimide groups can be used, such as CROSSLINKER CX-300 (manufactured by Covestro), Picassian(R) XL-Series (manufactured by Stahl), and HyMax. TM Examples include CA-01 / 02 / 50 (manufactured by HyMax), Carbodilite V-10, V-02, SV-02, E-02, E-05, E-07S, and H-01 (manufactured by Nisshinbo Chemical).
[0189] Examples of aziridine-based curing agents include N,N'-diphenylmethane-4,4'-bis(1-aziridinyl carboxite), N,N'-toluene-2,4-bis(1-aziridinyl carboxite), bisisophthaloyl-1-(2-methylaziridine), tri-1-aziridinylphosphine oxide, N,N'-hexamethylene-1,6-bis(1-aziridinyl carboxite), trimethylolpropane-tri-β-aziridinyl propionate, tetramethylolmethane-tri-β-aziridinyl propionate, tris-2,4,6-(1-aziridinyl)-1,3,5-triazine, trimethylolpropane-tris[3-(1-aziridinyl)propionate], and trimethylolpropane. Examples include lis[3-(1-aziridinyl)butyrate], trimethylolpropanetris[3-(1-(2-methyl)aziridinyl)propionate], trimethylolpropanetris[3-(1-aziridinyl)-2-methylpropionate], 2,2'-bishydroxymethylbutanoltris[3-(1-aziridinyl)propionate], pentaerythritoltetra[3-(1-aziridinyl)propionate], diphenylmethane-4,4-bis-N,N'-ethyleneurea, 1,6-hexamethylenebis-N,N'-ethyleneurea, 2,4,6-(triethyleneimino)-Syn-triazine, and bis[1-(2-ethyl)aziridinyl]benzene-1,3-carboxylic acid amide. In particular, 2,2'-bishydroxymethylbutanoltris[3-(1-aziridinyl)propionate] is preferred because it can improve heat resistance while maintaining the flexibility of the cured product.
[0190] Examples of amine-based curing agents include hexamethylenediamine, triethylenediamine, 1,3-bisaminomethylcyclohexane, diethylaminopropylamine, polyethyleneimine, hexamethylenetetramine, diethylenetriamine, triethyltetramine, methanediamine, metaxylylenediamine and reaction products of metaxylylenediamine and styrene, isophoronediamine, and amino resins.
[0191] The curing agent may be included in an amount of 0.1 to 20% by mass, 0.5 to 15% by mass, 1 to 10% by mass, or 2 to 8% by mass, relative to the total mass of the inactive energy ray curing type aqueous matte coating agent. Within these ranges, the abrasion resistance of the matte coating layer can be further improved. It is more preferable that an isocyanate-based curing agent is included within these ranges.
[0192] In a non-active energy ray curable aqueous matte coating agent, the amount of curing agent may be 1 to 50 parts by mass, 5 to 45 parts by mass, or 10 to 40 parts by mass per 100 parts by mass of total emulsion urethane resin and emulsion acrylic resin. Within these ranges, the abrasion resistance of the matte coating layer can be further improved. It is more preferable that isocyanate-based curing agents are included within these ranges.
[0193] The curing agent is provided as a second liquid and may be provided separately from at least the emulsion acrylic resin, emulsion urethane resin, and resin fine particles. For example, in an inactive energy ray curing aqueous matte coating agent, the other components excluding the curing agent may be provided as a first liquid, and the curing agent may be provided as a second liquid. Preferably, the emulsion acrylic resin, emulsion urethane resin, and resin fine particles may be provided as the first liquid, and the curing agent may be provided as the second liquid. The second liquid may consist only of the curing agent, but may also contain some or all of the aqueous medium.
[0194] In some embodiments, the solid content of the first liquid may be 10-90% by mass, 20-80% by mass, or 40-70% by mass. Here, the solid content of the first liquid is the mass ratio of the dry film obtained by coating the first liquid to the amount of the first liquid applied.
[0195] In some embodiments, the second liquid may be solvent-free and may contain an isocyanate-based curing agent and optional additives. The second liquid may optionally contain an aqueous medium.
[0196] In some embodiments, the solid content of the inactive energy ray-curable aqueous matte coating agent may be 10-90% by mass, 20-80% by mass, or 30-70% by mass. Here, the solid content of the inactive energy ray-curable aqueous matte coating agent is the mass ratio of the cured film obtained by coating the inactive energy ray-curable aqueous matte coating agent to the amount of the inactive energy ray-curable aqueous matte coating agent applied. In this disclosure, the solid content refers to the total mass of non-volatile components in the inactive energy ray-curable aqueous matte coating agent.
[0197] <Viscosity> The viscosity of the inactive energy ray-curable aqueous matte coating agent at 25°C is preferably 10 to 2000 mPa·s, 30 to 1500 mPa·s, or 50 to 1300 mPa·s, and more preferably 100 to 1000 mPa·s. Having these viscosity ranges effectively suppresses excessive penetration into the paper substrate after coating with the inactive energy ray-curable aqueous matte coating agent. Furthermore, it enables the formation of a uniform film on the surface of the cured layer, preventing uneven appearance such as mottling. Additionally, it improves the quality of laminates comprising a matte coating layer made of the inactive energy ray-curable aqueous matte coating agent, thereby increasing the commercial value of the product.
[0198] <Average particle size of non-active energy ray curing aqueous matte coating agent> The average particle size of the inactive energy ray-curable aqueous matte coating agent is preferably 0.1 to 10 μm, more preferably 0.5 to 8 μm, and even more preferably 1 to 5 μm. Within these ranges, the stability and applicability of the inactive energy ray-curable aqueous matte coating agent, as well as the uniformity of the matte coating layer, can be further improved, and the gloss value and abrasion resistance of the laminate are also improved.
[0199] The average particle size of the inactive energy ray-curable aqueous matte coating agent is determined by diluting the inactive energy ray-curable aqueous matte coating agent 500 times with water, measuring approximately 5 ml of the diluted solution using dynamic light scattering (measurement device: NanoTrac UPA (manufactured by MicroTrac Bell)), and taking the particle size of the peak with the largest particle size (mode diameter) among the peaks in the obtained volume-based particle size distribution data (histogram) as the particle size of the inactive energy ray-curable aqueous matte coating agent.
[0200] The method for producing a non-active energy ray curable aqueous matte coating agent is not particularly limited. For example, one method involves preparing the first and second liquids separately and mixing them immediately before or several hours before coating. One example of a method for producing the first liquid is to mix an emulsified urethane resin, an emulsified acrylic resin, resin fine particles, and an aqueous medium all at once or in stages. Mixing can be performed by stirring with a vane-type agitator (disperser). The stirring time is preferably 30 minutes to 3 hours. Furthermore, to improve mixing efficiency and obtain viscosity uniformity, stirring may be performed using a roller mill, ball mill, pebble mill, attritor, sand mill, etc.
[0201] If the first liquid contains air bubbles or unexpectedly large particles, these can degrade the quality of the printed material, so it is preferable to remove them by filtration or other means. Conventional filters can be used.
[0202] The method for producing the second liquid is not particularly limited. As an example of a method for producing the second liquid, the components including the curing agent may be mixed together or separately, and the second liquid may be produced by optionally filtering or otherwise performing other methods.
[0203] The inactive energy ray-curable aqueous matte coating agent may be a one-component inactive energy ray-curable aqueous matte coating agent containing all components, either all at once or by mixing them separately. In this case, a blocked polyisocyanate-based curing agent is preferably used.
[0204] <Activated energy ray curing type aqueous matte coating agent> Below, we will describe an example of an aqueous matte coating agent: an activated energy ray-curing aqueous matte coating agent.
[0205] One embodiment of the aqueous active energy ray curable matte coating agent may include a polyfunctional urethane (meth)acrylate, resin fine particles, and an aqueous medium. This active energy ray curable aqueous matte coating agent offers excellent workability, environmental friendliness, and coating properties, and when the coating film is cured, it can form a matte coating layer with excellent matte properties, substrate adhesion, and abrasion resistance. Since the active energy ray curable aqueous matte coating agent contains a polyfunctional urethane (meth)acrylate, it functions as a resin raw material for forming a resin matrix having a urethane resin structure and an acrylic resin structure. Preferably, the aqueous active energy ray curable matte coating agent may further contain an ethylenically unsaturated monomer Ma.
[0206] Active energy ray curable aqueous matte coating agents use an aqueous medium, thus reducing or eliminating the need for organic solvents and further reducing the amount of reactive compounds used, thereby improving workability and environmental friendliness. The inclusion of an aqueous medium in active energy ray curable aqueous matte coating agents reduces the amount of volatile organic components. Furthermore, the inclusion of an aqueous medium in active energy ray curable aqueous matte coating agents reduces the content of reactive compounds, thus lowering the overall reactivity of the active energy ray curable aqueous matte coating agent and improving handling. Active energy ray curable aqueous matte coating agents are applied to a substrate and form a coating film when the aqueous medium is removed. However, if the active energy ray curable aqueous matte coating agent contains a polyfunctional (meth)acrylate, preferably an ethylenically unsaturated monomer Ma, then substrate adhesion and abrasion resistance can be obtained even in an aqueous state.
[0207] Furthermore, because the active energy ray curing aqueous matte coating agent uses an aqueous medium, it can be used to apply a thin film coating to a substrate. When the resulting matte coating layer is thin, resin fine particles protrude from the surface of the matte coating layer, and the resulting uneven shape makes it easier to obtain a matte finish with excellent aesthetic appeal.
[0208] When an aqueous active energy ray curing matte coating agent further contains the ethylenically unsaturated monomer Ma, the flexibility of the cured film using polyfunctional (meth)acrylate, the flexibility of the resin fine particles distributed in the cured film, and the hydrophilicity of the ethylenically unsaturated monomer Ma result in a matte finish with flexibility on the surface of the matte coating layer, a moist feel, and excellent cosmetic properties.
[0209] Furthermore, the flexibility of the cured film using polyfunctional (meth)acrylate, the flexibility of the resin fine particles distributed in the cured film, and the hydrophilicity of the ethylenically unsaturated monomer Ma allow the surface of the matte coat layer to maintain appropriate strength while possessing flexibility, thereby reducing the occurrence of damage even with repeated friction. For example, when multiple laminates are arranged with the matte coat layers overlapping each other, the occurrence of damage due to repeated friction between the matte coat layers can be reduced. Therefore, it is possible to provide laminates with excellent scratch resistance at the consumer use stage and even at the distribution stage.
[0210] <Polyfunctional urethane (meth)acrylate> The active energy ray-curable aqueous matte coating agent contains a polyfunctional urethane (meth)acrylate. The polyfunctional urethane (meth)acrylate is a urethane (meth)acrylate having two or more reactive functional groups. Preferably, the reactive functional group contains an ethylenically unsaturated double bond. The reactive functional group may be a (meth)acryloyl group, a (meth)acryloyloxy group, or any other group having an ethylenically unsaturated bond. The number of reactive functional groups contained in the polyfunctional urethane (meth)acrylate may be 2 to 16, 2 to 12, or 2 to 10, and more preferably 2 to 8. Having two or more reactive functional groups can further improve the adhesion and abrasion resistance of the matte coating layer to the substrate. Also, due to its polyfunctionality, the blocking resistance of the matte coating layer can be improved. Having 16 or fewer reactive functional groups can further improve the coatability of the active energy ray-curable aqueous matte coating agent and better prevent performance degradation due to poor coating of the matte coating layer.
[0211] It is preferable that the polyfunctional urethane (meth)acrylate is stably contained in an aqueous medium. For example, it is preferable that the polyfunctional urethane (meth)acrylate exhibits hydrophilicity and is soluble or dispersible in an aqueous medium. It is more preferable that the polyfunctional urethane (meth)acrylate is an aqueous dispersion.
[0212] The polyfunctional urethane (meth)acrylate is preferably an emulsion type (forced emulsion type, self-emulsifying type) or water-soluble type. An emulsion type is even more preferable. Emulsified polyfunctional urethane (meth)acrylates, such as self-emulsifying or forced emulsion types, obtained by introducing ionic groups into the polyfunctional urethane (meth)acrylate, are preferred from the viewpoint of stability in aqueous media, film-forming properties of the resulting matte coat layer, and coating suitability. Examples of ionic groups include carboxyl groups, sulfonic acid groups, phosphate groups, phosphonic acid groups, and quaternary ammonium bases. These ionic groups may be neutralized.
[0213] As an emulsified polyfunctional urethane (meth)acrylate, for example, one method uses polyfunctional urethane (meth)acrylate having a carboxyl group, polyfunctional urethane (meth)acrylate having an alkylene oxy group, or polyfunctional urethane (meth)acrylate having a carboxyl group neutralized with an amino compound. In another example, one method involves producing polyfunctional urethane (meth)acrylate having a carboxyl group in the presence of a water-soluble reactive diluent with a water miscibility of 100% by weight or more, then converting the carboxyl group of the said polyfunctional urethane (meth)acrylate into an amine salt, and then adding water to emulsify it, and using the resulting polyfunctional urethane (meth)acrylate having a carboxyl group. For example, see Japanese Patent Publication No. 11-209448, Japanese Patent Publication No. 11-279242, Japanese Patent Publication No. 2000-159847, and Japanese Patent Publication No. 9-137081.
[0214] The polyfunctional urethane (meth)acrylate preferably has aliphatic structural units. The aliphatic structural units are preferably included in the main chain of the polyfunctional urethane (meth)acrylate. For example, the aliphatic structural units may be included in at least one of the polyol structural units and polyisocyanate structural units that form the urethane skeleton, and preferably in the polyol structural units. The aliphatic structural units are preferably at least one selected from the group consisting of polyether structures, polyester structures, acrylic resin structures, and polycarbonate structures. From the viewpoint of abrasion resistance of the matte coat layer, the polyfunctional urethane (meth)acrylate is preferably at least one selected from the group consisting of polyether structures, acrylic resin structures, and polyester structures.
[0215] Polyfunctional urethane (meth)acrylates can be obtained, for example, from addition reaction products of polyols, polyisocyanates, and hydroxyl group-containing (meth)acrylates. One example is obtained by reacting an isocyanate group-containing urethane prepolymer, which is produced by reacting a polyol and a polyisocyanate under conditions of excess isocyanate groups, with a hydroxyl group-containing (meth)acrylate. Another example is obtained by reacting a polyisocyanate with a hydroxyl group-containing (meth)acrylate. Yet another example is obtained by reacting a hydroxyl group-containing urethane prepolymer, which is produced by reacting a polyol and a polyisocyanate under conditions of excess hydroxyl groups, with an isocyanate group-containing (meth)acrylate. In order to introduce aliphatic structural units into polyfunctional urethane (meth)acrylates, it is preferable to use at least one of aliphatic polyols and aliphatic polyisocyanates in these reactions.
[0216] The following describes polyols, polyisocyanates, and hydroxyl group-containing (meth)acrylates for constituting polyfunctional urethane (meth)acrylates.
[0217] <Polyol> Examples of polyols include polyether polyols, polyester polyols, polycarbonate polyols, polyolefin polyols, polysiloxane polyols, and (meth)acrylic polyols. Examples of polyolefin polyols include polybutadiene polyols and polyisoprene polyols. The polyol may contain one or more of the following: aliphatic structures, alicyclic structures, and aromatic structures. The polyol is preferably a diol. The polyol is preferably an aliphatic polyol, and more preferably an aliphatic diol.
[0218] Specific examples of polyols include polyether diols such as polyethylene glycol, polytetramethylene glycol, polypropylene glycol, polytrimethylene glycol, polybutylene glycol, 1-methylbutylene glycol, polyacrylic polyol, and copolymers thereof; polyester diols such as polycaprolactone diol, caprolactone adducts of alkylenediols, and polyester diols derived from dicarboxylic acids such as maleic acid; and polycarbonate diols. Polyols can be used individually or in combination of two or more.
[0219] (Structural units derived from polyester) The polyfunctional urethane (meth)acrylate preferably contains structural units derived from polyester. In this case, the polyol is preferably a polyester polyol. It is preferable that it has structural units derived from polyester polyol. This makes it possible to further improve the viscosity and coating properties of the active energy ray curable aqueous matte coating agent. In addition, the matte coating layer becomes more flexible, and a smooth feel can be provided while maintaining abrasion resistance. The polyester polyol is preferably a condensate of a dibasic acid and a diol. The dibasic acid is preferably an aliphatic dibasic acid such as adipic acid, and the diol is preferably an aliphatic diol such as neopentyl glycol.
[0220] <Polyisocyanate> The polyisocyanate is preferably a diisocyanate. As the diisocyanate, one or more of aliphatic diisocyanates, alicyclic diisocyanates, and aromatic diisocyanates may be used. Examples of aliphatic diisocyanates include butane-1,4-diisocyanate, hexamethylene diisocyanate, isopropyl diisocyanate, 2,2,4-trimethylhexamethylene diisocyanate, and lysine diisocyanate. Examples of alicyclic diisocyanates include cyclohexane-1,4-diisocyanate, hydrogenated xylylene diisocyanate, isophorone diisocyanate, dicyclohexylmethane-4,4'-diisocyanate, 1,3-bis(isocyanate-methyl)cyclohexane, methylcyclohexane diisocyanate, norbornane diisocyanate, and dimer isocyanates obtained by converting the carboxyl group of a dimer acid to an isocyanate group. Examples of aromatic diisocyanates include 1,5-naphthylene diisocyanate, 4,4'-diphenylmethane diisocyanate (MDI), 4,4'-diphenyldimethylmethane diisocyanate, 4,4'-dibenzyl isocyanate, 1,3-phenylene diisocyanate, 1,4-phenylene diisocyanate, tolylene diisocyanate, m-tetramethylxylylene diisocyanate, 4,4-diphenylmethane diisocyanate, xylylene diisocyanate, and 2,6-diisocyanate-benzyl chloride. These may be in the form of trimers with an isocyanurate ring structure. Preferably, tolylene diisocyanate, isophorone diisocyanate, xylylene diisocyanate, hydrogenated xylylene diisocyanate, hexamethylene diisocyanate, and isocyanurate derivatives of hexamethylene diisocyanate are used. Polyisocyanates can be used individually or in combination of two or more types.
[0221] <Hydroxy group-containing (meth)acrylate> The hydroxyl group-containing (meth)acrylate used to constitute the polyfunctional urethane (meth)acrylate is preferably a compound having one or more (meth)acryloyl groups and one or more hydroxyl groups in one molecule, more preferably a (meth)acrylate having one or more hydroxyl groups, and even more preferably a (meth)acrylate having one hydroxyl group.
[0222] Examples of hydroxyl group-containing (meth)acrylates include polyhydric alcohol (meth)acrylates, hydroxyalkyl (meth)acrylates, polycarboxylic acid (meth)acrylates with hydroxyalkylated carboxyl groups, caproic acid-added (meth)acrylates, alkylene oxide-modified (meth)acrylates, and α-(hydroxyalkyl)(meth)acrylates. Specifically, examples include the hydroxyl group-containing (meth)acrylates contained in the active energy ray-curable aqueous matte coating agent described later. Hydroxyl group-containing (meth)acrylates can be used individually or in combination of two or more types.
[0223] For the hydroxyl group-containing (meth)acrylate used to constitute the polyfunctional urethane (meth)acrylate, it is preferable to use (meth)acrylate of a polyhydric alcohol, 2-hydroxyethyl (meth)acrylate, 2-hydroxypropyl (meth)acrylic, 4-hydroxybutyl (meth)acrylate, or a combination of two or more of these. For example, the (meth)acrylate of a polyhydric alcohol may be a derivative of a polyhydric alcohol with three or more functions, having at least one hydroxyl group, and at least one of the remaining hydroxyl groups being substituted with a (meth)acrylate group. Examples of polyhydric alcohols include glycerin, erythritol, and dipentalithritol.
[0224] The polyfunctional urethane (meth)acrylate preferably has hydrophilic groups. For example, in the above-described method for producing polyfunctional (meth)acrylate, a polyfunctional (meth)acrylate having hydrophilic groups can be obtained by synthesizing it using a raw material into which hydrophilic groups have been introduced. Alternatively, a polyfunctional urethane (meth)acrylate having terminal hydroxyl groups or terminal isocyanate groups may be produced, and then hydrophilic groups may be introduced starting from these terminal groups. Yet another method may be used to synthesize the polyfunctional (meth)acrylate using a raw material that has a starting point for introducing hydrophilic groups, thereby introducing hydrophilic groups to the starting point of the polyfunctional (meth)acrylate after synthesis.
[0225] The polyfunctional urethane (meth)acrylate may have a carboxyl group as a side chain as a hydrophilic group. For example, it can be synthesized using dimethylolbutanoic acid and dimethylolpropionic acid as raw materials, and then neutralized with an alkali to obtain an aqueous dispersion, thereby obtaining a polyfunctional (meth)acrylate having a hydrophilic group. Furthermore, the polyfunctional urethane (meth)acrylate may also have alkylene oxide chains as hydrophilic groups, and there are no particular restrictions on the number of moles added, which may be 1 to 30, 2 to 20, or 3 to 15.
[0226] The polyfunctional urethane (meth)acrylate is preferably in emulsion form, and may, for example, be obtained by a forced emulsification method. Here, emulsion form and the above-mentioned emulsified form are synonymous. For example, polyfunctional urethane (meth)acrylate is produced by emulsifying urethane (meth)acrylate with a surfactant in an aqueous medium. In this process, the selection and amount of surfactant used are important, as they determine the particle size and particle distribution of the resulting dispersion, as well as the physical and chemical properties of the product. An aqueous dispersion can be provided by using urethane (meth)acrylate and a (reactive) surfactant, charging them together with an aqueous solvent, and stirring. This method allows for proper emulsification of the urethane (meth)acrylate and surfactant, and the usual operating temperature is 15 to 70°C, preferably in the temperature range of 20 to 60°C. Alternatively, an aqueous dispersion can be provided by mixing urethane (meth)acrylate and a large amount of (reactive) surfactant at 15 to 70°C, preferably 20 to 60°C, and then adding an aqueous solvent dropwise to the mixture while stirring. Furthermore, it is also possible to provide an aqueous dispersion by adjusting the temperature of the urethane (meth)acrylate to 20-50°C, then dropping in a (reactive) surfactant dispersed in water and stirring. The aqueous dispersions of polyfunctional urethane (meth)acrylate obtained by these methods have a uniform particle size and excellent dispersion stability, and the manufacturing method is efficient and can be easily implemented on an industrial scale. In addition, as an example, it may be obtained by a self-emulsification method.
[0227] The polyfunctional urethane (meth)acrylate may have a weight-average molecular weight (Mw) of 1,000 to 100,000, 2,000 to 80,000, or 3,000 to 50,000. Within these ranges, it is possible to improve the coatability while appropriately maintaining the viscosity of the active energy ray curable aqueous matte coating agent. The resulting matte coating layer has uniformity and moderate hardness, and its substrate adhesion, blocking resistance, and abrasion resistance can be further improved. Preferably, the polyfunctional urethane (meth)acrylate has a weight-average molecular weight (Mw) of 1,000 to 30,000, more preferably 3,000 to 20,000.
[0228] The polyfunctional urethane (meth)acrylate preferably has a glass transition temperature (Tg) of 0 to 80°C, more preferably 5 to 70°C, even more preferably 10 to 60°C, and particularly preferably 15 to 50°C. Within these ranges, the adhesion and abrasion resistance of the matte coat layer to the substrate can be further improved. A glass transition temperature of 50°C or lower for the polyfunctional urethane (meth)acrylate can impart more mattiness to the matte coat layer and provide a smoother feel. A glass transition temperature of 50°C or lower also imparts flexibility to the matte coat layer, further improving its abrasion resistance.
[0229] The polyfunctional urethane (meth)acrylate may be present in an amount of 1-45% by mass, 2-40% by mass, 5-35% by mass, or 10-30% by mass relative to the total solid content of the active energy ray-curable aqueous matte coating agent. Within these ranges, the stability of the active energy ray-curable aqueous matte coating agent and the appearance of the matte coating layer can be further improved.
[0230] <Ethylene-unsaturated monomers> Active energy ray curable aqueous matte coating agents may contain ethylenically unsaturated monomers other than polyfunctional urethane (meth)acrylate. The ethylenically unsaturated monomer may be monofunctional or polyfunctional (two or more functions). Active energy ray curable aqueous matte coating agents preferably contain a monofunctional ethylenically unsaturated monomer, and a combination of a monofunctional ethylenically unsaturated monomer and a polyfunctional ethylenically unsaturated monomer may be used. In the ethylenically unsaturated monomer, the functional group having an ethylenically unsaturated bond may be a (meth)acryloyl group, a (meth)acryloyloxy group, a vinyl group, an allyl group, a vinylaryl group, a vinyl aralkyl group, an allylaryl group, an allylaralkyl group, etc., and preferably a (meth)acryloyl group or a (meth)acryloyloxy group.
[0231] The active energy ray curable aqueous matte coating agent may contain an ethylenically unsaturated monomer, namely Ma, as the ethylenically unsaturated monomer. However, the ethylenically unsaturated monomer Ma is a monomer other than polyfunctional urethane (meth)acrylate. The ethylenically unsaturated monomer Ma may be at least one selected from the group consisting of hydroxyl group-containing ethylenically unsaturated monomers and alkylene oxy group-containing ethylenically unsaturated monomers. The hydroxyl group-containing ethylenically unsaturated monomer and the alkylene oxy group-containing ethylenically unsaturated monomer may be used individually or in combination of two or more, or a combination of the hydroxyl group-containing ethylenically unsaturated monomer and the alkylene oxy group-containing ethylenically unsaturated monomer may be used.
[0232] In a hydroxyl group-containing ethylenically unsaturated monomer, there may be one or more hydroxyl groups. In a hydroxyl group-containing ethylenically unsaturated monomer, the hydroxyl group may be either an alcoholic hydroxyl group or a phenolic hydroxyl group, but an alcoholic hydroxyl group is preferred.
[0233] The hydroxyl group-containing ethylenically unsaturated monomer may be a hydroxyl group-containing monofunctional ethylenically unsaturated monomer. In the hydroxyl group-containing monofunctional ethylenically unsaturated monomer, there are preferably 1 to 3 hydroxyl groups, more preferably 1 or 2, and even more preferably 1. The hydroxyl group-containing monofunctional ethylenically unsaturated monomer is preferably a hydroxyl group-containing mono(meth)acrylate. The mono(meth)acrylate has the effect of moderately reducing the viscosity of the active energy ray-curable aqueous matte coating agent, and can improve the smoothness of the matte coating layer.
[0234] Examples of hydroxyl group-containing (meth)acrylates include hydroxyalkyl (meth)acrylates, glycols or (meth)acrylates of polyhydric alcohols of three or more valents, partially etherified thereof, caproic acid adducts thereof, alkylene oxide adducts thereof, and α-(hydroxyalkyl)(meth)acrylates.
[0235] Examples of hydroxyl group-containing (meth)acrylates include hydroxyalkyl (meth)acrylates such as 2-hydroxyethyl (meth)acrylate, 1-hydroxypropyl (meth)acrylate, 2-hydroxypropyl (meth)acrylate, 3-hydroxypropyl (meth)acrylate, 1-hydroxybutyl (meth)acrylate, 2-hydroxybutyl (meth)acrylate, 3-hydroxybutyl (meth)acrylate, 4-hydroxybutyl (meth)acrylate, 5-hydroxypentyl (meth)acrylate, 6-hydroxyhexyl (meth)acrylate, 8-hydroxyoctyl (meth)acrylate, 10-hydroxydecyl (meth)acrylate, 12-hydroxylauryl (meth)acrylate, etc.; 2-hydroxy-3-butoxypropyl (meth)acrylate, 2-hydroxy- Examples include alkyl ethers or aryl ethers of hydroxyalkyl (meth)acrylates such as 3-methoxypropyl (meth)acrylate and 2-hydroxy-3-phenoxypropyl (meth)acrylate; mono(meth)acrylates of diols such as diethylene glycol mono(meth)acrylate, triethylene glycol mono(meth)acrylate, polyethylene glycol mono(meth)acrylate, dipropylene glycol mono(meth)acrylate, and polypropylene glycol mono(meth)acrylate; mono(meth)acrylates of polyhydric alcohols such as glycerin mono(meth)acrylate; and cyclohexanedimethanol mono(meth)acrylate, ethyl-α-(hydroxymethyl)(meth)acrylate, and 2-(meth)acryloyloxyethyl-2-hydroxyethyl phthalate.
[0236] Furthermore, examples include hydroxyl group-containing (meth)acrylates having a hydroxycaproic acid group due to ring-opening addition of these hydroxyl group-containing (meth)acrylates to ε-caprolactone. Furthermore, examples include alkylene oxide-modified (meth)acrylates obtained by repeatedly adding alkylene oxides such as ethylene oxide, trimethylene oxide, propylene oxide, n-butylene oxide, and 2,3-butylene oxide to these hydroxyl group-containing (meth)acrylates.
[0237] Furthermore, examples include hydroxyl group-containing polyfunctional (meth)acrylates such as trimethylolpropanedi(meth)acrylate, trimethylolethanedi(meth)acrylate, pentaerythritol tri(meth)acrylate, and dipentaerythritol penta(meth)acrylate. Hydroxyl group-containing (meth)acrylates can be used individually or in combination of two or more.
[0238] The hydroxyl group-containing (meth)acrylate is preferably a hydroxyalkyl mono(meth)acrylate, and more preferably a hydroxyalkyl mono(meth)acrylate in which the hydroxyalkyl group has 2 to 10, 2 to 6, or 2 to 4 carbon atoms. In particular, it is preferable to include 2-hydroxyethyl (meth)acrylate, 4-hydroxybutyl (meth)acrylate, or a combination thereof. The hydroxyalkyl mono(meth)acrylate has the effect of moderately reducing the viscosity of the active energy ray-curable aqueous matte coating agent, and can improve the smoothness of the matte coating layer.
[0239] The hydroxyl group-containing (meth)acrylate may be present in an amount of 0.1 to 30% by mass, 1 to 25% by mass, or 3 to 20% by mass relative to the total mass of the active energy ray-curable aqueous matte coating agent. Within these ranges, the stability of the active energy ray-curable aqueous matte coating agent and the appearance of the matte coating layer can be further improved.
[0240] In alkylene oxy group-containing ethylenically unsaturated monomers, the number of carbon atoms in the alkylene oxy group may be 1 to 22, 1 to 16, or 1 to 12, and preferably 1 to 8, 2 to 4, or 2 to 3. For example, the alkylene oxy group may be an ethylene oxy group, a trimethylene oxy group, a propylene oxy group, an n-butylene oxy group, a 2,3-butylene oxy group, etc. In alkylene oxy group-containing ethylenically unsaturated monomers, the number of alkylene oxy groups may be 1 to 30, 2 to 20, or 3 to 15.
[0241] The alkylene oxy group-containing ethylenically unsaturated monomer may be an alkylene oxy group-containing monofunctional ethylenically unsaturated monomer. Preferably, the alkylene oxy group-containing monofunctional ethylenically unsaturated monomer is an alkylene oxy group-containing mono(meth)acrylate. The monofunctional (meth)acrylate has the effect of significantly reducing the viscosity of the active energy ray curable aqueous matte coating agent and can improve the smoothness of the matte coating layer.
[0242] The alkylene oxy group-containing ethylenically unsaturated monomer may be an alkylene oxide-modified ethylenically unsaturated monomer having an alkylene oxide chain. In the alkylene oxide-modified ethylenically unsaturated monomer, the number of moles of added alkylene oxide chain is not particularly limited, but is preferably 1 to 30, 2 to 20, or 3 to 15. The alkylene oxide chain may be polyethylene glycol, polytetramethylene glycol, polypropylene glycol, poly-n-butylene glycol, poly-2,3-butylene glycol, or copolymers thereof.
[0243] Examples of alkylene oxy group-containing (meth)acrylates include alkylene oxide-modified (meth)acrylates obtained by repeatedly adding alkylene oxides such as ethylene oxide, trimethylene oxide, propylene oxide, n-butylene oxide, and 2,3-butylene oxide to the hydroxyl group-containing (meth)acrylates mentioned above.
[0244] The alkylene oxy group-containing (meth)acrylate may, for example, be obtained by alkylating the hydroxyl group of the hydroxyl group-containing (meth)acrylate described above. For example, it may be a (meth)acrylate having a methoxy group, ethoxy group, trimethyloxy group, propyloxy group, n-butoxy group, 2,3-butoxy group, etc. Alternatively, the terminal hydroxyl group of the alkylene oxide chain of the alkylene oxide-modified (meth)acrylate described above may be alkylated or arylated, and preferably it may be a (meth)acrylate of an ethylene oxide adduct having a methoxy group or ethoxy group at the terminal.
[0245] Examples of alkylene oxy group-containing (meth)acrylates include polyethylene glycol di(meth)acrylates such as polyethylene glycol 200 di(meth)acrylate (the number represents the molecular weight, the same applies hereinafter), polyethylene glycol 300 di(meth)acrylate, polyethylene glycol 400 di(meth)acrylate, polyethylene glycol 600 di(meth)acrylate, polyethylene glycol 1000 di(meth)acrylate, and polyethylene glycol di(meth)acrylate, preferably polyethylene glycol di(meth)acrylate with a molecular weight of 200 to 1000; tetraethylene glycol di(meth)acrylate. Examples include di(meth)acrylates of alkylene glycols with an addition number of 2 or more moles, such as tetramethylene glycol di(meth)acrylate, preferably di(meth)acrylates of alkylene glycols with an addition number of 2 to 10 moles; polyfunctional(meth)acrylates containing alkylene oxy groups, such as tri(meth)acrylate of an alkylene oxide adduct of trimethylolpropane; tetra(meth)acrylate of an alkylene oxy adduct of pentaerythritol; and hexa(meth)acrylate of an alkylene oxide adduct of dipentaerythritol.
[0246] Alkylene oxy group-containing (meth)acrylates can be used individually or in combination of two or more types.
[0247] The alkylene oxy group-containing (meth)acrylate is preferably an alkylene oxide-modified mono(meth)acrylate. Furthermore, it is more preferable that the alkylene oxide-modified mono(meth)acrylate has a terminal hydroxyl group. The terminal end of the alkylene oxide-modified mono(meth)acrylate may also be alkyl etherified. The alkylene oxide-modified mono(meth)acrylate has the effect of moderately reducing the viscosity of the active energy ray-curable aqueous matte coating agent, thereby improving the smoothness of the matte coating layer.
[0248] The alkylene oxy group-containing (meth)acrylate may be present in an amount of 1-30% by mass, 2-20% by mass, or 3-15% by mass relative to the total mass of the active energy ray-curable aqueous matte coating agent. Within these ranges, the stability of the active energy ray-curable aqueous matte coating agent and the appearance of the matte coating layer can be further improved.
[0249] <Other ethylenically unsaturated monomers> From the viewpoint of long-term storage stability and substrate adhesion, in one embodiment, the active energy ray curable aqueous matte coating agent preferably contains one or more other ethylenically unsaturated monomers in addition to the polyfunctional urethane (meth)acrylate and the ethylenically unsaturated monomer Ma, such as a monofunctional ethylenically unsaturated monomer or a polyfunctional ethylenically unsaturated monomer with two or more functions. It is also preferable to use a monomer with three or more functions as the other ethylenically unsaturated monomer. The following shows a preferred form.
[0250] Other monofunctional ethylenically unsaturated monomers include, for example, alkyl(meth)acrylates such as methyl(meth)acrylate, ethyl(meth)acrylate, butyl(meth)acrylate, hexyl(meth)acrylate, octyl(meth)acrylate, dodecyl(meth)acrylate, and stearyl(meth)acrylate, preferably alkyl(meth)acrylates in which the alkyl group has 1 to 18 carbon atoms; benzyl(meth)acrylate; and aromatic group-containing(meth)acrylates such as (meth)acrylates of alkylphenol adducts such as butylphenol, octylphenol, nonylphenol, or dodecylphenol; isoborn Examples include alicyclic group-containing (meth)acrylates such as 1-(meth)acrylate, cyclohexyl(meth)acrylate, and tricyclodecane monomethylol(meth)acrylate; carboxyl group-containing (meth)acrylates such as 2-(meth)acryloyloxypropyl phthalate, β-carboxyethyl(meth)acrylate, (meth)acrylate dimer, and ω-carboxy-polycaprolactone mono(meth)acrylate; amino group-containing (meth)acrylates such as dimethylaminoethyl(meth)acrylate and diethylaminoethyl(meth)acrylate; and N-vinylpyrrolidone, N-vinylformamide, and (meth)acryloylmorpholine. Other monofunctional ethylenically unsaturated monomers can be used individually or in combination of two or more.
[0251] Other examples of difunctional ethylenically unsaturated monomers include alkylene glycol di(meth)acrylates such as butanediol di(meth)acrylate, hexanediol di(meth)acrylate, and octanediol di(meth)acrylate, preferably alkylene glycol di(meth)acrylates in which the alkylene glycol group has 1 to 8 carbon atoms.
[0252] Examples of other polyfunctional ethylenically unsaturated monomers with 3 or more functional groups include trimethylolpropane tri(meth)acrylate, pentaerythritol tetra(meth)acrylate, ditrimethylolpropane tetra(meth)acrylate, dipentaerythritol hexa(meth)acrylate, and the like.
[0253] The ethylenically unsaturated monomers other than polyfunctional urethane (meth)acrylate may be 1 to 30 mass%, 2 to 25 mass%, 3 to 20 mass%, or 4 to 15 mass% based on the total mass of the active energy ray-curable aqueous matte coating agent. The ethylenically unsaturated monomer Ma may be 100 mass%, or may be 50 mass% or more, 80 mass% or more, or 90 mass% or more, based on the total mass of the ethylenically unsaturated monomers other than polyfunctional urethane (meth)acrylate. The monofunctional ethylenically unsaturated monomer may be 100 mass%, or may be 0.1 mass% or more, 10 mass% or more, or 20 mass% or more, based on the total mass of the ethylenically unsaturated monomers other than polyfunctional urethane (meth)acrylate. The polyfunctional ethylenically unsaturated monomer is preferably 0.1 to 20 mass%, 0.5 to 18 mass%, or 1 to 15 mass% based on the total mass of the active energy ray-curable aqueous matte coating agent. Since the polyfunctional ethylenically unsaturated monomer can function as a crosslinking agent, it may be contained in the active energy ray-curable aqueous matte coating agent. Within these ranges, it is possible to further improve the stability and coatability of the active energy ray-curable aqueous matte coating agent while further improving the abrasion resistance of the matte coat layer.
[0254] The ethylenically unsaturated monomer Ma is preferably 40 to 140 parts by mass, 50 to 120 parts by mass, or 60 to 110 parts by mass based on 100 parts by mass of the polyfunctional urethane (meth)acrylate. The other polyfunctional ethylenically unsaturated monomers other than the polyfunctional urethane (meth)acrylate and the ethylenically unsaturated monomer Ma may be 10 to 120 parts by mass, 20 to 110 parts by mass, or 30 to 100 parts by mass based on 100 parts by mass of the polyfunctional urethane (meth)acrylate.
[0255] <Resin Fine Particles> The active energy ray-curable aqueous matting coating agent contains resin fine particles. Thereby, the matting property of the matting coat layer can be improved. As the resin fine particles contained in the active energy ray-curable aqueous matting coating agent, those described for the aforementioned aqueous non-active energy ray-curable matting coating agent can be used.
[0256] The resin fine particles are preferably contained in an amount of 5 to 90 mass% based on the total solid content of the active energy ray-curable aqueous matting coating agent. Further, the content is more preferably 8 to 60 mass%, and a content of 10 to 50 mass% is a particularly preferred embodiment. Thereby, further improvement in the physical properties of the active energy ray-curable aqueous matting coating agent can be expected. In addition, the glass transition temperature of the resin fine particles is preferably in the range of -80 to 130°C, more preferably -60 to 100°C, and even more preferably -50 to 50°C. Within these ranges of the glass transition temperature, the resin fine particles easily protrude from the surface of the matting coat layer, so that more excellent matting property can be imparted, and further, the flexibility of the resin fine particles can further improve the friction resistance of the matting coat layer. The setting of the specific content and glass transition temperature of the resin fine particles as described above is important for improving the stability and coating properties of the active energy ray-curable aqueous matting coating agent, and enhancing the physical property values of the matting coat layer.
[0257] The active energy ray-curable aqueous matte coating agent preferably contains urethane resin fine particles, acrylic resin fine particles, or a combination thereof, and more preferably contains urethane resin fine particles alone or a combination of urethane resin fine particles and acrylic resin fine particles. Since urethane resin fine particles tend to orient themselves on the surface of the matte coating layer and protrude from the surface to form an uneven shape, they can impart a greater matte finish. Furthermore, since urethane resin fine particles are flexible, they impart flexibility to the matte coating layer, further improving abrasion resistance. The amount of urethane resin fine particles is preferably 5 to 90% by mass, 8 to 60% by mass, or 10 to 50% by mass of the total mass of the active energy ray-curable aqueous matte coating agent. The amount of urethane resin fine particles is preferably 50 to 140 parts by mass, 60 to 120 parts by mass, or 70 to 110 parts by mass per 100 parts by mass of polyfunctional urethane (meth)acrylate. A combination of urethane resin fine particles and acrylic resin fine particles can further improve blocking resistance and abrasion resistance. When using a combination of urethane resin microparticles and acrylic resin microparticles, the mass of the urethane resin microparticles relative to the total mass of the urethane resin microparticles and acrylic resin microparticles should be, for example, 10-90% by mass, 15-70% by mass, or 30-60% by mass.
[0258] <Polyolefin wax particles> The active energy ray-curable aqueous matte coating agent may contain polyolefin wax particles. The polyolefin wax particles contained in the active energy ray-curable aqueous matte coating agent can be those described above for the aqueous non-active energy ray-curable matte coating agent.
[0259] By using polyolefin wax particles, matte properties and abrasion resistance can be imparted to the matte coat layer. The polyolefin wax particles are preferably present in an amount of 0.1 to 20% by mass, 1 to 15% by mass, or 2 to 10% by mass in the total solid content of the active energy ray-curable aqueous matte coat agent. A polyolefin wax particle content of 0.1% by mass or more can further impart surface smoothness to the matte coat layer. A polyolefin wax particle content of 20% by mass or less can further improve the stability and applicability of the active energy ray-curable aqueous matte coat agent. The polyolefin wax is preferably present in an amount of 5 to 100 parts by mass, 7 to 80 parts by mass, or 5 to 40 parts by mass per 100 parts by mass of resin fine particles.
[0260] The polyolefin wax particles may be present in an amount of 50 to 150 parts by mass, 60 to 130 parts by mass, or 70 to 120 parts by mass per 100 parts by mass of resin fine particles. The polyolefin wax particles may be present in an amount of 5 to 60 parts by mass, 10 to 40 parts by mass, or 15 to 30 parts by mass per 100 parts by mass of polyfunctional urethane (meth)acrylate.
[0261] The average particle size (mode diameter) of the polyolefin wax particles is the volume-based mode diameter measured by dynamic light scattering, and is preferably 0.01 to 15 μm, 0.02 to 10 μm, or 0.03 to 8 μm. From the viewpoint of blocking resistance, it may be 1 μm or more, 2 μm or more, or 3 μm or more, and it is also preferable that it be 15 μm or less, 10 μm or less, or 8 μm or less.
[0262] <Aqueous medium> Active energy ray curable aqueous matte coating agents contain an aqueous medium. The aqueous medium contains water, and may be water alone or a mixed solvent of water and an organic solvent. The aqueous medium may be 10-80% by mass, 15-75% by mass, or 20-70% by mass relative to the total mass of the active energy ray curable aqueous matte coating agent. Preferably, the aqueous medium is 25-70% by mass relative to the total mass of the active energy ray curable aqueous matte coating agent. Having 25% by mass or more of the aqueous medium maintains an appropriate viscosity during coating, thereby further improving workability. Having 70% by mass or less of the aqueous medium further improves the film strength of the matte coating layer. Furthermore, having 20% by mass or more, 45% by mass or more, 50% by mass or more, 55% by mass or more, or 60% by mass or more of the aqueous medium relative to the total mass of the active energy ray curable aqueous matte coating agent further reduces the environmental burden and improves safety in the working environment and skin irritation.
[0263] The amount of water relative to the total mass of the aqueous medium may be 100% by mass, but if an organic solvent is included, the amount of the organic solvent may be 0.1-20% by mass, 0.5-15% by mass, 1-10% by mass, or 1-8% by mass. The organic solvent is as described above for the aqueous inactive energy ray curable matte coating agent.
[0264] The active energy ray-curable aqueous matte coating agent preferably does not contain water-insoluble organic solvents. The amount of water-insoluble organic solvent relative to the total mass of the active energy ray-curable aqueous matte coating agent may be 5% by mass or less, 3% by mass or less, 1.5% by mass or less, or 1% by mass or less, and preferably 0.5% by mass or less, or 0.1% by mass or less. Within these ranges, the stability of the active energy ray-curable aqueous matte coating agent can be better maintained from the viewpoint of compatibility with aqueous media. As a result, the coating properties are improved, and the film strength of the matte coating layer can be further improved. It is also possible to reduce the environmental impact. The water-insoluble organic solvent is an organic solvent other than the water-soluble organic solvent mentioned above. In particular, it is preferable that the active energy ray-curable aqueous matte coating agent does not contain water-insoluble organic solvents with a solubility in water of 10 g / 100 ml or less, and its content should be within the above range.
[0265] <Surfactants> Active energy ray curing aqueous mat coat agents may contain surfactants. The surfactants contained in active energy ray curing aqueous mat coat agents can be those described above for aqueous non-active energy ray curing mat coat agents. Preferably, the surfactants contained in active energy ray curing aqueous mat coat agents may include polymer surfactants, nonionic surfactants, or a combination thereof.
[0266] (Polymer surfactant) The active energy ray-curable aqueous matte coating agent preferably contains a polymer surfactant. The polymer surfactant is preferably an acrylic resin-type surfactant, and more preferably an acrylic resin-type surfactant that is a copolymer of two or more monomers. The acrylic resin-type surfactant can further enhance the dispersion stability of resin fine particles in the active energy ray-curable aqueous matte coating agent and function as a dispersant.
[0267] The polymer surfactant is preferably a polymer surfactant having an acid value and / or amine value. A polymer surfactant having an acid value and / or amine value can further enhance the dispersion stability of resin fine particles in an active energy ray curable aqueous matte coating agent. For example, using a polymer surfactant having an acid value and / or amine value in combination with urethane fine particles can further improve the dispersion stability and coating properties of the active energy ray curable aqueous matte coating agent. The polymer surfactant having an acid value and / or amine value is preferably a copolymer of two or more monomers. The polymer surfactant is preferably an acrylic resin type surfactant having an acid value and / or amine value, and more preferably an acrylic resin type surfactant that is a copolymer of two or more monomers and has an acid value.
[0268] The amine value of the polymer surfactant may be 0 to 100 mg KOH / g, 0.1 to 60 mg KOH / g, 1 to 40 mg KOH / g, or 10 to 30 mg KOH / g. The acid value of the polymer surfactant may be greater than 0 and 110 mg KOH / g or less, 0.1 to 60 mg KOH / g, 1 to 30 mg KOH / g, or 5 to 20 mg KOH / g. A polymer surfactant with an amine value of 100 mg KOH / g or less can further improve the stability of the active energy ray-curable aqueous matte coating agent.
[0269] The amine value is a numerical value expressed in milligrams of potassium hydroxide equivalent to the amount of hydrogen chloride required to neutralize 1 g of the sample. The acid value is a numerical value expressed in milligrams of potassium hydroxide required to neutralize 1 g of the sample.
[0270] (Nonionic surfactant) The active energy ray-curable aqueous matte coating agent preferably contains a nonionic surfactant. The nonionic surfactant can improve the coating stability of the active energy ray-curable aqueous matte coating agent and further improve the surface properties of the matte coating layer. Furthermore, the nonionic surfactant can improve the wettability of resin fine particles and polyfunctional urethane (meth)acrylate in the active energy ray-curable aqueous matte coating agent and further improve the dispersibility. For example, using a combination of a polymer surfactant, a nonionic surfactant, and urethane fine particles can impart a moist appearance or feel to the matte coating layer, and further improve the dispersibility and coatability of the active energy ray-curable aqueous matte coating agent. The active energy ray-curable aqueous matte coating agent preferably uses a combination of the polymer surfactant and the nonionic surfactant described above.
[0271] The nonionic surfactant is preferably an acetylene glycol-based surfactant or an acetylene alcohol-based surfactant, and more preferably an acetylene glycol-based surfactant. The nonionic surfactant and acetylene glycol-based surfactant are as described above for the aqueous inactive energy ray curable matte coating agent.
[0272] The active energy ray curing aqueous matte coating agent may contain surfactants other than those described above. When using a polymeric surfactant having an acid value and / or amine value, it is preferable to use it in combination with a cationic surfactant, an amphoteric surfactant, or a combination thereof.
[0273] For example, examples of cationic surfactants include alkylamine salts, quaternary ammonium salts and the like. Examples of anionic surfactants include alkylbenzene sulfonates such as dodecylbenzenesulfonic acid, aromatic sulfonic acid-based surfactants such as dodecyl phenyl ether sulfonate, monosoap-based anionic surfactants, ether sulfate-type surfactants, phosphate-based surfactants, carboxylic acid-based surfactants and the like. Examples of amphoteric surfactants include alkylbetaine-based surfactants, amine oxide-based surfactants and the like.
[0274] The molecular weight of the surfactant may be, for example, 500 to 100,000, 1,000 to 50,000, 2,000 to 20,000, or 5,000 to 10,000. In the case of polymeric surfactants, the weight average molecular weight (Mw) is preferably within these ranges. In the case of a polymeric surfactant having an amine value, the weight average molecular weight (Mw) is preferably 1,000 or more, 5,000 or more, or 10,000 or more. Within these ranges, the dispersibility of fine resin particles in the active energy ray-curable aqueous matting coating agent can be further improved.
[0275] The total mass of the surfactant is preferably 0.1 to 25 mass%, 0.5 to 20 mass%, or 1 to 15 mass% relative to the total mass of the active energy ray-curable aqueous matting coating agent. When a polymeric surfactant having an acid value is used, the content of the polymeric surfactant having an acid value is preferably 0.1 to 25 mass%, 2 to 20 mass%, or 3 to 15 mass% relative to the total mass of the active energy ray-curable aqueous matting coating agent. When a nonionic surfactant is used, the content of the nonionic surfactant is preferably 0.1 to 20 mass%, 0.5 to 15 mass%, or 1 to 10 mass% relative to the total mass of the active energy ray-curable aqueous matting coating agent.
[0276] When using a polymer surfactant having an acid value and / or amine value and a nonionic surfactant, the amount of the nonionic surfactant may be 100 parts by mass or less, 90 parts by mass or less, 80 parts by mass or less, or 70 parts by mass or less per 100 parts by mass of the polymer surfactant having an acid value and / or amine value. Preferably, a higher content of the polymer surfactant having an acid value and / or amine value than the nonionic surfactant can further improve the dispersibility and coating properties of resin fine particles in the active energy ray curable aqueous matte coating agent, and further improve the surface properties of the matte coating layer.
[0277] <Polymerization initiator> Active energy ray curable aqueous matte coating agents may contain a polymerization initiator. A photopolymerization initiator is preferred. The photopolymerization initiator generates radicals when irradiated with active energy rays such as light, initiating the crosslinking and polymerization reactions of ethylenically unsaturated bond-containing groups, such as the (meth)acryloyl group, of the polyfunctional urethane (meth)acrylate and the ethylenically unsaturated monomer Ma. Examples of photopolymerization initiators include acetophenone-based, alkylphenone-based, benzoin-based, and acylphosphine oxide-based agents, with acetophenone-based and acylphosphine oxide-based agents being particularly preferred. The amount of the photopolymerization initiator is preferably 0.3 to 15% by mass, more preferably 1 to 10% by mass, and more preferably 1.5 to 8% by mass, relative to the total mass of the active energy ray curable aqueous matte coating agent. Within these ranges, curing characteristics and coating film properties can be further improved.
[0278] Examples of acetophenone-based photopolymerization initiators include 4-phenoxydichloroacetophenone, diethoxyacetophenone, α-hydroxyacetophenone ("Omnirad 1173"), 2-hydroxy-2-methyl-1-phenylpropan-1-one, 1-(4-isopropylphenyl)-2-hydroxy-2-methylpropan-1-one, 1-hydroxycyclohexylphenyl ketone, 4-(2-hydroxyethoxy)-phenyl(2-hydroxy-2-propyl)ketone, 2-methyl-[4-(methylthio)phenyl]-2-morpholino-1-propanone, and 2,2-dimethoxy-2-phenylacetophenone.
[0279] Examples of alkylphenone-based photopolymerization initiators include 2,2-dimethoxy-1,2-diphenylethane-1-one, 1-hydroxycyclohexylphenyl ketone, 2-hydroxy-2-methyl-1-phenylpropane-1-one, 1-[4-(2-hydroxyethoxy)-phenyl]-2-hydroxy-2-methyl-1-propane-1-one, 2-hydroxy-1-{4-[4-(2-hydroxy-2-methylpropionyl)-benzyl]phenyl}-2-methylpropane-1-one, 2-methyl-1-(4-methylthiophenyl)-2-morpholinopropane-1-one, 2-benzyl-2-dimethylamino-1-(4-morpholinophenyl)-butanone-1, and 2-(dimethylamino)-2-[(4-methylphenyl)methyl]-1-[4-(4-morpholinyl)phenyl]-1-butanone.
[0280] Examples of benzoin-based photopolymerization initiators include benzoin, benzoin methyl ether, benzoin isoethyl ether, benzoin isopropyl ether, and benzoin isobutyl ether.
[0281] Examples of benzophenone-based photopolymerization initiators include benzophenone, 4-methylbenzophenone, 4,4'-bis(dimethylamino)benzophenone, 4,4'-bis(diethylamino)benzophenone, methyl-o-benzoylbenzoate, benzoylbenzoic acid, methyl benzoylbenzoate, 4-phenylbenzophenone, hydroxybenzophenone, 4-benzoyl-4'-methyldiphenyl sulfide, and 3,3-dimethyl-4-methoxybenzophenone. Among these, 4-methylbenzophenone is preferred.
[0282] Examples of thioxanthone-based photopolymerization initiators include thioxanthone, 2-chlorothioxanthone, 2,4-dichlorothioxanthone, 2-methylthioxanthone, 2,4-dimethylthioxanthone, 2,4-diethylthioxanthone, isopropylthioxanthone, and 2,4-diisopropylthioxanthone.
[0283] Examples of anthraquinone-based photopolymerization initiators include α-acyloxime esters, methylbenzoyl formate ("ViaCure 55"), and 2-ethylanthraquinone.
[0284] Examples of acylphosphine oxide-based photopolymerization initiators include 2,4,6-trimethylbenzoyldiphenylphosphine oxide ("Omnirad TPO") and bis(2,4,6-trimethylbenzoyl)-phenylphosphine oxide ("IRGACURE819").
[0285] Polymerization initiators may be used individually or in combination of two or more.
[0286] <Additives> Active energy ray curing aqueous matte coatings may optionally contain additives. Examples of additives include leveling agents, polymerization inhibitors, UV absorbers, light stabilizers, sensitizers, curing agents, plasticizers, wetting agents, adhesion aids, defoamers, slip agents, antistatic agents, and pH adjusters. These additives are selected according to the properties of the active energy ray curing aqueous matte coating, and each plays a specific role. For example, leveling agents are used to improve the surface smoothness of the matte coating layer. Polymerization inhibitors are used to prevent premature curing of uncured active energy ray curing aqueous matte coatings during storage. UV absorbers and light stabilizers are used to prevent degradation of the active energy ray curing aqueous matte coating or matte coating layer when exposed to ultraviolet light. Sensitizers accelerate the curing process and shorten the curing time. Curing agents are available to ensure proper curing of the active energy ray curing aqueous matte coating. Plasticizers are available to improve the flexibility of the matte coating layer. Wetting agents are available to ensure uniform spread of the active energy ray curing aqueous matte coating and to improve coatability. Adhesion aids can be used to ensure that the active energy ray-curable aqueous matte coating agent is firmly fixed to the substrate. Antifoaming agents can be used to suppress foam formation during the coating process. Antistatic agents can be used to prevent problems caused by static electricity. Acids, ammonia water, and other bases may be used as appropriate as pH adjusters. These additives may be included in the active energy ray-curable aqueous matte coating agent as appropriate, and their content may be adjusted as appropriate according to their function.
[0287] <Hardening agent> Active energy ray curing aqueous matte coating agents may further contain a curing agent. The curing agent is preferably a compound that can react with hydroxyl groups, carboxyl groups, etc., possessed by polymerizable components such as polyfunctional (meth)acrylates and ethylenically unsaturated monomers such as Ma. For example, compounds having two or more crosslinking groups such as isocyanate groups, blocked isocyanate groups, amino groups, epoxy groups, carbodiimide groups, and aziridine groups can be used. In particular, from the viewpoint of reactivity with hydroxyl groups, it is preferable to include an isocyanate-based curing agent, for example, a polyisocyanate-based curing agent or a blocked polyisocyanate-based curing agent can be included. Furthermore, from the viewpoint of reactivity with carboxyl groups, it is preferable to include an aziridine-based curing agent. In particular, those having a 2,2'-bishydroxymethylbutanoltris[3-(1-aziridinyl)propionate] structure are preferred because they can improve heat resistance while maintaining the flexibility of the cured product.
[0288] The curing agent may be included in an amount of 0.1 to 20% by mass, 0.5 to 15% by mass, 1 to 10% by mass, or 2 to 8% by mass, relative to the total mass of the active energy ray curing type aqueous matte coating agent. Within these ranges, the abrasion resistance of the matte coating layer can be further improved. It is more preferable that an aziridine-based curing agent is included within these ranges.
[0289] In an active energy ray curing aqueous matte coating agent, the amount of curing agent may be 1 to 50 parts by mass, 5 to 40 parts by mass, or 8 to 30 parts by mass per 100 parts by mass of the total of polyfunctional urethane (meth)acrylate, ethylenically unsaturated monomer Ma, and other ethylenically unsaturated monomers. Within these ranges, the abrasion resistance of the matte coating layer can be further improved. It is more preferable that aziridine-based curing agents are included within these ranges.
[0290] The curing agent is provided as a second liquid and may be provided separately from at least the polymerizable compound. For example, in an active energy ray curable aqueous matte coating agent, the other components excluding the curing agent may be provided as a first liquid, and the curing agent as a second liquid. Preferably, a polyfunctional urethane (meth)acrylate and resin fine particles may be provided as the first liquid, and the curing agent as the second liquid. The second liquid may consist only of the curing agent, but may also contain some or all of the aqueous medium. The first liquid may further contain any polymerizable compound such as ethylenically unsaturated monomer Ma and other ethylenically unsaturated monomers.
[0291] In some embodiments, the solid content of the first liquid may be 10-90% by mass, 20-80% by mass, or 40-70% by mass. Here, the solid content of the first liquid is the mass ratio of the dry film obtained by coating the first liquid to the amount of the first liquid applied.
[0292] In some embodiments, the second liquid may be solvent-free and may contain a curing agent and optional additives. The second liquid may optionally contain an aqueous medium.
[0293] In some embodiments, the solid content of the active energy ray-curable aqueous matte coating agent may be 10-90% by mass, 20-80% by mass, or 40-70% by mass. Here, the solid content of the active energy ray-curable aqueous matte coating agent is the mass ratio of the cured film obtained by coating the active energy ray-curable aqueous matte coating agent to the amount of the active energy ray-curable aqueous matte coating agent applied. In this disclosure, the solid content refers to the total mass of non-volatile components in the active energy ray-curable aqueous matte coating agent.
[0294] <Viscosity> The viscosity of the active energy ray-curable aqueous matte coating agent at 25°C is preferably 10 to 2000 mPa·s. Having this viscosity range effectively suppresses excessive penetration into the paper substrate after coating. Furthermore, it allows for the formation of a uniform film on the surface of the cured layer, preventing uneven appearance such as mottling. The viscosity of the active energy ray-curable aqueous matte coating agent at 25°C is preferably 30 to 1500 mPa·s, more preferably 50 to 1300 mPa·s, or particularly preferably 100 to 1000 mPa·s. By setting the viscosity within this specific range, the quality of the laminate with the matte coating layer can be improved, increasing the commercial value of the product.
[0295] The method for producing an active energy ray-curable aqueous matte coating agent is not particularly limited. One example of a method for producing an active energy ray-curable aqueous matte coating agent is to mix a polyfunctional urethane (meth)acrylate, an ethylenically unsaturated monomer Ma, resin fine particles, and an aqueous medium all at once or in stages. Mixing can be performed by stirring with a vane-type stirrer (disperser). The stirring time is preferably 30 minutes to 3 hours. Furthermore, to improve mixing efficiency and obtain viscosity uniformity, stirring may be performed using a roller mill, ball mill, pebble mill, attritor, sand mill, etc.
[0296] If the activated energy ray-curing aqueous matte coating agent contains air bubbles or unexpectedly coarse particles, these can degrade the quality of the printed material, so it is preferable to remove them by filtration or other means. Conventional known filters can be used.
[0297] <Water-based matte coating agent> In some embodiments, the aqueous matte coating agent comprises a resin raw material for forming a resin matrix having a urethane resin structure, resin fine particles encapsulated in the resin matrix in the matte coating layer, and an aqueous medium, satisfying the following conditions (A), (B), and (C). (A) When a matte coat layer with a thickness of 4 μm ± 3 μm is formed on a paper substrate using an aqueous matte coat agent, the surface roughness Sq of the matte coat layer in a measurement field of view of 506 μm × 675 μm is 0.5 to 3.5. Here, the surface roughness Sq of the paper substrate used to measure the surface roughness Sq is 0.4 in a measurement field of view of 506 μm × 675 μm before the matte coat layer is formed. (B) When a matte coating layer with a thickness of 4 μm ± 3 μm is formed on a paper substrate using an aqueous matte coating agent, the composite modulus of elasticity is 4 GPa or less. Here, the composite modulus of elasticity is measured by nanoindentation and is the measurement value in the resin matrix portion. (C) When a matte coating layer with a thickness of 4 μm ± 3 μm is formed on a paper substrate using an aqueous matte coating agent, the ratio (a / b) of the absorbance (a) of peak (A) below and the absorbance (b) of peak (B) below, obtained by attenuated total reflection measurement using a germanium prism at an incident angle of 45° by Fourier transform infrared spectroscopy, is 0.40 to 1.50. Peak (A): 1070-1130cm -1 The single point with the highest absorbance in this region. Peak (B): 1220~1280cm -1 The single point with the highest absorbance in this region.
[0298] In conditions (A), (B), and (C), the matte coat layer can be formed by coating a paper substrate with an aqueous matte coat agent. The thickness of the matte coat layer can be adjusted by adjusting the amount of aqueous matte coat agent applied. For example, the aqueous matte coat agent can be applied by flexographic printing. The paper substrate used has a surface roughness Sq of 0.4 ± 0.2 in a measurement field of view of 506 μm × 675 μm before the aqueous matte coat agent is formed. As a paper substrate with such a surface roughness Sq, for example, an aurora coated paper can be used, which has been offset printed with offset ink at a black density of 1.75 and cured with a UV lamp. Specifically, according to the manufacturing method of the laminate disclosed in the examples, a paper substrate with a predetermined surface roughness Sq can be prepared after the printing layer is formed but before the aqueous matte coat agent is formed, and an aqueous matte coat layer can be formed on this paper substrate. Note that even if no printing layer is formed, the numerical range will be approximately the same.
[0299] The surface roughness Sq, composite modulus, and absorbance ratio (a / b) of the matte coat layer formed in this manner can be measured as described above. The more preferable ranges for the surface roughness Sq, composite modulus, and absorbance ratio (a / b) of the matte coat layer are also as described above.
[0300] As the aqueous matte coating agent, inactive energy ray curable aqueous matte coating agents, active energy ray curable aqueous matte coating agents, etc., can be used. For the inactive energy ray curable aqueous matte coating agent, the resin raw material preferably contains an emulsion-type urethane resin, an emulsion-type acrylic resin, and a curing agent. For the active energy ray curable aqueous matte coating agent, the resin raw material preferably contains a polyfunctional urethane (meth)acrylate and at least one selected from the group consisting of hydroxyl group-containing ethylenically unsaturated monomers and alkylene oxy group-containing ethylenically unsaturated monomers. The active energy ray curable aqueous matte coating agent may further contain a curing agent.
[0301] The aqueous matte coating agent preferably contains 20 to 80% by mass of aqueous medium relative to the total mass of the aqueous matte coating agent, more preferably 20 to 70% by mass, even more preferably 25 to 75% by mass, and most preferably 30 to 70% by mass.
[0302] Details of the inactive energy ray-curable aqueous matte coating agent and the active energy ray-curable aqueous matte coating agent are as described above.
[0303] <Ink Set> In some embodiments, the ink set is characterized by comprising an aqueous matte coating agent and an active energy ray-curable offset ink, an active energy ray-curable flexographic ink, or a combination thereof.
[0304] As the aqueous matte coating agent, those described above can be used. Specifically, inactive energy ray curable aqueous matte coating agents and active energy ray curable aqueous matte coating agents can be used. Active energy ray curable offset inks and active energy ray curable flexographic inks are described below.
[0305] (Activated energy ray curing offset ink, activated energy ray curing flexographic ink) The above-mentioned active energy ray-curable offset ink and active energy ray-curable flexographic ink can be appropriately obtained, for example, by the methods described in Japanese Patent Application Publication No. 2025-110240 or Japanese Patent Application Publication No. 2019-127550. Preferably, the active energy ray-curable offset ink is an ink comprising a monomer, a resin, and a pigment.
[0306] The resin constituting the active energy ray-curable offset ink is preferably a resin having a ring structure, and preferably contains one or more selected from the group consisting of allyl resin, diallyl phthalate resin, rosin, maleated rosin, acrylic rosin, rosin-modified resin, epoxy resin, polyester resin, polyurethane resin, alkyd resin, and petroleum resin. The amount of the resin having a ring structure is preferably 2 to 30% by mass, and more preferably 4 to 25% by mass, based on the total amount of ink. The resin having a ring structure preferably contains diallyl phthalate resin.
[0307] The above monomer is preferably a (meth)acrylic compound, and more preferably a polyfunctional (meth)acrylate. The (meth)acrylic compound is not particularly limited and includes monofunctional (meth)acrylic compounds such as methyl (meth)acrylate and ethyl (meth)acrylate, ethylene glycol di(meth)acrylate, polyethylene glycol di(meth)acrylate (n=2-20), propylene glycol di(meth)acrylate, polypropylene glycol di(meth)acrylate (n=2-20), alkane (C4-C12) glycol di(meth)acrylate, and alkane (C4-C12) glycol ethylene glycol Diacrylate (2-20 mol) di(meth)acrylate, Alkane (C4-12) glycol propylene oxide adduct (2-20 mol) di(meth)acrylate, Hydroxypivalyl hydroxypivalate di(meth)acrylate, Tricyclodecane dimethylol di(meth)acrylate, Bisphenol A ethylene oxide adduct (2-20 mol) di(meth)acrylate, Hydrogenated bisphenol A di(meth)acrylate, Hydrogenated bisphenol A ethylene oxide adduct (2-20 mol) di(meth)acrylate Trifunctional (meth)acrylic compounds such as rilate, glycerin tri(meth)acrylate, glycerin ethylene oxide adduct (3-30 mol) tri(meth)acrylate, glycerin propylene oxide adduct (3-30 mol) tri(meth)acrylate, trimethylolpropane tri(meth)acrylate, trimethylolpropane ethylene oxide adduct (3-30 mol) tri(meth)acrylate, trimethylolpropane propylene oxide adduct (3-30 mol) tri(meth)acrylate, and trifunctional (meth)acrylic compounds such as rilate, glycerin tri(meth)acrylate, glycerin tri(meth)acrylate, trimethylolpropane propylene oxide adduct (3-30 mol) tri(meth)acrylate, etc. (Meth)acrylic compounds, pentaerythritol tetra(meth)acrylate, pentaerythritol ethylene oxide adduct (4-40 mol) tetra(meth)acrylate, pentaerythritol propylene oxide adduct (4-40 mol) tetra(meth)acrylate, diglycerin tetra(meth)acrylate, pentaerythritol ethylene oxide adduct (4-40 mol) tetra(meth)acrylate, pentaerythritol propylene oxide adduct (4-40 mol) tetra(meth)acrylate,Examples include (meth)acrylic compounds with four or more functions, such as ditrimethylolpropanetetra(meth)acrylate, ditrimethylolpropaneethylene oxide adduct (4-40 mol) tetra(meth)acrylate, ditrimethylolpropanepropylene oxide adduct (3-30 mol) tetra(meth)acrylate, dipentaerythritol hexa(meth)acrylate, dipentaerythritol ethylene oxide adduct (6-60 mol) hexa(meth)acrylate, dipentaerythritol propylene oxide adduct (6-60 mol) hexa(meth)acrylate, polyester (meth)acrylate, urethane (meth)acrylate other than (A), epoxy (meth)acrylate, and mixtures thereof. Among these, it is preferable to use a (meth)acrylic compound with three or more functions from the viewpoint of curability. Furthermore, from the viewpoint of curability, the proportion of the (meth)acrylic compound with three or more functions in the total amount of (meth)acrylic compounds is preferably 40-100% by mass. , [Examples]
[0308] The present disclosure will be described in detail below with reference to examples, but the present disclosure is not limited to these examples. In this disclosure, parts and % represent parts by mass and mass %, respectively, unless otherwise noted. In the table, Ex. indicates an example, and Comp. Ex. indicates a comparative example.
[0309] (Weight average molecular weight) The weight-average molecular weight was determined by measuring the molecular weight distribution using a GPC (gel permeation chromatography) instrument (HLC-8220, manufactured by Tosoh Corporation) and calculating the converted molecular weight using polystyrene as the standard substance. The measurement conditions are shown below. Columns: The following columns were used, connected in series. TSKgelSuperAW2500 manufactured by Tosoh Corporation TSKgel SuperAW3000 manufactured by Tosoh Corporation TSKgel SuperAW4000 manufactured by Tosoh Corporation TSKgel guard column Super AW-H manufactured by Tosoh Corporation Detector: RI (differential refractometer) Measurement conditions: Column temperature 40°C Eluent: Tetrahydrofuran Flow rate: 1.0 ml / min
[0310] (Glass transition temperature) The glass transition temperature (Tg) was determined by DSC (differential scanning calorimetry). A DSC8231 manufactured by Rigaku Corporation was used as the measuring apparatus, the measurement temperature range was -70 to 150°C, the temperature elevation rate was 10°C / min, and the midpoint between the endothermic onset temperature and end temperature based on the glass transition in the DSC curve was defined as the glass transition temperature.
[0311] (Acid value) The acid value is the mg amount of potassium hydroxide required to neutralize free fatty acids, resin acids and the like contained in 1 g of a sample, and was measured by the method described in JIS K 0070. The unit of the acid value is mgKOH / g.
[0312] (Hydroxyl value) The hydroxyl value is the mg amount of potassium hydroxide equivalent to the hydroxyl groups contained in 1 g of a sample, and was measured by the method described in JIS K 0070. The unit of the hydroxyl value is mgKOH / g.
[0313] (Average particle diameter of emulsified urethane resin, emulsified acrylic resin, fine resin particles, silica, and polyolefin wax) For each average particle diameter, each particle was diluted 500-fold with water, about 5 ml of the diluted solution was measured by a dynamic light scattering measurement method (measuring apparatus: Nanotrac UPA (manufactured by MicrotracBEL)), and the largest peak among the peaks of the obtained volume particle diameter distribution data (histogram) was taken as the particle diameter (mode diameter).
[0314] <Production of UV-curable offset ink> <Production of resin varnish A> Into a four-necked flask equipped with a stirrer, Dean-Stark tube, thermometer, and gas inlet tube, 30 parts of Daizodap A and 70 parts of MIRAMER M410 were charged, the mixture was heated to 100°C with stirring, and stirred and melted at 100°C for 2 hours to obtain Resin Varnish A. ·Daisodap A: weight average molecular weight 30,000, diallyl phthalate resin manufactured by Osaka Soda Co., Ltd. ·MIRAMER M410: ditrimethylolpropane tetraacrylate, manufactured by Miwon Specialty Chemical Co., Ltd.
[0315] <Production of UV-curable Offset Ink A> 18.0 parts of black pigment as a pigment, 40.0 parts of Resin Varnish A as a resin varnish, 12.9 parts of MIRAMER M600, 3.0 parts of MIRAMER M410, 8.0 parts of MIRAMER LR3130 as (meth)acrylate compounds, 4.0 parts of OMNIRAD 930, 1.5 parts of OMNIRAD DETX, 3.0 parts of OMNIRAD EMK as photopolymerization initiators, 4.0 parts of magnesium carbonate, 2.0 parts of Hi-Filler Talc 5000PJ as extender pigments, 1.0 part of Solsperse 24000, 2.5 parts of Sanwax 161P as additives, and 0.1 part of Q-1301 as a polymerization inhibitor were added, the mixture was stirred and mixed using a mixer, and dispersed with a three-roll mill to prepare UV-curable offset ink A.
[0316] [Colorant] ·Black pigment: MA-11, manufactured by Mitsubishi Chemical Corporation [(Meth)acrylate Compound] ·MIRAMER M600: dipentaerythritol hexaacrylate, manufactured by Miwon Specialty Chemical Co., Ltd. ·MIRAMER LR3130: trimethylolpropane EO-modified triacrylate, manufactured by Miwon Specialty Chemical Co., Ltd. [Photopolymerization Initiator] ·OMNIRAD 930: 2-dimethylamino-2-(4-methylbenzyl)-1-(4-morpholin-4-yl-phenyl)-butan-1-one, manufactured by IGM • OMNIRAD DETX: Manufactured by IGM, 2,4-diethylthioxanthone • OMNIRAD EMK: 4,4'-bis(diethylamino)benzophenone, manufactured by IGM. [Body pigments] • High-filler talc 5000PJ: Matsumura Sangyo Co., Ltd., talc [Polymerization inhibitor] • Q-1301: N-nitrosophenylhydroxylamine aluminum salt, manufactured by Fujifilm Wako Pure Chemical Industries, Ltd. [Additives (dispersants)] • Solspers 24000: Manufactured by Lubrizol, a pigment dispersant. [Additives (wax)] • Sanwax 161P: Manufactured by Sanyo Chemical Industries, Ltd., made from polyethylene resin.
[0317] <Test Example 1: Inactive Energy Ray Curing Type Aqueous Matte Coating Agent> <Manufacturing Example 1: Emulsified Urethane Resin A> In a reaction vessel equipped with a stirrer, thermometer, dropping funnel, and reflux apparatus, 50.0 parts of polycarbonate diol (product name: ETERNACOLL UH-200, manufactured by UBE Corporation, number average molecular weight 1958, hydroxyl value 57.3 mg KOH / g, polycarbonate diol obtained by reacting 1,6-hexanediol with a carbonate ester), 1.7 parts of 2,2-dimethylolpropionic acid, 10.0 parts of dicyclohexylmethane diisocyanate, and 10.0 parts of tetramethylxylene diisocyanate were heated at 80-90°C for 4 hours under a nitrogen atmosphere in the presence of 15.2 parts of dipropylene glycol dimethyl ether and 0.05 parts of dibutylsus laurate. Quantification of residual NCO revealed an OH conversion rate of 98% or more. After the reaction mixture was brought to 80°C, 2.8 parts of triethylamine were added and the mixture was stirred for 30 minutes. Furthermore, this reaction mixture was added to 233.3 parts of water while being vigorously stirred, and then 10.2 parts of 2-(2-aminoethylamino)ethanol was added to obtain emulsified urethane resin A.
[0318] <Manufacturing Examples 2 and 3: Emulsified Urethane Resins B and C> Emulsified urethane resins B and C were obtained in the same manner as emulsion-type urethane resin A, except that the raw materials and mixing ratios listed in Table 1 were changed.
[0319] [Table 1]
[0320] <Manufacturing Example 4: Emulsified Acrylic Resin A> 65.0 parts styrene, 11.5 parts n-butyl acrylate, 1.9 parts acrylic acid, 1.5 parts tert-dodecyl mercaptan, 1.4 parts Hythenol NF-08 (manufactured by Daiichi Kogyo Seiyaku Co., Ltd.), and 40.4 parts deionized water were pre-mixed and stirred to prepare an emulsion of ethylenically unsaturated monomers. In a reaction vessel equipped with a stirrer, thermometer, dropping funnel, and reflux apparatus, 68.9 parts deionized water and 5% of the emulsion were added. The internal temperature was raised to 80°C and the mixture was thoroughly purged with nitrogen. Then, 2.0 parts 5% aqueous solution of potassium persulfate (0.1 parts solids) was added as an initiator to start emulsion polymerization. While maintaining the internal temperature at 80°C, the remaining emulsion and 2.0 parts 5% aqueous solution of potassium persulfate (0.1 parts solids) were added dropwise over 3 hours, and the reaction was continued for a further 4 hours. After the reaction was complete, 1.8 parts of 25% aqueous ammonia were added to neutralize the mixture, and the solid content of the aqueous dispersion was adjusted to 30.0% with deionized water to obtain emulsion-type acrylic resin A.
[0321] <Manufacturing Examples 5 and 6: Emulsified Acrylic Resins B and C> Emulsified acrylic resins B and C were obtained in the same manner as emulsion acrylic resin A, except that the raw materials and mixing ratios listed in Table 2 were changed.
[0322] [Table 2]
[0323] (Example 1) Table 3 shows the formulations of aqueous matte coating agents. In the table, NV (solid content) is in mass%, particle size (average particle size) is in μm, Tg is the glass transition temperature (°C), and acid value and hydroxyl value are in mgKOH / g.
[0324] <Preparation of water-based matte coating agent> 60 parts of emulsified urethane resin A, 17 parts of emulsified acrylic resin A, 15 parts of urethane resin fine particles A, and as additives 0.5 parts of defoaming agent, 1 part of slip agent, 3.5 parts of polyolefin wax, and 3.5 parts of water were added and mixed, and stirred for 90 minutes with a bladed stirrer to obtain aqueous matte coating agent W1.
[0325] <Preparation of paper substrate> Using a sheet-fed printing press "Lithrone 26" (manufactured by Komori Corporation), UV-curable offset ink A was printed onto Aurora Coat (coated paper, high-gloss type, 81 μm thickness, manufactured by Nippon Paper Industries Co., Ltd.) paper substrate to a black density of 1.75 (measurement instrument: X-RiteeXact (manufactured by X-Rite Corporation), conditions: illuminant D50, standard observer 2°, density status E, no filter), and cured with a UV lamp. The printing speed for the above printing was 8000 sheets / hour, the UV lamps consisted of two air-cooled metal halide lamps and one high-pressure mercury lamp, and the UV lamp intensity for all three lamps was set to 160 W / cm (cumulative light intensity 450 mJ / cm). 2 The surface roughness Sq of the paper substrate after printing was 0.4.
[0326] <Fabrication of laminates> On the printed material of UV-curable offset ink A obtained above, an aqueous matte coating agent W1 containing 5% by mass of isocyanate-based curing agent Aquanate AQ-140 (Tosoh Corporation) was applied using a Lithrone 26 flexographic coating unit immediately before printing. After drying with an IR lamp, the aqueous matte coating agent W1 was applied again in the same manner and dried to obtain a laminate L1. The anilox roll of the above coating unit had a trihelical engraving pattern, a line count of 300 lines / inch, and a cell volume of 9 ml / m². 2The following materials were used. Furthermore, during flexographic coating, the printing speed was set to 8000 sheets / hour, the liquid temperature of the water-based matte coating agent W1 was 25°C, and the ambient temperature inside the IR drying oven was controlled to 60-100°C. The thickness of the matte coating layer was 4 μm.
[0327] (Examples 2-40, Comparative Examples 1-13) Except for using the aqueous matte coating agent with the components shown in Table 3 and the printing conditions shown in Table 4, aqueous matte coating agents W2-18 and T1-T6 for Examples 2-18 and Comparative Examples 1-6, and laminates L1-L22 and M1-M7 for Examples 19-40 and Comparative Examples 7-13 were prepared according to the same procedure as in Example 1. In Comparative Example 7, PET was used as the substrate.
[0328] (component) Details of the components used in each example and comparative example are shown below.
[0329] (Emulsified epoxy resin) Emulsified epoxy resin: W2821R70, solids content 70% by mass, manufactured by Mitsubishi Chemical Corporation.
[0330] (Resin fine particles) Urethane resin microparticles A: ART PEARL MM-120T, average particle size 2 μm, Tg = 22℃, manufactured by Negami Kogyo Co., Ltd. Urethane resin microparticles B: ART PEARL CE-1000T, average particle size 3 μm, Tg = 34℃, manufactured by Negami Kogyo Co., Ltd. Urethane resin microparticles C: ART PEARL MM120TK, average particle size 2 μm, Tg = 80℃, manufactured by Negami Kogyo Co., Ltd. Urethane resin fine particles D:ART PEARL C-1000T, average particle size 3μm, Tg=-13℃, manufactured by Negami Kogyo Co., Ltd. Urethane resin microparticles E:ART PEARL C800T, average particle size 6μm, Tg=-13℃, manufactured by Negami Kogyo Co., Ltd. Urethane resin microparticles F:ART PEARL C600T, average particle size 10 μm, Tg = -13℃, manufactured by Negami Kogyo Co., Ltd. Acrylic resin fine particles A: ART PEARL J-4PY, average particle size 2 μm, manufactured by Negami Kogyo Co., Ltd. Acrylic resin fine particles B: ART PEARL BE-003TC, average particle size 2.5 μm, manufactured by Negami Kogyo Co., Ltd. Acrylic resin fine particles C: ART PEARL J-3PY, average particle size 1.2μm, manufactured by Negami Kogyo Co., Ltd. Benzoguanamine resin microparticles: Epostor L15, manufactured by Nippon Shokubai Co., Ltd.
[0331] (Additives) Antifoaming agent: Tegoformex 1488, manufactured by Evonik Japan Co., Ltd. Slip agent: BYK-SILCLEAN 3720, manufactured by BYK Chemie Japan Co., Ltd. Polyolefin wax: Hi-Tec S-3121, average particle size 0.04 μm, manufactured by Toho Chemical Industry Co., Ltd.
[0332] (Hardening agent) Isocyanate-based curing agent: Bahijur 2487 / 1 (manufactured by Covestro). Carbodiimide-based curing agent: Carbodilite E-02 (manufactured by Nisshinbo Chemical Co., Ltd.). Aziridine-based hardener: Cross Linker CX-100 (manufactured by COVESTRO). Amine-based curing agent: Gaskimine 240 (manufactured by Mitsubishi Gas Chemical Company, Ltd.).
[0333] (Comparative Example 14) <Solvent-free activated energy ray curing matte coating agent T7> <Synthesis of urethane acrylate> In a 4 L separable four-necked flask equipped with a stirrer, thermometer, and condenser, 262 parts (1 mole) of dicyclohexylmethane 4,4'-diisocyanate (product name: Desmodulo W, manufactured by Sumika Covestro Urethane Co., Ltd.), 2000 parts (2 moles) of polytetramethylene ether glycol (product name: PTMG1000, manufactured by Mitsubishi Chemical Corporation), 232 parts (2 moles) of 2-hydroxyethyl acrylate (product name: Hydroxyethyl acrylate, manufactured by Osaka Organic Chemical Industry Co., Ltd.), and 1.247 parts (500 ppm) of p-methoxyphenol were charged. The mixture was stirred while introducing air and reacted at 80°C for 4 hours. After confirming the disappearance of the peak attributable to the isocyanate group by IR spectroscopy, the reaction was terminated, and the mixture was cooled to 40°C to obtain 2262 parts of a pale yellow liquid (UA11). The weight-average molecular weight of urethane acrylate UA11 was 2200, the Tg was 25°C, and the number of functional groups was 2.
[0334] <Preparation of Active Energy Ray Curable Matte Coating Agent T7> Twelve parts of urethane acrylate UA11, forty-seven parts of 4-HBA (4-hydroxybutyl acrylate, manufactured by Osaka Organic Co., Ltd.), twenty-five parts of ART PEARL MM-120T (urethane-based fine particles, average particle size 2 μm, glass transition temperature "Tg" 22°C, manufactured by Negami Kogyo Co., Ltd.), four parts of the photopolymerization initiator Omnirad TPO (2,4,6-trimethylbenzoyldiphenylphosphine oxide, manufactured by IGM), and twelve parts of a silicone-based defoaming agent as an additive were mixed and stirred for 90 minutes with a bladed stirrer to obtain a solvent-free active energy ray curable matte coating agent T7.
[0335] Laminate M8 was obtained in the same manner as in Example 1, except that the solvent-free active energy ray curable matte coating agent T7 was used.
[0336] (evaluation) The aqueous matte coating agents and laminates obtained in the examples and comparative examples were evaluated as follows. The evaluation results are shown in Tables 3 and 4.
[0337] <Viscosity of water-based matte coating agent at 25°C> Viscosity was measured according to the method specified in JIS K5600-2, using a cone-plate type viscometer with a cone diameter of 35 mm and a cone angle of 2°, at a shear rate of 100 units per second in a 25°C environment.
[0338] <Surface roughness of the matte coat layer (Sq)> The mean square roughness (Sq) of the matte coat layer surface of the laminates obtained in the examples and comparative examples was measured. Sq was measured using a laser microscope (VK-X3000, manufactured by Keyence Corporation, measurement field of view 506 μm vertically × 675 μm horizontally) according to the measurement method compliant with ISO 25178.
[0339] The surface roughness Sq was determined in accordance with the roughness standard ISO25178-2:2012, using the average value measured at five arbitrary locations on the surface of the matte coat layer by the following method. The surface shape measurement conditions were as follows: Measurement mode: surface shape, Scan mode: laser confocal, Measurement magnification: objective lens magnification (20x, optical zoom 1x, numerical aperture (NA) 0.46), Measurement field of view: 506 μm vertical × 675 μm horizontal, Image processing: reference plane setting processing, Filter type: Gaussian, S-filter: none, L-filter: none, F-operation: none, Termination effect correction: enabled, Measurement pitch: 0.5 μm, Illumination filter: 100%, Double scan: OFF, Field curvature correction: ON, Light intensity eccentricity correction: ON, Received light intensity correction mode: γ correction, γ coefficient: 0.45, Offset: 0%. The thickness of the matte coat layer in each example and comparative example was 4 μm. The thickness of the matte coating layer was measured using a cross-sectional sample of the matte coating, and the measurement was taken from cross-sectional images using a scanning electron microscope (SEM) (JEOL JIB-4600F, 3,000x magnification). Specifically, the distance from the substrate or the interface between the printed layer and the coating layer to the vertices of the spherical surfaces of the microparticles protruding from the surface was measured at five randomly selected measurement points in the cross-sectional image, and the average value was used.
[0340] <Composite modulus of elasticity of matte coat layer Er> The composite modulus Er of the matte coat layer was measured for the laminates obtained in the examples and comparative examples using the following method. The composite modulus is a parameter measured using a micro-area mechanical property evaluation device (nanoindenter), and was measured using a Hyzitron TI Premier (manufactured by Bruker). In the matte coat layer, the resin matrix portion is the portion other than the resin nanoparticles. Since the resin nanoparticles are observed as spherical in the matte coat layer, the composite modulus was measured in the portion excluding these spherically observed portions. Furthermore, in the matte coat layer, the uneven shape of the 50 μm square observation area was further observed in a 20 μm square area using the SPM function attached to the nanoindenter, particularly for the taller convex portions, and then measured in the portion excluding the spherically observed resin nanoparticle portions.
[0341] The measurement conditions involve using a triangular pyramidal cubecorner indenter as the indenter of the nanoindenter. The cubecorner indenter is pressed into the sample under the indentation conditions described below, and the indentation depth h (nm) for each indentation load F (μN) is continuously measured to create a load-displacement curve. From the created load-displacement curve, the slope S (contact stiffness) of the unloading curve is determined, and the contact projected area Ac (μm²) between the indenter and the sample is calculated. 2 The following formula (1) is used to determine the value. Here, Ac is the contact projected area obtained by correcting the curvature of the indenter tip using the standard method of the apparatus with fused silica of the standard sample. The indentation conditions are as follows: at room temperature, first the indenter is pressed to a depth of 200 nm for 5 seconds (i.e., 40 nm / s), then held at a depth of 200 nm for 2 seconds, and finally unloaded to 0 nm in 5 seconds. The composite modulus of the matte coat layer means the arithmetic mean of 10 or more measured values.
[0342]
number
[0343] <Infrared spectroscopy of matte coated layer: absorbance ratio (a / b)> The absorbance ratio (a / b) was determined by measuring the absorbance (a) of peak (A) and the absorbance (b) of peak (B) below using attenuated total reflectance (ATR) measurement by Fourier transform infrared spectroscopy (FT-IR) according to the following conditions, and then calculating the ratio between them. Equipment: Fourier transform infrared spectrophotometer (Thermo Fisher Scientific, Inc., equivalent to Nicolet iS5) Detector: MCT detector (liquid nitrogen cooled type) Prism: Germanium (Ge) Incident angle: 45° Wavenumber resolution: 4cm -1 Total number of times: 32 Gain: 4 Measurement wavefrequency range: 700~2000cm -1 Peak (A): 1070-1130cm -1 The single point with the highest absorbance in this region. Peak (B): 1220~1280cm -1 The single point with the highest absorbance in this region.
[0344] <Water-based matte coating agent: skin irritation> The compositions obtained in the examples and comparative examples were subjected to primary skin irritation tests in rabbits in accordance with the OECD Guideline for the Testing of Chemicals 404 (2002). In the primary skin irritation test in rabbits, a 2cm x 2cm gauze impregnated with the test composition was placed on the shaved back skin of a male Japanese white rabbit, secured with Serapore® tape (3.8cm x 5cm, Nichiban Co., Ltd.), fitted with a rabbit jacket (14101320: LOMIR Co., Ltd.), and returned to the cage. After 24 hours, the cotton impregnated with the test composition was removed, and the formation of erythema, scabs, and edema was observed macroscopically at 1 hour, 24 hours, and 48 hours after removal, and scored according to the scoring criteria of Draize et al. Primary skin irritation was determined by calculating the Primary Irritation Index (PII). The primary skin irritation index was calculated based on ISO 10993-10 Biological Evaluation of Medical Devices-Part 10 (2010). The average scores for erythema, crusting, and edema formation were determined for each individual at 1, 24, and 48 hours after peeling. The sum of the average scores for each group was then calculated and divided by 3 to determine the primary skin irritation index. The evaluation criteria are as follows:
[0345] 5 (Excellent): PII 0 or higher and less than 0.4 4 (Good): PII 0.5 or higher and less than 0.9 3 (Acceptable): PII 0.9 or higher and less than 2.0 2 (Not acceptable): PII 2.0 or higher and less than 5.0 1 (poor): PII 5.0 or more but less than 8.0 Note that values 3-5 are within a range that does not pose any practical problems.
[0346] Draize et al.'s scoring criteria (evaluation of skin reactions) <Formation of erythema and scabs> No erythema: 0 Very mild erythema (barely discernible): 1 Clear erythema: 2 Moderate to severe erythema: 3 From severe erythema to slight scab formation (up to deep injury): 4
[0347] <Edema formation> No edema: 0 Very mild edema (barely discernible): 1 Mild edema (with a clearly defined border due to a distinct bulge): 2 Moderate edema (bulge of approximately 1 mm): 3 Severe edema (bulge of 1 mm or more and spread beyond the exposed area): 4
[0348] <Soft touch feel of the matte coating layer> The soft-touch feel of the matte coat layer surface was evaluated for the laminates obtained in the examples and comparative examples. Here, soft-touch feel refers to the feeling of "soft, smooth, and moist" that a person feels when touching the surface of an object. The soft-touch feel was evaluated by having 30 sensory evaluators directly touch the matte coat layer with their fingertips, and the percentage of people who felt a soft touch was calculated relative to the total number of evaluators. Before conducting the sensory evaluation, the evaluators washed their hands with detergent and dried them thoroughly. The evaluation criteria are as follows. 5 (Excellent): Over 95% of users felt it had a soft touch. 4 (Good): 70% to less than 95% of people felt it had a soft touch. 3 (Acceptable): The percentage of people who felt it had a soft touch was between 50% and 70%. 2 (Not acceptable): The percentage of people who felt it had a soft touch was between 30% and 50%. 1 (Inferior): Less than 30% of people felt it had a soft touch. Note that values 3-5 are within a range that does not pose any practical problems.
[0349] <Glossiness of matte coat layer: 60°> The glossiness of the matte coat layer surface was measured for the laminates obtained in the examples and comparative examples. Glossiness was measured at an incident angle of 60 degrees. The evaluation criteria are as follows. A MicroTrigloss measuring device manufactured by BYK was used for gloss measurement. 5 (Excellent): Glossiness less than 8 4 (Good): Glossiness level 8 or higher but less than 10 3 (Acceptable): Glossiness level between 10 and 15 2 (Not acceptable): Gloss level 15 or higher but less than 20 1 (Inferior): Glossiness 20 or higher The ratings for practical use are 3, 4, and 5.
[0350] <Blocking resistance of the matte coating layer> The matte coated side of the laminate obtained in the examples and comparative examples was bonded to the back side of an Aurora Coat paper substrate (coated paper high gloss type, paper thickness 81 μm, manufactured by Nippon Paper Industries Co., Ltd.), and the results were obtained at a temperature of 50°C, humidity of 80%, and a load of 2 kgf / cm². 2 The samples were pressed together for 24 hours under the specified conditions, and the resistance to peeling and the degree of peeling of the printed surface were evaluated. The evaluation criteria were as follows: 5 (Excellent): No peeling or resistance was felt on surfaces with a matte coating. 4 (Good): There is no peeling on surfaces with a matte coating, but some resistance can be felt. 3 (Acceptable): There is a thin peel of less than 2% on the surface with the matte coating layer. 2 (Not acceptable): Thin peeling of 2% to less than 5% and / or thick peeling on the surface with the matte coating layer. 1 (Inferior): More than 5% peeling on the surface with the matte coating layer. Note that values 3-5 are within a range that does not pose any practical problems.
[0351] <Friction and abrasion properties of the matte coating layer> The laminates obtained in the examples and comparative examples were subjected to abrasion resistance tests using a JSPS-type friction fastness tester (load 500g, 2000 cycles, paper: high-quality paper) manufactured by Tester Sangyo Co., Ltd., and scratches that occurred on the coating surface were evaluated. The evaluation criteria were as follows. 5 (Excellent): Completely undamaged 4 (Good): Damage area is between 1% and less than 3%. 3 (Acceptable): Area of injury is 3% or more but less than 5% 2 (Not acceptable): Damaged area is 5% or more but less than 10% 1 (Inferior): Area of injury is 10% or more. The ratings for practical use are 3, 4, and 5.
[0352] [Table 3]
[0353] [Table 3]
[0354] [Table 4]
[0355] <Test Example 2: Active Energy Ray Curing Aqueous Matte Coating Agent> (Examples 41 and 97) <Preparation of Active Energy Ray Curable Aqueous Matte Coating Agent U1> 40 parts of polyfunctional urethane (meth)acrylate UA3 (polyester polyol-based aliphatic urethane (meth)acrylate, 2 functional groups) (dispersion of 40 parts solids and 60 parts water), 10 parts of 4-hydroxybutyl acrylate, 15 parts of ART PEARL MM-120T (urethane fine particles), 5 parts of OmniradTPO-L (2,4,6-trimethylbenzoyldiphenylphosphine oxide) as a photopolymerization initiator, 15 parts of a dispersant (acrylic resin-type dispersant) as an additive, 3 parts of a surfactant (acetylene glycol-based surfactant, HLB value 4), 1 part of an antifoaming agent, 1 part of a slip agent, and 10 parts of polyolefin wax were mixed and stirred for 90 minutes with a bladed stirrer to obtain an active energy ray-curable aqueous matte coating agent U1.
[0356] <Preparation of paper substrate> Using a sheet-fed printing press "Lithrone 26" (manufactured by Komori Corporation), UV-curable offset ink A was printed onto a paper substrate, Aurora Coat (coated paper, high gloss type, paper thickness 81 μm, manufactured by Nippon Paper Industries Co., Ltd.), to a black density of 1.75 (measurement instrument: X-RiteeXact (manufactured by X-Rite Corporation), conditions: illuminant D50, standard observer 2°, density status E, no filter), and cured with a UV lamp. The printing speed for the above printing was 8000 sheets / hour, and the UV lamps consisted of two air-cooled metal halide lamps and one high-pressure mercury lamp, with the UV lamp intensity set to 160 W / cm for all three lamps (cumulative light intensity 450 mJ / cm2). The surface roughness Sq of the paper substrate after printing was 0.4.
[0357] <Fabrication of laminate G1> On the printed material of UV-curable offset ink A obtained above, an active energy ray-curable aqueous matte coating agent U1 was applied using the Lithrone 26 flexographic coating unit. After IR drying, it was cured with a UV lamp, and then U1 was applied again in the same manner, dried, and cured to obtain laminate G1. The anilox roll of the above coating unit had a trihelical engraving pattern, a line count of 300 lines / inch, and a cell volume of 9 ml / m². 2 The following materials were used. During flexographic coating, the printing speed was set to 8000 sheets / hour, the liquid temperature of U1 was 25°C, and the ambient temperature inside the IR drying oven was controlled to 60-100°C. The type, number, and intensity of the UV lamps were the same as those used for the curing conditions of UV-curable offset ink A described above. The thickness of the matte coat layer was 4 μm.
[0358] (Examples 42-96, 98-156) Except for using an active energy ray-curable aqueous matte coating agent with the components shown in Tables 5 and 6, aqueous matte coating agents U2 to U56 of Examples 42 to 96 and laminates G2 to G60 of Examples 98 to 156 were prepared according to the same procedure as in Example 41.
[0359] (Example 95) Laminate G55 was obtained in the same manner as in Example 41, except that aqueous matte coating agent U55 was used, which was prepared by adding 3% by mass of the aziridine-based curing agent Cross linker CX-100 (manufactured by COVESTRO) to the active energy ray curing aqueous matte coating agent U1 described in Example 41 immediately before printing.
[0360] (Example 96) Laminate G56 was obtained in the same manner as in Example 41, except that aqueous matte coating agent U56 was used, which was prepared by adding 3% by mass of the carbodiimide-based curing agent Carbodilite SV-02 (manufactured by Nisshinbo Chemical Co., Ltd.) to the active energy ray-curable aqueous matte coating agent U1 described in Example 41 immediately before printing.
[0361] <Ingredients> Details of the components used in each example and comparative example are shown below. (Polyfunctional urethane (meth)acrylate) UA1 is an aliphatic urethane (meth)acrylate (containing a polyether structure, with 2 functional groups), with a weight-average molecular weight of 6,000. UA2 is an aliphatic urethane (meth)acrylate (containing a polyether structure, with 6 functional groups), with a weight-average molecular weight of 6,000. UA3 is an aliphatic urethane (meth)acrylate (containing polyester structure, 2 functional groups), with a weight-average molecular weight of 6,000. UA4 is an aliphatic urethane (meth)acrylate (containing polyester structure, 6 functional groups), with a weight-average molecular weight of 3,000. UA5 is an aliphatic urethane (meth)acrylate (containing a polycarbonate structure, with 2 functional groups), with a weight-average molecular weight of 6,000. UA6 is an aliphatic urethane (meth)acrylate (containing a polycarbonate structure, with 6 functional groups), with a weight-average molecular weight of 6,000.
[0362] (Ethylene-unsaturated monomer Ma) (Hydroxy group-containing ethylenically unsaturated monomer) M1 4-Hydroxybutylacrylate M2 Hydroxyethyl Acrylate
[0363] (Ethylene oxy group-containing ethylenic monomer) M3 Tetraethylene glycol di(meth)acrylate M4 Polyethylene Glycol 200 Diacrylate M5 Polyethylene Glycol 400 Diacrylate M6 Polyethylene Glycol 600 Diacrylate M7 Propion oxide-modified trimethylolpropane triacrylate M8 Propylene Oxide Modified Glycerin Triacrylate M9 Ethylene oxide-modified pentaerythritol tetraacrylate
[0364] (Ethylene-unsaturated monomer without alkylene oxy groups) M10 Dipentaerythritol Hexaacrylate M11 Ditrimethylolpropanetetraacrylate M12 Pentaerythritol Triacrylate
[0365] (Polymerization initiator) Omnirad TPO-L, manufactured by IGM Corporation. Omnirad 1173, manufactured by IGM Corporation.
[0366] (Resin fine particles) ART PEARL MM-120T (urethane resin microparticles), average particle size 2μm, Tg=22℃, manufactured by Negami Kogyo Co., Ltd. ART PEARL C-800 transparent (urethane resin microparticles), average particle size 6μm, Tg=-13℃, manufactured by Negami Kogyo Co., Ltd. ART PEARL C-1000 transparent (urethane resin fine particles), average particle size 3μm, Tg=-13℃, manufactured by Negami Kogyo Co., Ltd. Urethane resin fine particles S1:TG-30℃, aqueous dispersion. Urethane resin fine particles S2:TG-40℃, aqueous dispersion. Urethane resin fine particles S3:Tg-50℃, aqueous dispersion. ART PEARL J-4P (acrylic resin fine particles), average particle size 2.2μm, manufactured by Negami Kogyo Co., Ltd.
[0367] (Inorganic fine particles) Silica microparticles (Silysia 310P, manufactured by Fuji Silysia Chemical Co., Ltd.)
[0368] (Additives) Antifoaming agent Tegoformex 1488, manufactured by Evonik Japan Co., Ltd. Dispersant BYK-193, manufactured by BIC Chemie Japan Co., Ltd. Surfactant Surfinol 440, manufactured by Nisshin Chemical Industry Co., Ltd. Slip agent Tegoglide 496, manufactured by Evonik Japan Co., Ltd. Polyolefin wax Chemipearl W500, manufactured by Mitsui Chemicals, Inc.
[0369] (evaluation) The active energy ray-curable aqueous matte coating agents and laminates obtained in the examples and comparative examples were evaluated in the same manner as the non-active energy ray-curable aqueous matte coating agent described above. The evaluation results are shown in Tables 5 and 6.
[0370] [Table 5]
[0371] [Table 5]
[0372] [Table 5]
[0373] [Table 5]
[0374] Table 5
[0375] Table 6
[0376] Table 6
Claims
1. It has a paper substrate and a matte coating layer. The matte coating layer comprises a resin matrix having a urethane resin structure and an acrylic resin structure, and resin fine particles. The constituent component having the urethane resin structure is present in an amount of 15 to 95% by mass relative to the total solid content of the resin matrix. The component having the acrylic resin structure is present in an amount of 5 to 60% by mass relative to the total solid content of the resin matrix. A matte laminate that satisfies the following conditions (1), (2), and (3). (1) The surface roughness Sq of the matte coating layer in a measurement field of view of 506 μm × 675 μm is 0.5 to 3.
5. (2) The matte coating layer has a composite modulus of 4 GPa or less (wherein the composite modulus is the composite modulus of the resin matrix portion measured by nanoindentation). (3) The matte coating layer has a ratio (a / b) of the absorbance (a) of peak (A) and the absorbance (b) of peak (B) obtained at an incident angle of 45° using a germanium prism by attenuated total reflection measurement by Fourier transform infrared spectroscopy, which is 0.40 to 1.
50. Peak (A): 1070–1130 cm -1 The single point with the highest absorbance in the region. Peak (B): 1220–1280 cm -1 The single point with the highest absorbance in the region.
2. The matte laminate according to claim 1, wherein the resin matrix is a cured product of a resin raw material comprising an emulsion-type urethane resin, an emulsion-type acrylic resin, and a curing agent.
3. The matte laminate according to claim 2, wherein the amount of emulsion-type urethane resin solids is 30 to 95% by mass, the amount of emulsion-type acrylic resin solids is 0.1 to 50% by mass, and the amount of curing agent is 1 to 40% by mass, with respect to the total amount of solids in the resin matrix.
4. The matte laminate according to claim 2, wherein the curing agent comprises an isocyanate-based curing agent, an aziridine-based curing agent, or a combination thereof.
5. The matte laminate according to claim 1, wherein the resin matrix is a cured product of a resin raw material comprising a polyfunctional urethane (meth)acrylate and at least one selected from the group consisting of a hydroxyl group-containing ethylenically unsaturated monomer and an alkylene oxy group-containing ethylenically unsaturated monomer.
6. The matte laminate according to claim 1, wherein the polyfunctional urethane (meth)acrylate is 15 to 100% by mass with respect to the total solid content of the resin matrix, and at least one selected from the group consisting of hydroxyl group-containing ethylenically unsaturated monomers and alkylene oxy group-containing ethylenically unsaturated monomers is 0.03 to 85% by mass in total.
7. The matte laminate according to claim 5, wherein the resin raw material further comprises a curing agent.
8. The matte laminate according to claim 7, wherein the curing agent comprises an isocyanate-based curing agent, an aziridine-based curing agent, or a combination thereof.
9. The matte laminate according to any one of claims 1 to 8, wherein the paper substrate further comprises a printed layer.
10. The matte laminate according to claim 9, wherein the printed layer includes a printed layer obtained using an active energy ray-curable offset ink, a printed layer obtained using an active energy ray-curable flexographic ink, or a combination thereof.
11. The resin raw material for forming a resin matrix having a urethane resin structure and an acrylic resin structure, resin fine particles, and an aqueous medium, The constituent component having the urethane resin structure is present in an amount of 15 to 95% by mass relative to the total solid content of the resin matrix. The component having the acrylic resin structure is present in an amount of 5 to 60% by mass relative to the total solid content of the resin matrix. A water-based matte coating agent that satisfies the following conditions (A), (B), and (C). (A) When a matte coat layer with a thickness of 4 μm ± 3 μm is formed on a paper substrate using an aqueous matte coat agent, the surface roughness Sq of the matte coat layer in a measurement field area of 506 μm × 675 μm is 0.5 to 3.
5. Here, the surface roughness Sq of the paper substrate used to measure the surface roughness Sq is 0.4 ± 0.2 in a measurement field area of 506 μm × 675 μm before the matte coat layer is formed. (B) When a matte coating layer with a thickness of 4 μm ± 3 μm is formed on a paper substrate using an aqueous matte coating agent, the composite modulus of elasticity is 4 GPa or less (wherein the composite modulus of elasticity is the composite modulus of the resin matrix portion measured by the nanoindentation method). (C) When a matte coat layer with a thickness of 4 μm ± 3 μm is formed on a paper substrate using an aqueous matte coat agent, the ratio (a / b) of the absorbance (a) of peak (A) below and the absorbance (b) of peak (B) below, obtained by the attenuated total reflection measurement method of Fourier transform infrared spectroscopy using a germanium prism at an incident angle of 45°, is 0.40 to 1.
50. Peak (A): 1070–1130 cm -1 The single point with the highest absorbance in the region. Peak (B): 1220–1280 cm -1 The single point with the highest absorbance in the region.
12. The aqueous matte coating agent according to claim 11, wherein the content of the aqueous medium is 20 to 70% by mass.
13. The aqueous matte coating agent according to claim 11 or 12, wherein the resin raw material is of the inactive energy ray curing type, and comprises an emulsion-type urethane resin, an emulsion-type acrylic resin, and a curing agent.
14. The aqueous matte coating agent according to claim 13, wherein the amount of emulsion-type urethane resin solids is 30 to 100% by mass, the amount of emulsion-type acrylic resin solids is 0.1 to 50% by mass, and the amount of curing agent is 1 to 40% by mass, with respect to the total amount of solids in the resin matrix.
15. The aqueous matte coating agent according to claim 13, wherein the curing agent comprises an isocyanate-based curing agent, an aziridine-based curing agent, or a combination thereof.
16. The aqueous matte coating agent according to claim 11 or 12, wherein the active energy ray curing type is wherein the resin raw material comprises a polyfunctional urethane (meth)acrylate and at least one selected from the group consisting of hydroxyl group-containing ethylenically unsaturated monomers and alkylene oxy group-containing ethylenically unsaturated monomers.
17. The aqueous matte coating agent according to claim 16, wherein the polyfunctional urethane (meth)acrylate is 15 to 100% by mass with respect to the total solid content of the resin matrix, and the sum of at least one selected from the group consisting of hydroxyl group-containing ethylenically unsaturated monomers and alkylene oxy group-containing ethylenically unsaturated monomers is 0.03 to 85% by mass.
18. The aqueous matte coating agent according to claim 16, wherein the resin raw material further comprises a curing agent.
19. The aqueous matte coating agent according to claim 18, wherein the curing agent comprises an isocyanate-based curing agent, an aziridine-based curing agent, or a combination thereof.
20. The aqueous matte coating agent according to claim 11 or 12, wherein the paper substrate further comprises a printed layer.
21. An ink set comprising the aqueous matte coating agent according to claim 11 or 12, and an active energy ray-curable offset ink, an active energy ray-curable flexographic ink, or a combination thereof.
22. A non-activating energy ray curing aqueous matte coating agent, In relation to the total solid content of the inactive energy ray curable aqueous matte coating agent, 15 to 50% by mass of an emulsified urethane resin having an acid value of 0 to 50 mg KOH / g, 5 to 50% by mass of an emulsified acrylic resin having an acid value of 1 to 100 mg KOH / g, and It contains 5 to 70% by mass of resin fine particles having a glass transition temperature (Tg) of -80 to 130°C. The aqueous matte coating agent according to claim 11.
23. An activated energy ray curing aqueous matte coating agent, The active energy ray curable aqueous matte coating agent contains 10 to 45% by mass of a polyfunctional urethane (meth)acrylate having an acidic group, based on the total solid content. The polyfunctional urethane (meth)acrylate contains a total of 40 to 140 parts by mass of at least one selected from the group consisting of hydroxyl group-containing ethylenically unsaturated monomers and alkylene oxy group-containing ethylenically unsaturated monomers, per 100 parts by mass. The active energy ray curable aqueous matte coating agent contains 10 to 90% by mass of resin fine particles having a glass transition temperature (Tg) of -80 to 130°C, relative to the total solid content. The aqueous matte coating agent according to claim 11.
24. The paper substrate and the matte coat layer obtained using the aqueous matte coat agent described in claim 22 or 23 are provided. The matte coating layer comprises a resin matrix having a urethane resin structure and an acrylic resin structure, and resin fine particles. A matte laminate that satisfies the following conditions (1), (2), and (3). (1) The surface roughness Sq of the matte coating layer in a measurement field of view of 506 μm × 675 μm is 0.5 to 3.
5. (2) The matte coating layer has a composite modulus of 4 GPa or less (wherein the composite modulus is the composite modulus of the resin matrix portion measured by nanoindentation). (3) The matte coating layer has a ratio (a / b) of the absorbance (a) of peak (A) and the absorbance (b) of peak (B) obtained at an incident angle of 45° using a germanium prism by attenuated total reflection measurement by Fourier transform infrared spectroscopy, which is 0.40 to 1.
50. Peak (A): 1070–1130 cm -1 The single point with the highest absorbance in the region. Peak (B): 1220–1280 cm -1 The single point with the highest absorbance in the region.
Citation Information
Patent Citations
Coating composition for forming velvety coating film
JP1989271463A
Aqueous coating agent composition
JP2009227707A
Active energy ray curable resin composition, coating agent composition, and laminated body
JP2014122338A
Ultraviolet-curable coating agent composition and laminate
JP2017171794A
One-part curable soft-feel coating
JP2018528999A